Curable resin composition, dry film, cured product, and printed wiring board

A curable resin composition with polyphenylene ether and (meth)acrylate group addresses adhesion issues on uneven substrates, enhancing embeddability and preventing cracks in multilayer printed wiring boards.

JP2024147422APending Publication Date: 2024-10-16TAIYO HOLDINGS CO LTD

Patent Information

Application Number
JP2023060429
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-16

AI Technical Summary

Technical Problem

Conventional resin layers fail to adequately adhere to substrates with surface irregularities, leading to cracks and poor embedment, especially during desmear treatment in multilayer printed wiring boards.

Method used

A curable resin composition combining polyphenylene ether with a branched structure and a (meth)acrylate group, along with specific compounds and fillers, is used to enhance adhesion and prevent cracking on uneven surfaces.

Benefits of technology

The composition improves embeddability and suppresses crack formation during desmear processing, ensuring effective lamination on substrates with surface irregularities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147422000001
    Figure 2024147422000001
  • Figure 2024147422000002
    Figure 2024147422000002
  • Figure 2024147422000003
    Figure 2024147422000003
Patent Text Reader

Abstract

To provide a curable resin composition that is suitable for application to even a substrate with surface irregularities.SOLUTION: A curable resin composition according to one embodiment of the present invention includes: a polyphenylene ether with a branched structure, including functional groups that include unsaturated carbon bonds; and a compound with (meth)acrylate groups.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition, a dry film, a cured product, and a printed wiring board. [Background technology]

[0002] One known method for manufacturing multilayer printed wiring boards is the build-up method, in which insulating layers and conductor layers are alternately stacked on an inner layer circuit board (a so-called copper-clad laminate) in which circuits are formed by pressing prepreg and copper foil (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-087927 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0004] In recent years, the structure of substrates has become more complex, and some substrates have surface irregularities.

[0005] In a multilayer printed wiring board, an opening (through hole or via hole) is formed using a laser, a drill, or the like in order to provide electrical continuity between two layers. In addition, a desmear treatment is performed using a desmear treatment solution or the like in order to remove residues (smears) that are generated when forming the opening. It has been found that when a conventional resin layer is applied to a substrate including surface irregularities, cracks are particularly likely to occur in the resin layer around the surface irregularities after the desmear treatment.

[0006] Furthermore, when a conventional resin layer is laminated on a substrate having an uneven surface, the layer may lack the ability to fill the uneven surface (flatness).

[0007] Thus, conventional resin layers are sometimes unable to adequately accommodate substrates having uneven surfaces.

[0008] Therefore, an object of the present invention is to provide a curable resin composition that can be preferably used even on substrates having surface irregularities. [Means for solving the problem]

[0009] The present inventors have found that the above-mentioned problems can be solved by combining a specific resin with a specific compound, and have completed the present invention.

[0010] A form (1) of the present invention is a curable resin composition comprising a polyphenylene ether having a branched structure and a functional group containing an unsaturated carbon bond, and a compound having a (meth)acrylate group.

[0011] The content of the compound having a (meth)acrylate group is preferably 15 parts by mass or more per 100 parts by mass of the polyphenylene ether in terms of solid content. The content of the compound having a (meth)acrylate group is preferably 30 parts by mass or more per 100 parts by mass of the polyphenylene ether in terms of solid content. The molecular weight of the compound having a (meth)acrylate group is preferably 3,000 or less.

[0012] The compound having a (meth)acrylate group is preferably a compound not containing an aromatic ring.

[0013] The embodiment (2) of the present invention is a dry film having a resin layer made of the curable resin composition of the embodiment (1).

[0014] A third aspect of the present invention relates to a cured product obtained by curing the resin layer in the curable resin composition of the first aspect or the dry film of the second aspect.

[0015] The fourth aspect of the present invention is a printed wiring board having the cured product of the third aspect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] When isomers exist in the described compounds, all possible isomers can be used in the present invention unless otherwise specified.

[0017] In this specification, phenols that are used as raw materials for polyphenylene ether (PPE) and can become structural units of polyphenylene ether are collectively referred to as "raw material phenols".

[0018] In this specification, when the raw material phenols are described using expressions such as "ortho position" and "para position", the position of the phenolic hydroxyl group is taken as the reference (ipso position) unless otherwise specified.

[0019] In this specification, when simply expressed as "ortho position" or the like, it means "at least one of the ortho positions", etc. Therefore, unless there is any particular contradiction, when simply expressed as "ortho position", it may be interpreted as indicating either one of the ortho positions, or it may be interpreted as indicating both ortho positions.

[0020] In this specification, monohydric phenols are mainly disclosed as the raw material phenols, but polyhydric phenols may also be used as the raw material phenols within the range that does not impair the effects of the present invention.

[0021] In this specification, when the upper limit and the lower limit of a numerical range are separately described, all combinations of the lower limit and the upper limit are substantially described, provided that there is no contradiction.

[0022] In this specification, unless otherwise specified, various measurements are performed at room temperature (25° C.).

[0023] In this specification, the number average molecular weight and weight average molecular weight are values ​​measured by gel permeation chromatography (GPC) and converted using a calibration curve prepared using standard polystyrene.

[0024] In this specification, there may be cases where the components contained in the curable resin composition and the components contained in the curable resin layer or the like which is a dried coating film of the curable resin composition are described without distinction.

[0025] Hereinafter, the curable resin composition, the dry film, the cured product, the printed wiring board, the electronic part, and the like will be described, but the present invention is not limited to the following in any way.

[0026] <<<<Composition of Curable Resin Composition>>>> The curable resin composition according to the present disclosure contains a polyphenylene ether having a branched structure and a functional group containing an unsaturated carbon bond, and a compound having a (meth)acrylate group. The curable resin composition according to the present disclosure may contain a filler. The curable resin composition according to the present disclosure may be a varnish containing an organic solvent. The curable resin composition according to the present disclosure may contain other components.

[0027] Hereinafter, a compound having a (meth)acrylate group may be referred to as a (meth)acrylate-based compound.

[0028] <<<Polyphenylene ether>>> The polyphenylene ether of the present disclosure is a polyphenylene ether having a functional group containing an unsaturated carbon bond and having a branched structure.

[0029] Here, polyphenylene ether having a functional group containing an unsaturated carbon bond and a branched structure is sometimes referred to as reactive branched polyphenylene ether.

[0030] Hereinafter, the polyphenylene ether having a branched structure will be described, and then the reactive branched polyphenylene ether will be described.

[0031] The polyphenylene ether having a branched structure is obtained from a raw material phenol containing a phenol satisfying at least condition 1. (Condition 1) Contains hydrogen atoms at the ortho and para positions

[0032] Phenols satisfying condition 1 {e.g., phenols (A) and (B) described later} have a hydrogen atom at the ortho position, and therefore, when oxidatively polymerized with a phenol, an ether bond can be formed not only at the ipso position and para position but also at the ortho position, making it possible to form a branched chain structure.

[0033] In this way, a part of the structure of the polyphenylene ether having a branched structure is branched by a benzene ring having ether bonds at least at three positions, i.e., the ipso position, the ortho position, and the para position. The polyphenylene ether having this branched structure is considered to be, for example, a polyphenylene ether compound having at least a branched structure represented by formula (i) in the skeleton.

[0034] [ka]

[0035] In formula (i), R a ~R k are each independently a hydrogen atom or a hydrocarbon group having 1 to 15 carbon atoms (preferably, 1 to 12 carbon atoms).

[0036] In addition, the reactive branched polyphenylene ether has a functional group containing an unsaturated carbon bond, which has the effect of imparting crosslinkability and excellent reactivity, resulting in excellent properties of the cured product.

[0037] The method for introducing such a functional group containing an unsaturated carbon bond into a polyphenylene ether having a branched structure is not particularly limited, but may be, for example, As raw phenols, This method comprises adding a phenol (A) which satisfies at least both the following condition 1 and the following condition 2 (Mode 1), or adding a mixture of a phenol (B) which satisfies at least the following condition 1 but does not satisfy the following condition 2, and a phenol (C) which does not satisfy the following condition 1 but satisfies the following condition 2 (Mode 2). (Condition 1) Contains hydrogen atoms at the ortho and para positions (Condition 2) It has a hydrogen atom at the para position and a functional group containing an unsaturated carbon bond.

[0038] The reactive branched polyphenylene ether obtained by the above-mentioned method uses at least a phenol satisfying condition 2 {e.g., either phenol (A) or phenol (C)} as a phenol raw material, and therefore has crosslinkability due to a hydrocarbon group containing at least an unsaturated carbon bond.

[0039] That is, the reactive branched polyphenylene ether obtained by the above method is, for example, a polyphenylene ether having at least a branched structure as shown in formula (i) in the skeleton, and is considered to be a compound having a hydrocarbon group containing at least one unsaturated carbon bond as a functional group. a ~R k At least one of the above is a hydrocarbon group having an unsaturated carbon bond.

[0040] In particular, in the above embodiment 2, from the industrial and economical viewpoints, it is preferable that the phenol (B) is at least one of o-cresol, 2-phenylphenol, 2-dodecylphenol, and phenol, and the phenol (C) is 2-allyl-6-methylphenol.

[0041] Here, the raw material phenols constituting the reactive branched polyphenylene ether may contain other phenols not satisfying condition 1 within a range that does not impair the effects of the present disclosure.

[0042] Examples of such other phenols include phenols (C) and (D) described later, and phenols that do not have a hydrogen atom at the para position. In particular, when phenols (C) and (D) described later are oxidatively polymerized, ether bonds are formed at the ipso and para positions, and the phenols are polymerized in a linear chain. Therefore, in order to increase the molecular weight of polyphenylene ether, it is preferable to further include phenols (C) and (D) as raw material phenols.

[0043] The phenols (A) to (D) will be described in more detail below.

[0044] The phenol (A) is a phenol that satisfies both the condition 1 and the condition 2 as described above, i.e., a phenol that has hydrogen atoms at the ortho-position and the para-position and has a functional group containing an unsaturated carbon bond, and is preferably a phenol (a) represented by the following formula (1).

[0045] [ka]

[0046] In formula (1), R1 to R3 are each independently a hydrogen atom or a hydrocarbon group having 1 to 15 carbon atoms. However, at least one of R1 to R3 is a hydrocarbon group having an unsaturated carbon bond. From the viewpoint of facilitating polymerization by oxidative polymerization, the hydrocarbon group preferably has 1 to 12 carbon atoms.

[0047] Examples of the phenol (a) represented by formula (1) include o-vinylphenol, m-vinylphenol, o-allylphenol, m-allylphenol, 3-vinyl-6-methylphenol, 3-vinyl-6-ethylphenol, 3-vinyl-5-methylphenol, 3-vinyl-5-ethylphenol, 3-allyl-6-methylphenol, 3-allyl-6-ethylphenol, 3-allyl-5-methylphenol, 3-allyl-5-ethylphenol, etc. The phenol represented by formula (1) may be used alone or in combination of two or more.

[0048] As described above, the phenol (B) is a phenol that satisfies the condition 1 but does not satisfy the condition 2, i.e., a phenol that has hydrogen atoms at the ortho- and para-positions and does not have a functional group containing an unsaturated carbon bond, and is preferably a phenol (b) represented by the following formula (2).

[0049] [ka]

[0050] In formula (2), R4 to R6 are each independently a hydrogen atom or a hydrocarbon group having 1 to 15 carbon atoms. However, R4 to R6 do not have an unsaturated carbon bond. From the viewpoint of facilitating polymerization by oxidative polymerization, the hydrocarbon group preferably has 1 to 12 carbon atoms.

[0051] Examples of the phenol (b) represented by formula (2) include phenol, o-cresol, m-cresol, o-ethylphenol, m-ethylphenol, 2,3-xylenol, 2,5-xylenol, 3,5-xylenol, o-tert-butylphenol, m-tert-butylphenol, o-phenylphenol, m-phenylphenol, 2-dodecylphenol, etc. The phenol represented by formula (2) may be used alone or in combination of two or more.

[0052] As described above, the phenol (C) is a phenol that does not satisfy condition 1 but satisfies condition 2, i.e., a phenol that has a hydrogen atom at the para position, does not have a hydrogen atom at the ortho position, and has a functional group containing an unsaturated carbon bond, and is preferably a phenol (c) represented by the following formula (3).

[0053] [ka]

[0054] In formula (3), R7 and R 10 are each independently a hydrocarbon group having 1 to 15 carbon atoms, and R8 and R9 are each independently a hydrogen atom or a hydrocarbon group having 1 to 15 carbon atoms. 10 At least one of the above is a hydrocarbon group having an unsaturated carbon bond. From the viewpoint of facilitating polymerization into a polymer during oxidative polymerization, the hydrocarbon group preferably has 1 to 12 carbon atoms.

[0055] Examples of the phenols (c) represented by formula (3) include 2-allyl-6-methylphenol, 2-allyl-6-ethylphenol, 2-allyl-6-phenylphenol, 2-allyl-6-styrylphenol, 2,6-divinylphenol, 2,6-diallylphenol, 2,6-diisopropenylphenol, 2,6-dibutenylphenol, 2,6-diisobutenylphenol, 2,6-diisopentenylphenol, 2-methyl-6-styrylphenol, 2-vinyl-6-methylphenol, 2-vinyl-6-ethylphenol, etc. The phenols represented by formula (3) may be used alone or in combination of two or more.

[0056] As described above, the phenol (D) is a phenol having a hydrogen atom at the para position, no hydrogen atom at the ortho position, and no functional group containing an unsaturated carbon bond, and is preferably a phenol (d) represented by the following formula (4).

[0057] [ka]

[0058] In formula (4), R 11 and R 14 are each independently a hydrocarbon group having 1 to 15 carbon atoms and no unsaturated carbon bond, R 12 and R 13 are each independently a hydrogen atom or a hydrocarbon group having 1 to 15 carbon atoms and no unsaturated carbon bond. From the viewpoint of facilitating polymerization by oxidative polymerization, the hydrocarbon group preferably has 1 to 12 carbon atoms.

[0059] Examples of the phenol (d) represented by formula (4) include 2,6-dimethylphenol, 2,3,6-trimethylphenol, 2-methyl-6-ethylphenol, 2-ethyl-6-n-propylphenol, 2-methyl-6-n-butylphenol, 2-methyl-6-phenylphenol, 2,6-diphenylphenol, 2,6-ditolylphenol, etc. The phenol represented by formula (4) may be used alone or in combination of two or more.

[0060] Here, in the present disclosure, examples of the hydrocarbon group include an alkyl group, a cycloalkyl group, an aryl group, an alkenyl group, and an alkynyl group, and preferably an alkyl group, an aryl group, and an alkenyl group. Examples of the hydrocarbon group having an unsaturated carbon bond include an alkenyl group and an alkynyl group. These hydrocarbon groups may be linear or branched.

[0061] When the reactive branched polyphenylene ethers as described above are used as a component of a curable composition, one type may be used alone, or two or more types may be used.

[0062] The ratio of the phenols satisfying condition 1 to the total of the raw material phenols used in the synthesis of the reactive branched polyphenylene ether is preferably 1 to 50 mol %.

[0063] The ratio of the phenols satisfying the condition 2 to the total amount of the raw material phenols is preferably 0.5 to 99 mol %, and more preferably 1 to 99 mol %.

[0064] The number average molecular weight of the reactive branched polyphenylene ether is preferably 2,000 to 30,000, more preferably 5,000 to 30,000, further preferably 8,000 to 30,000, and particularly preferably 8,000 to 25,000. By setting the molecular weight within such a range, it is possible to improve the film-forming property of the curable composition while maintaining the solubility in the solvent. Furthermore, it is preferable that the polydispersity index (PDI: weight average molecular weight / number average molecular weight) is 1.5 to 20.

[0065] The molecular weight of the reactive branched polyphenylene ether depends on the type of raw material phenol used, but can be adjusted by changing the reaction temperature, reaction time, etc. during synthesis. In addition, by increasing the proportion of phenols that satisfy at least condition 2 among the raw material phenols, the polymerization reaction is suppressed, the rate of increase in molecular weight is slowed down, and it becomes easy to control the molecular weight of the reactive branched polyphenylene ether.

[0066] The content of the reactive branched polyphenylene ether in the curable resin composition is preferably 20 to 80 mass %, more preferably 30 to 60 mass %, based on the total amount of solids in the curable resin composition excluding the filler.

[0067] <<Production method of polyphenylene ether>> The reactive branched polyphenylene ether of the present disclosure can be produced by a known polyphenylene ether synthesis method, except that the raw material phenols and the ratio of the raw material phenols used are as described above. For example, it can be produced by the synthesis method disclosed in International Publication WO2020 / 017570.

[0068] <<<(Meth)acrylate compounds>>> The (meth)acrylate compound is a compound having at least one or more (meth)acrylate groups. More specifically, the (meth)acrylate group is a compound having at least one of an acrylate group represented by H2C=CH-C(=O)-O- and a methacrylate group represented by H2C=C(CH3)-C(=O)-O-.

[0069] The combined use of reactive branched polyphenylene ether and a (meth)acrylate compound is likely to provide an effect of improving embedding ability into irregularities and an effect of suppressing the occurrence of cracks during desmearing (desmear resistance). In addition, the combined use of reactive branched polyphenylene ether and a (meth)acrylate compound is likely to provide an effect of improving crosslink density, heat resistance, and the like, and also to maintain the low dielectric properties derived from the reactive branched polyphenylene ether.

[0070] The (meth)acrylate compound is not particularly limited and may be an aliphatic compound, an aromatic compound, a heterocyclic compound, an alicyclic compound, etc. The (meth)acrylate compound is preferably a compound that does not contain an aromatic ring.

[0071] The (meth)acrylate compound is preferably difunctional or higher, and more preferably difunctional or higher and tetrafunctional or lower.

[0072] Examples of bifunctional (meth)acrylate compounds not containing an aromatic ring include tricyclodecane dimethanol di(meth)acrylate, cyclohexane dimethanol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dioxane glycol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, and ethylene oxide-modified phosphate di(meth)acrylate.

[0073] Examples of trifunctional or higher (meth)acrylate compounds not containing an aromatic ring include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, tris((meth)acryloxyethyl)isocyanurate, isocyanuric acid modified tri(meth)acrylate, 4-pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, propionic acid modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone modified dipentaerythritol hexa(meth)acrylate.

[0074] Examples of the difunctional or higher functional (meth)acrylate compounds containing an aromatic ring include propoxylated ethoxylated bisphenol A di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene.

[0075] The (meth)acrylate compound may be an oligomer having a (meth)acrylate group (for example, polyphenylene ether having a (meth)acrylate group), or the like.

[0076] The molecular weight of the (meth)acrylate compound is preferably not more than 3,000, more preferably not more than 1,000, and even more preferably not more than 500. By using such a (meth)acrylate compound, it is easy to obtain an effect of improving embedding ability into irregularities and an effect of suppressing the occurrence of cracks during desmear treatment (desmear resistance).

[0077] The (meth)acrylate group equivalent of the (meth)acrylate compound [molecular weight of the (meth)acrylate compound / number of (meth)acrylate groups in one molecule] is preferably 80 or more, more preferably 100 or more. Also, it is preferably 1,000 or less, more preferably 500 or less, and even more preferably 200 or less. By using such a (meth)acrylate compound, it is easy to obtain an effect of improving embedding ability into irregularities and an effect of suppressing the occurrence of cracks during desmear treatment (desmear resistance).

[0078] The content of the (meth)acrylate compound in the curable resin composition is, in terms of solid content, preferably 10 parts by mass or more, more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, and particularly preferably 50 parts by mass or more, based on 100 parts by mass of the reactive branched polyphenylene ether in the curable resin composition. Also, it is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, even more preferably 120 parts by mass or less, and particularly preferably 100 parts by mass or less.

[0079] <<<Filler>>> Examples of the filler include inorganic fillers and organic fillers.

[0080] Examples of inorganic fillers that can be used include metal oxides such as silica, alumina, and titanium oxide; metal hydroxides such as aluminum hydroxide and magnesium hydroxide; clay minerals such as talc and mica; fillers having a ferovskite crystal structure such as barium titanate and strontium titanate; boron nitride, aluminum borate, barium sulfate, and calcium carbonate.

[0081] Examples of organic fillers that can be used include fluororesin fillers such as polytetrafluoroethylene (PTFE), tetrafluoroethylene / ethylene copolymer (ETFE), tetrafluoroethylene / perfluoroalkylvinyl ether copolymer (PFA), tetrafluoroethylene / hexafluoropropylene copolymer (FEP), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), and polyvinyl fluoride (PVF); and hydrocarbon resin fillers such as cycloolefin polymer (COP) and cycloolefin copolymer (COC).

[0082] The filler is preferably silica. The average particle size of the silica is preferably 0.01 to 5 μm, more preferably 0.01 to 1 μm. The average particle size can be determined as the median diameter (d50, volume basis) based on cumulative distribution from the particle size distribution measured by a laser diffraction / scattering method using a commercially available laser diffraction / scattering particle size distribution measuring device. The average particle size of the silica refers to the value measured as described above for the powder before preparing (pre-mixing, kneading) the resin composition.

[0083] The filler may be surface-treated with a coupling agent. By treating the surface with a silane coupling agent, the dispersibility with the reactive branched polyphenylene ether can be improved. Also, the affinity with an organic solvent can be improved.

[0084] The content of the filler in the curable resin composition is, in terms of solid content, preferably 20 parts by mass or more, more preferably 50 parts by mass or more, or even more preferably 100 parts by mass or more, relative to 100 parts by mass of the reactive branched polyphenylene ether in the curable resin composition, and is preferably 1500 parts by mass or less, more preferably 1000 parts by mass or less, and even more preferably 800 parts by mass or less.

[0085] <<<Organic solvents>>> The organic solvent that can dissolve the reactive branched polyphenylene ether can be used, and is not particularly limited, and examples thereof include chloroform, methylene chloride, toluene, etc. In addition, solvents such as N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), cyclohexanone, propylene glycol monomethyl ether acetate (PMA), diethylene glycol monoethyl ether acetate (CA), methyl ethyl ketone, ethyl acetate, and anisole may be used. The organic solvent may be used alone or in combination of two or more kinds.

[0086] <<<Other ingredients>>> Examples of the other components include peroxides, crosslinking curing agents, elastomers, polyphenylene ethers other than reactive branched polyphenylene ethers, resins and polymer components such as maleimide resins, sensitizers, adhesion aids, surfactants, leveling agents, plasticizers, adhesion agents, colorants, fibers, silane coupling agents, flame retardants, cellulose nanofibers, dispersants, thermosetting catalysts, thickeners, defoamers, antioxidants, rust inhibitors, adhesion promoters, etc. The other components may be used alone or in combination of two or more. It is preferable to use other components with low dielectric properties in combination.

[0087] The content of other components in the curable resin composition may be appropriately adjusted depending on the application, etc. For example, the total content of other components in the curable resin composition is 200 parts by mass or less, 150 parts by mass or less, or 100 parts by mass or less, based on 100 parts by mass of the reactive branched polyphenylene ether in the curable resin composition, calculated as solid content.

[0088] <<Peroxide>> Peroxides include methyl ethyl ketone peroxide, methyl acetoacetate peroxide, acetylacetonate peroxide, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(t-butylperoxy)butane, t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, di-t-butyl hydroperoxide, t-butyl hydroperoxide, dicumyl peroxide, 2,5-di Examples of the peroxide include methyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-butene, acetyl peroxide, octanoyl peroxide, lauroyl peroxide, benzoyl peroxide, m-toluyl peroxide, diisopropyl peroxydicarbonate, t-butylene peroxybenzoate, di-t-butyl peroxide, t-butylperoxyisopropyl monocarbonate, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, etc. Only one type of peroxide may be used, or two or more types may be used.

[0089] The content of the peroxide in the curable resin composition is preferably 0.1 to 10 parts by mass, or 1 to 5 parts by mass, based on 100 parts by mass of the reactive branched polyphenylene ether in the curable resin composition, calculated as solid content.

[0090] <<Cross-linking hardener>> As the crosslinking type curing agent, one having good compatibility with reactive branched polyphenylene ether is used, and examples thereof include polyfunctional vinyl compounds such as divinylbenzene, divinylnaphthalene, and divinylbiphenyl; vinylbenzyl ether compounds synthesized by the reaction of phenol with vinylbenzyl chloride; allyl ether compounds synthesized by the reaction of styrene monomer, phenol with allyl chloride; and further, trialkenyl isocyanurate. As the crosslinking type curing agent, trialkenyl isocyanurate having particularly good compatibility with reactive branched polyphenylene ether is preferred, and specifically, triallyl isocyanurate (hereinafter, TAIC (registered trademark)) and triallyl cyanurate (hereinafter, TAC) are preferred. These exhibit low dielectric properties and can increase heat resistance. In particular, TAIC (registered trademark) is preferred because of its excellent compatibility with reactive branched polyphenylene ether.

[0091] The content of the crosslinking curing agent in the curable resin composition is preferably 1 to 100 parts by mass, or 10 to 80 parts by mass, based on 100 parts by mass of the reactive branched polyphenylene ether in the curable resin composition, calculated as solid content.

[0092] <<Elastomer>> The elastomer may be either a thermoplastic elastomer or a thermosetting elastomer. Examples of the thermoplastic elastomer include olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, acrylic-based elastomers, and silicone-based elastomers. Examples of thermosetting elastomers include diene-based synthetic rubbers such as polyisoprene rubber, polybutadiene rubber, styrene-butadiene rubber, polychloroprene rubber, nitrile rubber, and ethylene-propylene rubber; non-diene-based synthetic rubbers such as ethylene-propylene rubber, butyl rubber, acrylic rubber, polyurethane rubber, fluororubber, silicone rubber, and epichlorohydrin rubber; and natural rubber.

[0093] The content of the elastomer in the curable resin composition is preferably 10 to 100 parts by mass, or 40 to 80 parts by mass, based on 100 parts by mass of the reactive branched polyphenylene ether in the curable resin composition, calculated as solid content.

[0094] <<<<Dry film>>>> The dry film has a resin layer made of the curable resin composition of the present disclosure on a first film (support film).

[0095] The dry film can be obtained by uniformly applying the curable resin composition onto the first film using an appropriate method such as a blade coater, lip coater, comma coater, or film coater, and drying the composition to form a resin layer.

[0096] The dry film may have a second film (protective film) laminated on the surface. The second film and the first film may be made of the same film material or different films.

[0097] The film materials for the first film and the second film may be any of those known to be used for dry films.

[0098] As the first film, for example, a thermoplastic film such as a polyester film made of polyethylene terephthalate or the like having a thickness of 2 to 150 μm is used.

[0099] The second film may be a polyethylene film, a polypropylene film, or the like, but it is preferable that the adhesive strength with the resin layer is smaller than that of the first film.

[0100] The thickness of the resin layer on the dry film can be appropriately changed depending on the application, and is preferably 100 μm or less, more preferably in the range of 5 to 50 μm.

[0101] <<<<Cured product>>>> The method for obtaining a cured product from the curable resin composition of the present disclosure is not particularly limited, and can be appropriately changed depending on the composition of the curable resin composition. As an example, after the curable resin composition is applied (e.g., applied using an applicator, etc.) onto a substrate (including a substrate), a drying step may be carried out as necessary to remove the organic solvent in the composition, and then a thermal curing step may be carried out in which the thermosetting component in the composition is thermally crosslinked by heating.

[0102] As a coating method, for example, an organic solvent is used to adjust the viscosity to a level suitable for the coating method, and the composition is applied onto a substrate by a method such as an inkjet method, a dip coating method, a flow coating method, a roll coating method, a bar coater method, a screen printing method, or a curtain coating method, and then the organic solvent contained in the composition is evaporated and dried at a temperature of about 60 to 100° C., thereby forming a tack-free resin layer.

[0103] Drying can be carried out using a hot air circulation drying oven, IR oven, hot plate, convection oven, etc. (a method in which hot air in the dryer is brought into countercurrent contact using a heat source that uses steam for air heating, or a method in which hot air is blown onto the support from a nozzle).

[0104] Examples of the thermal curing method include heating using an inert gas oven, a hot plate, a vacuum oven, a vacuum press, or the like.

[0105] The conditions for each step (for example, coating thickness, temperature and time in drying and heating steps) may be appropriately changed depending on the composition and application of the curable resin composition.

[0106] The cured product can also be obtained by curing the resin layer of the above-mentioned dry film.

[0107] In addition, when the above-mentioned dry film is used, the resin layer can be formed on the substrate by laminating the resin layer on the substrate with a laminator or the like so that the resin layer contacts the substrate, and then peeling off the first film. The lamination of the dry film to the substrate is preferably performed under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a substrate on which a circuit is formed is used, even if the surface of the circuit substrate is uneven, the dry film adheres to the circuit substrate, so that no air bubbles are mixed in, and the filling of the recesses on the substrate surface is also improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 140°C.

[0108] <<<<Printed wiring boards or electronic components>>>> The printed wiring board or electronic part has the above-mentioned cured product and has excellent peel strength and the like, and can be used for various applications.

[0109] Its applications are not particularly limited, but preferred applications include large-capacity, high-speed communications such as those represented by the fifth-generation communication system (5G) and millimeter-wave radar for automotive ADAS (advanced driving systems).

[0110] Here, the curable resin composition according to the present disclosure can be preferably used in a manufacturing process for a printed wiring board or an electronic component, which includes a desmear treatment.

[0111] The method of carrying out the desmear treatment will be outlined below.

[0112] The curable resin composition according to the present disclosure is applied onto a substrate (including a board) and dried, or a resin layer on a dry film is laminated onto the substrate to form a resin layer. Examples of the substrate include printed wiring boards and flexible printed wiring boards on which circuits have been formed in advance using copper or the like, metal substrates, glass substrates, ceramic substrates, wafer plates, metal foils such as copper foil, films such as polyimide films, polyester films, and polyethylene naphthalate (PEN) films, glass cloth, and fibers such as aramid fibers.

[0113] The resin layer is then cured (for example, thermally cured).

[0114] Next, holes are formed in the cured layer using a laser such as a CO2 laser or a UV-YAG laser, or a drill. The holes may be either through holes intended to provide electrical continuity between the front and back of the substrate, or bottomed holes (via holes) intended to provide electrical continuity between the circuit on the substrate and the circuit on the second layer.

[0115] Next, after the holes (holes) are formed, residues (smears) generated by processing are removed with a desmear solution.

[0116] Next, a plating layer is formed on the surface of the cured layer. The plating metal is not particularly limited and may be copper, tin, solder, nickel, or the like, and may be used in combination. The method for forming the plating layer is not particularly limited and may be electroless plating, electrolytic plating, or a combination thereof.

[0117] Furthermore, by repeating the formation of such resin layers and plating layers, a multi-layer printed wiring board may be formed.

[0118] When the curable resin composition according to the present disclosure is used, the occurrence of cracks and the like can be suppressed when such a desmear treatment is performed. Therefore, even when a substrate having surface irregularities that are particularly prone to cracking is used, the occurrence of cracks can be suppressed.

[0119] In addition, when a substrate having surface irregularities is used, the curable resin composition according to the present disclosure is likely to give a cured product with excellent embedding properties (flatness). Examples of substrates having surface irregularities include substrates having degassing holes and substrates having wiring patterns. The substrate having degassing holes is a substrate in which holes are provided in advance in a metal layer provided on a core layer, and the metal layer can be prevented from swelling by promoting the escape of gas generated from the core layer during heating or the like. The diameter of the degassing holes is not particularly limited, and is 10 to 500 μm, for example. The pitch of the degassing holes is not particularly limited, and is 0.1 to 5 mm, for example. EXAMPLES

[0120] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to the following.

[0121] <<<Preparation of varnish from curable resin composition>>> <<Example 1>> <Synthesis of reactive branched PPE> In a 500 mL separable flask, 19.8 g (0.16 mol) of 2,6-dimethylphenol and 2.42 g (0.018 mol) of 2-allylphenol were added, and the resulting mixture was dissolved in 261 g of toluene. Furthermore, di-μ-hydroxo-bis[(N,N,N',-tetramethylethylenediamine)copper(II)] chloride (Cu / TMEDA) was adjusted to 0.18 wt% and tetramethylethylenediamine (TMEDA) to 0.16 wt%, and the reaction solution was stirred at a stirring speed of 200 rpm using a four-blade paddle blade while blowing dry air into the reaction solution at a flow rate of 75 mL / min, and reacted at 40°C for a predetermined time to obtain a reaction solution containing polyphenylene ether. After stopping heating the reaction solution and blowing in dry air, di-μ-hydroxo-bis[(N,N,N',N'-tetramethylethylenediamine)copper(II)] chloride (Cu / TMEDA) was removed by filtration, reprecipitated in a mixture of 1,200 mL of methanol, 4.0 mL of concentrated hydrochloric acid, and 7.0 mL of H2O2, filtered under reduced pressure, washed with methanol, and dried at 80°C for 24 hours to obtain a reactive branched polyphenylene ether. The number average molecular weight of the obtained reactive branched polyphenylene ether was 13,000 and the weight average molecular weight was 45,000.

[0122] <Preparation of Varnish> An organic solvent was added to 100 parts by mass of reactive branched PPE and 24.5 parts by mass of styrene-based elastomer (manufactured by Asahi Kasei Corporation: product name "Tuftec H1051"), and the mixture was stirred at 40°C for 30 minutes to completely dissolve the mixture. To the reactive branched PPE resin solution thus obtained, 60 parts by mass of tricyclodecane dimethanol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.: product name "A-DCP"), 60 parts by mass of triallylisocyanurate (manufactured by Mitsubishi Chemical Corporation: product name "TAIC"), and 165 parts by mass of spherical silica filler (manufactured by Admatechs Co., Ltd.: product name "SC2050-HNF") were added and mixed, and then dispersed using a three-roll mill. Finally, 4 parts by mass of α,α'-bis(t-butylperoxy-m-isopropyl)benzene (manufactured by NOF Corporation: product name "Perbutyl P-40"), which is a peroxide, was added and stirred with a magnetic stirrer. In this manner, a varnish of the curable resin composition of Example 1 was obtained.

[0123] <<Example 2>> A varnish of the curable resin composition of Example 2 was obtained in the same manner as in Example 1, except that A-DCP: 30 parts by mass was used.

[0124] <<Example 3>> A varnish of the curable resin composition of Example 3 was obtained in the same manner as in Example 1, except that A-DCP: 15 parts by mass was used.

[0125] <<Example 4>> A varnish of the curable resin composition of Example 4 was obtained in the same manner as in Example 1, except that TAIC was not added and the amounts of A-DCP: 75 parts by mass, Tuftec H1051: 75 parts by mass, and spherical silica filler: 169 parts by mass were used.

[0126] <<Example 5>> A varnish of the curable resin composition of Example 5 was obtained in the same manner as in Example 2, except that Tuftec H1051 was not added, and A-DCP: 100 parts by mass and spherical silica filler: 136 parts by mass were used.

[0127] <<Example 6>> A varnish of the curable resin composition of Example 6 was obtained in the same manner as in Example 3, except that dioxane glycol diacrylate ("A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.) was used instead of A-DCP.

[0128] <<Example 7>> A varnish of the curable resin composition of Example 7 was obtained in the same manner as in Example 3, except that A-DCP was changed to 1,6-hexanediol diacrylate ("HDDA" manufactured by Nippon Shokubai Co., Ltd.).

[0129] <<Example 8>> A varnish of the curable resin composition of Example 8 was obtained in the same manner as in Example 5, except that A-DCP was changed to ditrimethylolpropane tetraacrylate ("Aronix M408" manufactured by Toagosei Co., Ltd.).

[0130] <<Example 9>> A varnish of the curable resin composition of Example 7 was obtained in the same manner as in Example 4, except that Tuftec H1051 was 50 parts by mass and A-DCP was 100 parts by mass of isocyanuric acid EO-modified di- and triacrylate ("Aronix M313" manufactured by Toagosei Co., Ltd.).

[0131] <<Example 10>> A varnish of the curable resin composition of Example 10 was obtained in the same manner as in Example 9, except that ARONIX M313 was replaced with "SA-9000" (reactive low molecular weight polyphenylene ether) manufactured by SABIC Japan LLC.

[0132] <<Comparative Example 1>> A varnish of the curable resin composition of Comparative Example 1 was obtained in the same manner as in Example 1, except that no A-DCP was added, and Perbutyl P-40: 3 parts by mass and spherical silica filler: 123 parts by mass were used.

[0133] <<Comparative Example 2>> A varnish of the curable resin composition of Comparative Example 2 was obtained in the same manner as in Example 5, except that A-DCP was changed to "EPICLON NE-X-0470S" manufactured by DIC Corporation.

[0134] <<Comparative Example 3>> A varnish of the curable resin composition of Comparative Example 3 was obtained in the same manner as in Example 5, except that "SLK2600" manufactured by Shin-Etsu Chemical Co., Ltd. was used as A-DCP.

[0135] <<Comparative Example 4>> A varnish of the curable resin composition of Comparative Example 4 was obtained in the same manner as in Example 5, except that TAIC was used instead of A-DCP.

[0136] <<<Evaluation>>> <<Preparation of test board>> The varnish of the curable resin composition of each Example and Comparative Example was applied with an applicator onto a 38 μm thick PET film (manufactured by Toray Industries, Inc.: product name "R80") so that the thickness after drying would be 35 μm, and then dried at 90°C for 15 minutes in a hot air circulation drying oven to obtain each test dry film.

[0137] Each test dry film was placed on both sides of a copper-clad laminate with a copper thickness of 35 μm, a degassing hole diameter of 200 μm, and a large number of degassing structures with a pitch of 0.5 mm, so that the resin composition of the dry film was in contact with each other. After lamination at 140°C and 0.8 MPa using a vacuum laminator (Nikko Materials Co., Ltd. "CVP-600"), the plate was completely filled with nitrogen using an inert oven, heated to 200°C, and held for 60 minutes to prepare a test board with each resin layer.

[0138] <<Desmear processing>> The surface of each test substrate was desmeared using a commercially available desmearing solution. Specifically, the test substrate from which the PET had been peeled off was immersed in a swelling solution (Atotech Japan's "Swelling Dip Securigant P") at 60°C for 5 minutes, then in a roughening solution (Atotech Japan's "Concentrate Compact CP") at 80°C for 20 minutes, and then in a neutralizing solution (Atotech Japan's "Reduction Securigant P500") at 40°C for 5 minutes.

[0139] <<Evaluation of cracks after desmear>> The surface layer around the degassing holes after desmearing in the test substrates produced in each of the Examples and Comparative Examples was observed at 150x magnification using a digital microscope (Keyence Corporation, VHX-5000) to evaluate cracks. The number of cracks occurring in the surface layer around 100 degassing holes was counted and evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 1 and 2.

[0140] <Evaluation criteria> "◎": When the number of degassing holes where cracks occurred is 0 "Good": The number of degassing holes where cracks have occurred is 1 or more but less than 3 "△": When the number of degassing holes where cracks have occurred is 3 or more but less than 10 "X": When the number of degassing holes where cracks have occurred is 10 or more

[0141] <<Evaluation of embeddability>> The surface layer around the degassing holes after curing in the test substrates produced in each of the examples and comparative examples was observed at 150x magnification using a digital microscope (Keyence Corporation, VHX-5000) to evaluate the embeddability. The number of degassing holes with poor embedding in the surface layer around 100 degassing holes was counted and evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 1 and 2.

[0142] <Evaluation criteria> "◎": The number of defective degassing holes is 0 "Good": If the number of degassing holes with poor filling is 1 or more but less than 5 "X": When the number of degassing holes with poor filling is 5 or more

[0143] [Table 1]

[0144] [Table 2]

Claims

1. A curable resin composition comprising: a polyphenylene ether having a branched structure and a functional group containing an unsaturated carbon bond; and a compound having a (meth)acrylate group.

2. The curable resin composition according to claim 1 , wherein the content of the compound having a (meth)acrylate group is 15 parts by mass or more per 100 parts by mass of the polyphenylene ether, calculated as a solid content.

3. The curable resin composition according to claim 1, wherein the content of the compound having a (meth)acrylate group is 30 parts by mass or more per 100 parts by mass of the polyphenylene ether, calculated as a solid content.

4. The curable resin composition according to claim 1, wherein the compound having a (meth)acrylate group has a molecular weight of 3,000 or less.

5. The curable resin composition according to claim 1 , wherein the compound having a (meth)acrylate group is a compound not containing an aromatic ring.

6. A dry film having a resin layer made of the curable resin composition according to claim 1.

7. A cured product obtained by curing the resin layer in the curable resin composition according to claim 1 or the dry film according to claim 6.

8. A printed wiring board having the cured product according to claim 7.

Citation Information

Patent Citations

  • Curable composition, composition for application, cured film, laser processing method, and manufacturing method for multi-layer wiring structure

    WO2013073638A1

  • Resin composition, prepreg, resin-coated film, resin-coated metal foil, metal-clad laminate, and wiring board

    WO2018159080A1

  • Inter-layer adhesive film for multilayered printed wiring board and multilayered printed wiring board using the same

    JP1999087927A

Cited By

  • Curable resin composition, dry film, cured product, and printed wiring board

    JP2026081190A

  • Curable composition, dry film, cured product, and printed wiring board

    WO2026186692A1