Method for preparing high-adhesion aluminum laminated film by adopting magnetron sputtering method

The high adhesion aluminum-plated film is prepared by magnetron sputtering method, which solves the problems of easy falling off and unstable performance of the aluminum-plated film in the mobile phone case, achieves high adhesion and performance improvement of the aluminum-plated film, and ensures the quality of the aluminum-plated film and service life.

CN118932306AInactive Publication Date: 2024-11-12ZHEJIANG YICAI ELECTRONICS CO LTD
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202410998432.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The aluminum-plated film of existing mobile phone cases is prone to fall off during use, and the aluminum-plated process cannot ensure the stability of the subsequent film performance.

Method used

Magneto-controlled sputtering method is used to prepare high adhesion aluminum coating, including substrate cleaning and treatment, vacuum chamber preparation, target installation, sputtering gas introduction, magnetron sputtering coating, coating parameter control, annealing and surface treatment, finished products Test.

Benefits of technology

It effectively improves the adhesion and performance of the aluminum-plated film, avoids falling off during long-term use, and ensures the thickness, adhesion and optical performance of the aluminum-plated film through quality inspection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932306A_ABST
    Figure CN118932306A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flexible packaging film materials, and discloses a method for preparing a high-adhesion aluminum laminated film by adopting a magnetron sputtering method. The method for preparing the high-adhesion aluminum laminated film through the magnetron sputtering method comprises the following specific steps of substrate preparation, vacuum chamber preparation, target material installation, sputtering gas introduction, magnetron sputtering coating, coating parameter control, coating post-treatment and finished product detection. According to the method for preparing the high-adhesion aluminum laminated film by adopting the magnetron sputtering method, the flatness treatment is performed on the surface of the substrate after aluminum plating is finished, and the surface modification treatment is performed through plasma treatment, so that the adhesion and the performance of the film layer can be effectively improved, and the falling phenomenon caused by long-time use is effectively avoided. Through thickness measurement, adhesive force test, surface roughness test and optical performance test on a finished product, the quality of the aluminum laminated film can be effectively ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flexible packaging film materials, in particular to a method for preparing a high-adhesion aluminum-plated film by adopting a magnetron sputtering method. Background Art

[0002] Mobile phone cases are generally made of plastic. The aluminum plating process of plastic films generally adopts the direct plating method, that is, the aluminum layer is directly plated on the surface of the substrate film. BOPET (biaxially oriented polyester) and BOPA (biaxially oriented nylon) film substrates do not need surface treatment before aluminum plating, and can be directly evaporated. However, non-polar plastic films such as BOPP (biaxially oriented polypropylene film), CPP (cast polypropylene film), PE (polyethylene) need to be coated with an adhesive layer, corona treated or low-temperature plasma surface modified before evaporation, so that the surface tension reaches 38-42 dynes / cm or has good adhesion. Otherwise, the vapor-deposited aluminum film on its surface has poor adhesion and is easy to fall off due to external force.

[0003] At present, the performance of the subsequent aluminum-plated film cannot be guaranteed after the aluminum-plating process of mobile phone cases is completed. Moreover, with long-term use, the aluminum-plated film on the surface of the mobile phone case can easily fall off due to repeated friction during use. Therefore, we propose a method for preparing a high-adhesion aluminum-plated film using magnetron sputtering. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a high-adhesion aluminum-plated film by magnetron sputtering, so as to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a high-adhesion aluminum-plated film by magnetron sputtering, the method for preparing a high-adhesion aluminum-plated film by magnetron sputtering comprising the following specific steps:

[0006] S1. Substrate preparation: a plastic film is selected as the substrate, and the plastic film is cleaned and treated to remove pollutants and impurities on the surface;

[0007] S2. Preparation of vacuum chamber: Place the processed substrate into the vacuum chamber, close the vacuum chamber door, start the vacuum system, remove the air in the vacuum chamber, and make the vacuum degree reach the target value;

[0008] S3. Target installation: Install the pure aluminum target on the magnetron sputtering target and ensure that the distance between the target and the substrate surface is appropriate;

[0009] S4, sputtering gas introduction: introducing sputtering gas into the vacuum chamber;

[0010] S5. Magnetron sputtering coating: Turn on the magnetron sputtering power supply to generate a magnetic field to ionize the argon gas to form plasma. Under the action of the magnetic field, the argon ions in the plasma will accelerate to hit the surface of the aluminum target and sputter out aluminum atoms. These aluminum atoms will be deposited on the substrate surface and form an aluminum film;

[0011] S6. Coating parameter control: During the sputtering coating process, it is necessary to control the coating parameters such as sputtering power, sputtering time, sputtering gas flow rate, and working pressure, which can effectively ensure the quality and performance of the aluminum coating;

[0012] S7, post-coating treatment: After sputtering coating, the aluminum film needs to be annealed and surface treated, which can effectively improve the performance and adhesion of the aluminum film;

[0013] S8. Finished product inspection: Conduct quality inspection on the prepared aluminum-plated film, including thickness measurement, adhesion test, surface roughness test, and optical performance test to ensure that the aluminum-plated film meets the requirements.

[0014] Preferably, the preparation of the substrate in S1 comprises the following specific steps:

[0015] S1.1. Use a cleaning agent to clean the surface of the selected plastic film substrate. First, place the plastic film in the cleaning agent and soak it. After soaking for 5-10 minutes, wipe it with a cotton cloth to remove the oil, dust and other pollutants attached to the surface;

[0016] S1.2. After wiping, rinse the plastic film of the cleaning dog with deionized water to remove the residual detergent and impurities on the surface of the plastic film;

[0017] S1.3. Place the washed plastic film in a drying oven for drying. The temperature of the drying oven should be controlled at 60℃-80℃ and the drying time should be controlled at 8-15min.

[0018] S1.4. Activating the surface of the plastic film by plasma treatment can effectively improve the adhesion between the aluminum mold and the plastic film;

[0019] S1.5. Before aluminum plating, the treated plastic film should be thoroughly inspected to ensure that its surface is clean, free of contaminants and damage.

[0020] Preferably, the sputtering gas introduced in S4 is argon.

[0021] Preferably, the vacuum chamber preparation in S2 comprises the following specific steps:

[0022] S2.1. Ensure that the vacuum chamber is clean, free of dirt and impurities, check the sealing performance of the vacuum chamber, and ensure that the door can be closed tightly and maintain vacuum;

[0023] S2.2. Carefully place the treated plastic film substrate on the fixture in the vacuum chamber, ensuring that the substrate is placed stably and will not be damaged or contaminated;

[0024] S2.3. Ensure that the door is tightly closed and the vacuum chamber is well sealed. Check whether the door seal is intact and replace it if necessary.

[0025] S2.4. Turn on the power of the vacuum system and start the vacuum pump. The vacuum pump will begin to extract the air in the vacuum chamber and gradually reduce the pressure in the chamber.

[0026] S2.5. Use a vacuum gauge to monitor the pressure changes in the vacuum chamber. As the vacuum pump runs, the vacuum degree will gradually increase.

[0027] S2.6. Determine the required target vacuum degree according to the specific process requirements and continue to operate the vacuum pump until the vacuum degree reaches or exceeds the target value;

[0028] S2.7. Once the target vacuum degree is reached, it is necessary to maintain the vacuum state of the vacuum chamber, ensure that the vacuum pump continues to operate, and check whether there is any leakage in the vacuum system. If any leakage is found, it should be repaired in time.

[0029] Preferably, in the S6, parameters such as vacuum chamber pressure and current are continuously monitored during the sputtering process. Due to different sputtering rates and uneven heat dissipation of the blocking material, the final aluminum-plated film may have an uneven film thickness problem, which can be alleviated by adjusting the sputtering power, target-base distance, argon gas flow rate and sputtering time, and the key point is to change the position of each sputtering point from time to time. During the sputtering process, the growth rate, thickness, flatness and other properties of the film are controlled by regulating the sputtering parameters. After sputtering is completed, the sputtering power is turned off and the introduction of sputtering gas is stopped.

[0030] Preferably, the annealing treatment of the aluminum-plated film in S7 includes the following specific steps:

[0031] S7.1.1. Place the aluminum-coated substrate into an annealing furnace, gradually increase the temperature of the annealing furnace to reach a preset annealing temperature, and maintain the preset annealing temperature for a certain period of time to ensure that the film layer completes the annealing process;

[0032] S7.1.2. As annealing continues, gradually lower the temperature of the annealing furnace, allow it to slowly cool to room temperature, and carefully take out the annealed substrate.

[0033] Preferably, the surface treatment of the aluminum-plated film in S7 comprises the following specific steps:

[0034] S7.2.1. Use appropriate solvents to remove contaminants from the substrate surface and rinse the substrate surface with deionized water to ensure cleanliness;

[0035] S7.2.2. The substrate is treated for surface flatness, polished to improve the surface condition, and treated with plasma to modify the surface, which can effectively improve the adhesion and performance of the film layer. After the treatment, the treated substrate is cleaned and dried to remove any residual treatment agent or moisture.

[0036] Preferably, after the pure aluminum target is installed in S3, a laser rangefinder is used to measure the distance between the target and the substrate surface, and the height of the substrate stage and the position of the target are adjusted to make the distance reach an appropriate value, thereby ensuring that the distance between the target and the substrate surface is appropriate.

[0037] Preferably, in S7, when the coating reaches the predetermined thickness and quality requirements, the sputtering process is stopped and the equipment is allowed to cool down naturally. After the temperature drops to a safe range, air is slowly introduced into the sputtering chamber to balance the internal and external pressures. The aluminum-plated substrate is then carefully taken out for subsequent testing and analysis, which can effectively ensure the quality of the aluminum-plated substrate.

[0038] Compared with the prior art, the present invention provides a method for preparing a high-adhesion aluminum-plated film by magnetron sputtering, which has the following beneficial effects:

[0039] 1. The method of preparing a high-adhesion aluminum-plated film by magnetron sputtering can effectively improve the adhesion and performance of the film layer by flattening the surface of the substrate after aluminum plating and performing surface modification by plasma treatment, and effectively avoid shedding after long-term use.

[0040] 2. The method of preparing high-adhesion aluminum-plated film by magnetron sputtering can effectively ensure the quality of the aluminum-plated film by measuring the thickness, adhesion, surface roughness and optical performance of the finished product.

[0041] 3. The method of preparing high-adhesion aluminum-coated film by magnetron sputtering continuously monitors parameters such as vacuum chamber pressure and current during the sputtering process. Due to different sputtering rates and uneven heat dissipation of the blocking material, the final aluminum-coated film may have uneven film thickness. The problem is alleviated by adjusting the sputtering power, target-base distance, argon gas flow rate and sputtering time, and the key point is to change the position of each sputtering point from time to time. In the sputtering process, the growth rate, thickness, flatness and other properties of the film are controlled by adjusting the sputtering parameters. After the sputtering is completed, the sputtering power is turned off and the introduction of the sputtering gas is stopped, which can effectively ensure the quality and performance of the aluminum-coated film. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 It is a schematic diagram of the steps of the present invention;

[0043] Figure 2 The present invention is a schematic diagram of the specific steps of the method for preparing a high-adhesion aluminum-plated film by magnetron sputtering. DETAILED DESCRIPTION

[0044] like Figure 1-Figure 2 As shown, the present invention provides a technical solution: a method for preparing a high-adhesion aluminum-plated film by magnetron sputtering, and the method for preparing a high-adhesion aluminum-plated film by magnetron sputtering comprises the following specific steps:

[0045] S1. Substrate preparation: a plastic film is selected as a substrate, and the plastic film is cleaned and treated to remove pollutants and impurities on the surface. The substrate preparation includes the following specific steps:

[0046] S1.1. Use a cleaning agent to clean the surface of the selected plastic film substrate. First, place the plastic film in the cleaning agent and soak it. After soaking for 5-10 minutes, wipe it with a cotton cloth to remove the oil, dust and other pollutants attached to the surface;

[0047] S1.2. After wiping, rinse the plastic film of the cleaning dog with deionized water to remove the residual detergent and impurities on the surface of the plastic film;

[0048] S1.3. Place the washed plastic film in a drying oven for drying. The temperature of the drying oven should be controlled at 60℃-80℃ and the drying time should be controlled at 8-15min.

[0049] S1.4. Activating the surface of the plastic film by plasma treatment can effectively improve the adhesion between the aluminum mold and the plastic film;

[0050] S1.5. Before aluminum plating, the treated plastic film should be fully inspected to ensure that its surface is clean, free of contaminants and damage;

[0051] S2. Preparation of vacuum chamber: Place the processed substrate into the vacuum chamber, close the vacuum chamber door, start the vacuum system, remove the air in the vacuum chamber, and make the vacuum degree reach the target value. The vacuum chamber preparation includes the following specific steps:

[0052] S2.1. Ensure that the vacuum chamber is clean, free of dirt and impurities, check the sealing performance of the vacuum chamber, and ensure that the door can be closed tightly and maintain vacuum;

[0053] S2.2. Carefully place the treated plastic film substrate on the fixture in the vacuum chamber, ensuring that the substrate is placed stably and will not be damaged or contaminated;

[0054] S2.3. Ensure that the door is tightly closed and the vacuum chamber is well sealed. Check whether the door seal is intact and replace it if necessary.

[0055] S2.4. Turn on the power of the vacuum system and start the vacuum pump. The vacuum pump will begin to extract the air in the vacuum chamber and gradually reduce the pressure in the chamber.

[0056] S2.5. Use a vacuum gauge to monitor the pressure changes in the vacuum chamber. As the vacuum pump runs, the vacuum degree will gradually increase.

[0057] S2.6. Determine the required target vacuum degree according to the specific process requirements and continue to operate the vacuum pump until the vacuum degree reaches or exceeds the target value;

[0058] S2.7. Once the target vacuum degree is reached, the vacuum state of the vacuum chamber needs to be maintained, the vacuum pump needs to be ensured to continue to operate, and the vacuum system needs to be checked for leaks. If leaks are found, they should be repaired in time.

[0059] S3. Target installation: Install the pure aluminum target on the magnetron sputtering target. After the pure aluminum target is installed, use a laser rangefinder to measure the distance between the target and the substrate surface, adjust the height of the substrate stage and the position of the target to make the distance reach an appropriate value, thereby ensuring that the distance between the target and the substrate surface is appropriate;

[0060] S4, introducing sputtering gas: introducing sputtering gas into the vacuum chamber, wherein the introduced sputtering gas is argon gas;

[0061] S5. Magnetron sputtering coating: Turn on the magnetron sputtering power supply to generate a magnetic field to ionize the argon gas to form plasma. Under the action of the magnetic field, the argon ions in the plasma will accelerate to hit the surface of the aluminum target and sputter out aluminum atoms. These aluminum atoms will be deposited on the substrate surface and form an aluminum film;

[0062] S6. Control of coating parameters: During the sputtering coating process, it is necessary to control the coating parameters such as sputtering power, sputtering time, sputtering gas flow rate, and working pressure. During the sputtering process, the vacuum chamber pressure and current and other parameters are continuously monitored. Due to different sputtering rates and uneven heat dissipation of the blocking material, the final aluminum coating may have uneven film thickness. This problem can be alleviated by adjusting the sputtering power, target-base distance, argon gas flow rate, and sputtering time, and the key point is to change the position of each sputtering point from time to time. In the sputtering process, the growth rate, thickness, flatness and other properties of the film are controlled by adjusting the sputtering parameters. After the sputtering is completed, the sputtering power is turned off and the introduction of the sputtering gas is stopped, which can effectively ensure the quality and performance of the aluminum coating.

[0063] S7, post-coating treatment: After the sputtering coating is completed, the aluminum-plated film needs to be annealed and surface treated, which can effectively improve the performance and adhesion of the aluminum-plated film. When the coating reaches the predetermined thickness and quality requirements, the sputtering process is stopped and the equipment is allowed to cool down naturally. After the temperature drops to a safe range, air is slowly introduced into the sputtering chamber to balance the internal and external pressures, and then the aluminum-plated substrate is carefully taken out for subsequent testing and analysis, which can effectively ensure the quality of the aluminum-plated substrate;

[0064] The annealing treatment of the aluminum-plated film includes the following specific steps:

[0065] S7.1.1. Place the aluminum-coated substrate into an annealing furnace, gradually increase the temperature of the annealing furnace to reach a preset annealing temperature, and maintain the preset annealing temperature for a certain period of time to ensure that the film layer completes the annealing process;

[0066] S7.1.2. As annealing continues, gradually lower the temperature of the annealing furnace, allow it to slowly cool to room temperature, and carefully take out the annealed substrate.

[0067] The surface treatment of aluminum film includes the following specific steps:

[0068] S7.2.1. Use appropriate solvents to remove contaminants from the substrate surface and rinse the substrate surface with deionized water to ensure cleanliness;

[0069] S7.2.2. Treat the substrate surface for flatness, improve the surface condition by polishing, and perform surface modification by plasma treatment, which can effectively improve the adhesion and performance of the film layer. After the treatment, clean and dry the substrate after surface treatment to remove any residual treatment agent or moisture;

[0070] S8. Finished product inspection: Conduct quality inspection on the prepared aluminum-plated film, including thickness measurement, adhesion test, surface roughness test, and optical performance test to ensure that the aluminum-plated film meets the requirements.

[0071] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.

Claims

1. A method for preparing a high-adhesion aluminum-plated film by magnetron sputtering, characterized in that: The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering comprises the following specific steps: S1. Substrate preparation: a plastic film is selected as the substrate, and the plastic film is cleaned and treated to remove pollutants and impurities on the surface; S2. Preparation of vacuum chamber: Place the processed substrate into the vacuum chamber, close the vacuum chamber door, start the vacuum system, remove the air in the vacuum chamber, and make the vacuum degree reach the target value; S3. Target installation: Install the pure aluminum target on the magnetron sputtering target and ensure that the distance between the target and the substrate surface is appropriate; S4, sputtering gas introduction: introducing sputtering gas into the vacuum chamber; S5. Magnetron sputtering coating: Turn on the magnetron sputtering power supply to generate a magnetic field to ionize the argon gas to form plasma. Under the action of the magnetic field, the argon ions in the plasma will accelerate to hit the surface of the aluminum target and sputter out aluminum atoms. These aluminum atoms will be deposited on the substrate surface and form an aluminum film; S6. Coating parameter control: During the sputtering coating process, it is necessary to control the coating parameters such as sputtering power, sputtering time, sputtering gas flow rate, and working pressure; S7, post-coating treatment: After the sputtering coating is completed, the aluminum film needs to be annealed and surface treated; S8. Finished product inspection: Conduct quality inspection on the prepared aluminum-plated film, including thickness measurement, adhesion test, surface roughness test, and optical performance test.

2. The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering according to claim 1, characterized in that: The preparation of the substrate in S1 comprises the following specific steps: S1.

1. Use a cleaning agent to clean the surface of the selected plastic film substrate. First, place the plastic film in the cleaning agent and soak it. After soaking for 5-10 minutes, wipe it with a cotton cloth to remove the oil, dust and other pollutants attached to the surface; S1.

2. After wiping, rinse the plastic film of the cleaning dog with deionized water to remove the residual detergent and impurities on the surface of the plastic film; S1.

3. Place the washed plastic film in a drying oven for drying. The temperature of the drying oven should be controlled at 60℃-80℃ and the drying time should be controlled at 8-15min. S1.

4. Activating the surface of the plastic film by plasma treatment can effectively improve the adhesion between the aluminum mold and the plastic film; S1.

5. Before aluminum plating, the treated plastic film should be thoroughly inspected to ensure that its surface is clean, free of contaminants and damage.

3. The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering according to claim 1, characterized in that: The sputtering gas introduced in S4 is argon gas.

4. The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering according to claim 1, characterized in that: The vacuum chamber preparation in S2 includes the following specific steps: S2.

1. Ensure that the vacuum chamber is clean, free of dirt and impurities, check the sealing performance of the vacuum chamber, and ensure that the door can be closed tightly and maintain vacuum; S2.

2. Carefully place the treated plastic film substrate on the fixture in the vacuum chamber, ensuring that the substrate is placed stably and will not be damaged or contaminated; S2.

3. Ensure that the door is tightly closed and the vacuum chamber is well sealed. Check whether the door seal is intact and replace it if necessary. S2.

4. Turn on the power of the vacuum system and start the vacuum pump. The vacuum pump will begin to extract the air in the vacuum chamber and gradually reduce the pressure in the chamber. S2.

5. Use a vacuum gauge to monitor the pressure changes in the vacuum chamber. As the vacuum pump runs, the vacuum degree will gradually increase. S2.

6. Determine the required target vacuum degree according to the specific process requirements and continue to operate the vacuum pump until the vacuum degree reaches or exceeds the target value; S2.

7. Once the target vacuum degree is reached, it is necessary to maintain the vacuum state of the vacuum chamber, ensure that the vacuum pump continues to operate, and check whether there is any leakage in the vacuum system. If any leakage is found, it should be repaired in time.

5. The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering according to claim 1, characterized in that: In the S6, during the sputtering process, parameters such as the vacuum chamber pressure and current are continuously monitored. Due to different sputtering rates and uneven heat dissipation of the blocking material, the final aluminum-plated film may have an uneven film thickness. This problem is alleviated by adjusting the sputtering power, target-base distance, argon gas flow rate and sputtering time, and the key point is to change the position of each sputtering point from time to time. During the sputtering process, the growth rate, thickness, flatness and other properties of the film are controlled by adjusting the sputtering parameters. After the sputtering is completed, the sputtering power is turned off and the introduction of the sputtering gas is stopped.

6. The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering according to claim 1, characterized in that: The annealing treatment of the aluminum-plated film in S7 includes the following specific steps: S7.1.

1. Place the aluminum-coated substrate into an annealing furnace, gradually increase the temperature of the annealing furnace to reach a preset annealing temperature, and maintain the preset annealing temperature for a certain period of time to ensure that the film layer completes the annealing process; S7.1.

2. As annealing continues, gradually lower the temperature of the annealing furnace, allow it to slowly cool to room temperature, and carefully take out the annealed substrate.

7. The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering according to claim 1, characterized in that: The surface treatment of the aluminum-plated film in S7 includes the following specific steps: S7.2.

1. Use appropriate solvents to remove contaminants from the substrate surface and rinse the substrate surface with deionized water to ensure cleanliness; S7.2.

2. The substrate is treated for surface flatness, polished to improve the surface condition, and treated with plasma to modify the surface. After the treatment, the treated substrate is cleaned and dried to remove any residual treatment agent or moisture.

8. The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering according to claim 1, characterized in that: After the pure aluminum target is installed in S3, a laser rangefinder is used to measure the distance between the target and the substrate surface, and the height of the substrate stage and the position of the target are adjusted to make the distance reach an appropriate value, thereby ensuring that the distance between the target and the substrate surface is appropriate.

9. The method for preparing a high-adhesion aluminum-plated film by magnetron sputtering according to claim 1, characterized in that: In S7, when the coating reaches the predetermined thickness and quality requirements, the sputtering process is stopped and the equipment is allowed to cool down naturally. After the temperature drops to a safe range, air is slowly introduced into the sputtering chamber to balance the internal and external pressures, and then the aluminum-plated substrate is carefully taken out for subsequent testing and analysis.

Citation Information

Cited By

  • Method suitable for preparing special metal rhodium coating

    CN119351946A

  • Ultraviolet radiation resistant ostrich hair moon dust brush and preparation method thereof

    CN119411087A

  • Control system for vacuum coating machine

    CN119710611A

  • Double-layer aluminized composite film based on magnetron sputtering aluminizing process and preparation and application of double-layer aluminized composite film

    CN120719265A

  • Double-layer aluminized composite film based on magnetron sputtering aluminizing process and preparation and application thereof

    CN120719265B