Aluminum alloy sheet, method for manufacturing the same, and heat exchanger
A specially formulated aluminum alloy plate with controlled composition and grain structure addresses the challenges of single-phase heat bonding, ensuring effective brazing and material strength while minimizing deformation and corrosion.
Patent Information
- Application Number
- JP2023059807
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
Existing aluminum alloy materials for single-phase heat bonding face challenges in achieving both excellent brazing properties and material strength, with issues such as reduced joinability, corrosion resistance, and deformation due to insufficient liquid phase formation and excessive Si or Cu content.
An aluminum alloy plate with specific compositions (2.00 to 3.00% Si, 0.05 to 0.40% Fe, 0.80 to 1.80% Mn, and controlled grain boundary distribution and size) is developed, allowing for effective heat bonding without additional brazing materials, ensuring adequate liquid phase formation and material strength.
The solution provides an aluminum alloy plate with enhanced brazing properties and material strength, maintaining shape integrity during bonding and improving corrosion resistance.
Smart Images

Figure 2024147043000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to an aluminum alloy plate for single-phase thermal bonding and a heat exchanger manufactured using the same. [Background technology]
[0002] Brazing is often used in the manufacturing of products made of aluminum, such as heat exchangers and heat sinks, that have numerous metal joints. Brazing sheets, which are aluminum cores clad with brazing filler metals, and pre-placed brazing filler metals have been used as aluminum materials for brazing. However, the use of clad materials, such as brazing sheets, which join multiple layers together, and additional joining materials, such as pre-placed brazing filler metals, has been a factor in increasing the cost of heat exchangers and other products due to their manufacturing and material costs.
[0003] Therefore, in recent years, aluminum alloy materials that can be thermally bonded in a single layer have been proposed (for example, Patent Documents 1 and 2). These aluminum alloy materials are made of an Al-Si alloy, and utilize the liquid phase generated inside the alloy material upon heating for bonding. With this aluminum alloy material, the liquid phase acts as a brazing material, so that it can be bonded to other components even though it is a single layer, without using a bonding material such as a pre-placed brazing material. In the present invention, the ability to bond by heating without a bonding material is referred to as a "thermal bonding function." Furthermore, bonding using such an aluminum alloy material that has a thermal bonding function in a single layer is referred to as "thermal bonding," and the heating temperature at that time is referred to as the "thermal bonding temperature."
[0004] In aluminum alloy materials having a thermal bonding function in a single layer, it is important to ensure deformation resistance at the brazing temperature because the material becomes semi-molten during thermal bonding. As a method for improving the deformation resistance of aluminum alloy materials, for example, Patent Documents 3 and 4 disclose aluminum alloy materials having a thermal bonding function in a single layer with excellent deformation resistance, which are obtained by forming a metal structure in which crystal grains become coarse after brazing heating and the generation of a liquid phase at grain boundaries is suppressed. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5436714 specification [Patent Document 2] International Publication No. 2022 / 176420 [Patent Document 3] Patent No. 5345264 specification [Patent Document 4] Patent No. 5732594 specification Summary of the Invention [Problem to be solved by the invention]
[0006] Aluminum alloy materials can be joined to other components by their own action (liquid phase seeping out from the base material) without using joining materials such as brazing or filler metals, and require a smaller amount of liquid phase for brazing joining compared to brazing sheet fin materials clad with conventional brazing materials.
[0007] As a result, the fillet area formed at the joint between the fin and the tube is small, which reduces the fin's bondability (brazing ability). Furthermore, if this fillet area is small, the corrosion wear time (corrosion protection life) when exposed to a corrosive environment is shortened, causing the fin to peel off early and no longer functioning adequately as sacrificial corrosion protection. Furthermore, there is the problem that this fin peeling can cause deformation of the material.
[0008] One way to increase this liquid phase is to increase the Si content, but if the Si content is too high, excessive Si seeps out of the base material during brazing heating, drastically reducing the material's strength, making it difficult to obtain sufficient strength and reducing corrosion resistance.Another method is to increase the Cu content to increase the liquid phase ratio, but this can cause problems such as a significant deterioration in corrosion resistance and a decrease in formability due to the increased material strength, making it difficult to solve the problems by adjusting the composition.
[0009] Therefore, the present invention has been made under the above-mentioned background, and an object of the present invention is to provide an aluminum alloy sheet that has excellent brazability while ensuring material strength when producing various aluminum alloy structures. [Means for solving the problem]
[0010] As a result of intensive research, the present inventors have found that the distribution of grain boundaries and the average grain size of an aluminum alloy sheet after a predetermined heating test affect the brazability and material strength. The present inventors have also found an aluminum alloy material having joining ability and material strength, wherein the aluminum alloy sheet contains 2.00 to 3.00 mass% Si, 0.05 to 0.40 mass% Fe, and 0.80 to 1.80 mass% Mn, a Cu content of 0.20 mass% or less (inclusive of 0.00 mass%), and a Zn content of 6.00 mass% or less (inclusive of 0.00 mass%), and in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after a brazing heating test, the proportion of regions with one or more grain boundaries in the sheet thickness direction is 25% or more but less than 90% in the width direction, and the average grain size in the direction perpendicular to the rolling direction on the sheet surface is 950 μm or less, thereby completing the present invention.
[0011] That is, the present invention (1) is an aluminum alloy plate having a function of being heat-bonded in a single layer, an aluminum alloy containing 2.00 to 3.00% by mass of Si, 0.05 to 0.40% by mass of Fe, and 0.80 to 1.80% by mass of Mn, a Cu content of 0.20% by mass or less (inclusive of 0.00% by mass), a Zn content of 6.00% by mass or less (inclusive of 0.00% by mass), and optionally containing one or more of 0.08% by mass or less of Mg, 0.30% by mass or less of Ti, 0.30% by mass or less of Zr, 0.30% by mass or less of Cr, 0.30% by mass or less of V, 0.10% by mass or less of Be, 0.10% by mass or less of Sr, 0.30% by mass or less of Bi, 0.10% by mass or less of Na, and 0.05% by mass or less of Ca, with the remainder being Al and unavoidable impurities; After a heating test in which the temperature is raised from 300°C to 400°C at an average heating rate of 60°C / min or less and held at 600±3°C for 5±3 minutes, the area with one or more grain boundaries in the thickness direction in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction accounts for 25% or more but less than 90% of the area in the width direction, and the average grain size in the direction perpendicular to the rolling direction on the sheet surface is 950μm or less. The present invention provides an aluminum alloy sheet characterized by the above.
[0012] The present invention (2) provides an aluminum alloy sheet according to (1), characterized in that, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test, regions having two or more grain boundaries in the sheet thickness direction are present in a proportion of 3% or more in the width direction.
[0013] The present invention (3) provides an aluminum alloy sheet according to (1) or (2), characterized in that, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test, the maximum width of a region having no grain boundaries in the sheet thickness direction is 2000 μm or less.
[0014] The present invention (4) also provides an aluminum alloy sheet according to (1) or (2), characterized in that the sheet thickness is 0.08 mm or less.
[0015] The present invention (5) also provides an aluminum alloy sheet according to (3), characterized in that the sheet thickness is 0.08 mm or less.
[0016] The present invention (6) is directed to a steel sheet produced by continuous casting and rolling, which contains 2.00 to 3.00% by mass of Si, 0.05 to 0.40% by mass of Fe, and 0.80 to 1.80% by mass of Mn, has a Cu content of 0.20% by mass or less (including 0.00% by mass), a Zn content of 6.00% by mass or less (including 0.00% by mass), and optionally contains 0.08% by mass or less of Mg, 0.30% by mass or less of Ti, 0.30% by mass or less of Zr, 0.30% by mass or less of Zr, and 0.30% by mass or less of Mg. a casting step of casting a cast-rolled sheet of an aluminum alloy comprising an aluminum alloy containing any one or two or more of 0.30% by mass or less of Cr, 0.30% by mass or less of V, 0.10% by mass or less of Be, 0.10% by mass or less of Sr, 0.30% by mass or less of Bi, 0.10% by mass or less of Na, and 0.05% by mass or less of Ca, with the balance being Al and unavoidable impurities, at a casting speed of more than 0.50 m / min and less than 0.70 m / min; a cold rolling step of cold rolling the cast-rolled sheet two or more times; and Annealing is performed at least once between the casting process and the final cold rolling in the cold rolling process. The annealing conditions for all annealing treatments are an annealing temperature of 200 to 550°C and an annealing time of 1 to 10 hours. The present invention provides a method for producing an aluminum alloy sheet, characterized by the above.
[0017] The present invention (7) is a heat exchanger having tubes made of an aluminum alloy through which a working fluid flows, and fins made of an aluminum alloy metallically joined to the tubes, The tube is formed using a heat exchanger tube material made of an aluminum alloy, the fin is made of an aluminum alloy containing 2.00 to 3.00% by mass of Si, 0.05 to 0.40% by mass of Fe, and 0.80 to 1.80% by mass of Mn, a Cu content of 0.20% by mass or less (inclusive of 0.00% by mass), a Zn content of 6.00% by mass or less (inclusive of 0.00% by mass), and optionally containing one or more of 0.08% by mass or less of Mg, 0.30% by mass or less of Ti, 0.30% by mass or less of Zr, 0.30% by mass or less of Cr, 0.30% by mass or less of V, 0.10% by mass or less of Be, 0.10% by mass or less of Sr, 0.30% by mass or less of Bi, 0.10% by mass or less of Na, and 0.05% by mass or less of Ca, with the remainder being Al and unavoidable impurities, and is formed using an aluminum alloy plate having a function of being heat-bonded in a single layer; In a cross section of the fin perpendicular to the rolling surface and perpendicular to the rolling direction, the area having one or more crystal grain boundaries in the thickness direction accounts for 25% or more and less than 90% in the width direction, and the average crystal grain size in the direction perpendicular to the rolling direction on the plate surface is 950 μm or less; The present invention provides a heat exchanger characterized by the above.
[0018] The present invention (8) provides a heat exchanger according to (7), characterized in that in a cross section of the fin perpendicular to the rolling surface and perpendicular to the rolling direction, regions with two or more grain boundaries in the thickness direction are present in a proportion of 3% or more in the width direction.
[0019] The present invention (9) provides a heat exchanger according to (7) or (8), characterized in that in a cross section of the fin perpendicular to the rolling surface and perpendicular to the rolling direction, the maximum width of a region with no grain boundaries in the thickness direction is 2000 μm or less.
[0020] The present invention (10) is a heat exchanger having tubes made of an aluminum alloy through which a working fluid flows, and fins made of an aluminum alloy metallically joined to the tubes, The heat exchanger is obtained by combining at least a heat exchanger tube material made of an aluminum alloy with a heat exchanger fin material made of an aluminum alloy, then heating the resulting combination to bond the heat exchanger tube material and the heat exchanger fin material, and the heat exchanger fin material is a molded body of an aluminum alloy plate according to any one of (1) to (5). The present invention provides a heat exchanger characterized by the above. [Effects of the Invention]
[0021] According to the present invention, it is possible to provide an aluminum alloy sheet that has excellent brazability while ensuring material strength when producing various aluminum alloy structures. [Brief explanation of the drawings]
[0022] [Figure 1] This is a schematic phase diagram of an Al-Si alloy, which is a typical binary eutectic alloy. [Figure 2] FIG. 2 is an explanatory diagram showing a mechanism for generating a liquid phase in an aluminum alloy forming an aluminum alloy plate according to the present invention, in joining using the aluminum alloy according to the present invention. [Figure 3] FIG. 2 is an explanatory diagram showing a mechanism for generating a liquid phase in an aluminum alloy forming an aluminum alloy plate according to the present invention, in joining using the aluminum alloy according to the present invention. [Figure 4] This is a schematic phase diagram of an Al-Si alloy, a typical binary eutectic crystal. [Figure 5] FIG. 10 is a diagram showing an example of measurement of a cross-sectional grain boundary. [Figure 6] FIG. 10 is a diagram showing an example of measurement of a cross-sectional grain boundary. [Figure 7] FIG. 1 is a diagram showing an example of measuring the average crystal grain size on the surface of a plate. DETAILED DESCRIPTION OF THE INVENTION
[0023] The aluminum alloy plate of the present invention is an aluminum alloy plate having a function of being heat-bonded in a single layer, an aluminum alloy containing 2.00 to 3.00% by mass of Si, 0.05 to 0.40% by mass of Fe, and 0.80 to 1.80% by mass of Mn, a Cu content of 0.20% by mass or less (inclusive of 0.00% by mass), a Zn content of 6.00% by mass or less (inclusive of 0.00% by mass), and optionally containing one or more of 0.08% by mass or less of Mg, 0.30% by mass or less of Ti, 0.30% by mass or less of Zr, 0.30% by mass or less of Cr, 0.30% by mass or less of V, 0.10% by mass or less of Be, 0.10% by mass or less of Sr, 0.30% by mass or less of Bi, 0.10% by mass or less of Na, and 0.05% by mass or less of Ca, with the remainder being Al and unavoidable impurities; After a heating test in which the temperature is raised from 300°C to 400°C at an average heating rate of 60°C / min or less and held at 600±3°C for 5±3 minutes, the area with one or more grain boundaries in the thickness direction in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction accounts for 25% or more but less than 90% of the area in the width direction, and the average grain size in the direction perpendicular to the rolling direction on the sheet surface is 950μm or less. The aluminum alloy plate is characterized by the following.
[0024] The aluminum alloy sheet of the present invention contains Si, Fe, and Mn as essential elements, and is composed of the essential elements, optional elements added as needed, and aluminum and unavoidable impurities as the balance.
[0025] The aluminum alloy sheet of the present invention is made of an aluminum alloy containing 2.00 to 3.00 mass% Si, 0.05 to 0.40 mass% Fe, 0.80 to 1.80 mass% Mn, and the remainder being Al and unavoidable impurities. That is, the aluminum alloy sheet of the present invention is made of an aluminum alloy.
[0026] The aluminum alloy according to the aluminum alloy sheet of the present invention may further contain, as optional additive elements, 0.20 mass% or less of Cu and 6.00 mass% or less of Zn. That is, in the aluminum alloy according to the aluminum alloy sheet of the present invention, the Cu content is 0.00 to 0.20 mass%, and the Zn content is 0.00 to 6.00 mass%.
[0027] The aluminum alloy according to the present invention may further contain, as optional additional elements, one or more of 0.08% by mass or less of Mg, 0.30% by mass or less of Ti, 0.30% by mass or less of Zr, 0.30% by mass or less of Cr, 0.30% by mass or less of V, 0.10% by mass or less of Be, 0.10% by mass or less of Sr, 0.30% by mass or less of Bi, 0.10% by mass or less of Na, and 0.05% by mass or less of Ca. The aluminum alloy according to the present invention may also contain, as optional additional elements, 0.10% by mass or less of In, 0.10% by mass or less of Sn, and 0.10% by mass or less of rare earth elements.
[0028] Si is an element that generates an Al-Si liquid phase and contributes to bonding. The Si content of the aluminum alloy according to the present invention is 2.00 to 3.00 mass%, preferably 2.10 to 2.80 mass%, and more preferably 2.20 to 2.60 mass%. When the Si content of the aluminum alloy is within the above range, a sufficient amount of liquid phase can be generated, and the liquid phase seeps out in sufficient amount, resulting in good bonding. Furthermore, when the Si content of the aluminum alloy is within the above range, the temperature difference between the solidus and liquidus of the aluminum alloy increases, thereby lengthening the time until solidification is complete near the center of the plate thickness during casting. As a result, solute atoms are expelled from the surface to the center, and the higher concentration of solute atoms results in the dense presence of second-phase particles. This inhibits grain growth in the center of the plate thickness, increasing the number of grains in the plate thickness direction during thermal bonding, thereby suppressing deformation due to grain boundary sliding. Since the amount of liquid phase that seeps out increases with increasing plate thickness and heating temperature, the amount of liquid phase required during heat bonding is adjusted according to the structure or dimensions of the fins of the heat exchanger to be manufactured. The Si content of the aluminum alloy and the heat bonding temperature are then adjusted according to the amount of liquid phase required during heat bonding. On the other hand, if the Si content of the aluminum alloy is below the above range, a sufficient amount of liquid phase cannot be generated, resulting in less liquid phase seepage and incomplete bonding. On the other hand, if the Si content of the aluminum alloy is above the above range, the amount of melting of the aluminum alloy material during brazing increases, which may result in a decrease in the strength of the aluminum alloy material. As a result, the sag resistance of the aluminum alloy material may decrease, and the aluminum alloy material may be more likely to deform or buckle due to its own weight during brazing.
[0029] Fe not only improves strength by dissolving in the matrix to a certain extent, but also disperses as crystallized or precipitated substances, preventing strength degradation, particularly at high temperatures. The Fe content of the aluminum alloy according to the present invention is 0.05 to 0.40 mass%, preferably 0.08 to 0.35 mass%. The Fe content of the aluminum alloy within this range increases strength and prevents strength degradation at high temperatures. On the other hand, if the Fe content of the aluminum alloy is less than this range, not only is the above effect small, but high-purity metal must be used, increasing costs. Furthermore, if the Fe content of the aluminum alloy exceeds this range, coarse intermetallic compounds are formed during casting, causing problems with manufacturability, and the joined body will have reduced corrosion resistance when exposed to a corrosive environment (especially a corrosive environment where liquid flows). Furthermore, the recrystallized grains will become finer due to heating during joining, resulting in reduced deformation resistance.
[0030] Mn dissolves in the aluminum matrix during casting, promoting the formation of Al-based intermetallic compounds with equivalent circle diameters of 0.01 to 0.50 μm in subsequent processing steps. The Mn content of the aluminum alloy according to the present invention is 0.80 to 1.80 mass%, preferably 1.00 to 1.60 mass%. When the Mn content of the aluminum alloy is within the above range, a sufficient amount of Al-based intermetallic compounds with equivalent circle diameters of 0.01 to 0.50 μm is present, providing a pinning effect with appropriate strength, and only limited crystal grains grow, resulting in coarse crystal grains. The coarse crystal grains suppress grain boundary sliding, thereby improving deformation resistance. On the other hand, if the Mn content of the aluminum alloy is below the above range, the above effect is not sufficiently achieved, resulting in reduced deformation resistance. Conversely, if the Mn content exceeds the above range, coarse intermetallic compounds are formed during casting, causing problems with manufacturability.
[0031] The aluminum alloy according to the present invention may contain, in addition to Si, Fe, and Mn, one or more of Cu, Zn, Mg, Ti, Zr, Cr, V, Be, Sr, Bi, Na, Ca, In, Sn, and rare earth elements as optional additive elements, as needed.
[0032] Cu is an additive element that dissolves in the matrix to improve strength. When the aluminum alloy according to the aluminum alloy sheet of the present invention contains Cu, the Cu content of the aluminum alloy according to the aluminum alloy sheet of the present invention is 0.20 mass% or less, preferably 0.01 to 0.18 mass%. When the Cu content of the aluminum alloy is within the above range, the strength is increased. On the other hand, when the Cu content of the aluminum alloy exceeds the above range, the corrosion resistance is reduced.
[0033] Zn is an element effective in improving corrosion resistance through sacrificial protection. Zn dissolves almost uniformly in the matrix to lower the self-potential. For example, by using the aluminum alloy material of the present invention as a fin material and lowering the self-potential, a sacrificial protection effect can be exhibited, which relatively suppresses corrosion of the tubes joined to the fin. When the aluminum alloy according to the aluminum alloy sheet of the present invention contains Zn, the Zn content of the aluminum alloy according to the aluminum alloy sheet of the present invention is 6.00 mass% or less, preferably 0.05 to 6.00 mass%, and particularly preferably 0.10 to 5.00 mass%. When the Zn content of the aluminum alloy is within the above range, the corrosion resistance is increased. On the other hand, when the Zn content of the aluminum alloy exceeds the above range, the corrosion rate becomes too high, resulting in a decrease in self-corrosion resistance and a decrease in sacrificial protection.
[0034] After heat bonding, Mg becomes Mg2Si, which causes age hardening and improves strength. Therefore, Mg is an additive element that exhibits the effect of improving strength. When the aluminum alloy according to the aluminum alloy sheet of the present invention contains Mg, the Mg content of the aluminum alloy according to the aluminum alloy sheet of the present invention is 0.08 mass% or less, preferably 0.005 to 0.07 mass%. If the Mg content of the aluminum alloy exceeds the above range, Mg reacts with the flux to form a compound with a high melting point, resulting in poor bondability. Note that in the present invention, when referring to Mg and not only Mg but also other alloy components, "a predetermined content or less" is intended to include 0 mass%.
[0035] Cr improves strength through solid solution strengthening, and also precipitates Al-Cr intermetallic compounds, which act to coarsen crystal grains after heating. When the aluminum alloy according to the aluminum alloy sheet of the present invention contains Cr, the Cr content of the aluminum alloy according to the aluminum alloy sheet of the present invention is 0.30 mass% or less, preferably 0.05 to 0.30 mass%. When the Cr content of the aluminum alloy is within the above range, the strength is increased. On the other hand, when the Cr content of the aluminum alloy exceeds the above range, coarse intermetallic compounds are easily formed, and the plastic workability is reduced.
[0036] Zr precipitates as an Al-Zr intermetallic compound and exerts the effect of improving the strength after heat bonding by dispersion strengthening. When the aluminum alloy according to the aluminum alloy sheet of the present invention contains Zr, the Zr content of the aluminum alloy according to the aluminum alloy sheet of the present invention is 0.30 mass% or less, preferably 0.05 to 0.30 mass%. When the Zr content of the aluminum alloy is within the above range, the strength is increased. On the other hand, when the Zr content of the aluminum alloy exceeds the above range, coarse intermetallic compounds are easily formed, and the plastic workability is reduced.
[0037] Ti and V not only improve strength by dissolving in the matrix, but also have the effect of preventing corrosion from progressing in the thickness direction by distributing in layers. When the aluminum alloy according to the aluminum alloy sheet of the present invention contains Ti, the Ti content of the aluminum alloy according to the aluminum alloy sheet of the present invention is 0.30 mass% or less, preferably 0.05 to 0.30 mass%. When the aluminum alloy contains V, the V content of the aluminum alloy according to the aluminum alloy sheet of the present invention is 0.30 mass% or less, preferably 0.05 to 0.30 mass%. When the Ti content or V content of the aluminum alloy is within the above range, the strength is increased and corrosion progression in the thickness direction can be prevented. On the other hand, when the Ti content or V content of the aluminum alloy exceeds the above range, large crystals are generated, which impairs formability and corrosion resistance.
[0038] Be, Sr, Bi, Na, and Ca can improve bondability by finely dispersing Si particles and improving the fluidity of the liquid phase. When the aluminum alloy according to the present invention contains Be, the Be content of the aluminum alloy according to the present invention is 0.10% by mass or less, preferably 0.0001 to 0.10% by mass. When the aluminum alloy according to the present invention contains Sr, the Sr content of the aluminum alloy according to the present invention is 0.10% by mass or less, preferably 0.0001 to 0.10% by mass. When the aluminum alloy according to the present invention contains Bi, the Bi content of the aluminum alloy according to the present invention is 0.30% by mass or less, preferably 0.0001 to 0.30% by mass. When the aluminum alloy according to the present invention contains Na, the Na content of the aluminum alloy according to the present invention is 0.10% by mass or less, preferably 0.0001 to 0.10% by mass. Furthermore, when the aluminum alloy according to the present invention contains Ca, the Ca content of the aluminum alloy according to the present invention is 0.05% by mass or less, preferably 0.0001 to 0.05% by mass. When the Be content, Sr content, Bi content, Na content, or Ca content of the aluminum alloy is within the above range, the joinability is improved. On the other hand, when the Be content, Sr content, Bi content, Na content, or Ca content of the aluminum alloy exceeds the above range, adverse effects such as reduced corrosion resistance may occur. When the aluminum alloy contains one or more of Be, Sr, Bi, Na, and Ca, it is necessary that each of the additional elements is within the above range. Furthermore, the aluminum alloy according to the present invention may contain 0.10% by mass or less of In, 0.10% by mass or less of Sn, and 0.10% by mass or less of rare earth elements.
[0039] In a heating test in which the aluminum alloy sheet of the present invention is heated from 300°C to 400°C at an average heating rate of 60°C / min or less and held at 600±3°C for 5±3 minutes, the heating test is preferably performed at an average heating rate of 60°C / min or less, preferably 45°C / min or less, from 300°C to 400°C, from 400°C to 580°C in 8±3 minutes, from 580°C to the holding temperature in 8±3 minutes, and held at 600±3°C for 5±3 minutes, the aluminum alloy sheet of the present invention has the following characteristics: in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test, the proportion of regions having one or more grain boundaries in the sheet thickness direction is 25% or more but less than 90%, preferably 30 to 85%, more preferably 35 to 80%, in the width direction; and the average grain size in the direction perpendicular to the rolling direction on the sheet surface is 950μm or less, preferably 200 to 900μm, more preferably 300 to 850μm. That is, the aluminum alloy sheet of the present invention is heated by heating from 300°C to 400°C at an average heating rate of 60°C / min or less, and holding at 600±3°C for 5±3 minutes, preferably by heating from 300°C to 400°C at an average heating rate of 60°C / min or less, preferably 45°C / min or less, heating from 400°C to 580°C in 8±3 minutes, heating from 580°C to the holding temperature in 8±3 minutes, and holding at 600±3°C for 5±3 minutes. As a result, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test, the area with one or more grain boundaries in the thickness direction of the sheet accounts for 25% or more but less than 90%, preferably 30 to 85%, more preferably 35 to 80%, in the width direction, and the metal structure has an average grain size in the direction perpendicular to the rolling direction on the sheet surface of 950 μm or less, preferably 200 to 900 μm, more preferably 300 to 850 μm.The present inventors have found that an aluminum alloy sheet having a metal structure in which the grain boundaries in the sheet thickness direction are within the above range in a cross section perpendicular to the rolling surface and perpendicular to the rolling direction and the average crystal grain size in the direction perpendicular to the rolling direction on the sheet surface are within the above range, can ensure both material strength and brazeability in single-layer heat joining by heating the sheet at a temperature increase from 300°C to 400°C at an average temperature increase rate of 60°C / min or less and holding at 600±3°C for 5±3 minutes, preferably at an average temperature increase rate of 60°C / min or less, and preferably at 45°C / min or less, heating the sheet at a temperature increase from 400°C to 580°C in 8±3 minutes, heating the sheet at 580°C to the holding temperature in 8±3 minutes, and holding at 600±3°C for 5±3 minutes.
[0040] In a heating test in which the aluminum alloy sheet of the present invention is heated from 300°C to 400°C at an average heating rate of 60°C / min or less and held at 600±3°C for 5±3 minutes, the aluminum alloy sheet is heated from 300°C to 400°C preferably at an average heating rate of 60°C / min or less, preferably 45°C / min or less, heated from 400°C to 580°C in 8±3 minutes, heated from 580°C to the holding temperature in 8±3 minutes, and held at 600±3°C for 5±3 minutes, the aluminum alloy sheet of the present invention has, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test, a region having one or more grain boundaries in the sheet thickness direction, which accounts for 25% or more but less than 90%, preferably 30 to 85%, more preferably 35 to 80% in the width direction. In the aluminum alloy sheet of the present invention, there are many flow paths for the liquid phase exuded from the base metal, i.e., grain boundaries. In the aluminum alloy sheet of the present invention, the number of liquid phase flow paths is increased, thereby enabling an increase in fillet area. Therefore, in a heating test in which the temperature is increased from 300°C to 400°C at an average heating rate of 60°C / min or less and then held at 600±3°C for 5±3 minutes, preferably in which the temperature is increased from 300°C to 400°C at an average heating rate of 60°C / min or less, preferably 45°C / min or less, the temperature is increased from 400°C to 580°C in 8±3 minutes, the temperature is increased from 580°C to the holding temperature in 8±3 minutes, and then the temperature is held at 600±3°C for 5±3 minutes, if the region with one or more grain boundaries in the sheet thickness direction in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test falls within the above range, the number of liquid phase flow paths is increased, enabling an increase in fillet area. Since it is extremely difficult to observe the number of grain boundaries in the thickness direction of the plate cross section during heating, the judgment is made based on the number of grain boundaries in the thickness direction of the plate cross section after heating.
[0041] In a heating test in which the aluminum alloy sheet of the present invention is heated from 300°C to 400°C at an average heating rate of 60°C / min or less and held at 600±3°C for 5±3 minutes, the heating test is preferably performed at an average heating rate of 60°C / min or less, preferably 45°C / min or less, from 300°C to 400°C, from 400°C to 580°C in 8±3 minutes, from 580°C to the holding temperature in 8±3 minutes, and held at 600±3°C for 5±3 minutes, the average crystal grain size in the direction perpendicular to the rolling direction on the sheet surface after the heating test is 950 μm or less, preferably 900 μm or less, more preferably 850 μm or less. Finer crystal grain sizes result in more liquid phase flow paths, and therefore the fillet area can be increased. Therefore, in a heating test in which the temperature is increased from 300°C to 400°C at an average heating rate of 60°C / min or less and held at 600±3°C for 5±3 minutes, preferably at an average heating rate of 60°C / min or less, and preferably at 45°C / min or less, from 300°C to 400°C, the temperature is increased from 400°C to 580°C in 8±3 minutes, the temperature is increased from 580°C to the holding temperature in 8±3 minutes, and the temperature is held at 600±3°C for 5±3 minutes, if the average crystal grain size in the direction perpendicular to the rolling direction on the sheet surface after the heating test falls within the above range, the fillet area can be increased. Note that, since it is extremely difficult to observe the average crystal grain size during heating, the judgment is based on the average crystal grain size after heating.
[0042] Furthermore, in a heating test in which the aluminum alloy sheet of the present invention is heated from 300°C to 400°C at an average heating rate of 60°C / min or less and held at 600±3°C for 5±3 minutes, the heating test is preferably performed at an average heating rate of 60°C / min or less, preferably 45°C / min or less, from 300°C to 400°C, from 400°C to 580°C in 8±3 minutes, from 580°C to the holding temperature in 8±3 minutes, and held at 600±3°C for 5±3 minutes, the average crystal grain size in the direction perpendicular to the rolling direction on the sheet surface after the heating test is preferably 200 μm or more, more preferably 300 μm or more. If the crystal grain size is too small, grain boundary sliding and a significant decrease in material strength occur. Therefore, in a heating test in which the temperature is increased from 300°C to 400°C at an average heating rate of 60°C / min or less and then held at 600±3°C for 5±3 minutes, preferably in which the temperature is increased from 300°C to 400°C at an average heating rate of 60°C / min or less, preferably 45°C / min or less, the temperature is increased from 400°C to 580°C in 8±3 minutes, the temperature is increased from 580°C to the holding temperature in 8±3 minutes, and then the temperature is held at 600±3°C for 5±3 minutes, an aluminum alloy plate having an average crystal grain size in the direction perpendicular to the rolling direction on the plate surface after the heating test that falls within the above range is unlikely to experience grain boundary sliding or a significant decrease in material strength.
[0043] In the aluminum alloy sheet of the present invention, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after a heating test, regions with two or more grain boundaries in the sheet thickness direction are present in a proportion of 3% or more, preferably 5% or more in the width direction. When the regions with two or more grain boundaries exist in the above range, the number of flow paths for the liquid phase exuding from the base material increases, resulting in excellent brazability.
[0044] In the aluminum alloy sheet of the present invention, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after a heating test, the maximum width of a region with no grain boundaries in the sheet thickness direction is 2000 μm or less, preferably 1800 μm or less. When the region with no grain boundary crystals is in the above range, the number of flow paths for the liquid phase seeping out from the base material increases, resulting in excellent brazability.
[0045] In the present invention, the heating test involves increasing the temperature from 300°C to 400°C at an average heating rate of 60°C / min or less and holding at 600±3°C for 5±3 minutes, preferably increasing the temperature from 300°C to 400°C at an average heating rate of 60°C / min or less, preferably 45°C / min or less, increasing the temperature from 400°C to 580°C in 8±3 minutes, increasing the temperature from 580°C to the holding temperature in 8±3 minutes, and holding at 600±3°C for 5±3 minutes. First, the aluminum alloy sheet of the present invention, which is a test sample, is subjected to the heating test under the above heating conditions in an inert gas atmosphere. Then, for the test sample after the heating test, the number of grain boundaries in the plate thickness direction in a cross section perpendicular to the rolling surface and perpendicular to the rolling direction and the average grain size in the plate surface perpendicular to the rolling direction are measured. The heating conditions for the heating test were to increase the temperature from 300°C to 400°C at an average rate of 60°C / min or less, and then increase the temperature to 600°C, preferably to increase the temperature from 300°C to 400°C at an average rate of 60°C / min or less, preferably 45°C / min or less, to increase the temperature from 400°C to 580°C in 8±3 minutes, and then to increase the temperature from 580°C to the holding temperature in 8±3 minutes.
[0046] In the present invention, the number of grain boundaries in the thickness direction in a cross section perpendicular to the rolling surface and the rolling direction is measured as follows. Specifically, a sample after brazing heating is cut in a direction perpendicular to the rolling surface and the rolling direction, embedded in resin, and mirror-polished. The polished embedded resin is then immersed in the SWAAT test solution for 12 hours. The resin surface is then lightly polished to remove any dirt. This process corrodes the grain boundaries to make them easier to identify. Next, the cross-sectional structure is photographed at 200x magnification using a microscope for metallographic observation. In the photographed cross-section, regions with one or more grain boundaries are framed, the widthwise length of each framed portion is determined, and the total length of all framed portions is divided by the total widthwise length of the photographed cross section to calculate the proportion (percentage) of regions with one or more grain boundaries. In addition, for the photographed cross-sectional image, regions with two or more grain boundaries were framed, the widthwise length of each framed portion was determined, and the sum of all framed lengths was divided by the total widthwise length of the photographed cross-section to calculate the proportion (percentage) of regions with two or more grain boundaries. Furthermore, the widthwise length of the longest region with zero grain boundaries, i.e., the region not framed as one or more grain boundaries, was measured, and this was calculated as the maximum width of the region with zero grain boundaries in the thickness direction. The number of grain boundaries in the thickness direction refers to the number of grain boundary lines of crystal grains that intersect with a line drawn in the thickness direction (perpendicular to the rolling surface) on the photographed cross-section.
[0047] FIG. 5 shows an example of measuring grain boundaries in the cross section of an aluminum alloy sheet of the present invention. In FIG. 5, FIG. 5A is a micrograph of the cross section before image processing, and FIG. 5B is a diagram in which the micrograph of FIG. 5A has been image processed, with the grain boundaries indicated by black lines. In FIG. 5B, the grain boundaries are indicated by black lines, and regions with one or more grain boundaries in the sheet thickness direction are surrounded by white frames. In the example of FIG. 5B, there are three regions with one or more grain boundaries in the sheet thickness direction. Then, the widthwise length of each framed region, which is a region with one or more grain boundaries in the sheet thickness direction, is measured. Next, the widthwise lengths of the framed regions with one or more grain boundaries in the sheet thickness direction that exist in the entire photographed region are added together, and the sum is calculated using the following formula: Percentage of areas with one or more grain boundaries in the thickness direction (%) = ((Total width of the framed areas with one or more grain boundaries in the thickness direction that exist in the entire photographed area) / (Total length of the photographed area)) × 100 In addition, in Fig. 5A, the unframed areas are regions with zero or more crystal grain boundaries in the thickness direction, and the width direction length of the region with the longest width direction length among the unframed regions present in the entire photographed region (the length indicated by the white double arrow in Fig. 5A) is defined as the maximum width of the region with zero crystal grain boundaries in the thickness direction.
[0048] FIG. 6 shows an example of measuring grain boundaries in the cross section of an aluminum alloy sheet of the present invention. In FIG. 6, FIG. 6A is a micrograph of the cross section before image processing, and FIG. 6B is a diagram in which the micrograph of FIG. 6A has been image processed, with the grain boundaries indicated by black lines. In FIG. 6B, regions with two or more grain boundaries in the sheet thickness direction are surrounded by white frames, and in the example of FIG. 6B, there are two regions with two or more grain boundaries in the sheet thickness direction. Then, the widthwise length of each framed region representing a region with two or more grain boundaries in the sheet thickness direction was measured. Next, the widthwise lengths of the framed regions with two or more grain boundaries in the sheet thickness direction that exist in the entire photographed region were added together, and the sum was calculated using the following formula: Percentage of areas with two or more grain boundaries in the plate thickness direction (%) = ((Total width of the framed areas with two or more grain boundaries in the plate thickness direction that exist in the entire photographed area) / (Total length of the photographed area)) × 100 Calculated as follows.
[0049] In the present invention, the average crystal grain size in the direction perpendicular to the rolling direction on the sheet surface is measured as follows. That is, a sample after brazing heating is cut into 20 mm × 30 mm, and the sheet surface is polished and chamfered to expose the center of the sheet thickness. Next, mirror polishing and parker etching are performed, and polarized observation is performed using a metallurgical microscope. Six fields of view are photographed at 20x magnification, and the crystal structure is observed in a connected manner for each of the six fields of view at 20x magnification (observation is performed parallel to the rolling direction). Ten 6 mm lines are drawn perpendicular to the rolling direction at 1 mm intervals, and the number of crystal grains on the 10 lines is counted, and the total number of crystal grains is measured and calculated using the following formula: Average grain size (μm) = (6000 × 10) / total number of grains on 10 lines The average crystal grain size is calculated using the above formula.
[0050] Figure 7 shows an example of measuring the average crystal grain size on the surface of an aluminum alloy sheet of the present invention. As shown in Figure 7, ten 6 mm lines are drawn perpendicular to the rolling direction at 1 mm intervals. Next, the number of crystal grains on each of the ten lines is counted. The total number of crystal grains on each of the ten lines is then measured and calculated using the following formula: Average grain size (μm) = (6000 × 10) / total number of grains on 10 lines The average crystal grain size is calculated using the formula: In Fig. 7, the crystals near the center on each line are indicated by black circles. The numbers above each line in Fig. 7 indicate the line number, and the numbers below each line indicate the number of crystal grains on each line.
[0051] The thickness of the aluminum alloy sheet of the present invention is preferably 0.08 mm or less. A thickness of 0.08 mm or less is suitable for use as a fin material for a heat exchanger. The aluminum alloy sheet of the present invention has excellent deformation resistance even when the thickness is as small as 0.08 mm or less.
[0052] The aluminum alloy sheet of the present invention is an aluminum alloy sheet having a function of single-layer thermal bonding at a temperature at which the liquid phase ratio is 5.0% or more and 35.0% or less (aluminum alloy sheet having a single-layer thermal bonding function). In other words, the aluminum alloy sheet of the present invention is a single-layer brazing sheet.
[0053] An aluminum alloy sheet (hereinafter also referred to as a single-layer brazing sheet) having a function of heat-bonding in a single layer at a temperature where the liquid phase ratio is 5.0% or more and 35.0% or less will be described below.
[0054] A single-layer brazing sheet must be bonded at a temperature where the ratio of the mass of the liquid phase generated in the aluminum alloy material to the total mass of the aluminum alloy material (hereinafter referred to as the "liquid phase ratio") is 5% or more and 35% or less. If the liquid phase ratio exceeds 35%, the amount of liquid phase generated is too large, and the aluminum alloy material cannot maintain its shape, resulting in significant deformation. On the other hand, if the liquid phase ratio is less than 5%, bonding becomes difficult. The liquid phase ratio is preferably 5 to 30%, and more preferably 10 to 20%.
[0055] The mechanism of liquid phase formation is explained below. Figure 1 shows a schematic diagram of an Al-Si alloy, a typical binary eutectic alloy. When an aluminum alloy with a Si concentration of c1 is heated, liquid phase formation begins at a temperature T1 near the eutectic temperature (solidus temperature) Te. Below the eutectic temperature Te, as shown in Figure 2(a), crystal precipitates are distributed in the matrix separated by grain boundaries. When liquid phase formation begins, as shown in Figure 2(b), the grain boundaries with high segregation of crystal precipitates melt and become liquid, as shown in Figure 2(c). Next, as shown in Figure 2(c), the crystal precipitate particles and intermetallic compounds of Si, the main additive element dispersed in the aluminum alloy matrix, melt into spherical liquid phases. Furthermore, as shown in Figure 2(d), these spherical liquid phases redissolve into the matrix over time and temperature due to interfacial energy and migrate to the grain boundaries and surface by solid-phase diffusion. Next, as the temperature increases to T2 as shown in Figure 1, the amount of liquid increases according to the phase diagram. As shown in Figure 1, in the case of c2, where the Si concentration of one aluminum alloy material is lower than the maximum solubility limit, liquid phase formation begins near the solidus temperature Ts2. However, unlike in the case of c1, the structure immediately before melting may not contain any crystal precipitates in the matrix, as shown in Figure 3(a). In this case, as shown in Figure 3(b), the grain boundaries first melt and become liquid, and then, as shown in Figure 3(c), liquid phases emerge from areas of locally high solute element concentration in the matrix. As shown in Figure 3(d), the spherical liquid phases formed in the matrix, as in the case of c1, redissolve into the matrix over time and with increasing temperature due to interfacial energy and then migrate to the grain boundaries and surface by solid-phase diffusion. When the temperature rises to T3, the amount of liquid phase increases according to the phase diagram. Thus, the bonding in the present invention utilizes the liquid phase generated by partial melting within the single-layer brazing sheet (the heat exchanger fin material of the present invention), achieving both bonding and shape retention.
[0056] The behavior of the metallurgical structure from the time the liquid phase is generated until the joining is complete is explained. A single-layer brazing sheet that generates a liquid phase is combined with the aluminum alloy mating material to be joined, and then heated to a temperature where the liquid phase ratio is 5.0% to 35.0%. Microscopic observation of the joint reveals that, as mentioned above, the very small amount of liquid generated on the surface of the single-layer brazing sheet fills the gap between the aluminum alloy mating material and the single-layer brazing sheet, where the oxide film has been destroyed by the action of flux, etc. Next, the liquid phase near the joining interface between the two alloy materials migrates into the aluminum alloy mating material. As a result, the solid α-phase crystal grains of the single-layer brazing sheet in contact with the joining interface grow toward the aluminum alloy mating material. Meanwhile, the crystal grains of the aluminum alloy mating material also grow toward the single-layer brazing sheet. The resulting structure is such that the single-layer brazing sheet is embedded in the aluminum alloy mating material near the joining interface, resulting in a joining process. Therefore, no metallurgical structure other than that of the single-layer brazing sheet and the aluminum alloy mating material is present at the joining interface.
[0057] On the other hand, when a brazing sheet clad with a brazing filler metal is used to join an aluminum alloy mating material by brazing heat, a fillet is formed at the joint, and a eutectic structure is observed, resulting in a joint structure that is different from that formed when a single-layer brazing sheet is used to join an aluminum alloy mating material by brazing heat. In other words, when a brazing sheet clad with a brazing filler metal is used to join an aluminum alloy mating material by brazing heat, the liquid phase brazing fills the joint and forms a fillet, resulting in a eutectic structure at the joint that is different from the surrounding area. Furthermore, when a welding method is used, the joint melts locally, resulting in a metal structure that is different from that of other parts.
[0058] For this reason, when a single-layer brazing sheet is used to heat-bond an aluminum alloy mating material, the metal structure of the bonded portion is composed only of those of both joined materials, or is composed of both joined materials integrated together, which means that the bonded structure differs from that when a brazing sheet clad with a filler metal is used or when welding is used.
[0059] Because of this joining behavior, when a single-layer brazing sheet is used to heat-bond an aluminum alloy mating material, almost no deformation occurs near the bonded area after the bonding process. In other words, when a single-layer brazing sheet is used to heat-bond an aluminum alloy mating material, almost no deformation occurs after bonding, such as the bead formed in welding or the fillet formed in brazing. Nevertheless, it allows for metallurgical bonding, similar to welding and brazing. For example, when a drawn cup-type stacked heat exchanger is assembled using a brazing sheet clad with brazing material (with a brazing material cladding ratio of 5% on each side), the molten brazing material concentrates at the joint after brazing heating, reducing the height of the stacked heat exchanger by 5–10%. Therefore, this reduction must be taken into account in product design. In contrast, when a single-layer brazing sheet is used to heat-bond an aluminum alloy mating material, dimensional change after bonding is extremely small, enabling high-precision product design.
[0060] In the present invention, it is extremely difficult to measure the actual liquid phase ratio during heating of a single-layer brazing sheet. Therefore, the liquid phase ratio specified in the present invention is determined by equilibrium calculation. Specifically, it is calculated from the alloy composition and the maximum temperature reached during heating using thermodynamic equilibrium calculation software such as Thermo-Calc (registered trademark) manufactured by Thermo-Calc Software AB.
[0061] The relationship between the liquidus fraction and temperature will be explained based on the phase diagram shown in Figure 4. Figure 4 is a modified version of Figure 1. In Figure 4, the line extending parallel to the horizontal axis through temperature Te (hereinafter referred to as "solidus 1") and the line extending from the left end of solidus 1 to 660°C on the vertical axis, defining the boundary with the α phase, both represent solidus lines. In addition, the line extending downward and right from 660°C on the vertical axis and tangent to solidus 1 (hereinafter referred to as "liquidus 1") and the line extending upward and right from the tangent position, defining the boundary with the (Si + liquid phase), both represent liquidus lines.
[0062] Here, the point at temperature T2 is designated as P0, and a line is drawn through P0 parallel to the horizontal axis of the diagram. The intersection with liquidus 1 is designated as P1, and the intersection with solidus 2 is designated as P2. An Al-Si alloy with a Si concentration of C1 is in a state where the liquid and solid phases coexist at temperature T2, and the Si concentration in the liquid phase is the concentration C at point P1. P1 and the Si concentration in the solid phase is the concentration C P2 The ratio of the liquid mass to the total mass at temperature T2, i.e., the liquid fraction, is the ratio of the length of the line segment P0 to P2 to the length of the line segment P1 to P2.
[0063] As described above, the liquid fraction can be calculated by drawing a diagram of the alloy components and temperature based on the phase diagrams of binary alloys such as those shown in Figures 1 and 4. Similarly, for ternary or higher component systems, the liquid fraction can also be calculated by drawing a diagram of the alloy components and temperature based on the phase diagram. It is difficult to represent the phase diagram of a ternary or higher component system as a simple XY plane diagram like Figure 4, but the liquid fraction can be calculated by computer using Thermo-Calc thermodynamic equilibrium calculation software.
[0064] The aluminum alloy sheet of the present invention has a metallographic structure in which, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after a heating test in which the temperature is raised from 300°C to 400°C at an average heating rate of 60°C / min or less and then held at 600±3°C for 5±3 minutes, the region having one or more grain boundaries in the sheet thickness direction accounts for 25% to less than 90% of the cross section, and the average grain size in the direction perpendicular to the rolling direction on the sheet surface is 950 μm or less. Therefore, there are many flow paths for the liquid phase that seeps out of the base metal during brazing heating, i.e., many grain boundaries, and the fillet area produced by heat bonding can be increased. Therefore, the aluminum alloy sheet of the present invention has excellent brazability even when the Si content is low, and can therefore achieve both brazability and material strength.
[0065] The aluminum alloy sheet of the present invention is suitable for use as a material for manufacturing heat exchangers. That is, the aluminum alloy sheet of the present invention is suitable as an aluminum alloy sheet for heat exchangers.
[0066] The aluminum alloy sheet of the present invention may be produced by any production method, and is preferably produced, for example, by the production method of the aluminum alloy sheet of the present invention described below.
[0067] The method for producing an aluminum alloy sheet of the present invention is to produce an aluminum alloy sheet by continuous casting and rolling, the aluminum alloy sheet containing 2.00 to 3.00% by mass of Si, 0.05 to 0.40% by mass of Fe, and 0.80 to 1.80% by mass of Mn, with a Cu content of 0.20% by mass or less (inclusive of 0.00% by mass), a Zn content of 6.00% by mass or less (inclusive of 0.00% by mass), and optionally 0.08% by mass or less of Mg, 0.30% by mass or less of Ti, 0.30% by mass or less of Zr, a casting step of casting a cast-rolled sheet of an aluminum alloy comprising an aluminum alloy containing any one or two or more of 0.30% by mass or less of Cr, 0.30% by mass or less of V, 0.10% by mass or less of Be, 0.10% by mass or less of Sr, 0.30% by mass or less of Bi, 0.10% by mass or less of Na, and 0.05% by mass or less of Ca, with the balance being Al and unavoidable impurities, at a casting speed of more than 0.50 m / min and less than 0.70 m / min; a cold rolling step of cold rolling the cast-rolled sheet two or more times; and Annealing is performed at least once between the casting process and the final cold rolling in the cold rolling process. The annealing conditions for all annealing treatments are an annealing temperature of 200 to 550°C and an annealing time of 1 to 10 hours. This is a method for producing an aluminum alloy sheet, characterized by the above.
[0068] The method for producing an aluminum alloy sheet of the present invention includes at least a casting step, a cold rolling step, and an annealing treatment.
[0069] The casting process involves continuous casting and rolling to produce a cast-rolled aluminum alloy sheet having a predetermined chemical composition. In continuous casting, the rapid cooling rate during solidification reduces the formation of coarse crystals, suppressing the formation of Si-based intermetallic compounds with a circle-equivalent diameter of 5.0 to 10 μm. As a result, the number of recrystallization nuclei is reduced, allowing only specific crystal grains to grow, resulting in coarse grains. Furthermore, compared to DC (Direct Chill) casting, which water-cools thick ingots, continuous casting has a smaller difference in cooling rate across the width, making it easier for solute atoms to be concentrated uniformly across the width, resulting in more stable aluminum alloy quality. The continuous casting method is not particularly limited as long as it continuously casts a plate-shaped ingot, such as twin-roll continuous casting and rolling, or twin-belt continuous casting. Twin-roll continuous casting and rolling involves supplying molten aluminum between a pair of water-cooled rolls from a refractory nozzle, and continuously casting and rolling a thin sheet. Known methods include the Hunter process and the 3C process. The twin-belt continuous casting method is a continuous casting method in which molten metal is poured between two opposing water-cooled rotating belts, solidified by cooling from the belt surface to form a slab, and the slab is continuously drawn from the opposite side of the belt and wound into a coil. In twin-roll continuous casting and rolling, the cooling rate during casting is several to several hundred times faster than that of semi-continuous casting. For example, the cooling rate in semi-continuous casting is 0.5 to 20°C / sec, while the cooling rate in twin-roll continuous casting and rolling is 100 to 1000°C / sec. Therefore, twin-roll continuous casting and rolling is characterized by the finer and more densely distributed dispersed particles generated during casting compared to semi-continuous casting. This suppresses the generation of coarse crystals, thereby coarsening the crystal grains during joining and heating. Furthermore, the fast cooling rate can increase the amount of solid solution of additive elements. This allows fine precipitates to be formed by subsequent heat treatment, contributing to the coarsening of crystal grains during joining and heating. In the casting process, the cooling rate when casting using twin-roll continuous casting is preferably 100 to 1000°C / sec. A cooling rate below 100°C / sec makes it difficult to obtain the desired metal structure, while a cooling rate above 1000°C / sec makes stable production difficult. The speed of the rolled sheet when casting using twin-roll continuous casting is greater than 0.50 m / min and less than 0.70 m / min, preferably 0.53 to 0.69 m / min, and more preferably 0.58 to 0.68 m / min. The casting speed affects the cooling rate. If the casting speed is 0.50 m / min or less, the above-mentioned sufficient cooling rate cannot be obtained, resulting in coarsening of the compounds and a decrease in the amount of solid solution of the additive elements in the base material. As a result, the formation of fine precipitates during subsequent heat treatment is reduced, resulting in coarsening of the crystal grain size. On the other hand, if the cooling rate is 0.70 m / min or more, the cooling rate is too fast, resulting in the formation of too many fine precipitates, resulting in a refined crystal grain size. This makes grain boundary sliding more likely to occur, leading to deformation during brazing heating. The molten metal temperature when casting using the twin-roll continuous casting and rolling method is preferably 650 to 800°C, more preferably 680 to 750°C. The molten metal temperature is the temperature of the head box located immediately before the molten metal supply nozzle. If the molten metal temperature is below the above range, coarse dispersed particles of intermetallic compounds are generated inside the molten metal supply nozzle, and these particles are mixed into the ingot, causing sheet breakage during cold rolling. Furthermore, if the molten metal temperature exceeds the above range, the aluminum material does not solidify sufficiently between the rolls during casting, and a normal plate-shaped ingot cannot be obtained.
[0070] The thickness of the plate-shaped ingot cast by twin-roll continuous casting is preferably 2 to 10 mm, and particularly preferably 4 to 8 mm. Within this thickness range, the solidification rate at the center of the plate thickness is fast, making it easy to obtain a uniform structure. If the plate thickness is less than the above range, the amount of aluminum passing through the casting machine per unit time is small, making it difficult to stably supply the molten metal in the plate width direction. On the other hand, if the plate thickness exceeds the above range, it becomes difficult to wind the plate on the rolls.
[0071] The casting speed is more than 0.50 m / min and less than 0.70 m / min, preferably 0.53 to 0.69 m / min, and more preferably 0.58 to 0.68 m / min. When the casting speed is within the above range, an aluminum alloy sheet is easily obtained in which "in a heating test in which the temperature is increased from 300°C to 400°C at an average heating rate of 60°C / min or less and then held at 600±3°C for 5±3 minutes, or in which the temperature is increased preferably from 300°C to 400°C at an average heating rate of 60°C / min or less, preferably 45°C / min or less, then the temperature is increased from 400°C to 580°C in 8±3 minutes, then the temperature is increased from 580°C to the holding temperature in 8±3 minutes, and then the temperature is held at 600±3°C for 5±3 minutes, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test, the proportion of regions in the thickness direction having one or more grain boundaries is 25% or more and less than 90% in the width direction, and the average grain size on the sheet surface in the direction perpendicular to the rolling direction is 950 μm or less."
[0072] In the casting step, a cast rolled plate is cast from an aluminum alloy containing 2.00 to 3.00 mass%, preferably 2.10 to 2.80 mass%, and more preferably 2.20 to 2.60 mass% Si, 0.05 to 0.40 mass%, preferably 0.08 to 0.35 mass% Fe, and 0.80 to 1.80 mass%, preferably 1.00 to 1.60 mass% Mn, with the remainder being Al and unavoidable impurities. Furthermore, the cast rolled sheet obtained by the casting step may further contain, as optional additive elements, 0.20 mass% or less, preferably 0.01 to 0.18 mass% of Cu, 6.00 mass% or less, preferably 0.05 to 6.00 mass%, particularly preferably 0.10 to 5.00 mass% of Zn, 0.08 mass% or less, preferably 0.005 to 0.07 mass% of Mg, 0.30 mass% or less, preferably 0.05 to 0.30 mass% of Ti, 0.30 mass% or less, preferably 0.05 to 0.30 mass% of Zr, 0.30 mass% or less, preferably 0.05 The cast rolled sheet obtained by the casting step may contain one or more of the following: up to 0.30% by mass of Cr, 0.30% by mass or less, preferably 0.05 to 0.30% by mass of V, 0.10% by mass or less, preferably 0.0001 to 0.10% by mass of Be, 0.10% by mass or less, preferably 0.0001 to 0.10% by mass of Sr, 0.30% by mass or less, preferably 0.0001 to 0.30% by mass of Bi, 0.10% by mass or less, preferably 0.0001 to 0.10% by mass of Na, and 0.05% by mass or less, preferably 0.0001 to 0.05% by mass of Ca. The cast rolled sheet obtained by the casting step may also contain, as optional additive elements, up to 0.10% by mass of In, up to 0.10% by mass of Sn, and up to 0.10% by mass of rare earth elements, if necessary. In the casting process, a molten aluminum alloy having the above-mentioned chemical composition is prepared, and the molten aluminum alloy is subjected to continuous casting and rolling, so that the chemical composition of the cast and rolled sheet can be made to be the above-mentioned chemical composition.
[0073] The cold rolling process is a process of cold rolling the cast-rolled sheet obtained by the casting process. In the cold rolling process, cold rolling is performed two or more times. That is, in the cold rolling process, cold rolling passes are performed two or more times. The number of cold rolling passes in the cold rolling process is selected appropriately. Then, in the cold rolling process, cold rolling is performed until the thickness of the aluminum alloy sheet becomes the thickness of the final sheet. That is, the thickness of the aluminum alloy sheet after the last cold rolling in the cold rolling process is the thickness of the final sheet.
[0074] In the method for producing an aluminum alloy sheet of the present invention, annealing is performed one or more times between the casting step and the final cold rolling step in the cold rolling step. In the method for producing an aluminum alloy sheet of the present invention, the timing of annealing is (1) after the casting step and before the cold rolling step, or (2) between cold rolling steps when two or more cold rolling steps are performed in the cold rolling step. In either or both of (1) and (2), annealing is performed one or more times, preferably one to three times, and more preferably one to two times. In the cold rolling step when three or more cold rolling steps are performed, there are two or more times between cold rolling steps. In such a case, annealing may be performed two or more times in the cold rolling step. The annealing is performed to soften the aluminum alloy sheet to make it easier to obtain the desired strength in the final cold rolling, and this annealing can optimally adjust the size and density of intermetallic compounds in the aluminum alloy sheet and the amount of solid solution of additive elements. In the method for producing an aluminum alloy sheet according to the present invention, after the final cold rolling step in the cold rolling process, no annealing treatment is carried out.
[0075] The annealing conditions for the annealing treatment are an annealing temperature of 200 to 550°C, preferably 250 to 450°C, and an annealing time of 1 to 10 hours. That is, in the annealing treatment, heating is performed at an annealing temperature of 200 to 550°C, preferably 250 to 450°C, for an annealing time of 1 to 10 hours. If the annealing temperature is below the above range, softening of the aluminum alloy sheet is insufficient, resulting in a high tensile strength before heat bonding. If the tensile strength before heat bonding is high, formability is poor, resulting in a worse core dimension and, as a result, low durability. On the other hand, if the annealing temperature exceeds the above range, annealing is performed at an excessive temperature exceeding the softening temperature of the aluminum alloy sheet, which is economically disadvantageous.
[0076] In the method for producing an aluminum alloy sheet of the present invention, the total reduction rate of the cold rolling carried out after the final annealing treatment is preferably 20 to 50%, and particularly preferably 25 to 40%. When the total reduction ratio of the cold rolling performed after the final annealing treatment is within the above range, an aluminum alloy sheet can be easily obtained in which "in a heating test in which the temperature is increased from 300°C to 400°C at an average heating rate of 60°C / min or less and then held at 600±3°C for 5±3 minutes, or in a heating test in which the temperature is increased preferably from 300°C to 400°C at an average heating rate of 60°C / min or less, preferably 45°C / min or less, then the temperature is increased from 400°C to 580°C in 8±3 minutes, then the temperature is increased from 580°C to the holding temperature in 8±3 minutes, and then the temperature is held at 600±3°C for 5±3 minutes, the cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test has one or more regions in the thickness direction that account for 25% or more but less than 90% in the width direction, and the average crystal grain size in the direction perpendicular to the rolling direction on the sheet surface is 950 μm or less." In the present invention, the final annealing treatment refers to the single annealing treatment when only one annealing treatment is performed, and refers to the final annealing treatment among the two or more annealing treatments when two or more annealing treatments are performed. The total reduction ratio A (%) of the cold rolling performed after the final annealing treatment is a value calculated by the following formula. A(%)=((BC) / B)×100 A: Total reduction rate (%) of cold rolling performed after the final annealing treatment B: Thickness of the rolled sheet immediately after the final annealing treatment C: Thickness of the rolled sheet after the final cold rolling
[0077] When only one cold rolling is performed after the final annealing treatment, the thickness of the rolled sheet before the cold rolling is B, and the thickness of the rolled sheet after the cold rolling is C. When multiple cold rollings are performed after the final annealing treatment, the thickness of the rolled sheet before the first cold rolling of the multiple cold rollings after the final annealing treatment is B, and the thickness of the rolled sheet after the last cold rolling is C.
[0078] The temper of the aluminum alloy sheet obtained by the manufacturing method of the aluminum alloy sheet of the present invention may be either O material or H material. When the aluminum alloy sheet is made into an H1n material or an H2n material, the final cold rolling reduction is 50% or less, preferably 5 to 50%. If the final cold rolling reduction exceeds 50%, many recrystallization nuclei are generated during heating, resulting in a fine grain size after joining and heating. Note that if the final cold rolling reduction is less than 5%, manufacturing may be substantially difficult.
[0079] The aluminum alloy sheet obtained by the method for producing an aluminum alloy sheet of the present invention has the function of being heat-bonded in a single layer at a temperature at which the liquid phase ratio is 5.0% or more and 35.0% or less.
[0080] In the method for producing an aluminum alloy sheet of the present invention, in the casting step, a cast-rolled sheet is cast by continuous casting and rolling, preferably by twin-roll continuous casting and rolling, and annealing is performed once or more during the period from the casting step to obtaining a final sheet, and the annealing conditions in all of the annealing treatments are an annealing temperature of 200 to 550°C, preferably 250 to 450°C, and an annealing time of 1 to 10 hours, and preferably further a total reduction in cold rolling after the final annealing treatment is 20 to 50%, preferably 25 to 40%, thereby "heating from 300°C to 400°C at an average heating rate of 60°C / min or less, and reducing to 5±3°C at 600±3°C" In a heating test in which the temperature is preferably increased from 300°C to 400°C at an average heating rate of 60°C / min or less, preferably 45°C / min or less, the temperature is increased from 400°C to 580°C in 8±3 minutes, the temperature is increased from 580°C to the holding temperature in 8±3 minutes, and the temperature is held at 600±3°C for 5±3 minutes, an aluminum alloy sheet can be produced in which, in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction after the heating test, the proportion of regions with one or more grain boundaries in the sheet thickness direction is 25% or more and less than 90% in the width direction, and the average crystal grain size on the sheet surface in the direction perpendicular to the rolling direction is 950 μm or less.
[0081] When heat bonding is performed using the aluminum alloy sheet of the present invention, the aluminum alloy sheet of the present invention is formed into a predetermined shape, combined with a mating material to be bonded, and heated at a heat bonding temperature to perform heat bonding. The appropriate heat bonding temperature for heat bonding using the aluminum alloy sheet of the present invention is a temperature range in which the liquid phase fraction is 5 to 35%, and the time for maintaining the liquid phase fraction at 5% or more is preferably 30 to 3600 seconds. Since a small liquid phase may make bonding difficult, a liquid phase fraction of 5% or more is preferred. If the liquid phase fraction exceeds 35%, too much liquid phase is generated, causing the aluminum alloy material to significantly deform during heat bonding and making it impossible to maintain its shape. If the time for maintaining the liquid phase fraction at 5% or more is less than 30 seconds, the liquid phase may not be sufficiently filled in the bonded portion, and if it exceeds 3600 seconds, deformation of the aluminum material may progress. To achieve these conditions, the heating temperature during heat bonding may be set to 580°C to 640°C, and the holding time at the heating temperature may be set to approximately 0 to 10 minutes. Here, 0 minutes means that cooling begins as soon as the temperature of the components reaches the predetermined bonding temperature. Heating conditions during thermal bonding may be adjusted to an appropriate range to achieve a sound bond without deformation. Furthermore, the heating atmosphere during thermal bonding is preferably a non-oxidizing atmosphere substituted with nitrogen or argon. When obtaining a bonded body through thermal bonding, better bonding can be achieved by using a non-corrosive flux. Furthermore, thermal bonding can also be performed by heating in a vacuum or under reduced pressure.
[0082] The heat exchanger of the present invention is a heat exchanger having tubes made of an aluminum alloy through which a working fluid flows, and fins made of an aluminum alloy metallurgically joined to the tubes, The heat exchanger is obtained by combining at least a heat exchanger tube material made of an aluminum alloy and a heat exchanger fin material made of an aluminum alloy, and then heating the resulting combination to bond the heat exchanger tube material and the heat exchanger fin material together, The heat exchanger fin material is a molded product of the aluminum alloy plate of the present invention. This is a heat exchanger characterized by the above.
[0083] The heat exchanger tube material made of an aluminum alloy for the heat exchanger of the present invention is not particularly limited as long as it is an aluminum alloy material that is normally used as a tube material for aluminum alloy heat exchangers and is formed into a tubular shape.
[0084] The chemical composition of the aluminum alloy forming the heat exchanger tube material is not particularly limited, but typical examples of aluminum alloys forming the heat exchanger tube material include 1000-series and 3000-series aluminum, i.e., pure aluminum and aluminum alloys containing one or more of 0.60 mass% or less of Si, 0.70 mass% or less of Fe, 0.70 mass% or less of Cu, and 2.00 mass% or less of Mn relative to the pure aluminum, with the remainder being Al and unavoidable impurities.
[0085] The heat exchanger fin material made of the aluminum alloy according to the present invention is a molded product of the aluminum alloy plate of the present invention. The aluminum alloy plate used for the heat exchanger fin material of the heat exchanger of the present invention is the same as the aluminum alloy plate of the present invention.
[0086] The heat exchanger of the present invention is a combination of at least a heat exchanger tube material made of an aluminum alloy and a heat exchanger fin material made of an aluminum alloy, and further includes necessary components such as a header, a tank, and piping materials, which are then heat-bonded together.
[0087] The heating temperature during heat bonding of the combined body is appropriately selected depending on the Si content. Furthermore, since Zn and Cu, in addition to Si, also affect the solidus temperature, when the aluminum alloy sheet of the present invention contains Zn and / or Cu in addition to Si, the heating temperature during heat bonding of the combined body is appropriately selected depending on the Si and Zn and / or Cu contents. The heating temperature during heat bonding of the combined body is preferably in a temperature range where the liquid phase fraction of the aluminum alloy sheet of the present invention is 5 to 35%, and the time during which the liquid phase fraction is maintained at 5% or more is preferably 30 to 3600 seconds. The heating rate during heat bonding of the combined body is not uniquely specified, but is appropriately selected depending on the furnace structure and product design, and is generally 20 to 300°C / min.
[0088] That is, the heat exchanger of the present invention is a heat exchanger having tubes made of an aluminum alloy through which a working fluid flows, and fins made of an aluminum alloy metallically joined to the tubes, The tube is formed using a heat exchanger tube material made of an aluminum alloy, the fin is made of an aluminum alloy containing 2.00 to 3.00% by mass of Si, 0.05 to 0.40% by mass of Fe, and 0.80 to 1.80% by mass of Mn, a Cu content of 0.20% by mass or less (inclusive of 0.00% by mass), a Zn content of 6.00% by mass or less (inclusive of 0.00% by mass), and optionally containing one or more of 0.08% by mass or less of Mg, 0.30% by mass or less of Ti, 0.30% by mass or less of Zr, 0.30% by mass or less of Cr, 0.30% by mass or less of V, 0.10% by mass or less of Be, 0.10% by mass or less of Sr, 0.30% by mass or less of Bi, 0.10% by mass or less of Na, and 0.05% by mass or less of Ca, with the remainder being Al and unavoidable impurities, and is formed using an aluminum alloy plate having a function of being heat-bonded in a single layer; In a cross section of the fin perpendicular to the rolling surface and perpendicular to the rolling direction, the area having one or more crystal grain boundaries in the thickness direction accounts for 25% or more and less than 90% in the width direction, and the average crystal grain size in the direction perpendicular to the rolling direction on the plate surface is 950 μm or less; This is a heat exchanger characterized by the above.
[0089] The heat exchanger of the present invention uses an aluminum alloy plate, which can be thermally bonded in a single layer, as the fin material, and a heat exchanger tube material made of an aluminum alloy as the mating material, which is thermally bonded.
[0090] The fins of the heat exchanger of the present invention are formed using aluminum alloy plates capable of being thermally bonded in a single layer. For example, the fins of the heat exchanger of the present invention are formed using the aluminum alloy of the present invention.
[0091] The aluminum alloy from which the fins of the heat exchanger of the present invention are formed contains 2.00 to 3.00 mass%, preferably 2.10 to 2.80 mass%, and more preferably 2.20 to 2.60 mass% Si, 0.05 to 0.40 mass%, and preferably 0.08 to 0.35 mass% Fe, and 0.80 to 1.80 mass%, and preferably 1.00 to 1.60 mass% Mn, with the remainder being Al and unavoidable impurities. Furthermore, the aluminum alloy forming the fin material according to the heat exchanger of the present invention may further contain, as optional additive elements, 0.20 mass% or less, preferably 0.01 to 0.18 mass% Cu, 6.00 mass% or less, preferably 0.05 to 6.00 mass%, particularly preferably 0.10 to 5.00 mass% Zn, 0.08 mass% or less, preferably 0.005 to 0.070 mass% Mg, 0.30 mass% or less, preferably 0.05 to 0.30 mass% Ti, 0.30 mass% or less, preferably 0.05 to 0.30 mass% Zr, 0.30 mass% or less, preferably 0.05 to 0.30 mass% or 0.05 to 0.30 mass% Cr, 0.30 mass% or less, preferably 0.05 to 0.30 mass% V, 0.10 mass% or less, preferably 0.0001 to 0.10 mass% Be, 0.10 mass% or less, preferably 0.0001 to 0.10 mass% Sr, 0.30 mass% or less, preferably 0.0001 to 0.30 mass% Bi, 0.10 mass% or less, preferably 0.0001 to 0.10 mass% Na, and 0.05 mass% or less, preferably 0.0001 to 0.05 mass% Ca. The aluminum alloy according to the aluminum alloy sheet of the present invention may also contain 0.10 mass% or less, preferably 0.0001 to 0.10 mass% In, 0.10 mass% or less, preferably 0.0001 to 0.10 mass% Sn, 0.10 mass% or less, preferably 0.0001 to 0.10 mass% Be, and 0.10 mass% or less, preferably 0.0001 to 0.10 mass% rare earth elements.
[0092] In the heat exchanger of the present invention, in a cross section perpendicular to the rolling surface and perpendicular to the rolling direction of the fin, the region with one or more grain boundaries in the thickness direction accounts for 25% to less than 90% of the width, and the average grain size in the direction perpendicular to the rolling direction on the plate surface is 950 μm or less. During brazing, there are many flow paths for the liquid phase that seeps out of the base material, i.e., many grain boundaries, and the fillet area resulting from thermal bonding is increased. Therefore, the fin of the heat exchanger of the present invention has excellent brazability even with a low Si content, and therefore the heat exchanger of the present invention is a heat exchanger that achieves both brazability and material strength.
[0093] In the fin of the heat exchanger of the present invention, in a cross section perpendicular to the rolling surface and perpendicular to the rolling direction after a heating test, regions with two or more grain boundaries in the thickness direction are present in a proportion of 3% or more, preferably 5% or more, in the width direction. The presence of regions with two or more grain boundaries in this range increases the number of flow paths for the liquid phase seeping out of the base material, resulting in excellent brazability.
[0094] In the fin of the heat exchanger of the present invention, in a cross section perpendicular to the rolling surface and perpendicular to the rolling direction after a heating test, the maximum width of a region with no grain boundaries in the plate thickness direction is 2000 μm or less, preferably 1800 μm or less. When the region with no grain boundary crystals is in the above range, there are more flow paths for the liquid phase that seeps out of the base material, resulting in excellent brazability.
[0095] The aluminum alloy from which the tubes of the heat exchanger of the present invention are made is not particularly limited, as long as it is an aluminum alloy that is normally used for tubes of aluminum alloy heat exchangers.
[0096] The chemical composition of the aluminum alloy forming the tube is not particularly limited, but typical examples of aluminum alloys forming heat exchanger tube materials include 1000-series and 3000-series aluminums, namely, pure aluminum and aluminum alloys containing one or more of 0.60 mass% or less of Si, 0.70 mass% or less of Fe, 0.70 mass% or less of Cu, and 2.00 mass% or less of Mn relative to pure aluminum, with the remainder being Al and unavoidable impurities.
[0097] The present invention will be specifically described below by showing examples, but the present invention is not limited to the examples shown below. [Example]
[0098] (Example 1, Comparative Examples 1 and 2) Aluminum alloys having the alloy compositions shown in Table 1 were used to cast and rolled sheets by twin-roll continuous casting and rolling. In the alloy compositions in Table 1, "-" indicates that the content is below the detection limit, and "balance" includes unavoidable impurities. The molten metal temperature during casting by twin-roll continuous casting and rolling was 600 to 800°C, and the thickness of the cast and rolled sheets was 6.0 mm. The resulting cast-rolled sheet was then annealed at 420°C for 2 hours and then cold rolled to the thickness (after the first cold rolling) shown in Table 2. Next, the sheet was annealed at 370°C for 2 hours and then cold rolled to a thickness of 0.070 mm to obtain a test material (final sheet). For each of the above test materials, the maximum width of the region with two or more grain boundaries, one or more grain boundaries, and zero grain boundaries in the thickness direction were measured in a cross section perpendicular to the rolling surface and the rolling direction after the heating test, as well as the average grain size perpendicular to the rolling direction as viewed from the sheet surface, the fillet area, and the tensile strength after brazing heating. The results are shown in Table 2.
[0099] <Heating test> The test material was heated in an inert gas atmosphere from 300°C to 400°C at a heating rate of 41°C / min, from 400°C to 580°C in 7.2 minutes, from 580°C to 600°C in 7.4 minutes, heated to a holding temperature of 600±3°C, then held at 600±3°C for 4.7 minutes, and then cooled to room temperature to obtain the test material after the heating test.
[0100] <Measurement of grain boundaries in cross sections> After brazing and heating, the sample was cut out in a direction perpendicular to the rolling surface and perpendicular to the rolling direction, embedded in resin, and mirror-polished. The polished embedding resin was then immersed in the SWAAT test solution for 12 hours, after which the resin surface was lightly mirror-polished to remove any dirt. Next, the cross-sectional structure was photographed at 200x magnification using a microscope for metallographic observation, with the total observation length set to approximately 25 mm. The cross-sectional photographs were colored red to make the grain boundaries more visible. The proportion of areas with one or more crystal grain boundaries was calculated by surrounding areas with one or more crystal grain boundaries with a frame, finding the widthwise length of each framed area, adding them all up, and dividing the total by the total widthwise length of the observed area.Furthermore, the proportion of areas with two or more crystal grain boundaries was calculated by surrounding areas with two or more crystal grain boundaries with a frame, finding the widthwise length of each framed area, adding them all up, and dividing the total by the total widthwise length of the observed area. For regions with zero grain boundaries, the widthwise length of the longest part of the part not enclosed by a frame as one or more regions was measured, and this was calculated as the maximum width of the region with zero grain boundaries in the thickness direction.
[0101] <Measurement of surface grain boundaries> The sample after brazing heating was cut into a size of 20 mm x 30 mm, and the plate surface was ground and chamfered to expose the center of the plate thickness. Next, the specimen was mirror-polished and parker-etched, and then observed under polarized light using a metallurgical microscope. Six fields of view were photographed at 20x magnification, and the crystal structure was observed in a series of six fields of view at 20x magnification (observation was performed parallel to the rolling direction). Ten 6 mm lines were drawn perpendicular to the rolling direction at 1 mm intervals, and the number of crystal grains on the 10 lines was counted to calculate the total number of crystal grains, using the following formula: Average grain size (μm) = (6000 × 10) / total number of grains on 10 lines The average crystal grain size was calculated using the above formula.
[0102] [Table 1]
[0103] [Table 2]
[0104] [Table 3]
[0105] Casting method CC: Twin-roll continuous casting and rolling Average grain size: Average grain size in the direction perpendicular to the rolling direction on the plate surface after the heating test
Claims
1. It is an aluminum alloy plate that can be thermally bonded in a single layer. an aluminum alloy containing 2.00 to 3.00 mass% Si, 0.05 to 0.40 mass% Fe, and 0.80 to 1.80 mass% Mn, a Cu content of 0.20 mass% or less (including 0.00 mass%), a Zn content of 6.00 mass% or less (including 0.00 mass%), and optionally containing one or more of 0.08 mass% or less Mg, 0.30 mass% or less Ti, 0.30 mass% or less Zr, 0.30 mass% or less Cr, 0.30 mass% or less V, 0.10 mass% or less Be, 0.10 mass% or less Sr, 0.30 mass% or less Bi, 0.10 mass% or less Na, and 0.05 mass% or less Ca, with the balance being Al and unavoidable impurities; After a heating test in which the temperature is increased from 300°C to 400°C at an average heating rate of 60°C / min or less and the temperature is kept at 600±3°C for 5±3 minutes, the area having one or more grain boundaries in the thickness direction in a cross section perpendicular to the rolled surface and perpendicular to the rolling direction accounts for 25% or more but less than 90% in the width direction, and the average grain size in the direction perpendicular to the rolling direction on the sheet surface is 950 μm or less. An aluminum alloy plate characterized by:
2. The aluminum alloy sheet according to claim 1, characterized in that, in a cross section after the heating test in a direction perpendicular to the rolled surface and perpendicular to the rolling direction, a region having two or more crystal grain boundaries in the sheet thickness direction is present in a proportion of 3% or more in the width direction.
3. The aluminum alloy sheet according to claim 1 or 2, characterized in that in a cross section after the heating test in a direction perpendicular to the rolled surface and perpendicular to the rolling direction, a maximum width of a region having no crystal grain boundaries in a sheet thickness direction is 2000 μm or less.
4. 3. The aluminum alloy sheet according to claim 1, wherein the sheet has a thickness of 0.08 mm or less.
5. 4. The aluminum alloy plate according to claim 3, wherein the plate has a thickness of 0.08 mm or less.
6. By continuous casting and rolling, it contains 2.00 to 3.00 mass% Si, 0.05 to 0.40 mass% Fe, and 0.80 to 1.80 mass% Mn, the Cu content is 0.20 mass% or less (including 0.00 mass%), the Zn content is 6.00 mass% or less (including 0.00 mass%), and optionally, 0.08 mass% or less Mg, 0.30 mass% or less Ti, 0.30 mass% or less Zr, 0.30 mass% or less a casting step of casting a cast rolled sheet of an aluminum alloy comprising an aluminum alloy containing one or more of Cr, 0.30 mass% or less of V, 0.10 mass% or less of Be, 0.10 mass% or less of Sr, 0.30 mass% or less of Bi, 0.10 mass% or less of Na, and 0.05 mass% or less of Ca, with the balance being Al and unavoidable impurities, at a casting speed of more than 0.50 m / min and less than 0.70 m / min; a cold rolling step of cold rolling the cast-rolled plate two or more times; having Performing annealing treatment at least once between the casting process and the final cold rolling in the cold rolling process; The annealing conditions in all annealing treatments are an annealing temperature of 200 to 550°C and an annealing time of 1 to 10 hours. A method for producing an aluminum alloy sheet, comprising the steps of:
7. A heat exchanger having an aluminum alloy tube through which a working fluid flows and an aluminum alloy fin metallically joined to the tube, The tube is formed using a heat exchanger tube material made of an aluminum alloy, The fin is made of an aluminum alloy containing 2.00 to 3.00 mass% Si, 0.05 to 0.40 mass% Fe, and 0.80 to 1.80 mass% Mn, a Cu content of 0.20 mass% or less (including 0.00 mass%), a Zn content of 6.00 mass% or less (including 0.00 mass%), and optionally containing one or more of 0.08 mass% or less Mg, 0.30 mass% or less Ti, 0.30 mass% or less Zr, 0.30 mass% or less Cr, 0.30 mass% or less V, 0.10 mass% or less Be, 0.10 mass% or less Sr, 0.30 mass% or less Bi, 0.10 mass% or less Na, and 0.05 mass% or less Ca, with the balance being Al and unavoidable impurities, and is formed using an aluminum alloy plate having a function of being heat-bonded in a single layer, In a cross section of the fin perpendicular to the rolled surface and perpendicular to the rolling direction, the area having one or more crystal grain boundaries in the plate thickness direction is 25% or more and less than 90% in the width direction, and the average crystal grain size in the direction perpendicular to the rolling direction on the plate surface is 950 μm or less; A heat exchanger comprising:
8. A heat exchanger as described in claim 7, characterized in that in a cross section of the fin perpendicular to the rolling surface and perpendicular to the rolling direction, an area with two or more crystal grain boundaries in the plate thickness direction is present in a proportion of 3% or more in the width direction.
9. 9. The heat exchanger according to claim 7 or 8, characterized in that in a cross section of the fin perpendicular to the rolling surface and perpendicular to the rolling direction, the maximum width of a region having zero crystal grain boundaries in the plate thickness direction is 2000 μm or less.
10. A heat exchanger having an aluminum alloy tube through which a working fluid flows and an aluminum alloy fin metallically joined to the tube, The heat exchanger is obtained by combining at least a heat exchanger tube material made of an aluminum alloy with a heat exchanger fin material made of an aluminum alloy, and then heating the combined body to bond the heat exchanger tube material and the heat exchanger fin material, The heat exchanger fin material is a molded body of the aluminum alloy plate according to any one of claims 1 to 5. A heat exchanger comprising:
Citation Information
Patent Citations
Detector for moving body
JP1978045264A
Performance effect device for electronic instrument
JP1979036714A
Method of producing sheathed heater
JP1982032594A
Aluminum alloy sheet and method for producing same, and heat exchanger
WO2022176420A1