Photocurable composition for adhesive sheet, adhesive sheet, optical laminate, and image display device
The combination of photopolymerization initiators with varying reaction rates in a photocurable composition addresses peeling and foaming issues in adhesive sheets for image display devices, ensuring reliable performance in high-temperature conditions.
Patent Information
- Application Number
- JP2024039511
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-15
AI Technical Summary
Photocurable pressure-sensitive adhesive sheets used in image display devices face issues with image quality deterioration due to peeling and foaming in high-temperature environments.
A photocurable composition is developed using a combination of photopolymerization initiators with different reaction rates, specifically a first photoinitiator with a relatively small reaction rate and a second photoinitiator with a larger reaction rate, where the ratio of the second reaction rate to the first is 1.1 or more, to enhance polymerization and molecular weight, reducing peeling and foaming.
The solution results in a pressure-sensitive adhesive sheet suitable for high-temperature environments, minimizing peeling and foaming, thereby maintaining image quality in image display devices.
Smart Images

Figure 2024146806000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a photocurable composition for a pressure-sensitive adhesive sheet, a pressure-sensitive adhesive sheet, an optical laminate, and an image display device. [Background technology]
[0002] Various image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices, generally include an optical laminate including an optical film such as a polarizing film and an adhesive sheet. An adhesive sheet is usually used for bonding between the optical films included in the optical laminate and for bonding between the optical laminate and an image display panel. A typical adhesive sheet is a sheet obtained by curing a monomer group including an acrylic monomer, a silicone monomer, etc., by polymerization and crosslinking. Patent Document 1 discloses an adhesive sheet formed from a photocurable composition (hereinafter referred to as a photocurable adhesive sheet). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-70150 A Summary of the Invention [Problem to be solved by the invention]
[0004] When a photocurable pressure-sensitive adhesive sheet is used in an optical laminate, problems tend to occur in the quality of images displayed in an image display device that may be exposed to a high-temperature environment.
[0005] An object of the present invention is to provide a pressure-sensitive adhesive sheet suitable for use in an image display device that may be exposed to a high-temperature environment, and a photocurable composition capable of forming the pressure-sensitive adhesive sheet. [Means for solving the problem]
[0006] The present inventors have focused on the photopolymerization initiator contained in the photocurable composition and found that the above-mentioned problems can be solved by combining photopolymerization initiators having different reaction rates.
[0007] That is, the present invention provides: The composition includes a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator, the first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively; The ratio of the second reaction rate to the first reaction rate is 1.1 or more, expressed as a ratio of polymerization rates A evaluated by the following measurement method using only each of the photopolymerization initiators. A photocurable composition for pressure-sensitive adhesive sheets is provided. [Measurement method] A mixed solution of 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of a photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The ultraviolet light irradiation is continued until the viscosity of the mixed solution at 30°C reaches 20 Pa·s. Next, a coating layer of 20 μm thickness made of the prepared monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets, each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED having a peak wavelength of 340 nm±10 nm from the side of one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are, respectively, 4 mW / cm. 2 and 1200 seconds. The polymerization rate of the monomer measured for the coating layer photocured by the irradiation of ultraviolet light is specified as the polymerization rate A.
[0008] Further, the present invention relates to There is provided a pressure-sensitive adhesive sheet formed from the above photocurable composition.
[0009] Further, the present invention relates to There is provided an optical laminate comprising the above pressure-sensitive adhesive sheet and an optical film.
[0010] Further, the present invention relates to There is provided an image display device including the above optical laminate. Effect of the Invention
[0011] According to the present invention, it is possible to provide a pressure-sensitive adhesive sheet suitable for use in an image display device that may be exposed to a high-temperature environment, and a photocurable composition capable of forming the pressure-sensitive adhesive sheet. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view illustrating a schematic example of a pressure-sensitive adhesive sheet of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a method for forming the pressure-sensitive adhesive sheet of the present invention from the photocurable composition of the present invention. [Diagram 3] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Figure 4] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Diagram 5] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Figure 6] FIG. 1 is a cross-sectional view illustrating an example of an optical laminate of the present invention. [Figure 7] FIG. 1 is a cross-sectional view that illustrates an example of an image display device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The photocurable composition according to the first aspect of the present invention comprises: The composition includes a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator, the first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively; The ratio of the second reaction rate to the first reaction rate is 1.1 or more, expressed as a ratio of the polymerization rate A evaluated by the following measurement method using only each of the photopolymerization initiators. [Measurement method] A mixed solution of 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of a photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The ultraviolet light irradiation is continued until the viscosity of the mixed solution at 30°C reaches 20 Pa·s. Next, a coating layer of 20 μm thickness made of the prepared monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets, each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED having a peak wavelength of 340 nm±10 nm from the side of one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are, respectively, 4 mW / cm. 2 and 1200 seconds. The polymerization rate of the monomer measured for the coating layer photocured by the irradiation of ultraviolet light is specified as the polymerization rate A.
[0014] In a second aspect of the present invention, for example, in the photocurable composition according to the first aspect, the polymerization rate A of the first photopolymerization initiator is 80% or less, and the polymerization rate A of the second photopolymerization initiator is 90% or more.
[0015] In a third aspect of the present invention, for example, in the photocurable composition according to the first or second aspect, the first photopolymerization initiator is an α-hydroxyacetophenone-based compound.
[0016] In a fourth aspect of the present invention, for example, in the photocurable composition according to any one of the first to third aspects, the first photopolymerization initiator has one α-hydroxyacetophenone structure in one molecule.
[0017] In a fifth aspect of the present invention, for example, in the photocurable composition according to any one of the first to fourth aspects, the second photopolymerization initiator is an α-hydroxyacetophenone-based compound.
[0018] In a sixth aspect of the present invention, for example, in the photocurable composition according to any one of the first to fifth aspects, the first photopolymerization initiator is 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone.
[0019] In a seventh aspect of the present invention, for example, in the photocurable composition according to any one of the first to sixth aspects, the monomer group includes a (meth)acrylic monomer.
[0020] An adhesive sheet according to an eighth aspect of the present invention is an adhesive sheet formed from the photocurable composition according to any one of the first to seventh aspects.
[0021] In a ninth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet according to the eighth aspect, the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 97% or more, and the weight average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet exceeds 700,000.
[0022] In a tenth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet according to the eighth or ninth aspect, the pressure-sensitive adhesive sheet has a thickness of 300 μm or less.
[0023] An optical laminate according to an eleventh aspect of the present invention comprises the pressure-sensitive adhesive sheet according to any one of the eighth to tenth aspects, and an optical film.
[0024] In a twelfth aspect of the present invention, for example, in the optical laminate according to the eleventh aspect, the optical film is a polarizing film, and the pressure-sensitive adhesive sheet is in contact with the polarizing film.
[0025] An image display device according to a thirteenth aspect of the present invention comprises the optical laminate according to the eleventh or twelfth aspect.
[0026] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in any manner without departing from the gist of the present invention.
[0027] [Photocurable composition] The photocurable composition of this embodiment includes a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator. The photocurable composition of this embodiment is for an adhesive sheet. An adhesive sheet can be formed from the photocurable composition of this embodiment.
[0028] (Photopolymerization initiator) The first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively. The reaction rate of each photopolymerization initiator can be specified by the polymerization rate reached when the monomer is polymerized using only the photopolymerization initiator. The ratio of the second reaction rate to the first reaction rate is 1.1 or more, expressed by the ratio of the polymerization rate A evaluated by the following measurement method using only each photopolymerization initiator. The ratio of the polymerization rate A may be 1.15 or more, 1.2 or more, 1.22 or more, 1.25 or more, or even 1.27 or more. The upper limit of the ratio is not particularly limited, but is, for example, 3 or less. The ratio of the polymerization rate A is specified by [polymerization rate A when only the second photopolymerization initiator is used] / [polymerization rate A when only the first photopolymerization initiator is used]. [Measurement method] A mixed solution of 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of the photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The ultraviolet light irradiation is continued until the viscosity of the mixed solution at 30°C reaches 20 Pa·s. Next, a coating layer of 20 μm thickness made of the prepared monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets, each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED having a peak wavelength of 340 nm ± 10 nm from the side of one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are 4 mW / cm2, respectively. 2 and 1200 seconds. The polymerization rate of the monomer measured for the coating layer photocured by irradiation with ultraviolet light is specified as the polymerization rate A.
[0029] According to the study by the present inventors, it was found that one of the factors of the deterioration of image quality due to exposure to a high temperature environment is that the adhesive sheet in the optical laminate and the optical film in contact therewith, typically a polarizing film, tend to peel off at high temperatures. In addition, the deterioration of visibility due to the monomer remaining in the adhesive sheet foaming at high temperatures can also be a factor. The combination of the first and second photopolymerization initiators makes the polymerization state at the time of forming the adhesive sheet suitable for increasing both the molecular weight and the polymerization rate of the polymer. It is considered that the peeling is caused by the contraction of the optical film at high temperatures, but the highly molecular weight polymer can improve the stress relaxation property of the adhesive sheet and can resist peeling. It is presumed that the combination of the first and second photopolymerization initiators makes the state of generation and movement of radicals in the polymerization system suitable for the progress of the polymerization. The composition of the monomer syrup used to evaluate the polymerization rate A is known as a general composition for forming an acrylic adhesive sheet. In addition, the above-mentioned ultraviolet irradiation conditions are suitable for evaluating the state of polymerization.
[0030] The polymerization rate A of the first photopolymerization initiator may be 80% or less, 79% or less, or even 78% or less. The lower limit of the polymerization rate A is, for example, 65% or more, and may be 66% or more, 67% or more, 68% or more, 69% or more, or even 70% or more.
[0031] The polymerization rate A of the second photopolymerization initiator may be 90% or more, 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, 96% or more, 97% or more, 98% or more, or even 99% or more. The upper limit of the polymerization rate A is, for example, 99.9% or less, or even 99.5% or less.
[0032] The polymerization rate A of the first photopolymerization initiator and the polymerization rate A of the second photopolymerization initiator may simultaneously satisfy the above-mentioned ranges. For example, the polymerization rate A of the first photopolymerization initiator may be 80% or less, and the polymerization rate A of the second photopolymerization initiator may be 90% or more.
[0033] Examples of the first and second photopolymerization initiators include benzoyl ethers, substituted benzoyl ether compounds, substituted acetophenone compounds, α-hydroxyacetophenone compounds, substituted alpha-ketol compounds, aromatic sulfonyl chloride compounds, photoactive oximes, benzophenone compounds, thioxanthone compounds, triazine compounds, oxime ester compounds, phosphine compounds, quinone compounds, borate compounds, carbazole compounds, imidazole compounds, and titanocene compounds.
[0034] The first photopolymerization initiator is preferably an α-hydroxyacetophenone compound. The first photopolymerization initiator, which is an α-hydroxyacetophenone compound, is particularly suitable for increasing the molecular weight of a polymer in combination with a second photopolymerization initiator. The number of α-hydroxyacetophenone structures in one molecule of the first photopolymerization initiator is, for example, 1 to 3, preferably 1 or 2, and more preferably 1.
[0035] A specific example of the first photoinitiator is 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone, which is an α-hydroxyacetophenone compound and is commercially available as Omnirad 2959 (manufactured by IGM Resins).
[0036] The second photopolymerization initiator is not limited, and may be an α-hydroxyacetophenone compound. The second photopolymerization initiator, which is an α-hydroxyacetophenone compound, is particularly suitable for increasing the molecular weight of the polymer in combination with the first photopolymerization initiator, particularly the first photopolymerization initiator, which is an α-hydroxyacetophenone compound. The number of α-hydroxyacetophenone structures in one molecule of the second photopolymerization initiator is, for example, 1 to 3, preferably 1 or 2, and more preferably 2.
[0037] The photocurable composition may include one or more first photoinitiators. The photocurable composition may include one or more second photoinitiators.
[0038] The amount of the photopolymerization initiator in the photocurable composition is 0.01 to 1 part by weight per 100 parts by weight of the total of the monomer group and the partial polymer, in terms of the total of all the photopolymerization initiators including the first and second photopolymerization initiators. The upper limit of the amount may be 0.9 parts by weight or less, 0.8 parts by weight or less, 0.7 parts by weight or less, 0.6 parts by weight or less, 0.5 parts by weight or less, 0.4 parts by weight or less, 0.3 parts by weight or less, 0.25 parts by weight or less, or even 0.2 parts by weight or less. The lower limit of the amount may be 0.05 parts by weight or more, 0.08 parts by weight or more, 0.1 parts by weight or more, or even 0.15 parts by weight or more.
[0039] The ratio of the amount X1 of the first photopolymerization initiator to the amount X2 of the second photopolymerization initiator is, for example, 5:1 to 1:5, and may be 4:1 to 1:4, 3:1 to 1:3, 2:1 to 1:2, or even 1.5:1 to 1:1.5, in weight ratio.
[0040] The ratio of the remaining amounts B of the first and second photopolymerization initiators evaluated by the following measurement method B is, for example, 0.6 or less, and may be 0.55 or less, or even 0.5 or less. The lower limit of the ratio may be, for example, 0.01 or more. The ratio of the remaining amounts B is specified by [the remaining amount B when only the second photopolymerization initiator is used] / [the remaining amount B when only the first photopolymerization initiator is used]. [Measurement method B] A mixed solution of 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers, and 0.1 parts by weight of a photopolymerization initiator to be evaluated, is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The ultraviolet light irradiation is continued until the viscosity of the mixed solution at 30°C reaches 20 Pa·s. Next, a coating layer of 20 μm thickness made of the prepared monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets, each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED having a peak wavelength of 340 nm±10 nm from the side of one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are 14 mW / cm2, respectively. 2 and 100 seconds. The remaining amount B is determined as the remaining amount of the photopolymerization initiator measured for the coating layer photocured by the irradiation of the ultraviolet rays.
[0041] In addition, regardless of the ratio of the polymerization rate A, by using a combination of the first photopolymerization initiator and the second photopolymerization initiator in which the ratio of the residual amount B is within the above range, it is possible to make the polymerization state during the formation of the pressure-sensitive adhesive sheet suitable for increasing the molecular weight of the polymer. The composition includes a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator, the first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively; The photocurable composition for pressure-sensitive adhesive sheets has a ratio of the second reaction rate to the first reaction rate, which is expressed as a ratio of the remaining amount B evaluated by the above-mentioned measurement method B using only each of the photopolymerization initiators, of 0.6 or less.
[0042] (Monomer group) The monomer group may contain a (meth)acrylic monomer. The content of the (meth)acrylic component in the photocurable composition, i.e., the (meth)acrylic monomer and its partial polymer, may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, an acrylic adhesive sheet mainly composed of a (meth)acrylic polymer and its crosslinked product can be formed. However, the photocurable composition is not limited to the above examples. In this specification, (meth)acrylic means acrylic and methacrylic. (Meth)acrylate means acrylate and methacrylate.
[0043] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and the like. acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate (lauryl (meth)acrylate), n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate and octadecyl (meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl (meth)acrylate.
[0044] The content of the (meth)acrylic acid alkyl ester in the monomer group is, for example, 40% by weight or more, and may be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or even 95% by weight or more. In calculating the content, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.
[0045] The monomer group may contain a carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a carboxyl group-containing monomer. Examples of the carboxyl group-containing monomer are (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The content of the carboxyl group-containing monomer in the monomer group may be, for example, 10% by weight or less, 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5.5% by weight or less, or even 5% by weight or less. The lower limit of the content may be, for example, 0.1% by weight or more, 0.5% by weight or more, or even 1% by weight or more. The monomer group may not contain a carboxyl group-containing monomer.
[0046] The monomer group may contain a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a hydroxyl group-containing monomer. The hydroxyl group-containing monomer may contribute to improving the cohesive strength of the adhesive sheet. Examples of the hydroxyl group-containing monomer are 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxyl group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. The content of the hydroxyl group-containing monomer in the monomer group is, for example, 10% by weight or less, and may be 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.5% by weight or less, 0.3% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less. The lower limit of the content may be, for example, 0.01% by weight or more, 0.03% by weight or more, or even 0.05% by weight or more. The monomer group may not contain a hydroxyl group-containing monomer.
[0047] The monomer group may include a nitrogen atom-containing monomer. The nitrogen atom-containing monomer means a monomer having at least one nitrogen atom in the molecule (per molecule).
[0048] As the nitrogen atom-containing monomer, from the viewpoint of improving foaming and peeling resistance, N-vinyl cyclic amide, (meth)acrylamide, etc. are preferable. The nitrogen atom-containing monomer may be used alone or in combination of two or more kinds.
[0049] The N-vinyl cyclic amide is preferably represented by the following formula (1). [ka]
[0050] In formula (1), R 1 is a divalent organic group, preferably a divalent saturated or unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (e.g., an alkylene group having 3 to 5 carbon atoms). 1 are directly bonded via a single bond to form a ring structure.
[0051] As the N-vinyl cyclic amide represented by formula (1), from the viewpoint of improving foaming and peeling resistance, N-vinyl-2-pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-morpholinone, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, etc. are preferred, more preferably N-vinyl-2-pyrrolidone, N-vinyl-2-caprolactam, and even more preferably N-vinyl-2-pyrrolidone.
[0052] Examples of (meth)acrylamides include (meth)acrylamide, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide, etc. Examples of N-alkyl(meth)acrylamide include N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, Nn-butyl(meth)acrylamide, N-octylacrylamide, etc. Examples of N-alkyl(meth)acrylamides include (meth)acrylamides having an amino group, such as dimethylaminoethyl(meth)acrylamide, diethylaminoethyl(meth)acrylamide, and dimethylaminopropyl(meth)acrylamide.
[0053] Examples of N,N-dialkyl(meth)acrylamides include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide.
[0054] (Meth)acrylamides also include, for example, various N-hydroxyalkyl (meth)acrylamides. Examples of N-hydroxyalkyl (meth)acrylamides include N-methylol (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, and N-methyl-N-2-hydroxyethyl (meth)acrylamide.
[0055] (Meth)acrylamides also include, for example, various N-alkoxyalkyl(meth)acrylamides, such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide.
[0056] Examples of nitrogen atom-containing monomers other than N-vinyl cyclic amides and (meth)acrylamides include amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; cyano group-containing monomers such as acrylonitrile and methacrylonitrile; (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyloxazole, vinylisoxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine, N-methyl Examples of the monomer include heterocyclic ring-containing monomers such as vinylpyrrolidone; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, and N-cyclohexylitaconimide; and succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; and other imide group-containing monomers; and isocyanate group-containing monomers such as 2-(meth)acryloyloxyethylisocyanate.
[0057] The content of the nitrogen atom-containing monomer in the monomer group is, for example, 40% by weight or less, and may be 35% by weight or less, 30% by weight or less, 25% by weight or less, 20% by weight or less, 15% by weight or less, 13% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, or even 5% by weight or less. The lower limit of the content is, for example, 0.5% by weight or more, and may be 1% by weight or more, 2% by weight or more, 3% by weight or more, 4% by weight or more, 5% by weight or more, 7% by weight or more, or even 10% by weight or more. The monomer group may not contain a nitrogen atom-containing monomer.
[0058] The monomer group may include monomers other than those mentioned above.
[0059] In the photocurable composition, each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The photocurable composition may not contain a partial polymer.
[0060] The photocurable composition may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. An example of the polyfunctional monomer is a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, methylol groups, etc. in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.
[0061] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N DDA), 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and other polyfunctional acrylates (such as ester compounds of polyhydric alcohols and (meth)acrylic acid); allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably 1,9-nonanediol diacrylate, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0062] The amount of the crosslinking agent to be added varies depending on the molecular weight, the number of functional groups, etc., but may be, for example, 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, or even 0.3 parts by weight or less, based on 100 parts by weight of the total of the monomer group and its partial polymer. The lower limit of the amount to be added is, for example, 0.01 parts by weight or more, or even 0.05 parts by weight or more. The photocurable composition may not contain a crosslinking agent.
[0063] The photocurable composition may contain additives other than those described above. Examples of additives include chain transfer agents, silane coupling agents, viscosity modifiers, tackifiers, plasticizers, softeners, antioxidants, fillers, colorants, antioxidants, surfactants, antistatic agents, and ultraviolet absorbing agents. The photocurable composition may not contain additives.
[0064] The viscosity of the photocurable composition is preferably 5 to 100 poise. A photocurable composition having a viscosity in the above range is particularly suitable for forming a pressure-sensitive adhesive sheet.
[0065] The content of the solvent in the photocurable composition is, for example, 5% by weight or less, and may be 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or even 0.5% by weight or less. The photocurable composition may be substantially free of a solvent. The phrase "substantially free of a solvent" means that the solvent derived from additives or the like is allowed to be present at a content of, for example, 0.1% by weight or less, preferably 0.05% by weight or less, and more preferably 0.01% by weight or less.
[0066] [Adhesive sheet] An example of the pressure-sensitive adhesive sheet of this embodiment is shown in Fig. 1. The pressure-sensitive adhesive sheet 1 in Fig. 1 is a sheet formed from the photocurable composition of this embodiment.
[0067] The polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 is, for example, 90% or more, and may be 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, more than 95%, 96% or more, 97% or more, 98% or more, 99% or more, 99.2% or more, 99.3% or more, 99.4% or more, 99.5% or more, or even 99.6% or more. The upper limit of the polymerization rate is, for example, 99.99% or less. A high polymerization rate can contribute to suppressing odor in the pressure-sensitive adhesive sheet 1 and suppressing foaming in a high-temperature environment.
[0068] The weight average molecular weight (Mw) of the polymer contained in the pressure-sensitive adhesive sheet 1 is, for example, 600,000 or more, and may be 650,000 or more, 700,000 or more, more than 700,000, 750,000 or more, 800,000 or more, 850,000 or more, or even 900,000 or more. The upper limit of Mw is not particularly limited, and is, for example, 3 million or less. The pressure-sensitive adhesive sheet 1 containing a polymer having Mw in the above range is suitable for suppressing peeling of the pressure-sensitive adhesive sheet 1 from an adhesive object under high temperature environments, etc. The adhesive object is, for example, an optical film. An example of an optical film is a polarizing film. The number average molecular weight (Mn) of the polymer is, for example, 150,000 or more, and may be 170,000 or more, 180,000 or more, 190,000 or more, 200,000 or more, 210,000 or more, 220,000 or more, 230,000 or more, 240,000 or more, or even 250,000 or more. The upper limit of Mn is not particularly limited, and is, for example, 600,000 or less. Mw / Mn, which means the molecular weight distribution, is, for example, 1.8 to 10, and may be 1.8 to 7, or even 1.8 to 5. Mw and Mn are determined from values measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.
[0069] In the pressure-sensitive adhesive sheet 1, both the polymerization rate of the monomer group and the molecular weight of the polymer can be increased. The polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 may be 97% or more, and the weight-average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet 1 may exceed 700,000. The polymerization rate and weight-average molecular weight may each be within the above-mentioned numerical ranges.
[0070] The gel fraction of the pressure-sensitive adhesive sheet 1 is, for example, 50% or more, and may be 75% or more, 80% or more, or even 85% or more.
[0071] The thickness of the pressure-sensitive adhesive sheet 1 is, for example, 2 to 500 μm, and may be 2 to 300 μm, 2 to 200 μm, or even 2 to 150 μm. The upper limit of the thickness may be 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more.
[0072] The pressure-sensitive adhesive sheet 1 can be used, for example, in optical laminates and image display devices. However, the uses of the pressure-sensitive adhesive sheet 1 are not limited to the above examples.
[0073] (Manufacturing method of adhesive sheets) The pressure-sensitive adhesive sheet 1 can be formed, for example, by irradiating light 14 to a first laminate 10 including a base sheet 11, a coating layer 12 containing the photocurable composition of the present embodiment, and a release liner 13 in this order (see FIG. 2). The coating layer 12 is irradiated with light 14 and hardened to become the pressure-sensitive adhesive sheet 1. Irradiation with light 14 is typically performed from the side of the base sheet 11. At this time, the light 14 penetrates the base sheet 11 and reaches the coating layer 12, hardening the coating layer 12. However, irradiation with light 14 may be performed from the side of the release liner 13, or may be performed from both the side of the release liner 13 and the side of the base sheet 11.
[0074] The formed pressure-sensitive adhesive sheet 1 is sandwiched between the base sheet 11 and the release liner 13 until the release liner 13 is peeled off, and constitutes a part of the second laminate 17. By peeling the release liner 13 from the second laminate 17, a third laminate 15 including the base sheet 11 and the pressure-sensitive adhesive sheet 1 is obtained. In the third laminate 15, the surface of the pressure-sensitive adhesive sheet 1 is exposed to the outside. An optical film can be laminated onto the exposed surface of the pressure-sensitive adhesive sheet 1 directly or via another layer.
[0075] The light 14 is, for example, visible light or ultraviolet light having a wavelength shorter than 450 nm. The light may contain light having a wavelength in the same region as the absorption wavelength of the photopolymerization initiator contained in the photocurable composition. Light with a wavelength of 300 nm or less cut by a filter or the like may be irradiated, and cutting short wavelength light is suitable for suppressing deterioration of the base sheet 11 and / or the release liner 13 caused by the light 14. The light source 18 of the light 14 is, for example, a light irradiation device equipped with an ultraviolet irradiation lamp. Examples of the ultraviolet irradiation lamp include an ultraviolet LED, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a xenon lamp, a microwave excited mercury lamp, a black light lamp, a chemical lamp, a germicidal lamp, a low pressure discharge mercury lamp, and an excimer laser. Two or more ultraviolet irradiation lamps may be combined. With the ultraviolet LED, the band of the irradiated ultraviolet light can be narrowed compared to the case of using other light sources.
[0076] The light source 18 may be an LED. Compared to a black light source, an LED tends to have a long light source life as well as an easy adjustment of illuminance. Compared to a black light source using mercury, an LED is superior in terms of reducing environmental load. When an ultraviolet LED is used as the light source, an LED having a peak wavelength of 325 to 350 nm may be selected. According to the study by the present inventors, the use of an LED having a peak wavelength of 325 to 350 nm may contribute to improving the polymerization rate of the monomer group in the adhesive sheet 1 and / or reducing the amount of remaining photopolymerization initiator compared to, for example, the use of a black light source. Furthermore, an LED that emits light 14 with a peak wavelength of 325 nm to 350 nm tends to generate less heat and to control the temperature of the coating layer 12 more easily than an LED that emits light with a peak wavelength of about 365 nm. As far as the present inventors know, there have been no reports of an adhesive sheet being produced using an LED that emits light with a peak wavelength of 325 nm to 350 nm.
[0077] As an LED having a peak wavelength of 325 to 350 nm, an LED having a peak wavelength of 340±10 nm (hereinafter referred to as LED340) may be selected.
[0078] Focusing on the peak wavelength of the light 14, the peak wavelength of the light 14 irradiated to the first laminate 10 (specifically, the coating layer 12) may be 325 nm to 350 nm. The peak wavelength of the light 14 is preferably 340±10 nm (330 nm to 350 nm), may be 340±5 nm (335 nm to 345 nm), may be 340±2 nm (338 nm to 342 nm), or may be 340 nm. The peak wavelength means a wavelength at which the intensity is a maximum value in a spectrum showing the relationship between the wavelength and intensity of the light 14. The light 14 may further have a peak wavelength in a wavelength range other than 325 nm to 350 nm, but it is preferable that the light 14 does not have such a peak wavelength.
[0079] The illuminance of the light 14 irradiated onto the first laminate 10 (specifically, the coating layer 12) is, for example, 2.0 to 30 mW / cm 2 The illuminance is 2.5mW / cm 2 More than 3.0mW / cm 2 More than 3.5mW / cm 2 More than 4.0mW / cm 2 More than 5.0mW / cm 2 More than 6.0mW / cm 2 More than 7.0mW / cm 2 More than 8.0mW / cm 2 More than 9.0mW / cm 2 or even 10mW / cm 2 The upper limit of the illuminance is, for example, 25 mW / cm 2 Less than 20mW / cm 2 Below 15mW / cm 2 It may be the following.
[0080] The time for irradiating the first laminate 10 (specifically, the coating layer 12) with the light 14 is, for example, 10 seconds to 1000 seconds, and may be 60 seconds or more, 100 seconds or more, 150 seconds or more, 200 seconds or more, 250 seconds or more, or even 300 seconds or more. The upper limit of the time is, for example, 800 seconds or less, and may be 600 seconds or less, 500 seconds or less, 400 seconds or less, 350 seconds or less, 300 seconds or less, or even 250 seconds or less. The irradiation with the light 14 may be continuous or intermittent.
[0081] The integrated amount of light 14 applied to the first laminate 10 (specifically, the coating layer 12) is, for example, 25 mJ / cm 2 More than 100 mJ / cm 2 More than 500mJ / cm 2 More than 1000mJ / cm 2 More than 2000mJ / cm 2 More than 2500mJ / cm 2 or more, even 2800mJ / cm 2 The upper limit of the integrated light amount is not particularly limited, and may be, for example, 30,000 mJ / cm. 2 Less than 10000mJ / cm 2 Below, 5000mJ / cm 2 Below that, and even 4000mJ / cm 2 It may be the following.
[0082] An example of the substrate of the release liner 13 (hereinafter, "liner substrate") is a resin film. Examples of resins that can be contained in the liner substrate are polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.
[0083] The release liner 13 may have a layer other than the liner substrate. The release liner 13 may have a release layer. The release liner 13 has, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 13 can be used such that the release layer is on the coating layer 12 side. The release layer is typically a cured layer of a release agent composition containing a release agent. As the release agent, various release agents such as silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder can be used.
[0084] The release liner 13 may be in the form of a sheet or a continuous piece.
[0085] An example of the base sheet 11 is a resin film. Examples of the resin contained in the base sheet 11 are the same as the examples of the resin that can be contained in the liner base material.
[0086] The thickness of the base sheet 11 is, for example, 10 to 200 μm, and may be 25 to 150 μm.
[0087] The base sheet 11 may have a release layer on the surface on the side of the coating layer 12. Examples of the release layer that may be provided on the base sheet 11 are the same as the examples of the release layer that may be provided on the release liner 13. Both the release liner 13 and the base sheet 11 may have a release layer.
[0088] For the base sheet 11, a sheet having a greater peeling strength from the adhesive sheet 1 than the release liner 13 can usually be selected.
[0089] The base sheet 11 may be in the form of a sheet or a continuous length.
[0090] The first laminate 10 can be formed, for example, by forming a coating layer 12 on a base sheet 11 (or a release liner 13) and then disposing a release liner 13 (or base sheet 11) on the formed coating layer 12. Alternatively, the first laminate 10 may be formed by applying a photocurable composition in a poured manner into the space between the base sheet 11 and the release liner 13 that are held at a predetermined distance such that their main surfaces face each other.
[0091] The coating layer 12 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.
[0092] The thickness of the coating layer 12 can be adjusted according to the desired thickness of the pressure-sensitive adhesive sheet 1, and may be, for example, 2 to 500 μm, 2 to 300 μm, 2 to 200 μm, or even 2 to 150 μm. The upper limit of the thickness may be 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more.
[0093] The first laminate 10 may include a long base sheet 11, a long coating layer 12, and a long release liner 13, in other words, may be long. The long first laminate 10 can be obtained, for example, by forming the coating layer 12 between the base sheet 11 and the release liner 13 while conveying them, the base sheet 11 and the release liner 13 being unwound from a roll.
[0094] As described above, the present invention further provides a method for producing a pressure-sensitive adhesive sheet, comprising irradiating a coating layer of a photocurable composition containing a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator with light 14 to photocure the coating layer.
[0095] [Optical laminate] An example of the optical laminate of this embodiment is shown in Fig. 3. The optical laminate 20A in Fig. 3 includes an adhesive sheet 1 and an optical film 2. The adhesive sheet 1 and the optical film 2 are laminated to each other. The optical laminate 20A can be used as an optical film with an adhesive sheet.
[0096] Examples of the optical film 2 include a polarizing film, a retardation film, and a laminated film including a polarizing film and / or a retardation film. However, the optical film 2 is not limited to the above examples. The optical film 2 may include a glass film.
[0097] The optical film 2 may be a polarizing film, and the adhesive sheet 1 may be in contact with the polarizing film. Among optical films, polarizing films tend to have a large dimensional change due to heat. The dimensional change of the polarizing film may cause peeling from the adhesive film. For this reason, the present invention is particularly advantageous when the optical laminate further includes a polarizing film.
[0098] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with the main surface (surface having the widest area) of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.
[0099] The polarizer is not particularly limited, and examples thereof include hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified ethylene-vinyl acetate copolymer films, which are uniaxially stretched after adsorbing dichroic substances such as iodine and dichroic dyes; polyene-based oriented films such as dehydrated polyvinyl alcohol and dehydrochlorinated polyvinyl chloride; etc. Polarizers are typically made of polyvinyl alcohol films (polyvinyl alcohol films include partially saponified ethylene-vinyl acetate copolymer films) and dichroic substances such as iodine.
[0100] The thickness of the polarizer is not particularly limited, and may be, for example, 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness of the polarizer is not particularly limited, and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change, and can contribute to improving the durability of the optical laminate, particularly the durability at high temperatures.
[0101] As the material of the protective film, for example, a thermoplastic resin excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc. is used. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material of the protective film may be a thermosetting resin or an ultraviolet-curing resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different from each other. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curing resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more types of optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.
[0102] The thickness of the protective film can be appropriately determined, but is generally about 5 to 200 μm in terms of strength, workability such as handleability, thinness, and the like.
[0103] The polarizer and the protective film are usually adhered to each other via a water-based adhesive or the like. Examples of the water-based adhesive include an isocyanate-based adhesive, a polyvinyl alcohol-based adhesive, a gelatin-based adhesive, a vinyl-based latex, a water-based polyurethane, and a water-based polyester. Examples of adhesives other than the above-mentioned adhesives include an ultraviolet-curable adhesive and an electron beam-curable adhesive. The electron beam-curable polarizing film adhesive exhibits suitable adhesion to various protective films. The adhesive may contain a metal compound filler.
[0104] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.
[0105] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for the purposes of anti-reflection, anti-sticking, diffusion, anti-glare, etc.
[0106] The polarizing film may be a circular polarizing film.
[0107] The thickness of the polarizing film is, for example, 500 μm or less, and may be 300 μm or less, 200 μm or less, 100 μm or less, or even 60 μm or less. The lower limit of the thickness is, for example, 10 μm or more, 25 μm or more, or even 40 μm or more.
[0108] The retardation film is a film having birefringence in the in-plane direction and / or the thickness direction, and is, for example, a stretched resin film or a film in which a liquid crystal material is oriented and fixed.
[0109] The retardation film may be a λ / 4 plate, a λ / 2 plate, an anti-reflection retardation film (see, for example, paragraphs 0221, 0222, and 0228 of JP 2012-133303 A), a retardation film for compensating for viewing angles (see, for example, paragraphs 0225 and 0226 of JP 2012-133303 A), or a tilted orientation retardation film for compensating for viewing angles (see, for example, paragraph 0227 of JP 2012-13303 A). The retardation film is not limited to the above examples as long as it has birefringence in the in-plane direction and / or the thickness direction. There are also no limitations on the retardation value, arrangement angle, three-dimensional birefringence, whether it is a single layer or a multilayer, and the like, of the retardation film. A known film can be used for the retardation film.
[0110] The optical film 2 has a thickness of, for example, 1 to 200 μm.
[0111] The optical film 2 may be a single layer or a laminated film composed of two or more layers. When the optical film 2 is a laminated film, the pressure-sensitive adhesive sheet 1 may be used to bond the layers together.
[0112] Another example of the optical laminate of the present embodiment is shown in Fig. 4. The optical laminate 20B in Fig. 4 has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 1, and an optical film 2 are layered in this order. By peeling off the release liner 3, the optical laminate 20B can be used as an optical film with a pressure-sensitive adhesive sheet.
[0113] The release liner 3 is typically a resin film. Examples of resins constituting the release liner 3 include polyesters such as polyethylene terephthalate (PET), polyolefins such as polyethylene and polypropylene, polycarbonate, acrylic, polystyrene, polyamide, and polyimide. The surface of the release liner 3 that contacts the pressure-sensitive adhesive sheet 1 may be subjected to a release treatment. The release treatment is, for example, a treatment with a silicone compound. However, the release liner 3 is not limited to the above example. The release liner 3 is peeled off when the optical laminate 20B is used, for example, when it is attached to the image forming layer.
[0114] Another example of the optical laminate of the present embodiment is shown in Fig. 5. The optical laminate 20C in Fig. 5 has a laminated structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, and a polarizing film 2A are laminated in this order. After the release liner 3 is peeled off, the optical laminate 20C can be used by being attached to, for example, an image forming layer.
[0115] A known adhesive sheet can be used as the adhesive sheet 4. The adhesive sheet 1 may be used as the adhesive sheet 4.
[0116] Another example of the optical laminate of this embodiment is shown in Fig. 6. Optical laminate 20D in Fig. 6 has a laminated structure in which a release liner 3, an adhesive sheet 4, a retardation film 2B, an adhesive sheet 1, a polarizing film 2A, and a protective film 5 are laminated in this order. After peeling off the release liner 3, optical laminate 20D can be used by being attached to, for example, an image forming layer.
[0117] The protective film 5 has a function of protecting the optical film 2 (polarizing film 2A) which is the outermost layer during distribution and storage of the optical laminate 20D and in a state where the optical laminate 20D is incorporated into an image display device. The protective film 5 may also function as a window to the external space in a state where it is incorporated into an image display device. The protective film 5 is typically a resin film. The resin constituting the protective film 5 is, for example, polyester such as PET, polyolefin such as polyethylene and polypropylene, acrylic, cycloolefin, polyimide, and polyamide, and polyester is preferable. However, the protective film 5 is not limited to the above examples. The protective film 5 may be a glass film or a laminated film including a glass film. The protective film 5 may be subjected to surface treatment such as anti-glare, anti-reflection, and anti-static.
[0118] The protective film 5 may be bonded to the optical film 2 by any pressure-sensitive adhesive. Bonding by a pressure-sensitive adhesive sheet 1 is also possible.
[0119] The optical laminate may have any configuration as long as it includes the pressure-sensitive adhesive sheet 1 and the optical film 2.
[0120] The optical laminate of this embodiment can be distributed and stored, for example, as a rolled body obtained by rolling up a strip-shaped optical laminate, or as a sheet-shaped optical laminate.
[0121] The optical laminate of the present embodiment is typically used in an image display device, such as a liquid crystal display, an organic EL display, or an inorganic EL display.
[0122] [Image display device] An example of the image display device of this embodiment is shown in Fig. 7. The image display device 21 in Fig. 7 has a laminated structure in which a substrate 7, an image forming layer (e.g., an organic EL layer or a liquid crystal layer) 6, an adhesive sheet 4, a retardation film 2B, an adhesive sheet 1, a polarizing film 2A, and a protective film 5 are laminated in this order. The image display device 21 has the optical laminates 20A, 20B, 20C, and 20D of Figs. 3 to 6 (excluding the release liner 3). The substrate 7 and the image forming layer 6 may have the same configurations as the substrate and the image forming layer, respectively, of a known image display device.
[0123] The image display device 21 in Fig. 7 may be an organic EL display or a liquid crystal display. However, the image display device 21 is not limited to this example. The image display device 21 may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), or the like. The image display device 21 may be used for home appliances, in-vehicle applications, public information displays (PID), and the like.
[0124] The image display device 21 may have any configuration as long as it includes the pressure-sensitive adhesive sheet 1 and / or the optical laminate 20. EXAMPLES
[0125] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.
[0126] [Evaluation of photopolymerization initiators] The photopolymerization initiator used in this example was measured for polymerization rate A and residual amount as follows. (Monomer syrup x1) 99 parts by weight of n-butyl acrylate (BA), 1 part by weight of 4-hydroxybutyl acrylate (HBA), and 0.1 parts by weight of 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone (Omnirad2959, IGM Resin) as a photopolymerization initiator were placed in a four-neck flask. Next, the liquid in the flask was irradiated with ultraviolet light under a nitrogen atmosphere to obtain monomer syrup X1 in which the monomer was partially photopolymerized. The ultraviolet light irradiation was continued until the viscosity of the liquid in the flask (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 20 Pa·s.
[0127] (Monomer syrup X2~X6) Monomer syrups X2 to X6 were prepared in the same manner as for the monomer syrup X1, except that the monomers and photopolymerization initiators were changed as shown in Table 1.
[0128] [Table 1]
[0129] The abbreviations in Table 1 are as follows. Omnirad2959 and Omnirad127 are α-hydroxyacetophenone compounds. BA: n-butyl acrylate HBA: 4-hydroxybutyl acrylate Omnirad2959: 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone (Omnirad2959, IGM Resin) Omnirad184: 1-Hydroxycyclohexyl-phenyl ketone (Omnirad184, IGM Resin) Omnirad651: 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad651, IGM Resins) Omnirad127: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad127, IGM Resin) Omnirad819: Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad819, IGM Resins) Omnirad1173: 2-hydroxy-2-methyl-1-phenylpropanone (Omnirad1173, IGM Resins)
[0130] (Preparation of release liner) Addition reaction curing type silicone (LTC761 containing hexenyl group-containing polyorganosiloxane, 30 wt% toluene solution, manufactured by Dow Corning Toray) 30 parts by weight, release control agent (BY24-850 containing unreactive silicone resin, manufactured by Dow Corning Toray) 0.9 parts by weight, curing catalyst (SRX212 containing platinum catalyst, manufactured by Dow Corning Toray) 2 parts by weight, and toluene / hexane mixed solvent (volume ratio 1: 1) as a dilution solvent were mixed to obtain a silicone-based release agent composition. The concentration of silicone solids in the release agent composition was 1.0 wt%. Next, the release agent composition was applied to one side of a liner substrate (Lumirror XD500P, a polyester film, thickness 75 μm) with a wire bar and heated at 130 ° C for 1 minute to prepare a release liner having a release layer (thickness 60 nm) on one side.
[0131] (Preparation of adhesive sheet) Monomer syrup X1 was applied to one side of a base sheet (Lumirror XD500P, a polyester film without a release layer, thickness 75 μm) using an applicator to form a coating layer (thickness 20 μm). Next, a release liner was placed on the formed coating layer to obtain a first laminate. The release liner was placed so that the release layer was in contact with the coating layer. Next, an illuminance of 4 mW / cm was applied from the side of the base sheet in the first laminate. 2 , irradiation time 1200 seconds (when evaluating polymerization rate A), or illuminance 14 mW / cm 2 The LED light was irradiated under the condition of 100 seconds irradiation time (when evaluating the remaining amount of photopolymerization initiator). The peak wavelength of this light was 340 nm. As a result, the coating layer was photocured, and an adhesive sheet (thickness 20 μm) for evaluating the polymerization rate A or remaining amount sandwiched between the base sheet and the release liner was obtained. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse Co., Ltd.) at a position near the ultraviolet ray incident surface on the base sheet. Similarly, an adhesive sheet (thickness 20 μm) for evaluating the polymerization rate A or remaining amount was obtained for each of the monomer syrups X2 to X6.
[0132] (Polymerization rate A) The polymerization rate A of each produced pressure-sensitive adhesive sheet was calculated from the change in weight of the pressure-sensitive adhesive sheet before and after 2 hours of heat drying at 130° C. Specifically, the weight of the pressure-sensitive adhesive sheet immediately after peeling off the base sheet and release liner was defined as W0 (weight before drying), and the weight of the pressure-sensitive adhesive sheet after cooling for about 20 minutes at room temperature (23° C.) after the above heating was defined as W1 (weight after drying), and the polymerization rate A was calculated from the formula: polymerization rate (%) = W1 / W0 × 100.
[0133] [Remaining amount of photopolymerization initiator] The composition of each pressure-sensitive adhesive sheet was analyzed, and the remaining amount (content) of the photopolymerization initiator was calculated based on the results. The composition analysis was performed using liquid chromatography (LC) under the following conditions. Equipment used: 1290 Infinity II (Agilent Technologies) Column: Acquity UPLC BEH C18 (Waters, 2.1 mmφ×100 mm, 1.7 μm) Eluent composition: Gradient conditions of ultrapure water / acetonitrile Column temperature: 40℃ Column flow rate: 0.2mL / min ·Injection volume: 2μL Detector: Photodiode array detector (PDA) Measurement wavelength: 190-400nm ·Extraction wavelength: Omnirad2959=278nm, Omnirad184=246nm, Omnirad651=253nm, Omnirad127=262nm, Omnirad819=296nm, Omnirad1173=246nm Sample preparation method: Approximately 0.5 g of sample (adhesive sheet) was weighed, 2 mL of chloroform was added, and the mixture was shaken overnight. 8 mL of methanol was added to the resulting solution, and the supernatant was filtered through a 0.45 μm membrane filter. The filtrate was injected into the LC for analysis.
[0134] The evaluation results are shown in Table 2 below.
[0135] [Table 2]
[0136] [Examples 1 to 5, Comparative Examples 1 to 6] (Monomer Syrup A1) 95.2 parts by weight of BA, 4.75 parts by weight of acrylic acid (AA), 0.05 parts by weight of HBA, 0.1 parts by weight of Omnirad2959 (manufactured by IGM Resins) and 0.1 parts by weight of Omnirad127 (manufactured by IGM Resins) as photopolymerization initiators were placed in a four-neck flask. Next, the liquid in the flask was irradiated with ultraviolet light under a nitrogen atmosphere to obtain a monomer syrup A1 in which the monomers were partially photopolymerized. The ultraviolet light irradiation was continued until the viscosity of the liquid in the flask (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached 20 Pa·s.
[0137] (Monomer syrup A2~A11) Monomer syrups A2 to A11 were prepared in the same manner as for the monomer syrup A1, except that the monomers and photopolymerization initiators were changed as shown in Table 3. In addition, "AA" is acrylic acid.
[0138] [Table 3]
[0139] (Photocurable compositions C1 to C11) Next, the monomer syrup and the crosslinking agent were mixed so as to obtain the compositions shown in Table 4 below, thereby obtaining photocurable compositions C1 to C11. Note that "NVP" is N-vinyl-2-pyrrolidone, and "NDDA" is 1,9-nonanediol diacrylate.
[0140] [Table 4]
[0141] The final composition of the monomers contained in the photocurable composition C11 is shown in Table 5 below.
[0142] [Table 5]
[0143] (Preparation of adhesive sheet) <Example 1> The photocurable composition C1 was applied to one side of a substrate sheet (Lumirror XD500P, a polyester film without a release layer, thickness 75 μm) using an applicator to form a coating layer (thickness 20 μm). Next, the release liner used in the evaluation of the photopolymerization initiator was placed on top of the formed coating layer to obtain a first laminate. The release liner was placed so that the release layer was in contact with the coating layer. Next, a light with an illuminance of 9 mW / cm was applied from the substrate sheet side of the first laminate. 2The LED light was irradiated under the conditions of 100 s, 100 s, and 320 s. The peak wavelength of this light was 340 nm. This caused the coating layer to photocure, and the adhesive sheet of Example 1 (thickness 20 μm) sandwiched between the base sheet and the release liner was obtained. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse) at a position near the ultraviolet ray incident surface of the base sheet.
[0144] <Examples 2 to 5 and Comparative Examples 1 to 6> Pressure-sensitive adhesive sheets of Examples 2 to 5 and Comparative Examples 1 to 6 were obtained in the same manner as in Example 1, except that the photocurable compositions used were changed as shown in Tables 6A and 6B.
[0145] (polymerization rate of monomer group) The polymerization rate in each of the pressure-sensitive adhesive sheets of the Examples and Comparative Examples was evaluated in the same manner as for the polymerization rate A.
[0146] (Number average molecular weight (Mn) and weight average molecular weight (Mw) of polymer) Samples were prepared that had the same composition as the photocurable compositions used in Examples 1 to 5 and Comparative Examples 1 to 6, except that they did not contain a crosslinking agent. The samples were irradiated with light under the conditions of the corresponding Examples and Comparative Examples. As a result, the monomer groups contained in the samples were polymerized to form a polymer. The number average molecular weight (Mn) and weight average molecular weight (Mw) of the polymer were measured.
[0147] The above Mn and Mw were measured by GPC (gel permeation chromatography). The measurement device and conditions were as follows. The measurement device and conditions were different for the NVP-containing composition and the NVP-free composition.
[0148] (NVP-free composition) Analytical equipment: Tosoh HLC-8120GPC Column: Tosoh G7000H XL +GMH XL +GMH XL Column size: 7.8mmφ×30cm each, total 90cm Column temperature: 40℃ ·Flow rate: 0.8mL / min ·Injection volume: 100μL Eluent: Tetrahydrofuran Detector: Differential refractometer (RI) Standard sample: polystyrene
[0149] (NVP-containing composition) Analytical equipment: Agilent Technologies, Agilent 1200 Column: Tosoh Corporation, TSKgel SuperAWM-H+superAW4000+superAW2500 Column size: 6.0mmφ×15cm each, total 45cm Column temperature: 40℃ ·Flow rate: 0.4mL / min ·Injection volume: 40μL Eluent: N,N-dimethylformamide (DMF) Detector: Differential refractometer (RI) Standard sample: polystyrene
[0150] (Reliability test) <Preparation of polarizing film> A polyvinyl alcohol film having a thickness of 80 μm was stretched to 3 times while being dyed for 1 minute in an iodine solution having a concentration of 0.3% at a temperature of 30° C. between rolls having different speed ratios. Next, the film was stretched to a total stretching ratio of 6 times while being immersed for 0.5 minutes in an aqueous solution having a temperature of 60° C. and containing boric acid at a concentration of 4% and potassium iodide at a concentration of 10%. Next, the film was immersed for 10 seconds in an aqueous solution having a temperature of 30° C. and containing potassium iodide at a concentration of 1.5%, and then dried at 50° C. for 4 minutes to obtain a polarizer having a thickness of 28 μm. A transparent protective film having a thickness of 30 μm and made of a modified acrylic polymer having a lactone ring structure was attached to one side of the polarizer with a polyvinyl alcohol adhesive. Furthermore, a 47 μm-thick transparent protective film made of a triacetyl cellulose film (Konica Minolta, product name "KC4UY") with a hard coat layer (HC) was attached to the other surface of the polarizer using a polyvinyl alcohol adhesive. The polarizing film was produced by heating and drying for 5 minutes in an oven set at 70°C. Furthermore, a discharge amount of 63 W / m was applied to the surface of the polarizing film on the transparent protective film side made of modified acrylic polymer. 2 Corona treatment was performed for 1 min.
[0151] <Preparation of optical laminate> An optical laminate was produced by disposing the above-mentioned polarizing film on the exposed surface of the pressure-sensitive adhesive sheet produced in Examples 1 to 5 and Comparative Examples 1 to 6. The polarizing film was disposed so that the surface on the transparent protective film side made of a modified acrylic polymer was in contact with the pressure-sensitive adhesive sheet.
[0152] <Reliability test (95℃)> The reliability (95°C reliability) of the prepared optical laminate was evaluated by the following method. First, the optical laminate was cut into a strip of 228 mm length x 128 mm width to prepare a test piece. Next, the test piece was attached to the surface of 0.7 mm thick alkali-free glass (manufactured by Corning, product name "EG-XG") with an adhesive sheet. The test piece was attached to the alkali-free glass using a laminator. After the test piece was attached, it was placed in an autoclave at 50°C and 0.5 MPa for 15 minutes to homogenize the bonding between the alkali-free glass and the adhesive sheet, and the adhesive sheet was adhered to the alkali-free glass. Next, the test piece was heat-treated at 95°C under atmospheric pressure for 500 hours. The vicinity of the end of the test piece was observed with an optical microscope to evaluate peeling from the end of the test piece, and the presence or absence of foaming near the end was identified. The evaluation criteria for peeling and foaming at the end are shown below. (Evaluation of peeling) A: There is slight peeling on the edge, but it is not at a level that affects the image display. B: There is peeling at the edges, but the effect on image display is minimal. C: There is significant peeling at the edges that affects image display. (Foam) A: No foaming C: With foaming
[0153] Based on the evaluation results for peeling and bubbling at the edges, a comprehensive evaluation was made for the reliability test (95°C) according to the following criteria. (comprehensive evaluation) A: Peeling of the edge is A and foaming is A B: Peeling at the edge is B and foaming is A C: Peeling at the edge is C and foaming is A D: Regardless of the evaluation result of peeling at the edge, foaming is C (foaming is present)
[0154] <Reliability test (105℃)> The 105°C reliability was evaluated in the same manner as the 95°C reliability, except that the heat treatment temperature was changed from 95°C to 105°C. The evaluation criteria for peeling, bubbling, and overall evaluation were the same as for 95°C.
[0155] The compositions and evaluation results of each photocurable composition are shown in Tables 6A and 6B below. In Table 6B, "-" means not measured.
[0156] [Table 6A]
[0157] [Table 6B]
[0158] As shown in Table 6B, the pressure-sensitive adhesive sheets of the examples were able to suppress foaming and peeling of the polarizing film in a high-temperature environment, and were able to improve reliability when used in image display devices. [Industrial Applicability]
[0159] The curable composition of the present invention can be used to form a pressure-sensitive adhesive sheet. [Explanation of symbols]
[0160] 1 Adhesive sheet 2. Optical Film 20A, 20B, 20C, 20D Optical laminate 21 Image display device
Claims
1. The composition includes a monomer group and / or a partial polymer of the monomer group, a first photopolymerization initiator, and a second photopolymerization initiator, the first photopolymerization initiator and the second photopolymerization initiator have a relatively small first reaction rate and a relatively large second reaction rate, respectively; a ratio of the second reaction rate to the first reaction rate, expressed as a ratio of polymerization rates A evaluated by the following measurement method using only each of the photopolymerization initiators, is 1.1 or more; Photocurable composition for adhesive sheets. [Measurement method] A mixed solution of 99 parts by weight of n-butyl acrylate and 1 part by weight of 4-hydroxybutyl acrylate as monomers and 0.1 part by weight of a photopolymerization initiator to be evaluated is irradiated with ultraviolet light to prepare a monomer syrup in which the monomers are partially polymerized. The irradiation with ultraviolet light is continued until the viscosity of the mixed solution at 30° C. becomes 20 Pa·s. Next, a 20 μm thick coating layer made of the monomer syrup is formed between a pair of polyethylene terephthalate (PET) sheets each having a thickness of 75 μm. Next, the coating layer is irradiated with ultraviolet light from an LED having a peak wavelength of 340 nm±10 nm as a light source from the side of one of the PET sheets. The illuminance and irradiation time of the irradiated ultraviolet light are, respectively, 4 mW / cm. 2 and 1200 seconds. As the polymerization rate A, the polymerization rate of the monomer measured for the coating layer photocured by irradiation with ultraviolet light is specified.
2. The polymerization rate A of the first photopolymerization initiator is 80% or less, The photocurable composition according to claim 1 , wherein the polymerization rate A of the second photopolymerization initiator is 90% or more.
3. The photocurable composition according to claim 1 , wherein the first photopolymerization initiator is an α-hydroxyacetophenone-based compound.
4. 4. The photocurable composition according to claim 3, wherein the first photopolymerization initiator has one α-hydroxyacetophenone structure in one molecule.
5. The photocurable composition according to claim 1 , wherein the second photopolymerization initiator is an α-hydroxyacetophenone-based compound.
6. 2. The photocurable composition of claim 1, wherein the first photoinitiator is 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methylpropanone.
7. The photocurable composition of claim 1 , wherein the monomer group includes a (meth)acrylic monomer.
8. A pressure-sensitive adhesive sheet formed from the photocurable composition according to claim 1 .
9. The pressure-sensitive adhesive sheet according to claim 8 , wherein the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 97% or more, and the weight-average molecular weight of the polymer contained in the pressure-sensitive adhesive sheet is more than 700,000.
10. The pressure-sensitive adhesive sheet according to claim 8 , wherein the pressure-sensitive adhesive sheet has a thickness of 300 μm or less.
11. An optical laminate comprising the pressure-sensitive adhesive sheet according to any one of claims 8 to 10 and an optical film.
12. The optical film is a polarizing film, The optical laminate according to claim 11 , wherein the pressure-sensitive adhesive sheet is in contact with the polarizing film.
13. An image display device comprising the optical laminate according to claim 11.
Citation Information
Patent Citations
Adhesive composition, adhesive layer, adhesive sheet, optical member, and touch panel
JP2019070150A