Composition liquid for surface treatment, and method for producing surface treatment substance, metal-coated resin, resin laminate, and resin-coated substance
A composition liquid with specific functional groups and a bisazide compound facilitates robust interfacial molecular bonding across diverse substances and pH ranges, addressing the limitations of existing technologies in adhesion and cost.
Patent Information
- Application Number
- JP2023059655
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing composition liquids for interfacial molecular bonding are limited to acidic pH ranges and are costly, failing to provide effective adhesion across a wide range of substances and combinations, particularly in neutral to basic conditions.
A composition liquid containing a polymer with primary or secondary amino groups, silanol or alkoxysilyl groups, epoxy, acryloyl, or methacryloyl groups, and a bisazide compound, which undergoes chemical reactions through heating or UV irradiation to enhance adhesion between substances.
The composition liquid enables strong interfacial molecular bonding across various substances, including resins and metals, in neutral to basic pH ranges, with improved adhesion and compatibility with electroless plating processes.
Smart Images

Figure 2024146631000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid composition for surface treatment that is applied to a substance for the purpose of improving adhesion, and to a method for producing a surface-treated substance, a method for producing a metal-coated resin, a method for producing a resin laminate, and a method for producing a resin-coated substance, all of which use the liquid composition. [Background technology]
[0002] Compounds having two or more functional groups can form chemical bonds by utilizing the characteristics of each functional group, and are therefore useful as interfacial molecular bonding agents for interface molecular bonding (IMB), which is a method of bonding two substances by chemical bonding by being interposed at the interface between the two substances. Since the interfacial molecular bonding agent bonds two substances by chemical bonding, the bond between the two substances is strong and does not necessarily require high temperatures to form the bond. Interfacial molecular bonding allows two substances to be bonded at a flat interface without relying on the anchor effect caused by roughening the surface. In addition, since only a small amount of molecules of the interfacial molecular bonding agent are present at the interface, the problem of weakening the bond due to volatile gases is unlikely to occur, and there is an advantage in terms of the environment.
[0003] Interfacial molecular bonding technology can be used in many applications to bond two materials at the interface. In particular, it has a wide range of applications in the electrical and electronic fields. For example, it can be used in the manufacture of electrical and electronic devices such as printed wiring boards, lightweight spacers, probe sockets (test jigs) for semiconductor test equipment, and resin-core metal foils for battery plates.
[0004] In order to use the interfacial molecular bonding technology, a composition liquid containing a compound having two or more functional groups is usually required. Patent Document 8 by some of the inventors of the present application discloses a composition liquid containing an azide aromatic carboxylic acid and an amine polymer, which is a composition liquid exhibiting a pH ranging from weakly acidic to acidic. This composition liquid is useful for ensuring adhesion between various substances, such as resin and resin, resin and metal, but is mainly suitable for use in a pH range ranging from weakly acidic to acidic. Patent Document 9 also discloses a composition liquid containing a siloxane oligomer obtained by hydrolysis and dehydration condensation of a silane compound monomer having an aromatic azide group and an alkoxysilyl group, and a silane compound monomer having an amino group and an alkoxysilyl group. This composition liquid is also useful for ensuring adhesion between various substances, such as resin and resin, resin and metal, but requires high manufacturing costs. There is a demand for a composition liquid that can be used in a wide pH range other than acidic and can ensure adhesion to a wide range of substance combinations.
[0005] Patent Document 1 discloses an invention of a surface treatment agent for plastics that contains an epoxysilane compound and a polyalkyleneimine. This surface treatment agent is not an interfacial molecular bonding agent for bonding two substances, but a composition liquid for forming a coating of a hardened material on the plastic surface. In addition, this surface treatment agent does not contain a bisazide compound.
[0006] Patent Document 2 discloses an invention of a composition having biocidal activity containing a silane-modified polymer amine. The composition is intended to form a coating that is substantially non-sticky after being applied to the surface of a resin film or the like, and is not an interfacial molecular bonding agent for bonding two substances. In addition, the composition does not contain a bisazide compound.
[0007] Patent Document 3 discloses a method for producing a printed circuit board, which includes coating a substrate with a multi-amine polymer and then contacting it with a precious metal ion. The method is characterized in that the multi-amine polymer is modified with a compound containing a functional group reactive to an amino group before the contact. However, this document does not disclose the modification of the multi-amine polymer with a silane compound, nor does it disclose a bisazide compound.
[0008] Patent Document 4 discloses a method for producing a composite material such as metal nanowires, which includes the steps of: obtaining a composite of a polymer aggregate and silica by adding an epoxy-based alkoxysilane to an aggregate of a polymer having a linear polyethyleneimine skeleton in an aqueous medium; contacting the aggregate with a solution in which a transition metal ion is dissolved to cause the transition metal ion to be coordinated to the linear polyethyleneimine skeleton in the polymer; and reducing the coordinated transition metal ion with a reducing agent. However, Patent Document 4 does not disclose the use of a composition solution containing silane-modified polyethyleneimine as a composition solution for pretreatment when electroless plating is performed on a macroscopic surface of a substrate such as the surface of a resin film, nor does it disclose a bisazide compound.
[0009] Patent Document 5 discloses a method for modifying the polymer surface of a substrate, and shows a method for forming a grafted crosslinked network by contacting a polyamine compound and a crosslinking agent with a polymer surface having functional groups. In this document, epoxy silane, acryloxy silane, glycidyl acrylate, etc. are exemplified as crosslinking agents, but bisazide compounds are not mentioned. In addition, although this document describes the adhesion between the polymer and the metal coating, it does not describe the application of the above modification method to an electroless plating process.
[0010] Patent Document 6 discloses an invention relating to a polyamine coating having barrier properties that is useful for interlayer adhesion of laminated packaging films. The liquid composition for forming the coating may contain polyamine and acryl silane, epoxy silane, glycidyl acrylate, etc. as a crosslinking agent, but there is no mention of a bisazide compound.
[0011] Patent Document 7 discloses an invention relating to a coating containing an ethylenically unsaturated acid, a polyamine, and a bis-silane, which has barrier properties useful for packaging applications, and describes the preferable addition of an epoxy silane, an acryloxy silane, glycidyl methacrylate, or the like as a crosslinking agent, but does not disclose bis-azide compounds. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Special Publication No. 59-043051 [Patent Document 2] Special Publication No. 2008-540753 [Patent Document 3] Japanese Patent Application Publication No. 03-173196 [Patent Document 4] Patent No. 3978440 [Patent Document 5] Special Publication No. 2003-512490 [Patent Document 6] Patent No. 3851354 [Patent Document 7] Special Publication No. 2004-528395 [Patent Document 8] Patent No. 7120695 [Patent Document 9] Patent Publication No. 2022-048068 Summary of the Invention [Problem to be solved by the invention]
[0013] The object of the present invention is, first, to provide a liquid composition to be applied to a substance for the purpose of ensuring adhesion in plating, lamination, etc., which can be used mainly in the neutral to basic range and is applicable to a variety of substances or combinations of substances, or, second, to provide a method for producing a surface-treated substance, a method for producing a metal-coated resin by plating or lamination, a method for producing a resin laminate, or a method for producing a resin-coated substance, using the above-mentioned dispersion. The above-mentioned liquid composition contains a compound or a combination of compounds that undergoes a chemical reaction related to interfacial molecular bonding upon heating and / or irradiation with ultraviolet light after application. [Means for solving the problem]
[0014] A first aspect of the present invention is a liquid composition to be applied to at least one of two substances for the purpose of improving adhesion between the two substances, the liquid composition comprising a polymer having a first repeating unit having a primary amino group or a secondary amino group, and a second repeating unit having one or more functional groups selected from the group consisting of a silanol group, an alkoxysilyl group, an epoxy group, an acryloyl group, and a methacryloyl group, and a bisazide compound.
[0015] A second aspect of the present invention is the liquid composition of the first aspect, wherein the second repeating unit has a silanol group or an alkoxysilyl group.
[0016] A third aspect of the present invention is a liquid composition to be applied to a material to be plated for the purpose of improving adhesion of the plating, the liquid composition comprising a polymer having a first repeating unit having a primary amino group or a secondary amino group, and a second repeating unit having a silanol group or an alkoxysilyl group.
[0017] A fourth aspect of the present invention is a liquid composition according to the first, second or third aspect, wherein the polymer has a second repeating unit having one or more functional groups selected from the group consisting of an epoxy group, an acryloyl group and a methacryloyl group.
[0018] A fifth aspect of the present invention is the liquid composition of the second or third aspect, wherein the second repeating unit contains a polysiloxane skeleton.
[0019] A sixth aspect of the present invention is the liquid composition according to the first, second or third aspect, wherein the polymer has a polyethyleneimine structure.
[0020] The seventh form of the present invention is a liquid composition according to the first or second form, wherein at least two of the azide groups contained in the bisazide compound are azide groups directly bonded to an aromatic ring.
[0021] The eighth aspect of the present invention is a method for producing a surface-treated substance, comprising a step (coating step) of coating the liquid composition according to the first, second or third aspect onto the surface of a substance.
[0022] A ninth aspect of the present invention is a method for producing a metal-coated resin, comprising the steps of applying the composition liquid according to the first, second or third aspect onto a surface of a resin (application step), heating the surface or irradiating the surface with ultraviolet light (activation step), and then forming a metal plating layer on the surface by wet plating (plating step).
[0023] The tenth aspect of the present invention is a method for producing a metal-coated resin, comprising the steps of applying the liquid composition according to the first aspect to at least one of the surfaces of a resin and a metal foil (application step), heating the surface or irradiating the surface with ultraviolet light (activation step), and then laminating the resin and metal foil via the surface and applying pressure to integrate them (pressing step).
[0024] The eleventh aspect of the present invention is a method for producing a resin laminate, comprising the steps of applying the composition liquid according to the first aspect onto a surface of a first resin (application step), heating the surface or irradiating the surface with ultraviolet light (activation step), and then laminating a second resin on the surface and integrating them by applying pressure (pressing step).
[0025] The twelfth form of the present invention is a method for producing a resin-coated material, comprising the steps of applying the liquid composition according to the first form to a surface of a material (application step), heating the surface or irradiating the surface with ultraviolet light (activation step), applying a resin varnish onto the surface (resin application step), and curing the varnish (curing step). Effect of the Invention
[0026] According to one aspect of the present invention, it is possible to provide a composition liquid that is applied to a substance for the purpose of ensuring adhesion in plating, lamination, etc., and that can be used mainly in the neutral to basic range and is applicable to a variety of substances or combinations of substances. The composition liquid contains a compound or a combination of multiple compounds that undergoes a chemical reaction related to interfacial molecular bonding upon heating and / or irradiation with ultraviolet light after application. According to another aspect of the present invention, there can be provided a method for producing a surface-treated substance, a method for producing a metal-coated resin by plating or lamination, a method for producing a resin laminate, or a method for producing a resin-coated substance, using the dispersion. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is an explanatory diagram of the interfacial molecular bonding mechanism. [Diagram 2] FIG. 2 is a flow diagram of a method for producing a surface treatment substance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Next, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the embodiments and examples described below, and should be understood to include various modifications and variations implemented within the scope of the technical concept of the present invention.
[0029] <Composition liquid> According to one embodiment of the present invention, there is provided a liquid composition to be applied to at least one of two substances for the purpose of improving adhesion between the two substances, the liquid composition comprising a polymer having a first repeating unit having a primary amino group or a secondary amino group, and a second repeating unit having one or more functional groups selected from the group consisting of a silanol group, an alkoxysilyl group, an epoxy group, an acryloyl group, and a methacryloyl group, and a bisazide compound.
[0030] (Purpose of improving adhesion) "Coating at least one of two substances for the purpose of improving the adhesion between them" means that the adhesion is improved by interposing a compound derived from the liquid composition at the interface between one substance and another substance. For example, the liquid composition according to this embodiment is coated on a resin, metal, or other inorganic substance for the purpose of producing a resin film laminate in which two resin films are integrally bonded together, for the purpose of forming a metal coating bonded to the surface of a resin by plating or lamination, or for the purpose of forming a coating of a cured resin varnish bonded to an inorganic substance such as a metal, glass, or ceramic.
[0031] (Coating) Here, "application" is not limited to a method such as brushing, but generally refers to "adhering" a liquid to the surface of a substance or "allowing the liquid to be in contact with the surface of the substance. Preferably, "application" includes a step of removing the solvent of the liquid by drying or the like after adhering or bringing the liquid into contact with the surface of the substance, thereby leaving the solute on the surface.
[0032] (First repeating unit having a primary amino group or a secondary amino group) This composition contains primary amino groups (-NH 2 The polymer includes a first repeating unit having a secondary amino group (-NH-) or a secondary amino group (-NH-). After the application of the composition liquid and the activation step, the polymer forms a bond with the surface of the substance and / or the bisazide compound by chemical reaction, and contributes to the formation of an interfacial molecular bond. Examples of the first repeating unit are repeating units represented by any of the following formulas (1) to (6).
[0033] [ka]
[0034] In each of formulas (1) to (6), a is an integer of 0 or more, for example, an integer of 1 or more and 10 or less, preferably an integer of 1 or more and 4 or less, more preferably 1; R 1 , R 2 and R 3 each independently represents a H atom, a substituted or unsubstituted alkyl group (e.g., having 1 to 25 carbon atoms, or 1 to 5 carbon atoms), or an aryl group (e.g., a phenyl group or a benzyl group), Z - represents an anion in the solution and is not included in the polymer. 1 , R 2 and R 3 At least one of these is a H atom.
[0035] In each of the formulas (1) to (6), R 1 , R 2 and R 3 The alkyl and aryl groups represented by the formula (I) may have one or more substituents. Suitable substituents include cationic groups, e.g., quaternary ammonium groups, or amine groups, e.g., primary, secondary or tertiary alkyl or aryl amines. Other suitable examples of substituents include hydroxy groups, alkoxy groups, alkyl groups, aryl groups, poly(alkyleneimines), e.g., poly(ethyleneimine), and the like.
[0036] The first repeat unit is preferably a poly(lower alkyleneimine) ([C m H 2m N.H. n , m is an integer of 1 or more and 4 or less, and n is an integer of 2 or more), a repeating unit contained in one or more polymers selected from the group consisting of polyvinylamine and polyallylamine, and more preferably a repeating unit contained in one or more polymers selected from the group consisting of polyethyleneimine, polyvinylamine and polyallylamine.
[0037] (Second repeat unit) The liquid composition contains a polymer having a second repeating unit having a silanol group, an alkoxysilyl group, an epoxy group, an acryloyl group, or a methacryloyl group. Since the polymer has the second repeating unit, it can form a bond with the surface of a wider range of substances and / or a bisazide compound through a chemical reaction after the liquid composition is applied and the activation process, thereby contributing to the formation of an interfacial molecular bond. As the second repeating unit, for example, in each of the formulae (1) to (6), which are examples of the first repeating unit, R 1 , R 2 and R 3 At least one of the formula -Z 1 -Q 1 In this case, Z 1 is a divalent linking group, and Q 1 is a group containing a silanol group or an alkoxysilyl group, an epoxy group, an acryloyl group, or a methacryloyl group. The "silanol group or alkoxysilyl group-containing group" is represented by the formula -Si(R 4 ) 3 where the three R 4 are each independently a group selected from the group consisting of a hydrogen atom, an OH group, an alkyl group having 4 or less carbon atoms, an alkoxy group having 4 or less carbon atoms, a phenyl group, a phenyloxy group, a benzyl group, and a benzyloxy group, and three R 4 At least one of them contains an O atom. Examples of the "group containing a silanol group or an alkoxysilyl group" include a trimethoxysilyl group, a triethoxysilyl group, and a trisilanol group. Z 1 is a substituted or unsubstituted linear alkylene group and has the formula -(CR 5 R 6 ) b - (wherein b is an integer of 1 or more and 25 or less, preferably an integer of 1 or more and 10 or less, more preferably an integer of 1 or more and 5 or less.5 , R 6 are each independently an H atom, an alkyl group (having 1 to 10 carbon atoms, or 1 to 5 carbon atoms), or an aryl group (having 9 carbon atoms or less, or a phenyl group or a benzyl group), or -(CR 5 R 6 ) b - A group in which one to three insertion groups are inserted, with overlapping allowed, at one, two or three positions selected from the left end, right end and any adjacent C atom of the group represented by the formula (I), and the insertion groups are each independently selected from the group consisting of -O-, -(C=O)-, -(C=O)NR-, -NR(C=O)-, -(C=O)O-, -O(O=C)-, -C(OH)- and -NR-. R is an H atom, a substituted or unsubstituted alkyl group (having 1 to 10 carbon atoms or 1 to 5 carbon atoms) or an aryl group (having 9 or less carbon atoms, or a phenyl group or a benzyl group). Here, the alkyl group or aryl group represented by R may have one or more substituents. Suitable substituents include a cationic group, such as a quaternary ammonium group, or an amine group, such as a primary, secondary or tertiary alkylamine or arylamine. Other examples of suitable substituents include hydroxy groups, alkoxy groups or alkyl groups (having 1 to 10 carbon atoms, or 1 to 5 carbon atoms), aryl groups (having 9 carbon atoms or less, or phenyl or benzyl groups), poly(alkyleneimines) such as poly(ethyleneimine), and the like.
[0038] Other examples of the second repeating unit include, for example, the first repeating unit in each of the formulae (1) to (6), 1 , R 2 and R 3 At least one of the formula -Z 1 -*-Q 1 In this case, Z 1 and Q 1represents the same groups as above, and * represents a siloxane polymer (or oligomer) or an organic polymer (or oligomer). In this manner, in one embodiment of the present composition liquid having a second repeating unit being a polymer or oligomer, the side chain of the polymer contained in the composition liquid has a functional group Q 1 Since the composition liquid of this embodiment has a polymer or oligomer having the above structure, it has an advantage that it can absorb the difference in the distance between the surfaces of two substances facing each other at the interface depending on the location when viewed microscopically, and can stably ensure the adhesion in the interfacial molecular bond. In addition, when the second repeating unit contains a siloxane polymer, the composition liquid of this embodiment is generally suitable for interfacial molecular bonding in which at least one of the two substances is an inorganic material, and when the second repeating unit contains an organic polymer, the composition liquid of this embodiment is generally suitable for interfacial molecular bonding in which at least one of the two substances is an organic material.
[0039] (Specific Examples of Polymers According to the Invention) The polymer according to the present invention necessarily has a first repeating unit. The first repeating unit has a primary amino group or a secondary amino group. The second repeating unit is a general term for those having other functional groups, and multiple types of second repeating units may be present in the polymer. A specific example of a polymer in which the second repeating unit has a trimethoxysilyl group and the polymer has a polyethyleneimine structure is the following compound (hereinafter referred to as "compound ET"): (n and m are natural numbers or positive real numbers representing the composition ratio. The same applies below.)
[0040] [ka]
[0041] Furthermore, a specific example of a polymer having both a second repeating unit having a methacryloyl group and a second repeating unit having an epoxy group and having a polyethyleneimine structure is the following compound (hereinafter referred to as "compound ETG").
[0042] [ka]
[0043] Furthermore, a specific example of a polymer having a polyethyleneimine structure that includes a second repeating unit having a trimethoxysilyl group, a second repeating unit having a methacryloyl group, and a second repeating unit having an epoxy group is the following compound (hereinafter referred to as "compound ETMX").
[0044] [ka]
[0045] (Polymer manufacturing method) A method for producing the polymer having a first repeating unit contained in this liquid composition is publicly known and is disclosed, for example, in JP 2016-047849 A and patent documents cited therein. The polymer having a first repeating unit and a second repeating unit contained in this composition liquid can be prepared, for example, as shown in the synthesis example described later, by first preparing a polymer having a first repeating unit, and then reacting the polymer with an epoxy silane compound or an epoxy acrylate compound to modify a portion of the primary amino groups or secondary amino groups contained in the polymer. The epoxysilane compound used in the above reaction is not limited, but examples thereof include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and the like. The epoxy acrylate compound used in the above reaction is not limited, but examples thereof include glycidyl acrylate, glycidyl methacrylate, and the like.
[0046] (Polymer structure) The polymer having the first repeating unit and the second repeating unit contained in the liquid composition may have any of a linear structure, a branched structure, and a dendrimer structure, and may be crosslinked with a bifunctional crosslinking agent such as epichlorohydrin.
[0047] (Weight average molecular weight of polymer) The weight average molecular weight of the polymer having the first repeating unit and the second repeating unit contained in the present composition liquid is preferably 20000 or less, more preferably 3000 or less, and even more preferably 1500 or less, from the viewpoint of suppressing uneven coating of the present composition liquid. In addition, the weight average molecular weight is preferably 200 or more, more preferably 450 or more, and even more preferably 900 or more, from the viewpoint of ensuring adhesion in the interfacial molecular bond by absorbing the difference depending on the location of the distance between the surfaces of two substances facing each other at the interface when viewed microscopically. In this specification, the weight average molecular weight of the polymer means the weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC method).
[0048] In the present composition, the above polymers may be used alone or in combination of two or more.
[0049] (Polymer concentration) In this composition liquid, the concentration of the polymer is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.05% by mass or more, from the viewpoint of ensuring adhesion in interfacial molecular bonds. In addition, the concentration is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less, from the viewpoint of suppressing coating unevenness. In addition, when two or more kinds of the above polymers are used in combination, "the concentration of the above polymer" means the sum of the concentrations of the various polymers.
[0050] (Bisazide compounds) This liquid composition contains a bisazide compound. In this specification, the term "bisazide compound" refers to a compound having azide groups (-N 3 The azide group is a compound having two or more azide ions (N 3 -) may be a group derived from the azide group. The two azide groups are "located at different ends" means that the two azide groups are not directly bonded to the same atom in one molecule. The bisazide compound contains an azide group, and as a result of heating or light irradiation, it can generate nitrene as an active species. From the viewpoint that the generation of nitrene can be promoted even by heating at a low temperature of about 80 to 160°C or by irradiation with light having a long wavelength of about 260 to 365 nm among ultraviolet rays, the bisazide compound preferably contains a substituted or unsubstituted aromatic group (aromatic ring), more preferably the aromatic ring is directly bonded to the azide group, and further preferably the aromatic ring directly bonded to the azide group is a substituted or unsubstituted benzene ring. By including a bisazide compound in the present composition liquid, it is possible to promote the bonding reaction between the bisazide compound and the polymer and / or the bonding reaction between the bisazide compound and the substance to which the present composition liquid is applied or another substance layered on the substance, thereby improving the adhesion between the substance to which the present composition liquid is applied and another substance layered on the substance.
[0051] Bisazide compounds having two aromatic rings and preferred as components of the present liquid composition are listed in order of the distance between the two azide groups (here, "distance" means the minimum number of atoms included in the sequence of atoms connecting the two azide groups. For example, in diazidomethane, the two azide groups are connected via one C atom, so the "distance" between the two azide groups is 1.) as follows: 3,3'-Diazidodiphenyl sulfone, 3,3'-Diazidodiphenyl sulfide, 3,3'-Diazidodiphenyl disulfide, 4,4'-Diazidobiphenyl, 4,4'-diazidodiphenyl ether, 4,4'-diazidobenzophenone, 4,4'-diazidodiphenylmethane, 3,3'-dichloro-4,4'-diazidodiphenylmethane, 4,4'-diazidodiphenyl sulfone, 4,4'-diazidodiphenyl sulfide, 4,4'-Diazidostilbene, 4,4'-Diazidostilbene-2,2'-disulfonic acid (disodium salt), 4,4'-Diazidostilbene-2,2'-disulfonylamide, 4,4'-Diazidostilbene-2,2'-disulfonyl-N-(p-methoxyphenyl)amide, 4,4'-Diazidostilbene-2,2'-disulfonyl-N-(p-hydroxyethylphenyl)amide, 4,4'-Diazidostilbene-2,2'-disulfonyl-N-(p-hydroxyphenyl)amide, 4,4'-Diazidodiphenyl disulfide, 4,4'-Diazidochalcone, 4,4'-Diazidochalcone-2-sulfonic acid (sodium salt), 2,6-bis(4'-azidobenzylidene)cyclohexanone, 2,6-bis(4'-azidobenzylidene-2'-sulfonic acid (sodium salt))cyclohexanone, 2,6-bis(4'-azidobenzylidene)-4-methylcyclohexanone, 2,6-bis(4'-azidobenzylidene)-4-ethylcyclohexanone, 1,3-bis(4'-azidobenzylidene)-2-propanone, 1,3-bis(4'-azidobenzylidene-2'-sulfonic acid (sodium salt))-2-propanone, 4,4'-diazidobenzylideneacetone, 2,5-bis(4'-azidobenzylidene-2'-sulfonic acid (sodium salt))cyclopentanone, Examples thereof include 2,6-bis(4'-azidocinnamylidene)cyclohexanone, 2,6-bis(4'-azidocinnamylidene)-4-methylcyclohexanone, and 1,3-bis(4'-azidocinnamylidene)-2-propanone.
[0052] Examples of bisazide compounds having three or more aromatic rings or condensed rings and which are preferred as components of the present composition liquid are listed below, in order of the shortest distance between the two azide groups: Examples of the azido-9H-fluoren-9-one include 2,7-diazide-9H-fluoren-9-one, 6-azido-2-(4'-azidostyryl)benzimidazole, 1,4-bis(3'-azidostyryl)benzene, and 1,4'-azidobenzylidene-3-α-hydroxy-4"-azidobenzylindene.
[0053] In the present composition, the bisazide compound may be used alone or in combination of two or more kinds.
[0054] As an example of a bisazide compound having two azide groups directly bonded to a benzene ring and suitable for carrying out the present invention, the structural formula of 2,6-bis(4'-azidobenzylidene)-4-methylcyclohexanone (hereinafter referred to as "BABMC") is shown below.
[0055] [ka]
[0056] (Synthesis of bisazide compounds) The synthesis method of the above-mentioned bisazide compound is not particularly limited, but it can be obtained by known methods such as (1) introducing an azide group into an aromatic compound using sodium azide, (2) introducing an azide group into an aromatic compound using tosyl azide or trifluoromethanesulfonyl azide, (3) introducing an azide group by a coupling reaction using a copper catalyst, etc. In addition, many of the above-mentioned bisazide compounds are commercially available.
[0057] (Concentration of bisazide compound) The concentration of the bisazide compound in the present composition liquid is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.05% by mass or more, from the viewpoint of ensuring adhesion in interfacial molecular bonding. In addition, the concentration is preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less, from the viewpoint of suppressing coating unevenness. In addition, when two or more kinds of bisazide compounds are used in combination, the "concentration of the bisazide compound" means the sum of the concentrations of various bisazide compounds.
[0058] (Solvent for this composition) The liquid composition contains a solvent. The solvent is not particularly limited as long as it can dissolve the polymer and the bisazide compound. For example, alcohols such as methanol, ethanol, isopropanol, ethylene glycol, propylene glycol, cellosolve, carbitol, propylene glycol monomethyl ether, and 3-methoxy-3-methyl-1-butanol (hereinafter referred to as "SF"), ketones such as acetone, methyl ethyl ketone, and cyclohexanone, aromatic hydrocarbons such as benzene, toluene, and xylene, aliphatic hydrocarbons such as hexane, octane, decane, dodecane, and octadecane, esters such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, methyl propionate, and methyl phthalate, ethers such as tetrahydrofuran (THF), ethyl butyl ether, anisole, and propylene glycol monomethyl ether acetate (PGMEA), and water can be used. Among these, alcohols, ethers, and water are preferred. Only one type of solvent may be used, or two or more types may be mixed and used.
[0059] (pH of this composition) The pH of the present composition at 25°C is preferably 11.0 or less, more preferably 10.0 or less, and even more preferably 9.0 or less. The pH is preferably 7.0 or more, more preferably 7.5 or more, and even more preferably 8.0 or more. When the pH of the present composition satisfies the above conditions, the chemical stability of the present composition in the atmosphere is ensured, and the formation of interfacial molecular bonds after application is promoted. In this specification, the pH of the composition means a value measured at 25°C with a pH test paper (UNIVERSAL test paper, manufactured by Advantec Toyo Co., Ltd.), and the measurement error is about ±0.5.
[0060] (material) The two substances used in the method for producing a laminate using this liquid composition may be made of the same material or different materials. Each substance may be made of multiple materials. Each substance may have a coating film or the like formed on its surface. Each substance may be a part of an object made of multiple materials. Examples of materials constituting each substance include organic materials such as resins and elastomers, and inorganic materials such as glass, ceramics, metals, silicon wafers, and plating bases (catalysts).
[0061] In this specification, the term "resin" includes, for example, thermoplastic resins, thermosetting resins, and the like. Examples of thermoplastic resins include general-purpose resins, engineering resins, super engineering resins, etc. Examples of general-purpose resins include polyvinyl chloride (PVC), polyethylene (PE), polypropylene (PP), polystyrene (PS), acrylonitrile-butadiene-styrene (ABS), acrylonitrile-styrene (AS), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyvinylidene chloride (PVDC), polyethylene terephthalate (PET), cycloolefin polymer (COP), etc. Examples of engineering resins include polyamide (PA), polyacetal (POM), polycarbonate (PC), polyphenylene ether (PPE (modified PPO)), polybutylene terephthalate (PBT), ultra-high molecular weight polyethylene (U-PE), polyvinylidene fluoride (PVDF), etc. Examples of super engineering resins include polysulfone (PSU), polyethersulfone (PES), polyphenylene sulfide (PPS), polyarylate (PAR), polyamideimide (PAI), polyetherimide (PEI), polyetheretherketone (PEEK), thermoplastic polyimide (TPI), liquid crystal polymer (LCP), and polytetrafluoroethylene (PTFE). Examples of thermosetting resins include phenolic resin (PF), epoxy resin (EP), melamine resin (MF), urea resin (urea resin, UF), unsaturated polyester resin (UP), alkyd resin, polyurethane (PUR), polyimide (PI), modified polyimide (MPI), and thermosetting polyimide. Examples of commercial forms of thermosetting resins include C-stage (cured) sheets such as polyimide, B-stage (uncured) sheets such as build-up sheets, prepregs, die-bond sheets, and ACF (anisotropic conductive sheets), and A-stage materials such as conductive or insulating compounds, pastes, or inks.
[0062] Examples of the elastomer include natural rubber, synthetic rubber, urethane rubber, silicone rubber, and fluororubber.
[0063] Examples of metals include copper, silver, gold, nickel, and aluminum.
[0064] Examples of glass include ordinary soda glass (white plate glass, etc.), borosilicate glass, lead glass, flint glass, optical glass, and quartz glass.
[0065] Examples of ceramics include aluminum oxide, zirconium oxide, aluminum nitride, silicon carbide, silicon nitride, boron nitride, forsterite, steatite, cordierite, sialon, barium titanate, lead zirconate titanate, ferrite, mullite, and mica.
[0066] The shapes of the two substances are not particularly limited. Specific shapes of the substance to be applied with the liquid composition according to the present invention include, for example, a plate, a sheet, a film, a tube, a column, a string, an amorphous lump, or any other shape formed into a predetermined shape. In some embodiments of the present invention, the material to which the liquid composition is applied (the material to which the surface treatment is performed) is preferably a non-fibrous substrate. A fiber is, for example, a string-like solid having a maximum diameter of less than 0.1 mm and a length of more than 10 times the maximum diameter. When the material to which the liquid composition is applied is in the form of a string, the maximum diameter is preferably 0.1 mm or more, more preferably 1 mm or more. The length is preferably 10 times or less, more preferably 5 times or less, of the maximum diameter. By performing surface treatment on a non-fibrous material in this way, a bond between two materials can be efficiently obtained.
[0067] (Bonding ability of silanol group or alkoxysilyl group with substance) The alkoxysilyl group generates a silanol group by hydrolysis or solvolysis. The silanol group can form an Si-O bond with a carboxy group through silyl esterification, and can form an Si-O bond with a hydroxy group through a silane coupling reaction. The form of the present composition liquid, in which the second repeating unit has a silanol group or an alkoxysilyl group, is useful for interfacial molecular bonding of substances such as resins having a carboxy group and / or a hydroxy group. In addition, since the carboxy group and / or the hydroxy group are formed on the surface of various substances that have been subjected to a pretreatment process described below, the composition liquid in this form is useful for interfacial molecular bonding of various substances that have been subjected to a pretreatment process. An example of a resin having a carboxy group and / or a hydroxy group is polyallylamine (PAA).
[0068] (Binding ability between primary amino group or secondary amino group and substance) A primary amino group or a secondary amino group can form a C-N bond with a carboxy group by amidation, can form a C-N bond with an epoxy group by ring-opening amination, and can further form a C-N bond with an ester group -(C=O)O- by transamidation. Since the first repeating unit of the present composition liquid has a primary amino group or a secondary amino group, the composition liquid is useful for interfacial molecular bonding of materials such as resins having a carboxy group, an epoxy group, or an ester group. In addition, since the carboxy group is formed on the surface of various organic materials that have been subjected to a pretreatment process described below, the composition liquid in this form is useful for interfacial molecular bonding of various organic materials that have been subjected to a pretreatment process. Examples of various organic materials that have been subjected to a pretreatment process include organic materials that have been treated with atmospheric plasma and polyimide (PI) that has been treated with an alkali. Examples of the resin having a carboxy group are as described above. Examples of resins having an epoxy group include various epoxy resins. Examples of resins having an ester group include liquid crystal polymer (LCP), polycarbonate (PC), polymethyl methacrylic (PMMA), and polyethylene terephthalate (PET).
[0069] (Bonding between epoxy groups and substances) An epoxy group can form a C-O bond with a carboxy group through esterification, a C-O bond with a hydroxy group through etherification, a C-N bond with an amino group through ring-opening amination, and a C-C bond with an epoxy group through ring-opening polymerization. The form of the present composition liquid in which the second repeating unit has an epoxy group is useful for interfacial molecular bonding of substances such as resins having a carboxy group, a hydroxy group, an amino group, or an epoxy group. In addition, since the carboxy group and / or the hydroxy group are formed on the surface of various substances that have been subjected to a pretreatment process described below, the composition liquid in this form is useful for interfacial molecular bonding of various substances that have been subjected to a pretreatment process. Examples of the resin having a carboxy group or a hydroxy group, and examples of the resin having an epoxy group are as described above. Examples of resins having amino groups include polyallylamine (PAA) and various resins modified to have amino groups.
[0070] (Binding ability of acryloyl or methacryloyl groups to substances) An acryloyl group or a methacryloyl group can form a C-N bond by aza-Michael addition with an amino group. The form of the present composition liquid in which the second repeating unit has an acryloyl group or a methacryloyl group is useful for interfacial molecular bonding of substances such as resins having amino groups. Examples of the resin having an amino group are as described above.
[0071] (Binding ability between azide group and substance) The azide group releases a nitrogen molecule upon heating or irradiation with light to become a nitrene. Azide groups (nitrenes) can form C-N bonds with alkenyl groups (-CH=CH-) by aziridination, and methylene groups (-CH 2 -) and CH amination to form a C-N bond, and further, a methyl group (-CH 3 ) to form a C-N bond by hydrogen abstraction amination, and in addition, it can form a C-N bond by a [2+1] cycloaddition reaction with a phenyl group. The azide group can also undergo a [3+2] cycloaddition reaction with an alkenyl group (-CH=CH-) to form a triazole ring, forming a C-N bond. The present liquid composition containing a bisazide compound is useful for interfacial molecular bonding of substances such as resins having an alkenyl group, a methylene group, a methyl group, or a phenyl group. Examples of resins having an alkenyl group include ABS resins and polyolefins having double bonds at the polymerization terminals. Examples of resins having a methylene group include ABS resin, polypropylene (PP), polyethylene (PE), polystyrene (PS), and polymethyl methacrylic (PMMA). Examples of resins having a methyl group include polypropylene (PP), polycarbonate (PC), and polymethyl methacrylate (PMMA). Examples of resins having a phenyl group include polystyrene (PS), polyphenylene sulfide (PPS), liquid crystal polymer (LCP), carbon nanotube (CNT), polyimide (PI), polycarbonate (PC), and polyether ether ketone (PEEK). Each of the at least two azide groups contained in the bisazide compound contained in this form of the composition liquid can form a C-N bond with a polymer having a first repeating unit and a second repeating unit, as described above, and therefore the bisazide compound acts as a crosslinking agent for the polymer, strengthening the interfacial molecular bond between any two substances.
[0072] (Interfacial molecular bonding mechanism) Although it is not easy to verify the mechanism of the interfacial molecular bond in the present invention, it is presumed that a chemical bond as shown in FIG. 1 is generated at the interface where the present composition liquid is interposed. FIG. 1 shows a state where a condensate layer 3 related to the present composition liquid is interposed at the interface between the substance 2 and the substance 4 in a laminate 1 formed by laminating substances 2, 4, and 5. The substance 4 and the substance 5 may be joined by an interfacial molecular bond in the same manner as the joining of the substance 2 and the substance 4, or may be joined by other methods such as high-temperature pressing. In the figure, A1 to A4 represent portions derived from the bisazide compound related to the present composition liquid, and P1 and P2 represent polymers (hereinafter referred to as amine polymers) having the first repeating unit and the second repeating unit related to the present composition liquid. P1 is a linear amine polymer, and P2 is a branched amine polymer. The surfaces of the substances 2 and 4 have functional groups such as OH groups, carboxy groups, carbonyl groups, primary amino groups, and secondary amino groups, either originally or generated in a pretreatment step, and the functional groups contained in the amine polymers P1 and P2, such as amino groups, silanol groups, epoxy groups, and acryloyl groups, react with the functional groups on the surfaces to form bonds. The bisazide compound-derived portion A1 is radically bonded to the surface of the substance 4 by the nitrene generated by decomposition of the azide group at one end of the bisazide compound. The other end of A1 is radically bonded to the amine polymer P1. Similarly, one end of the bisazide compound-derived portion A2 is radically bonded to the surface of the substance 4, and the other end of A2 is radically bonded to the amine polymer P2. One end of the bisazide compound-derived portion A3 is radically bonded to the surface of the substance 2, and the other end of A3 is radically bonded to the amine polymer P2. One end of the bisazide compound-derived portion A4 is radically bonded to the amine polymer P1, and the other end of A4 is radically bonded to the amine polymer P2. In this way, the bisazide compound of this composition crosslinks two substances and the amine polymers to each other to form bonds. Although not shown in Fig. 1, a bond may be formed between P1 and P2, or between branched chains of P2, by a reaction between functional groups of the amine polymers P1 and P2. For example, when P1 and P2 have a silanol group, P1 and P2 may be bonded by a siloxane bond. In addition, a bond may be formed between amine polymers by a reaction between an epoxy group and an amino group, or a (meth)acryloyl group and an amino group, or the like.
[0073] <Method of manufacturing surface treatment material> With reference to the flow chart of FIG. 2, one embodiment of the present invention can provide a method for manufacturing a surface-treated material, comprising a step of applying any of the above-described liquid compositions to the surface of a material (application step (S2)). The manufacturing method preferably comprises a pretreatment step S1 and an activation step. The activation step may include a step of heating the surface of the material to which the liquid composition has been applied (thermal activation step (S4)), and a step of irradiating the surface of the material to which the liquid composition has been applied with ultraviolet light (UV activation step (S6)). The manufacturing method may comprise a post-activation cleaning step (S8).
[0074] (Coating process) In the coating step (S2), a treatment liquid such as the present composition liquid is coated on a material such as a polyimide film. Here, "coating" refers to "adhering" the treatment liquid to the surface of the material or "allowing it to be present in contact with the surface". Coating methods include conventionally known coating methods, such as brush coating, inkjet coating, gravure coating, lip coating, comma coating, blade coating, roll coating, knife coating, spray coating, bar coating, spin coating, and dip coating. The lower limit of the thickness of the coating film (wet film thickness) when the present composition liquid is applied is, for example, preferably 0.5 μm, more preferably 1.5 μm, and even more preferably 5 μm, from the viewpoint of ensuring adhesion between the surface treatment material and other materials (materials and metals). Similarly, the lower limit of the thickness of the coating film (dry film thickness) is, for example, preferably 1 nm, more preferably 3 nm, and even more preferably 10 nm. On the other hand, the upper limit of the coating thickness (wet film thickness) is, for example, preferably 500 μm, more preferably 150 μm, and even more preferably 50 μm, from the viewpoint of ease of application and suppression of coating unevenness. Similarly, the upper limit of the coating thickness (dry film thickness) is, for example, preferably 1 μm, more preferably 300 nm, and even more preferably 100 nm. When using the dip coating method, the immersion time is preferably, for example, 3 seconds or more and 60 seconds or less. "Coating" may be performed on a part of the surface of the substance, or on the entire surface of the substance. In addition, when the substance is in the form of a film or sheet, "coating" may be performed only on one side of the substance, the front or back, or on both the front and back of the substance. After the "coating", a step (drying step) is usually performed in which the surface of the substance to which the treatment liquid has been applied is dried by natural drying in the air, air drying, or by blowing hot air at about 40° C. to 70° C. The amine polymer and bisazide compound contained in the present composition liquid are disposed on the surface of the substance by the above-mentioned coating and drying steps.
[0075] (Heating activation process) In the thermal activation step (S4), the surface of the material to which the liquid composition has been applied is heated. By heating, the surface becomes suitable for bonding with other materials by thermocompression bonding or metal plating. The temperature of the surface of the material during heating is, for example, 80 to 160°C, preferably 90°C to 120°C, and the time for which the surface of the material is kept at that temperature is, for example, 30 seconds to 60 minutes, preferably 5 to 20 minutes. Although it is difficult to analyze the phenomenon occurring in the thermal activation step, it is assumed that the following phenomenon occurs approximately. The azide group of the bisazide compound is decomposed by the heat treatment to form N 2 Molecules will be released and nitrenes will be generated, making the bisazide compound suitable for bonding with materials such as resins and metals and with the amine polymer. Heating will also make the various functional groups of the amine polymer suitable for bonding with the bisazide compound and materials such as resins and metals. The bisazide compound and the amine polymer will bond with each other and with the material to form an extremely thin layer of condensation on the surface of the material. In this way, the heat activation step will form an extremely thin layer of condensation in close contact with the surface of the material, and the surface of the condensation is considered to be suitable for bonding with other materials such as resins and metals.
[0076] (UV activation process) In the above-mentioned heat activation process, the azide group of the bisazide compound is decomposed by heating, but in the UV activation process, the azide group of the bisazide compound is decomposed by irradiation with ultraviolet light to form N 2 It is considered that the molecules are released, nitrene is generated, and the bisazide compound becomes suitable for bonding with materials such as resins and metals and amine polymers. The wavelength of the ultraviolet light to be irradiated is preferably 260 to 420 nm, more preferably 330 to 365 nm, from the viewpoint of ensuring adhesion and preventing deterioration of resins such as polyimide films due to ultraviolet light. Any of a mercury lamp, a metal halide lamp, and a UV-LED may be used as the ultraviolet light source. When the amine polymer in the present composition solution has a photosensitive functional group such as a (meth)acryloyl group, it is believed that the amine polymer becomes suitable for bonding with substances such as resins and metals and with bisazide compounds by ultraviolet irradiation treatment. In the present invention, the above-mentioned heat activation step may be performed in addition to the UV activation step. In that case, the order of the heat activation step and the UV activation step does not matter, and either one may be performed first, or they may be performed simultaneously. Also, the coating step, the heat activation step, and the UV activation step may be repeatedly applied in any order, either in combination with other treatments such as a post-activation cleaning treatment step (S8) for removing by-products, or without combination. By-products that do not contribute to bonding can be removed by cleaning, thereby improving adhesion.
[0077] (Pretreatment process) According to one aspect of the present invention, there can be provided a method for producing a surface-treated material, further comprising a step (pretreatment step (S1)) of subjecting the material to one or more pretreatments selected from the group consisting of cleaning treatment, acid treatment, alkali treatment, corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, silicate flame treatment (also called "Itro treatment"), and defluorination treatment, prior to the step of applying a liquid composition according to any one of the aspects of the present invention to the surface of the material. The pretreatment step is a step of pretreating the surface of a material such as a polyimide film, and is performed for the purpose of making it easier for the bisazide compound and amine polymer to be placed on the surface of the material in the subsequent coating and drying steps to be fixed to the surface, and for the purpose of efficiently performing the subsequent heat activation step and / or UV activation step. By performing the pretreatment step, the material is activated on its surface, in which functional groups such as OH groups, carboxy groups, carbonyl groups, primary amino groups, and secondary amino groups are present, and it becomes easier to form bonds with the bisazide compound and the amine polymer. The pretreatment step can be one or more treatments selected from the group consisting of cleaning treatment, acid treatment, alkali treatment, corona discharge treatment in which the surface of the material is irradiated with corona discharge, plasma treatment in which the surface of the material is treated with plasma such as argon plasma, oxygen plasma, or atmospheric plasma, ultraviolet irradiation treatment, and silicic acid flame treatment (Itro treatment) in which the surface of the material is exposed to the combustion flame of combustion gas containing a coupling agent such as a silane compound. Only one treatment may be performed, or a combination of two or more of these treatments may be performed.
[0078] <Metal-coated resin manufacturing method (wet plating)> According to one embodiment of the present invention, there is provided a method for producing a metal-coated resin, the method comprising the steps of: applying a composition liquid according to any one of the embodiments of the present invention to a surface of a resin (application step); heating the surface or irradiating the surface with ultraviolet light (activation step); and then forming a metal plating layer on the surface by wet plating (plating step). In this embodiment, a metal coating is formed on the surface of the resin that has been subjected to the coating and activation steps, for example, by electroless plating, vapor deposition, or sputtering (seed layer formation step). The metal coating may then be thickened by electrolytic plating (electrolytic plating step). The metal coating may be formed on the entire surface, or may be formed in a pattern by a known method such as photolithography. The metal-coated resin produced by this embodiment is suitable for flexible metal-clad laminates and printed wiring boards. From the viewpoint of processing time and processing cost, the thickness of the metal coating formed by electroless plating, vapor deposition, or sputtering is preferably 0.1 to 2 μm, more preferably 0.2 to 1 μm. When the metal coating is thickened by electrolytic plating, the thickness of the metal coating after thickening is preferably 0.2 to 50 μm, more preferably 0.5 to 20 μm. The metal to be electrolessly plated is, for example, Cu, Ni, etc. The metal of the metal coating formed by vapor deposition or sputtering is, for example, Al, Cr, Sn, Ti, Cu, In, Au, Pt, Ag, etc. When the metal coating includes a layer formed by electrolytic plating, the metal to be electrolytically plated is, for example, Cu, Ni, Ag, Pd, Au, Pt, Zn, Cr, Sn, Bi, etc. The metal coating may be a single metal or an alloy. In order to improve the adhesion between the resin and the plating metal of the metal-coated resin obtained by this method, an annealing treatment is preferably performed at a temperature of 100°C to 250°C for 5 to 60 minutes after the seed layer formation step and / or the electrolytic plating step.
[0079] <Metal-coated resin manufacturing method (bonding of metal foil)> According to one embodiment of the present invention, there can be provided a method for producing a metal-coated resin, comprising the steps of applying the liquid composition according to any one of the embodiments of the present invention to at least one of the surfaces of a resin and a metal foil (application step), heating the surface or irradiating the surface with ultraviolet light (activation step), and then laminating the resin and the metal foil via the surface and integrating them under pressure to obtain a metal-coated resin (pressing step). The thickness of the metal foil to be laminated is preferably 0.2 to 50 μm, more preferably 0.5 to 20 μm. Examples of metals constituting the metal foil include Cu, Ni, Ag, Pd, Au, Pt, Zn, Cr, Sn, Bi, Al, Ti, and In, and particularly Cu, Ag, Au, Pt, and Al. The metal foil may be a single metal or an alloy. The surface of the metal foil to be laminated to the resin may be roughened or not roughened. The metal-coated resin produced by this embodiment is suitable for flexible metal-clad laminates and printed wiring boards. The pressing step includes a step of overlapping the resin and the metal foil via the surface of the resin or metal foil that has been surface-treated with the present composition (overlapping step), and a step of integrally bonding the two by applying force (pressing step). In the pressing step, for example, flat plate pressing, roll pressing, or the like is performed in an air atmosphere, a nitrogen atmosphere, or a vacuum. From the viewpoint of improving productivity and reducing processing costs, flat plate pressing or roll pressing in an air atmosphere is preferable. From the viewpoint of the quality stability of the metal-coated resin produced, pressing in a nitrogen atmosphere or a vacuum is preferable. The pressing pressure is preferably 1 to 100 MPa, and more preferably 20 to 70 MPa. In general, the higher the pressing pressure, the higher the adhesion strength of the metal-coated resin produced, which is preferable, but if the pressing pressure is too high, the support may be damaged. The time for applying the pressure is, for example, 5 to 60 minutes, more preferably 10 to 20 minutes. In the pressing step, it is preferable to heat the resin at the same time. The temperature of the resin in the pressing step is set within a range not exceeding its heat resistance temperature. The temperature is, for example, 40°C or higher and 350°C or lower, preferably 120°C or higher and 250°C or lower, and more preferably 150°C or higher and 230°C or lower.
[0080] <Method of manufacturing resin laminate> According to one embodiment of the present invention, there can be provided a method for producing a resin laminate, comprising the steps of applying a composition liquid according to any one of the embodiments of the present invention to a surface of a first resin (application step), heating the surface or irradiating the surface with ultraviolet light (activation step), and then laminating a second resin on the surface and integrating them by applying pressure (pressing step). Examples of the shape of the resin include a resin film, a resin sheet, and a resin block. The pressing step includes a step of overlapping two resins via the surfaces that have been surface-treated with the present composition liquid (overlapping step), and a step of integrally bonding the two by applying force (pressing step). In the pressing step, for example, flat plate pressing, roll pressing, or the like is performed in an air atmosphere, a nitrogen atmosphere, or a vacuum. From the viewpoint of improving productivity and reducing processing costs, flat plate pressing or roll pressing in an air atmosphere is preferable. From the viewpoint of the quality stability of the resin laminate produced, pressing in a nitrogen atmosphere or a vacuum is preferable. The pressing pressure is preferably 1 to 100 MPa, and more preferably 20 to 70 MPa. In general, the higher the pressing pressure, the higher the adhesion strength of the laminate produced, which is preferable, but if the pressing pressure is too high, there is a risk of damaging the support. The time for applying the pressure is, for example, 5 to 60 minutes, more preferably 10 to 20 minutes. In the pressing step, it is preferable to simultaneously perform heating. The temperature of the resin film in the pressing step is set within a range not exceeding its heat resistance temperature. The temperature is, for example, 40°C or higher and 350°C or lower, preferably 120°C or higher and 250°C or lower, and more preferably 150°C or higher and 230°C or lower.
[0081] <Method of manufacturing resin-coated material> According to one embodiment of the present invention, there is provided a method for producing a resin-coated material, comprising the steps of applying a composition liquid according to any one of the embodiments of the present invention to a surface of a material (application step), heating the surface or irradiating the surface with ultraviolet light (activation step), then applying a resin varnish onto the surface (resin application step), and curing the varnish (curing step). In this embodiment, a resin-coated material is produced by applying a resin varnish to the surface of a material that has been subjected to the application step and activation step using this composition liquid, and then curing the resin varnish. The resin varnish is preferably made of a thermosetting or UV-curable resin. The resin-coated material produced in this embodiment has excellent adhesion. In a modified embodiment of this embodiment, the resin varnish contains a conductive filler and is applied (printed) in a pattern on the material, and the resin-coated material obtained through the curing step has a patterned conductive portion.
[0082] (Polyimide) Among resins, polyimide is a thermosetting resin with high heat resistance, and its physical properties change very little over a wide temperature range from as low as -269°C to as high as +300°C, which is why its use in the electrical and electronic fields is expanding. In the electrical field, it is used, for example, in the insulation of coils and superconducting wires in industrial motors, and in the electronic field, for example, in base films for flexible printed circuit boards, lightweight spacers, and probe sockets (test jigs) for semiconductor testing equipment.
[0083] The polyimide used as the resin in the present invention is a known substance and can be obtained by polycondensation reaction using a diamine component and a tetracarboxylic dianhydride component as the main components. A polyimide film is generally obtained by applying a polyamic acid solution obtained by reacting a diamine component with a tetracarboxylic dianhydride component in a solvent to a support, drying the resulting solution to form a green film, and further subjecting the resulting film to high-temperature heat treatment to cause a dehydration ring-closing reaction. The diamine component and tetracarboxylic dianhydride component used as raw materials are appropriately selected from the optimum ones, taking into consideration the various properties required depending on the application of the resin film laminate or metal-coated resin.
[0084] As the tetracarboxylic dianhydride component constituting the polyamic acid, aromatic tetracarboxylic dianhydrides, alicyclic tetracarboxylic dianhydrides, and aliphatic tetracarboxylic dianhydrides that are usually used in polyimide synthesis can be used. Among them, aromatic tetracarboxylic dianhydrides and alicyclic tetracarboxylic dianhydrides are preferred. From the viewpoint of heat resistance, aromatic tetracarboxylic dianhydrides are more preferred, and from the viewpoint of light transmittance, alicyclic tetracarboxylic dianhydrides are more preferred.
[0085] The aromatic tetracarboxylic acid dianhydrides are not particularly limited, but in the case where the bisazide compound has a benzene ring, from the viewpoints of affinity and ease of binding with the bisazide compound, it is preferable that the aromatic tetracarboxylic acid dianhydride is an acid dianhydride having a benzene ring or a benzene ring having a substituent, and it is more preferable that the aromatic tetracarboxylic acid dianhydride is an acid dianhydride having no aromatic ring other than a benzene ring or a benzene ring having a substituent.
[0086] Examples of aromatic tetracarboxylic dianhydrides that do not have a benzene ring or an aromatic ring other than a benzene ring having a substituent include pyromellitic dianhydride. 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 3,4,3',4'-benzophenonetetracarboxylic dianhydride, 3,4,3',4'-diphenylsulfonetetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, p-Terphenyl-3,4,3',4'-tetracarboxylic dianhydride, m-Terphenyl-3,4,3',4'-tetracarboxylic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, Examples of such anhydrides include p-quaterphenyl-3,4,3''',4'''-tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[4-(3,4-dicarboxyphenyl)phenyl]propane dianhydride, and 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride.
[0087] Examples of aromatic tetracarboxylic dianhydrides having a benzene ring or an aromatic ring other than a benzene ring having a substituent include naphthalene-2,3,6,7-tetracarboxylic dianhydride, naphthalene-1,2,5,6-tetracarboxylic dianhydride, naphthalene-1,2,6,7-tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, 1,4,5,8-tetrachloronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,7 ... naphthalene-1,4,5,8-tetracarboxylic dianhydride, 4,8-dimethyl-3,7-dihydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 4,8-dimethyl-1,5-dihydronaphthalene-2,3,6,7-tetracarboxylic dianhydride, phenanthrene-1,2,6,7-tetracarboxylic dianhydride, phenanthrene-1,2,7,8-tetracarboxylic dianhydride, perylene-2,3,8,9-tetracarboxylic dianhydride, perylene-3,4,9,10-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, and thiophene-2,3,4,5-tetracarboxylic dianhydride.
[0088] Examples of alicyclic tetracarboxylic dianhydrides include cyclobutane-1,2,3,4-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, cyclohexane-1,2,4,5-tetracarboxylic dianhydride, bicyclohexyl-3,3',4,4'-tetracarboxylic dianhydride, 1-carboxymethyl-cyclopentane-2,3,5-carboxylic-2,6:3,5-dianhydride, and pyrrolidine-2,3,4,5-tetracarboxylic dianhydride.
[0089] Examples of the aliphatic tetracarboxylic dianhydrides include ethane-1,1,2,2-tetracarboxylic dianhydride, ethylene tetracarboxylic dianhydride, propane-1,1,3,3-tetracarboxylic dianhydride, and butane-1,2,3,4-tetracarboxylic dianhydride.
[0090] The tetracarboxylic dianhydride components may be used alone or in combination of two or more kinds.
[0091] As the diamine component constituting the polyamic acid, aromatic diamines, alicyclic diamines, and aliphatic diamines that are commonly used in polyimide synthesis can be used. Among them, aromatic diamines and alicyclic diamines are preferred. From the viewpoint of heat resistance, aromatic diamines are more preferred, and from the viewpoint of light transmittance, alicyclic diamines are more preferred.
[0092] The aromatic diamines are not particularly limited, but in the case where the bisazide compound has a benzene ring, from the viewpoints of affinity and ease of binding with the bisazide compound, it is preferable that the aromatic diamine has a benzene ring or a benzene ring having a substituent, and it is more preferable that the aromatic diamine has no aromatic ring other than a benzene ring or a benzene ring having a substituent.
[0093] Examples of aromatic diamines that do not have a benzene ring or an aromatic ring other than a benzene ring having a substituent include p-phenylenediamine, m-phenylenediamine, 2,4-diaminotoluene, 4,6-dihydroxy-1,3-phenylenediamine, 3,5-diaminobenzoic acid, m-aminobenzylamine, p-aminobenzylamine, 3,3'-Dimethyl-4,4'-diaminobiphenyl, 2,2'-Dimethyl-4,4'-diaminobiphenyl, 2,2'-Bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-Dihydroxy-4,4'-diaminobiphenyl, 3,3',4,4'-Tetraaminobiphenyl, 4,4'-Diaminodiphenylmethane, 3,3'-Dicarboxy-4,4'-diaminodiphenylmethane, 3,3'-Dimethyl-4,4'-diamino-5,5'-diethyldiphenylmethane, 4,4'-Diaminodiphenyl-difluoromethane, Bis(2-methyl) 4,4'-Diaminodiphenyl ether, 3,4'-Diaminodiphenyl ether, 3,3'-Diaminodiphenyl ether, 4,4'-Diaminobenzophenone, 3,3'-Diaminobenzophenone, 4,4'-Thiodianiline, 3,3'-Thiodianiline, 4,4'-Sulfonyldianiline, 3,3'-Sulfonyldianiline, 4,4'-Diaminodiphenyl Sulfoxide, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminobenzanilide, 4,4'-diamino-1'-methoxybenzanilide, 1,3-bis(4-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)n-butane, 1,5-bis(4-aminophenoxy)n-pentane, 1,3-bis(4-aminophenoxy)-2,2-dimethylpropane, 1,2-bis[2-(4-aminophenoxy)ethoxy]ethane, 2,2-bis(3-amino-4-hydroxyphenyl )Hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis(3-aminophenyl)hexafluoropropane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)propane, 1,3-bis(4-aminophenoxy)-2,2-dimethylpropane, 5-amino-1-(4-aminophenyl)-1,3,3-trimethylindane, 3,7-diamino-dimethyldibenzothiophene-5,5-dioxide, 2,6-diaminoanthraquinone, 2,7-diaminoanthraquinone, 1,4-Diaminoanthraquinone, 1,5-Diaminoanthraquinone, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, Examples of the fluorene include 9,9-bis(4-aminophenyl)fluorene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]hexafluoropropane, and 9,10-bis(4-aminophenyl)anthracene.
[0094] Examples of aromatic diamines having a benzene ring or an aromatic ring other than a benzene ring having a substituent include 2,6-diaminonaphthalene, 2,7-diaminonaphthalene, 1,5-diaminonaphthalene, and 1,4-diaminonaphthalene.
[0095] Examples of the alicyclic diamines include 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, 1,4-diaminocyclohexane, and bis(4-amino-2,6-dimethylcyclohexyl)methane.
[0096] Examples of the aliphatic diamines include 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,8-diaminooctane, and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.
[0097] The diamine components may be used alone or in combination of two or more kinds.
[0098] The polyimide film used as the resin in the present invention is preferably one containing an aromatic ring from the viewpoint of heat resistance, and the type is not particularly limited regardless of whether it is non-thermoplastic or thermoplastic. Specific examples include non-thermoplastic polyimide films such as Kapton series manufactured by DuPont-Toray Co., Ltd., Upilex series manufactured by Ube Industries, Ltd., Apical series manufactured by Kanegafuchi Chemical Industry Co., Ltd., U-Film series manufactured by Nitto Denko Corporation, and Xenomax series manufactured by Xenomax Japan Co., Ltd. When the bisazide compound and the amine polymer have a benzene ring, a film made of a polyimide containing a benzene ring, particularly a film made of a polyimide containing only a benzene ring as an aromatic ring, can be preferably used from the viewpoint of ensuring affinity and adhesion. The glass transition temperature of the polyimide constituting the film for high heat resistance applications is preferably 300°C or higher, more preferably 350°C or higher. The thickness of the polyimide film is not particularly limited, but examples thereof include 12.5 μm, 25 μm, 30 μm, 40 μm, 50 μm, 75 μm, 100 μm, 125 μm, and 250 μm. EXAMPLES
[0099] <Synthesis Example 1> (Synthesis example of compound ET) In a glass reactor, 1 g of polyethyleneimine (trade name: Epomin (registered trademark), product number: SP-012, manufactured by Nippon Shokubai Co., Ltd., average molecular weight: 1200, amine value: 19 mmol / g, amine ratio: primary amino group 35%, secondary amino group 35%, tertiary amino group 30%) liquid was dissolved in 19 g of 3-methoxy-3-methyl-1-butanol (hereinafter referred to as "SF"). The glass reactor was purged with dry nitrogen and the internal temperature was raised to 150°C while stirring. As soon as the internal temperature reached 150°C, a solution containing 1 g of 3-(glycidoxy)propyltrimethoxysilane in 9 g of SF was added dropwise over a period of 30 minutes. The mixture was then stirred at 150°C for an additional 3 hours. After this, the reaction batch in the glass reactor was slowly cooled. A pale yellow solution with 6.7% active ingredient was obtained. When this solution was measured by gas chromatography, no signal of the raw material 3-(glycidoxy)propyltrimethoxysilane was detected, so it was determined that the reaction was complete. It can be estimated that in the target compound produced, approximately 31.8% by mole of the primary or secondary amino groups contained in the raw material polyethyleneimine were modified with silane. This compound is hereinafter referred to as "Compound ET." (See formula (7))
[0100] Example 1 (Preparation of ETBA Liquid Composition) As a "bisazide compound", powder of 2,6-bis(4'-azidobenzylidene)-4-methylcyclohexanone (trade name: BAC-M, manufactured by Toyo Gosei Co., Ltd., hereinafter referred to as "BABMC") was dissolved in methyl benzoate to prepare a 2% solution. The 2%-adjusted solution and the compound ET synthesized above as a "polymer having a repeating unit having a primary amino group or a secondary amino group and a repeating unit having a silanol group or an alkoxysilyl group" were weighed out in the required masses and mixed with ethanol to obtain a pale yellow composition solution. The concentration of each component (mass % of the total composition solution; hereinafter simply referred to as "%") was 0.2% for the bisazide compound and 0.60% for the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution will be referred to as "ETBA composition solution" below.
[0101] Example 1' (Preparation of Liquid Composition ET) The compound ET synthesized above was weighed out to the required mass and dissolved in ethanol to obtain a pale yellow composition solution. The concentration of the component was 0.60% of the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution is hereinafter referred to as "composition solution ET".
[0102] <Synthesis Example 2> (Synthesis example of compound ETG) In a glass reactor, 1 g of polyethyleneimine (ibid.) liquid was dissolved in 19 g of SF. The glass reactor was purged with dry nitrogen and the internal temperature was raised to 150° C. with stirring. As soon as the internal temperature reached 150° C., a solution containing 0.5 g of glycidyl methacrylate in 9 g of SF was added dropwise over 30 minutes. The mixture was then stirred at 150° C. for an additional 3 hours. After this, the reaction batch in the glass reactor was slowly cooled. A pale yellow solution of 5.1% active ingredient was obtained. When this solution was measured by gas chromatography, no signal of the raw material glycidyl methacrylate was detected, and therefore the reaction was deemed to be complete. It is estimated that in the target compound produced, approximately 26.5% by mole of the primary or secondary amino groups contained in the raw material polyethyleneimine had been modified. From IR analysis, it was estimated that the ratio of epoxy groups to acryloyl groups (or methacryloyl groups) in the compound produced was approximately 1:7. This compound is hereinafter referred to as "compound ETG." (See formula (8))
[0103] Example 2 (Preparation of ETGBA Solution) Powder of BABMC was dissolved in methyl benzoate as a "bisazide compound" to prepare a 2% solution. The 2% solution and the compound ETG synthesized above as a "polymer having a repeating unit having a primary amino group or a secondary amino group, a repeating unit having an epoxy group, and a repeating unit having an acryloyl group or a methacryloyl group" were weighed out in the required masses and mixed with ethanol to obtain a pale yellow composition solution. The concentration of each component was 0.20% for the bisazide compound and 0.60% for the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution will be referred to as "ETGBA composition solution" below.
[0104] Example 2' (Preparation of ETG Liquid) The compound ETG synthesized above was weighed out to the required mass and dissolved in ethanol to obtain a pale yellow composition solution. The concentration of the component was 0.60% of the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution is hereinafter referred to as "ETG composition solution".
[0105] <Synthesis Example 3> (Synthesis example of compound ETMX) In a glass reactor, 1 g of polyethyleneimine (ibid.) liquid was dissolved in 19 g of SF. The glass reactor was purged with dry nitrogen and the internal temperature was raised to 150° C. with stirring. As soon as the internal temperature reached 150° C., a solution containing 0.5 g of 3-(glycidoxy)propyltrimethoxysilane in 4.5 g of ethanol was added dropwise over 30 minutes, followed by a solution containing 0.25 g of glycidyl methacrylate in 4.5 g of ethanol over 30 minutes. The mixture was further stirred at 150° C. for 3 hours. After this, the reaction batch in the glass reactor was slowly cooled. A pale yellow solution containing 5.9% active ingredient was obtained. When this solution was measured by gas chromatography, no signals of the raw materials 3-(glycidoxy)propyltrimethoxysilane and glycidyl methacrylate were detected, and therefore the reaction was deemed to be complete. It can be estimated that in the target compound produced, approximately 29.1% by mole of the primary or secondary amino groups contained in the raw material polyethyleneimine had been modified. From IR analysis, it was estimated that the ratio of epoxy groups to acryloyl groups (or methacryloyl groups) in the compound produced was approximately 1:8. This compound is hereinafter referred to as "compound ETMX." (See formula (9))
[0106] Example 3 (Preparation of ETMXBA Solution) Powder of BABMC was dissolved in methyl benzoate as a "bisazide compound" to prepare a 2% solution. The 2% solution and the compound ETMX synthesized above as a "polymer having a repeating unit having a primary amino group or a secondary amino group, a repeating unit having a silanol group or an alkoxysilyl group, a repeating unit having an epoxy group, and a repeating unit having an acryloyl group or a methacryloyl group" were weighed out in the required masses and mixed with ethanol to obtain a pale yellow composition solution. The concentration of each component was 0.20% for the bisazide compound and 0.60% for the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution will be referred to as "composition solution ETMXBA" below.
[0107] Example 3' (Preparation of ETMX Liquid Composition) The compound ETMX synthesized above was weighed out to the required mass and mixed with ethanol to obtain a pale yellow composition solution. The concentration of the component was 0.60% of the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution will be referred to as "composition solution ETMX" below.
[0108] <Synthesis Example 4> (Synthesis example of compound ETX (organic chain type)) In a glass reactor, 1 g of polyethyleneimine (same as above) liquid was dissolved in 19 g of SF. The glass reactor was purged with dry nitrogen and the internal temperature was raised to 150° C. with stirring. As soon as the internal temperature reached 150° C., a solution containing 1 g of an organic chain-type silane coupling agent having an epoxy group and an ethoxysilyl group (product number: X-12-981S, manufactured by Shin-Etsu Chemical Co., Ltd., epoxy equivalent: 290 g / mol) in 9 g of SF was added dropwise over 30 minutes. The mixture was then stirred at 150° C. for 3 hours. After this, the reaction batch in the glass reactor was slowly cooled. A pale yellow solution containing 6.7% active ingredient was obtained. When this solution was analyzed by high performance liquid chromatography, no signal for X-12-981S was detected, and therefore the reaction was deemed complete. It can be estimated that in the target compound produced, approximately 25.9% of the primary or secondary amino groups contained in the raw polyethyleneimine were modified with silane in terms of molar ratio. This compound is hereinafter referred to as "compound ETX (organic chain type)".
[0109] Example 4 (Preparation of ETXBA (organic chain type) liquid) Powder of BABMC was dissolved in methyl benzoate as a "bisazide compound" to prepare a 2% solution. The 2% solution and the compound ETX (organic chain type) synthesized above as a "polymer having a repeating unit having a primary amino group or a secondary amino group and a repeating unit having a silanol group or an alkoxysilyl group" were weighed out in the required masses and mixed with ethanol to obtain a pale yellow composition solution. The concentration of each component was 0.20% for the bisazide compound and 0.60% for the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution will be referred to as "ETXBA (organic chain type) composition solution" below.
[0110] Example 4' (Preparation of ETX (organic chain type) liquid composition) The compound ETX (organic chain type) synthesized above was weighed out to the required mass and dissolved in ethanol to obtain a pale yellow composition solution. The concentration of the component was 0.60% of the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution will be referred to as "ETX (organic chain type) composition solution" below.
[0111] <Synthesis Example 5> (Synthesis example of compound ETKR (inorganic chain type)) In a glass reactor, 1 g of polyethyleneimine (same as above) liquid was dissolved in 19 g of SF. The glass reactor was purged with dry nitrogen and the internal temperature was raised to 150°C while stirring. As soon as the internal temperature reached 150°C, a solution containing 3 g of an inorganic chain type (polysiloxane skeleton) silane coupling agent having an epoxy group and a methoxysilyl group (product number: KR-517, Shin-Etsu Chemical Co., Ltd., epoxy equivalent: 830 g / mol) in 9 g of SF was added dropwise over 30 minutes. The mixture was then stirred at 150°C for 3 hours. After this, the reaction batch in the glass reactor was slowly cooled. A pale yellow solution containing 12.5% active ingredient was obtained. When this solution was analyzed by high performance liquid chromatography, no signal for KR-517 was detected, and therefore the reaction was deemed complete. It can be estimated that in the target compound produced, approximately 27.2% of the primary or secondary amino groups contained in the raw polyethyleneimine were modified with silane, in terms of molar ratio. This compound is hereinafter referred to as "compound ETKR (inorganic chain type)".
[0112] Example 5 (Preparation of ETKRBA (inorganic chain type) solution) Powder of BABMC was dissolved in methyl benzoate as a "bisazide compound" to prepare a 2% solution. The 2% solution and the compound ETKR (inorganic chain type) synthesized above as a "polymer having a repeating unit having a primary amino group or a secondary amino group and a repeating unit having a silanol group or an alkoxysilyl group" were weighed out in the required masses and mixed with ethanol to obtain a pale yellow composition solution. The concentration of each component was 0.20% for the bisazide compound and 0.60% for the polymer, and the pH of the composition solution measured with pH test paper was 8.0. This composition solution will be referred to as "composition solution ETKRBA (inorganic chain type)" below.
[0113] Example 5' (Preparation of ETKR (inorganic chain type) liquid composition) The compound ETKR (inorganic chain type) synthesized above was weighed out to the required mass and dissolved in ethanol to obtain a pale yellow composition solution. The concentration of the component was 0.60% of the polymer, and the pH of the composition solution measured with a pH test paper was 8.0. This composition solution is hereinafter referred to as "composition solution ETKR (inorganic chain type)".
[0114] <Comparative Example 1> (Preparation of Solution IMB-KP) A 1% ethanol solution of the compound IMB-KP was prepared according to the description of Patent Document 9. The pH was about 4.5. The compound IMB-KP is a siloxane oligomer having an amino group, an alkoxysilyl group, and an azidophenyl group. This solution is hereinafter referred to as "solution IMB-KP".
[0115] Comparative Example 2 (Preparation of Liquid Composition IMB-8) According to the description in Patent Document 8, 0.10% 4-azidobenzoic acid, 0.05% polyethyleneimine, A 10% SF solution and 0.15% maleic anhydride solution were prepared. The pH was about 4.0. This solution is hereinafter referred to as "composition solution IMB-8."
[0116] The functional groups possessed by the compounds constituting each liquid composition (or solution) are summarized in the table below. [Table 1]
[0117] <Example 6-1> (Manufacture of surface-treated resins) As the resin, two polyimide films (trade name "Kapton 200H", thickness 50 μm, manufactured by Toray DuPont Co., Ltd.) with a size of 3 cm x 6 cm were prepared. After each was washed with acetone, one side was subjected to argon plasma treatment (argon flow rate 100 mL / min, 5 min, 200 W) (pretreatment step). Next, using a bar coater, a previously prepared composition liquid ETGBA (concentration of each component: bisazide compound 0.05%, polymer 0.4%) was applied to a wet film thickness of 25 μm on the argon plasma-treated side (application step). After that, the two polyimide films were kept in a thermostatic bath at 100°C for 10 minutes (heat activation step). (Production of resin laminate) These two surface-treated polyimide films were stacked with the surface-treated sides facing each other, and were then heat-pressed with a flat plate press at a press temperature of 200°C, a press time of 5 minutes, and a press pressure of 27.2 MPa to produce a polyimide film laminate (resin laminate) (pressing step). This polyimide film laminate was placed in an oven at 250°C and left for 30 minutes (annealing step). (Peel strength measurement) After natural cooling, a 90° peel strength test was performed on the 30 mm wide polyimide film laminate. A force gauge ZTA-50N was attached to a vertical motorized test stand MX2-500N (manufactured by Imada Co., Ltd.) to configure a 90° peel strength tester. The peel speed was 50 mm / min. Of the total length of 6 cm, the peel strength was continuously measured for 4 cm, excluding 1 cm at both ends, and the average value was calculated.
[0118] <Examples 6-2 and 6-3> A polyimide film laminate was produced in the same manner as in Example 6-1, except that two sheets of polyimide film having a size of 3 cm×6 cm were used as the resin, and the average peel strength was measured. Example 6-2 Product name "Kapton EN-Y", thickness 50 μm, manufactured by Toray DuPont Co., Ltd., (Low-CTE) Example 6-3: Product name "Xenomax", thickness 38 μm, manufactured by Xenomax Japan Co., Ltd. (high heat resistance, Low-CTE)
[0119] <Comparative Examples 6-1 to 6-3> Except for using the composition liquid IMB-8 instead of the composition liquid ETGBA, polyimide film laminates were prepared in the same manner as in Examples 6-1 to 6-3, and the average peel strength was measured.
[0120] (Measurement results) The measurement results of the peel strength (average value) are as follows. Examples Comparative Examples No. 2 resins Liquid composition ETGBA Liquid composition IMB-8 6-1 Kapton H200 Base material destruction Base material destruction 6-2 Kapton EN-Y 6.0N / 3cm 1.5N / 3cm 6-3 Xenomax 27.0N / 3cm 0.0N / 3cm (Consideration) As can be seen from Examples 6-1 to 6-3, the composition liquid ETGBA according to the present invention can obtain adhesion to all polyimide resins. On the other hand, as can be seen from Comparative Examples 6-1 to 6-3, the composition liquid IMB-8 can obtain adhesion only with Kapton 200H. Note that "base material destruction" means that during the 90° peel strength test, peeling does not occur inside the condensate layer derived from the applied composition liquid, but peeling occurs due to destruction of the base material (polyimide film). "Base material destruction" indicates that the bond related to the interfacial molecular bond between two substances is strong.
[0121] <Example 6-1'> A polyimide film laminate was prepared and the average peel strength was measured in the same manner as in Example 6-1, except that air drying and UV activation steps were performed instead of the heat activation step in Example 6-1. In the UV activation step, the UV irradiation device was used to irradiate the polyimide film laminate with an irradiation energy of 1000 mJ / cm. 2 The coated surface was irradiated with ultraviolet light. As a result, similar to Example 6-1, adhesion strong enough to cause destruction of the base material was obtained.
[0122] <Example 7-1> (Production of metal-coated resin by plating) One sheet of the same polyimide film as in Example 6-1 was prepared, and one side of the film was subjected to the same surface treatment as in Example 1 using the same composition liquid as in Example 6-1, except that the heat activation treatment was changed to 160° C. for 10 minutes. Next, the electroless plating process was carried out using the surface-treated polyimide film as a sample. In the electroless plating process, the sample was immersed in a pre-dip solution for pre-dip treatment, followed by immersing the sample in Inducer AM (manufactured by Okuno Chemical Industries Co., Ltd.) for catalyst application treatment, followed by immersing the sample in OPC-150 Crystal RW (manufactured by Okuno Chemical Industries Co., Ltd.) for accelerator treatment, followed by electroless plating treatment for electrolessly plating the sample with copper, followed by post-electroless plating annealing treatment for keeping the sample at a temperature of 100°C for 30 minutes to reduce plating stress. The plating thickness of the electroless plating was 0.1 μm. Next, an electrolytic plating process was carried out to apply electrolytic copper plating to the sample for thick plating. The thickness of the plating film was 20 μm. Next, in order to reduce plating stress, an annealing process was carried out after electrolytic plating in which the sample was kept at a temperature of 150° C. for 30 minutes. Thus, a metal-coated polyimide film was obtained. Thereafter, the metal-coated polyimide film was cut to a width of 10 mm, and the peel strength (average value) was measured in the same manner as in Example 6-1. The solution used in the above catalyst application process was an alkaline Pd catalyst-containing solution, which is suitable for forming fine wiring.
[0123] <Examples 7-2 to 7-5> A metal-coated polyimide film was prepared by plating in the same manner as in Example 7-1, except that the liquid composition ET, ETBA, ETMXBA or ETKRBA according to the present invention was used instead of the liquid composition ETGBA used in Example 7-1, and the peel strength (average value) was measured.
[0124] <Comparative Examples 7-1 and 7-2> A metal-coated polyimide film was prepared by plating in the same manner as in Example 7-1, except that the composition liquid IMB-8 or the solution IMB-KP, which is another composition liquid according to the comparative example, was used instead of the composition liquid ETGBA used in Example 7-1, and the peel strength (average value) was measured.
[0125] (Measurement results) The measurement results of the peel strength (average value) are as follows. Code Liquid composition Resin Peel strength Example 7-1 ETGBA Kapton H200 4.3N / cm Example 7-2 ET Same as above 3.5N / cm Example 7-3 ETBA Same as above 6.0N / cm Example 7-4 ETMXBA Same as above 5.0N / cm Comparative example 7-1 IMB-8 Same as above 4.5N / cm Comparative example 7-2 IMB-KP Same as above 3.5N / cm (Consideration) These five examples show adhesion equal to or better than the two comparative examples. A comparison of the ET and ETBA liquid compositions shows that the addition of a bisazide compound to the liquid composition improves adhesion. A comparison of the ETBA, ETMXBA, and ETGBA liquid compositions shows that the silanol group improves plating adhesion. Comparative example 7-2 has a liquid composition with a pH of about 4.5, which is on the acidic side, and is therefore presumed to have poor adhesion with alkaline Pd plating. In contrast, the five examples have a pH of about 8.0, which is on the alkaline side, and therefore are compatible with alkaline Pd plating, which is suitable for fine wiring.
[0126] <Examples 7-1' to 7-4'> An OPP film laminate was produced in the same manner as in Examples 7-1 to 7-4, except that the air drying and UV activation steps were carried out instead of the heat activation step in Examples 7-1 to 7-4, biaxially oriented polypropylene (OPP) was used instead of Kapton H200 as the resin, and the electrolytic annealing conditions were changed to 100°C and 60 minutes. In the UV activation step, the UV irradiation device was used to irradiate the OPP film with an energy of 1000 mJ / cm2.2 The coated surface was irradiated with ultraviolet light at 7-1' to 7-4'. As a result, similar to Examples 7-1 to 7-4, good plating adhesion was confirmed.
[0127] <Example 8-1> (Production of metal-coated resin by lamination) A sheet of the following polyimide film measuring 6 cm x 3 cm and unroughened copper foil were prepared. Example 8-1 Product name "Kapton EN", thickness 25 μm, manufactured by Toray DuPont Co., Ltd., (Low-CTE) Unroughened copper foil, thickness 12μm, surface roughness Sa0.19μm, manufactured by Fukuda Metal Foil & Powder Co., Ltd. One side of the polyimide film was subjected to the same surface treatment as in Example 7-1 using the same composition liquid as in Example 7-1. The copper foil was not subjected to the surface treatment. Next, the above-mentioned surface-treated polyimide film and copper foil were laminated. The above-mentioned copper foil was placed on the surface-treated side of the surface-treated polyimide film, and the copper foil was heated and pressed with a flat press at a press temperature of 230°C, a press time of 5 minutes, and a press pressure of 58.3 MPa via cushion plates attached above and below to produce a metal-coated polyimide film (pressing step). After natural cooling, the metal-coated polyimide film was cut to a width of 10 mm without performing an annealing step, and the peel strength was measured in the same manner as in Example 6-1.
[0128] <Examples 8-2 to 8-4> A metal-coated polyimide film was prepared by lamination in the same manner as in Example 8-1, except that the ETGBA liquid used in Example 8-1 was replaced with another liquid composition according to the present invention, that is, liquid composition ETBA, liquid composition ETMXBA, or liquid composition ETXBA, and the peel strength (average value) was measured.
[0129] <Comparative Examples 8-1 and 8-2> Except for using the composition liquid IMB-8 or solution IMB-KP, which are other composition liquids according to comparative examples, instead of the composition liquid ETGBA used in Example 8-1, a metal-coated polyimide film was prepared by lamination in the same manner as in Example 8-1, and the peel strength (average value) was measured.
[0130] <Examples 8-5 and 8-6> Except for using another polyimide film, "Xenomax", instead of the resin (polyimide film "Kapton EN") used in Example 8-1, a metal-coated polyimide film was prepared by lamination in the same manner as in Example 8-1, and the peel strength (average value) was measured.
[0131] <Comparative Examples 8-3 and 8-4> Except for using the polyimide film "Xenomax" instead of the polyimide film "Kapton EN" used in Comparative Examples 8-1 and 8-2, metal-coated polyimide films were prepared by lamination in the same manner as in Comparative Examples 8-1 and 8-2, and the peel strength (average value) was measured.
[0132] (Measurement results) The measurement results of the peel strength (average value) are as follows. Code Liquid composition Resin Peel strength Example 8-1 ETGBA Kapton EN 6.0N / cm Example 8-2 ETBA Kapton EN 7.0N / cm Example 8-3 ETMXBA Kapton EN 7.0N / cm Example 8-4 ETXBA Kapton EN 7.0N / cm *) Example 8-5 ETKRBA Kapton EN 6.8N / cm Comparative Example 8-1 IMB-8 Kapton EN 0.0N / cm Comparative Example 8-2 IMB-KP Kapton EN 8.0N / cm Example 8-5 ETBA Xenomax 4.5N / cm Example 8-6 ETXBA Xenomax 5.0N / cm Comparative Example 8-3 IMB-8 Xenomax 0.0N / cm Comparative Example 8-4 IMB-KP Xenomax 3.5N / cm *) In Example 8-4, strong adhesion of 15.0 N / cm was observed in some of the samples. (Consideration) The comparative liquid composition IMB-8 has poor adhesion, but the IMB-KP solution has high adhesion. The examples according to the present invention show similar adhesion to Kapton EN, although it is slightly lower than the IMB-KP solution according to the comparative example. The examples according to the present invention also show higher adhesion to Xenomax than the IMB-KP solution according to the comparative example. In Example 8-4, which uses a liquid composition containing a polymer having a repeating unit with an organic chain in the side chain, strong adhesion was observed in some of the samples.
[0133] (Dependence on coating thickness) In Example 8-3, the relationship between the coating thickness (wet thickness) when the composition liquid ETMXBA was applied to the polyimide film and the peel strength was investigated. The results are as follows. Coating thickness (wet thickness) Peel strength 1.5μm 3.5N / cm 7.0μm 6.0N / cm 12.0μm 6.0N / cm 25.0μm 6.0N / cm When the coating thickness is less than 7 μm, the thinner the coating thickness, the lower the peel strength becomes, whereas when the coating thickness is 7 μm or more and 25.0 μm or less, the peel strength does not change.
[0134] <Example 9> (Preparation of resin-coated material) (Surface treatment) A silicon wafer was prepared and washed with ethanol. Next, a previously prepared composition liquid ETBA (concentration of each component was 0.05% bisazide compound, 0.4% polymer) was applied to one side of the silicon wafer with a wet film thickness of 25 μm using a bar coater (application step). After that, the silicon wafer was kept in a thermostatic bath at 100° C. for 10 minutes (heat activation step). (Manufacture of resin-coated materials) Polyimide varnish (UPIA AT, Ube Industries, solids concentration 18±1%, viscosity 5±1 Pa·s, solvent NMP, heat curing conditions 350°C 20 minutes) was prepared and spin-coated (1500 rpm, 20 seconds) onto the above-mentioned coated surface of the silicon wafer. Next, heat treatment was performed under the recommended heat curing conditions for the polyimide varnish to harden the polyimide varnish. After that, cuts were made into 1 mm wide 5 × 5 squares in the resulting coating film, and a tape peeling test (cross-cut test) was performed to confirm the number of adhesions of the lattice (= 25 - number of peels). The number of adhesions was 25, and the coating thickness was 33 μm.
[0135] <Comparative Examples 9-1 and 9-2> A silicon wafer similar to that of Example 9 was prepared, and a coating film was formed on the silicon wafer in the same manner as in Example 9, except that the composition liquid ETBA was replaced with the following composition liquid (or no composition liquid was used at all). Thereafter, the adhesion of the coating film was confirmed by a tape peeling test. The results are as follows, and it was confirmed that the composition liquid ETBA according to the present invention had the same adhesion improving effect as Comparative Example 9-1. (result) Code Liquid composition Film thickness Number of contacts Example 9 ETBA 33μm 25 Comparative example 9-1 IMB-KP 29μm 25 Comparative Example 9-2 None 20μm 0 [Industrial Applicability]
[0136] The composition liquid of the present invention can be used mainly in the neutral to alkaline pH range, and can improve the adhesion between various substances by interfacial molecular bonding, so it can be used in many applications. In particular, it can be widely applied in the electrical and electronic fields. For example, it can be used in the manufacture of electrical and electronic devices such as printed wiring boards, lightweight spacers, probe sockets (test jigs) for semiconductor testing equipment, and resin core metal foils for battery plates. [Explanation of symbols]
[0137] 1. Laminate 2,4,5 substances 3. Condensate layer A1-A4 Bisazide compound-derived moiety P1, P2 Polymer (polymer amine) S1 Pretreatment process S2 coating process S4 Heat activation process S6 UV activation process S8 Post-activation cleaning process S3, S5, S7, S9 Branching decision steps
Claims
1. A composition liquid to be applied to at least one of two substances for the purpose of improving the adhesion between the two substances, A polymer comprising a first repeating unit having a primary amino group or a secondary amino group, and a second repeating unit having one or more functional groups selected from the group consisting of a silanol group, an alkoxysilyl group, an epoxy group, an acryloyl group, and a methacryloyl group; A bisazide compound; A liquid composition comprising:
2. The liquid composition according to claim 1 , wherein the second repeating unit has a silanol group or an alkoxysilyl group.
3. A composition liquid that is applied to the material to be plated in order to improve the adhesion of the plating, A polymer comprising a first repeating unit having a primary amino group or a secondary amino group, and a second repeating unit having a silanol group or an alkoxysilyl group. A liquid composition comprising:
4. 4. The liquid composition according to claim 1, 2 or 3, wherein the polymer has a second repeating unit having one or more functional groups selected from the group consisting of an epoxy group, an acryloyl group and a methacryloyl group.
5. The liquid composition according to claim 2 or 3, wherein the second repeating unit includes a polysiloxane skeleton.
6. The liquid composition according to claim 1 , 2 or 3 , wherein the polymer has a polyethyleneimine structure.
7. 3. The liquid composition according to claim 1, wherein at least two of the azide groups contained in the bisazide compound are azide groups directly bonded to an aromatic ring.
8. A method for producing a surface-treated substance, comprising a step of applying the liquid composition according to claim 1 to the surface of a substance (application step).
9. A step of applying the composition liquid according to claim 1, 2 or 3 to a surface of a resin (application step); a step of heating the surface or irradiating the surface with ultraviolet light (activation step); Next, a step of forming a metal plating layer on the surface by wet plating (plating step); A method for producing a metal-coated resin comprising the steps of:
10. A step of applying the composition liquid according to claim 1 to at least one of a surface of a resin and a surface of a metal foil (application step); a step of heating the surface or irradiating the surface with ultraviolet light (activation step); Next, a step of laminating the resin and the metal foil via the surface and pressing them together (a pressing step); A method for producing a metal-coated resin comprising the steps of:
11. A step of applying the composition liquid according to claim 1 to a surface of a first resin (application step); a step of heating the surface or irradiating the surface with ultraviolet light (activation step); Next, a step of laminating a second resin on the surface and integrating it by pressing (pressing step); A method for producing a resin laminate comprising the steps of:
12. A step of applying the composition liquid according to claim 1 to a surface of a substance (application step); a step of heating the surface or irradiating the surface with ultraviolet light (activation step); Next, a step of applying a resin varnish onto the surface (resin application step); A step of curing the varnish (curing step); A method for producing a resin-coated material comprising the steps of:
Citation Information
Patent Citations
Reactive Silicone / Alkyleneimine Barrier Lamination Adhesives and Their Applications
JP2001514583A
Compositions, methods for making articles, and articles
JP2019519633A
Surface treatment method, surface treatment agent, production method of conjugate, production method of substance with conductor coating, production method of substance with coating film, and compound
JP2022048068A
Resin film laminate, its manufacturing method, and metal-coated resin manufacturing method
JP7120695B1
Insulating materials containing cycloolefinic polymers
WO1998056011A1
Cited By
Adhesive for resin material having low dielectric properties, and laminate
JP2025103973A
Adhesive for resin material having low dielectric properties, and laminate
WO2025142345A1