Photosensitive resin composition, dry film, cured product, and printed wiring board

The photosensitive resin composition addresses the challenges of thermal expansion, melt viscosity, and embeddability by incorporating specific components, achieving improved reliability and stability in printed wiring boards.

JP2024146830APending Publication Date: 2024-10-15TAIYO HOLDINGS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024048000
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-25
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The challenge lies in developing a photosensitive resin composition that can form a cured product with a low coefficient of thermal expansion, suppress an increase in melt viscosity, and improve embeddability, while addressing the issues of stress and crack resistance in solder resists due to miniaturization and increased heat generation in electronic components.

Method used

A photosensitive resin composition containing an inorganic filler, a compound with acryloyl or methacryloyl groups, a photopolymerization initiator, and an inorganic colloid, with specific ratios and properties to achieve low thermal expansion and reduced melt viscosity, enhancing embeddability and crack resistance.

Benefits of technology

The composition forms a cured product with a low coefficient of thermal expansion, suppresses melt viscosity increase, and improves embeddability, resulting in enhanced reliability and stability of printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146830000001
    Figure 2024146830000001
  • Figure 2024146830000002
    Figure 2024146830000002
  • Figure 2024146830000003
    Figure 2024146830000003
Patent Text Reader

Abstract

To provide a photosensitive resin composition which enables formation of a cured product having low coefficient of thermal expansion, suppresses increase of melt viscosity, and can improve embedding properties.SOLUTION: A photosensitive resin composition contains (A) an inorganic filler, (B) a compound having at least one acryloyl group or methacryloyl group in one molecule, (C) a photopolymerization initiator, and (D) an inorganic colloid, wherein the total blending amount of (A) the inorganic filler and (D) the inorganic colloid is 30.0 mass% or more with respect to the total amount of the photosensitive resin composition in terms of solid content, the blending amount of (D) the inorganic colloid is 2.0 mass% or more with respect to the total amount of the photosensitive resin composition in terms of solid content, and melt viscosity at 100°C is less than 1,000 dPa s.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition. The present invention further relates to a dry film, a cured product, and a printed wiring board using the photosensitive resin composition. [Background technology]

[0002] In recent years, as electronic components have become smaller and more powerful, the semiconductor chips mounted on them have also become denser and more functional. Accordingly, printed wiring boards on which semiconductor chips are mounted must also become smaller and denser, and the development of insulating materials (such as solder resists and insulating films) with high resolution and reliability is underway to manufacture highly integrated printed wiring boards.

[0003] As electronic components become smaller, printed wiring boards on which semiconductor chips are mounted are required to have higher smoothness. When mounting electronic components on a printed wiring board, if there is variation in height on the surface of the printed wiring board, the connection between the electronic components and the printed wiring board becomes unstable, resulting in reduced reliability. For this reason, a dry film type solder resist with high surface smoothness is preferably used for the solder resist used in the outermost layer of a printed wiring board (for example, Patent Document 1).

[0004] Dry film type solder resist is formed by heating and pressing onto a printed wiring board using equipment such as a vacuum laminator. If the solder resist is not properly embedded between the wiring of the printed wiring board, the insulation reliability of the electronic components will be significantly reduced. For this reason, solder resist has been designed to be more fluid so that it can be properly embedded even in areas that are difficult to penetrate, such as between wiring. However, with the recent trend toward smaller electronic components, the wiring on printed wiring boards is becoming finer and finer, and therefore dry film type solder resists are required to have high embedding properties.

[0005] Furthermore, the increased performance of electronic components has led to an increase in the amount of heat generated. This has resulted in greater volume changes caused by heating and cooling in insulating materials such as solder resist that make up electronic components, and therefore greater stress. When the solder resist is no longer able to withstand the increased stress, cracks occur, causing failure of electronic components, so there is a demand for improved crack resistance in solder resist.

[0006] To improve the crack resistance of solder resist, it is necessary to suppress the stress that occurs with the volume change caused by heating and cooling. Effective methods for achieving this are known to be suppressing the volume change of the solder resist or matching the thermal expansion coefficient with that of the various constituent materials that come into contact with the solder resist. In this case, it is preferable that the solder resist has a low thermal expansion coefficient. In order to reduce the thermal expansion coefficient, it is effective to highly fill the solder resist with inorganic filler. However, increasing the amount of inorganic filler increases the melt viscosity, which reduces the embeddability. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-13486 A Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, an object of the present invention is to provide a photosensitive resin composition capable of forming a cured product having a low thermal expansion coefficient, suppressing an increase in melt viscosity, and improving embeddability. Another object of the present invention is to provide a dry film having a resin layer formed of a dried coating film of the resin composition, a cured product of the resin composition or the resin layer of the dry film, and a printed wiring board having the cured product. [Means for solving the problem]

[0009] Means for Solving the Problem The inventors of the present invention have conducted intensive research in order to achieve the above-mentioned object, and have found that by blending an inorganic filler, a compound having at least one acryloyl group or methacryloyl group in each molecule, a photopolymerization initiator, and an inorganic colloid in a photosensitive resin composition, a cured product having a low thermal expansion coefficient can be formed, an increase in melt viscosity can be suppressed, and an embeddability can be improved.

[0010] That is, according to the present invention, the following inventions are provided. [1] A photosensitive resin composition comprising: (A) an inorganic filler; (B) a compound having at least one acryloyl group or methacryloyl group in one molecule; (C) a photopolymerization initiator; and (D) an inorganic colloid, the total amount of the (A) inorganic filler and the (D) inorganic colloid is 30.0 mass% or more, calculated as a solid content, based on the total amount of the photosensitive resin composition; the blending amount of the (D) inorganic colloid is 2.0 mass% or more in terms of solid content with respect to the total amount of the photosensitive resin composition, A photosensitive resin composition having a melt viscosity at 100°C of less than 1000 dPa·s. [2] The surface area of ​​the inorganic colloid (D) is 100 m 2 / g or more. [3] The photosensitive resin composition according to [1] or [2], wherein the (D) inorganic colloid is colloidal silica having an average particle size of 30 nm or less and having a surface treated with a silane coupling agent. [4] The photosensitive resin composition according to [3], wherein the colloidal silica has acryloyl groups or methacryloyl groups added to less than 50% of the total surface area. [5] The photosensitive resin composition according to [3] or [4], wherein the colloidal silica is colloidal silica derived from sodium silicate. [6] The photosensitive resin composition according to any one of [3] to [5], wherein the colloidal silica has a density of 1.9 to 2.2. [7] The photosensitive resin composition according to any one of [1] to [6], wherein the average particle size of the inorganic filler (A) is 200 nm or more and less than 1000 nm. [8] The photosensitive resin composition according to any one of [1] to [7], wherein the (A) inorganic filler is silica having an acryloyl group or a methacryloyl group added to the surface thereof by a silane coupling treatment. [9] The photosensitive resin composition according to any one of [1] to [8], wherein the (A) inorganic filler and the (D) inorganic colloid are spherical.

[10] The photosensitive resin composition according to any one of [1] to [9], wherein a ratio of an average particle size of the (A) inorganic filler to an average particle size of the (D) inorganic colloid is 8 or more.

[11] The photosensitive resin composition according to any one of [1] to

[10] , further comprising (E) a carboxyl group-containing resin.

[12] A dry film comprising: a first film; and a resin layer formed on the first film and comprising a dried coating film of the photosensitive resin composition according to any one of [1] to

[11] .

[13] A cured product obtained by curing the photosensitive resin composition according to any one of [1] to

[11] .

[14] A cured product obtained by curing the resin layer of the dry film described in

[12] .

[15] A printed wiring board comprising the cured product described in

[13] .

[16] A printed wiring board comprising the cured product according to

[14] . Effect of the Invention

[0011] According to the present invention, it is possible to provide a photosensitive resin composition that can form a cured product having a low thermal expansion coefficient, suppress an increase in melt viscosity, and improve embeddability. Furthermore, the photosensitive resin composition of the present invention can also reduce the thermal expansion coefficient. In addition, according to the present invention, it is possible to provide a dry film having a resin layer made of a dried coating film of the resin composition, a cured product of the resin composition or the resin layer of the dry film, and a printed wiring board having the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] [Photosensitive resin composition] The photosensitive resin composition according to the present invention contains at least (A) an inorganic filler, (B) a compound having at least one acryloyl group or methacryloyl group in one molecule, (C) a photopolymerization initiator, and (D) an inorganic colloid. The photosensitive resin composition according to the present invention may further contain (E) a carboxyl group-containing resin, a thermosetting component, a cation scavenger, a colorant, an organic solvent, and other additives. Each component constituting the photosensitive resin composition according to the present invention will be described below.

[0013] The melt viscosity of the photosensitive composition at 100° C. is less than 1000 dPa·s, preferably less than 900 dPa·s, and more preferably less than 700 dPa·s. When the melt viscosity of the photosensitive composition at 100° C. is less than 1000 dPa·s, the embeddability into a circuit can be improved. In the present invention, the melt viscosity of the photosensitive composition at 100°C is a value measured under the following conditions using a rheometer MARS40, by laminating dry films at a lamination temperature of 30 to 40°C using a vacuum laminator CVP-300 manufactured by Nikko Materials Co., Ltd. to prepare a resin layer having a thickness of 300 μm and a width of 20 mm. (Melt viscosity measurement conditions) Heating rate: 5℃ / min Frequency: 1Hz Pressure: 3Pa

[0014] ((A) Inorganic filler) The average particle size of the inorganic filler is preferably 200 nm or more and less than 1000 nm, more preferably 250 nm or more and 900 nm or less, and more preferably 300 nm or more and 800 nm or less. When the photosensitive resin composition contains an inorganic filler having the above average particle size, the photosensitive resin composition has good embeddability. Furthermore, the ratio of the average particle size of the inorganic filler to the average particle size of the inorganic colloid (average particle size of inorganic filler / average particle size of inorganic colloid) is preferably 8 or more, more preferably from 8 to 100, and even more preferably from 8 to 50. When the ratio of the average particle size of the inorganic colloid to the average particle size of the inorganic filler is within the above numerical range, the embeddability is good.

[0015] In the present invention, the average particle size of the inorganic filler is a volume average particle size (D50 volume %) measured by dynamic light scattering using a laser diffraction measuring device. Specifically, the average particle size of the inorganic filler can be measured by the following method. Particle size distribution meter: Nikkiso Microtrac MT3300EX Circulation device: ASVR manufactured by Nikkiso Co., Ltd. First, enter the measurement conditions using the following procedure. Start the software that comes with the Microtrac ("Particle Size Distribution Measurement"), proceed from the SET UP screen, and set the time from the measurement condition setting options. Set the Set Zero time to 30 sec., the measurement to 30 sec., and the number of measurements to 2. Next, enter the analysis conditions. In the analysis information, set the particle refractive index to 1.81 (fixed value: average value of the refractive index of all inorganic substances), the particle characteristics to transparent, and the shape to non-spherical. In the solvent information, select PMA (propylene glycol monomethyl ether acetate) and set the solvent refractive index to 1.4. Next, enter the scale settings. In the particle size range, set the minimum particle size to 0.021 μm and the maximum particle size to 704 μm. Next, enter the sampling system. Set the number of ASVR cleanings to 4, the flow rate to 50%, the ultrasonic output to 40 W, and the ultrasonic time to 300 sec. After entering all the measurement conditions, click Save in the measurement condition settings to close. Next, the sample is adjusted according to the following procedure. The sample is the inorganic filler before being mixed with the photosensitive resin composition. When the inorganic filler is mixed in powder form, the powder is used as the sample, and when the inorganic filler is dispersed in a solvent or the like and mixed, the solvent dispersion is used as the sample. 0.3 g of the sample is weighed out and placed in a screw bottle, and 30 g of propylene glycol monomethyl ether acetate is added little by little using a dropper, and the sample is dispersed by shaking the screw bottle to prepare an adjusted sample. The adjusted sample is not subjected to external dispersion or preliminary dispersion. Next, the adjusted sample is measured. Click on the particle size distribution measurement of the software attached to the Microtrack to open the sample loading screen. Drop several drops of the adjusted sample into the sample inlet of the main body using a dropper. When a red indication bar is displayed on the sample loading screen, drop the adjusted sample into the sample inlet until it is within the range from red to green. When it is within the green range, press the measurement button to start the measurement. The process from sample adjustment to measurement of the adjusted sample is performed within 5 minutes. The value of the cumulative volume average diameter of 50% displayed as the measurement result is taken as the average particle diameter D50.

[0016] In order to enhance dispersibility in the photosensitive resin composition, the inorganic filler is preferably an inorganic filler with at least a part of its surface treated. In particular, it is preferable that the surface of the inorganic filler is subjected to a surface treatment capable of introducing a curable reactive group. Here, the curable reactive group is not particularly limited as long as it is a group that undergoes a curing reaction with a curable compound such as (B) a compound having at least one acryloyl group or methacryloyl group in one molecule and (E) a carboxyl group-containing resin, and may be a photocurable reactive group or a thermosetting reactive group. Examples of the photocurable reactive group include an acryloyl group, a methacryloyl group, a vinyl group, and a styryl group. Examples of the thermosetting reactive group include an epoxy group, an amino group, a hydroxyl group, a carboxyl group, an isocyanate group, an imino group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group.

[0017] The method of introducing a curable reactive group to the surface of the inorganic filler is not particularly limited, and may be introduced using a known and commonly used method, and the surface of the inorganic filler may be treated with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group. As the coupling agent, silane-based, titanate-based, aluminate-based, zircoaluminate-based, and other coupling agents may be used. Among these, silane coupling agents are preferred. Examples of the silane coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. These can be used alone or in combination. The amount of the silane coupling agent to be treated with respect to 100 parts by mass of the inorganic filler is preferably 0.5 to 10 parts by mass.

[0018] The type of inorganic filler is not particularly limited, and conventionally known inorganic fillers can be used.As inorganic fillers, for example, silica, crystalline silica, Neuburg silica, aluminum hydroxide, glass powder, talc, clay, magnesium carbonate, calcium carbonate, natural mica, synthetic mica, aluminum hydroxide, barium sulfate, barium titanate, iron oxide, non-fibrous glass, hydrotalcite, mineral wool, aluminum silicate, calcium silicate, zinc oxide, etc. can be used.Among these, silica is preferred, and spherical silica is more preferred.

[0019] The amount of the inorganic filler is preferably 2.4 mass% or more, more preferably 2.4 mass% or more and less than 60.0 mass%, and even more preferably 2.4 mass% or more and less than 50.0 mass%, calculated as solid content, based on the total amount of the photosensitive resin composition. When the amount of the inorganic filler is within the above numerical range, the embeddability is good.

[0020] The total amount of the inorganic filler and the inorganic colloid described below is 30.0 mass% or more, preferably 30.0 mass% or more and less than 60.0 mass%, and more preferably 30.0 mass% or more and less than 50.0 mass%, calculated as solid content, based on the total amount of the photosensitive resin composition. If the total amount of the inorganic filler and the inorganic colloid is within the above numerical range, a cured product having a low thermal expansion coefficient and good embeddability can be formed.

[0021] ((B) Compound having at least one acryloyl group or methacryloyl group in one molecule) The compound having at least one acryloyl group or methacryloyl group in one molecule can be used as a reactive diluent to reduce the melt viscosity of the photosensitive resin composition. The compound having at least one acryloyl group or methacryloyl group in one molecule may be used alone or in combination of two or more kinds.

[0022] The upper limit of the molecular weight of the compound having at least one acryloyl group or methacryloyl group in one molecule is preferably 600 g / mol or less, more preferably 550 g / mol or less. The lower limit of the molecular weight of the compound having at least one acryloyl group or methacryloyl group in one molecule is not particularly limited, but may be preferably 300 g / mol or more. By making the molecular weight of the compound having at least one acryloyl group or methacryloyl group in one molecule 600 g / mol or less, the melt viscosity of the photosensitive resin composition can be reduced, and the embeddability in the circuit can be improved.

[0023] The compound having at least one acryloyl group or methacryloyl group in one molecule may be any compound that satisfies the above-mentioned molecular weight, and examples thereof include well-known and commonly used polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, epoxy (meth)acrylates, etc. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-methylolacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; and various other compounds such as hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, and trishydroxyethyl isocyanurate. Polyhydric acrylates derived from hydric alcohols or their alkylene oxide adducts or ε-caprolactone adducts; polyhydric acrylates such as phenols such as phenoxy acrylate and bisphenol A diacrylate or their alkylene oxide adducts; acrylates derived from glycidyl ethers such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether and triglycidyl isocyanurate; and, without being limited to the above, acrylates and melamine acrylates obtained by directly acrilating polyols such as polyether polyols, polycarbonate diols, hydroxyl group-terminated polybutadienes and polyester polyols or by urethane acrylate via diisocyanates, and methacrylates corresponding to the above acrylates can be appropriately selected and used.

[0024] The amount of the compound having at least one acryloyl or methacryloyl group in one molecule is preferably 4.0% by mass or more, more preferably 4.0% by mass to 10% by mass, and even more preferably 4.0% by mass to 8.0% by mass, calculated as solid content based on the total amount of the photosensitive resin composition. When the amount of the compound having at least one acryloyl or methacryloyl group in one molecule is 4.0% by mass or more, the photocurability is good while suppressing an increase in the viscosity of the photosensitive resin composition, and pattern formation is easy in alkaline development after irradiation with active energy rays.

[0025] ((C) Photopolymerization initiator) The photopolymerization initiator is for reacting at least one of (B) a compound having at least one acryloyl group or methacryloyl group in one molecule and (E) a carboxyl group-containing resin by exposure. Any known photopolymerization initiator can be used. The photopolymerization initiator may be used alone or in combination of two or more.

[0026] Specific examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentane. Bisacylphosphine oxides such as 2,6-dimethoxybenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloyl monoacylphosphine oxides such as phenylphosphinic acid isopropyl ester and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate, 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether, and other benzoins; benzoin alkyl ethers; benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, and other benzophenones;Acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl]-1-butanone acetophenones such as acetophenone, N,N-dimethylaminoacetophenone; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, Anthraquinones such as 2-aminoanthraquinone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzoic acid esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetylacetone) oxime esters such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium, and other titanocenes; phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, tetramethylthiuram disulfide, and the like.

[0027] Commercially available α-aminoacetophenone-based photopolymerization initiators include Omnirad 907, 369, 369E, and 379 manufactured by IGM Resins. Commercially available acylphosphine oxide photopolymerization initiators include Omnirad 819 manufactured by IGM Resins. Commercially available oxime ester photopolymerization initiators include Irgacure OXE01 and OXE02 manufactured by BASF Japan Ltd., N-1919, ADEKA Arcles NCI-831 and NCI-831E manufactured by ADEKA Corporation, and TR-PBG-304 manufactured by Changzhou Strong Electronic New Materials Co., Ltd.

[0028] Other examples include carbazole oxime ester compounds described in JP-A-2004-359639, JP-A-2005-097141, JP-A-2005-220097, JP-A-2006-160634, JP-A-2008-094770, JP-T-2008-509967, JP-T-2009-040762, and JP-T-2011-80036.

[0029] The amount of the photopolymerization initiator is preferably 0.5% by mass or more and 5.0% by mass or less, more preferably 0.5% by mass or more and 3.0% by mass or less, calculated as solid content based on the total amount of the photosensitive resin composition. When the amount of the photopolymerization initiator is 0.5% by mass or more, the photocurability of the photosensitive resin composition is good, and the coating properties such as chemical resistance are also good. On the other hand, when the amount is 5.0% by mass or less, the light absorption at the surface of the resist film (cured coating film) is good, and the deep curability is not easily reduced.

[0030] A photoinitiator assistant or a sensitizer may be used in combination with the above-mentioned photopolymerization initiator. Examples of the photoinitiator assistant or sensitizer include benzoin compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds. In particular, it is preferable to use thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, and 4-isopropylthioxanthone. By including a thioxanthone compound, it is possible to improve the deep curing property. Although these compounds may be used as photopolymerization initiators, it is preferable to use them in combination with a photopolymerization initiator. In addition, the photoinitiator assistant or sensitizer may be used alone or in combination of two or more kinds.

[0031] In addition, since these photopolymerization initiators, photoinitiator assistants, and sensitizers absorb specific wavelengths, in some cases the sensitivity is reduced and they may function as ultraviolet absorbers. However, they are not used only for the purpose of improving the sensitivity of the resin composition. If necessary, they can absorb light of a specific wavelength to increase the photoreactivity of the surface, change the line shape and opening of the resist pattern to a vertical, tapered, or reverse tapered shape, and improve the accuracy of the line width and opening diameter.

[0032] (D) Inorganic colloids The inorganic colloid in the present invention may be any known or commonly used one, but it is preferable that it is synthesized by any liquid phase method and has never been in the form of a dry powder before being blended into the photosensitive resin composition. Nanoparticles that have been in the form of a dry powder are difficult to redisperse, causing secondary aggregation and making the decrease in melt viscosity unstable.

[0033] The amount of the inorganic colloid is 2% by mass or more, preferably 2.0% by mass or more and less than 47.0% by mass, more preferably 2.0% by mass or more and less than 30.0% by mass, calculated as solid content, based on the total amount of the photosensitive resin composition. When the amount of the inorganic colloid is within the above range, the embeddability is good.

[0034] The surface area of ​​the inorganic colloid is preferably 100 m 2 / g or more, more preferably 100m 2 / g or more 250m 2 / g or less, and more preferably 150m 2 / g or more 250m 2 / g or less. When the surface area of ​​the inorganic colloid is within the above range, the embedding property is good. In the present invention, the surface area of ​​the inorganic colloid is a value calculated by the BET method using a nitrogen adsorption apparatus.

[0035] The inorganic colloid is preferably a colloidal silica having at least a part of its surface treated in order to enhance dispersibility in the photosensitive resin composition. In particular, it is preferable that the surface of the inorganic colloid is subjected to a surface treatment capable of introducing a curable reactive group. Here, the curable reactive group is not particularly limited as long as it is a group that undergoes a curing reaction with a curable compound such as (B) a compound having at least one acryloyl group or methacryloyl group in one molecule and (E) a carboxyl group-containing resin, and may be a photocurable reactive group or a thermosetting reactive group. Examples of the photocurable reactive group include an acryloyl group, a methacryloyl group, a vinyl group, and a styryl group. Examples of the thermosetting reactive group include an epoxy group, an amino group, a hydroxyl group, a carboxyl group, an isocyanate group, an imino group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group. Among these, an acryloyl group or a methacryloyl group is preferable. In particular, it is preferred that the inorganic colloid has acryloyl or methacryloyl groups on less than 50% of the total surface area.

[0036] The method of introducing a curable reactive group to the surface is not particularly limited, and may be introduced using a known and commonly used method, and the surface of the inorganic filler may be treated with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group. The coupling agent may be the same as that used for the surface treatment of the inorganic filler. The amount of the silane coupling agent to be treated with respect to 100 parts by mass of the inorganic colloid is preferably 0.5 to 10 parts by mass.

[0037] The average particle size of the inorganic colloid is preferably 30 nm or less, more preferably 5 nm or more and 25 nm or less, further preferably 5 nm or more and 15 nm or less, and particularly preferably 5 nm or more and 12 nm or less. By including an inorganic colloid having the above average particle size in the photosensitive resin composition, it is possible to reduce the melt viscosity and improve the embeddability.

[0038] Colloidal silica is preferably prepared by neutralizing or ion-exchanging sodium silicate (Na2SiO3, also called "water glass") as a raw material. The method for producing colloidal silica is not particularly limited, but as an example, a sodium silicate aqueous solution (also called water glass) is prepared from sodium silicate as a raw material, an acid is added to the sodium silicate aqueous solution to obtain colloidal particles, and the colloidal particles are treated with an ion exchange resin, and then a base is added to adjust the pH to obtain colloidal silica. The average particle size of colloidal silica can be adjusted by the concentration of the aqueous solution when preparing the colloidal particles. Specifically, colloidal silica having a desired average particle size can be obtained by a known method such as that described in JP-A-06-16414.

[0039] The average particle size of colloidal silica derived from sodium silicate can be adjusted by the conditions during production. In addition, as the colloidal silica derived from sodium silicate, a commercially available product having an average particle size within the above range may be used as it is. Specific examples include SNOWTEX (registered trademark) manufactured by Nissan Chemical Industries, Ltd.: (product numbers) ST-XS, ST-S, ST-30, ST-50-T, ST-UP, ST-PS-S, ST-PS-M, ST-OXS, ST-OS, ST-O, ST-O-40, ST-OUP, ST-PS-SO, ST-PS-MO, ST-NXS, ST-NS, ST-N, ST-N-40, ST-CXS, ST-C, ST-CM, ST-AK; and Organosilica sol manufactured by Nissan Chemical Industries, Ltd.: (product numbers) MA-ST-M, IPA- ST, IPA-ST-UP, NPC-ST-30, PGM-ST, PGM-ST-UP, DMAC-ST, NMP-ST, MEK-ST-40, MEK-ST-UP, MIBK-ST, CHO-ST-M, EAC-ST, PMA-ST, TOL -ST, MEK-AC-2140Z, PGM-AC-2140Y, PGM-AC-3140Y, MIBK-AC-2140Z, MEK-EC-2130Y, MEK-EC-2430Z, EP-M2130Y, EP-M2230Y, etc.

[0040] The colloidal silica derived from sodium silicate may be blended in a slurry state, which facilitates high dispersion and prevents aggregation, making it easy to handle as silica having an average particle size in the above-mentioned specific range.

[0041] The colloidal silica derived from sodium silicate may be used alone or in combination of two or more kinds.

[0042] The density of the colloidal silica is preferably 1.9 or more and 2.2 or less, and more preferably 2.0 or more and 2.2 or less. When the density of the colloidal silica is within the above range, the embeddability is good.

[0043] ((E) Carboxyl group-containing resin) As the carboxyl group-containing resin, various conventionally known resins having a carboxyl group in the molecule can be used. The carboxyl group-containing resin may or may not have an ethylenically unsaturated double bond in the molecule, but a carboxyl group-containing photosensitive resin having an ethylenically unsaturated double bond in the molecule is particularly preferred in terms of photocurability and development resistance. When the photosensitive resin composition of the present invention contains a carboxyl group-containing resin, it may be used not only in applications where alkaline development is performed, but also in applications where alkaline development is not performed. The ethylenically unsaturated double bond is preferably derived from acrylic acid or methacrylic acid or a derivative thereof. When only a carboxyl group-containing resin without an ethylenically unsaturated double bond is used, the above-mentioned (B) compound having at least one acryloyl group or methacryloyl group in one molecule is necessary to make the composition photocurable. Specific examples of the carboxyl group-containing resin include the following compounds (which may be either oligomers or polymers).

[0044] (1) Carboxyl group-containing resins obtained by copolymerizing unsaturated carboxylic acids such as (meth)acrylic acid with unsaturated group-containing compounds such as styrene, α-methylstyrene, lower alkyl (meth)acrylates, and isobutylene (lower alkyl (meth)acrylates include methyl (meth)acrylate, etc.).

[0045] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0046] (3) Carboxylic acid-containing photosensitive urethane resins obtained by the polyaddition reaction of diisocyanates with (meth)acrylates of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins, and biphenol type epoxy resins, or their partial acid anhydride modified products, carboxyl group-containing dialcohol compounds, and diol compounds.

[0047] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).

[0048] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3).

[0049] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.

[0050] (7) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.

[0051] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.

[0052] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.

[0053] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0054] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0055] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11).

[0056] In this specification, (meth)acrylate is a term that collectively refers to acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.

[0057] The carboxyl group-containing resins that can be used in the present invention are not limited to those listed above. The carboxyl group-containing resins listed above may be used alone or in combination.

[0058] In the present invention, in consideration of the developability and drawing ability of the resist pattern when using a weak alkaline developer such as an aqueous sodium carbonate solution, the acid value of the carboxyl group-containing resin is preferably in the range of 30 to 150 mgKOH / g, more preferably in the range of 50 to 120 mgKOH / g. The higher the acid value of the carboxyl group-containing resin, the better the developability, but the exposed area is more likely to be dissolved by the developer, and the exposed area may be dissolved and peeled off by the developer without distinction between the exposed area and the unexposed area.

[0059] The weight average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally in the range of 1,500 to 150,000, preferably in the range of 1,800 to 100,000. By using a carboxyl group-containing resin having a weight average molecular weight of 2,000 or more, it is possible to improve the resolution and tack-free performance. In addition, by using a carboxyl group-containing resin having a weight average molecular weight of 150,000 or less, it is possible to improve the developability and storage stability. The weight average molecular weight can be measured by gel permeation chromatography (GPC).

[0060] The amount of the carboxyl group-containing resin is preferably 20.0% by mass or more and 40.0% by mass or less, more preferably 20.0% by mass or more and 30.0% by mass or less, calculated as solid content, based on the total amount of the photosensitive resin composition. By making the amount of the carboxyl group-containing resin 20.0% by mass or more, the photoreactivity of the photosensitive resin composition can be improved. In addition, by making the amount of the carboxyl group-containing resin 40.0% by mass or less, the coefficient of linear thermal expansion can be reduced.

[0061] (thermosetting component) The photosensitive resin composition of the present invention may contain a thermosetting component in addition to the above-mentioned components. Examples of the thermosetting component include known and commonly used components such as isocyanate compounds, blocked isocyanate compounds, amino resins, maleimide compounds, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, epoxy resins, oxetane compounds, and episulfide resins. Among these, the preferred thermosetting component is an epoxy resin.

[0062] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, biphenyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, triphenylmethane type epoxy resins, and the like. These may be used alone or in combination of two or more.

[0063] Examples of commercially available epoxy resins include jER 828, 806, 807, YX8000, YX8034, and 834 manufactured by Mitsubishi Chemical Corporation; YD-128, YDF-170, ZX-1059, and ST-3000 manufactured by Nippon Steel Chemical & Material Co., Ltd.; EPICLON 830, 835, 840, 850, N-730A, and N-695 manufactured by DIC Corporation; and RE-306 manufactured by Nippon Kayaku Co., Ltd.

[0064] The equivalent weight of the epoxy group of the epoxy resin in the photosensitive resin composition is preferably 0.5 to 2.5 in terms of solid content relative to the equivalent weight of the carboxyl group of the carboxyl group-containing resin (1). By making it 0.5 equivalent weight or more, it is possible to prevent the carboxyl group from remaining in the cured product, and to obtain good heat resistance, alkali resistance, electrical insulation, etc. Also, by making the blending amount 2.5 equivalent weight or less, it is possible to prevent the low molecular weight cyclic (thio)ether group from remaining in the dried coating film, and to ensure good strength of the cured product, etc.

[0065] When the photosensitive resin composition of the present invention contains a thermosetting component, it may contain a thermosetting catalyst for promoting the curing of the thermosetting component. Examples of the thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. Other commercially available compounds include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT 3513N (trade name of dimethylamine-based compound), DBU, DBN, and U-CAT SA 102 (all bicyclic amidine compounds and salts thereof) manufactured by San-Apro Co., Ltd.

[0066] The compounds are not limited to the above, and may be used alone or in combination of two or more as long as they are heat curing catalysts for epoxy resins or oxetane compounds, or catalysts that promote the reaction of at least one of epoxy groups and oxetanyl groups with carboxyl groups. In addition, S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct may also be used, and preferably, these compounds that also function as adhesion promoters are used in combination with the heat curing catalyst.

[0067] The thermosetting catalyst may be used alone or in combination of two or more. The amount of the thermosetting catalyst is preferably 0.1% by mass or more and 10.0% by mass or less, and more preferably 0.3% by mass or more and 5.0% by mass or less, in terms of solid content, based on the total amount of the photosensitive resin composition, from the viewpoint of the storage stability of the photosensitive resin composition and the heat resistance of the cured coating film.

[0068] (cation scavenger) The cation scavenger may be a compound capable of capturing cations by ion exchange. The cation scavenger may be used alone or in combination of two or more.

[0069] The cation scavenger is preferably an inorganic compound having a positively or negatively charged layer structure, and more preferably an inorganic compound having a positively charged layer structure. In particular, the ion exchange capacity of the cation scavenger is preferably Na + is 2.0 meq / g or more, or Cu 2+ It is preferable that the molecular weight is 2.2 meq / g or more.

[0070] An example of a cation scavenger is hydrotalcite, which is a compound represented by the following formula (1). Mg a Al b (OH) c (CO3) d nH2O (1) (In formula (1), a, b, c, and d are positive numbers and satisfy 2a+3b-c-2d=0. Also, n represents the number of hydrations and is 0 or a positive number, preferably 1 to 5.)

[0071] In the formula (1), a part of Mg may be replaced by other divalent metal ions, and among the other divalent metal ions, Zn is particularly preferred.

[0072] Specific examples of hydrotalcite include, but are not limited to, Mg 4.5 Al2(OH) 13CO3·nH2O, Mg5Al 1.5 (OH) 12.5 CO3·nH2O, Mg6Al2(OH) 16 CO3·nH2O, Mg 4.2 Al2(OH) 12.4 CO3·nH2O, Mg 4.3 Al2(OH) 12.6 CO3·nH2O, Mg 2.5 Zn2Al2(OH) 13 CO3·nH2O, Mg 4.2 Al2(OH) 12.4 CO3·nH2O, Mg 4.2 Al2(OH) 12.4 CO3·nH2O, Mg4Al2(OH) 12 CO3·nH2O, etc. (where n represents the number of hydrations, which is 0 or a positive number, preferably 1 to 5). Among these, Mg 4.3 Al2(OH) 12.6 CO3·nH2O is preferred.

[0073] In the hydrotalcite represented by formula (1), a / b is preferably 1.5 or more and 5 or less, more preferably 1.7 or more and 3 or less, and even more preferably 1.8 or more and 2.5 or less.

[0074] As the cation scavenger, commercially available products may be used, for example, "IXEPLAS-A1", "IXEPLAS-A2", "IXEPLAS-B1" and the like manufactured by Toagosei Co., Ltd.

[0075] The amount of the cation scavenger is 0.2 mass% or more, preferably 0.2 mass% or more and 5.0 mass% or less, more preferably 0.2 mass% or more and 3.0 mass% or less, calculated as solid content, based on the total amount of the photosensitive resin composition. By making the amount of the cation scavenger 0.2 mass% or more, the insulation reliability can be improved.

[0076] (Coloring agent) A colorant can be blended in the photosensitive resin composition of the present invention. The colorant is not particularly limited, and known colorants such as red, blue, green, and yellow can be used. Any of pigments, dyes, and coloring matters can be used, but from the viewpoint of reducing the environmental load and having little effect on the human body, a colorant that does not contain halogen is preferable.

[0077] Red colorants include monoazos, disazos, azo lakes, benzimidazolone, perylene, diketopyrrolopyrrole, condensed azos, anthraquinones, and quinacridones. Specific examples of red colorants include those having the following Color Index (CI; published by The Society of Dyers and Colourists) numbers:

[0078] Examples of monoazo red colorants include Pigment Red 1, 2, 3, 4, 5, 6, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 112, 114, 146, 147, 151, 170, 184, 187, 188, 193, 210, 245, 253, 258, 266, 267, 268, and 269. Examples of disazo red colorants include Pigment Red 37, 38, and 41. Examples of monoazo lake-based red colorants include Pigment Red 48:1, 48:2, 48:3, 48:4, 49:1, 49:2, 50:1, 52:1, 52:2, 53:1, 53:2, 57:1, 58:4, 63:1, 63:2, 64:1, and 68. Examples of benzimidazolone-based red colorants include Pigment Red 171, 175, 176, 185, and 208. Examples of perylene-based red colorants include Solvent Red 135, 179, Pigment Red 123, 149, 166, 178, 179, 190, 194, and 224. Examples of diketopyrrolopyrrole red colorants include Pigment Red 254, 255, 264, 270, and 272. Examples of condensed azo red colorants include Pigment Red 220, 144, 166, 214, 220, 221, and 242. Examples of anthraquinone red colorants include Pigment Red 168, 177, and 216, Solvent Red 149, 150, 52, and 207. Examples of quinacridone red colorants include Pigment Red 122, 202, 206, 207, and 209.

[0079] Blue colorants include phthalocyanine and anthraquinone types, and pigment types include compounds classified as pigments, such as Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, and 60. Dye types include Solvent Blue 35, 63, 68, 70, 83, 87, 94, 97, 122, 136, 67, and 70. In addition to the above, metal-substituted or unsubstituted phthalocyanine compounds can also be used.

[0080] Examples of yellow colorants include monoazo, disazo, condensed azo, benzimidazolone, isoindolinone, and anthraquinone. For example, anthraquinone yellow colorants include Solvent Yellow 163, Pigment Yellow 24, 108, 193, 147, 199, and 202. Examples of isoindolinone yellow colorants include Pigment Yellow 110, 109, 139, 179, and 185. Examples of condensed azo yellow colorants include Pigment Yellow 93, 94, 95, 128, 155, 166, and 180. Examples of benzimidazolone yellow colorants include Pigment Yellow 120, 151, 154, 156, 175, and 181. Examples of monoazo yellow colorants include Pigment Yellow 1, 2, 3, 4, 5, 6, 9, 10, 12, 61, 62, 62:1, 65, 73, 74, 75, 97, 100, 104, 105, 111, 116, 167, 168, 169, 182, and 183. Examples of disazo yellow colorants include Pigment Yellow 12, 13, 14, 16, 17, 55, 63, 81, 83, 87, 126, 127, 152, 170, 172, 174, 176, 188, and 198.

[0081] In addition, colorants such as purple, orange, brown, and black may be added. Specific examples include Pigment Black 1, 6, 7, 8, 9, 10, 11, 12, 13, 18, 20, 25, 26, 28, 29, 30, 31, and 32, Pigment Violet 19, 23, 29, 32, 36, 38, and 42, Solvent Violet 13 and 36, CI Pigment Orange 1, 5, 13, 14, 16, 17, 24, 34, 36, 38, 40, 43, 46, 49, 51, 61, 63, 64, 71, and 73, Pigment Brown 23 and 25, and carbon black.

[0082] The amount of the colorant blended is preferably 0.3% by mass or more and 1.0% by mass or less, and more preferably 0.3% by mass or more and 0.6% by mass or less, calculated as solid content based on the total amount of the photosensitive resin composition.

[0083] (Organic solvent) The photosensitive resin composition of the present invention may contain an organic solvent for the purpose of adjusting the viscosity when preparing the composition or when applying it to a substrate or film. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, diethylene glycol monoethyl ether acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Known and commonly used organic solvents can be used. These organic solvents may be used alone or in combination of two or more kinds.

[0084] The amount of the organic solvent to be added is not particularly limited, and can be appropriately set according to the target viscosity so as to facilitate the preparation of the photosensitive resin composition.

[0085] (Other added ingredients) The photosensitive resin composition of the present invention may further contain, as necessary, components such as cyanate compounds, elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper inhibitors, antioxidants, rust inhibitors, thickeners, at least one of silicone-based, fluorine-based, and polymer-based defoamers and leveling agents, imidazole-based, thiazole-based, and triazole-based silane coupling agents, and phosphorus compounds such as phosphinates, phosphate ester derivatives, and phosphazene compounds. These may be known in the field of electronic materials.

[0086] The photosensitive resin composition of the present invention may be used in the form of a dry film.

[0087] [Preparation method] In preparing the photosensitive resin composition of the present invention, each component is weighed, mixed, and then pre-mixed with a mixer, and then each component is dispersed and kneaded in a kneader to prepare the photosensitive resin composition.

[0088] Examples of the kneading machine include a bead mill, a ball mill, a sand mill, a three-roll mill, and a two-roll mill. Among these, it is preferable to use a bead mill in order to improve dispersibility. Dispersion conditions such as the type and particle size of the beads of the bead mill can be appropriately set according to the desired viscosity.

[0089] [Application] The photosensitive resin composition according to the present invention is useful for forming a pattern layer as a permanent coating for a printed wiring board, such as a solder resist, a coverlay, an interlayer insulating layer, etc., and is particularly useful for forming a solder resist. In addition, since the photosensitive resin composition according to the present invention can form a cured product having excellent film strength even in a thin film, it can also be suitably used for forming a pattern layer in a printed wiring board that requires a thin film, such as a package substrate (a printed wiring board used for a semiconductor package).

[0090] Furthermore, the photosensitive resin composition of the present invention can be used not only for forming a pattern layer of a cured coating film, but also for applications in which a pattern layer is not formed, such as molding applications (sealing applications).

[0091] [Dry film] The photosensitive resin composition of the present invention can also be in the form of a dry film comprising a first film and a resin layer formed on the first film as a dried coating of the photosensitive resin composition. The first film in the present invention refers to a film that is at least adhered to the resin layer when the resin layer side formed on the dry film is laminated by heating or the like so as to contact a base material such as a substrate and integrally molded. The first film may be peeled off from the resin layer in a process after lamination. In particular, in the present invention, it is preferable to peel off from the resin layer in a process after exposure. When forming a dry film, the photosensitive resin composition of the present invention is diluted with the organic solvent to adjust the viscosity to an appropriate level, and applied to a uniform thickness on the first film using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and usually dried at a temperature of 50 to 130 ° C. for 1 to 30 minutes to obtain a film. There is no particular restriction on the coating thickness, but it is generally appropriately selected within the range of 1 to 150 μm, preferably 5 to 60 μm, in terms of the thickness after drying.

[0092] As the first film, any known film can be used without any particular limitation, and for example, a film made of a thermoplastic resin such as a polyester film such as polyethylene terephthalate or polyethylene naphthalate, a polyimide film, a polyamideimide film, a polypropylene film, or a polystyrene film can be suitably used. Among these, a polyester film is preferred from the viewpoints of heat resistance, mechanical strength, handling, etc. A laminate of these films can also be used as the first film.

[0093] From the viewpoint of improving mechanical strength, the above-mentioned thermoplastic resin film is preferably a film stretched in a uniaxial or biaxial direction.

[0094] The thickness of the first film is not particularly limited, but can be, for example, 10 μm to 150 μm.

[0095] After forming a resin layer consisting of a dried coating film of the photosensitive resin composition of the present invention on the first film, it is preferable to further laminate a peelable second film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer. The second film in the present invention refers to a film that is peeled off from the photosensitive resin layer before lamination when the resin layer side of the photosensitive film laminate is laminated by heating or the like so as to be in contact with a base material such as a substrate and integrally molded. As the peelable second film, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, a surface-treated paper, etc. can be used, and it is sufficient that the adhesive force between the resin layer and the second film is smaller than the adhesive force between the resin layer and the first film when the second film is peeled off.

[0096] The thickness of the second film is not particularly limited, but can be, for example, 10 μm to 150 μm.

[0097] To prepare a cured coating film on a printed wiring board using a dry film, the second film is peeled off from the dry film, and the exposed resin layer of the dry film is placed on a substrate on which a circuit is formed, and the two are laminated using a laminator or the like to form a resin layer on the substrate on which a circuit is formed. The formed resin layer is then exposed to light, developed, and cured by heating to form a cured coating film. The second film may be peeled off either before or after exposure.

[0098] [Cured product] The cured product of the present invention is obtained by curing the photosensitive resin composition of the present invention or the resin layer of the dry film of the present invention. The manufacturing conditions such as curing conditions will be described later in [Printed wiring board]. The cured product of the present invention can be suitably used for printed wiring boards, electronic parts, etc.

[0099] [Printed wiring board] The printed wiring board of the present invention has a cured product obtained from the resin layer of the photosensitive resin composition or dry film of the present invention. As a method for producing the printed wiring board of the present invention, for example, the photosensitive resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and applied to a substrate by a method such as dip coating, flow coating, roll coating, bar coater, screen printing, or curtain coating, and then the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of 60 to 100°C for 15 to 90 minutes to form a tack-free resin layer. In addition, in the case of a dry film, the resin layer is attached to the substrate by a laminator or the like so that the resin layer contacts the substrate, and then the first film is peeled off to form a resin layer on the substrate.

[0100] The above-mentioned substrates include printed wiring boards and flexible printed wiring boards on which circuits have already been formed using copper or the like, as well as materials such as copper-clad laminates for high-frequency circuits made from paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, fluororesin-polyethylene-polyphenylene ether, polyphenylene oxide-cyanate, etc., including copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc.

[0101] The dry film is preferably laminated onto the substrate under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a circuit-formed substrate is used, even if the surface of the substrate is uneven, the dry film adheres closely to the substrate, so that no air bubbles are mixed in, and the filling of the recesses on the substrate surface is improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.

[0102] The volatilization drying carried out after the photosensitive resin composition of the present invention is applied to a substrate can be carried out using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method of countercurrent contact of hot air in a dryer using a heat source of an air heating method using steam, and a method of blowing hot air onto a substrate from a nozzle). As an apparatus, a hot air circulation drying oven such as DF610 manufactured by Yamato Scientific Co., Ltd. can be mentioned.

[0103] After forming a resin layer on a substrate, the resin layer is selectively exposed to active energy rays through a photomask having a predetermined pattern formed thereon, and the unexposed areas are developed with a dilute alkaline aqueous solution (e.g., 0.3 to 3.0 mass % sodium carbonate aqueous solution) to form a pattern of the cured product. In the case of a dry film, after exposure, the first film is peeled off from the dry film and development is carried out to form a patterned cured product on the substrate. Note that, as long as the characteristics are not impaired, the first film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed.

[0104] The exposure machine used for the above-mentioned active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm, and further, a direct imaging machine (for example, a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1,000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 As an example of the exposure device, HMW-680-GW20 manufactured by Oak Manufacturing Co., Ltd., etc., may be used as an exposure device equipped with a metal halide lamp.

[0105] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.

[0106] Furthermore, the cured product is irradiated with active energy rays and then heat-cured (for example, at a temperature of 100 to 220°C for 30 to 90 minutes), or irradiated with active energy rays after heat-curing (for example, at 1,000 to 2,000 mJ / cm 2), or by heat curing only for final finish curing (main curing), a cured coating film with excellent properties such as adhesion and hardness is formed. As an example of the equipment, QRM-2082 manufactured by Oak Seisakusho Co., Ltd. is a UV conveyor using a high-pressure mercury lamp. EXAMPLES

[0107] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.

[0108] (Preparation of inorganic filler A-1 dispersion) 70 g of spherical silica particles (SO-C2 manufactured by Admatechs Co., Ltd., average particle size: 500 nm), 28 g of propylene glycol monomethyl ether acetate as a solvent, and 2 g of a silane coupling agent having a methacryl group (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.) were uniformly dispersed to obtain a dispersion of methacrylsilane-treated inorganic filler A-1 with a solid content of 70%.

[0109] (Preparation of inorganic filler A-2 dispersion) 70 g of spherical silica particles (SFP-30MHE manufactured by Denka Co., Ltd., average particle size: 600 nm), 28 g of propylene glycol monomethyl ether acetate as a solvent, and 2 g of a silane coupling agent having a methacryl group (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.) were uniformly dispersed to obtain a dispersion of methacrylsilane-treated inorganic filler A-2 with a solid content of 70%.

[0110] (Synthesis of Carboxyl Group-Containing Resin E-1) In a flask equipped with a cooling tube and a stirrer, 456 parts of bisphenol A, 228 parts of water, and 649 parts of 37% formalin were charged, and the temperature was kept below 40°C, and 228 parts of 25% aqueous sodium hydroxide solution was added. After the addition was completed, the mixture was reacted at 50°C for 10 hours. After the reaction was completed, the mixture was cooled to 40°C, and neutralized to pH 4 with 37.5% aqueous phosphoric acid solution while keeping the temperature below 40°C. The mixture was then left to stand and the aqueous layer was separated. After the separation, 300 parts of methyl isobutyl ketone was added and dissolved uniformly, and the mixture was washed three times with 500 parts of distilled water, and water, solvent, etc. were removed under reduced pressure at a temperature below 50°C. The obtained polymethylol compound was dissolved in 550 parts of methanol to obtain 1230 parts of a methanol solution of the polymethylol compound. A part of the obtained methanol solution of the polymethylol compound was dried at room temperature in a vacuum dryer, and the solid content was 55.2%. 500 parts of the resulting methanol solution of the polymethylol compound and 440 parts of 2,6-xylenol were charged and dissolved uniformly at 50°C. After the mixture was dissolved uniformly, methanol was removed under reduced pressure at a temperature of 50°C or less. Then, 8 parts of oxalic acid was added and reacted at 100°C for 10 hours. After the reaction was completed, the distillate was removed under reduced pressure at 180°C and 50 mmHg to obtain 550 parts of novolak resin A. Further, 130 parts of the above novolak resin A, 2.6 parts of a 50% aqueous sodium hydroxide solution, and 100 parts of toluene / methyl isobutyl ketone (mass ratio = 2 / 1) were charged into an autoclave equipped with a thermometer, a nitrogen introducing device / alkylene oxide introducing device, and a stirrer, and the inside of the system was replaced with nitrogen while stirring. Next, the temperature was increased to 150°C and 8 kg / cm 2 45 parts of ethylene oxide was gradually introduced and reacted at a gauge pressure of 0.0 kg / cm. 2 After the reaction was continued for about 4 hours until the reaction solution reached a state where the mixture was cooled to room temperature. 3.3 parts of a 36% aqueous hydrochloric acid solution was added and mixed to neutralize the sodium hydroxide. The neutralized reaction product was diluted with toluene, washed with water three times, and the solvent was removed using an evaporator to obtain an ethylene oxide adduct of novolak resin A with a hydroxyl value of 175 g / eq. This product had an average of 1 mole of ethylene oxide added per equivalent of phenolic hydroxyl group. 175 parts of the ethylene oxide adduct of the novolak resin A thus obtained, 50 parts of acrylic acid, 3.0 parts of p-toluenesulfonic acid, 0.1 parts of hydroquinone monomethyl ether, and 130 parts of toluene were charged into a reactor equipped with a stirrer, a thermometer, and an air-inlet tube, and the mixture was stirred while blowing in air, heated to 115°C, and reacted for another 4 hours while distilling off the water generated by the reaction as an azeotropic mixture with toluene, and then cooled to room temperature. The resulting reaction solution was washed with a 5% aqueous NaCl solution, and the toluene was removed by distillation under reduced pressure, and diethylene glycol monoethyl ether acetate was added to obtain an acrylate resin solution with a solid content of 68%. Next, 312 parts of the obtained acrylate resin solution, 0.1 parts of hydroquinone monomethyl ether, and 0.3 parts of triphenylphosphine were charged into a four-neck flask equipped with a stirrer and a reflux condenser, and this mixture was heated to 110°C, 45 parts of tetrahydrophthalic anhydride was added, and the mixture was reacted for 4 hours. After cooling, a solution of carboxyl group-containing resin E-1 with a solid content of 70% and an acid value of the solid content of 65 mgKOH / g was obtained.

[0111] (Synthesis of carboxyl group-containing resin E-2) 220 parts of cresol novolac epoxy resin (EPICLON N-695, epoxy equivalent: 220, manufactured by DIC Corporation) was placed in a four-neck flask equipped with a stirrer and a reflux condenser, and 214 parts of carbitol acetate was added and dissolved by heating. Next, 0.1 parts of hydroquinone as a polymerization inhibitor and 2.0 parts of dimethylbenzylamine as a reaction catalyst were added. This mixture was heated to 95-105°C, and 72 parts of acrylic acid were gradually added dropwise and reacted for 16 hours. This reaction product was cooled to 80-90°C, and 106 parts of tetrahydrophthalic anhydride was added, reacted for 8 hours, cooled, and then taken out. In this way, a solution of carboxyl group-containing resin E-2 having a solid content of 65%, a solid matter acid value of 100 mgKOH / g, and a weight average molecular weight Mw of about 3,500 was obtained.

[0112] [Examples 1 to 15, Comparative Examples 1 to 4] (Preparation of Photosensitive Resin Composition) For each composition, the components were mixed according to the recipe shown in Tables 1 and 2 below, stirred with a stirrer, and then kneaded with a three-roll mill to prepare a photosensitive resin composition. Each value in the tables indicates parts by mass (equivalent to solid content).

[0113] [Table 1]

[0114] [Table 2]

[0115] Details of each component in Tables 1 and 2 are as follows. *1: YA010C: Spherical silica, average particle size 10 nm, methacrylic surface treatment, manufactured by Admatechs Co., Ltd. *2: DA-600: Dipentaerythritol hexaacrylate, manufactured by Sanyo Chemical Industries, Ltd. *3: Omnirad 819: Acylphosphine oxide photopolymerization initiator, manufactured by IGM Resins *4: PGM-AC-2140Y: Spherical silica, average particle size 12 nm, surface area 230 m 2 / g, methacrylic surface treatment, methacrylic treatment rate less than 50%, density 2.0-2.2, Nissan Chemical Co., Ltd. *5: PGM-AC-3140Y: Spherical silica, average particle size 22 nm, surface area 120 m 2 / g, methacrylic surface treatment rate less than 50%, density 2.0-2.2, Nissan Chemical Co., Ltd. *6: PGM-AC-4130Y: Spherical silica, average particle size 45 nm, surface area 60 m 2 / g, methacrylic surface treatment rate less than 50%, density 2.0-2.2, Nissan Chemical Co., Ltd. *7:PMA-ST: Spherical silica, average particle size 12nm, surface area 230m 2 / g, no surface treatment, density 2.0-2.2, Nissan Chemical Co., Ltd. *8: PL-1: Spherical silica, average particle size 15 nm, surface treated, density 0.86-1.16, manufactured by Fuso Chemical Co., Ltd. *9: N-730A: Phenol novolac epoxy resin, manufactured by DIC Corporation *10: VG3101L: Trifunctional epoxy resin, manufactured by Air Water Inc. *11: IXEPLAS-A1: Cation scavenger, hydrotalcite, manufactured by Toagosei Co., Ltd. *12: BYK-361N: Surface conditioner, manufactured by BYK Japan *13: QS-30: Polymerization inhibitor, manufactured by Air Water Performance Chemical Inc.

[0116] (Preparation of dry film) Each of the photosensitive resin compositions prepared above was applied onto a first film (T-60, manufactured by Toray Industries, Inc., thickness 38 μm) using an applicator so that the film thickness after drying would be 20 μm, and then dried at 80° C. for 10 minutes in a hot air circulation drying oven to obtain a dry film having a resin layer consisting of a dried coating film of each photosensitive resin composition.

[0117] (Measurement of Melt Viscosity of Photosensitive Composition) The melt viscosity (dPa s) at 100°C of each of the photosensitive compositions prepared above was measured using a vacuum laminator CVP-300 (manufactured by Nikko Materials Co., Ltd.) by laminating the dry films prepared above at a lamination temperature of 30 to 40°C to prepare a resin layer 300 μm thick and 20 mm wide, and using a rheometer MARS40 under the following conditions. The measurement results are shown in Tables 3 and 4. (Melt viscosity measurement conditions) Heating rate: 5℃ / min Frequency: 1Hz Pressure: 3Pa

[0118] (Embeddability) Using each of the photosensitive compositions prepared above, the embeddability was evaluated by the following method. The dry film was heat laminated on a substrate having a lattice pattern at 100°C for 1 minute using a vacuum laminator (CVP-300, manufactured by Nikko Materials Co., Ltd.) and pressed at 80°C for 1 minute to obtain an evaluation substrate. The number of bubbles generated in the evaluation substrate was confirmed using an optical microscope, and the embeddability was evaluated from the rate of bubbles generated. The embeddability was evaluated according to the following criteria, and the results are shown in Tables 3 and 4. Evaluation results of "◎" to "△" are acceptable. [Evaluation Criteria] ◎: 0% or more but less than 10% ○: 10% to less than 30% △: 30% to less than 60% ×: 60% or more

[0119] (Measurement of thermal expansion coefficient) The thermal expansion coefficient was measured by the following method using each of the photosensitive compositions prepared above. The dry film was heat laminated on copper foil at 100°C for 1 minute using a vacuum laminator (CVP-300, manufactured by Nikko Materials Co., Ltd.), and pressed at 80°C for 1 minute. After that, the entire surface was exposed to an optimal exposure amount using an exposure device equipped with a high-pressure mercury lamp (short arc lamp). After peeling off the first film, a 1% by mass Na2CO3 aqueous solution at 30°C was sprayed at a pressure of 2 kg / cm. 2 After development, the film was transferred to a UV conveyor with an integrated light dose of 2000 mJ / cm 2 The resulting cured coating was photocured at 400°C and then heated in a hot air circulating drying oven at 170°C for 60 minutes to obtain a cured coating film. The average linear thermal expansion coefficient of the resulting cured coating film (3mm x 10mm size) was measured twice under the following conditions using a TMA-Q400EM1797, and the linear expansion coefficient was determined using the results of the second measurement. The linear expansion coefficient was evaluated according to the following criteria, and the evaluation results are shown in Tables 3 and 4. (Measurement conditions) Heating rate: 10℃ / min Test load: 5g [Evaluation Criteria] Thermal expansion coefficient α1 〇:35ppm or less ×: More than 35ppm Thermal expansion coefficient α2 〇: 100ppm or less ×: More than 100ppm

[0120] [Table 3]

[0121] [Table 4]

Claims

1. A photosensitive resin composition comprising: (A) an inorganic filler; (B) a compound having at least one acryloyl group or methacryloyl group in one molecule; (C) a photopolymerization initiator; and (D) an inorganic colloid, the total amount of the inorganic filler (A) and the inorganic colloid (D) is 30.0 mass% or more in terms of solid content with respect to the total amount of the photosensitive resin composition; the blending amount of the inorganic colloid (D) is 2.0 mass% or more in terms of solid content with respect to the total amount of the photosensitive resin composition, A photosensitive resin composition having a melt viscosity at 100°C of less than 1000 dPa·s.

2. The surface area of ​​the inorganic colloid (D) is 100 m 2 The photosensitive resin composition according to claim 1, wherein the photosensitive resin composition has a molecular weight of 1 / g or more.

3. 2. The photosensitive resin composition according to claim 1, wherein the inorganic colloid (D) is colloidal silica having an average particle size of 30 nm or less and having a surface treated with a silane coupling agent.

4. 4. The photosensitive resin composition according to claim 3, wherein the colloidal silica has acryloyl or methacryloyl groups added to less than 50% of the total surface area.

5. 4. The photosensitive resin composition according to claim 3, wherein the colloidal silica is derived from sodium silicate.

6. 4. The photosensitive resin composition according to claim 3, wherein the colloidal silica has a density of 1.9 to 2.

2.

7. 2. The photosensitive resin composition according to claim 1, wherein the inorganic filler (A) has an average particle size of 200 nm or more and less than 1000 nm.

8. 2. The photosensitive resin composition according to claim 1, wherein the inorganic filler (A) is silica having an acryloyl group or a methacryloyl group added to its surface by a silane coupling treatment.

9. The photosensitive resin composition according to claim 1 , wherein the inorganic filler (A) and the inorganic colloid (D) are spherical.

10. 2. The photosensitive resin composition according to claim 1, wherein a ratio of an average particle size of the inorganic filler (A) to an average particle size of the inorganic colloid (D) is 8 or more.

11. The photosensitive resin composition according to claim 1 , further comprising (E) a carboxyl group-containing resin.

12. A dry film comprising a first film and a resin layer formed on the first film and comprising a dry coating film of the photosensitive resin composition according to any one of claims 1 to 11.

13. A cured product obtained by curing the photosensitive resin composition according to any one of claims 1 to 11.

14. A cured product obtained by curing the resin layer of the dry film according to claim 12.

15. A printed wiring board comprising the cured product according to claim 13.

16. A printed wiring board comprising the cured product according to claim 14.

Citation Information

Patent Citations

  • Photocurable thermosetting resin composition, dry film and cured product thereof, and printed wiring board using those

    JP2011013486A