Polarizing plate

A polarizing plate with a (meth)acrylic resin film and adhesive layers, combined with a boron-containing polyvinyl alcohol resin, addresses warping and solvent resistance issues in high-temperature, high-humidity environments, ensuring structural integrity and performance.

JP2024146938APending Publication Date: 2024-10-15SUMITOMO CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024058924
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-04-01
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Polarizing plates made of acrylic resin film and cycloolefin resin film warp when stored in high-temperature, high-humidity environments and lack sufficient solvent resistance.

Method used

A polarizing plate comprising a (meth)acrylic resin film with specific mechanical properties, a first and second adhesive layer, and a protective film, where the (meth)acrylic resin film has a Martens hardness of 140N/mm², controlled moisture permeability, and is combined with a polyvinyl alcohol resin film containing a boron compound, enhancing solvent resistance and reducing warpage.

Benefits of technology

The solution provides a polarizing plate with improved solvent resistance and reduced warping in high-temperature, high-humidity conditions, maintaining structural integrity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146938000001_ABST
    Figure 2024146938000001_ABST
Patent Text Reader

Abstract

To provide a polarizing plate which is excellent in solvent resistance and can reduce warpage in a high temperature and high humidity environment.SOLUTION: A polarizing plate 100 includes a (meth)acrylic resin film 10, a first adhesive layer 12, a polarizer 20, a second adhesive layer 14, a protective film 30, and an adhesive layer 40 in this order. Martens hardness of the (meth)acrylic resin film 10 is 140 N / mm2 or more, and storage elastic modulus at 25°C and a measuring frequency of 1 Hz of the adhesive layer 40 is 1.5×105 Pa or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate. [Background technology]

[0002] A polarizing plate having a structure of an acrylic resin film / polarizer / cycloolefin resin film is known. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-200339 A [Patent Document 2] JP 2017-204007 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, this polarizing plate has problems such as warping when it is stored in a high-temperature and high-humidity environment in a state where it is attached to a substrate film such as a display panel, and problems such as insufficient solvent resistance.

[0005] An object of the present invention is to provide a polarizing plate which has excellent solvent resistance and is capable of reducing warping in a high-temperature and high-humidity environment. [Means for solving the problem]

[0006] [1] A polarizing plate comprising, in this order, a (meth)acrylic resin film, a first adhesive layer, a polarizer, a second adhesive layer, a protective film, and a pressure-sensitive adhesive layer, The (meth)acrylic resin film has a Martens hardness of 140 N / mm 2 That's all. The pressure-sensitive adhesive layer has a storage modulus of 1.5×10 at 25° C. and a measurement frequency of 1 Hz. 5 The polarizing plate has a temperature of 0.1 Pa or less.

[0007] [2] The (meth)acrylic resin film is The tensile modulus in the MD direction at 25°C is T MD (25℃), tensile modulus in MD direction at 80℃ is T MD (80℃), The tensile modulus in the TD direction at 25°C is T TD (25℃), tensile modulus in TD direction at 80℃ is T TD (80℃) T MD (25℃) / T MD (80°C) and T TD (25℃) / T TD (80° C.) is less than 2.0.

[0008] [3] The (meth)acrylic resin film is Storage modulus G' in the MD direction at 80℃ and a measurement frequency of 10Hz MD (80℃) and tensile modulus T in MD direction at 80℃ MD (80℃) G' MD (80℃) / T MD (80° C.) is less than 1.2.

[0009] [4] The (meth)acrylic resin film is Storage modulus in the MD direction at 80°C and a measurement frequency of 10 Hz is G' MD (80℃), storage modulus in the TD direction at 80℃ and a measurement frequency of 10Hz is G' TD (80℃), then G' MD (80℃) / G' TD The polarizing plate according to any one of [1] to [3], wherein (80° C.) is 1.05 or less.

[0010] [5] The (meth)acrylic resin film has a moisture permeability and thickness product of 2500 (g / m 2 The polarizing plate according to any one of [1] to [4], wherein the thickness of the polarizing plate is equal to or less than 24 hr·μm.

[0011] [6] The polarizing plate according to any one of [1] to [5], wherein the polarizer is a polyvinyl alcohol-based resin film, contains a boron compound, and has a boron content of 4.0 wt % or less.

[0012] [7] The polarizing plate according to any one of [1] to [6], wherein the first adhesive layer is a cured product of a (meth)acrylic adhesive.

[0013] [8] The polarizing plate according to any one of [1] to [7], wherein the protective film is a cyclic polyolefin resin film. Effect of the Invention

[0014] According to the present invention, there is provided a polarizing plate which has excellent solvent resistance and is capable of reducing warping in a high-temperature and high-humidity environment. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a schematic cross-sectional view of a polarizing plate according to one embodiment. [Diagram 2] FIG. 2 is a schematic diagram illustrating measurement points for the amount of warping in a wet heat warping test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] (Polarizing plate) As shown in FIG. 1, a polarizing plate 100 according to one embodiment of the present invention comprises, in this order, a (meth)acrylic resin film 10, a first adhesive layer 12, a polarizer 20, a second adhesive layer 14, a protective film 30, and a pressure-sensitive adhesive layer 40.

[0017] ((Meth)acrylic resin film 10) The (meth)acrylic resin film 10 is a film containing a (meth)acrylic resin, and functions as a protective film for the polarizer 20 .

[0018] The (meth)acrylic resin is a polymer having a (meth)acrylic acid ester, particularly an alkyl (meth)acrylate ester, as the main structural unit (50% by mass or more relative to the total structural units). This resin may be a homopolymer of a (meth)acrylic acid ester, a copolymer using two or more kinds of (meth)acrylic acid esters, or a copolymer of a (meth)acrylic acid ester and a monomer copolymerizable therewith. In this specification, (meth)acrylic acid means acrylic acid and / or methacrylic acid. Similarly, (meth)acrylic acid ester means acrylic acid ester and / or methacrylic acid ester.

[0019] Specific examples of (meth)acrylic acid esters include acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, hexyl acrylate, cyclohexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, decyl acrylate, and dodecyl acrylate; and methacrylic acid alkyl esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, decyl methacrylate, and dodecyl methacrylate.

[0020] These (meth)acrylic acid alkyl esters may have any substituent such as a hydroxyl group or a halogen atom at the alkyl portion. Examples of (meth)acrylic acid alkyl esters having such a substituent include 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 3-chloro-2-hydroxypropyl methacrylate, and glycidyl methacrylate.

[0021] Among these (meth)acrylic acid esters, methyl methacrylate is preferably used as the main raw material of the acrylic resin. That is, as will be specifically described later, a homopolymer of methyl methacrylate, a copolymer of methyl methacrylate as the main constituent monomer and other (meth)acrylic acid esters, a copolymer of methyl methacrylate as the main constituent monomer and other monomers than (meth)acrylic acid esters, or a copolymer of methyl methacrylate as the main constituent monomer and other (meth)acrylic acid esters and monomers than (meth)acrylic acid esters are suitable as the (meth)acrylic resin.

[0022] Examples of monomers copolymerizable with (meth)acrylic acid esters include α,β-ethylenically unsaturated carboxylic acid esters other than the above-mentioned (meth)acrylic acid esters, α,β-ethylenically unsaturated carboxylic acids, alkenyl aromatic compounds, conjugated dienes, non-conjugated dienes, vinyl cyanide, α,β-ethylenically unsaturated carboxylic acid amides, carboxylic acid unsaturated alcohol esters, and olefins.

[0023] Specific examples of α,β-ethylenically unsaturated carboxylic acid esters other than (meth)acrylic acid esters include dimethyl fumarate, diethyl fumarate, dimethyl maleate, diethyl maleate, dimethyl itaconate, monoethyl maleate, monobutyl fumarate, etc. The α,β-ethylenically unsaturated carboxylic acid may be any of a monocarboxylic acid, a polycarboxylic acid, and a polycarboxylic acid anhydride, and specific examples thereof include acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, maleic anhydride, and itaconic anhydride.

[0024] Specific examples of alkenyl aromatic compounds include styrene, α-methylstyrene, α-methyl-2-, -3- or -4-methylstyrene, vinyltoluene, and divinylbenzene.Specific examples of conjugated dienes include 1,3-butadiene, 2-methyl-1,3-butadiene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, and cyclopentadiene.Specific examples of non-conjugated dienes include 1,4-hexadiene, dicyclopentadiene, and ethylidenenorbornene.

[0025] Specific examples of vinyl cyanides include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, and α-ethylacrylonitrile. Specific examples of α,β-ethylenically unsaturated carboxylic acid amides include acrylamide, methacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, and N,N-dimethylacrylamide. Specific examples of carboxylic acid unsaturated alcohol esters include vinyl acetate. Specific examples of olefins include ethylene, propylene, butene, and pentene.

[0026] When a monomer other than a (meth)acrylic acid ester is copolymerized, only one type of monomer other than a (meth)acrylic acid ester may be copolymerized, or two or more types of monomers other than a (meth)acrylic acid ester may be copolymerized. When such a monomer other than a (meth)acrylic acid ester is copolymerized, the content of structural units derived from the monomer in the (meth)acrylic resin is preferably 50% by weight or less, more preferably 15% by weight or less, and even more preferably 10% by weight or less of the total structural units.

[0027] Specific examples of the (meth)acrylic resins preferred for use in the present invention include poly(methyl methacrylate), methyl methacrylate / methyl acrylate copolymers, methyl methacrylate / methyl acrylate / butyl acrylate / styrene copolymers, methyl methacrylate / styrene / butyl acrylate copolymers, and methyl methacrylate / ethylene copolymers. Among these, polymers in which structural units derived from methyl methacrylate account for 70% by weight or more, further 80% by weight or more, and particularly 90% by weight or more of the total structural units are preferred. The (meth)acrylic resins may be used alone or in combination of two or more types. The molecular weight of the (meth)acrylic resin is, for example, about 50,000 to 500,000 in terms of the weight average molecular weight in terms of polystyrene. If the weight average molecular weight is within this range, a homogeneous film is easily obtained when the film is formed by melt extrusion.

[0028] When the (meth)acrylic resin has a ring structure in its main chain, the heat resistance and hardness of the finally obtained (meth)acrylic resin film can be improved. When the (meth)acrylic resin has a ring structure in its main chain, the content of the ring structure in the resin can generally be in the range of 0.1 to 99 mass%, 1 to 95 mass%, 2 to 93 mass%, or 5 to 90 mass%, but it is preferable to set it in the range of 10 to 70 mass%, further 10 to 60 mass%, and especially 10 to 50 mass% in order to improve the heat resistance and hardness while maintaining the stretchability and handleability of the (meth)acrylic resin film at a suitable level. If the content of the ring structure is excessively large, the stretchability and handleability of the (meth)acrylic resin film will decrease.

[0029] Examples of the ring structure that the (meth)acrylic resin may have in the main chain include a glutarimide structure, a lactone ring structure, a succinic anhydride structure, and a succinimide structure.

[0030] The glutarimide structure is preferably represented by the following general formula (1):

[0031] [ka]

[0032] In the general formula (1), R 11 and R 12 each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 13 represents an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms. 11 and R 12 are each independently a hydrogen atom or a methyl group, and R 13 is hydrogen, a methyl group, a butyl group, or a cyclohexyl group. More preferably, R 11 is a methyl group, and R 12 is hydrogen, and R 13 is a methyl group. The acrylic resin may contain only a single glutarimide unit, and R 11 , R 12 and R 13 Acrylic resins having a glutarimide structure are described in, for example, JP-A-2006-309033, JP-A-2006-317560, JP-A-2006-328334, JP-A-2006-337491, JP-A-2006-337492, JP-A-2006-337493, and JP-A-2006-337569.

[0033] The glutarimide ring content in the (meth)acrylic resin can be from 0.1 to 20% by mass, and may be from 1 to 10% by mass.

[0034] (Meth)acrylic resins having a ring structure in the main chain are commercially available, and can also be produced by known methods.

[0035] The (meth)acrylic resin film may contain rubber particles in addition to the (meth)acrylic resin. Examples of rubber particles that may be contained include rubber polymers having acrylic acid esters as the main monomer, rubber polymers having butadiene as the main monomer, and ethylene-vinyl acetate copolymers. Among these, acrylic rubber particles, which are rubber polymers having acrylic acid esters as the main monomer, are preferred. Of course, acrylic rubber particles may be used in combination with other rubber particles.

[0036] The acrylic rubber particles may be those whose main constituent monomer is an acrylic acid alkyl ester having a large number of carbon atoms in the alkyl group, for example, about 4 to 8 carbon atoms, such as butyl acrylate or 2-ethylhexyl acrylate. Among these, an elastic polymer whose main constituent monomer is butyl acrylate is preferable. Although the rubber particles may have a single-layer structure made of an elastic polymer whose main constituent monomer is an acrylic acid alkyl ester, a multi-layer structure including a layer of the elastic polymer is also effective. A representative example of the latter is a rubber particle in which a layer of an acrylic elastic polymer, such as a grafted elastic polymer of an alkyl acrylate such as butyl acrylate and styrene, and a hard polymer layer whose main constituent monomer is methyl methacrylate form a layer in a core-shell structure. More specifically, there are those having a two-layer structure in which the above-mentioned hard polymer layer is formed on the outside of the acrylic elastic body, and those having a three-layer structure in which the above-mentioned hard polymer layer is formed on the inside of the acrylic elastic body and the above-mentioned hard polymer layer is also formed on the outside of the acrylic elastic body.

[0037] In particular, a suitable example is one that contains such multi-layered acrylic rubber particles. By containing multi-layered acrylic rubber particles, the tensile breaking strain value can be adjusted without lowering the Vicat softening point of the (meth)acrylic resin more than necessary, and breakage during film molding can be prevented without lowering heat resistance.

[0038] The rubber particles have a number average particle size of 1,000 nm or less, more preferably 100 to 1,000 nm, and particularly preferably 100 to 500 nm, when dispersed in the (meth)acrylic base resin. If the number average particle size of the rubber particles is large, the haze of the film becomes too large, resulting in a low light transmittance. On the other hand, if the number average particle size is too small, the flexibility of the film tends to decrease.

[0039] The average particle size of acrylic rubber particles containing acrylic elastomer is measured as follows. That is, when such rubber particles are mixed with an acrylic base resin to form a film, and the cross section is dyed with an aqueous solution of ruthenium oxide, only the layer of the acrylic elastomer is colored and observed as a nearly circular shape, and the acrylic resin of the parent layer is not dyed. Therefore, from the cross section of the film dyed in this way, a thin section is prepared using a microtome or the like, and this is observed under an electron microscope. Then, 100 dyed elastomer particles are randomly extracted, and the particle size of each is calculated, and the number average value is taken as the average particle size. Since it is measured by this method, the average particle size of the rubber particles specified here is the number average particle size.

[0040] When a rubber particle having an outermost layer made of a hard polymer mainly made of methyl methacrylate and an acrylic elastomer wrapped therein is used, the outermost layer of the rubber particle is mixed with the acrylic base resin when it is mixed with an acrylic base resin. Therefore, when the cross section is stained with ruthenium oxide and observed under an electron microscope, the rubber particle is observed as a particle without the outermost layer. Specifically, when a two-layer rubber particle having an inner layer made of an acrylic elastomer and an outer layer made of a hard polymer mainly made of methyl methacrylate is used, the acrylic elastomer part of the inner layer is stained and observed as a particle with a single layer structure, and when a three-layer rubber particle having an inner layer made of a hard polymer mainly made of methyl methacrylate, an acrylic elastomer part of the middle layer, and an outer layer made of a hard polymer mainly made of methyl methacrylate is used, the center part of the particle in the innermost layer is not stained, and only the acrylic elastomer part of the middle layer is stained and observed as a particle with a two-layer structure.

[0041] The amount of rubber particles added to the (meth)acrylic base resin is preferably 10 to 50% by weight, more preferably 10 to 40% by weight, based on the total amount of the (meth)acrylic resin composition containing the rubber particles. If the amount of rubber particles is too small, the film will not have sufficient slip properties or flexibility, and conversely, if the amount is too large, the film will not have sufficient heat resistance.

[0042] In the (meth)acrylic resin film, the amount of the (meth)acrylic resin may be 10 mass% or more, 20 mass% or more, 40 mass% or more, 50 mass% or more, 80 mass% or more, 90 mass% or more, or 100 mass% based on the total mass.

[0043] The (meth)acrylic resin film may contain an ultraviolet absorbing agent. The ultraviolet absorbing agent may be selected from those that are generally blended into resins. Examples of the ultraviolet absorbing agent include hydroxybenzophenone compounds, benzotriazole compounds, triazine compounds, and salicylic acid ester compounds.

[0044] The film can be produced by a known method, namely, by melt-kneading a thermoplastic composition containing a (meth)acrylic resin, extruding it through a T-die to form a film, and then cooling it.

[0045] The (meth)acrylic resin film may be a non-stretched film, a uniaxially stretched film, or a biaxially stretched film. The stretching ratio can be 1.5 to 3.5.

[0046] (Thickness) The thickness of the (meth)acrylic resin film is not particularly limited, but may be 15 μm or more, preferably 30 μm or more, and may be 65 μm or less, preferably 50 μm or less.

[0047] (Martens hardness) The Martens hardness of the (meth)acrylic resin film is 140N / mm 2 Above 145N / mm 2 or more, 150N / mm 2 or more, and 300N / mm 2 Less than 280N / mm 2 may be less than 250N / mm 2 may be less than 200N / mm 2 It may be the following: A film having a desired Martens hardness can be obtained by adjusting the type of (meth)acrylic resin constituting the (meth)acrylic resin film (the type of structural unit constituting the (meth)acrylic resin, and the blending ratio of the structural units when there are multiple structural units), the glass transition temperature, and the stereoregularity. For example, the Martens hardness tends to be increased by making the (meth)acrylic resin have a ring structure in its main chain and making the content of the ring structure in the resin 5% by mass or more, increasing the glass transition temperature of the (meth)acrylic resin, and increasing the stereoregularity (syndiotacticity in triplet notation) of the (meth)acrylic resin. In addition, when multiple (meth)acrylic resins are contained, a film having a desired Martens hardness can be obtained by adjusting the blending ratio of the resin. Furthermore, the Martens hardness can be adjusted by the type and amount of additives contained in the (meth)acrylic resin film. For example, when the additive is rubber particles, the Martens hardness tends to be increased by reducing the blending amount of the additive.

[0048] (Product of moisture permeability and thickness) (Meth)acrylic resin film has a moisture permeability and thickness product of 2500 (g / m 2 ·24hr·μm) or less, and 2400 (g / m 2 ·24hr·μm) or less, and 1800 (g / m 2 ·24hr·μm) or more, and 2000 (g / m 2 ·24hr·μm) or more.

[0049] The (meth)acrylic resin film has a tensile modulus in the MD direction at 25°C of T MD (25℃), tensile modulus in MD direction at 80℃ is T MD (80℃), tensile modulus in TD direction at 25℃ is T TD (25℃), T at 80℃ TD The tensile modulus in the T direction is TD (80℃), T MD (25℃) / T MD (80°C) and T TD (25℃) / T TD (80°C) is preferably less than 2.0, may be less than 1.9, may be less than 1.85, or may be 1.5 or more. When this ratio is low, the hardness of the (meth)acrylic resin film is maintained at high temperatures, which contributes to reducing wet heat warping.

[0050] The (meth)acrylic resin film has a storage modulus G' in the MD direction at 80°C and a measurement frequency of 10 Hz. MD (80℃) and tensile modulus T in MD direction at 80℃ MD (80℃) G' MD (80℃) / T MD (80° C.) is preferably less than 1.2, may be less than 1.1, and may be 0.7 or more. If this ratio is low, there is an effect of reducing wet heat warping.

[0051] The (meth)acrylic resin film has a storage modulus in the MD direction at 80°C and a measurement frequency of 10 Hz, G' MD (80℃), storage modulus in the TD direction at 80℃ and a measurement frequency of 10Hz is G' TD (80℃), then G' MD (80℃) / G' TD (80°C) is preferably 1.05 or less, may be 1.00 or less, or may be 0.7 or more. If this ratio is low, there is an effect of reducing wet heat warping.

[0052] The MD direction of the (meth)acrylic resin film is the machine flow direction from the die in film molding, and the TD direction is the width direction perpendicular to the machine flow direction from the die in film molding.

[0053] The relationship between the MD direction of the (meth)acrylic resin film 10 and the absorption axis direction of the polarizer 20 is not particularly limited, but it is preferable that they are parallel to each other.

[0054] (Polarizer) In the present invention, the polarizer is a uniaxially stretched polyvinyl alcohol resin film on which a dichroic pigment (iodine or a dichroic dye) is adsorbed and aligned, and crosslinked with a boron compound such as boric acid or borax.

[0055] The boron content in the polarizer may be 5.0 mass% or less, 4.2 mass% or less, and preferably 4.0 mass% or less. The boron content in the polarizer may be 0.5 mass% or more, 1.0 mass% or more, or 1.5 mass% or more, and preferably 2.0 mass% or more. The boron content (mass %) of the polarizer can be calculated from the amount of sodium hydroxide solution (1 mol / L) added dropwise to a measurement sample solution prepared by dissolving 0.2 g of the polarizer in 200 g of a 1.9 wt % aqueous mannitol solution, and then dropping the solution until it reaches its neutralization point.

[0056] The polyvinyl alcohol resin constituting the polyvinyl alcohol resin film may be, for example, a saponified polyvinyl acetate resin. Examples of the polyvinyl acetate resin include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate and other monomers copolymerizable therewith.

[0057] Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth)acrylamides having an ammonium group.

[0058] The degree of saponification of the polyvinyl alcohol resin is usually about 85 mol % or more, preferably about 90 mol % or more, and more preferably about 99 mol % or more.

[0059] The polyvinyl alcohol resin may be modified. For example, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc., which are modified with aldehydes may also be used.

[0060] The average degree of polymerization of the polyvinyl alcohol resin is preferably 100 or more and 10,000 or less, more preferably 1,500 or more and 8,000 or less, and even more preferably 2,000 or more and 5,000 or less. The average degree of polymerization of the polyvinyl alcohol resin can be determined in accordance with JIS K 6726 (1994). When the average degree of polymerization is within the above range, the polarizing performance and film processability tend to be excellent.

[0061] A polarizer can be manufactured by a process of contacting a raw material polyvinyl alcohol-based resin film (raw film) with a treatment liquid (hereinafter also referred to as a "treatment process"). The method of contacting with the treatment liquid may be a method of immersing the film in a treatment liquid (hereinafter also referred to as a "treatment bath") contained in a treatment tank, or a method of treating the film by attaching the treatment liquid to the film surface by spraying, flowing, dropping, or the like. When the treatment process is performed by a method of immersing the film in a treatment bath, the treatment bath for one treatment process is not limited to one, and one treatment process may be completed by sequentially immersing the film in two or more treatment baths.

[0062] Examples of the treatment liquid include a swelling liquid, a dyeing liquid, a crosslinking liquid, and a cleaning liquid. Examples of the treatment process include a swelling process in which a swelling liquid is brought into contact with the raw film to perform a swelling process, a dyeing process in which a dyeing liquid is brought into contact with the film after the swelling process to perform a dyeing process, a crosslinking process in which a crosslinking liquid is brought into contact with the film after the dyeing process to perform a crosslinking process, and a cleaning process in which a cleaning liquid is brought into contact with the film after the crosslinking process to perform a cleaning process. In addition, between these series of treatment processes (i.e., before and after any one or more treatment processes and / or during any one or more treatment processes), a uniaxial stretching process is performed in a wet or dry manner. Other treatment processes may be added as necessary.

[0063] The swelling step is carried out for the purposes of removing foreign matter from the surface of the raw film, removing plasticizers in the raw film, imparting ease of dyeing, plasticizing the raw film, etc. As the swelling liquid, a medium mainly composed of water, such as water, distilled water, or pure water, is usually used.

[0064] The crosslinking step is a treatment carried out for the purpose of water resistance and color adjustment by crosslinking. As the crosslinking liquid, a solution in which a crosslinking agent is dissolved in a solvent can be used. Examples of the crosslinking agent include boron compounds such as boric acid and borax. These may be used alone or in combination of two or more. As the solvent, for example, water can be used, but an organic solvent compatible with water may also be included. The concentration of the crosslinking agent in the crosslinking liquid, the temperature of the crosslinking bath, the immersion time of the film, and the number of crosslinking baths in which the film is immersed are not particularly limited, and by appropriately selecting these, a polarizing film having a boron content of 5.0 mass% or less can be obtained. When the dichroic dye used in the dyeing process is iodine, the crosslinking liquid preferably contains an iodide in addition to boric acid, and the amount of iodide can be, for example, 1 to 30 parts by weight per 100 parts by weight of water. Examples of the iodide include potassium iodide and zinc iodide. In addition, compounds other than iodides, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, sodium sulfate, etc., may be present. The crosslinking treatment may be carried out multiple times, usually 2 to 5 times. In this case, the composition and temperature of each crosslinking bath used may be the same or different.

[0065] The cleaning step is carried out for the purpose of removing excess agents such as boric acid and iodine attached to the polyvinyl alcohol-based resin film. The cleaning step is carried out, for example, by immersing the crosslinked polyvinyl alcohol-based resin film in a cleaning bath containing a cleaning liquid. The cleaning step can also be carried out by spraying the cleaning liquid as a shower onto the film, instead of immersing the film in the cleaning bath, or by combining immersion in the cleaning bath and spraying the cleaning liquid. The boron content of the finally obtained polarizer can be adjusted by adjusting the cleaning treatment conditions (for example, the time of contact with the cleaning liquid and the temperature of the cleaning liquid).

[0066] As described above, the raw film is uniaxially stretched in a wet or dry manner during the series of processing steps (i.e., before or after any one or more processing steps and / or during any one or more processing steps). The uniaxial stretching step can be carried out multiple times from the raw film to the production of a polarizer.

[0067] The thickness of the polarizer is usually 65 μm or less, preferably 50 μm or less, more preferably 35 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The thickness of the polarizer is usually 2 μm or more, preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thickness of the polarizer can be controlled, for example, by selecting a polyvinyl alcohol-based resin film, adjusting the stretching ratio, etc.

[0068] (First adhesive layer and second adhesive layer) The first adhesive layer 12 bonds the (meth)acrylic resin film 10 and the polarizer 20, and the second adhesive layer 14 bonds the protective film 30 and the polarizer 20. The first adhesive layer 12 and the second adhesive layer 14 are preferably a cured product of a curable adhesive containing a curable (polymerizable) compound. The curable compound is preferably an active energy ray-curable adhesive that is cured by heating or by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays. The polymerizable compound refers to a compound or oligomer that undergoes a polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, or X-rays, or when heated.

[0069] Examples of the curable adhesive include epoxy adhesives and (meth)acrylic adhesives. The first adhesive layer and the second adhesive layer may be made of the same cured adhesive or may be made of different cured adhesives.

[0070] (Epoxy adhesive) The epoxy adhesive contains an epoxy compound as a polymerizable compound. An epoxy compound is a compound having one or more, preferably two or more, epoxy groups in a molecule. The epoxy compound may be used alone or in combination of two or more. The epoxy adhesive may further contain an oxetane compound, a vinyl compound, or the like as a polymerizable compound.

[0071] Examples of the epoxy compound include alicyclic epoxy compounds, aromatic epoxy compounds, hydrogenated epoxy compounds, aliphatic epoxy compounds, etc. Among them, from the viewpoints of weather resistance, curing speed, and adhesiveness, the epoxy compound preferably contains an alicyclic epoxy compound or an aliphatic epoxy compound, and more preferably contains an alicyclic epoxy compound.

[0072] An alicyclic epoxy compound is a compound having one or more epoxy groups bonded to an alicyclic ring in the molecule. The "epoxy group bonded to an alicyclic ring" means a bridging oxygen atom -O- in the structure shown in the following formula (2). In the following formula (2), m is an integer of 2 to 5.

[0073] [ka]

[0074] (CH2) in the above formula (2) mCompounds in which one or more hydrogen atoms have been removed and the resulting group is bonded to another chemical structure can be called alicyclic epoxy compounds. (CH2) m One or more hydrogen atoms therein may be appropriately substituted with a straight-chain alkyl group such as a methyl group or an ethyl group.

[0075] Among them, alicyclic epoxy compounds having an epoxycyclopentane structure (where m=3 in the above formula (2)) or an epoxycyclohexane structure (where m=4 in the above formula (2)) have a high glass transition temperature of the cured product and are also advantageous in terms of adhesion between the polarizing film and the protective film. Specific examples of alicyclic epoxy compounds are listed below. Here, the compound names are listed first, followed by the corresponding chemical formulas, and the compound names and the corresponding chemical formulas are given the same symbols.

[0076] A: 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, B: 3,4-epoxy-6-methylcyclohexyl methyl 3,4-epoxy-6-methylcyclohexane carboxylate, C: ethylene bis(3,4-epoxycyclohexane carboxylate), D: bis(3,4-epoxycyclohexylmethyl)adipate, E: bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, F: diethylene glycol bis(3,4-epoxycyclohexyl methyl ether), G: ethylene glycol bis(3,4-epoxycyclohexyl methyl ether), H: 2,3,14,15-diepoxy-7,11,18,21-tetraoxatrispiro[5.2.2.5.2.2]henicosane, I: 3-(3,4-epoxycyclohexyl)-8,9-epoxy-1,5-dioxaspiro[5.5]undecane, J: 4-vinylcyclohexene dioxide, K: Limonene dioxide, L: bis(2,3-epoxycyclopentyl) ether, M: Dicyclopentadiene dioxide.

[0077] [ka]

[0078] [ka]

[0079] The aromatic epoxy compound is a compound having an aromatic ring and an epoxy group in the molecule. Specific examples thereof include bisphenol type epoxy compounds or oligomers thereof, such as diglycidyl ether of bisphenol A, diglycidyl ether of bisphenol F, and diglycidyl ether of bisphenol S; novolac type epoxy resins, such as phenol novolac epoxy resin, cresol novolac epoxy resin, and hydroxybenzaldehyde phenol novolac epoxy resin; polyfunctional epoxy compounds, such as glycidyl ether of 2,2',4,4'-tetrahydroxydiphenylmethane and glycidyl ether of 2,2',4,4'-tetrahydroxybenzophenone; and polyfunctional epoxy resins, such as epoxidized polyvinylphenol.

[0080] The hydrogenated epoxy compound is a glycidyl ether of a polyol having an alicyclic ring, and can be a glycidyl ether of a nuclear hydrogenated polyhydroxy compound obtained by selectively hydrogenating an aromatic ring of an aromatic polyol under pressure in the presence of a catalyst. Specific examples of aromatic polyols include bisphenol type compounds such as bisphenol A, bisphenol F, and bisphenol S; novolac type resins such as phenol novolac resin, cresol novolac resin, and hydroxybenzaldehyde phenol novolac resin; and polyfunctional compounds such as tetrahydroxydiphenylmethane, tetrahydroxybenzophenone, and polyvinylphenol. The glycidyl ether can be obtained by reacting epichlorohydrin with an alicyclic polyol obtained by hydrogenating the aromatic ring of an aromatic polyol. Among the hydrogenated epoxy compounds, a preferred one is a hydrogenated diglycidyl ether of bisphenol A.

[0081] Aliphatic epoxy compounds are compounds having at least one oxirane ring (three-membered cyclic ether) bonded to an aliphatic carbon atom in the molecule. For example, monofunctional epoxy compounds such as butyl glycidyl ether and 2-ethylhexyl glycidyl ether; bifunctional epoxy compounds such as 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and neopentyl glycol diglycidyl ether; trifunctional or higher epoxy compounds such as trimethylolpropane triglycidyl ether and pentaerythritol tetraglycidyl ether; and epoxy compounds having one epoxy group directly bonded to an alicyclic ring and an oxirane ring bonded to an aliphatic carbon atom, such as 4-vinylcyclohexene dioxide and limonene dioxide. Among them, from the viewpoint of adhesion between the polarizing film and the protective film, bifunctional epoxy compounds (also called aliphatic diepoxy compounds) having two oxirane rings bonded to an aliphatic carbon atom in the molecule are preferred. Such a suitable aliphatic diepoxy compound can be represented, for example, by the following formula (3).

[0082] [ka]

[0083] In the above formula (3), Y is an alkylene group having 2 to 9 carbon atoms, an alkylene group having a total of 4 to 9 carbon atoms and an ether bond therebetween, or a divalent hydrocarbon group having 6 to 18 carbon atoms and an alicyclic structure.

[0084] The aliphatic diepoxy compound represented by the above formula (3) is specifically a diglycidyl ether of an alkanediol, a diglycidyl ether of an oligoalkylene glycol having a repeat number of up to about 4, or a diglycidyl ether of an alicyclic diol.

[0085] Specific examples of diols (glycols) capable of forming the aliphatic diepoxy compound represented by the above formula (3) are given below. Alkanediols include ethylene glycol, propylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 3-methyl-2,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-2,4-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 3,5-heptanediol, 1,8-octanediol, 2-methyl-1,8-octanediol, and 1,9-nonanediol. Examples of the oligoalkylene glycol include diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, etc. Examples of the alicyclic diol include cyclohexanediol, cyclohexanedimethanol, etc.

[0086] An oxetane compound, which is one of the cationic polymerizable compounds, is a compound containing one or more oxetane rings (oxetanyl groups) in the molecule, and specific examples thereof include 3-ethyl-3-hydroxymethyloxetane (also called oxetane alcohol), 2-ethylhexyloxetane, 1,4-bis[{(3-ethyloxetane-3-yl)methoxy}methyl]benzene (also called xylylene bisoxetane), 3-ethyl-3[{(3-ethyloxetane-3-yl)methoxy}methyl]oxetane, 3-ethyl-3-(phenoxymethyl)oxetane, and 3-(cyclohexyloxy)methyl-3-ethyloxetane. The oxetane compound may be used as the main component of the cationic polymerizable compound, or may be used in combination with an epoxy compound. By using an oxetane compound in combination, the curing speed and adhesiveness may be improved.

[0087] Examples of vinyl compounds that can be cationic polymerizable compounds include aliphatic or alicyclic vinyl ether compounds. Specific examples thereof include vinyl ethers of alkyl or alkenyl alcohols having 5 to 20 carbon atoms, such as n-amyl vinyl ether, i-amyl vinyl ether, n-hexyl vinyl ether, n-octyl vinyl ether, 2-ethylhexyl vinyl ether, n-dodecyl vinyl ether, stearyl vinyl ether, and oleyl vinyl ether; hydroxyl group-containing vinyl ethers, such as 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, and 4-hydroxybutyl vinyl ether; vinyl ethers of monoalcohols having an aliphatic ring or an aromatic ring, such as cyclohexyl vinyl ether, 2-methylcyclohexyl vinyl ether, cyclohexylmethyl vinyl ether, and benzyl vinyl ether; glycerol monovinyl ether, 1,4-butanediol monovinyl ether, 1,4-butanediol monovinyl ether, and 1,4-butanediol monovinyl ether. Mono- to polyvinyl ethers of polyhydric alcohols such as hexanediol divinyl ether, 1,6-hexanediol divinyl ether, neopentyl glycol divinyl ether, pentaerythritol divinyl ether, pentaerythritol tetravinyl ether, trimethylolpropane divinyl ether, trimethylolpropane trivinyl ether, 1,4-dihydroxycyclohexane monovinyl ether, 1,4-dihydroxymethylcyclohexane monovinyl ether, and 1,4-dihydroxymethylcyclohexane divinyl ether; polyalkylene glycol mono- to divinyl ethers such as diethylene glycol divinyl ether, triethylene glycol divinyl ether, and diethylene glycol monobutyl monovinyl ether; and other vinyl ethers such as glycidyl vinyl ether and ethylene glycol vinyl ether methacrylate. The vinyl compound may be used as the main component of the cationic polymerizable compound, or may be used in combination with an epoxy compound, or an epoxy compound and an oxetane compound. By using a vinyl compound in combination, the curing speed and the viscosity of the adhesive may be improved.

[0088] The cationically polymerizable adhesive may further contain other curable compounds other than those mentioned above. Specific examples of the other curable compounds include other cationically polymerizable compounds other than those mentioned above, such as lactone compounds, cyclic acetal compounds, cyclic thioether compounds, and spiro orthoester compounds.

[0089] In the epoxy-based adhesive, from the viewpoint of suppressing outflow of dichroic dyes such as iodine from the polarizer 20, when the total amount of curable compounds contained in the adhesive is taken as 100 mass %, the content of all polymerizable compounds is preferably 80 weight % or more, more preferably 90 weight % or more, and even more preferably 100 weight %.

[0090] The epoxy adhesive may be active energy ray curable or heat curable, but is preferably active energy ray curable. When the adhesive is given active energy ray curability, it is preferable to blend a photocationic polymerization initiator into the adhesive. The photocationic polymerization initiator generates cationic species or Lewis acid by irradiation with active energy rays such as visible light, ultraviolet light, X-rays, or electron beams, and initiates the polymerization reaction of the cationic curable compound. The photocationic polymerization initiator acts catalytically with light, so that it has excellent storage stability and workability even when mixed with the photocationic curable compound. Examples of compounds that generate cationic species or Lewis acids by irradiation with active energy rays include onium salts such as aromatic iodonium salts and aromatic sulfonium salts, aromatic diazonium salts, and iron-arene complexes. The photocationic polymerization initiator may be used alone or in combination of two or more. Among them, aromatic sulfonium salts are preferably used because they have ultraviolet absorbing properties even in the wavelength region around 300 nm, and therefore can provide a cured product with excellent curability, mechanical strength, and adhesive strength.

[0091] The amount of the cationic photopolymerization initiator is usually 0.5 to 10 parts by weight, preferably 6 parts by weight or less, based on 100 parts by weight of the cationic polymerizable compound. By adding 0.5 parts by weight or more of the cationic photopolymerization initiator, the cationic polymerizable compound can be sufficiently cured, and the obtained optical laminate can be given high mechanical strength and adhesive strength. On the other hand, if the amount is excessively large, the ionic substance in the cured product increases, which increases the hygroscopicity of the cured product, and the durability of the polarizer may decrease.

[0092] ((Meth)acrylic adhesive) The (meth)acrylic adhesive contains a (meth)acrylate compound as a polymerizable compound.

[0093] ((Meth)acrylate Compounds) The (meth)acrylate compound is a radically polymerizable compound having one or more (meth)acryloyloxy groups in the molecule. The adhesive composition may contain one or more (meth)acrylate compounds.

[0094] Examples of the (meth)acrylate compound include a monofunctional (meth)acrylate compound having one (meth)acryloyloxy group in the molecule, a bifunctional (meth)acrylate compound having two (meth)acryloyloxy groups in the molecule, and a polyfunctional (meth)acrylate compound having three or more (meth)acryloyloxy groups in the molecule. The (meth)acrylate compound may contain one or more of each of the monofunctional (meth)acrylate compound, the bifunctional (meth)acrylate compound, and the polyfunctional (meth)acrylate compound.

[0095] An example of a monofunctional (meth)acrylate compound is an alkyl (meth)acrylate. Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isostearyl (meth)acrylate, and stearyl acrylate.

[0096] Other examples of the monofunctional (meth)acrylate compound include aromatic (meth)acrylate compounds in which the group bonded to -O- of the ester bond (-C(=O)-O-) contains an aromatic ring, such as aralkyl (meth)acrylates such as benzyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and ethoxylated-o-phenylphenol (meth)acrylate; alicyclic alkyl (meth)acrylate compounds in which the group bonded to -O- of the ester bond (-C(=O)-O-) contains an alicyclic ring, such as cyclohexyl (meth)acrylate, cyclohexylmethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, and isobornyl (meth)acrylate; Aminoalkyl (meth)acrylate compounds such as N,N-dimethylaminoethyl (meth)acrylate; Examples of the (meth)acrylate compounds in which the group bonded to -O- of the ester bond (-C(=O)-O-) contains an ether bond include those other than the above, such as dicyclopentenyloxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate.

[0097] Further examples of the monofunctional (meth)acrylate compound include (meth)acrylate compounds in which the group bonded to -O- of the ester bond (-C(=O)-O-) contains a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2- or 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, trimethylolpropane mono(meth)acrylate, and pentaerythritol mono(meth)acrylate; Examples of such (meth)acrylate compounds include those in which the group bonded to -O- of the ester bond (-C(=O)-O-) contains a carboxyl group, such as 2-carboxyethyl (meth)acrylate, ω-carboxy-polycaprolactone (n≒2) mono(meth)acrylate, 1-[2-(meth)acryloyloxyethyl]phthalic acid, 1-[2-(meth)acryloyloxyethyl]hexahydrophthalic acid, 1-[2-(meth)acryloyloxyethyl]succinic acid, 4-[2-(meth)acryloyloxyethyl]trimellitic acid, and N-(meth)acryloyloxy-N',N'-dicarboxymethyl-p-phenylenediamine.

[0098] Examples of bifunctional (meth)acrylate compounds include alkylene glycol di(meth)acrylates, polyoxyalkylene glycol di(meth)acrylates, halogen-substituted alkylene glycol di(meth)acrylates, di(meth)acrylates of aliphatic polyols, di(meth)acrylates of hydrogenated dicyclopentadiene or tricyclodecane dialkanol, di(meth)acrylates of dioxane glycol or dioxane dialkanol, di(meth)acrylates of alkylene oxide adducts of bisphenol A or bisphenol F, and epoxy di(meth)acrylates of bisphenol A or bisphenol F.

[0099] More specific examples of the bifunctional (meth)acrylate compound include ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol di(meth)acrylate, ditrimethylolpropane di(meth)acrylate, and ethylene glycol di(meth)acrylate. Polyethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, silicone di(meth)acrylate, di(meth)acrylate of hydroxypivalic acid neopentyl glycol ester Meth)acrylate, 2,2-bis[4-(meth)acryloyloxyethoxyethoxyphenyl]propane, 2,2-bis[4-(meth)acryloyloxyethoxyethoxycyclohexyl]propane, hydrogenated dicyclopentadienyl di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 1,3-dioxane-2,5-diyl di(meth)acrylate [also known as dioxane glycol di(meth)acrylate], hydroxypivalaldehyde and trimethylolpropane These include di(meth)acrylate of acetal compound with bisphenol A [chemical name: 2-(2-hydroxy-1,1-dimethylethyl)-5-ethyl-5-hydroxymethyl-1,3-dioxane], tris(hydroxyethyl)isocyanurate di(meth)acrylate, di(meth)acrylate of ethoxylated bisphenol A, di(meth)acrylate of propoxylated bisphenol A, di(meth)acrylate of ethoxylated bisphenol F, and di(meth)acrylate of propoxylated bisphenol F.

[0100] The bifunctional (meth)acrylate preferably has at least one alicyclic skeleton or at least one aromatic ring in the molecule, and more preferably has at least one aromatic ring.

[0101] From the viewpoints of moisture permeability of the cured product, compatibility with the maleic anhydride-modified compound described below, and adhesion to resin films (particularly (meth)acrylic resin films), it is preferable that the bifunctional (meth)acrylate contains a compound represented by the following formula (4):

[0102] [ka]

[0103] (In the formula, R 1 and R 2 each independently represents a hydrogen atom or a methyl group, X represents ethylene oxide (-C2H4O-) or propylene oxide (-C3H6O-), n represents an integer of 1 to 20, and m represents an integer of 1 to 20. X is preferably ethylene oxide, and the average of the sum of m and n is preferably 2-20, more preferably 3-15, and particularly preferably 4-13.

[0104] Examples of polyfunctional (meth)acrylate compounds having three or more (meth)acryloyloxy groups in the molecule include poly(meth)acrylates of trifunctional or higher aliphatic polyols, such as glycerin tri(meth)acrylate, alkoxylated glycerin tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; Poly(meth)acrylates of halogen-substituted polyols having three or more functional groups; Tri(meth)acrylate of alkylene oxide adduct of glycerin; Tri(meth)acrylate of alkylene oxide adduct of trimethylolpropane; 1,1,1-tris[(meth)acryloyloxyethoxyethoxy]propane; Examples thereof include tris(hydroxyethyl)isocyanurate tri(meth)acrylate.

[0105] From the viewpoint of reducing the viscosity of the acrylic adhesive and the adhesive ability of the acrylic adhesive to the polarizer 20 and the films 10 and 30, the (meth)acrylate compound preferably contains a monofunctional (meth)acrylate compound.

[0106] From the viewpoint of reducing the viscosity of the acrylic adhesive and the adhesive ability to the polarizer 20 and the films 10 and 30, the monofunctional (meth)acrylate compound preferably contains at least one compound selected from the group consisting of alicyclic alkyl (meth)acrylate compounds and aromatic (meth)acrylate compounds. Among them, from the viewpoint of reducing the moisture permeability of a cured film formed from the acrylic adhesive (hereinafter sometimes referred to as low moisture permeability), alicyclic alkyl (meth)acrylate compounds are more preferable.

[0107] When the total amount of the (meth)acrylic adhesive is taken as 100% by mass, the content of the (meth)acrylate compound is typically 15% by mass or more and 75% by mass or less, and from the viewpoint of the adhesive ability to the polarizer 20 and the films 10, 30, it is preferably 15% by mass or more and 70% by mass or less, more preferably 20% by mass or more and 60% by mass or less, and even more preferably 30% by mass or more and 55% by mass or less.

[0108] When the total amount of the (meth)acrylate compounds is 100 mass%, the content of the monofunctional (meth)acrylate compounds is usually 60 mass% or more, and from the viewpoint of adhesion ability to the polarizer 20 and the films 10 and 30, it is preferably 70 mass% or more, and more preferably 80 mass% or more.

[0109] When the total amount of the (meth)acrylate compounds is taken as 100% by mass, the content of the monofunctional (meth)acrylate compounds may be 100% by mass, but from the viewpoint of the mechanical strength of the cured product of the (meth)acrylic adhesive and ultimately the mechanical strength of a polarizing plate produced using the adhesive, it is preferably 99% by mass or less, more preferably 98% by mass or less, and may be 90% by mass or less.

[0110] When the content of the monofunctional (meth)acrylate compound is less than 100 mass%, the remainder of the (meth)acrylate compound is a difunctional (meth)acrylate compound and / or a polyfunctional (meth)acrylate compound, and preferably contains a difunctional (meth)acrylate compound.

[0111] When the total amount of the (meth)acrylate compounds is 100 mass%, the content of the bifunctional (meth)acrylate compounds is preferably 0.5 mass% or more, more preferably 1 mass% or more, and is preferably 10 mass% or less, and more preferably 5 mass% or less.

[0112] (Maleic anhydride modified compounds) It is preferable that the (meth)acrylic adhesive further contains a maleic anhydride modified compound. The maleic anhydride modified compound is a compound containing a maleic anhydride structure in the molecule. The (meth)acrylic adhesive may contain one type of maleic anhydride modified compound, or may contain two or more types of maleic anhydride modified compounds. Examples of the maleic anhydride modified compound include maleic anhydride modified polymers.

[0113] The maleic anhydride modified polymer is a polymer modified by introducing a maleic anhydride structure as a side chain of the polymer. The adhesive composition may contain one type of maleic anhydride modified polymer or may contain two or more types of maleic anhydride modified polymers.

[0114] The maleic anhydride structure refers to a structure of the following formula (5).

[0115] [ka] (* represents a bond to the main chain.)

[0116] In the maleic anhydride modified polymer, examples of the polymer modified with maleic anhydride include diene polymers, polyolefin polymers, (meth)acrylic polymers, polyester polymers, polystyrene polymers, polyether polymers, etc. These polymers may be homopolymers composed of one type of monomer, or copolymers composed of two or more types of monomers.

[0117] In this specification, "(meth)acrylic" refers to at least one selected from the group consisting of acrylic and methacrylic. The same applies to the expressions "(meth)acryloyl" and "(meth)acrylate".

[0118] The maleic anhydride modified polymer is preferably in a liquid state, since it is possible to prepare a solvent-free adhesive composition having good adhesive ability. The term "liquid state" means that the polymer exhibits flowability at a temperature of 25°C.

[0119] From the viewpoint of obtaining an adhesive composition with good coatability, the viscosity of the liquid maleic anhydride modified polymer at 25°C is preferably from 10 Pa·sec to 10,000 Pa·sec, more preferably from 15 Pa·sec to 7,000 Pa·sec, even more preferably from 15 Pa·sec to 300 Pa·sec, and particularly preferably from 15 Pa·sec to 100 Pa·sec.

[0120] A preferred example of the liquid maleic anhydride modified polymer is, for example, maleic anhydride modified polybutadiene. Each of these polymers may be a homopolymer or a copolymer, and is preferably a homopolymer.

[0121] The number average molecular weight of the maleic anhydride modified polymer is usually 500 or more and 15,000 or less, and from the viewpoints of viscosity and coatability, it is preferably 600 or more and 12,000 or less, more preferably 700 or more and 10,000 or less, even more preferably 2,000 or more and 10,000 or less, and particularly preferably 3,500 or more and 10,000 or less.

[0122] The number average molecular weight of the maleic anhydride modified polymer can be measured as a value converted into standard polystyrene by gel permeation chromatography (GPC).

[0123] The acid value of the maleic anhydride modified polymer is usually 10 KOHmg / g or more and 200 KOHmg / g or less, and from the viewpoint of the adhesive ability of the adhesive composition to the protective film, it is preferably 15 KOHmg / g or more and 150 KOHmg / g or less, more preferably 20 KOHmg / g or more and 100 KOHmg / g or less, even more preferably 30 KOHmg / g or more and 100 KOHmg / g or less, and particularly preferably 45 KOHmg / g or more and 100 KOHmg / g or less. The use of a maleic anhydride modified polymer having an acid value in this range is advantageous in terms of increasing the adhesive ability of the adhesive composition to the protective film, and is particularly advantageous in terms of providing an adhesive composition having high adhesion between a polyvinyl alcohol polarizer and a thermoplastic resin film when a polyvinyl alcohol polarizer is used as the polarizer.

[0124] The acid value of the maleic anhydride modified polymer is measured by neutralization titration method using phenolphthalein as an indicator in accordance with JIS K 0070:1992.

[0125] When the total amount of the (meth)acrylic adhesive is taken as 100 mass%, the content of the maleic anhydride modified compound is usually 3 mass% or more and 40 mass% or less, and from the viewpoint of adhesive ability, particularly when a polyvinyl alcohol-based polarizer is used as the polarizer, from the viewpoint of improving adhesion between the polyvinyl alcohol-based polarizer and the films 10, 30, the content is preferably 5 mass% or more and 35 mass% or less, and more preferably 10 mass% or more and 30 mass% or less.

[0126] (Photopolymerization initiator) The (meth)acrylic adhesive preferably contains a photopolymerization initiator. The photopolymerization initiator is not particularly limited as long as it is a compound that generates active radicals, acids, etc. by the action of light and can initiate polymerization of a (meth)acrylate compound.

[0127] The adhesive composition may contain only one type of photopolymerization initiator, or may contain two or more types of photopolymerization initiators. Examples of the photopolymerization initiator include, but are not limited to, oxime compounds such as O-acyloxime compounds, alkylphenone compounds, and acylphosphine oxide compounds.

[0128] The O-acyloxime compound is a compound having a structure represented by the following formula (6): In the following, * represents a bond.

[0129] [ka]

[0130] Examples of O-acyloxime compounds include N-benzoyloxy-1-(4-phenylsulfanylphenyl)butan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, N-benzoyloxy-1-(4-phenylsulfanylphenyl)-3-cyclopentylpropan-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethan-1-imine, and N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2,4-dioxacyclopentanylmethyloxy)benzoyl}-9H-carbazol-3-yl] ethane-1-imine, N-acetoxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-3-cyclopentylpropan-1-imine, N-benzoyloxy-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-3-cyclopentylpropan-1-one-2-imine, N-acetyloxy-1-[4-(2-hydroxyethyloxy)phenylsulfanylphenyl]propan-1-one-2-imine, N-acetyloxy-1-[4-(1-methyl-2-methoxyethoxy)-2-methylphenyl]-1-(9-ethyl-6-nitro-9H-carbazol-3-yl)methane-1-imine, and the like.

[0131] Commercially available products such as Irgacure (trade name) OXE01, OXE02, and OXE03 (all manufactured by BASF), N-1919, NCI-930, and NCI-831 (all manufactured by ADEKA) may also be used.

[0132] The alkylphenone compound is a compound having a partial structure represented by the following formula (6a) or a partial structure represented by the following formula (6b): In these partial structures, the benzene ring may have a substituent.

[0133] [ka]

[0134] Examples of compounds having a structure represented by formula (6a) include 2-methyl-2-morpholino-1-(4-methylsulfanylphenyl)propan-1-one, 2-dimethylamino-1-(4-morpholinophenyl)-2-benzylbutan-1-one, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]butan-1-one.

[0135] Commercially available products such as Omnirad (trade name) 369, 907, and 379 (all manufactured by IGM Resins BV) may also be used.

[0136] Examples of compounds having a structure represented by formula (6b) include 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, oligomers of 2-hydroxy-2-methyl-1-(4-isopropenylphenyl)propan-1-one, α,α-diethoxyacetophenone, and benzyl dimethyl ketal.

[0137] Commercially available products such as Omnirad (trade name) 184 (manufactured by IGM Resins BV) may also be used.

[0138] Examples of the acylphosphine oxide compound include phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (for example, trade name "Omnirad 819" (manufactured by IGM Resins BV)), 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and the like.

[0139] Further examples of the photopolymerization initiator (C) include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; benzophenone compounds such as benzophenone, o-benzoyl methyl benzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, and 4,4'-di(N,N'-dimethylamino)-benzophenone; Xanthone compounds such as 2-isopropylthioxanthone and 2,4-diethylthioxanthone; Anthracene compounds such as 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, and 2-ethyl-9,10-diethoxyanthracene; quinone compounds such as 9,10-phenanthrenequinone, 2-ethylanthraquinone, camphorquinone, etc.; Benzyl, methyl phenylglyoxylate, titanocene compounds, etc.

[0140] When the total amount of the (meth)acrylic adhesive composition is taken as 100 mass%, the content of the photopolymerization initiator is typically 0.1 mass% or more and 20 mass% or less, and from the viewpoint of the curing property of the (meth)acrylic adhesive and the adhesive ability to the polarizer 20 and the films 10, 30, the content is preferably 0.5 mass% or more and 15 mass% or less, and more preferably 1 mass% or more and 10 mass% or less (for example, 8 mass% or less).

[0141] When the total amount of the (meth)acrylate compound is 100 parts by mass, the content of the photopolymerization initiator is usually 0.1 parts by mass or more and 30 parts by mass or less, and from the viewpoint of the curing property of the (meth)acrylic adhesive and the adhesive ability to the polarizer 20 and the films 10, 30, the content is preferably 0.5 parts by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 10 parts by mass or less.

[0142] (Petroleum resin) The acrylic adhesive may further contain a petroleum resin. When the (meth)acrylic adhesive composition further contains a petroleum resin, the moisture permeability of the cured film can be reduced. An adhesive capable of forming a cured film with low moisture permeability is suitable for applications requiring the suppression of moisture ingress and egress through the cured film. For example, in a polarizing plate having a protective film laminated on at least one surface of a polarizer via an adhesive layer or an image display panel including the same, if the adhesive layer has low moisture permeability, it is possible to suppress curling (warping) of the polarizing plate or image display panel caused by moisture ingress and egress.

[0143] The (meth)acrylic adhesive further containing a petroleum resin can be advantageous in terms of improving the adhesion between the polarizer and the thermoplastic resin film.

[0144] Examples of the petroleum resin include aromatic petroleum resin, aliphatic petroleum resin, cyclic aliphatic petroleum resin, aliphatic-aromatic petroleum resin, coumarone resin, etc. Hydrogenated versions of these resins are also included.

[0145] The aromatic petroleum resin is a resin containing one or more types of structural units derived from aromatic hydrocarbons, and may be a hydrogenated or modified version of the resin.

[0146] The aromatic petroleum resin is preferably a C9 petroleum resin. The C9 petroleum resin is a resin obtained by copolymerizing a C9 fraction, and may be a hydrogenated or modified version of the resin.

[0147] The C9 petroleum resin may be a resin obtained by copolymerizing a C9 fraction with other monomer components, or may be a hydrogenated or modified resin. Examples of the other monomer components include a C5 fraction.

[0148] Examples of C9 fractions include petroleum fractions having about 8 to 10 carbon atoms, such as styrene, alkylstyrene, vinyltoluene, 1-methyl-1-phenylethylene, indene, and methylindene.

[0149] Examples of C5 fractions include petroleum fractions having about 4 to 5 carbon atoms, such as cyclopentadiene, pentene, pentadiene, and piperylene.

[0150] The petroleum resin may be a C5 petroleum resin obtained by copolymerizing the above-mentioned C5 fraction, a hydrogenated C5 petroleum resin, or a modified C5 petroleum resin. Furthermore, it may be an alicyclic hydrocarbon resin obtained by cyclodimerizing a C5 fraction and then polymerizing the resulting resin. Examples of the alicyclic hydrocarbon resin include polymers containing structural units derived from dicyclopentadiene.

[0151] The weight average molecular weight of the petroleum resin is usually 500 or more and 10,000 or less, and from the viewpoint of reducing the moisture permeability of the cured film formed from the adhesive composition and from the viewpoint of the adhesive ability of the adhesive composition to a protective film (or layer), it is preferably 500 or more and 7,000 or less, more preferably 600 or more and 5,000 or less, even more preferably 60 or more and 3,000 or less, and particularly preferably 600 or more and 1,500 or less.

[0152] The weight average molecular weight of the petroleum resin can be measured as a standard polystyrene equivalent value by gel permeation chromatography (GPC).

[0153] When the acrylic adhesive composition contains a petroleum resin, when the total amount of the adhesive is taken as 100 mass%, the content of the petroleum resin is preferably from 20 mass% to 70 mass% and more preferably from 30 mass% to 65 mass% from the viewpoint of reducing the moisture permeability of the cured film and from the viewpoint of the adhesive ability of the adhesive composition to a protective film, and in particular, from the viewpoint of improving the adhesion between a polyvinyl alcohol-based polarizer and a protective film when a polyvinyl alcohol-based polarizer is used as the polarizer.

[0154] When the acrylic adhesive contains a monofunctional (meth)acrylate compound and a petroleum resin, the mass ratio thereof (monofunctional (meth)acrylate compound / petroleum resin) is preferably 0.5 or more and 3.0 or less, more preferably 0.7 or more and 2.0 or less, even more preferably 0.9 or more and 1.5 or less, and even more preferably 1.0 or more and 1.3 or less, from the viewpoints of reducing the moisture permeability of a cured film formed from the adhesive composition and of the adhesive ability of the adhesive composition to a protective film, and in particular, from the viewpoint of enhancing adhesion between a polyvinyl alcohol-based polarizer and a protective film when a polyvinyl alcohol-based polarizer is used as the polarizer.

[0155] (Additives) The first adhesive and / or the second adhesive may contain other additives as necessary. Specific examples of additives include ion trapping agents, antioxidants, chain transfer agents, polymerization accelerators (polyols, etc.), sensitizers, sensitization assistants, light stabilizers, tackifiers, thermoplastic resins, fillers, flow control agents, plasticizers, defoamers, leveling agents, silane coupling agents, dyes, antistatic agents, ultraviolet absorbers, and thermal polymerization initiators. Note that thermal polymerization initiators are used instead of photopolymerization initiators when preparing thermosetting adhesives. Examples of ion trapping agents include powdered inorganic compounds such as bismuth-, antimony-, magnesium-, aluminum-, calcium-, and titanium-based compounds, and mixtures thereof, and examples of antioxidants include hindered phenol-based antioxidants.

[0156] The thickness of the first adhesive layer 150 and the second adhesive layer 160 is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less, and may be 5 μm or less, or may be 0.05 μm or more, or 0.5 μm or more.

[0157] (Protection film 30) The protective film 30 is not particularly limited as long as it is a transparent optical film. For example, the protective film may be a film of a polyolefin-based resin such as polyethylene, polypropylene, or cyclic polyolefin; a cellulose acetate-based resin such as triacetyl cellulose or diacetyl cellulose; a polyester-based resin such as polyethylene terephthalate, polyethylene naphthalate, or polybutylene terephthalate, a polycarbonate-based resin, a (meth)acrylic-based resin, or a polypropylene-based resin.

[0158] In particular, it is preferable that the protective film 30 is a cyclic polyolefin resin film.

[0159] Cyclic polyolefin resin is a general term for resins polymerized using cyclic olefins as polymerization units, and examples thereof include the resins described in JP-A-1-240517, JP-A-3-14882, and JP-A-3-122137.

[0160] Specific examples of cyclic polyolefin resins include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers (representatively random copolymers) of cyclic olefins with chain olefins such as ethylene and propylene, graft polymers of these modified with unsaturated carboxylic acids or their derivatives, and hydrogenated products thereof. Among these, norbornene-based resins obtained by polymerizing norbornene-based monomers such as norbornene and polycyclic norbornene-based monomers as cyclic olefins are preferably used.

[0161] From the viewpoint of thinning, the thickness of the protective film 30 is usually 100 μm or less, preferably 80 μm or less, and more preferably 65 μm or less, and is usually 15 μm or more, and preferably 20 μm or more. The protective film 30 may have a retardation.

[0162] When the protective film 30 is a retardation film, the machine flow direction (MD direction) from the die in film formation of the protective film 30 and the direction of the absorption axis of the polarizer 20 are not particularly limited, but are preferably parallel to each other.

[0163] (Adhesive layer 40) An adhesive layer 40 is attached to the outer surface of the protective film 30. This adhesive layer 40 can be used to attach the polarizing plate 100 to a display element (e.g., a liquid crystal cell) or other optical members. It is also preferable that a release film is laminated on the lower surface of this adhesive layer 40.

[0164] There is no particular limitation on the material of the adhesive layer 40. The adhesive layer can be composed of an adhesive composition mainly composed of a resin such as a (meth)acrylic, rubber, urethane, ester, silicone, or polyvinyl ether resin. Among them, an adhesive composition having a (meth)acrylic resin as a base polymer, which is excellent in transparency, weather resistance, heat resistance, etc., is preferable. The adhesive composition may be of an active energy ray curing type or a heat curing type.

[0165] As the (meth)acrylic resin (base polymer) used in the pressure-sensitive adhesive composition, for example, a polymer or copolymer containing one or more (meth)acrylic acid esters as monomers, such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, is preferably used. It is preferable to copolymerize a polar monomer into the base polymer.

[0166] Examples of polar monomers include monomers having a carboxyl group, a hydroxyl group, an amide group, an amino group, an epoxy group, or the like, such as (meth)acrylic acid, 2-hydroxypropyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate.

[0167] The pressure-sensitive adhesive composition may contain only the base polymer, but usually further contains a crosslinking agent. Examples of the crosslinking agent include divalent or higher metal ions that form carboxylate metal salts with carboxyl groups, polyamine compounds that form amide bonds with carboxyl groups, polyepoxy compounds or polyols that form ester bonds with carboxyl groups, and polyisocyanate compounds that form amide bonds with carboxyl groups. Among these, polyisocyanate compounds are preferred.

[0168] The active energy ray curable adhesive composition has a property of being cured by irradiation with active energy rays such as ultraviolet rays and electron beams, and has adhesiveness even before irradiation with active energy rays, can be adhered to an adherend such as a film, and can be cured by irradiation with active energy rays to adjust the adhesive strength. The active energy ray curable adhesive composition is preferably an ultraviolet ray curable type. The active energy ray curable adhesive composition further contains an active energy ray polymerizable compound in addition to a base polymer and a crosslinking agent. If necessary, a photopolymerization initiator, a photosensitizer, etc. can also be contained.

[0169] The pressure-sensitive adhesive composition can contain additives such as microparticles for imparting light scattering properties, beads (e.g., resin beads, glass beads), glass fibers, resins other than the base polymer, antistatic agents, tackifiers, fillers (e.g., metal powders and other inorganic powders), antioxidants, UV absorbers, dyes, pigments, colorants, defoamers, corrosion inhibitors, and photopolymerization initiators.

[0170] The thickness of the adhesive layer 40 is usually 1 to 40 μm, but from the viewpoint of making the optical sheet thinner and suppressing dimensional changes in the polarizing plate 100 while maintaining good processability, it is preferably 3 to 25 μm (for example, 3 to 20 μm, or even 3 to 15 μm).

[0171] (Storage modulus) The storage modulus of the pressure-sensitive adhesive layer 40 at 25° C. and a measurement frequency of 1 Hz is 1.5×10 5 Pa or less, 1.3×10 5 Pa or less is acceptable, 1.0×10 5 Pa or less is acceptable, 5.0××10 4 The storage modulus of the pressure-sensitive adhesive layer 40 at 25° C. and a measurement frequency of 1 Hz may be 5.0×10 3 Pa or more, and 4 Pa or more. The storage modulus of the pressure-sensitive adhesive layer at 25°C and a measurement frequency of 1 Hz can be measured with a rheometer. For example, the pressure-sensitive adhesive layers are stacked to a thickness of 200 μm to prepare a measurement sample, and the storage modulus is measured by raising the temperature at 10°C / min with a strain of 1% and a frequency of 1 Hz using a rheometer ("MCR-301" (trade name) manufactured by Anton Parr, with a parallel plate of PP25), and reading the value of the storage modulus at 25°C. The storage modulus of the pressure-sensitive adhesive layer 40 at 25°C and a measurement frequency of 1 Hz can be adjusted to a desired value by, for example, adjusting the type of resin that is the main component of the pressure-sensitive adhesive composition (for example, the type of monomer constituting the resin, and the blending ratio when there are multiple monomers), molecular weight (weight average molecular weight or number average molecular weight), glass transition temperature, the type and blending amount of the crosslinking agent in the pressure-sensitive adhesive composition, etc. Furthermore, when the pressure-sensitive adhesive layer 40 is formed from an active energy ray-curable pressure-sensitive adhesive composition, the desired storage modulus can be achieved by adjusting the type and blending amount of the active energy ray-polymerizable compound in addition to adjusting the resin and crosslinking agent described above.

[0172] (Action and effect) It is believed that when the (meth)acrylic resin film 10 is relatively hard, the (meth)acrylic resin film 10 has a dense structure and thus has excellent solvent resistance. In addition, when the (meth)acrylic resin protective film 10 is relatively hard and the pressure-sensitive adhesive layer 40 is relatively soft, when the polarizing plate 100 attached to a substrate or the like is placed in a high-temperature and high-humidity environment, even if the polarizer 20 shrinks, the pressure-sensitive adhesive layer 40 deforms and absorbs the stress, so that the entire device including the polarizing plate 100 and the substrate (such as a liquid crystal panel) is less likely to warp.

[0173] Such a polarizing plate can be applied not only to ordinary liquid crystal displays, but also to various image displays such as electroluminescent displays, plasma displays, and field emission displays. EXAMPLES

[0174] [Preparation of (meth)acrylic resin film I] Polymethylmethacrylate with a glutarimide ring content of 5% (Mw=48×10 3 Pellets containing a copolymer of 1,2-difluorophenyl ether (Mw / Mn=2.0) were melt-kneaded at 245° C. in an extruder and fed to a T-die set at 245° C. The film-like molten resin extruded from the T-die was sandwiched between a first cooling roll and a second cooling roll arranged opposite each other, and then wrapped around a third cooling roll for molding and cooling to obtain a resin film. The glass transition temperature of this film was measured and found to be 115.0°C. The film was subjected to sequential biaxial stretching. The film was stretched 1.8 times in the machine direction at a temperature 20°C higher than the glass transition temperature to obtain a machine-stretched film. Then, the film was stretched 1.8 times in the transverse direction at a temperature 20°C higher than the glass transition temperature to obtain a biaxially stretched film having a thickness of 40 μm.

[0175] [Preparation of (meth)acrylic resin film II] Polymethylmethacrylate with a glutarimide ring content of 5% (Mw=48×10 3Pellets containing a copolymer of 1,2-difluorophenyl ether (Mw / Mn=2.0) were melt-kneaded at 245° C. in an extruder and fed to a T-die set at 245° C. The film-like molten resin extruded from the T-die was sandwiched between a first cooling roll and a second cooling roll arranged opposite each other, and then wrapped around a third cooling roll for molding and cooling to obtain a resin film. The glass transition temperature of this film was measured and found to be 115.4°C. The film was subjected to sequential biaxial stretching. The film was stretched 2.0 times in the machine direction at a temperature 20°C higher than the glass transition temperature to obtain a machine-stretched film. Then, the film was stretched 2.0 times in the transverse direction at a temperature 20°C higher than the glass transition temperature to obtain a biaxially stretched film having a thickness of 40 μm.

[0176] [Preparation of (meth)acrylic resin film III] (Meth)acrylic resin (Mw = 107 × 10) with a mass ratio of methyl methacrylate / methyl acrylate = 98.6 / 1.4 3 Pellets containing 72 parts by mass of styrene / maleic anhydride copolymer (Mw / Mn=2.6), 8 parts by mass of a copolymer of styrene / maleic anhydride = 18 / 82 (mass ratio) (SMA700, manufactured by Jiaxing Huawen Chemical Co.), and 20 parts by mass of (meth)acrylic rubber particles, which are a (meth)acrylic multilayer polymer having a three-layer structure (first layer (innermost layer): a copolymer of methyl methacrylate, methyl acrylate, and allyl methacrylate (mass ratio 93.8 / 6.0 / 0.2) / second layer: a copolymer of butyl acrylate, styrene, and allyl methacrylate (mass ratio 80.6 / 17.4 / 2.0) / third layer (outermost layer): a copolymer of methyl methacrylate and methyl acrylate (mass ratio 94 / 6)) were melt-kneaded at 245°C in an extruder and fed to a T-die set at a temperature of 245°C. The film-like molten resin extruded from the T-die was sandwiched between the first and second cooling rolls arranged opposite each other, and then wrapped around the third cooling roll for forming and cooling to obtain an unstretched film with a thickness of 70 μm. The glass transition temperature of this film was measured and found to be 102.8°C.

[0177] [Preparation of (meth)acrylic resin film IV] (Meth)acrylic resin (Mw = 107 × 10) with a mass ratio of methyl methacrylate / methyl acrylate = 98.6 / 1.4 3 , Mw / Mn=2.6) and 64 parts by mass of a methacrylic resin (a homopolymer of methyl methacrylate, Mw=69×10 3 Pellets containing 16 parts by mass of a (meth)acrylic rubber particle having a three-layer structure (first layer (innermost layer): a copolymer of methyl methacrylate, methyl acrylate, and allyl methacrylate (mass ratio 93.8 / 6.0 / 0.2) / second layer: a copolymer of butyl acrylate, styrene, and allyl methacrylate (mass ratio 80.6 / 17.4 / 2.0) / third layer (outermost layer): a copolymer of methyl methacrylate and methyl acrylate (mass ratio 94 / 6)) were melt-kneaded at 245°C in an extruder and fed to a T-die set at 245°C. The film-like molten resin extruded from the T-die was sandwiched between a first cooling roll and a second cooling roll arranged opposite each other, and was formed and cooled by being wrapped around a third cooling roll to obtain an unstretched film having a thickness of 60 μm. The glass transition temperature of this film was measured and found to be 104.0°C.

[0178] [Preparation of (meth)acrylic resin film V] (Meth)acrylic resin (Mw = 111 × 10) with a mass ratio of methyl methacrylate / methyl acrylate = 97.2 / 2.8 3Pellets containing 70 parts by mass of a (meth)acrylic rubber particle having a three-layer structure (first layer (innermost layer): a copolymer of methyl methacrylate, methyl acrylate, and allyl methacrylate (mass ratio 93.8 / 6.0 / 0.2) / second layer: a copolymer of butyl acrylate, styrene, and allyl methacrylate (mass ratio 80.6 / 17.4 / 2.0) / third layer (outermost layer): a copolymer of methyl methacrylate and methyl acrylate (mass ratio 94 / 6)) were melt-kneaded at 245°C in an extruder and fed to a T-die set at a temperature of 245°C. The film-like molten resin extruded from the T-die was sandwiched between a first cooling roll and a second cooling roll arranged opposite each other, and was formed and cooled by being wrapped around a third cooling roll to obtain an unstretched film having a thickness of 60 μm. The glass transition temperature of this film was measured and found to be 98.9°C.

[0179] [Curable adhesive composition A (epoxy type)] Curable adhesive composition A was prepared by mixing and degassing 20 parts by mass of 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexane carboxylate (manufactured by Daicel Corporation under the trade name "Celloxide 2021P"), 70 parts by mass of neopentyl glycol diglycidyl ether (manufactured by Nagase ChemteX Corporation under the trade name "EX-211L"), 2 parts by mass of 4-hydroxybutyl vinyl ether (manufactured by Nippon Carbide Corporation under the trade name "HBVE"), 8 parts by mass of methyl methacrylate-methacrylic acid glycidyl ether copolymer (cationic polymerizable polymer) (manufactured by NOF Corporation under the trade name "Marproof G-01100"), and 2.25 parts by mass of solids of a photopolymerization initiator (manufactured by San-Apro Co., Ltd. under the trade name "CPI-100P")

[0180] [Curable adhesive composition B (epoxy type)] Curable adhesive composition B was prepared by mixing and degassing 70 parts by mass of 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (manufactured by Daicel Corporation under the product name "Celloxide 2021P"), 20 parts by mass of neopentyl glycol diglycidyl ether (manufactured by Nagase ChemteX Corporation under the product name "EX-211"), 10 parts by mass of 2-ethylhexyl glycidyl ether (manufactured by Nagase ChemteX Corporation under the product name "EX-121"), and 2.8 parts by mass of solids of a photopolymerization initiator (manufactured by San-Apro Ltd. under the product name "CPI-100P").

[0181] [Curable adhesive composition C ((meth)acrylic)] The curable adhesive composition C contained 17 parts by mass of maleic anhydride-modified liquid polybutadiene (trade name "Lithene ultra N4-5000-10MA" manufactured by Synthomer, number average molecular weight: 5500, viscosity at 25°C: 25 to 60 Pa·sec, acid value: 54 KOHmg / g), 34 parts by mass of dicyclopentanyl acrylate (trade name "FA-513AS" manufactured by Hitachi Chemical Co., Ltd.), 12 parts by mass of stearyl acrylate (trade name "STA" manufactured by Osaka Organic Chemical Co., Ltd.), 2 parts by mass of ethoxylated bisphenol A diacrylate (trade name "A-BPE-10" manufactured by Shin-Nakamura Chemical Co., Ltd., EO 10 mol), 5.0 parts by mass of tricyclodecane dimethanol diacrylate (trade name (A-DCP) manufactured by Shin-Nakamura Chemical Co., Ltd.), and The following mixture was prepared by mixing 30 parts by mass of a petroleum resin (trade name "T-REZ HA105" manufactured by JXTG Nippon Oil & Energy Corporation), 30 parts by mass of a hydrogenated resin (alicyclic saturated hydrocarbon resin having dicyclopentadiene as a monomer component), softening point (nominal value): 104.5°C, weight average molecular weight (nominal value): 610), and adding 3.0 parts by mass of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (trade name "Omnirad 819" manufactured by IGM Resins BV) per 100 parts by mass of the total weight. After mixing, the mixture was degassed to prepare the composition.

[0182] Example 1 [Preparation of polarizing plate] The surface (inner surface of the roll) of the (meth)acrylic resin film I was subjected to a corona treatment, and the curable adhesive composition A was applied to the corona-treated surface using an adhesive applicator. The resulting coating layer and a polyvinyl alcohol-iodine polarizer I having a thickness of 23 μm and a boron content of 4.2 mass% were laminated using a nip roll to obtain a polarizer with the (meth)acrylic resin film I. In the polarizer with the (meth)acrylic resin film I, the machine direction (MD) of the (meth)acrylic resin film I and the absorption axis of the polarizer were parallel to each other.

[0183] Next, a corona treatment was applied to the surface of a 50 μm-thick retardation film made of a cyclic polyolefin resin (manufactured by Zeon Corporation under the trade name "ZEONOR"), and the curable adhesive composition B was applied to the corona-treated surface using an adhesive applicator. The resulting coating layer and the polarizer surface of the (meth)acrylic resin film I-attached polarizer were laminated using a nip roll to obtain a laminate. In the laminate, the machine flow direction (MD) of the retardation film and the absorption axis of the polarizer were parallel to each other.

[0184] From the retardation film side of this laminate, the total integrated light quantity (integrated light irradiation intensity in the wavelength region of 320 to 400 nm) is about 200 mJ / cm 2 A polarizing plate was produced by curing the layer of curable adhesive composition B and the layer of curable adhesive composition A by irradiating them with ultraviolet light (UVB) of 1000 nm (measured by UV Power Puck II manufactured by FusionUV). The cured layer of curable adhesive composition A had a thickness of about 3 μm, and the cured layer of curable adhesive composition B had a thickness of about 3 μm.

[0185] The cyclic polyolefin film side of the prepared polarizing plate was coated with a 25 μm thick film having a storage modulus of 2.5×10 at 25°C. 4 The (meth)acrylic adhesive layer A having a thickness of 1 Pa (measurement frequency 1 Hz) was laminated on the polarizing plate having the adhesive layer. The adhesive layer side of the produced polarizing plate having the adhesive layer was cut to a size of 150 mm x 90 mm, and the adhesive layer side was attached to a non-alkali glass substrate (thickness: 0.7 mm) to obtain a laminate.

[0186] Example 2 A polarizing plate was produced in the same manner as in Example 1, except that curable adhesive composition C was used instead of curable adhesive composition A, and the thickness of the cured layer of curable adhesive composition C was 10 μm.

[0187] Example 3 A polarizing plate was produced in the same manner as in Example 1, except that the polyvinyl alcohol-iodine polarizer I was replaced with a polyvinyl alcohol-iodine polarizer II having a thickness of 18 μm and a boron content of 3.9 mass %.

[0188] Example 4 A polarizing plate was produced in the same manner as in Example 3, except that curable adhesive composition C was used instead of curable adhesive composition A, and the thickness of the cured layer of curable adhesive composition C was 10 μm.

[0189] Example 5 A polarizing plate was produced in the same manner as in Example 1, except that the (meth)acrylic resin film II was used instead of the (meth)acrylic resin film I.

[0190] Example 6 A polarizing plate was produced in the same manner as in Example 5, except that curable adhesive composition C was used instead of curable adhesive composition A, and the thickness of the cured layer of curable adhesive composition C was 10 μm.

[0191] Example 7 A polarizing plate was produced in the same manner as in Example 5, except that the polyvinyl alcohol-iodine polarizer I was replaced with a polyvinyl alcohol-iodine polarizer II having a thickness of 18 μm and a boron content of 3.9 mass %.

[0192] Example 8 A polarizing plate was produced in the same manner as in Example 7, except that curable adhesive composition C was used instead of curable adhesive composition A, and the thickness of the cured layer of curable adhesive composition C was 10 μm.

[0193] Example 9 A polarizing plate was produced in the same manner as in Example 3, except that the (meth)acrylic resin film III was used instead of the (meth)acrylic resin film I.

[0194] Example 10 A polarizing plate was produced in the same manner as in Example 9, except that curable adhesive composition C was used instead of curable adhesive composition A, and the thickness of the cured layer of curable adhesive composition C was 10 μm.

[0195] Example 11 A polarizing plate was produced in the same manner as in Example 3, except that (meth)acrylic resin film IV was used instead of (meth)acrylic resin film I.

[0196] Example 12 A polarizing plate was produced in the same manner as in Example 11, except that curable adhesive composition C was used instead of curable adhesive composition A, and the thickness of the cured layer of curable adhesive composition C was 10 μm.

[0197] Examples 13 to 20 Instead of the (meth)acrylic pressure-sensitive adhesive layer A, a layer having a thickness of 20 μm and a storage modulus at 25° C. of 1.5×10 4 A polarizing plate was produced in the same manner as in Examples 1 to 8, except that a (meth)acrylic pressure-sensitive adhesive layer B of 1 Pa (measurement frequency 1 Hz) was used.

[0198] Examples 21 to 28 Instead of the (meth)acrylic adhesive layer A, a layer having a thickness of 5 μm and a storage modulus of 1.1 × 10 5 A polarizing plate was produced in the same manner as in Examples 1 to 8, except that the (meth)acrylic pressure-sensitive adhesive layer C having a resistance of 1 Pa (measurement frequency 1 Hz) was used.

[0199] Comparative Example 1 A polarizing plate was produced in the same manner as in Example 1, except that the (meth)acrylic resin film V was used instead of the (meth)acrylic resin film I.

[0200] Comparative Example 2 A polarizing plate was produced in the same manner as in Comparative Example 1, except that curable adhesive composition C was used instead of curable adhesive composition A, and the thickness of the cured layer of curable adhesive composition C was 10 μm.

[0201] Comparative Example 3 A polarizing plate was produced in the same manner as in Comparative Example 1, except that the polyvinyl alcohol-iodine polarizer I was replaced with a polyvinyl alcohol-iodine polarizer II having a thickness of 18 μm and a boron content of 3.9 mass %.

[0202] Comparative Example 4 A polarizing plate was produced in the same manner as in Comparative Example 3, except that curable adhesive composition C was used instead of curable adhesive composition A, and the thickness of the cured layer of curable adhesive composition C was 10 μm.

[0203] [Table 1]

[0204] [Table 2]

[0205] [Table 3]

[0206] [Table 4]

[0207] <Measurement and Evaluation> Martens hardness A (meth)acrylic resin film was cut to a size of 30 mm × 30 mm, and the thickness was 25 μm and the storage modulus at 25 °C was 2.5 × 10 4The specimen was attached to a non-alkali glass substrate (thickness: 0.7 mm) using an acrylic adhesive with a tensile strength of 1 Pa (measurement frequency: 1 Hz) to obtain a measurement sample. A load was applied to the surface of the measurement sample at a pressure rate of 10 mN / 5 s using an ultra-microhardness tester (FISCHERSCOPE HM2000: manufactured by Fischer Instruments Co., Ltd.) in an atmosphere of 23°C temperature and 55% relative humidity, and the Martens hardness HM (N / mm 2 ) was measured.

[0208] Glass transition temperature (Tg) Using a DSC device (EXSTAR6000, manufactured by Seiko Instruments Inc.), according to the differential scanning calorimetry based on JIS K7121:1987, the (meth)acrylic film was cooled to -80°C at a rate of 10°C / min with a nitrogen flow rate of 40mL / min, held for 10 minutes, then heated to 160°C at a rate of 10°C / min and held for 10 minutes. Next, the temperature was lowered from 160°C to -80°C at a rate of 10°C / min, held for 10 minutes, and then heated to 160°C at a rate of 10°C / min to determine the onset glass transition temperature (Tg), which was taken as the glass transition temperature. The higher this value, the higher the heat resistance.

[0209] Tensile modulus in MD direction T MD (25℃ and 80℃) The (meth)acrylic resin film was cut into a rectangle of 70 mm long x 10 mm wide. The length direction of the test piece was the MD direction of the resin film, and the width direction was the TD direction (direction perpendicular to the MD direction) of the resin film. Then, the test piece was clamped at both ends in the length direction (MD direction of the resin film) with the upper and lower grips of a tensile tester (Autograph AG-1S tester, manufactured by Shimadzu Corporation) so that the distance between the grips was 5 cm, and the test piece was pulled in the length direction (MD direction of the resin film) at a pulling speed of 50 mm / min under an environment of 80 ° C. and 25 ° C., and the tensile modulus (MPa) in the MD direction of the resin film at 80 ° C. and 25 ° C. was calculated from the slope of the initial straight line in the obtained stress-strain curve.

[0210] Tensile modulus in TD direction T TD (25℃ and 80℃) The (meth)acrylic resin film was cut into a rectangle of 70 mm long x 10 mm wide. The length direction of the test piece was the TD direction of the resin film, and the width direction was the MD direction (direction perpendicular to the TD direction) of the resin film. Then, the test piece was clamped at both ends in the length direction (TD direction of the resin film) with the upper and lower grips of a tensile tester (Autograph AG-1S tester, manufactured by Shimadzu Corporation) so that the distance between the grips was 5 cm, and the test piece was pulled in the length direction (TD direction of the resin film) at a pulling speed of 50 mm / min under an environment of 80 ° C. and 25 ° C., and the tensile modulus (MPa) in the TD direction of the resin film at 80 ° C. and 25 ° C. was calculated from the slope of the initial straight line in the obtained stress-strain curve.

[0211] Storage modulus G' in MD MD (80℃) The (meth)acrylic resin film was cut into a rectangle of 30 mm long x 5 mm wide. The length direction of the test piece was the MD direction of the resin film, and the width direction was the TD direction (direction perpendicular to the MD direction) of the resin film. Then, the test piece was clamped at both ends in the length direction (MD direction of the resin film) with the clamps of a dynamic viscoelasticity measuring device "DVA-220" manufactured by IT Measurement Control Co., Ltd., with the clamps spaced 2 cm apart, and the tensile and contraction frequency was set to 10 Hz, and the heating rate was set to 10 ° C. / min, to determine the storage modulus in the MD direction of the resin film at a temperature of 80 ° C.

[0212] Storage modulus G' in the TD direction TD (80℃) The (meth)acrylic resin film was cut into a rectangle of 30 mm in length and 5 mm in width. The length direction of the test piece was the TD direction of the resin film, and the width direction was the MD direction (direction perpendicular to the TD direction) of the resin film. Next, the test piece was clamped at both ends in the length direction (TD direction of the resin film) with the gripping tools of a dynamic viscoelasticity measuring device "DVA-220" manufactured by IT Measurement Control Co., Ltd., with the gripping tools spaced 2 cm apart, and the tensile and contraction frequency was set to 10 Hz, and the heating rate was set to 10 ° C. / min, to determine the storage modulus in the TD direction of the resin film at a temperature of 80 ° C.

[0213] moisture permeability The moisture permeability (g / (m) of (meth)acrylic resin film at a temperature of 40°C and a relative humidity of 90% was measured using the cup method specified in JIS Z 0208. 2 -24hr) was measured.

[0214] Internal Haze Dimethyl phthalate was dripped onto both sides of a (meth)acrylic resin film cut to 30 mm x 30 mm, the film was sandwiched between PMMA plates (Sumipex E00 1.0 mm), and the haze was measured in accordance with JIS K7136 using a haze meter (HM-150N, manufactured by Murakami Color Research Laboratory Co., Ltd.).

[0215] Preparation of samples for chemical resistance tests A (meth)acrylic resin film was cut into a square of 80 mm long x 80 mm wide, and the resin film was attached to an alkali-free glass substrate (thickness: 0.7 mm) using an acrylic adhesive with a thickness of 25 μm to prepare a sample for a chemical resistance test (a sample before a chemical resistance test). This sample was left to stand at 80°C for 5 minutes, and immediately after being taken out to a condition of 23°C / 55% RH, 1.5 mL of a mixed solvent of ethanol and water (99.5% ethyl alcohol Fujifilm Wako Pure Chemical Industries, Ltd. / pure water = 9 / 1, weight ratio) was dropped onto the surface of the resin film. Then, a cylindrical weight of 0.6 kg and diameter of 5.5 cm covered with a clean wiper (CFW8009L, manufactured by CHANG-FONG TEXTILE TECHNOLOGY CO., LTD.) was placed on the resin film so that the bottom of the cylinder was in contact with the droplet of the mixed solvent, and left to stand for 30 seconds. Next, the weight after the cylinder was removed from the film to obtain a sample after the chemical resistance test. The following evaluations were performed on the samples before and after the chemical resistance test.

[0216] Chemical resistance test (1) Appearance evaluation The appearance of the samples was visually inspected before and after the chemical resistance test and evaluated according to the following criteria. ○: No change in appearance before and after chemical resistance test ×: After the chemical resistance test, the film surface became cloudy and cracks occurred. (2) ΔHaze (chemical resistance) evaluation The haze values ​​of the samples before and after the chemical resistance test were measured using a haze meter (HM-150N, manufactured by Murakami Color Research Laboratory Co., Ltd.) in accordance with JIS K7136. The haze value of the sample after the chemical resistance test minus the haze value of the sample before the chemical resistance test was taken as ΔHaze (chemical resistance) and used as an index of chemical resistance. A smaller ΔHaze (chemical resistance) value indicates less change due to contact with alcohol and better chemical resistance. (3) Sa(post-test) / Sa(pre-test) evaluation The surface roughness of the samples before and after the chemical resistance test was evaluated using a laser microscope (LEXT OLS5000, manufactured by OLYMPUS). The arithmetic mean height Sa was used as an index of surface roughness. The ratio of the Sa value of the sample before the chemical resistance test (Sa(before test)) to the Sa value of the sample after the chemical resistance test (Sa(after test)), Sa(after test) / Sa(before test), was used as an index of chemical resistance. The smaller the value of Sa(after test) / Sa(before test), the smaller the change due to contact with alcohol and the better the chemical resistance.

[0217] Humidity and heat warping The polarizing plate with the adhesive layer was cut into a rectangle of 150 mm long (parallel to the absorption axis of the polarizer) x 90 mm wide (orthogonal to the absorption axis of the polarizer), and attached to the center of an alkali-free glass substrate (thickness: 0.2 mm) of 160 mm long x 102 mm wide, to prepare a sample for a wet heat warping test. This sample was left standing for 75 hours in an environment of 30 ° C and 95% humidity. The laminate was taken out of the test tank and left standing for 2 hours in an environment of 25 ° C and 50% relative humidity, and then placed on the measurement table of a two-dimensional measuring device (Nikon Corporation, NEXIV (registered trademark) MR-12072) so that the front polarizing plate was on the upper side. Next, the surface of the measurement table was focused, and 25 points on the glass sample surface were focused on using that as a reference, and the height from the reference focus was measured. The difference between the maximum and minimum heights at the 25 measurement points was taken as the amount of warping. Specifically, point 50 shown in FIG. 2 was taken as the measurement point. The 25 points shown in FIG. 2 were points in a region 5 mm inward from the edge of the polarizing plate, and were provided at intervals of about 20 mm along the short side and at intervals of about 35 mm along the long side.

[0218] GPC analysis conditions Measuring device: Tosoh Corporation HLC-8320GPC Column configuration: Sample column: Two TSKgel SuperMultipore HZ-M columns and one TSKguardColumn SuperMP(HZ)-M column connected in series Reference column: Two TSKgel Super H-RC columns connected in series Detector: RI (differential refractometer) detector ·Calculation method: Molecular weight calculation ·Internal standard: Chloroform was used as the internal standard. Allowable time for internal standard peak: 0.15 min Elution time of internal standard peak: This was set as the elution time of chloroform when the standard sample for the calibration curve was measured. Reference sample: THF (special grade, Fujifilm Wako Pure Chemical Industries, Ltd.) Measurement sample: A measurement sample was prepared by thoroughly dissolving 25 mg of (meth)acrylic resin in 5 mL of a THF / chloroform solution prepared by dissolving chloroform (Fuji Film Wako Pure Chemical Industries, Ltd.) as an internal standard in THF (special grade, Fuji Film Wako Pure Chemical Industries, Ltd.) to a concentration of 0.04 vol%. Column temperature: 40℃ ·Injection volume: 10μL Sample pump flow rate: 0.35ml / min Reference pump flow rate: 0.60ml / min

[0219] Under the above GPC analysis conditions, the RI detection intensity was measured against the elution time of the (meth)acrylic resin. As standard samples for the calibration curve, the following seven types of methacrylic resins (Shodex STANDARD M-75, Showa Denko K.K.) with known monodisperse mass average molecular weights and different molecular weights were used. Peak Molecular Weight Standard sample 1:1,050,000 Standard sample 2: 569,000 Standard sample 3: 211,000 Standard sample 4: 68,800 Standard sample 5: 18,500 Standard sample 6: 7,360 Standard sample 7: 3,070

[0220] The standard samples for the calibration curve were measured under the same conditions as the (meth)acrylic resin, and the peak top elution time of each standard sample was obtained. From the obtained elution times and peak molecular weights, the following third-order approximation equation was obtained and used as the calibration equation for analyzing the measurement results of the (meth)acrylic resin. ·Log M(molecular weight)=At3+Bt2+Ct+D A, B, C, D: Variables ·t: Elution time The (meth)acrylic resin was analyzed by the above-mentioned GPC measurement to obtain Mw and Mn. [Explanation of symbols]

[0221] 10...(meth)acrylic resin film, 12...first adhesive layer, 20...polarizer, 14...second adhesive layer, 30...protective film, 40...pressure-sensitive adhesive layer, 100...polarizing plate.

Claims

1. A polarizing plate including, in this order, a (meth)acrylic resin film, a first adhesive layer, a polarizer, a second adhesive layer, a protective film, and a pressure-sensitive adhesive layer, The (meth)acrylic resin film has a Martens hardness of 140 N / mm 2 That's all. The pressure-sensitive adhesive layer has a storage modulus of 1.5×10 at 25° C. and a measurement frequency of 1 Hz. 5 A polarizing plate having a tensile strength of 10 Pa or less.

2. The (meth)acrylic resin film is The tensile modulus in the MD direction at 25°C is T MD The tensile modulus in the MD direction at 25°C and 80°C is T MD (80° C.), The tensile modulus in the TD direction at 25°C is T TD The tensile modulus in the TD direction at 25°C and 80°C is T TD (80°C), T MD (25° C.) / T MD (80° C.) and T TD (25° C.) / T TD 2. The polarizing plate according to claim 1, wherein each of the polarizing angles (80° C.) is less than 2.

0.

3. The (meth)acrylic resin film is Storage modulus G' in the MD direction at 80° C. and a measurement frequency of 10 Hz MD (80°C) and the tensile modulus T in the MD direction at 80°C MD (80°C) G' MD (80° C.) / T MD 3. The polarizing plate according to claim 1, wherein the polarizing coefficient of curvature (80° C.) is less than 1.

2.

4. The (meth)acrylic resin film is The storage modulus in the MD direction at 80° C. and a measurement frequency of 10 Hz is G' MD (80° C.), the storage modulus in the TD direction at 80° C. and a measurement frequency of 10 Hz is G' TD (80° C.), then G' MD (80° C.) / G′ TD 3. The polarizing plate according to claim 1, wherein the polarizing coefficient (80° C.) is 1.05 or less.

5. The (meth)acrylic resin film has a moisture permeability and thickness product of 2500 (g / m 2 3. The polarizing plate according to claim 1, wherein the thickness is 24 hr.μm or less.

6. 3. The polarizing plate according to claim 1, wherein the polarizer is a polyvinyl alcohol-based resin film containing a boron compound and having a boron content of 4.0 wt % or less.

7. The polarizing plate according to claim 1 , wherein the first adhesive layer is a cured product of a (meth)acrylic adhesive.

8. The polarizing plate according to claim 1 , wherein the protective film is a cyclic polyolefin resin film.

Citation Information

Patent Citations

  • Polarizing plate and liquid crystal display panel using the same

    JP2017204007A

  • Polarization film, polarization film with adhesive layer and image display device

    JP2018200339A