Optical substrate, method of manufacturing optical substrate, solid-state image pickup device, and method of manufacturing solid-state image pickup device

By incorporating a light diffusion film with an irregular wrinkle structure and a textured frame, the solid-state imaging device minimizes optical noise from stray light, enhancing image capture quality.

JP2024146881APending Publication Date: 2024-10-15KANEKA CORP

Patent Information

Application Number
JP2024053298
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In solid-state imaging devices with a hollow structure, strong light incidence leads to increased reflected light from the frame and transparent substrate surfaces, causing optical noise such as flare and ghost in captured images.

Method used

The implementation of a transparent substrate with a light diffusion film having a surface roughness of 50 nm to 3000 nm and an irregular wrinkle structure, combined with a frame having a similar surface texture, to diffuse and reduce stray light.

Benefits of technology

This configuration significantly reduces optical noise like flare and ghost in captured images by diffusing and reflecting light effectively, improving image quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146881000001_ABST
    Figure 2024146881000001_ABST
Patent Text Reader

Abstract

To provide an optical substrate capable of reducing optical noise in a solid-state image pickup device.SOLUTION: An optical substrate 30A comprises: a transparent substrate 30; and a light diffusion film 45 which is laminated on one principal surface of the transparent substrate 30 and has an optical path opening, wherein a principal surface 46 of the light diffusion film 45 on the opposite side from the transparent substrate 30 has a surface roughness Ra of 50 to 3,000 nm, a surface layer of the principal surface 46 of the light diffusion film 45 has a density of 1.1 to 1.6 g / cm3, and the density of the surface layer of the principal surface 46 of the light diffusion film 45 is higher than that of any part other than the surface layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical substrate, a method for manufacturing an optical substrate, a solid-state imaging device, and a method for manufacturing a solid-state imaging device. [Background technology]

[0002] Solid-state imaging devices that are image sensors such as CMOS sensors or CCD sensors are known. Such solid-state imaging devices include, for example, a solid-state imaging element (semiconductor chip), a substrate on which the solid-state imaging element is mounted, a transparent substrate arranged to face the substrate, and a frame arranged between the substrate and the transparent substrate to surround the solid-state imaging element, and have a hollow structure in which the solid-state imaging element is sealed by the substrate, the transparent substrate, and the frame (see, for example, Patent Document 1). In addition, the transparent substrate on one main surface of which a frame-shaped frame that defines a hollow space (inner space) is formed is called an optical substrate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-216475 A Summary of the Invention [Problem to be solved by the invention]

[0004] In such a hollow-structure solid-state imaging device, when strong light is incident, the amount of reflected light (stray light) from, for example, the surface of the frame or the surface of the transparent substrate increases, resulting in increased optical noise such as flare or ghosting in the captured image.

[0005] An object of the present invention is to provide an optical substrate that reduces optical noise in a solid-state imaging device, an optical substrate, a solid-state imaging device, and a method for manufacturing a solid-state imaging device. [Means for solving the problem]

[0006] The optical substrate according to the present invention includes a transparent substrate and a light diffusing film having an optical path opening laminated on one main surface of the transparent substrate, the main surface of the light diffusing film opposite to the transparent substrate having a surface roughness Ra of 50 nm to 3000 nm, and a density of a surface layer of the main surface of the light diffusing film being higher than a density of a portion other than the surface layer.

[0007] Another optical substrate according to the present invention includes a transparent substrate, and a light diffusing film having an optical path opening laminated on one main surface of the transparent substrate, The main surface of the light diffusing film opposite to the transparent substrate has an irregular wrinkle structure.

[0008] The manufacturing method of the optical substrate of the present invention is a manufacturing method of the above-mentioned optical substrate or another optical substrate, and includes a printing step of printing the material of the light diffusion film on the transparent substrate using a photocurable material or a photocurable and thermosetting material by a printing method using a printing plate, a provisional curing step of irradiating the material of the light diffusion film with light to provisionally cure the material of the light diffusion film, an excimer light irradiation step of irradiating the main surface of the material of the light diffusion film opposite the transparent substrate after the provisional curing step with excimer light, and a final curing step of irradiating the material of the light diffusion film after the excimer light irradiation step with light, heating, or irradiating with light and heating the material of the light diffusion film to fully cure the material of the light diffusion film to obtain the light diffusion film.

[0009] Another manufacturing method of the optical substrate according to the present invention is a manufacturing method of the above-mentioned optical substrate or another optical substrate, and includes a printing step of printing the material of the light diffusion film on the transparent substrate using a thermosetting material or a photocurable and thermosetting material by a printing method using a printing plate, a provisional curing step of heating the material of the light diffusion film to provisionally cure the material of the light diffusion film, an excimer light irradiation step of irradiating excimer light onto a main surface of the material of the light diffusion film opposite the transparent substrate after the provisional curing step, and a final curing step of heating, irradiating with light, or irradiating with light and heating the material of the light diffusion film after the excimer light irradiation step to fully cure the material of the light diffusion film to obtain the light diffusion film.

[0010] The present invention relates to a solid-state imaging device, and a method for manufacturing the same, comprising: forming a solid-state imaging element on a substrate having a first main surface and a second main surface of the first main surface, the first main surface being a first main surface of the first main surface, the second main surface being a second main surface of the first main surface, the third main surface being a second main surface of the first main surface, the fourth main surface being a second main surface of the first main surface, the fifth main surface being a second main surface of the first main surface, the fifth main surface being a second main surface of the first main surface, the sixth main surface being a second main surface of the first main surface, the sixth main surface being a second main surface of the first main surface, the seventh main surface being a second main surface of the first main surface, the eighth main surface being a second main surface of the first main surface, the eighth main surface being a second main surface of the first main surface, the eighth main surface being a second main surface of the first main surface, the eighth main surface being a second main surface of the first main surface, the eighth main surface being a second main surface of the first main surface, the eighth main surface being a second main surface of the first main surface, the eighth main surface being a third ... fourth main surface of the first main surface, the eighth main surface being a

[0011] Another solid-state imaging device according to the present invention includes a solid-state imaging element, a transparent substrate arranged to face the solid-state imaging element, a light diffusion film arranged on the inner surface of the transparent substrate at a position corresponding to the periphery of an imaging area of ​​the solid-state imaging element, and a frame arranged between the solid-state imaging element and the transparent substrate so as to surround the imaging area of ​​the solid-state imaging element. The inner main surface of the light diffusion film has an irregular wrinkle structure.

[0012] The method for manufacturing a solid-state imaging device according to the present invention is a method for manufacturing the above-mentioned solid-state imaging device, and includes a printing step of printing the material of the light diffusion film on the transparent substrate using a photocurable material or a photocurable and thermosetting material by a printing method using a printing plate; a provisional curing step of irradiating the material of the light diffusion film with light to provisionally cure the material of the light diffusion film; an excimer light irradiation step of irradiating the inner main surface of the material of the light diffusion film after the provisional curing step with excimer light; a final curing step of irradiating the material of the light diffusion film after the excimer light irradiation step with light, heating, or irradiating with light and heating the material of the light diffusion film after the excimer light irradiation step to fully cure the material of the light diffusion film to obtain the light diffusion film; a step of forming the frame on the transparent substrate; and an assembling step of combining the transparent substrate on which the light diffusion film and the frame are formed after the final curing step, or the transparent substrate on which the material of the light diffusion film and the material of the frame are formed before the final curing step, with the substrate on which the solid-state imaging element is mounted.

[0013] Another manufacturing method for a solid-state imaging device according to the present invention is a manufacturing method for the above-mentioned another solid-state imaging device, and includes a printing step of printing the material of the light diffusion film on the transparent substrate using a photocurable material or a photocurable and thermosetting material by a printing method using a printing plate; a provisional curing step of irradiating the material of the light diffusion film with light to provisionally cure the material of the light diffusion film; an excimer light irradiation step of irradiating the inner main surface of the material of the light diffusion film after the provisional curing step with excimer light; a final curing step of irradiating the material of the light diffusion film after the excimer light irradiation step with light, heating, or irradiating with light and heating the material of the light diffusion film after the excimer light irradiation step to final cure the material of the light diffusion film to obtain the light diffusion film; a step of forming the frame on the transparent substrate; and an assembling step of combining the transparent substrate on which the light diffusion film and the frame are formed after the final curing step, or the transparent substrate on which the material of the light diffusion film and the material of the frame are formed before the final curing step, with the solid-state imaging element.

[0014] Another manufacturing method of a solid-state imaging device according to the present invention is a manufacturing method of the above-mentioned solid-state imaging device, and includes a printing step of printing the material of the light diffusion film on the transparent substrate using a thermosetting material or a photocurable and thermosetting material by a printing method using a printing plate; a provisional curing step of heating the material of the light diffusion film to provisionally cure the material of the light diffusion film; an excimer light irradiation step of irradiating the inner main surface of the material of the light diffusion film after the provisional curing step with excimer light; a final curing step of heating, irradiating with light, or irradiating with light and heating the material of the light diffusion film after the excimer light irradiation step to fully cure the material of the light diffusion film to obtain the light diffusion film; a step of forming the frame on the transparent substrate; and an assembling step of combining the transparent substrate on which the light diffusion film and the frame are formed after the final curing step, or the transparent substrate on which the material of the light diffusion film and the material of the frame are formed before the final curing step, with the substrate on which the solid-state imaging element is mounted.

[0015] Another manufacturing method of a solid-state imaging device according to the present invention is a manufacturing method of the above-mentioned other solid-state imaging device, and includes a printing step of printing the material of the light diffusion film on the transparent substrate using a thermosetting material or a photocurable and thermosetting material by a printing method using a printing plate, a provisional curing step of heating the material of the light diffusion film to provisionally cure the material of the light diffusion film, an excimer light irradiation step of irradiating the inner main surface of the material of the light diffusion film after the provisional curing step with excimer light, a final curing step of heating, irradiating with light, or irradiating with light and heating the material of the light diffusion film after the excimer light irradiation step to final cure the material of the light diffusion film to obtain the light diffusion film, a step of forming the frame on the transparent substrate, and an assembling step of combining the transparent substrate on which the light diffusion film and the frame are formed after the final curing step, or the transparent substrate on which the material of the light diffusion film and the material of the frame are formed before the final curing step, with the solid-state imaging element. Effect of the Invention

[0016] According to the present invention, in a solid-state imaging device, optical noise such as flare or ghosting occurring in a captured image can be reduced. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic diagram showing a solid-state imaging device and an optical substrate according to a first embodiment, viewed from the light-receiving surface side. [Diagram 2] 2 is a schematic cross-sectional view of the solid-state imaging device and the optical substrate according to the first embodiment, taken along line II-II in FIG. [Figure 3A] 11 shows an example of an image of the surface of a frame material and a light diffusion film material after an excimer light irradiation process. [Figure 3B] 11 is an image of an example of the surface of a frame material and a light diffusion film material before an excimer light irradiation step and after a provisional curing step. [Figure 4A] 11 shows an example of an image of a cross section of a frame material and a light diffusion film material after an excimer light irradiation process. [Figure 4B]13 is an image of another example of a cross section of a frame material and a light diffusion film material after an excimer light irradiation process. [Figure 5A] 3A to 3C are schematic views showing a printing step in a method for manufacturing the solid-state imaging device and the optical substrate according to the first embodiment. [Figure 5B] 5A to 5C are schematic views showing a provisional curing step in the method for manufacturing the solid-state imaging device and the optical substrate according to the first embodiment. [Figure 5C] 3A to 3C are schematic views showing a printing step in a method for manufacturing the solid-state imaging device and the optical substrate according to the first embodiment. [Figure 5D] 5A to 5C are schematic views showing a provisional curing step in the method for manufacturing the solid-state imaging device and the optical substrate according to the first embodiment. [Figure 5E] 3 is a schematic diagram showing an excimer light irradiation step in a method for manufacturing the solid-state imaging device and the optical substrate according to the first embodiment. FIG. [Figure 5F] 5A to 5C are schematic views showing a main curing step in the method for manufacturing the solid-state imaging device and the optical substrate according to the first embodiment. [Figure 5G] 4 is a schematic diagram showing a step of dividing a light diffusion film and a framed transparent substrate (optical substrate) into individual pieces in a manufacturing method of a solid-state imaging device and an optical substrate according to the first embodiment. FIG. [Figure 5H] 4 is a schematic diagram showing a process of assembling a transparent substrate (optical substrate) with a light diffusion film and a frame and a solid-state imaging element mounting substrate in a manufacturing method for the solid-state imaging device according to the first embodiment. FIG. [Figure 6] 11 is a schematic cross-sectional view of a solid-state imaging device and an optical substrate according to a second embodiment. FIG. [Figure 7] 10 is a schematic diagram showing a process of assembling a transparent substrate (optical substrate) with a light diffusion film and a frame and a solid-state imaging element mounting substrate in a manufacturing method for a solid-state imaging device according to a second embodiment. FIG. [Figure 8] 11 is a schematic cross-sectional view of a solid-state imaging device and an optical substrate according to a second embodiment. FIG. [Figure 9] 13 is a schematic diagram showing a process of assembling a transparent substrate (optical substrate) with a light diffusion film and a frame and a substrate mounting a solid-state imaging element in a manufacturing method for a solid-state imaging device according to a third embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. In each drawing, the same or corresponding parts are denoted by the same reference numerals. For convenience, hatching and reference numerals may be omitted, in which case other drawings shall be referred to.

[0019] [First embodiment] (Solid-state imaging device and optical substrate) FIG. 1 is a schematic diagram showing the solid-state imaging device and the optical substrate according to the first embodiment from the light receiving surface side, and FIG. 2 is a schematic cross-sectional view of the solid-state imaging device and the optical substrate according to the first embodiment, taken along the line II-II in FIG. 1. The solid-state imaging device 1 shown in FIG. 1 and FIG. 2 is an image sensor such as a CMOS sensor or a CCD sensor, and is a so-called box-shaped solid-state imaging device. The solid-state imaging device 1 includes a solid-state imaging element 10, a substrate 20, a transparent substrate 30, a frame (rib material) 40, and a light diffusion film 45. The transparent substrate 30 and the light diffusion film 45 constitute the optical substrate 30A. Alternatively, the transparent substrate 30, the frame 40, and the light diffusion film 45 constitute the optical substrate 30A.

[0020] <Solid-state imaging element> The solid-state imaging element 10 is a semiconductor chip of an image sensor such as a CMOS sensor or a CCD sensor. The semiconductor chip is made of, for example, a silicon substrate (wafer), and has an imaging region 12 including a plurality of pixels arranged two-dimensionally. Each pixel is made of, for example, a photodiode. A color filter, a microlens, or the like may be arranged on the imaging region 12. The solid-state imaging element 10 is mounted on a substrate 20.

[0021] <Substrate> The substrate 20 is a wiring substrate. The substrate 20 and the solid-state imaging element 10 are electrically connected by wiring 22 such as bonding wires. In addition, the substrate 20 is electrically connected to conductive members 24 such as solder balls for transferring signals and power between the solid-state imaging element 10 and the outside.

[0022] Examples of the substrate 20 include organic materials such as polyimide, polyester, ceramic, epoxy, bismaleimide triazine, and phenol resin, structures in which paper or nonwoven glass fiber is impregnated with the organic materials and then heat-cured, ceramics such as alumina, aluminum nitride, beryllium oxide, and silicon nitride, and metal substrates. Among these, glass epoxy substrates and ceramic substrates are preferred. Circuits having metal wiring patterns, metal bumps, metal vias, or metal film-coated through-holes can be formed on or inside these insulating substrates.

[0023] <Transparent substrate> The transparent substrate 30 is disposed so as to face the substrate 20, specifically, so as to face the main surface on which the solid-state imaging element 10 is mounted, out of the two main surfaces of the substrate 20. The transparent substrate 30 may be made of glass, acrylic resin, or transparent plastic such as polycarbonate, and glass is preferred from the viewpoint of reliability. The type of glass is not particularly limited, but examples include quartz glass, borosilicate glass, and non-alkali glass.

[0024] If necessary, a coating film such as an infrared reflective film (or an infrared cut filter), an anti-reflective film (AR coating), a protective film, or a reinforced film can be formed on the surface of the transparent substrate 30. In particular, an anti-reflective film or an infrared reflective film (or an infrared cut filter) is preferable because it reduces optical noise in the captured image. In particular, when the coating is an anti-reflective film, TiO 2 , Nb 2 O 5 , Ta 2 O 5 , CaF 2 , SiO 2 , Al 2 O 3, MgS 2 , ZrO 2 , NiO, or MgF 2 It is preferable to form a multi-layer film of several types selected from the above.

[0025] These coating films can be applied to both sides or just one side of the glass. When applied to both sides, the types of coatings can be the same or different. It is also possible to laminate different types of coating films having the same function on one side, or to laminate different types of coating films having different functions. There is no particular limit to the number of layers, and it can be several to several tens of layers.

[0026] <Light diffusion film> The light diffusion film 45 is disposed on the inner surface side (one of the main surfaces) of the transparent substrate 30 at a position corresponding to the periphery of the solid-state imaging element 10 and the periphery of the imaging region 12 of the solid-state imaging element 10, and has an optical path opening. The light diffusion film 45 diffuses light incident on the inner surface of the transparent substrate 30 by irregularly reflecting it. This makes it possible to reduce the reflected light (stray light) from the inner surface of the transparent substrate 30 that is incident on the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0027] Examples of the light diffusion film 45 include photocurable resins such as epoxy resins, acrylic resins, and silicone resins, thermosetting resins, and photocurable and thermosetting resins. The details of the light diffusion film 45 will be described later. When the main curing is performed by light irradiation as described later, the resin may be a thermo- and photocurable resin having a thermosetting group and a photocurable group, or a blend of a thermosetting resin and a photocurable resin may be used.

[0028] Furthermore, when the main curing is performed by thermal irradiation (heating) as described below, the light diffusion film may be formed by curing the light curable group (light curable resin) in the provisional curing and curing the thermosetting group (thermosetting resin) in the final curing. Furthermore, when the main curing is performed by light irradiation, the light diffusion film may be formed by curing the thermosetting group (thermosetting resin) in the provisional curing and curing the light curable group (light curable resin) in the final curing. Details of the light diffusion film 45 will be described later.

[0029] <frame> The frame (rib material) 40 is disposed between the substrate 20 and the transparent substrate 30, more specifically between the substrate 20 and the light diffusion film 45, so as to surround the solid-state imaging element 10. In other words, the frame 40 is disposed on the inner main surface side (the main surface side opposite to the transparent substrate 30) of the light diffusion film 45, and has an inner diameter larger than the optical path opening of the light diffusion film 45. The frame 40 and the substrate 20 are bonded together using, for example, an adhesive 50. Meanwhile, the frame 40 and the transparent substrate 30, more specifically, the frame 40 and the light diffusion film 45, are bonded together by the adhesive force of the material of the frame 40.

[0030] Examples of the frame 40 include photocurable resins such as epoxy resin, acrylic resin, and silicone resin, thermosetting resins, and photocurable and thermosetting resins. When the main curing is performed by light irradiation as described later, the resin may be a thermo- and photocurable resin having a thermosetting group and a photocurable group in the resin, or a blend of a thermosetting resin and a photocurable resin may be used.

[0031] Furthermore, when the main curing is performed by thermal irradiation (heating) as described below, the frame may be formed by curing the photocurable group (photocurable resin) in the provisional curing and curing the thermosetting group (thermosetting resin) in the main curing. Furthermore, when the main curing is performed by light irradiation, the frame may be formed by curing the thermosetting group (thermosetting resin) in the provisional curing and curing the photocurable group (photocurable resin) in the main curing.

[0032] When an adhesive photocurable resin or photocurable and thermosetting resin is used for the frame 40, the temporarily cured frame material may be placed on the substrate 20 on which the solid-state imaging element 10 is mounted and then fully cured (not shown) without using the adhesive 50, as described below. The frame 40 will be described in detail later.

[0033] <Adhesive> A UV-curable or heat-curable adhesive can be used as the adhesive 50. The adhesive is preferably a curable resin such as an epoxy resin, an acrylic resin, or a silicone resin. The adhesive may also contain a filler such as silica in order to adjust the viscosity.

[0034] In this manner, in the solid-state imaging device 1, the solid-state imaging element is sealed by the substrate 20, the transparent substrate 30, and the frame 40. The solid-state imaging device 1 has a hollow structure having a space above the solid-state imaging element .

[0035] The transparent substrate 30 having a light diffusion film 45 with an optical path opening formed on one of its main surfaces is called an optical substrate 30A. Alternatively, the transparent substrate 30 having a light diffusion film 45 with an optical path opening and a frame-shaped frame 40 having an inner diameter larger than the optical path opening and defining a hollow space (inner space) formed on one of its main surfaces is called an optical substrate 30A.

[0036] (Details of the light diffusion film and frame) Fig. 3A is an image of an example of the surface of the frame material and the light diffusion film material after the excimer light irradiation process described later, and Fig. 3B is an image of an example of the surface of the frame material and the light diffusion film material before the excimer light irradiation process described later and after the provisional curing process. Meanwhile, Fig. 4A is an image of an example of the cross section of the frame material and the light diffusion film after the excimer light irradiation process described later, and Fig. 4B is an image of another example of the cross section of the frame material and the light diffusion film material after the excimer light irradiation process described later. The UV light irradiation conditions in the provisional curing process and the excimer light irradiation conditions in the excimer light irradiation process in the example of Figs. 3A to 4B are as follows. UV light irradiation conditions for the temporary curing process: Illuminance 70mW / cm 2 , exposure time 15 seconds, Alternatively, the heating conditions for the temporary curing process are: temperature 100 degrees, time 60 seconds, Excimer light irradiation conditions in the excimer light irradiation process: Illuminance 170 mW / cm 2 , exposure time 4 minutes The imaging device was a laser microscope (model number VK-9700, manufactured by Keyence Corporation).

[0037] As described later, when the surface of the material of the light diffusion film 45 after the provisional curing process (see FIG. 3B) is irradiated with excimer light, the surface of the material of the light diffusion film 45 (see FIG. 3A) is altered and contracted. Such an altered and contracted structure is called a microfold structure. Also, such an altered and contracted structure can be called an irregular wrinkle structure. The wrinkle structure is a fine periodic uneven structure (wrinkles and wrinkles) formed on the surface. In this embodiment, as shown in FIG. 3A, the altered and contracted structure can be said to be an irregular wrinkle structure in which a fine uneven structure (wrinkles and wrinkles) is irregularly formed.

[0038] With this structure, the surface of the material of the light diffusion film 45 has a matte effect and can diffusely reflect light. This makes it possible to reduce the reflected light (stray light) from the surface of the light diffusion film 45 and incident on the imaging region 12 of the solid-state imaging element 10 in the solid-state imaging device 1, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0039] On the other hand, the excimer light does not affect the inside of the material of the light diffusion film 45, and the inside of the material of the light diffusion film 45 does not change (see FIGS. 4A and 4B).

[0040] As a result, as shown in FIG. 3A, the inner principal surface 46 of the light diffusion film 45 (the principal surface opposite to the transparent substrate 30) has an irregular wrinkle structure. The surface roughness, i.e., the arithmetic mean roughness (JIS B061:2013, ISO 1365-1) Ra of the inner principal surface 46 of the light diffusion film 45 is 50 nm or more and 3000 nm or less, and preferably 200 nm or more and 3000 nm or less. Also, as shown in FIG. 4A and FIG. 4B, the density of the surface layer 45a of the inner principal surface 46 of the light diffusion film 45 is higher than the density of the portion 45b other than the surface layer. Also, the elastic modulus of the surface layer 45a of the inner principal surface 46 of the light diffusion film 45 is higher than the elastic modulus of the portion 45b other than the surface layer.

[0041] For example, the density of the surface layer 45a of the inner main surface 46 of the light diffusion film 45, i.e., the mass per unit volume ρ, is 1.1 g / cm when measured in accordance with JIS K7112:1980 (ISO 1183:1987). 3 More than 1.6g / cm 3 and preferably 1.3 g / cm 3 More than 1.6g / cm 3 The relative density ratio of the surface layer 45a to the portion other than the surface layer 45b of the inner main surface 46 of the light diffusing film 45 is preferably surface layer:other than the surface layer=1.05 to 1.4, and more preferably 1.1 to 1.2. The elastic modulus of the surface layer 45a of the inner main surface 46 of the light diffusing film 45, i.e., Young's modulus E, is 2.1 GPa or more and 3.0 GPa or less, and preferably 2.3 GPa or more and 3.0 GPa or less. The elastic modulus (i.e., Young's modulus E) can be measured by a scanning probe microscope.

[0042] Similarly, when the surface of the material of frame 40 after the provisional curing step (see FIG. 3B) is irradiated with excimer light, the surface of the material of frame 40 (see FIG. 3A) changes in quality and shrinks. This gives the surface of the material of frame 40 a matte effect and allows light to be diffusely reflected. This makes it possible to reduce the reflected light (stray light) from the surface of frame 40 that enters imaging region 12 of solid-state imaging element 10 in solid-state imaging device 1, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0043] On the other hand, the inside of the material of frame 40 is not affected by the excimer light, and the inside of the material of frame 40 is not altered (see FIGS. 4A and 4B).

[0044] Thus, as shown in Fig. 3A, the inner surface 41 of the frame 40 has an irregular wrinkle structure. The surface roughness of the inner surface 41 of the frame 40, i.e., the arithmetic mean roughness (JIS B061:2013, ISO 1365-1) Ra, may be 50 nm or more and 3000 nm or less, or 200 nm or more and 3000 nm or less. In addition, as shown in Figs. 4A and 4B, the density of the surface layer 40a of the inner surface 41 of the frame 40 may be higher than the density of the portion 40b other than the surface layer. In addition, the elastic modulus of the surface layer 40a of the inner surface 41 of the frame 40 may be higher than the elastic modulus of the portion 40b other than the surface layer.

[0045] For example, the density ρ of the surface layer 40a of the inner surface 41 of the frame 40 is 1.1 g / cm 3 More than 1.6g / cm 3 or less, preferably 1.3 g / cm 3 More than 1.6g / cm 3 The relative density ratio of the surface layer 40a to the portion 40b other than the surface layer of the inner side surface 41 of the frame 40 may be surface layer:other than the surface layer=1.05 to 1.4, and preferably 1.1 to 1.2. The elastic modulus E of the surface layer 40a of the inner side surface 41 of the frame 40 may be 2.1 GPa or more and 3.0 GPa or less, and preferably 2.3 GPa or more and 3.0 GPa or less.

[0046] As shown in FIG. 3A, the outer surface 42 and the lower end surface of the frame 40 may also have an irregular wrinkle structure. The surface roughness, i.e., the arithmetic mean roughness (JIS B061:2013, ISO 1365-1) Ra, of the outer surface 42 and the lower end surface of the frame 40 may be 50 nm or more and 3000 nm or less, or 200 nm or more and 3000 nm or less. As shown in FIG. 4A and FIG. 4B, the density of the surface layer 40a of the outer surface 42 and the lower end surface of the frame 40 may also be higher than the density of the portion 40b other than the surface layer. The elastic modulus of the surface layer 40a of the outer surface 42 and the lower end surface of the frame 40 may also be higher than the elastic modulus of the portion 40b other than the surface layer.

[0047] For example, the density ρ of the surface layer 40a of the outer surface 42 and the lower end surface of the frame 40 is 1.1 g / cm 3 More than 1.6g / cm 3 or less, preferably 1.3 g / cm 3 More than 1.6g / cm 3 The relative density ratio of surface layer 40a to portion 40b other than the surface layer on the outer side 42 and lower end face of frame 40 may be surface layer:other than the surface layer=1.05 to 1.4, and preferably 1.1 to 1.2. The elastic modulus E of the surface layer 40a of the outer surface 42 and the lower end surface of the frame 40 may be 2.1 GPa or more and 3.0 GPa or less, and preferably 2.3 GPa or more and 3.0 GPa or less.

[0048] (Method of manufacturing solid-state imaging device and optical substrate) Next, a method for manufacturing a solid-state imaging device and an optical substrate according to the first embodiment will be described with reference to Figs. 5A to 5H. Fig. 5A is a schematic diagram showing a printing step in the method for manufacturing a solid-state imaging device and an optical substrate according to the first embodiment, and Fig. 5B is a schematic diagram showing a provisional curing step in the method for manufacturing a solid-state imaging device and an optical substrate according to the first embodiment. Fig. 5C is a schematic diagram showing a printing step in the method for manufacturing a solid-state imaging device and an optical substrate according to the first embodiment, and Fig. 5D is a schematic diagram showing a provisional curing step in the method for manufacturing a solid-state imaging device and an optical substrate according to the first embodiment. Fig. 5E is a schematic diagram showing an excimer light irradiation step in the method for manufacturing a solid-state imaging device and an optical substrate according to the first embodiment, and Fig. 5F is a schematic diagram showing a main curing step in the method for manufacturing a solid-state imaging device and an optical substrate according to the first embodiment. Fig. 5G is a schematic diagram showing a step of dividing a light diffusion film and a framed transparent substrate (optical substrate) in the method for manufacturing a solid-state imaging device and an optical substrate according to the first embodiment, and Fig. 5H is a schematic diagram showing a step of assembling a light diffusion film and a framed transparent substrate (optical substrate) with a solid-state imaging element mounting substrate in the method for manufacturing a solid-state imaging device according to the first embodiment.

[0049] First, as shown in FIG. 5A, a printing method using a printing plate M1, such as a screen printing method, is used to print multiple (or one) light diffusion film materials 45Z on a large-sized transparent substrate 30Z (or a transparent substrate 30) using a photocurable material, a thermosetting material, or a combination of photocurable and thermosetting materials (printing process).

[0050] The surface of the printing plate M1 may be treated to be water-repellent. Examples of water-repellent treatment include coating with a liquid-repellent material such as a fluororesin or silicone resin. This can improve plate release and the rectangular shape of the light diffusion film.

[0051] Next, as shown in FIG. 5B, the material 45Z of the multiple (or one) light diffusion films is irradiated with light (e.g., ultraviolet light) to provisionally cure the material 45Z of the multiple (or one) light diffusion films (provisional curing step). Alternatively, the material 45Z of the multiple (or one) light diffusion films is heated to provisionally cure the material 45Z of the multiple (or one) light diffusion films (provisional curing step). Provisional curing refers to a state in which there is still room for further curing of the material of the light diffusion film in the step of irradiating the material of the light diffusion film with light or heating it. The UV light irradiation conditions in the provisional curing step are, for example, an illuminance of 70 mW / cm. 2 The irradiation time is 15 seconds. Alternatively, the heating conditions for the provisional curing step are, for example, a temperature of 100° C. and a time of 60 seconds.

[0052] In the provisional curing step, light irradiation or heating may be performed from the opposite side of the large-sized transparent substrate 30Z (or the transparent substrate 30), or light irradiation or heating may be performed from the large-sized transparent substrate 30Z (or the transparent substrate 30) side.

[0053] In the provisional curing step, light irradiation may be performed with the printing plate M1 in place, which can prevent the printing material from dripping and make the light diffusion film rectangular.

[0054] Next, as shown in FIG. 5C, a printing method using a printing plate M2, such as a screen printing method, is used to print multiple (or one) frame materials 40Z on the large-sized transparent substrate 30Z (or the transparent substrate 30) using a photocurable material, a thermosetting material, or a combination of photocurable and thermosetting materials (printing process).

[0055] The surface of the printing plate M2 may be treated to be water-repellent. Examples of water-repellent treatment include coating with a liquid-repellent material such as a fluororesin or silicone resin. This can improve plate release and the rectangular shape of the frame.

[0056] Next, as shown in FIG. 5D, the material 40Z of the multiple (or one) frames is irradiated with light (e.g., ultraviolet light) to temporarily cure the material 40Z of the multiple (or one) frames (temporary curing step). Alternatively, the material 40Z of the multiple (or one) frames is heated to temporarily cure the material 40Z of the multiple (or one) frames (temporary curing step). The UV light irradiation conditions for the temporary curing step are, for example, an illuminance of 70 mW / cm. 2 The irradiation time is 15 seconds. Alternatively, the heating conditions for the provisional curing step are, for example, a temperature of 100° C. and a time of 60 seconds.

[0057] In the provisional curing step, light irradiation or heating may be performed from the opposite side of the large-sized transparent substrate 30Z (or the transparent substrate 30), or light irradiation or heating may be performed from the large-sized transparent substrate 30Z (or the transparent substrate 30) side.

[0058] In the provisional curing step, light irradiation may be performed while the printing plates M1 and M2 are in place, which can prevent the printing material from dripping and allow the light diffusion film and frame to have a rectangular shape.

[0059] Next, as shown in FIG. 5E, the printing plates M2 and M1 are removed, and the multiple (or one) light diffusion film materials 45Z and the multiple (or one) frame materials 40Z after the provisional curing process are irradiated with excimer light (excimer light irradiation process). The excimer light irradiation conditions for the excimer light irradiation process are, for example, an illuminance of 170 mW / cm. 2 , and the exposure time is 4 minutes.

[0060] Specifically, the excimer light is irradiated onto the inner main surface 46 of the plurality (or one) of light diffusion film materials 45Z and the inner side surface 41 of the plurality (or one) of frame materials 40Z. For example, the excimer light may be irradiated from the opposite side of the large-sized transparent substrate 30Z (or transparent substrate 30). At this time, the outer side surface 42 and end surface of the plurality (or one) of frame materials 40Z may be covered with a mask member.

[0061] At this time, as described above, the surfaces of the inner principal surfaces 46 of the materials 45Z of the multiple (or one) light diffusion films are altered and contract (see FIG. 3A). As a result, the surfaces of the inner principal surfaces 46 of the light diffusion film 45 have a matte effect and can diffusely reflect light.

[0062] As described above, the surface of the inner side 41 of the material 40Z of the frames (or one of them) changes in quality and shrinks (see FIG. 3A). This allows the surface of the inner side 41 of the frame 40 to have a matte effect and to diffusely reflect light.

[0063] At this time, the surfaces of the outer faces 42 and the lower end faces of the material 40Z of the multiple (or one) frames may also change in quality and shrink.

[0064] Next, as shown in FIG. 5F, the material 45Z of the multiple (or one) light diffusion films and the material 40Z of the multiple (or one) frames after the excimer light irradiation process are irradiated with light (e.g., ultraviolet light), heated, or irradiated with light and heated to completely harden the material 45Z of the multiple (or one) light diffusion films and the material 40Z of the multiple (or one) frames. This results in multiple light diffusion films 45 and frames 40 (complete hardening process). Complete hardening refers to a state in which the entire surface and interior are dried and hardened. The UV light irradiation conditions for the complete hardening process are, for example, an illuminance of 140 mW / cm. 2 The irradiation time is 10 seconds. Alternatively, the heating conditions for the main curing step are, for example, a temperature of 150° C. and a time of 30 minutes.

[0065] In the main curing step, light irradiation or heating may be performed from the opposite side of the large-sized transparent substrate 30Z (or the transparent substrate 30), or light irradiation or heating may be performed from the large-sized transparent substrate 30Z (or the transparent substrate 30) side.

[0066] 5G, the large-sized transparent substrate 30Z (or the transparent substrate 30) is cut along cutting lines CL to be individualized (single process). This results in a plurality of transparent substrates 30 on which the light diffusion film 45 and the frame 40 are formed, i.e., a plurality of optical substrates 30A.

[0067] The frame 40 may be formed after obtaining the transparent substrate 30 on which the light diffusion film 45 is formed, that is, the optical substrate 30A, by the provisional curing step, the excimer light irradiation step, and the main curing step described above.

[0068] Next, as shown in Fig. 5H, adhesive 50 is applied to frame 40, and transparent substrate 30 (optical substrate 30A) on which light diffusion film 45 and frame 40 are formed is combined and bonded to substrate 20 on which solid-state imaging element 10 is mounted (combination process). At this time, conductive members 24 such as solder balls may be combined and bonded to the back side of substrate 20. In this way, solid-state imaging device 1 shown in Fig. 2 is obtained.

[0069] The order of the singulation step and the assembly step may be reversed. For example, the large-sized transparent substrate 30 on which the plurality of light diffusion films 45 and the plurality of frames 40 are formed may be assembled with the large-sized substrate 20 on which the plurality of solid-state imaging elements 10 are mounted, and then the combined substrate may be singulated to obtain the solid-state imaging device 1 shown in FIG.

[0070] The combining step may be performed before the main curing step. In particular, when an adhesive resin is used as the frame material, the transparent substrate 30 on which the frame material 40Z is formed after the provisional curing step but before the main curing step may be bonded to the substrate 20 on which the solid-state imaging element 10 is mounted, and then the main curing step may be performed. In this way, the adhesive 50 may not be used.

[0071] As described above, the manufacturing method of the solid-state imaging device and the optical substrate of the first embodiment includes an excimer light irradiation step of irradiating the inner surface 41 of the frame material 40Z with excimer light. As a result, the inner surface 41 of the frame material 40Z is altered and shrinks. As a result, according to the solid-state imaging device 1 and the optical substrate 30A of the first embodiment, the inner surface 41 of the frame 40 has an irregular wrinkle structure.

[0072] Thus, according to the solid-state imaging device 1 and optical substrate 30A of the first embodiment, and the method for manufacturing the solid-state imaging device and the optical substrate, the inner surface 41 of the frame 40 can obtain a matte effect and can diffusely reflect light. As a result, in the solid-state imaging device 1 using the optical substrate 30A, it is possible to reduce the reflected light (stray light) from the inner surface 41 of the frame 40 that enters the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0073] Moreover, according to the solid-state imaging device 1 and optical substrate 30A of the first embodiment, a light diffusion film 45 is disposed on the inner surface side of the transparent substrate 30 at a position corresponding to the periphery of the solid-state imaging element 10 and the periphery of the imaging region 12 of the solid-state imaging element 10. This makes it possible to reduce reflected light (stray light) from the inner surface of the transparent substrate 30 in the solid-state imaging device 1 that enters the imaging region 12 of the solid-state imaging element 10, thereby reducing optical noise such as flare or ghost that occurs in the captured image.

[0074] Furthermore, the manufacturing method of the solid-state imaging device and the optical substrate of the first embodiment includes an excimer light irradiation step of irradiating the inner main surface (the main surface opposite to the transparent substrate 30) 46 of the light diffusion film material 45Z with excimer light. As a result, the inner main surface 46 of the light diffusion film material 45Z is altered and shrinks. As a result, according to the solid-state imaging device 1 and the optical substrate 30A of the first embodiment, the inner main surface (the main surface opposite to the transparent substrate 30) 46 of the light diffusion film 45 has an irregular wrinkle structure.

[0075] Thus, according to the solid-state imaging device 1 and optical substrate 30A, and the manufacturing method for the solid-state imaging device of the first embodiment, the inner main surface 46 of the light diffusion film 45 has a matte effect and can diffusely reflect light. As a result, in the solid-state imaging device 1 using the optical substrate 30A, it is possible to reduce the reflected light (stray light) from the inner main surface 46 of the light diffusion film 45 that enters the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0076] Here, the material of the light diffusion film or frame was printed and temporarily cured on a white glass plate, and the reflectance of the surface of the light diffusion film or frame material, the density and elastic modulus of the light diffusion film or frame material were measured before and after excimer light irradiation. The conditions were as follows. Material for light diffusion film or frame: Resin having multiple cationic polymerizable groups (specifically alicyclic epoxy groups) in one molecule and having a cyclic polysiloxane structure in the main chain, thickness 100 μm Pre-curing: UV light irradiation, illuminance 70mW / cm 2 , exposure time 15 seconds Excimer light irradiation: Illuminance 170mW / cm 2 , exposure time 4 minutes

[0077] The measurement results of the reflectance of the surface of the light diffusion film or frame material before and after irradiation with excimer light are shown in Table 1. As shown in Table 1, by irradiating the light diffusion film or frame material with excimer light, the reflectance of the surface of the light diffusion film or frame material could be reduced in the wavelength range from visible light to near infrared light. [Table 1]

[0078] The density of the light diffusion film or the material of the frame, i.e., the mass per unit volume ρ, was measured in accordance with JIS K7112:1980 (ISO 1183:1987). As a result, the density of the surface layer of the light diffusion film or the material of the frame was 1.361 to 1.512 g / cm 3 The density of the part other than the surface layer is 1.172 to 1.288 g / cm 3 It was.

[0079] The elastic modulus (i.e., Young's modulus E) of the light diffusion film or frame material was measured using a scanning probe microscope (Bruker AXS). As a result, the elastic modulus of the surface layer of the light diffusion film or frame material was 2.30 to 2.95 GPa, and the elastic modulus of the portion other than the surface layer was 1.55 to 2.25 GPa.

[0080] [Second embodiment] (Solid-state imaging device and optical substrate) Fig. 6 is a schematic cross-sectional view of a solid-state imaging device and an optical substrate according to the second embodiment. The solid-state imaging device 1A shown in Fig. 6 is a so-called GoC (Glass on Chip) type solid-state imaging device. The solid-state imaging device 1A of the second embodiment differs from the solid-state imaging device 1 of the first embodiment described above in that a frame 40 is disposed on the solid-state imaging element 10, and the solid-state imaging element 10 and the substrate 20 are electrically connected by wiring 22 such as bonding wires outside the frame 40.

[0081] Specifically, the solid-state imaging element 10 is mounted on a substrate 20, and the transparent substrate 30 is disposed so as to face the solid-state imaging element 10. A light diffusion film 45 is disposed on the inner surface of the transparent substrate 30 at a position corresponding to the periphery of the imaging region 12 of the solid-state imaging element 10. The frame (rib material) 40 is disposed between the solid-state imaging element 10 and the transparent substrate 30, more specifically, between the solid-state imaging element 10 and the light diffusion film 45, so as to surround the imaging region 12 of the solid-state imaging element 10. The solid-state imaging element 10 and the substrate 20 are electrically connected by wiring 22 such as bonding wires outside the frame 40. The wiring 22 such as bonding wires is covered and protected by potting resin 60.

[0082] (Method of manufacturing solid-state imaging device and optical substrate) Next, a method for manufacturing the solid-state imaging device and the optical substrate according to the second embodiment will be described with reference to Fig. 7. Fig. 7 is a schematic diagram showing an assembly process of a transparent substrate (optical substrate) with a light diffusion film and a frame and a substrate mounting a solid-state imaging element in the method for manufacturing the solid-state imaging device according to the second embodiment.

[0083] 5A to 5G, the transparent substrate 30 on which the light diffusion film 45 and the frame 40 are formed, i.e., the optical substrate 30A, is obtained. Note that, as described above, the frame 40 may be formed after the transparent substrate 30 on which the light diffusion film 45 is formed, i.e., the optical substrate 30A, is obtained.

[0084] 7, an adhesive 50 is applied to the frame 40, and the transparent substrate 30 (optical substrate 30A) on which the light diffusion film 45 and the frame 40 are formed is combined and bonded to the solid-state imaging element 10 mounted on the substrate 20 (combination process). At this time, the wiring 22 such as the bonding wire may be potted with resin, and the wiring 22 such as the bonding wire may be covered with a potting resin 60. Also, a conductive member 24 such as a solder ball may be combined and bonded to the back side of the substrate 20. In this way, the solid-state imaging device 1A shown in FIG. 6 is obtained.

[0085] In the second embodiment, the combining step may be performed before the main curing step. In particular, when an adhesive resin is used as the frame material, the transparent substrate 30 on which the frame material 40Z is formed after the provisional curing step but before the main curing step may be bonded to the solid-state imaging element 10, and then the main curing step may be performed. In this way, the adhesive 50 may not be used.

[0086] The method for manufacturing the solid-state imaging device and the optical substrate of the second embodiment also includes the step shown in Fig. 5E, that is, the excimer light irradiation step of irradiating the inner surface 41 of the frame material 40Z with excimer light. As a result, the inner surface 41 of the frame material 40Z is altered and contracts. As a result, in the solid-state imaging device 1A and the optical substrate 30A of the second embodiment, the inner surface 41 of the frame 40 also has an irregular wrinkle structure.

[0087] In this way, in the solid-state imaging device 1A and optical substrate 30A, and the manufacturing method of the solid-state imaging device and the optical substrate of the second embodiment, the inner surface 41 of the frame 40 can obtain a matte effect and can diffusely reflect light. As a result, in the solid-state imaging device 1A using the optical substrate 30A, it is possible to reduce the reflected light (stray light) from the inner surface 41 of the frame 40 that is incident on the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0088] Also, in the solid-state imaging device 1A and optical substrate 30A of the second embodiment, a light diffusion film 45 is disposed on the inner surface side of the transparent substrate 30 at a position corresponding to the periphery of the solid-state imaging element 10 and the periphery of the imaging region 12 of the solid-state imaging element 10. This makes it possible to reduce reflected light (stray light) from the inner surface of the transparent substrate 30 in the solid-state imaging device 1A that enters the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0089] Furthermore, the manufacturing method of the solid-state imaging device and the optical substrate of the second embodiment also includes an excimer light irradiation step of irradiating the inner main surface (the main surface opposite to the transparent substrate 30) 46 of the light diffusion film material 45Z with excimer light. As a result, the inner main surface 46 of the light diffusion film material 45Z is altered and shrinks. As a result, in the solid-state imaging device 1A and the optical substrate 30A of the second embodiment, the inner main surface (the main surface opposite to the transparent substrate 30) 46 of the light diffusion film 45 also has an irregular wrinkle structure.

[0090] In this way, in the solid-state imaging device 1A and optical substrate 30A, and the manufacturing method of the solid-state imaging device and the optical substrate of the second embodiment, the inner main surface 46 of the light diffusion film 45 can also obtain a matte effect and can diffusely reflect light. As a result, in the solid-state imaging device 1A using the optical substrate 30A, it is possible to reduce the reflected light (stray light) from the inner main surface 46 of the light diffusion film 45 that enters the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0091] [Third embodiment] (Solid-state imaging device and optical substrate) Fig. 8 is a schematic cross-sectional view of a solid-state imaging device and an optical substrate according to the third embodiment. The solid-state imaging device 1B shown in Fig. 8 is a so-called CSP (Chip Size Package) type solid-state imaging device. The solid-state imaging device 1B of the third embodiment differs from the solid-state imaging device 1A of the second embodiment described above in that it does not include a substrate 20 and directly connects electrically to the outside through electrodes such as pads formed on the back surface of the solid-state imaging element 10.

[0092] Specifically, the transparent substrate 30 is disposed so as to face the solid-state imaging element 10. A light diffusion film 45 is disposed on the inner surface side of the transparent substrate 30 at a position corresponding to the periphery of the imaging region 12 of the solid-state imaging element 10. The frame (rib material) 40 is disposed between the solid-state imaging element 10 and the transparent substrate 30, more specifically, between the solid-state imaging element 10 and the light diffusion film 45 so as to surround the imaging region 12 of the solid-state imaging element 10. An electrode 25 such as a pad is formed on the back surface of the solid-state imaging element 10, and a conductive member 24 such as a solder ball is electrically connected to the electrode 25 such as the pad.

[0093] (Method of manufacturing solid-state imaging device and optical substrate) Next, a method for manufacturing a solid-state imaging device and an optical substrate according to the third embodiment will be described with reference to Fig. 9. Fig. 9 is a schematic diagram showing an assembly process of a transparent substrate (optical substrate) with a light diffusion film and a frame and a substrate mounting a solid-state imaging element in the method for manufacturing a solid-state imaging device according to the third embodiment.

[0094] 5A to 5G, the transparent substrate 3 on which the light diffusion film 45 and the frame 40 are formed, i.e., the optical substrate 30A, is obtained. Note that, as described above, the frame 40 may be formed after the transparent substrate 30 on which the light diffusion film 45 is formed, i.e., the optical substrate 30A, is obtained.

[0095] 9, an adhesive 50 is applied to the frame 40, and the transparent substrate 30 (optical substrate 30A) on which the light diffusion film 45 and the frame 40 are formed is combined and bonded to the solid-state imaging element 10 (combination process). At this time, a conductive member 24 such as a solder ball may be combined and bonded to an electrode 25 such as a pad on the back side of the solid-state imaging element 10. In this way, the solid-state imaging device 1B shown in FIG. 8 is obtained.

[0096] In the third embodiment, the combining step may be performed before the main curing step. In particular, when an adhesive resin is used as the frame material, the transparent substrate 30 on which the frame material 40Z is formed after the provisional curing step but before the main curing step may be bonded to the solid-state imaging element 10, and then the main curing step may be performed. In this way, the adhesive 50 may not be used.

[0097] The manufacturing method of the solid-state imaging device and the optical substrate of the third embodiment also includes the step shown in Fig. 5E, that is, the excimer light irradiation step of irradiating the inner surface 41 of the frame material 40Z with excimer light. As a result, the inner surface 41 of the frame material 40Z is altered and contracts. As a result, in the solid-state imaging device 1B and the optical substrate 30A of the third embodiment, the inner surface 41 of the frame 40 has an irregular wrinkle structure.

[0098] In this way, in the solid-state imaging device 1B and optical substrate 30A, and the manufacturing method of the solid-state imaging device and the optical substrate of the third embodiment, the inner surface 41 of the frame 40 can obtain a matte effect and can diffusely reflect light. As a result, in the solid-state imaging device 1B using the optical substrate 30A, it is possible to reduce the reflected light (stray light) from the inner surface 41 of the frame 40 that is incident on the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0099] Also, in the solid-state imaging device 1B and optical substrate 30A of the third embodiment, a light diffusion film 45 is disposed on the inner surface side of the transparent substrate 30 at a position corresponding to the periphery of the solid-state imaging element 10 and the periphery of the imaging region 12 of the solid-state imaging element 10. This makes it possible to reduce reflected light (stray light) from the inner surface of the transparent substrate 30 in the solid-state imaging device 1B that enters the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0100] Furthermore, the manufacturing method of the solid-state imaging device and the optical substrate of the third embodiment also includes an excimer light irradiation step of irradiating the inner main surface (the main surface opposite to the transparent substrate 30) 46 of the material 45Z of the light diffusion film with excimer light. As a result, the inner main surface 46 of the material 45Z of the light diffusion film is altered and shrinks. As a result, in the solid-state imaging device 1B and the optical substrate 30A of the third embodiment, the inner main surface (the main surface opposite to the transparent substrate 30) 46 of the light diffusion film 45 also has an irregular wrinkle structure.

[0101] In this way, in the solid-state imaging device 1B and optical substrate 30A, and the manufacturing method of the solid-state imaging device and the optical substrate of the third embodiment, the inner main surface 46 of the light diffusion film 45 can also obtain a matte effect and can diffusely reflect light. As a result, in the solid-state imaging device 1B using the optical substrate 30A, it is possible to reduce the reflected light (stray light) from the inner main surface 46 of the light diffusion film 45 that enters the imaging region 12 of the solid-state imaging element 10, and to reduce optical noise such as flare or ghost that occurs in the captured image.

[0102] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-mentioned embodiments, and various changes and modifications are possible. For example, in the above-mentioned embodiments, a so-called box-type solid-state imaging device and optical substrate (FIG. 2), a so-called GoC (Glass on Chip) type solid-state imaging device and optical substrate (FIG. 6), and a so-called CSP (Chip Size Package) type solid-state imaging device and optical substrate (FIG. 8) are exemplified. However, the features of the present invention are not limited to these, and can be applied to various types of solid-state imaging devices and optical substrates. [Explanation of symbols]

[0103] 1, 1A, 1B Solid-state imaging device 10 Solid-state imaging element 12 Imaging area 20 Substrate 22 Wiring 24 Conductive materials 25 electrodes 30 Transparent Substrate 30A optical board 30Z Large transparent substrate 40 frames 40Z Frame Materials 41 Inner surface 42 External surface 45 Light Diffusion Film 45Z Light Diffusion Film Material 46 Inner main surface 47 Outer surface 50 Adhesive 60 Resin M Print version

Claims

1. A transparent substrate; a light diffusing film laminated on one main surface of the transparent substrate and having an optical path opening; Equipped with The surface roughness Ra of the main surface of the light diffusion film opposite to the transparent substrate is 50 nm or more and 3000 nm or less, The density of the surface layer of the main surface of the light diffusing film is 1.1 g / cm 3 1.6g / cm or more 3 is as follows: The density of a surface layer of the main surface of the light diffusion film is higher than the density of a portion other than the surface layer. optical board.

2. The optical substrate according to claim 1 , further comprising a frame disposed on the main surface side of the light diffusion film and having an inner diameter larger than the light path opening.

3. The optical substrate according to claim 1 , wherein the main surface of the light diffusing film has a surface roughness Ra of 200 nm or more and 3000 nm or less.

4. The elastic modulus of the surface layer of the main surface of the light diffusion film is 2.3 GPa or more and 3.0 GPa or less; The elastic modulus of the surface layer of the main surface of the light diffusion film is higher than the elastic modulus of a portion other than the surface layer. The optical substrate of claim 1 .

5. 5. The optical substrate according to claim 1, wherein the main surface of the light diffusing film has an irregular wrinkle structure.

6. A transparent substrate; a light diffusing film laminated on one main surface of the transparent substrate and having an optical path opening; Equipped with An optical substrate, wherein a main surface of the light diffusion film opposite to the transparent substrate has an irregular wrinkle structure.

7. A method for producing an optical substrate according to claim 1 or 6, comprising the steps of: a printing step of printing a material of the light diffusion film on the transparent substrate by a printing method using a printing plate, using a photocurable material or a photocurable and thermosetting material; a temporary curing step of irradiating light onto the material of the light diffusion film to temporarily cure the material of the light diffusion film; an excimer light irradiation step of irradiating an excimer light onto a main surface of the light diffusion film material opposite to the transparent substrate after the provisional curing step; a main curing step of performing light irradiation, heating, or light irradiation and heating on the material of the light diffusion film after the excimer light irradiation step to main cure the material of the light diffusion film to obtain the light diffusion film; A method for manufacturing an optical substrate, comprising:

8. A method for producing an optical substrate according to claim 1 or 6, comprising the steps of: a printing step of printing a material of the light diffusion film on the transparent substrate by a printing method using a printing plate, using a thermosetting material or a photosetting and thermosetting material; a temporary curing step of heating the material of the light diffusion film to temporarily cure the material of the light diffusion film; an excimer light irradiation step of irradiating an excimer light onto a main surface of the light diffusion film material opposite to the transparent substrate after the provisional curing step; a main curing step of heating, irradiating with light, or irradiating with light and heating the material of the light diffusion film after the excimer light irradiation step to main cure the material of the light diffusion film to obtain the light diffusion film; A method for manufacturing an optical substrate, comprising:

9. A solid-state imaging element; A substrate on which the solid-state imaging element is mounted; a transparent substrate disposed opposite the substrate; a light diffusion film disposed on the inner surface side of the transparent substrate at a position corresponding to the periphery of the solid-state imaging element; a frame disposed between the substrate and the transparent substrate so as to surround the solid-state imaging element; Equipped with The inner main surface of the light diffusing film has an irregular wrinkle structure. Solid-state imaging device.

10. A solid-state imaging element; a transparent substrate disposed opposite the solid-state imaging element; a light diffusion film disposed on the inner surface side of the transparent substrate at a position corresponding to the periphery of an imaging area of ​​the solid-state imaging element; a frame disposed between the solid-state imaging element and the transparent substrate so as to surround an imaging region of the solid-state imaging element; Equipped with The inner main surface of the light diffusing film has an irregular wrinkle structure. Solid-state imaging device.

11. 11. The solid-state imaging device according to claim 9, wherein a surface roughness Ra of an inner main surface of the light diffusing film is 200 nm or more and 3000 nm or less.

12. The density of the surface layer of the inner main surface of the light diffusion film is 1.1 g / cm 3 1.6g / cm or more 3 is as follows: The density of a surface layer of the inner main surface of the light diffusion film is higher than the density of a portion other than the surface layer.

11. The solid-state imaging device according to claim 9.

13. The elastic modulus of the surface layer of the inner main surface of the light diffusion film is 2.3 GPa or more and 3.0 GPa or less, The elastic modulus of a surface layer of the inner main surface of the light diffusion film is higher than the elastic modulus of a portion other than the surface layer.

11. The solid-state imaging device according to claim 9.

14. A method for manufacturing a solid-state imaging device according to claim 9, comprising the steps of: a printing step of printing a material of the light diffusion film on the transparent substrate by a printing method using a printing plate, using a photocurable material or a photocurable and thermosetting material; a temporary curing step of irradiating light onto the material of the light diffusion film to temporarily cure the material of the light diffusion film; an excimer light irradiation step of irradiating an inner main surface of the material of the light diffusion film after the provisional curing step with excimer light; a main curing step of performing light irradiation, heating, or light irradiation and heating on the material of the light diffusion film after the excimer light irradiation step to main cure the material of the light diffusion film to obtain the light diffusion film; forming the frame on the transparent substrate; a combining process of combining the transparent substrate on which the light diffusion film and the frame are formed after the main curing process, or the transparent substrate on which the material of the light diffusion film and the material of the frame are formed before the main curing process, with the substrate on which the solid-state imaging element is mounted; A method for manufacturing a solid-state imaging device, comprising:

15. A method for manufacturing a solid-state imaging device according to claim 10, comprising the steps of: a printing step of printing a material of the light diffusion film on the transparent substrate by a printing method using a printing plate, using a photocurable material or a photocurable and thermosetting material; a temporary curing step of irradiating light onto the material of the light diffusion film to temporarily cure the material of the light diffusion film; an excimer light irradiation step of irradiating an inner main surface of the material of the light diffusion film after the provisional curing step with excimer light; a main curing step of performing light irradiation, heating, or light irradiation and heating on the material of the light diffusion film after the excimer light irradiation step to main cure the material of the light diffusion film to obtain the light diffusion film; forming the frame on the transparent substrate; a combining step of combining the transparent substrate on which the light diffusion film and the frame are formed after the main curing step, or the transparent substrate on which the material of the light diffusion film and the material of the frame are formed before the main curing step, with the solid-state imaging element; A method for manufacturing a solid-state imaging device, comprising:

16. A method for manufacturing a solid-state imaging device according to claim 9, comprising the steps of: a printing step of printing a material of the light diffusion film on the transparent substrate by a printing method using a printing plate, using a thermosetting material or a photosetting and thermosetting material; a temporary curing step of heating the material of the light diffusion film to temporarily cure the material of the light diffusion film; an excimer light irradiation step of irradiating an inner main surface of the material of the light diffusion film after the provisional curing step with excimer light; a main curing step of heating, irradiating with light, or irradiating with light and heating the material of the light diffusion film after the excimer light irradiation step to main cure the material of the light diffusion film to obtain the light diffusion film; forming the frame on the transparent substrate; a combining process of combining the transparent substrate on which the light diffusion film and the frame are formed after the main curing process, or the transparent substrate on which the material of the light diffusion film and the material of the frame are formed before the main curing process, with the substrate on which the solid-state imaging element is mounted; A method for manufacturing a solid-state imaging device, comprising:

17. A method for manufacturing a solid-state imaging device according to claim 10, comprising the steps of: a printing step of printing a material of the light diffusion film on the transparent substrate by a printing method using a printing plate, using a thermosetting material or a photosetting and thermosetting material; a temporary curing step of heating the material of the light diffusion film to temporarily cure the material of the light diffusion film; an excimer light irradiation step of irradiating an inner main surface of the material of the light diffusion film after the provisional curing step with excimer light; a main curing step of heating, irradiating with light, or irradiating with light and heating the material of the light diffusion film after the excimer light irradiation step to main cure the material of the light diffusion film to obtain the light diffusion film; forming the frame on the transparent substrate; a combining step of combining the transparent substrate on which the light diffusion film and the frame are formed after the main curing step, or the transparent substrate on which the material of the light diffusion film and the material of the frame are formed before the main curing step, with the solid-state imaging element; A method for manufacturing a solid-state imaging device, comprising:

Citation Information

Patent Citations

  • Solid state image pickup device and manufacturing method of the same

    JP2014216475A

Cited By

  • Semiconductor packages

    JP2026135682A