The polylactic acid resin foam sheet, enhanced with specific modifiers and cell diameter ratios, addresses brittleness and flexibility issues, achieving high mechanical strength and moldability while being environmentally friendly.
Patent Information
- Application Number
- JP2024050324
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-15
AI Technical Summary
Polylactic acid resins exhibit brittleness, poor impact resistance, and poor flexibility, making them difficult to mold into complex shapes while maintaining mechanical strength.
A polylactic acid resin foam sheet containing a brittleness modifier, such as butadiene rubber or acrylic rubber, with specific cell diameter ratios and compressive stress values, along with a biodegradable aliphatic polyester resin, to enhance mechanical strength and moldability.
The solution improves brittleness and achieves both high mechanical strength and moldability, reducing environmental impact.
Smart Images

Figure 2024146849000004 
Figure 2024146849000005 
Figure 2024146849000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a polylactic acid resin foamed sheet, a molded article, and a foamed board. [Background technology]
[0002] Containers formed from thermoplastic foamed sheets (foamed sheets) are widely used as containers for foods, etc. For example, containers formed from foamed sheets having a foam layer are widely used as containers for foods such as instant noodles that are cooked by pouring hot water into them.
[0003] In recent years, in consideration of the global environment, there has been a demand for the use of resins that can reduce the environmental load. Known examples of resins that can reduce the environmental load include biodegradable resins such as polylactic acid resins and plant-derived resins. For example, Patent Document 1 proposes a polylactic acid resin foam sheet, which is a biodegradable resin, and a polylactic acid resin foam molded article using the same. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-359910 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, polylactic acid resins have the problem that they are inferior to other resins in terms of brittleness and have poor impact resistance (poor toughness). In addition, the polylactic acid resin foam sheet has a problem that it is poor in conformity to the curved surface of a mold due to its poor flexibility, and the foam sheet is difficult to stretch, resulting in poor moldability. When an attempt is made to impart flexibility to the sheet in order to improve moldability, the mechanical strength is deteriorated. These properties are in a trade-off relationship, and it is difficult to achieve both. In Patent Document 1, moldability and heat resistance are considered, but improvement of brittleness is not considered, and achieving both high mechanical strength and moldability is not considered.
[0006] Therefore, an object of the present invention is to provide a polylactic acid resin foamed sheet, molded product, and foamed board that can reduce the environmental load, improve brittleness, and combine high mechanical strength with moldability. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention has the following aspects. [1] A polylactic acid-based resin foam sheet comprising a polylactic acid-based resin and a brittleness modifier, The compressive stress determined in accordance with JIS K 6400-2:2012 when the cushioning coefficient determined in accordance with JIS Z 0235:2002 is 10 or less is 0.20 MPa or more and 0.70 MPa or less, A polylactic acid resin foam sheet, in which the relationship between average cell diameters in each direction measured by the following measurement method satisfies both of the following formulas (1) and (2). 0.20 <D VD / {0.5×(D MD +D TD )}<0.50···(1) 400<(D MD ×D TD ×D VD ) 1 / 3 <900···(2) (In the formula (1) and the formula (2), D MD , D TD , D VD are the average bubble diameters in the extrusion direction (MD), width direction (TD), and thickness direction (VD) of the foamed sheet, respectively, and are expressed in μm. <Average cell diameter in each direction of polylactic acid resin foam sheet> A sample for cross-sectional observation was cut out from the center of the width direction of the foamed sheet, and the average bubble diameter was measured using a scanning electron microscope in the extrusion direction (MD), the direction perpendicular to the extrusion direction (TD cross section), and the thickness direction perpendicular to each direction (VD direction). MD , D TD , D VD Let us assume that. [2] The polylactic acid-based resin foam sheet according to [1], wherein the brittleness modifier is a butadiene-based rubber, and the rubber content is 0.30 parts by mass or more and 4.0 parts by mass or less per 100 parts by mass of the polylactic acid-based resin. [3] The polylactic acid-based resin foam sheet according to [1], wherein the brittleness modifier is an acrylic rubber, and the content of the acrylic rubber is 1.0 part by mass or more and 8.0 parts by mass or less per 100 parts by mass of the polylactic acid-based resin. [4] The polylactic acid-based resin foam sheet according to [1], wherein the brittleness modifier is a biodegradable aliphatic polyester-based resin, and the content of the biodegradable aliphatic polyester-based resin is 5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the polylactic acid-based resin. [5] The polylactic acid resin foam sheet according to [4], wherein the biodegradable aliphatic polyester resin is polybutylene succinate. [6] The polylactic acid resin foam sheet according to any one of [1] to [5], wherein the required punching energy as measured by a film impact tester is 0.30 J or more. [7] Apparent density 83kg / m 3 ~310kg / m 3 The polylactic acid resin foam sheet according to any one of [1] to [6], [8] The polylactic acid resin foam sheet according to any one of [1] to [7], having an open cell ratio of 25% or less. [9] The polylactic acid-based resin foamed sheet according to any one of [1] to [8], further comprising a cell regulator, the content of the cell regulator being 0.50 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the polylactic acid-based resin.
[10] The polylactic acid resin foam sheet according to any one of [1] to [9], which has a thickness of 0.50 to 5.0 mm.
[11] A molded product obtained by thermoforming the polylactic acid resin foam sheet according to any one of [1] to
[10] .
[12] The molded article according to
[11] , which is a food container.
[13] A foam board obtained by molding the polylactic acid resin foam sheet according to any one of [1] to
[10] into a board shape. Effect of the Invention
[0008] The polylactic acid-based resin foamed sheet, molded article, and foamed board of the present invention can reduce the environmental load, improve brittleness, and achieve both high mechanical strength and moldability. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic diagram showing a method for measuring an average bubble diameter. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a foam sheet manufacturing apparatus. [Diagram 3] FIG. 2 is a perspective view showing an example of a molded body according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following definitions of terms apply throughout the specification and claims. A numerical range expressed by "to" means that the numerical values before and after the "to" are the lower and upper limits of the numerical range. The "unit" constituting the resin means an atomic group formed directly by polymerization of a monomer. In addition, a unit derived from a monomer may be referred to by adding the unit to the name of the monomer. For example, a "butadiene unit" is a unit derived from butadiene.
[0011] <Polylactic acid resin composition> The polylactic acid resin composition for obtaining the polylactic acid resin foamed sheet of the present invention (hereinafter, also simply referred to as "foamed sheet") contains a polylactic acid resin and a brittleness modifier. The polylactic acid resin composition preferably further contains a cell regulator.
[0012] <Polylactic acid resin> The polylactic acid resin contained in the polylactic acid resin composition may be a homopolymer of lactic acid or a copolymer of lactic acid and another monomer. Examples of other monomers constituting the copolymer include aliphatic hydroxycarboxylic acids other than lactic acid, aliphatic polyhydric alcohols, and aliphatic polycarboxylic acids. The monomer may be, for example, a polyfunctional polysaccharide.
[0013] The lactic acid constituting the polylactic acid resin may be either or both of the L-form and the D-form. The polylactic acid-based resin, which is a homopolymer, may be any one of poly(L-lactic acid) resin, poly(D-lactic acid) resin, and poly(DL-lactic acid) resin. In order to provide a foamed layer with excellent strength, it is preferable that the polylactic acid resin contains more units derived from the L-form than units derived from the D-form. However, poly(L-lactic acid) resin containing substantially 100% by mass of L-isomer has excellent mechanical strength, but tends to cause the foam layer to become brittle. Therefore, it is preferable that the polylactic acid resin contained in the polylactic acid resin composition of this embodiment has a proportion (mass proportion) of units derived from the D-form to the total of units derived from the D-form and units derived from the L-form of 0.10 mass% or more. The mass proportion is more preferably equal to or greater than 0.20 mass%, and particularly preferably equal to or greater than 0.30 mass%. If the ratio of units derived from the D-form is high, the foamed layer may not exhibit excellent strength. Therefore, the proportion of units derived from the D-form in the total of units derived from the D-form and units derived from the L-form is preferably 4.0% by mass or less, more preferably 3.5% by mass or less, and particularly preferably 3.0% by mass or less. That is, the mass ratio of units derived from the D-form to units derived from the L-form (D-form / L-form) is preferably within the range of 0.10 / 99.9 to 4 / 96. The same is true for copolymers, in which the mass ratio of units derived from the D-form to units derived from the L-form is preferable.
[0014] Among the other monomers constituting the copolymer, examples of the aliphatic polycarboxylic acids include oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, and dodecanedioic acid. The aliphatic polycarboxylic acid may be an anhydride.
[0015] Examples of the aliphatic polyhydric alcohols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, neopentyl glycol, tetramethylene glycol, and 1,4-cyclohexanedimethanol.
[0016] Examples of the aliphatic hydroxycarboxylic acid other than lactic acid that constitutes the copolymer include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid.
[0017] Examples of the polyfunctional polysaccharides include cellulose, cellulose nitrate, methylcellulose, ethylcellulose, celluloid, viscose rayon, regenerated cellulose, cellophane, cupra, cuprammonium rayon, cuprophane, Bemberg, hemicellulose, starch, acropectin, dextrin, dextran, glycogen, pectin, chitin, chitosan, gum arabic, guar gum, locust bean gum, and acacia gum.
[0018] In the copolymer, it is preferable that units derived from lactic acid (L- and D-forms) account for 60% by mass or more of all units. The content of lactic acid units (L- and D-isomers) is more preferably 70% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more.
[0019] The polylactic acid resin preferably contains a polylactic acid resin in a crosslinked state (crosslinked polylactic acid resin), and it is preferable that the homopolymer is contained as a crosslinked polylactic acid resin in a crosslinked state. In particular, it is preferable that the polylactic acid resin contains a crosslinked polylactic acid resin crosslinked with an organic peroxide. By making at least a part of the polylactic acid resin contained in the polylactic acid resin a crosslinked polylactic acid resin crosslinked with an organic peroxide, it is possible to impart melting properties suitable for foaming to the polylactic acid resin.
[0020] Examples of the organic peroxide for crosslinking the polylactic acid resin include peroxy ester, hydroperoxide, dialkyl peroxide, diacyl peroxide, peroxydicarbonate, peroxyketal, and ketone peroxide.
[0021] Examples of the peroxy ester include t-butylperoxy 2-ethylhexyl carbonate, t-hexylperoxy isopropyl monocarbonate, t-hexylperoxybenzoate, t-butylperoxybenzoate, t-butylperoxylaurate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxyacetate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and t-butylperoxyisopropyl monocarbonate.
[0022] Examples of the hydroperoxide include permethane hydroperoxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide.
[0023] Examples of the dialkyl peroxide include dicumyl peroxide, di-t-butyl peroxide, and 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3.
[0024] Examples of the diacyl peroxide include dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, and di(3-methylbenzoyl) peroxide.
[0025] Examples of the peroxydicarbonate include di(2-ethylhexyl) peroxydicarbonate and diisopropyl peroxydicarbonate.
[0026] Examples of the peroxyketals include 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, 1,1-di-t-butylperoxycyclohexane, 2,2-di(t-butylperoxy)-butane, n-butyl 4,4-di-(t-butylperoxy)valerate, and 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane. Examples of the ketone peroxide include methyl ethyl ketone peroxide and acetylacetone peroxide.
[0027] Crosslinking with the organic peroxide may cause the crosslinked polylactic acid resin to contain components with excessively large molecular weights that will gel when thermally melted, or may cause odor problems due to the decomposition residues of the organic peroxide. The organic peroxide is preferably a peroxyester, since this can suppress the risk of such problems occurring and the resin composition can be easily brought into a state suitable for foaming. Among peroxyesters, the organic peroxide used for crosslinking the polylactic acid resin is preferably a peroxycarbonate-based organic peroxide such as peroxymonocarbonate or peroxydicarbonate. In the present embodiment, the organic peroxide used for crosslinking the polylactic acid resin is preferably a peroxymonocarbonate organic peroxide among peroxycarbonate organic peroxides, and particularly preferably t-butylperoxyisopropylmonocarbonate.
[0028] The amount of the organic peroxide is usually preferably 0.10 part by mass or more, more preferably 0.20 part by mass or more, and even more preferably 0.30 part by mass or more, per 100 parts by mass of the polylactic acid resin before crosslinking. When the amount of the organic peroxide used is equal to or more than the lower limit, the polylactic acid resin is sufficiently crosslinked and easily foamed. The amount of the organic peroxide used is preferably 2.0 parts by mass or less, more preferably 1.5 parts by mass or less, and even more preferably 1.0 part by mass or less. When the amount of the organic peroxide used is equal to or less than the above upper limit, it becomes easier to prevent gel from being mixed into the polylactic acid resin after crosslinking.
[0029] The polylactic acid resin contained in the polylactic acid resin composition preferably has a melt mass flow rate (MFR) of 0.10 g / 10 min or more. The melt mass flow rate of the polylactic acid resin is more preferably 0.50 g / 10 min or more, and further preferably 1.0 g / 10 min or more. The melt mass flow rate of the polylactic acid resin is preferably 10 g / 10 min or less, more preferably 8.0 g / 10 min or less, and even more preferably 5.0 g / 10 min or less.
[0030] The melt mass flow rate (MFR) of a polylactic acid resin or a polylactic acid resin composition can be determined as follows.
[0031] (How to determine the melt mass flow rate (MFR) of polylactic acid resins and polylactic acid resin compositions) The melt mass flow rate (MFR) of polylactic acid resins and polylactic acid resin compositions can be measured in accordance with JIS K 7210:1999. The melt mass flow rate (MFR) can be measured by "b) a method for measuring the time it takes for a piston to move a specified distance" described in Method B of the same standard. The melt mass flow rate (MFR) can be measured using a "Melt Flow Index Tester (Automatic) 120-SAS" manufactured by Yasuda Seiki Seisakusho Co., Ltd. The sample is vacuum dried at 70°C for 5 hours, and then sealed and stored in a desiccator until immediately before measurement. The measurement conditions are as follows. Sample: 3-8g Preheat(1): 200 seconds Preheat (2): 30 seconds Test temperature: 190℃ Test load: 21.18N Piston travel distance (interval): 25mm The test is performed on each sample three times, and the average of the three tests is taken as the melt mass-flow rate (g / 10 min).
[0032] The polylactic acid resin preferably has a mass average molecular weight (Mw) of 200,000 or more and 400,000 or less, and more preferably 250,000 or more and 350,000 or less. The molecular weight of the polylactic acid resin can be determined as follows.
[0033] (How to determine the average molecular weight of polylactic acid resin) The number average molecular weight (Mn), mass average molecular weight (Mw), and Z average molecular weight (Mz) of the polylactic acid resin can be determined as follows. 20 mg of the sample to be measured for molecular weight is dissolved in 6 mL of chloroform (immersion time: 6 ± 1.0 h (partially insoluble)), filtered through a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GLC, and then measured using a chromatograph under the following measurement conditions. The average molecular weight of the sample is calculated from a standard polystyrene calibration curve prepared in advance. Equipment used: Tosoh Corporation's "HLC-8320GPCEcoSEC" gel permeation chromatograph (with built-in RI and UV detectors)
[0034] <GPC Measurement Conditions> Sample side Guard column = TSKguardcolumn HXL-H (6.0 mm × 4.0 cm) × 1 piece Measurement column = TSKgel GMHXL (7.8 mm I.D. × 30 cm) × 2 pieces in series Reference side = Resistance tube (inner diameter 0.1 mm × 2 m) × 2 pieces in series Column temperature = 40 °C Mobile phase = Chloroform Mobile phase flow rate Reference side pump = 0.5 mL / min Sample side pump = 1.0 mL / min Detector = RI detector Injection volume = 50 μL Measurement time = 25 min Sampling pitch = 500 msec
[0035] As the standard polystyrene samples for the calibration curve, products with mass average molecular weights of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320 named "STANDARDS M-105" and "STANDARDS H-75" manufactured by Showa Denko K.K. are used. After grouping the above standard polystyrene for the calibration curve into A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320), weigh 2 mg, 3 mg, 4 mg, 4 mg, and 4 mg of A in descending order of the above mass average molecular weight and dissolve them in 30 mL of chloroform. Similarly, weigh 3 mg, 4 mg, 4 mg, 4 mg, and 4 mg of B in descending order of the above mass average molecular weight and dissolve them in 30 mL of chloroform. The standard polystyrene calibration curve is obtained by creating a calibration curve (cubic equation) from the retention times obtained after injecting 50 μL of each prepared A and B solution for measurement, and the average molecular weight is calculated using the calibration curve.
[0036] These polylactic acid resins may be used alone or in combination of two or more. The content of the polylactic acid resin is preferably 70% by mass or more, more preferably 80% by mass or more and 100% by mass or less, even more preferably 85% by mass or more and 100% by mass or less, and particularly preferably 90% by mass or more and 100% by mass or less, based on the total mass of the resin components (excluding the brittleness modifier) contained in the polylactic acid resin composition. When the content of the polylactic acid-based resin is equal to or more than the above lower limit, the biodegradability of the foamed sheet is easily increased, and the environmental load is easily reduced. When the content of the polylactic acid-based resin is equal to or less than the above upper limit, the moldability and mechanical strength of the foamed sheet are easily improved.
[0037] <Brittleness modifier> The brittleness modifier is a resin that can improve brittleness by being blended with the resin. Examples of the brittleness modifier include butadiene-based rubber, acrylic-based rubber, and biodegradable aliphatic polyester-based resin.
[0038] The glass transition temperature Tg of the brittle modifier is not higher than 0° C. The glass transition temperature Tg of the brittle modifier is preferably not higher than −30° C., and more preferably not higher than −40° C. The glass transition temperature (Tg) is the "midpoint glass transition temperature: Tmg" among the glass transition temperatures specified in JIS K 7121-1987 "Method of measuring transition temperature of plastics."
[0039] [Butadiene rubber] The butadiene rubber may be contained in the polylactic acid resin composition in the form of a homopolymer of butadiene, or may be contained in the polylactic acid resin composition in the form of a copolymer rubber composed of butadiene and another monomer copolymerizable with butadiene. The copolymer rubber may be a block polymer having a copolymer block composed of a monomer other than butadiene and a polybutadiene block, a graft copolymer of polybutadiene and another polymer, or a random copolymer of butadiene and another monomer.
[0040] The butadiene-based rubber of this embodiment is preferably contained in the polylactic acid-based resin composition in the form of a copolymer rubber, and is preferably contained in the polylactic acid-based resin composition in the form of a graft copolymer rubber. The copolymer rubber may be a copolymer rubber of butadiene and styrene or the like (styrene-butadiene rubber). The copolymer rubber may be a multicomponent copolymer rubber composed of three or more types of monomers. Examples of copolymerizable monomers other than styrene include acrylic monomers such as methyl acrylate, methyl methacrylate, butyl acrylate, and butyl methacrylate.
[0041] The copolymer rubber is preferably a core-shell type rubber. The core-shell type rubber has a core and a shell layer covering the core, and the core is preferably made of a polymer having a unit derived from butadiene, and the shell layer is preferably made of a polymer of methyl methacrylate.
[0042] As the copolymer rubber, it is preferable to adopt a multicomponent copolymer rubber containing styrene and an acrylic monomer in addition to butadiene. The styrene (St) and the acrylic monomer (Aa) are preferably contained in the multicomponent copolymer rubber in a molar ratio of 0.8:1 to 1:0.8 (St:Aa). As the acrylic monomer, methyl methacrylate is preferable. That is, as the copolymer rubber, MBS polymer (methyl methacrylate-butadiene-styrene copolymer) is preferable. The MBS polymer may further contain a small amount of butyl acrylate (for example, 0.5% by mass to 2% by mass).
[0043] When the butadiene-based rubber is a copolymer rubber, it preferably contains butadiene units in an amount of 35 mass% or more, more preferably 40 mass% or more, and even more preferably 45 mass% or more, based on all units constituting the copolymer rubber. When the butadiene-based rubber is a copolymer rubber, it preferably contains butadiene units in a proportion of 60 mass % or less based on all units constituting the copolymer rubber.
[0044] When the butadiene-based rubber is a butadiene homopolymer, it is preferably contained in an amount of 0.30 parts by mass or more and 4.0 parts by mass or less, and more preferably 0.50 parts by mass or more and 3.5 parts by mass or less, per 100 parts by mass of the polylactic acid-based resin. When the butadiene rubber is a copolymer rubber, it is preferably contained in an amount of 8.0 parts by mass or less, more preferably 7.0 parts by mass or less, and even more preferably 6.0 parts by mass or less, relative to 100 parts by mass of the polylactic acid resin, and is preferably contained in an amount of 0.50 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 2.0 parts by mass or more.
[0045] [Acrylic rubber] The acrylic rubber may be contained in the polylactic acid resin composition in the form of a homopolymer of an acrylic monomer, may be contained in the polylactic acid resin composition as a copolymer rubber composed of two or more kinds of acrylic monomers, or may be contained in the polylactic acid resin composition as a copolymer rubber composed of an acrylic monomer and another monomer copolymerizable with the acrylic monomer. The copolymer rubber may be a block polymer, a graft copolymer, or a random copolymer.
[0046] The acrylic rubber of the present embodiment is preferably contained in the polylactic acid resin composition in the form of a copolymer rubber, and is preferably contained in the polylactic acid resin composition in the form of a graft copolymer rubber. The graft copolymer rubber is preferably a core-shell type rubber obtained by graft polymerizing one or more vinyl monomers onto an acrylic rubber in the presence of the acrylic rubber.
[0047] When the acrylic rubber is a copolymer rubber containing units other than acrylic monomer units, it is preferably contained in an amount of 8.0 parts by mass or less, more preferably 7.0 parts by mass or less, and even more preferably 6.0 parts by mass or less, relative to 100 parts by mass of the polylactic acid resin, and is preferably contained in an amount of 0.50 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 2.0 parts by mass or more.
[0048] [Biodegradable aliphatic polyester resin] Examples of biodegradable aliphatic polyester resins include polyethylene succinate, polybutylene succinate, polyhexamethylene succinate, polyethylene adipate, polyhexamethylene adipate, polybutylene adipate, polyethylene oxalate, polybutylene oxalate, polyneopentyl oxalate, polyethylene sebacate, polybutylene sebacate, polyhexamethylene sebacate, etc., which are obtained by polycondensation of glycol and aliphatic dicarboxylic acid. Among these, polybutylene succinate is particularly preferred.
[0049] <Foam regulator> Examples of the cell regulator include inorganic powders such as talc, silica, mica, and the like, fluorine-based resin powders such as polytetrafluoroethylene, acid salts such as polycarboxylic acids, mixtures of polycarboxylic acids with sodium carbonate or sodium bicarbonate, etc. These cell regulators increase the closed cell ratio of the foamed layer and facilitate the formation of the foamed layer. The cell regulator may be used alone or in combination of two or more.
[0050] When the polylactic acid-based resin composition contains a bubble control agent, the content of the bubble control agent is, for example, preferably 0.50 parts by mass or more and 3.0 parts by mass or less, more preferably 0.80 parts by mass or more and 2.8 parts by mass or less, and even more preferably 1.5 parts by mass or more and 2.5 parts by mass or less, relative to 100 parts by mass of the polylactic acid-based resin. When the content of the cell regulator is equal to or more than the lower limit, it is easy to suppress an increase in the open cell ratio due to the cells of the foamed sheet becoming too large, and it is easy to increase the mechanical strength.When the content of the cell regulator is equal to or less than the upper limit, it is easy to suppress an increase in the open cell ratio due to the cells of the foamed sheet becoming too small, and it is easy to increase the mechanical strength, and it is easy to better prevent clogging of the die, etc., and to improve the appearance of the foamed sheet.
[0051] <Other resins> The polylactic acid resin composition may further contain a thermoplastic resin other than the polylactic acid resin (hereinafter, also referred to as "other resins") in addition to the polylactic acid resin and the brittleness modifier. Examples of the other resins include plant-derived resins other than the polylactic acid resins; petroleum-derived resins such as polystyrene resins and polyester resins. In this specification, resins having a glass transition temperature Tg of 0° C. or lower are classified as brittleness modifiers and are not treated as other resins.
[0052] Examples of plant-derived resins include polymers derived from plant materials such as sugar cane and corn. "Derived from plant materials" includes polymers synthesized or extracted from plant materials. Furthermore, for example, "derived from plant materials" includes polymers obtained by polymerizing monomers synthesized or extracted from plant materials. "Monomers synthesized or extracted from plant materials" include monomers synthesized using compounds synthesized or extracted from plant materials as raw materials. Plant-derived resins include those in which some of the monomers are "derived from plant materials". Examples of plant-derived resins include so-called bio-PET, bio-PP, plant-derived polyester-based resins, plant-derived polypropylene-based resins, and the like.
[0053] When the polylactic acid-based resin composition contains plant-derived resins as other resins, the total content of the other plant-derived resins is preferably 3 to 30 mass%, more preferably 4 to 25 mass%, and even more preferably 5 to 20 mass%, relative to the total mass of the polylactic acid-based resin composition. When the total content of the other resins derived from plants is equal to or greater than the above lower limit, the environmental impact is more easily reduced. When the total content of the other resins derived from plants is equal to or less than the above upper limit, the effects of the present invention are more easily enhanced.
[0054] Examples of polystyrene-based resins include homopolymers of styrene-based monomers such as styrene, α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, and bromostyrene, or copolymers thereof; copolymers of styrene-based monomers and vinyl monomers polymerizable therewith, with styrene-based monomers as the main component (50% by mass or more), and so-called high impact polystyrene resins (HIPS), which are mixtures or polymers of homopolymers of styrene-based monomers or copolymers thereof, or copolymers of styrene-based monomers and vinyl monomers and diene-based rubbery polymers; and the like. Examples of vinyl monomers polymerizable with styrene-based monomers include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and cetyl (meth)acrylate, and bifunctional monomers such as (meth)acrylonitrile, dimethyl maleate, dimethyl fumarate, diethyl fumarate, ethyl fumarate, divinylbenzene, and alkylene glycol dimethacrylate. These vinyl monomers may be used alone or in combination of two or more. Here, "(meth)acrylate" refers to one or both of "acrylate" and "methacrylate", and "(meth)acrylonitrile" refers to one or both of "acrylonitrile" and "methacrylonitrile". These polystyrene resins may be used alone or in combination of two or more.
[0055] The polystyrene-based resin may be a polystyrene-based resin that is not made from recycled raw materials, such as general-purpose polystyrene resin (GPPS), commercially available polystyrene-based resin, or polystyrene-based resin newly prepared by a method such as suspension polymerization, or it may be a polystyrene-based resin made from recycled raw materials. The recycled raw material is a used polystyrene-based resin foamed molded body. The recycled raw material is food containers, fish boxes, cushioning materials for home appliances, etc., which are collected and regenerated by a limonene dissolution method or a heat reduction method. In addition, the recycled raw material that can be used may be non-foamed polystyrene-based resin molded bodies collected and separated from home appliances (e.g., televisions, refrigerators, washing machines, air conditioners, etc.) and office equipment (e.g., copiers, facsimiles, printers, etc.), which are crushed, melted and kneaded, and repelletized.
[0056] The Z-average molecular weight of the polystyrene resin is, for example, preferably 800,000 or less, more preferably 100,000 to 650,000, even more preferably 150,000 to 600,000, and particularly preferably 150,000 to 550,000. When the Z-average molecular weight of the polystyrene resin is within the above numerical range, the fluidity is increased and the polylactic acid resin can be dispersed more uniformly. In order to disperse the polylactic acid resin more uniformly, the Z-average molecular weight of the polystyrene resin is more preferably larger than the Z-average molecular weight of the polylactic acid resin.
[0057] When the polylactic acid resin composition contains a polystyrene resin, the content of the polystyrene resin is preferably 0 to 10% by mass, more preferably 0 to 3.0% by mass, and even more preferably 0 to 1.0% by mass, based on the total mass of the polylactic acid resin composition. When the content of the polystyrene resin is equal to or more than the lower limit, the moldability of the foamed sheet can be further improved. When the content of the polystyrene resin is equal to or less than the upper limit, a larger amount of the polylactic acid resin can be blended, which makes it easier to reduce the environmental load.
[0058] Examples of petroleum-derived polyesters include polyethylene terephthalate resins, polybutylene terephthalate resins, polyethylene naphthalate resins, polyethylene furanoate resins, polybutylene naphthalate resins, copolymers of terephthalic acid, ethylene glycol, and cyclohexane dimethanol, mixtures thereof, and mixtures of these with other resins, etc. These petroleum-derived polyesters may be used alone or in combination of two or more.
[0059] When the polylactic acid-based resin composition contains a petroleum-derived polyester as another resin, the total content of the other petroleum-derived polyester resins is preferably 3 to 30 mass%, more preferably 4 to 25 mass%, and even more preferably 5 to 20 mass%, relative to the total mass of the polylactic acid-based resin composition. When the total content of the other resins, which are petroleum-derived polyesters, is equal to or greater than the above lower limit, the moldability of the foamed sheet can be further improved.When the total content of the other resins, which are petroleum-derived polyesters, is equal to or less than the above upper limit, a larger amount of polylactic acid-based resin can be blended, which makes it easier to reduce the environmental impact.
[0060] When the polylactic acid-based resin composition contains other resins, from the viewpoint of further improving the moldability of the foamed sheet and the impact resistance of the molded body, the other resins are preferably polystyrene-based resins such as general-purpose polystyrene resins and high-impact polystyrene resins, and more preferably high-impact polystyrene resins.
[0061] The other resins may be used alone or in combination of two or more. When the polylactic acid resin composition contains other resins, the total content of the other resins is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 3% by mass or less, based on the total mass of the polylactic acid resin composition. When the total content of the other resins is within the above range, the effects of the present invention are more easily enhanced.
[0062] <Other ingredients> The polylactic acid resin composition may contain components other than the polylactic acid resin, brittleness modifier, cell regulator, and other resins (hereinafter also referred to as optional components). Examples of optional components include surfactants, crosslinking agents, fillers, stabilizers, UV absorbers, antioxidants, colorants, deodorants, lubricants (hydrocarbons, fatty acids, fatty acid amides, esters, alcohols, metal soaps, silicone oils, waxes such as low molecular weight polyethylene, etc.), flame retardants, flame retardant assistants, spreading agents (liquid paraffin, polyethylene glycol, polybutene, etc.), antistatic agents, etc.
[0063] The type of optional component is determined taking into consideration the physical properties required for the foamed sheet. The optional components may be used alone or in combination of two or more. The total amount of optional components contained in the polylactic acid resin composition is preferably 0.010 to 5.0 parts by mass relative to 100 parts by mass of the polylactic acid resin.
[0064] Examples of the surfactant include anionic surfactants, nonionic surfactants, cationic surfactants, and amphoteric surfactants. Examples of anionic surfactants include higher fatty acid (carbon number 8 to 23) salts such as zinc stearate, alkyl (carbon number 8 to 18) sulfates such as sodium lauryl sulfate, alkyl (carbon number 10 to 15) benzenesulfonates such as sodium dodecylbenzenesulfonate, β-tetrahydroxynaphthalenesulfonates, etc. Examples of salts include sodium, potassium, magnesium, calcium, barium, lithium, zinc, aluminum, ammonium, triethanolamine, etc. Examples of nonionic surfactants include polyhydric alcohol fatty acid (carbon number: 8 to 18) esters such as stearic acid triglyceride, 12-hydroxystearic acid triglyceride, pentaerythritol distearate, etc., higher fatty acid (carbon number: 8 to 23) amides such as ethylene bisstearic acid amide, higher fatty acid (carbon number: 8 to 23) bisamides, alkylene (carbon number: 1 to 4) oxide adducts of hydrogenated castor oil, hydrogenated oils, etc. Examples of the cationic surfactant include alkyl (carbon number: 8 to 18) ammonium acetate salts, alkyl (carbon number: 8 to 18) dimethylbenzyl ammonium salts, alkyl (carbon number: 8 to 18) trimethyl ammonium salts, dialkyl (carbon number: 8 to 18) dimethyl ammonium salts, alkyl (carbon number: 8 to 18) pyridinium salts, oxyalkylene (carbon number: 1 to 4) alkyl (carbon number: 8 to 18) amines, polyoxyalkylene (carbon number: 1 to 4) alkyl (carbon number: 8 to 18) amines, and the like. Examples of amphoteric surfactants include alkyl (carbon number: 8 to 23) betaines, fatty acid (carbon number: 8 to 18) amidopropyl betaines, alkyl (carbon number: 8 to 23) imidazoles, amino acids, and amine oxides.
[0065] As the surfactant, a nonionic surfactant is preferred, and a polyhydric alcohol fatty acid ester is more preferred, because it can suppress the decomposition of the polylactic acid resin and has good compatibility with the polylactic acid resin. If the decomposition of the polylactic acid resin cannot be suppressed, the Z-average molecular weight of the polylactic acid resin decreases, and the moldability of the foamed sheet and the impact resistance of the molded product decrease.
[0066] When the polylactic acid resin composition contains a surfactant, the content of the surfactant is preferably 0.010 to 2.0 parts by mass, more preferably 0.050 to 1.5 parts by mass, and even more preferably 0.10 to 1.0 part by mass, per 100 parts by mass of the polylactic acid resin. The content of the surfactant is preferably 0.010 to 10 parts by mass, more preferably 0.010 to 7.0 parts by mass, and even more preferably 0.30 to 5.0 parts by mass, relative to 100 parts by mass of the polylactic acid resin. When the content of the surfactant is within the above range, the effects of the present invention are more easily enhanced.
[0067] Examples of the stabilizer include calcium zinc-based heat stabilizers, tin-based heat stabilizers, and lead-based heat stabilizers. Examples of the ultraviolet ray absorbent include cesium oxide-based ultraviolet ray absorbents and titanium oxide-based ultraviolet ray absorbents. Examples of the antioxidant include cerium oxide, cerium oxide / zirconia solid solution, cerium hydroxide, carbon, carbon nanotubes, titanium oxide, and fullerene. Examples of colorants include titanium oxide, carbon black, titanium yellow, iron oxide, ultramarine, cobalt blue, calcined pigments, metallic pigments, mica, pearl pigments, zinc oxide, precipitated silica, and cadmium red. Examples of deodorants include silica, zeolite, zirconium phosphate, and calcined hydrotalcite.
[0068] When the polylactic acid resin composition contains an optional component, the content of the optional component is, for example, preferably 0.050 to 20 parts by mass, more preferably 0.10 to 10 parts by mass, and even more preferably 0.30 to 5.0 parts by mass, relative to 100 parts by mass of the polylactic acid resin. When the content of the optional component is equal to or more than the lower limit, the effects derived from the optional component can be exhibited. When the content of the optional component is equal to or less than the upper limit, clogging of the die or the like can be more effectively prevented, and the appearance of the foamed sheet can be more improved.
[0069] <Polylactic acid resin foam sheet> The polylactic acid resin foamed sheet of the present invention (hereinafter, also simply referred to as "foamed sheet") is a sheet obtained by foaming the above-mentioned polylactic acid resin composition. Therefore, the composition contains a polylactic acid-based resin derived from the polylactic acid-based resin composition, a brittleness modifier, and, if necessary, a cell regulator, other resins, and optional components.
[0070] When the brittleness modifier in the polylactic acid-based resin composition is a butadiene-based rubber, the rubber content in the polylactic acid-based resin foam sheet is preferably 0.30 parts by mass or more and 4.0 parts by mass or less, more preferably 0.50 parts by mass or more and 3.5 parts by mass or less, and even more preferably 0.70 parts by mass or more and 3.0 parts by mass or less, per 100 parts by mass of the polylactic acid-based resin.
[0071] The rubber content corresponds to the content of butadiene units constituting the butadiene-based rubber. The rubber content is measured by analyzing the amount of butadiene monomer in the decomposition product of the foam sheet by gas chromatography. The peak of butadiene monomer overlaps with the peak of the decomposition product derived from polylactic acid, so it cannot be directly quantified, but it can be indirectly quantified from the peaks of other monomers that were copolymerized with butadiene. The amount of butadiene monomer in the decomposition product (rubber content) can be calculated from the peaks of other monomers based on a calibration curve prepared using the butadiene rubber before mixing with the polylactic acid resin as a standard sample. A specific measurement method will be described in detail in the Examples.
[0072] The expansion ratio of the foamed sheet (hereinafter, simply referred to as "expansion") is preferably 4.0 to 15, more preferably 4.5 to 12, and even more preferably 5.0 to 8.0. When the expansion ratio of the foamed sheet is within the above range, the mechanical strength is excellent and the thermoformability is easily improved. In this specification, the magnification can be measured by the method described in the Examples.
[0073] The density (apparent density) of the foam sheet is, for example, 83 kg / m 3 More than 310kg / m 3 Less than 100kg / m is preferable. 3 More than 280kg / m 3 Less than 150kg / m is more preferable. 3 More than 250kg / m 3 When the apparent density is equal to or higher than the lower limit, the open cell ratio does not become too high and the mechanical strength is easily increased. When the apparent density is equal to or lower than the upper limit, the flexibility and light weight are easily improved. In this specification, the apparent density can be measured by the method described in the Examples.
[0074] The thickness of the foamed sheet is, for example, preferably 0.50 to 5.0 mm, more preferably 1.0 to 3.0 mm. If the thickness of the foamed sheet is equal to or greater than the lower limit, sufficient mechanical strength is easily obtained. If the thickness is equal to or less than the upper limit, flexibility is excellent and molding is easy. In this specification, the thickness can be measured by the method described in the examples.
[0075] The basis weight of the foam sheet is, for example, 200 to 600 g / m 2 is preferable, and 300 to 500 g / m 2When the content is equal to or more than the above lower limit, moldability is easily ensured, and when the content is equal to or less than the above upper limit, the light weight of the molded product is easily ensured. In this specification, the basis weight can be measured by the method described in the examples.
[0076] The closed cell ratio of the foamed sheet is preferably 70% or more, more preferably 75% or more, and even more preferably 80% or more. The upper limit is not particularly limited, and is preferably, for example, 99% or less. When the closed cell ratio of the foamed sheet is within the above numerical range, the mechanical strength is excellent and the thermoformability is easily improved. The closed cell ratio of the foamed sheet is measured by the method described in JIS K7138:2006 "Rigid foamed plastics-Determination of open cell ratio and closed cell ratio."
[0077] The open cell ratio of the foamed sheet is preferably 25% or less, more preferably 23% or less. When the open cell ratio is equal to or less than the above upper limit, the mechanical strength can be easily increased. In this specification, the open cell ratio can be measured by the method described in the Examples.
[0078] In the polylactic acid resin foamed sheet, the relationship between the average cell diameters in each direction measured by the following measurement method satisfies both of the following formulas (1) and (2). 0.20 <D VD / {0.5×(D MD +D TD )}<0.50···(1) 400<(D MD ×D TD ×D VD ) 1 / 3 <900···(2) (In the formula (1) and the formula (2), D MD , D TD , D VD are the average bubble diameters in the extrusion direction (MD), width direction (TD), and thickness direction (VD) of the foamed sheet, respectively, and are expressed in μm.
[0079] In formula (1), D VD / {0.5×(D MD+D TD )} is more than 0.20 and less than 0.50, preferably 0.25 or more and 0.45 or less, and more preferably 0.30 or more and 0.42 or less. D VD / {0.5×(D MD +D TD When the value calculated by the formula {amount of the bubble in the VD direction} is equal to or greater than the above lower limit, the bubble size in the VD direction is appropriately increased, which makes it easier to prevent the bubble size from increasing only in the MD and TD directions and improve the mechanical strength. D VD / {0.5×(D MD +D TD When the value calculated by the above formula {amount of bubbles in the VD direction} is equal to or less than the upper limit above, the bubbles are prevented from becoming too large in the VD direction, thereby obtaining appropriate flexibility and making it easier to improve moldability. In formula (2), (D MD ×D TD ×D VD ) 1 / 3 The value calculated by the above formula is more than 400 and less than 900, preferably 480 or more and 800 or less, and more preferably 450 or more and 700 or less. (D MD ×D TD ×D VD ) 1 / 3 When the value calculated by is equal to or larger than the above lower limit, the bubbles are not too small and have an appropriate size, which makes it easier to suppress the occurrence of corrugations on the surface of the foamed sheet. (D MD ×D TD ×D VD ) 1 / 3 When the value calculated by is equal to or less than the above upper limit, the bubbles are not too large and have an appropriate size, making it easier to suppress a decrease in mechanical strength that would otherwise occur due to bubbles breaking and an increase in the open cell ratio. In this specification, the average cell diameter can be measured by the method described in the Examples.
[0080] The magnification, apparent density, thickness, basis weight, closed cell ratio, open cell ratio and average cell diameter of the polylactic acid-based resin foamed sheet can be adjusted by the production conditions of the polylactic acid-based resin foamed sheet, as well as the types, compositions, foaming agents, optional components and combinations of these of the polylactic acid-based resin and other resins constituting the polylactic acid-based resin foamed sheet.
[0081] In the polylactic acid resin foam sheet, when the cushioning coefficient (hereinafter also simply referred to as the "cushioning coefficient") determined in accordance with JIS Z 0235:2002 is 10 or less, the compressive stress (hereinafter also simply referred to as the "compressive stress") determined in accordance with JIS K 6400-2:2012 is 0.20 MPa or more and 0.70 MPa or less.
[0082] The compressive stress measured by the above-mentioned measuring method is preferably 0.25 MPa or more and 0.60 MPa or less, more preferably 0.28 MPa or more and 0.55 MPa or less, and even more preferably 0.30 MPa or more and 0.50 MPa or less. When the compressive stress is equal to or greater than the above lower limit, the mechanical strength is easily increased. When the compressive stress is equal to or less than the upper limit, appropriate flexibility is obtained, and therefore moldability is easily improved. The compressive stress can be measured by the method described in the Examples.
[0083] The punching energy required for the polylactic acid resin foamed sheet, as measured by a film impact tester, is preferably 0.30 J or more, more preferably 0.35 J or more, and particularly preferably 0.40 J or more. When the energy required for punching is equal to or greater than the above lower limit, brittleness can be improved and impact resistance can be increased.
[0084] The compressive stress and cushioning coefficient of the polylactic acid-based resin foam sheet can be adjusted by the production conditions of the polylactic acid-based resin foam sheet, as well as the types, compositions, foaming agents, optional components, and combinations of these of the polylactic acid-based resin and other resins that constitute the polylactic acid-based resin foam sheet.
[0085] <Production method of polylactic acid resin foam sheet> The foamed sheet of the present invention is produced in accordance with a conventionally known production method. Examples of methods for producing a foamed sheet include a method in which a polylactic acid-based resin composition is prepared, extruded into a sheet shape, and foamed (primary foaming) (extrusion foaming method).
[0086] <Extrusion foaming method> The step of extruding and foaming the resin composition can be carried out by using a known method. For example, when the raw materials for a foamed sheet (a polylactic acid-based resin composition and a foaming agent) are fed to an extruder equipped with a die (a flat die or a circular die), they are melt-mixed while being transported toward the die to form a polylactic acid-based resin composition mixed with the foaming agent (hereinafter referred to as the "mixed raw material"). The mixed raw material is extruded from the die, and the foaming agent foams to form a foamed sheet.
[0087] The ingredients of the foamed sheet other than the foaming agent, i.e., the polylactic acid-based resin composition, may be mixed in advance by a dry blending method or a full compounding method, and then fed to the extruder. The apparent density and open cell ratio of the foamed sheet can be adjusted by the amounts of foaming agent and cell regulator, the resin temperature during extrusion, etc. The resin temperature during extrusion can be set within a range in which the resin melts and the optional components are not denatured.
[0088] An example of a method for producing a foamed sheet by the extrusion foaming method will be described with reference to FIG. The foamed sheet manufacturing apparatus 200 in FIG. 2 is an apparatus for obtaining a foamed sheet by extrusion foam molding, and includes an extruder 202, a foaming agent supply source 208, a circular die 210, a mandrel 220, and two winders 240. The extruder 202 is a so-called tandem type extruder, and is configured such that an extruder A 202a and an extruder B 202b are connected by a pipe 206. The first extrusion section 202a includes a hopper 204, and a foaming agent supply source 208 is connected to the extruder A 202a. A circular die 210 is connected to the extruder B 202b, and a mandrel 220 is provided downstream of the circular die 210. The mandrel 220 includes a cutter 222.
[0089] First, the polylactic acid-based resin composition is charged from the hopper 204 into the extruder A 202 a. In the extruder A202a, the polylactic acid resin composition is mixed while being heated to a given temperature to form a resin melt, and a foaming agent is supplied from a foaming agent supply source 208 to the extruder A202a, and the foaming agent is mixed with the resin melt to form a resin composition. The heating temperature is appropriately determined in consideration of the type of resin, etc., so long as the resin melts and the additives are not denatured.
[0090] The polylactic acid resin composition (mixed raw material) mixed with the foaming agent is supplied from the extruder A 202a through the pipe 206 to the extruder B 202b, further mixed, cooled to a given temperature, and then supplied to the circular die 210. The temperature of the mixed raw material when extruded from the circular die 210 is 140 to 190°C, and more preferably 150 to 190°C.
[0091] The mixed raw material is extruded from the circular die 210, and the foaming agent foams to form a cylindrical foamed sheet 101a. The foamed sheet 101a extruded from the circular die 210 is blown with cooling air 211 and then supplied to a mandrel 220. The cooling speed of the foamed sheet 101a can be adjusted by combining the temperature, amount, and blowing position of the cooling air 211.
[0092] The cylindrical foamed sheet 101a is heated to an arbitrary temperature by the mandrel 220, sized, and cut into two pieces by the cutter 222 to become the foamed sheet 101. The foamed sheet 101 is stretched around a guide roll 242 and a guide roll 244, respectively, and taken up by the winder 240 to become the foamed sheet roll 102. The expansion ratio of the foamed sheet is, for example, 2 to 20 times. The foamed sheet may be produced by a method other than extrusion foam molding.
[0093] <Foaming agent> As the foaming agent, a known foaming agent can be used. Examples of the foaming agent include inorganic decomposable foaming agents such as sodium bicarbonate-citric acid foaming agents, ammonium carbonate, sodium bicarbonate, ammonium bicarbonate, ammonium nitrite, calcium azide, sodium azide, and sodium borohydride; azo compounds such as azodicarbonamide, azobissulfuramide, azobisisobutyronitrile, and diazoaminobenzene; nitroso compounds such as N,N'-dinitrosopentanemethylenetetramine and N,N'-dimethyl-N,N'-dinitrosoterephthalamide; benzenesulfonyl hydrazide, p-toluenesulfonyl hydrazide, p,p'-oxybisbenzenesulfonylsemicarbazide, p-toluenesulfonylsemicarbazide, trihydrazinotriazine, and barium azodicarboxylate.
[0094] Examples of gaseous blowing agents include air, nitrogen, carbon dioxide, propane, neopentane, methyl ether, dichlorofluoromethane, n-butane, and isobutane. Here, gas means that it is a gas at room temperature (15°C to 25°C). On the other hand, examples of volatile blowing agents include ether, petroleum ether, acetone, pentane, hexane, isohexane, heptane, isoheptane, benzene, and toluene. The blowing agents may be used alone or in combination of two or more.
[0095] The content of the foaming agent in the mixed raw material is appropriately determined taking into consideration the type and specific gravity of the foaming agent, and is, for example, preferably 0.50 to 20 parts by mass, more preferably 0.80 to 5.5 parts by mass, per 100 parts by mass of the polylactic acid resin.
[0096] <Molded body> The molded article of the present invention is obtained by molding the foamed sheet of the present invention. Examples of the molded article include containers for food, containers such as industrial part transport trays, cushioning materials, packaging materials, heat insulating materials, industrial parts for electrical appliances or automobiles, and building materials. The molded article of the present embodiment has excellent impact resistance and is therefore suitable for use in, for example, food containers, transport trays, vehicle components for automobiles and the like, building components, and the like.
[0097] The foamed sheet can be formed by any known thermoforming method, for example, by a method including the following steps: (1) a heating step in which the foam sheet is heated to soften it to a state in which it can be thermoformed; (2) a molding step in which the softened foam sheet is deformed to conform to the surface shape of a mold to form a product shape; and (3) A trimming process in which unnecessary portions of the foam sheet that has formed the product shape are cut off to obtain the desired molded product from the foam sheet.
[0098] The heating step (1) can be carried out, for example, by a method in which the foamed sheet is passed through a heating furnace equipped with a radiant heater or the like for a certain period of time. The molding step (2) can be carried out by contacting the heated and softened foamed sheet with the surface of a mold to cool it. As the mold, a general mold such as a vacuum mold, a pressure mold, a vacuum pressure mold, or a match mold mold can be used. When forming a relatively large molded body, a pair of male and female molds is preferred, and it is preferable to use a plug-assisted vacuum mold or a match mold mold. In deep drawing, the foamed sheet may be cooled rapidly during molding, causing breakage or thinning, so it is preferable to adjust the temperature as necessary. The trimming step (3) can be carried out by a general method using a Thompson blade or a puncher (punch).
[0099] As shown in FIG. 3, the molded body 300 is a bowl-shaped container having a perfect circular shape in plan view. The molded body 300 has a circular bottom wall 310 and a side wall 320 rising from the periphery of the bottom wall 310. The molded body 300 has an opening 330 surrounded by the upper end of the side wall 320. The side wall 320 widens outward toward the upper end. The opening 330 surrounded by the upper end of the side wall 320 has a perfect circular shape in plan view. The bottom wall 310 is formed of a convex portion 312 having a perfect circular shape in plan view that is convex toward the opening 330, and an annular concave portion 314 that surrounds the convex portion 312.
[0100] The thickness of the bottom wall and side wall of the molded article (hereinafter sometimes referred to as "wall thickness") is determined taking into consideration the application and the like, and is, for example, preferably 20 to 1000 μm, more preferably 40 to 800 μm, and even more preferably 60 to 600 μm. When the wall thickness of the molded article is equal to or greater than the above lower limit, the impact resistance of the molded article can be further improved. When the wall thickness of the molded article is equal to or less than the above upper limit, the molded article can be made lighter. The molded article 300 is suitable for use as a food container.
[0101] Although the molded body 300 of this embodiment has a perfect circular shape in plan view, the present invention is not limited to this. The shape of the molded body in plan view may be an ellipse or a polygon.
[0102] ≪Applications≫ The molded article of the present embodiment can be used as a cushioning material, packaging material, structural material, heat insulating material, etc., used in industrial parts such as food containers, electrical products, and automobiles.
[0103] <Foam board> The foam board in this embodiment is a plate-like body having a thickness of 1.0 mm or more and including a foam layer made of the polylactic acid resin as described above. The thickness of the polylactic acid resin foam board (hereinafter also simply referred to as "foam board") may be 2.0 mm or more. The thickness of the foam board is, for example, 10 mm or less. The thickness of the foam board may be 8.0 mm or less, or 6.0 mm or less. When the foam board of this embodiment includes other layers such as a non-foamed layer rather than a foam layer alone, the overall thickness can also be as described above. The thickness of the foam board in this embodiment is calculated as the arithmetic average value of thickness measurements at multiple randomly selected points (for example, 10 points), and is calculated as the arithmetic average value of measurements using a thickness gauge.
[0104] The foam board of the present embodiment may be an extruded foam sheet produced by an extrusion foaming method. The foam board of the present embodiment has an apparent density of the foam layer of 300 kg / m 3 The apparent density of the foam layer is preferably 250 kg / m or less. 3 It may be less than 200 kg / m 3 The apparent density of the foam layer may be, for example, 70 kg / m 3 It can be more than that.
[0105] In the foam board of this embodiment, the polylactic acid resin in the foam layer has a crystallinity of 25% or more. The crystallinity may be 30% or more, or may be 35% or more. The foam board of this embodiment, in which the polylactic acid resin is contained in the foam layer in a state of high crystallinity, is excellent in strength and toughness. The crystallinity is, for example, 60% or less.
[0106] In the case of an extruded foam sheet, the polylactic acid resin usually cools and hardens before it is sufficiently crystallized. In particular, when a crosslinked modified polylactic acid resin is included, the molecular motion of the polylactic acid resin is restricted by crosslinking, making it difficult to sufficiently crystallize. Therefore, in this embodiment, it is preferable to extrude and foam the polylactic acid resin in a heated and molten state by melt kneading it with an extruder or the like into the atmosphere to produce an extruded foam sheet with a crystallinity of less than 25%, and then heat the extruded foam sheet to improve the crystallinity to the above value to produce a foam board.
[0107] The foamed board with improved crystallinity in this way is not only excellent in strength and toughness, but also resistant to distortion due to heat (excellent dimensional stability). The foamed board of this embodiment, which is resistant to distortion due to heat, is suitable, for example, as a peripheral frame for folding lunch boxes that contain freshly cooked rice and side dishes immediately after cooking. The foamed board preferably has a dimensional change rate of 5% or less when heated at a temperature of 90°C. The dimensional change rate is more preferably 4% or less, and particularly preferably 3% or less.
[0108] <<Production method of foam board>> As a method for producing a foam board, for example, the polylactic acid resin foam sheet obtained by the above method is passed through a conveyor heater to heat and cool it, and then cut by a cutter to produce a foam board. The temperature of the heating zone is, for example, preferably 100°C to 140°C, more preferably 110°C to 130°C. When the temperature of the heating zone is within the above range, crystallization of the foam board is easily promoted, and excessive foaming can be suppressed, thereby further improving the surface smoothness. EXAMPLES
[0109] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following description. The raw materials used in this example are as follows:
[0110] ≪Raw materials used≫ <Polylactic acid resin> Biopolymer Ingeo 6202D: Polylactic acid resin, Nature Works, MFR=10.1g / 10min, density=1.24g / cm3). <Butadiene rubber> Metablen C-223A: Manufactured by Mitsubishi Chemical Corporation. Butadiene copolymer rubber. Tg=-90℃~-70℃. <Acrylic rubber> Metablen W-600A: Mitsubishi Chemical Corporation, acrylic copolymer rubber, Tg=-75℃~-45℃. <Polybutylene succinate> BioPBS FZ91PM: Polybutylene succinate resin, manufactured by PTT MCC Biochem, Tg=-40℃~-30℃. <Foam regulator> · Crown Talc: Talc, manufactured by Matsumura Sangyo Co., Ltd.
[0111] <Pretreatment of polylactic acid resin> A mixture was obtained by stirring and mixing 100 parts by mass of a polylactic acid resin (Nature Works' Biopolymer Ingeo6202D) and 0.5 parts by mass of t-butylperoxyisopropyl monocarbonate (Kayaku Akzo's Kayacarvon BIC-75, 1-minute half-life temperature T1: 158.8°C) in a ribbon blender. The obtained mixture was fed to a twin-screw extruder (L / D=31.5) with a diameter of 57 mm. The temperature of the feed section was set to 170°C, and the temperature thereafter was set to 230°C, and the mixture was melt-kneaded in the twin-screw extruder at a rotation speed of 150 rpm. The kneaded product was extruded in a strand shape at a discharge rate of 50 kg / h from a die with a diameter of 3 mm and 18 holes attached to the tip of the extruder. Next, the extruded strand-shaped kneaded product was passed through a 2 m long cooling water tank containing water at 30°C to cool it. The cooled strand was cut with a pelletizer to obtain pellets of the crosslinked modified polylactic acid resin. The melt mass flow rate (MFR) of the obtained modified polylactic acid resin was 1.5 g / 10 min, and the mass average molecular weight (Mw) was 330,000.
[0112] <Production of foam sheets> <Example 1> 100 parts by mass of the modified polylactic acid resin prepared by the above method, 2.4 parts by mass of a cell regulator ("Crown Talc" manufactured by Matsumura Sangyo Co., Ltd.), and 2.9 parts by mass of a butadiene rubber ("Metablen C-223A" manufactured by Mitsubishi Chemical Corporation) were fed into a mixing screw installed in a twin-screw extruder with a bore diameter of φ75 mm and mixed to obtain a polylactic acid resin composition. The polylactic acid resin composition was then fed into the extruder and heated to melt. Butane gas was injected into the melt at a predetermined position and kneaded. The mixture was then extruded through a circular die having an aperture of 125 mm at a discharge rate of 100 kg / h to obtain a cylindrical foam. The obtained cylindrical foam was placed on a φ339 mm mandrel whose inside was cooled with water at about 5°C, and its outer surface was cooled and molded by blowing air onto it using an air ring larger in diameter than the mandrel. The foam was then cut at one point on the circumference with a cutter to obtain a band-shaped foam sheet.
[0113] <Examples 2 to 11 and Comparative Examples 1 to 7> A foamed sheet was obtained in the same manner as in Example 1, except that the formulation of the polylactic acid-based resin composition was changed as shown in Tables 1 to 3, and the sheet specifications (cell diameter, magnification, air connection rate, etc.) were adjusted by changing the drawing speed of the winder and the air volume from the air ring.
[0114] <Measurement and evaluation of foam sheets> For the foamed sheets obtained in each example, the thickness, basis weight, expansion ratio (expansion ratio), apparent density, open cell ratio, and average cell diameter in each direction were measured by the following methods. For Examples 1 to 7 and Comparative Examples 1 to 5, the rubber content was also measured. In addition, the compressive stress, the energy required for punching, and the moldability when the cushioning coefficient was 10 or less were evaluated by the following methods. The results are shown in Tables 1 to 3.
[0115] <Rubber content> The rubber content was measured as follows. Approximately 0.1 g of the foamed sheet obtained in each example was dissolved in approximately 20 mL of chloroform, and a film was produced on a hot plate. Approximately 0.1 to 0.5 mg of the filmed sample was precisely weighed out. A test specimen was prepared by wrapping the sample in a ferromagnetic metal body called "Pyrofoil" manufactured by Japan Analytical Industry Co., Ltd., which has a Curie point of 590°C. The test specimen was prepared so that a ferromagnetic metal body was pressed against the sample. The test specimen was heated in a Japan Analytical Industry Co., Ltd. (JPS-700) Curie point pyrolyzer to decompose the sample. The 4-vinylcyclohexene produced by decomposition was measured using an Agilent Technologies GC7820A gas chromatograph (detector: FID) and the peak area was calculated. The amount of butadiene contained in the sample was calculated from a calibration curve prepared in advance. (Pyrolysis conditions) Measuring device: Japan Analytical Industry Co., Ltd. "JPS-700" PYROFOIL SAMPLER Heating temperature=590℃ Heating time=5sec Oven temperature = 300 °C Needle temperature = 300℃ (GC measurement conditions) Measurement equipment: Agilent Technologies "7820A" gas chromatograph Detector: FID Column: Agilent Technologies "DB-5" capillary column (0.25μm×0.25mmφ×30m) (GC oven heating conditions) Initial temperature = 50℃ (held for 0.5min) First stage heating rate = 10℃ / min (up to 200℃, hold for 0 min) Second stage heating rate = 20℃ / min (up to 320℃) Final temperature = 320℃ (held for 0.5min) Carrier gas = He He flow rate=63.736mL / min Inlet pressure = 100kPa Column inlet pressure = 100kPa Inlet temperature=300℃ Detector temperature = 300℃ Split ratio = 1 / 50 The standard sample used for preparing the calibration curve was Metablen C-223A manufactured by Mitsubishi Chemical Corporation.
[0116] <Thickness> Twenty-one arbitrary positions in the width direction (direction perpendicular to the extrusion flow direction) were used as measurement points. These measurement points were measured with a thickness measuring device (manufactured by Techclock Corporation, model: SM-125) to the nearest 0.01 mm. The arithmetic mean of these measurements was used as the thickness of the foamed sheet obtained in each example.
[0117] <Basic weight> From the foamed sheet obtained in each example, 20 mm from both ends in the width direction (direction perpendicular to the extrusion flow direction) was removed, and 10 pieces of 10 cm x 10 cm were cut out at equal intervals in the width direction, and the mass (g) of each piece was measured to the nearest 0.001 g. The average mass (g) of each piece was calculated using the formula: 2 The converted value is expressed as the mass per unit weight (g / m 2 ) was decided.
[0118] <Magnification> The apparent density was determined by the measurement method described below, and then the density of the polylactic acid resin was determined. The value obtained by dividing the density of the polylactic acid resin by the apparent density was used as the expansion ratio (expansion ratio) of the foamed sheet obtained in each example.
[0119] <Apparent density> From the foamed sheets obtained in each example, 50 cm 3 The sheet was cut out to prepare a test piece, the mass and volume of the test piece were measured, and the overall apparent density was calculated by the following formula: The test piece was cut out from a foamed sheet that was 72 hours or more old (maximum 90 days) after production, and left for 24 hours in an atmospheric condition of 23°C±2°C and 50RH%±5RH%. Apparent density (kg / m 3 ) = mass of test piece (kg) ÷ volume of test piece (m 3)
[0120] <Open cell ratio> From the foamed sheet obtained in each example, several sheet-like samples of 25 mm length × 25 mm width were cut out. The cut out samples were stacked so that there was no space, resulting in a thickness of 25 mm, which was used as a test piece. The apparent volume (cm) of the obtained test piece was 3 The apparent volume (cm 3 ) was obtained by measuring the outer dimensions of the test piece to 1 / 100 mm. A "Digimatic Caliper" caliper made by Mitutoyo Corporation was used for the measurement. Next, the volume (cm) of the test piece was measured using a Tokyo Science Co., Ltd. "1000" air comparison specific gravity meter by the 1-1 / 2-1 atmospheric pressure method. 3 ) was sought.
[0121] The open cell ratio (%) was calculated using the following formula. The open cell ratio was calculated as the average value of five test pieces. The test pieces were conditioned in a JIS K7100:1999, symbol 23 / 50, class 2 environment for 16 hours before use in the measurement. The measurement was carried out in the same environment. The air comparison specific gravity meter was used with a standard ball (large 28.96 cm 3 Small 8.58cm 3 ) was used for correction. Open cell rate (%) = (apparent volume - volume measured with an air comparison type specific gravity meter) / apparent volume x 100
[0122] <Average bubble diameter> Sample 1 for cross-sectional observation was cut out from the widthwise center of the foamed sheet obtained in each example. The cross-sections of the samples were photographed at 50x magnification using a scanning electron microscope (e.g., Hitachi High-Technologies Corporation's "TM3030Plus" scanning electron microscope). One of the cross-sections to be observed was a cross-section of the sample cut along a plane (arrow 1 in Figure 1) parallel to the extrusion direction (MD) and perpendicular to the surface of the foamed sheet (hereinafter referred to as the "MD cross-section"). The other cross-section to be observed was a cross-section of the sample cut along a plane (arrow 2 in Figure 1) perpendicular to the extrusion direction (hereinafter referred to as the "TD cross-section"). Microscopic images were taken using a scanning electron microscope, with two fields of view for each of the MD and TD cross sections, for a total of four fields of view.
[0123] The captured image was printed on a sheet of A4 paper, and three straight lines were drawn at arbitrary positions on the printed image connecting both ends of the image so that they were parallel to the extrusion direction (MD direction) and width direction (TD direction), and three straight lines were drawn at arbitrary positions connecting the back and front surfaces of the sheet so that they were parallel to the thickness direction (VD direction) perpendicular to each direction. In addition, we tried to avoid contacting any bubble with any point of contact for any line, and counted the number of bubbles that the line passed through. If any bubble was contacted only at a point of contact, the bubble was also included in the count.
[0124] The length of the drawn straight line and the scale bar on the image were measured, and the image magnification was calculated from the measured length of the scale bar and the displayed value of the scale bar, and the average chord length was calculated using the following formula. Average chord length t (μm) = measured value of straight line / (number of bubbles x image magnification) The bubble diameter in each direction was then calculated using the following formula. Bubble diameter D(μm)=t / 0.616 Furthermore, the cube root of the product was taken as the average bubble diameter. Average bubble diameter (μm)=(D MD ×D TD ×D VD ) 1 / 3 D MD : Bubble diameter in MD (μm) D TD : bubble diameter in TD direction (μm) D VD : Bubble diameter in VD direction (μm)
[0125] <Evaluation of compressive stress when the buffer coefficient is 10 or less> The compressive stress was determined in accordance with the measurement method for compressive stress-strain characteristics described in JIS K 6400-2:2012 or ISO 3386-1. The cushioning coefficient was determined in accordance with JIS Z 0235:2002 or ISO 4651. The cushioning coefficient indicates the performance of the foamed sheet according to one embodiment in absorbing impact energy, and was calculated as the compressive stress determined by a compression test divided by the compressive energy per unit volume (cushioning coefficient=compressive stress / compressive energy per unit volume).
[0126] The compressive stress was measured at multiple locations (3 locations) of the foamed sheet obtained in each example, and the cushioning coefficient was calculated by dividing each compressive stress by the compression energy. The average value was used as the cushioning coefficient of the foamed sheet obtained in each example.
[0127] Specifically, the compressive stress was measured as follows. That is, the compressive stress was measured using a device manufactured by A&D, model RTG-1310, and a calibrated load cell of 5 kN. From the foamed sheet obtained in each example, circles with a diameter of 50 mm were punched or cut out uniformly. When the sheet was thin, the necessary number of sheets were punched or cut out so that when multiple sheets were stacked, the thickness would be 25 mm to 35 mm (when the sample was sandwiched between a pressure plate and a fixed support plate of a universal testing machine and a force of 2.9 N to 3.0 N was applied). The sheet was sandwiched between the pressure plate and the support plate, and pressure was applied to (40 ± 1)% of the thickness of the test piece at a speed of (100 ± 20) mm / min. If the stress did not reach 0.30 MPa, the compression amount may be changed to 70% of the thickness. In addition, the cushioning coefficient was calculated based on the measured value of the first compression in accordance with JIS Z 0235:2002 and ISO 4651. The above procedure was repeated three times, and the cushioning coefficient was calculated based on the average value of the three measurements.
[0128] <Evaluation of required energy for punching> The impact absorption energy was measured using a film impact tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd., product name "No. 181 Film Impact Tester"). An evaluation sample of 100 mm x 90 mm was taken from the foamed sheet obtained in each example, and the energy (unit: J) required to punch the sample was determined using an impact ball size of 6.35 mmR and a pendulum angle of 90 degrees in an environment adjusted to a temperature of 22°C and a relative humidity of 40%. Specifically, the evaluation sample for which the required punching energy was to be calculated was set between the sample plate and the sample presser, the pointer was placed on the 1.5 J line, and the pendulum stopper handle was tilted to drop the pendulum. The evaluation sample broke, and the pendulum pushed the pointer, and the scale indicated was read. The above operation was performed five times on each side of the foamed sheet, and the average value was calculated.
[0129] <Evaluation of moldability> The foamed sheet obtained in each example was heated in a heater tank at 270°C for 15 seconds, and then the sheet was attached to a male plug mold and a female cavity mold designed with a clearance of 2 mm. Next, the plug mold and the cavity mold were closed for 3 seconds to perform vacuum and pressure molding, and a molded product having a circular shape in plan view with an opening dimension of φ190 mm, a bottom dimension of φ170 mm, and a height of 50 mm was obtained.
[0130] The appearance of the obtained molded article was visually observed, and the moldability was evaluated based on the following evaluation criteria. (Evaluation Criteria) ○: Molding was completed without any problems. ×: There is a tear or a wrinkle just below the opening of the molded article.
[0131] [Table 1]
[0132] [Table 2]
[0133] [Table 3]
[0134] Examples 1 to 11 to which the present invention was applied had improved brittleness and were excellent in mechanical strength and moldability. On the other hand, Comparative Example 1, which did not contain a brittleness modifier, was more brittle than Examples 1 to 11 and was inferior in impact resistance. In Comparative Example 2, in which the relationship of the average cell diameter does not satisfy the relationship of formula (1), the compressive stress when the cushioning coefficient was 10 or less exceeded 0.70 MPa, and the mechanical strength was excellent, but the flexibility was lower and the moldability was inferior to Examples 1 to 11. Comparative Examples 4 and 5, in which the relationship of the average cell diameter did not satisfy the relationship of formula (2), were highly flexible and excellent in moldability, but were inferior to Examples 1-11 in mechanical strength. Comparative Examples 3 to 7, in which the compressive stress when the cushioning coefficient was 10 or less was less than 0.20 MPa, were highly flexible and excellent in moldability, but were inferior to Examples 1 to 11 in mechanical strength.
[0135] These results demonstrate that the polylactic acid-based resin foamed sheet, molded article, and foamed board of the present invention can reduce the environmental load, improve brittleness, and achieve both high mechanical strength and moldability. [Explanation of symbols]
[0136] 1. Foam sheet (sample for cross-sectional observation) 300 Molded body 310 Bottom wall 312... Convex part 314...Recess 320...side wall 330...Opening
Claims
1. A polylactic acid-based resin foamed sheet comprising a polylactic acid-based resin and a brittleness modifier, The compressive stress measured in accordance with JIS K 6400-2:2012 when the cushioning coefficient measured in accordance with JIS Z 0235:2002 is 10 or less is 0.20 MPa or more and 0.70 MPa or less, A polylactic acid resin foam sheet, in which the relationship between average cell diameters in each direction measured by the following measurement method satisfies both of the following formulas (1) and (2): 0.20<D VD / {0.5 × (D MD +D TD )) < 0.50 ... (1) 400 < (D MD xD TD xD VD ) 1/3 <900...(2) (In the formula (1) and the formula (2), D MD , D TD , D VD are the average bubble diameters in the extrusion direction (MD), width direction (TD), and thickness direction (VD) of the foamed sheet, respectively, and are expressed in μm. <Average cell diameter in each direction of polylactic acid resin foam sheet> A sample for cross-section observation was cut out from the center of the width direction of the foamed sheet, and the average bubble diameters in the extrusion direction (MD), the direction perpendicular to the extrusion direction (TD cross section), and the thickness direction perpendicular to each direction (VD direction) were measured using a scanning electron microscope. MD , D TD , D VD Let us assume that.
2. 2. The polylactic acid-based resin foam sheet according to claim 1, wherein the brittleness modifier is a butadiene-based rubber, and the rubber content is 0.30 parts by mass or more and 4.0 parts by mass or less per 100 parts by mass of the polylactic acid-based resin.
3. 2. The polylactic acid-based resin foam sheet according to claim 1, wherein the brittleness modifier is an acrylic rubber, and the content of the acrylic rubber is 1.0 part by mass or more and 8.0 parts by mass or less per 100 parts by mass of the polylactic acid-based resin.
4. 2. The polylactic acid-based resin foam sheet according to claim 1, wherein the brittleness modifier is a biodegradable aliphatic polyester-based resin, and the content of the biodegradable aliphatic polyester-based resin is 5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the polylactic acid-based resin.
5. 5. The polylactic acid resin foam sheet according to claim 4, wherein the biodegradable aliphatic polyester resin is polybutylene succinate.
6. 2. The polylactic acid resin foam sheet according to claim 1, wherein the required punching energy as measured by a film impact tester is 0.30 J or more.
7. Apparent density: 83 kg / m 3 ~310kg / m 3 2. The polylactic acid resin foam sheet according to claim 1,
8. 2. The polylactic acid resin foam sheet according to claim 1, having an open cell ratio of 25% or less.
9. 2. The polylactic acid resin foam sheet according to claim 1, further comprising a cell regulator, the content of the cell regulator being 0.50 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the polylactic acid resin.
10. 2. The polylactic acid resin foam sheet according to claim 1, having a thickness of 0.50 to 5.0 mm.
11. A molded article obtained by thermoforming the polylactic acid resin foam sheet according to any one of claims 1 to 10.
12. The molded article according to claim 11, which is a food container.
13. A foam plate obtained by molding the polylactic acid resin foam sheet according to any one of claims 1 to 10 into a plate shape.
Citation Information
Patent Citations
Polylactic acid resin foamed sheet for thermal forming and polylactic acid resin formed foam
JP2004359910A