Absorber and absorbent article

The absorbent body with a continuous skeleton and pores addresses the challenge of thinness and absorption efficiency in absorbent articles by using a crosslinked polymer with -COONa groups to expand and absorb fluids rapidly and uniformly.

JP2024147542APending Publication Date: 2024-10-16UNI CHARM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024094413
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2024-06-11
Publication Date
2024-10-16

AI Technical Summary

Technical Problem

Existing absorbent articles face challenges in achieving both thinness and efficient absorption of body fluids, with absorbent resin particles offering poor absorption speed and combined use with hydrophilic fibers resulting in bulkiness.

Method used

An absorbent body comprising a polymer absorbent with a continuous skeleton and continuous pores, made from a crosslinked polymer of acrylic ester and a compound with two vinyl groups, containing at least one -COONa group, which expands to facilitate fluid absorption through capillary action.

Benefits of technology

The absorbent body effectively absorbs body fluids quickly and efficiently, reducing bulkiness and minimizing changes in absorption capacity due to fluid composition, while allowing rapid transfer and retention of fluids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147542000001_ABST
    Figure 2024147542000001_ABST
Patent Text Reader

Abstract

To provide an absorber and an absorbent article that are capable of readily absorbing bodily fluids.SOLUTION: The present invention pertains to an absorber for absorbing bodily fluids, the absorber comprising a polymer absorbent provided with a continuous skeleton and continuous pores, the polymer absorbent being a hydrolysate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups per molecule, and the polymer absorbent containing at least one -COONa group.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an absorbent body and an absorbent article. [Background technology]

[0002] Conventionally, absorbent articles such as disposable diapers and sanitary napkins that use superabsorbent polymers (so-called "SAP") with high absorption capacity have been known. For example, as disclosed in Patent Document 1, an absorbent article 30 using an absorbent body 15 that combines absorbent resin particles (superabsorbent polymers) 5 with high absorption capacity and hydrophilic fibers 13 such as pulp fibers with high absorption speed is disclosed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2013-018571 Summary of the Invention [Problem to be solved by the invention]

[0004] It is desirable to reduce the thickness of the absorbent article 30 from the viewpoints of distribution, storage, portability, etc. However, for example, when only the absorbent resin particles 5 are used as the absorbent body 15, the absorption speed is slow, and when bodily fluids are excreted with great force, the absorbent body 15 is not able to sufficiently absorb the bodily fluids. On the other hand, when the absorbent resin particles 5 are combined with the hydrophilic fibers 13, there is a risk that the absorbent body 15 becomes bulky.

[0005] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an absorbent body and an absorbent article that easily absorb body fluids. [Means for solving the problem]

[0006] The main invention for achieving the above object is an absorbent for absorbing body fluids, comprising a polymer absorbent having a continuous skeleton and continuous pores, the polymer absorbent being a hydrolysate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and containing at least one -COONa group. Other features of the present invention will become apparent from the following detailed description of the present invention and the accompanying drawings. Effect of the Invention

[0007] According to the present invention, when the polymer absorbent absorbs body fluid, the continuous skeleton is elongated, and as the continuous skeleton is elongated, the continuous pores also tend to expand, making it easier for the body fluid to be taken up into the continuous pores by capillary action, and making it easier for the polymer absorbent to absorb body fluid as an absorbent. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic perspective view of a pants-type disposable diaper 1. As shown in FIG. [Diagram 2] Fig. 2A is a schematic plan view of the diaper 1 in an unfolded and stretched state, as viewed from the skin side, and Fig. 2B is a schematic cross-sectional view taken along the line XX in Fig. 2A. [Diagram 3] FIG. 3 is a diagram illustrating the manufacturing process of the absorbent a. [Figure 4] FIG. 4 is a SEM photograph of absorbent a at a magnification of 50 times. [Diagram 5] FIG. 5 is a SEM photograph of absorbent a at a magnification of 100 times. [Figure 6] FIG. 6 is an SEM photograph of absorbent a at a magnification of 500 times. [Figure 7] FIG. 7 is a SEM photograph of absorbent a at a magnification of 1000 times. [Figure 8] FIG. 8 is a SEM photograph of absorbent a at a magnification of 1500 times. [Figure 9] FIG. 9 shows the measurement results of the absorbent a. [Figure 10]FIG. 10 is a graph showing the absorption rate and absorption amount test results of absorbent A. [Figure 11] FIG. 11 is a graph showing the absorption rate and absorption amount test results of the superabsorbent polymer of the comparative example. [Figure 12] Fig. 12A is an SEM photograph of the fracture surface of absorbent A. Fig. 12B is a mapping diagram of Na distribution in the same portion as Fig. 12A. [Figure 13] FIG. 13 is a graph showing the relationship between the amount of absorption and time for absorbents a and b when the liquid to be absorbed is pure water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] At least the following points will become apparent from the description of this specification and the accompanying drawings. The absorbent for absorbing body fluids comprises a polymer absorbent having a continuous skeleton and continuous pores, the polymer absorbent being a hydrolysate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and containing at least one -COONa group.

[0010] In such an absorbent, when the polymer absorbent absorbs body fluid, the continuous skeleton is elongated, and as the continuous skeleton is elongated, the continuous pores also tend to expand, making it easier for the body fluid to be taken up into the continuous pores by capillary action, and the absorbent is more likely to absorb body fluid.

[0011] In such an absorbent body, the polymer absorbent is desirably a monolithic absorbent.

[0012] According to such an absorbent, when the monolithic absorbent absorbs body fluid, the body fluid is easily taken up into the penetrating pores that have expanded as the continuous skeleton has been elongated, and the absorbent is easily able to absorb body fluid.

[0013] In such an absorbent, it is desirable that a first absorption weight, at which the polymer absorbent per unit weight absorbs an aqueous NaCl solution having a concentration of 0.9 wt%, and a second absorption weight, at which the polymer absorbent per unit weight absorbs an aqueous NaCl solution having a concentration of 0 to 2.0 wt%, be 0.5 to 1.9 times the second absorption weight.

[0014] With such an absorbent body, it is possible to reduce the risk that the absorption weight of the absorbent body will change due to the components of the body fluid.

[0015] In such an absorbent, a first polymer absorbent that has absorbed a 0.9 wt% NaCl aqueous solution by the first absorption weight, and a second polymer absorbent that has absorbed a 0-2.0 wt% NaCl aqueous solution by the second absorption weight are each dehydrated for a predetermined time using a centrifuge under conditions of 150 G and 850 rpm for 90 seconds, and it is desirable that the weight of the 0.9 wt% NaCl aqueous solution absorbed by the first polymer absorbent is 0.5 to 1.6 times the weight of the 0-2.0 wt% NaCl aqueous solution absorbed by the second polymer absorbent.

[0016] Such an absorbent body can reduce the risk of the water retention weight of the absorbent body being changed by the components of body fluids.

[0017] In such an absorbent, it is preferable that the weight of the NaCl aqueous solution having a concentration of 0.9 wt% absorbed by the first polymer absorbent after the dehydration is defined as a first water retention weight, and the weight of the NaCl aqueous solution having a concentration of 0 to 2.0 wt% absorbed by the second polymer absorbent after the dehydration is defined as a second water retention weight, and the value obtained by dividing the difference between the first absorption weight and the first water retention weight of the first polymer absorbent by the first absorption weight is 50 to 80%, and the value obtained by dividing the difference between the second absorption weight and the second water retention weight of the second polymer absorbent by the second absorption weight is 40 to 85%.

[0018] According to such an absorbent, the polymer absorbent can easily transfer the body fluid that it has absorbed to other substances, making it possible to repeatedly absorb and release water, and after the body fluid has been transferred to the outside of the polymer absorbent, the user is less likely to feel wet.

[0019] In such an absorbent, it is desirable that the time required for 2.0 g of the polymer absorbent to absorb 50 g of an aqueous NaCl solution having a concentration of 0.9 wt % by a vortex method is 1.0 to 10.0 seconds.

[0020] According to such an absorbent, the polymer absorbent can absorb liquid in a short time, and therefore, body fluids can be absorbed more quickly.

[0021] In such an absorbent, it is desirable that the absorption weight of the polymer absorbent when absorbing a CaCl2 aqueous solution with a concentration of 0.5 wt % is 13 times or more the weight of the polymer absorbent.

[0022] Such an absorbent material is capable of easily absorbing body fluids even if the body fluids contain a large amount of divalent ions.

[0023] In such an absorbent, it is desirable that after one minute has elapsed while the lower end of 1.0 g of the polymer absorbent is in contact with the water surface of a 0.9 wt % NaCl aqueous solution, the amount of the 0.9 wt % NaCl aqueous solution absorbed by the polymer absorbent is 15 ml or more.

[0024] According to such an absorbent body, the polymer absorbent can quickly absorb a large amount of liquid even in the direction against gravity, so that the absorbent body can easily absorb body fluids from various angles.

[0025] In such an absorbent, when a lower end of 2.0 g of the polymer absorbent under a load of 600 gw is brought into contact with the water surface of a 0.9 wt% NaCl aqueous solution, it is desirable that after 2 minutes, the amount of the 0.9 wt% NaCl aqueous solution absorbed by the polymer absorbent is 1.0 ml or more, and after 15 minutes, the amount of the 0.9 wt% NaCl aqueous solution absorbed by the polymer absorbent is 5.0 ml or more.

[0026] According to such an absorbent, even if a load is applied to the polymer absorbent, the absorbent can absorb liquid in a direction against gravity, so that the absorbent can easily absorb body fluids from various angles.

[0027] In such an absorbent body, it is desirable that the volume of voids of the pores per unit volume of the polymer absorbent is 85% or more.

[0028] According to such an absorbent, body fluids can be easily taken up into the interconnected pores by capillary action, and the absorbent can easily absorb body fluids.

[0029] In such an absorbent, it is desirable that the polymer absorbent contains 0.1 to 30.0% of cross-linked polymer residues.

[0030] When such an absorbent absorbs body fluid, the continuous skeleton extends, and as the continuous skeleton extends, the continuous pores also tend to expand, making it possible to form a polymer absorbent.

[0031] In such an absorbent material, it is desirable that the average diameter of the interconnected pores is 1 to 1000 μm.

[0032] According to such an absorbent, body fluids can be easily taken up into the interconnected pores by capillary action, and the absorbent can easily absorb body fluids.

[0033] In such an absorbent body, it is preferable that the absorbent body comprises the polymer absorbent and a polymer compound having a water retention capacity higher than that of the polymer absorbent.

[0034] With such an absorbent, the polymer absorbent, which easily absorbs body fluids through capillary action, first absorbs the body fluids while the polymer compound can retain the body fluids, so that the absorbent can quickly absorb body fluids and maintain a state in which the body fluids are retained.

[0035] In such an absorbent, it is desirable that the total ion exchange capacity of -COONa groups per unit weight of the polymer absorbent is 4.0 mg equivalent / g or more.

[0036] With such an absorbent, the polymer absorbent absorbs body fluids more easily than when the total ion exchange capacity of -COONa groups per unit weight is less than 4.0 mg equivalent / g, so that the continuous skeleton is more easily elongated, and as the continuous skeleton is elongated, the continuous pores are also more likely to expand, and body fluids are more easily taken up into the continuous pores by capillary action, making it easier for the absorbent to absorb body fluids.

[0037] It is desirable for the absorbent article to have any one of the above absorbents.

[0038] In such an absorbent article, when the polymer absorbent of the absorbent body absorbs body fluids, the continuous skeleton is elongated, and as the continuous skeleton is elongated, the continuous pores also tend to expand, making it easier for body fluids to be taken up into the continuous pores by capillary action, resulting in an absorbent article that easily absorbs body fluids.

[0039] === Implementation form === As an example of an absorbent article using the absorbent body according to the present embodiment, a so-called pants-type disposable diaper will be described. The absorbent body may be used as an absorbent body for absorbent articles such as not only pants-type disposable diapers but also tape-type disposable diapers, sanitary napkins, absorbent pads, disposable diapers for pets, and absorbent pads for pets. Disposable diapers and absorbent pads can be used for both infants and adults. Body fluids refer to liquids discharged from living organisms including not only humans but also animals. Examples include sweat, urine, feces, menstrual blood, vaginal discharge, breast milk, blood, and exudate.

[0040] ===Basic configuration of pants-type disposable diaper 1=== FIG. 1 is a schematic perspective view of a pants-type disposable diaper 1. FIG. 2A is a schematic plan view of the diaper 1 in an unfolded and stretched state, as viewed from the skin side. FIG. 2B is a schematic cross-sectional view taken along the line XX in FIG. 2A. The "unfolded state" refers to a state in which the diaper 1 is unfolded in a planar manner by separating and opening the joints between the side portion 30a of the ventral member 30 and the side portion 40a of the back member 40 on both sides of the diaper 1. The "stretched state" refers to a state in which the elastic members of the diaper 1 are stretched to such an extent that wrinkles in the diaper 1 are no longer visible. Specifically, the "stretched state" refers to a state in which the dimensions of each member constituting the diaper 1 (for example, the ventral member 30 described later, etc.) are stretched to the extent that the dimensions of the member are equal to or close to the dimensions of the member alone. The CC line in FIG. 2A and FIG. 2B is the center line in the left-right direction. For convenience, the adhesive is omitted in FIG. 2B.

[0041] As shown in FIG. 1, the pants-type diaper 1 has a vertical direction, a horizontal direction, and a front-rear direction, and the diaper 1 is formed with a waist opening BH and a pair of leg openings LH. The vertical direction of the diaper 1 in the unfolded and stretched state in FIG. 2A is referred to as the "longitudinal direction", one side of the longitudinal direction is also referred to as the "ventral side", and the other side is also referred to as the "dorsal side". In the front-rear direction, the side that faces the wearer's ventral side is referred to as the front side, and the side that faces the wearer's back is referred to as the rear side. In addition, the diaper 1 has a thickness direction as shown in FIG. 2B, and the side that contacts the wearer in the thickness direction is referred to as the skin side, and the opposite side is referred to as the non-skin side.

[0042] The diaper 1 is a so-called three-piece type, and includes an absorbent main body 10, an abdominal side member 30, and a back side member 40. The abdominal side member 30 and the back side member 40 are generally rectangular in plan view, with their longitudinal directions aligned with the left-right direction. The abdominal side member 30 covers the abdominal side of the wearer, and the back side member 40 covers the back side of the wearer. The absorbent main body 10 is generally rectangular in plan view. An abdominal end 10ea and a back end 10eb of the absorbent main body 10 are overlapped with the skin-side surfaces of the abdominal side member 30 and the back side member 40, respectively.

[0043] 2A, the diaper 1 in the unfolded and stretched state has a shape symmetrical with respect to the center line CC. The non-skin-side surfaces of the ventral end 10ea and the back end 10eb of the absorbent main body 10 are joined to the skin-side surfaces of the ventral member 30 and the back member 40 with an adhesive or the like (not shown), the absorbent main body 10 is folded in half so that the ventral member 30 and the back member 40 face each other, and both left and right side portions 30a of the ventral member 30 and both left and right side portions 40a of the back member 40 are welded and joined at the side welds SS, thereby forming the diaper 1 into a pants-type diaper.

[0044] The abdominal side member 30 and the back side member 40 each include a skin side sheet 31, 41 and a non-skin side sheet 32, 42 made of soft nonwoven fabric or the like, and a plurality of rubber threads 35, 45 that stretch in the left-right direction. The plurality of rubber threads 35, 45 are arranged side by side at intervals in the up-down direction, and are fixed between the two sheets (31 and 32, 41 and 42) in a state of being stretched in the left-right direction. Therefore, the abdominal side member 30 and the back side member 40 are stretchable in the left-right direction and fit the waist of the wearer.

[0045] The abdominal side member 30 is composed of a skin side sheet 31, a rubber thread 35, and a non-skin side sheet 32 ​​stacked in the thickness direction from the skin side, and joined together with an adhesive such as hot melt. Similarly, the dorsal side member 40 is composed of a skin side sheet 41, a rubber thread 45, and a non-skin side sheet 42 stacked in the thickness direction from the skin side, and joined together with an adhesive such as hot melt.

[0046] The skin side sheets 31, 41 and the non-skin side sheets 32, 42 are each made of a nonwoven fabric, specifically a spunbond nonwoven fabric. However, the present invention is not limited to this, and nonwoven fabrics such as SMS (spunbond / meltblown / spunbond) nonwoven fabrics may be used. In the present embodiment, a single fiber of polypropylene (PP), a thermoplastic resin, is used as the constituent fiber of the nonwoven fabric, but the present invention is not limited to this. For example, a single fiber of other thermoplastic resins such as polyethylene (PE) may be used, or composite fibers having a sheath-core structure such as PE and PP may be used. Furthermore, all of the skin side sheets 31, 41 and the non-skin side sheets 32, 42 do not have to be made of nonwoven fabric, and any one of the skin side sheets 31, 41 or the non-skin side sheets 32, 42 may be made of a soft sheet material other than nonwoven fabric.

[0047] The absorbent body 10 includes a top sheet 13, an absorbent body 11, and a back sheet 15, which are bonded together with an adhesive such as hot melt. The top sheet 13 may be a liquid-permeable sheet, and examples of such sheet include hydrophilic air-through nonwoven fabric and spunbond nonwoven fabric. The back sheet 15 may be a liquid-impermeable sheet, and examples of such sheet include polyethylene film, polypropylene film, and hydrophobic SMS nonwoven fabric. The top sheet 13 and the back sheet 15 are large enough to cover the entire absorbent body 11.

[0048] The absorbent body 10 has leg gathers LG that are provided at the left and right ends and stretch in the longitudinal direction, and three-dimensional gathers LSG that serve as leakage prevention walls for preventing side leakage and are provided on the skin side of the absorbent body 11. The leg gathers LG and three-dimensional gathers LSG each have elastic members 17 and 18 that stretch in the longitudinal direction (up and down direction), respectively.

[0049] The absorbent 11 has a generally rectangular shape in plan view and includes an absorbent core 11c that absorbs liquid. The absorbent core 11c is formed into a generally hourglass shape by wrapping a polymer absorbent (absorbent A) and a superabsorbent polymer (so-called SAP) in tissue or the like. The polymer absorbent (absorbent A) and the superabsorbent polymer (SAP) can each be, for example, granular, and it is preferable to use a sieve to make the particles have a particle size within a predetermined range. In the following description, a particulate polymer absorbent (absorbent A) will be described, but is not limited thereto. The polymer absorbent (absorbent A) used in absorbent articles such as the diaper 1 can be appropriately used in the form of particles, fine particles, blocks, sheets, threads, etc., depending on the usage state.

[0050] ===About polymer absorbents=== The polymer absorbent is a hydrolyzate of a crosslinked polymer of a (meth)acrylic acid ester and a compound having two or more vinyl groups in one molecule, and is a polymer compound having at least a -COONa group. The (meth)acrylic acid ester refers to an acrylic acid ester or a methacrylic acid ester. The polymer absorbent is a monolithic organic porous material having at least one or more -COONa groups in one molecule. It may further have a -COOH group. The -COONa groups are distributed approximately uniformly in the skeleton of the porous material. The term "monolithic" refers to a porous material having a penetrating hole and skeleton, and having a mesh-like bicontinuous structure.

[0051] The polymer absorbent, which is a hydrolysis product of a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene, has a continuous skeleton formed by an organic polymer having at least -COONa groups, and has interconnected holes (continuous pores) between the skeletons that serve as an absorption field for the liquid to be absorbed. In addition, since the hydrolysis treatment converts the -COOR groups (carboxylate ester groups) of the crosslinked polymer into -COONa groups or -COOH groups (Figure 3), the polymer absorbent may also have -COOR groups. The presence of -COOH groups and -COONa groups in the organic polymer that forms the continuous skeleton can be confirmed by analysis using infrared spectroscopy and a method for quantifying weakly acidic ion exchange groups.

[0052] Fig. 3 is a diagram illustrating the manufacturing process of absorbent A. In Fig. 3, the upper diagram shows the constituent raw materials for polymerization, the middle diagram shows monolith A as a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene, and the lower diagram shows absorbent A obtained by subjecting monolith A in the middle diagram to hydrolysis and drying treatment.

[0053] Hereinafter, a hydrolyzate of a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene (hereinafter also referred to as "absorbent A") will be described as an example of a polymer absorbent. The polymer absorbent is not limited to absorbent A, and may be a hydrolyzate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule. Hereinafter, "monolith A" refers to an organic porous body consisting of a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene before hydrolysis treatment, and is also referred to as a "monolithic organic porous body". "Absorbent A" refers to a hydrolyzate of a crosslinked polymer of (meth)acrylic acid ester and divinylbenzene (monolith A) after hydrolysis treatment and drying treatment. In the following description, absorbent A refers to a dry state.

[0054] The structure of absorbent A will be described. Absorbent A has a continuous skeleton and continuous pores. As shown in FIG. 3, absorbent A, which is an organic polymer forming a continuous skeleton, is obtained by cross-linking polymerization using (meth)acrylic acid ester, which is a polymerization monomer, and divinylbenzene, which is a cross-linking monomer, and hydrolyzing the resulting cross-linked polymer (monolith A). The organic polymer forming the continuous skeleton has, as structural units, a polymerized residue of an ethylene group (hereinafter also referred to as "structural unit X") and a cross-linked polymerized residue of divinylbenzene (hereinafter also referred to as "structural unit Y"). The polymerized residue of an ethylene group (structural unit X) in the organic polymer forming the continuous skeleton has a -COONa group, or a -COOH group and a -COONa group, which are generated by hydrolysis of a carboxylate ester group. Since the polymerized monomer is a (meth)acrylic acid ester, the polymerized residue of an ethylene group (structural unit X) has a -COONa group, a -COOH group, and an ester group. As a specific example, the production of absorbent a using butyl methacrylate as a polymerized monomer and divinylbenzene as a cross-linking monomer will be described later.

[0055] In the absorbent A, the ratio of the cross-linked polymer residue of divinylbenzene (structural unit Y) in the organic polymer forming the continuous skeleton is 0.1 to 30 mol %, preferably 0.1 to 20 mol %, based on the total structural units. In the absorbent a, in which butyl methacrylate is used as the polymerization monomer and divinylbenzene is used as the cross-linking monomer, the ratio of the cross-linked polymer residue of divinylbenzene (structural unit Y) in the organic polymer forming the continuous skeleton is about 3%, preferably 0.1 to 10 mol %, more preferably 0.3 to 8 mol %, based on the total structural units. If the ratio of the cross-linked polymer residue of divinylbenzene in the organic polymer forming the continuous skeleton is less than the above range, the strength of the absorbent A decreases, and if it exceeds the above range, the absorption amount of the liquid to be absorbed decreases.

[0056] In the absorbent A, the ratio of the structural unit Y to the total number of moles of the structural units X and Y in the organic polymer forming the continuous skeleton is preferably 0.1 to 30 mol%, particularly preferably 0.5 to 20 mol%. In the absorbent a in which butyl methacrylate is used as the polymerization monomer and divinylbenzene is used as the crosslinking monomer, the ratio of the structural unit Y to the total number of moles of the structural units X and Y in the organic polymer forming the continuous skeleton is preferably 0.1 to 10 mol%, particularly preferably 0.3 to 8 mol%. If the ratio of the structural unit Y to the total number of moles of the structural units X and Y in the organic polymer forming the continuous skeleton is less than the above range, the strength of the absorbent A decreases, and if it exceeds the above range, the absorption amount of the liquid to be absorbed decreases.

[0057] In the absorbent A, the organic polymer forming the continuous skeleton may be composed of only the structural unit X and the structural unit Y, or may have, in addition to the structural unit X and the structural unit Y, a structural unit other than the structural unit X and the structural unit Y, that is, a polymerization residue of a monomer other than (meth)acrylic acid ester and divinylbenzene. Examples of structural units other than the structural unit X and the structural unit Y include polymerization residues of monomers such as styrene, α-methylstyrene, vinyltoluene, vinylbenzyl chloride, (meth)acrylate, isobutene, butadiene, isoprene, chloroprene, vinyl chloride, vinyl bromide, vinylidene chloride, tetrafluoroethylene, (meth)acrylonitrile, vinyl acetate, ethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. In addition, in the organic polymer forming the continuous skeleton, the proportion of structural units other than the structural unit X and the structural unit Y is 0 to 50 mol%, preferably 0 to 30 mol%, based on the total structural units. In absorbent a, in which butyl methacrylate is used as a polymerization monomer and divinylbenzene is used as a crosslinking monomer, the proportion of structural units other than the structural unit X and the structural unit Y in the organic polymer forming the continuous skeleton is 0 to 50 mol %, and preferably 0 to 30 mol %, relative to all structural units.

[0058] The thickness of the continuous skeleton of absorbent A is 0.1 to 100 μm. If the thickness of the continuous skeleton of absorbent A is less than 0.1 μm, the spaces (pores) for absorbing water in the porous structure may be easily crushed during absorption, which may result in a decrease in the amount of absorption. On the other hand, if the thickness of the continuous skeleton is thicker than 100 μm, the absorption of liquid may be slowed. Since the pore structure of the continuous skeleton of absorbent A is a continuous bubble structure, the thickness of the continuous skeleton is measured by evaluating the cross section of the skeleton that appears on the test piece for electron microscope measurement. The skeleton is often polygonal because it is formed by the gaps between water (water droplets) that are removed by the dehydration and drying process after hydrolysis described later. Therefore, the thickness of the skeleton is the average diameter of the circle circumscribing the polygonal cross section. In rare cases, there may be small holes in the polygon, in which case the circumscribing circle of the polygonal cross section surrounding the small holes is measured.

[0059] The absorbent A has an average diameter of interconnected pores of 1 to 1000 μm. If the average diameter of interconnected pores of absorbent A is less than 1 μm, the porous space (pores) for absorbing water may be easily crushed during absorption, and the absorption rate may decrease. On the other hand, if the average diameter of interconnected pores is thicker than 1000 μm, the liquid absorption rate may decrease. The average diameter of interconnected pores of absorbent A can be measured by mercury intrusion porosimetry, and is the maximum value of the pore distribution curve obtained by mercury intrusion porosimetry. Regarding the sample for measuring the average diameter of interconnected pores, the sample is dried at 50° C. for 18 hours or more in a reduced pressure dryer regardless of the ion form of absorbent A. The final pressure reached is 0 Torr.

[0060] The absorbent A has a structure in which bubble-like macropores overlap each other (see Figs. 4 to 8), and the overlapping parts have an open cell structure (continuous macropore structure) in which common openings (mesopores) have an average diameter of 1 to 1000 µm, preferably 10 to 200 µm, and particularly preferably 20 to 100 µm. Most of them have an open pore structure. The number of overlapping macropores is 1 to 12 in one macropore, and in most cases 3 to 10.

[0061] FIG. 4 is an SEM photograph of absorbent a at a magnification of 50 times. FIG. 5 is an SEM photograph of absorbent a at a magnification of 100 times. FIG. 6 is an SEM photograph of absorbent a at a magnification of 500 times. FIG. 7 is an SEM photograph of absorbent a at a magnification of 1000 times. FIG. 8 is an SEM photograph of absorbent a at a magnification of 1500 times. Absorbent a is an example of absorbent A in which butyl methacrylate is used as a polymerization monomer and divinylbenzene is used as a cross-linking monomer, and absorbents a in FIGS. 4 to 8 are each a cube with a side of 2 mm.

[0062] 4 to 8 show scanning electron microscope (SEM) photographs of examples of absorbent a, which is a specific example of absorbent A. The absorbent a shown in Figs. 4 to 8 has a large number of cellular macropores, and the cellular macropores overlap each other, forming an open-cell structure where the overlapping portions form common openings (mesopores). Most of the open-pore structure is an open pore structure. If the average diameter of the mesopores in a dry state is less than the above range, the absorption rate of the liquid to be absorbed becomes too slow, and if it exceeds the above range, absorbent a (absorbent A) becomes brittle. By making absorbent A have such an open-cell structure, macropores and mesopores can be uniformly formed, and the pore volume and specific surface area can be significantly increased compared to particle agglomeration type porous bodies such as those described in JP-A-8-252579.

[0063] The total pore volume of the pores (voids) of the absorbent A is preferably 1 to 50 ml / g, and more preferably 2 to 30 ml / g. If the total pore volume of the absorbent A is less than 0.5 ml / g, the spaces (voids) for absorbing water in the porous material are likely to collapse during absorption, and the amount of absorption and the absorption rate may decrease. If it exceeds 50 ml / g, the strength of the absorbent A decreases. The total pore volume can be measured by mercury intrusion porosimetry. The sample for measuring the total pore volume is absorbent A that has been dried in a vacuum dryer at a temperature of 50°C for 18 hours or more, regardless of the ion form of the absorbent A. The final pressure reached is 0 Torr.

[0064] Hereinafter, the state when the absorbent A comes into contact with a liquid such as a body fluid (hereinafter also referred to as "body fluid") will be described, but the same applies when the absorbent 11 containing the absorbent A comes into contact with a body fluid. In addition, since the weight of absorbed body fluid is approximately proportional to the amount of body fluid, hereinafter, the weight of body fluid will also be referred to as the "amount of body fluid".

[0065] First, when body fluid comes into contact with absorbent A, it is absorbed into the pores (voids) of absorbent A by capillary action. As shown in Figs. 4 to 8, the continuous pores of absorbent A are pores in which a plurality of pores (voids) are interconnected, and it is possible to visually confirm from the outside that a large number of voids are provided. A certain amount of body fluid enters the large number of pores by capillary action, and absorbent A absorbs the body fluid. Of the certain amount of body fluid absorbed by absorbent A, a part is absorbed into the continuous skeleton by osmotic pressure, and the continuous skeleton is extended. Of the certain amount of body fluid absorbed by absorbent A, the body fluid that is not absorbed into the continuous skeleton is absorbed while remaining in the pores.

[0066] Absorbent A has a property that the continuous skeleton extends when it absorbs liquid. This extension of the continuous skeleton extends in almost all directions. As the external shape of absorbent A increases due to the extension of the continuous skeleton, the size of each pore also increases. When the size of the pore increases, the volume of the pore increases, and the amount of body fluid that can be retained in the pore increases. In other words, absorbent A that has absorbed a certain amount of body fluid and become large can absorb a further predetermined amount of body fluid by capillary action. In addition, since absorbent A absorbs body fluid by capillary action, absorbent A can quickly absorb body fluid. Note that, with respect to the body fluid absorbed by absorbent A, the amount of body fluid retained in the pores is greater than the body fluid absorbed by the continuous skeleton.

[0067] Thus, most of the body fluid absorption by absorbent A is achieved by retaining the body fluid within the pores due to capillary action, so the greater the porosity (the volume of the pores relative to the volume of absorbent A), which is the ratio of the volume of the pores (total pore volume), the more body fluid can be absorbed. It is preferable that this porosity is 85% or more.

[0068] Determine the porosity of absorbent a. The specific surface area of ​​absorbent a obtained by mercury intrusion is 400 m 2 / g, and the pore volume is 15.5ml / g. This pore volume of 15.5ml is the volume of the pores in 1g of absorbent A. If we assume that the specific gravity of absorbent A is 1g / ml, then the volumes that they occupy in 1g of absorbent A are 15.5ml of pore volume and 1ml of absorbent A. The total volume (volume) of 1g of absorbent A is 15.5+1[ml], and the ratio of the pore volume to that is the porosity. As a result, the porosity is 15.5 / (15.5+1)×100 ≒ 94%.

[0069] The absorbent A (absorbent a) has a small change in absorption amount due to the composition of the body fluid. The weight (first absorption weight) of the absorbent A per unit weight absorbing an aqueous NaCl solution with a concentration of 0.9 wt% is preferably 0.5 to 1.9 times the weight (second absorption weight) of the absorbent A absorbing an aqueous NaCl solution with a concentration of 0 to 2.0 wt%. An aqueous NaCl solution with a concentration of 0.9 wt% is a saline solution similar to so-called physiological saline, which is considered to have a composition close to that of body fluid. The absorbent 11 including the absorbent A with a first absorption weight of 0.5 to 1.9 times the second absorption weight has a less effect on the absorption amount of body fluid depending on the electrolyte ion concentration in the body fluid, so that the absorbent 11 can more reliably absorb body fluid.

[0070] The composition of body fluids, such as sweat, urine, feces, menstrual blood, vaginal discharge, breast milk, blood, and exudates, which are liquids excreted from living organisms, varies not only depending on the type of body fluid, but also on individual differences, health conditions, etc. For example, the electrolyte concentration in the urine of an organism is + , K + , Ca 2+The concentration of each ion, etc., differs between humans and animals, and also differs depending on the health condition, etc. Superabsorbent polymers (so-called SAPs), which are widely used in absorbent articles, absorb body fluids by the principle of osmotic pressure, and therefore there is a risk that the weight of body fluids that can be absorbed will decrease as the number of electrolyte ions increases (as the electrolyte concentration increases). On the other hand, absorbent A (absorbent a) absorbs more body fluids by taking them into pores due to capillary action than by the principle of osmotic pressure, so that the amount of absorption is less likely to decrease due to the composition of the body fluid, particularly the electrolyte concentration.

[0071] Fig. 9 shows the measurement results of absorbent a. In Fig. 9, "absorption weight" and "absorption rate" are synonymous with "absorption weight" and "absorption rate". As shown in Fig. 9, measurements were carried out multiple times for absorbent a with particle sizes of 500 to 850 µm and absorbent a with particle sizes of 250 µm or less. In addition, as a comparative example, the results of SAP (AQUAKEEP SA60S, manufactured by Sumitomo Seika Chemicals Co., Ltd.), which is a highly absorbent polymer, are also shown.

[0072] The absorption weight of the NaCl aqueous solution of each concentration can be measured by the following method. First, prepare containers containing 1000 ml of NaCl solution of each concentration. Next, two pieces of nylon net (255 mesh nylon net, N-No. 255HD, manufactured by NBC Meshtec Co., Ltd.) cut to 200 mm x 200 mm were stacked together, and 1.0 g of absorbent A was sandwiched between the nylon nets. The four sides were then heat-sealed to create a bag containing the sample. Next, the bag containing the sample is immersed so that it touches the bottom of a container containing NaCl aqueous solution of various concentrations, and left for one hour with one side of the top of the bag fixed to the edge of the container with a clothespin. Thereafter, the bag is removed from the NaCl aqueous solution and the water is drained for 15 minutes while the bag is clamped with clothespins at 5 mm from the top and 50 mm from both ends. Finally, the weight of the bag containing absorbent A is measured, and the weight of the bag alone and 1.0 g (the weight of absorbent A before absorbing the NaCl aqueous solution) are subtracted from the measurement result to obtain the weight of the NaCl aqueous solution absorbed by absorbent A.

[0073] 9, the weight (first absorption weight) of the NaCl aqueous solution with a concentration of 0.9 wt% absorbed by 1.0 g of absorbent a (first polymer absorbent, hereinafter also referred to as the "first absorbent") is 37.71 to 62.09 g, and the weight (second absorption weight) of the NaCl aqueous solution with a concentration of 0 to 2.0 wt% absorbed by 1.0 g of absorbent a (second polymer absorbent, hereinafter also referred to as the "second absorbent") is 34.40 to 68.61 g. From this measurement result, the lower limit of the ratio of the first absorption weight to the second absorption weight is (minimum value of the first absorption weight / maximum value of the second absorption weight), and the upper limit is (maximum value of the first absorption weight / minimum value of the second absorption weight). Therefore, the ratio of the first absorption weight to the second absorption weight is (37.71 / 68.61) to (62.09 / 34.40) ≒ 0.55 to 1.80, and the first absorption weight is 0.55 to 1.80 times the second absorption weight. Note that the calculation of the numerical values ​​is performed with two significant digits after the decimal point.

[0074] Similarly, for SAP, the weight of a 0.9 wt% NaCl aqueous solution absorbed by 1.0 g of SAP (first SAP) (first SAP absorption weight) is 60.08-63.69 g, and the weight of a 0-2.0 wt% NaCl aqueous solution absorbed by 1.0 g of SAP (second SAP) (second SAP absorption weight) is 45.74-311.12 g. The ratio of the first SAP absorption weight to the second SAP absorption weight is (minimum first SAP absorption amount / maximum second SAP absorption weight)-(maximum first SAP absorption weight / minimum second SAP absorption weight)=(60.08 / 311.12)-(63.69 / 45.74)≒0.19-1.39. The higher the concentration of the NaCl aqueous solution, the lower the amount of NaCl aqueous solution absorbed by SAP.

[0075] These results show that absorbent A (absorbent a) is capable of absorbing the same amount of body fluid as SAP or more than SAP, while there is little change in the amount of NaCl aqueous solution absorbed by absorbent A depending on the concentration. Therefore, the absorbent 11 using absorbent A can ensure the same amount of body fluid as SAP, while reducing the risk of the absorption power decreasing depending on the concentration of electrolyte ions as in SAP.

[0076] In addition, the amount of aqueous solution held within absorbent A (water retention capacity) is not easily affected by the electrolyte ion concentration. Because the change in the water retention capacity of an aqueous solution due to the electrolyte ion concentration is small, it is possible to reduce the risk that the amount of body fluid retained within absorbent A will change depending on the composition of the body fluid.

[0077] Using the same method as in the above-mentioned measurement of the weight of the NaCl aqueous solution, a first absorbent (first polymer absorbent) that has absorbed a first absorption amount of a 0.9 wt% NaCl aqueous solution and a second absorbent (second polymer absorbent) that has absorbed a second absorption amount of a 0-2.0 wt% NaCl aqueous solution are prepared. The first absorbent and the second absorbent are each dehydrated for a predetermined time using a centrifuge under conditions of 150 G and 850 rpm for 90 seconds. Then, when the weights of the NaCl aqueous solutions absorbed in the first absorbent and the second absorbent are measured, it is preferable that the weight of the 0.9 wt% NaCl aqueous solution absorbed by the first absorbent (first water retention weight) is 0.5 to 1.6 times the weight of the 0-2.0 wt% NaCl aqueous solution absorbed by the second absorbent (second water retention weight). Absorbent A, in which the first water retention weight is 0.5 to 1.6 times the second water retention weight, moves the body fluid once absorbed to the outside of absorbent A, making it easier for the body fluid to be absorbed by other substances.

[0078] 9, the weight of the NaCl aqueous solution with a concentration of 0.9 wt% when 1.0 g of absorbent a is retained (first retained weight) is 13.59 to 17.12 g, and the weight of the NaCl aqueous solution with a concentration of 0 to 2.0 wt% when 1.0 g of absorbent a is retained (second retained weight) is 11.46 to 19.47 g. This result shows that the difference in weight of the NaCl aqueous solution retained by absorbent a due to the difference in the concentration of the NaCl aqueous solution is small.

[0079] For absorbent a, the lower limit of the ratio of the first water retention weight to the second water retention weight is (minimum first water retention weight / maximum second water retention weight), and the upper limit is (maximum first water retention weight / minimum second water retention weight). Therefore, the ratio of the first water retention weight to the second water retention weight is (13.59 / 19.47) to (17.12 / 11.46) ≒ 0.70 to 1.49 times. The calculation of the numerical value is performed with two significant digits after the decimal point.

[0080] It is also found that the water retention weight of the NaCl aqueous solution at each concentration is generally less for absorbent a than for SAP. Regarding SAP, the weight of a NaCl aqueous solution with a concentration of 0.9 wt% in a state where 1.0 g of SAP (first SAP) is retained (first SAP water retention weight) is 39.98 to 40.41 g, and the weight of a NaCl aqueous solution with a concentration of 0 to 2.0 wt% in a state where 1.0 g of SAP (second SAP) is retained (second SAP water retention weight) is 29.31 to 286.11 g. Therefore, the lower limit of the ratio of the first SAP water retention capacity to the second SAP water retention capacity is (minimum value of first SAP water retention capacity / maximum value of second SAP water retention capacity), and the upper limit is (maximum value of first SAP water retention capacity / minimum value of second SAP water retention capacity). Therefore, the ratio of the first SAP water retention capacity to the second SAP water retention capacity is (39.98 / 286.11) to (40.41 / 29.31) ≒ 0.14 to 1.38 times.

[0081] The difference between the absorption weight and the water retention weight is the weight of the liquid that the absorbent A or SAP absorbed and released to the outside (water release) (hereinafter, also referred to as "water release weight"). The value obtained by dividing the water release weight by the absorption weight is the ratio of the water release weight to the amount of liquid that was once absorbed, and is also referred to as water release ratio. For the first absorbent, the absorbent A preferably has a value obtained by dividing the difference between the first absorption weight and the first water retention weight by the first absorption weight of 50 to 80%. Similarly, for the second absorbent, the value obtained by dividing the difference between the second absorption weight and the second water retention weight by the second absorption weight of 40 to 85%. The absorbent A having the water release rate of the above value easily transfers the body fluid that was once absorbed to other substances. In other words, it is easy to repeat absorption and water release. By transferring the body fluid that was once absorbed to the outside of the absorbent A, the absorbent 11 including the absorbent A easily reduces the wet feeling given to the wearer.

[0082] For the absorbent a, the lower limit of the first syneresis rate, which is the value obtained by dividing the syneresis weight of a NaCl aqueous solution having a concentration of 0.9 wt% by the first absorption weight, is {(minimum value of the first absorption weight-maximum value of the first water retention weight) / minimum value of the first absorption weight} x 100, and the upper limit of the first syneresis rate is {(maximum value of the first absorption weight-minimum value of the first water retention weight) / maximum value of the first absorption weight} x 100. The lower limit of the second syneresis rate, which is the value obtained by dividing the syneresis weight of a NaCl aqueous solution having a concentration of 0 to 2.0 wt% by the second absorption weight, is {(minimum value of the second absorption weight-maximum value of the second water retention weight) / minimum value of the second absorption weight} x 100, and the upper limit of the second syneresis rate is {(minimum value of the second absorption weight-maximum value of the second water retention weight) / minimum value of the second absorption weight} x 100. As shown in Fig. 9, the first syneresis rate of absorbent a is {(37.71-17.12) / 37.71} x 100 to {(62.09-13.59) / 62.09} x 100 ≒ 54.60 to 78.11. The second syneresis rate of absorbent a is {(34.40-19.47) / 34.40} x 100 to {(68.61-11.46) / 68.61} x 100 ≒ 43.40 to 83.30. The values ​​are calculated with two decimal places as significant figures.

[0083] As shown in Figure 9, when comparing the water retention weights of absorbent a and SAP, it is difficult to make a simple comparison because the values ​​of the absorption weights are different, but the water retention weight of absorbent a is generally less than that of SAP. In other words, absorbent a has a lower water retention weight than SAP.

[0084] Furthermore, it is preferable that the time required for 2.0 g of absorbent A to absorb 50 g of a 0.9 wt % NaCl aqueous solution by the vortex method is 1.0 to 10.0 seconds. Since absorbent A capable of absorbing the NaCl aqueous solution within this time period can absorb liquid in a short period of time, absorbent 11 provided with absorbent A can quickly absorb body fluids.

[0085] The absorption time is measured by the vortex method as follows. A rotor measuring 30 x 8 mm is placed in the container, and 50 g of a 0.9 wt % NaCl aqueous solution whose temperature has been adjusted to 25°C ± 1°C is added. The NaCl solution was stirred using a magnetic stirrer (MITAMURA RIKEN KOGYO INC. MAGMIX STIRRER (AC100W)) with the rotor adjusted to a speed of 600 ± 30 rpm. Add 2.00 g of absorbent A to the container under stirring, and start measuring the time as soon as the addition is completed. The time when the liquid surface becomes flat is measured, which is the point at which the inclination of the rapidly rotating vortex of the liquid approaches a plane, and is determined by observing the disappearance of the light reflected by the liquid surface of the vortex.

[0086] 9, the time for 2.0 g of absorbent a to absorb 50 g of a 0.9 wt% NaCl aqueous solution is 1.69 to 1.93 seconds. Note that for 2.0 g of absorbent a, the time for absorbing a lower concentration 0.3 wt% NaCl aqueous solution is 1.56 to 2.01 seconds, and the time for absorbing a higher concentration 2.0 wt% NaCl aqueous solution is 1.36 to 2.29 seconds. Therefore, the time for 2.0 g of absorbent a to absorb 50 g of a 0 to 2.0 wt% NaCl aqueous solution is 1.34 to 2.29 seconds, and it is found that the change in absorption time due to the concentration of the NaCl aqueous solution is small.

[0087] As described above, since the absorbent A has a high water release rate and a fast absorption rate, it is more preferable that the absorbent 11 of an absorbent article such as the diaper 1 includes, in addition to the absorbent A, a polymeric compound having a water retention rate higher than that of the absorbent A. Examples of polymeric compounds having a water retention rate higher than that of the absorbent A include so-called SAP such as sodium polyacrylate. SAP has high water retention and low water release rate, so that it can continue to hold body fluids once absorbed. However, it has a slow absorption rate (see FIG. 9), so it takes time to absorb body fluids. In this regard, by including the absorbent A and SAP in the absorbent 11, when body fluids come into contact with the absorbent 11, the absorbent A, which has a fast absorption rate, absorbs the body fluid first. Then, the absorbent A, which has a high water release rate, releases the body fluid into the absorbent 11. The released body fluid is absorbed by the SAP over a period of time, so that the body fluid is retained in the SAP. As a result, the absorbent 11 transfers the body fluid once absorbed by the absorbent A to the SAP, reducing the amount of body fluid retained in the absorbent A, thereby reducing the risk of body fluid remaining on the surface of the absorbent 11 and reducing the wet feeling felt by the wearer. In addition, the absorbent 11 can easily retain excrement in the SAP inside, thereby reducing the risk of excrement leaking from an absorbent article such as the diaper 1.

[0088] In addition, it is preferable that the amount of the 0.9 wt% NaCl aqueous solution absorbed by the absorbent A is 15 ml or more after one minute has elapsed while the lower end of 1.0 g of the absorbent A is in contact with the water surface of the 0.9 wt% NaCl aqueous solution. The state in which the lower end of the absorbent A is in contact with the water surface of the NaCl aqueous solution means that the absorbent A absorbs the NaCl aqueous solution in a direction against gravity. Even in such a direction against gravity, the absorbent A can absorb 15 ml or more of the 0.9 wt% NaCl aqueous solution in one minute, making it possible to quickly absorb a larger amount of NaCl aqueous solution, and the absorber 11 including the absorbent A can absorb body fluids from various angles.

[0089] As shown in Figure 9, the amount of 0.9 wt% NaCl aqueous solution absorbed by absorbent a after 1 minute was 20.2-26.5 ml. Thus, absorbent a is able to absorb well even in the direction against gravity. For SAP, the amount of 0.9 wt% NaCl aqueous solution absorbed after 1 minute was 14.0-18.0 ml. From this result, it can be seen that absorbent A is able to absorb body fluids more quickly than SAP, even in the direction against gravity.

[0090] Furthermore, it is more preferable that, when the lower end of 2.0 g of absorbent A under a load of 600 gw is brought into contact with the water surface of a 0.9 wt% NaCl aqueous solution, the absorbent A absorbs 1.0 ml or more of a 0.9 wt% NaCl aqueous solution after 2 minutes, and absorbs 5.0 ml or more of a 0.9 wt% NaCl aqueous solution after 15 minutes. When absorbent A is used in absorbent 11, absorbent 11, which has once absorbed excrement, may be crushed in the thickness direction by the weight of the wearer or crushed in the left-right direction by both legs of the wearer. In this regard, absorbent A can absorb NaCl aqueous solution even under a load of a certain amount, and can also absorb NaCl aqueous solution in a direction against gravity. Therefore, by providing absorbent A, absorbent 11 can absorb body fluids from various angles even when a load is applied to absorbent 11 (absorbent A).

[0091] As shown in Fig. 9, for absorbent A, the amount of 0.9 wt% NaCl aqueous solution absorbed by 2.0 g of absorbent A after 2 minutes is 2.6-5.6 ml, and the amount of 0.9 wt% NaCl aqueous solution absorbed by absorbent A after 15 minutes is 13.2-25.2 ml. For SAP, the amount of 0.9 wt% NaCl aqueous solution absorbed by 2.0 g of SAP after 2 minutes is 0.8-1.0 ml, and the amount of 0.9 wt% NaCl aqueous solution absorbed by absorbent A after 15 minutes is 4.0 ml. From these results, it can be seen that absorbent A has better absorbency than SAP even under pressure and against gravity.

[0092] In addition, it is preferable that the absorption weight of absorbent A per unit weight when absorbing a CaCl2 aqueous solution with a concentration of 0.5 wt% is 13 times or more the weight of absorbent A. Even in an aqueous solution of Ca2+, which has a larger number of electrolyte ions than Na+, it is possible to absorb 13 times or more the weight of absorbent A. Therefore, the absorber 11 including absorbent A can easily absorb body fluids regardless of the composition of the body fluid.

[0093] Figure 9 shows the weight of 1g of absorbent a absorbing a 0.5wt% CaCl2 aqueous solution. The absorption weight of the CaCl2 aqueous solution is measured in the same manner as the weight of the NaCl aqueous solution. As shown in Figure 9, the measurement result of the absorption weight of absorbent a absorbing a 0.5wt% CaCl2 aqueous solution is 16.29-27.69g, and 1g of absorbent a absorbs 0.5wt% CaCl2 aqueous solution in an amount 16.29 times or more the weight of absorbent a.

[0094] As shown in FIG. 9, the absorption weight of 1 g of SAP for a CaCl2 aqueous solution with a concentration of 0.5 wt% is 6.71 to 7.43 g. Comparing the weight of 1 g of absorbent a absorbing a CaCl2 aqueous solution with a concentration of 0.5 wt% and the weight of 1 g of SAP absorbing a CaCl2 aqueous solution with a concentration of 0.5 wt%, the weight absorbed by absorbent a is obviously larger. Also, the weight of 1 g of SAP absorbing a CaCl2 aqueous solution with a concentration of 0.5 wt% is less than the weight of 1 g of SAP absorbing a NaCl aqueous solution with a concentration of 0.9 wt%. In other words, while the amount of absorption of SAP decreases as the number of electrolyte ions increases, absorbent a does not decrease the amount of absorption due to the number of electrolyte ions as in SAP. Therefore, by using absorbent a (absorbent A), it is possible to reduce the risk of the amount of absorption decreasing due to the composition of the body fluid.

[0095] The following absorption rate test and absorption amount test were carried out on absorbent A. Fig. 10 is a graph showing the absorption rate and absorption amount test results of absorbent A. Fig. 11 is a graph showing the absorption rate and absorption amount test results of a comparative example of a high absorbent polymer.

[0096] As shown in Figure 10, the absorption rate test was conducted using pure water and 0.9% sodium chloride solution as the absorption target liquid, and the immersion time to reach 90% of the saturated absorption amount was within 5 seconds for both solutions. Furthermore, the absorption amount test of absorbent A was conducted using 0.9% sodium chloride solution, 4% NaOH solution, 35% hydrochloric acid, and 29% ammonia water as the test water. As a result, the absorption amount of 0.9% sodium chloride solution was 67g / g-resin, the absorption amount of 4% NaOH solution was 78g / g-resin, the absorption amount of 35% hydrochloric acid was 28g / g-resin, and the absorption amount of 29% ammonia water was 105g / g-resin.

[0097] (Absorption rate test method) A sample tube is made by filling one end of a 100 mm long tube with a 10 mm inner diameter and sealing it with nonwoven fabric, and putting dry absorbent A into it. The weight of the tube is measured before and after putting in absorbent A, and the weight of absorbent A inside the tube is calculated in advance. Next, the nonwoven fabric side of the sample tube is immersed in a liquid to be absorbed of known concentration, and after a predetermined time has elapsed, the tube is pulled out of the solution. The tube is then held in this state for one minute, after which the weight of the tube is measured. This immersion and measurement is repeated until there is no more change in weight. The amount of absorption at which there is no more change in weight is considered to be the saturated absorption amount.

[0098] (Absorption test method) The test is conducted in accordance with the JIS method. A tea bag containing absorbent A is used as a sample, and the amount of absorbed liquid is calculated from the weight before and after immersion of the sample in the liquid to be absorbed for 24 hours.

[0099] (Comparative Example) An absorption rate test and an absorption amount test were performed using a superabsorbent polymer (product name: high absorbent polymer (acrylate salt type) manufactured by Wako Pure Chemical Industries, Ltd. As shown in FIG. 11, the results of the absorption amount test showed that in the absorption rate test, the immersion time required to reach 90% of the saturated absorption amount in pure water was 12 minutes, and the immersion time required to reach 90% of the saturated absorption amount in 0.9% sodium chloride aqueous solution was 3.5 minutes. The absorption amount of the 0.9% sodium chloride aqueous solution was 52g / g-resin, the absorption amount of the 4% NaOH aqueous solution was not measurable because it dissolved during immersion, the absorption amount of the 35% hydrochloric acid was 2g / g-resin, and the absorption amount of the 29% ammonia water was 128g / g-resin.

[0100] The absorbent A can also be used as a monolith ion exchanger, and is also referred to as a "monolithic organic porous ion exchanger". The total ion exchange capacity of -COONa group and -COOH group per unit weight of the absorbent A is 5 mg equivalent / g or more, preferably 6 mg equivalent / g or more. If the total ion exchange capacity of -COOH group and -COONa group in the dry state of the monolith ion exchanger is less than the above range, the amount of absorption of the absorption target liquid decreases and the absorption rate also slows down. In addition, the upper limit of the total ion exchange capacity of -COOH group and -COONa group in the dry state of the monolith ion exchanger is not particularly limited, but may be, for example, 14.0 mg equivalent / g or less or 13.0 mg equivalent / g or less. The total ion exchange capacity of -COONa group and -COOH group per unit weight of the absorbent a, which uses butyl methacrylate as a polymerization monomer and divinylbenzene as a crosslinking monomer, is 4.0 mg equivalent / g or more, preferably 6 mg equivalent / g or more. In addition, the upper limit of the total ion exchange capacity of -COOH group and -COONa group in the dry state of the monolith ion exchanger of absorbent a is not particularly limited, but may be, for example, 11 mg equivalent / g or less, or 14 mg equivalent / g or less. The total ion exchange capacity of -COONa group per unit weight of absorbent A is desirably 4.0 mg equivalent / g or more. By making the total ion exchange capacity of -COONa group per unit weight 4.0 mg equivalent / g or more of absorbent A, the polymer absorbent is more likely to absorb body fluid than when the total ion exchange capacity of -COONa group per unit weight is less than 4.0 mg equivalent / g, so that the continuous skeleton is more easily extended, and the continuous pores are more likely to expand with the extension of the continuous skeleton, and the body fluid is more easily taken in by the continuous pores due to the capillary phenomenon, which makes it easier for the absorbent to absorb body fluid.

[0101] In the present invention, the total ion exchange capacity of -COOH groups and -COONa groups refers to the ion exchange capacity of -COOH groups when the monolith ion exchanger of the present invention has only -COOH groups among -COOH groups and -COONa groups, and refers to the ion exchange capacity of -COONa groups when the monolith ion exchanger of the present invention has only -COOH groups among -COOH groups and -COONa groups, and refers to the total ion exchange capacity of -COOH groups and -COONa groups when the monolith ion exchanger of the present invention has both -COOH groups and -COONa groups among -COOH groups and -COONa groups. The total ion exchange capacity of -COOH groups and -COONa groups per weight of the monolith ion exchanger in a dry state is measured by quantifying the amount of -COOH groups by neutralization titration using a sample in which all the ion exchange groups of the monolith ion exchanger are converted to -COOH groups using a sufficient amount of acid, recovering the entire amount of the monolith ion exchanger used at this time, and determining the value of the dry weight. The total ion exchange capacity of -COONa groups per unit weight can be determined from the amount of acid added to convert all the ion exchange groups of the monolith ion exchanger into -COOH groups.

[0102] In monolith ion exchangers, the introduced ion exchange groups are distributed uniformly not only on the surface of the monolith but also inside the monolith skeleton. Here, "the ion exchange groups are distributed uniformly" means that the ion exchange groups are distributed uniformly on the surface and inside the skeleton at least on the order of μm. The distribution of the ion exchange groups can be easily confirmed by using EPMA.

[0103] Examples of the structure of monolith ion exchangers include an open-cell structure (JP 2002-306976 A, JP 2009-62512 A), a co-continuous structure (JP 2009-67982 A), a particle aggregate structure (JP 2009-7550 A), and a particle composite structure (JP 2009-108294 A).

[0104] The ion exchange capacity of absorbent A as a monolithic cation exchanger was 8 mg equivalent / g in a dry state, and it was confirmed that carboxyl groups were quantitatively introduced. In addition, the average diameter of the three-dimensionally continuous pores of absorbent A in a dry state, as determined by mercury intrusion porosimetry, was 49.1 μm, and the total pore volume in a dry state was 13.5 mL / g. The thickness of the continuous framework obtained by SEM observation was 9.5 μm.

[0105] Figures 12A and 12B show the distribution of sodium by EPMA to confirm the distribution of carboxyl groups in monolith A. Figure 12A is an SEM photograph of the fracture surface of absorbent A. Figure 12B is a mapping diagram of Na distribution in the same part as Figure 12A. Figures 12A and 12B show that the distribution of carboxyl groups in the skeleton cross section is uniform not only on the skeleton surface of the monolith cation exchanger but also inside the skeleton, and it can be confirmed that the carboxyl groups are uniformly introduced into the monolith ion exchanger.

[0106] Further, examples of the structure of the absorbent A include the open cell structure disclosed in JP-A-2002-306976 and JP-A-2009-62512, the bicontinuous structure disclosed in JP-A-2009-67982, the particle aggregation type structure disclosed in JP-A-2009-7550, and the monolith ion structure disclosed as a particle composite type structure disclosed in JP-A-2009-108294.

[0107] ===About the manufacturing method of absorbent A=== The absorbent A can be obtained through a cross-linking polymerization step and a hydrolysis step, as shown in Fig. 3. The method for producing the absorbent A will be described below.

[0108] First, an oil-soluble monomer for crosslinking polymerization, a crosslinkable monomer, a surfactant, water, and optionally a polymerization initiator are mixed to obtain a water-in-oil emulsion, which is an emulsion in which the oil phase is the continuous phase and water droplets are dispersed therein.

[0109] As shown in the upper diagram of Figure 3, absorbent A is formed by cross-linking polymerization of monolith A using butyl methacrylate as the (meth)acrylic acid ester as the oil-soluble monomer, divinylbenzene as the cross-linking monomer, sorbitan monooleate as the surfactant, and isobutyronitrile as the polymerization initiator.

[0110] For absorbent A, as shown in the upper diagram of Figure 3, first, 9.2 g of t-butyl methacrylate as an oil-soluble monomer, 0.28 g of divinylbenzene as a cross-linking monomer, 1.0 g of sorbitan monooleate (hereinafter abbreviated as SMO) as a surfactant, and 0.4 g of 2,2'-azobis(isobutyronitrile) as a polymerization initiator are mixed and dissolved uniformly.

[0111] Next, the t-butyl methacrylate / divinylbenzene / SMO / 2,2'-azobis(isobutyronitrile) mixture is added to 180 g of pure water and stirred under reduced pressure using a planetary stirring device, a vacuum stirring and degassing mixer (manufactured by EME), to obtain a water-in-oil emulsion.

[0112] The emulsion is then quickly transferred to a reaction vessel, sealed, and polymerized at 60°C for 24 hours under static conditions. After polymerization is complete, the contents are removed, extracted with methanol, and dried under reduced pressure to obtain monolith A having a continuous macropore structure. The internal structure of monolith A was observed by SEM. Figure 10A is an SEM photograph of the fracture surface of absorbent A. Figure 10B is a mapping diagram of Na distribution in the same part as Figure 10A. Monolith A has a continuous cell structure, and the thickness of the continuous skeleton was 5.4 μm. The average diameter measured by mercury intrusion porosimetry was 36.2 μm, and the total pore volume was 15.5 mL / g.

[0113] The content of divinylbenzene in the total monomers is preferably 0.3 to 10 mol%, more preferably 0.3 to 5 mol%. The ratio of divinylbenzene to the total of butyl methacrylate and divinylbenzene is preferably 0.1 to 10 mol%, more preferably 0.3 to 8 mol%. In absorbent A, the ratio of butyl methacrylate to the total of butyl methacrylate and divinylbenzene is 97.0 mol%, and the ratio of divinylbenzene is 3.0 mol%.

[0114] The amount of surfactant added varies greatly depending on the type of oil-soluble monomer and the size of the desired emulsion particles (macropores), but is preferably in the range of about 2 to 70% of the total amount of the oil-soluble monomer and surfactant.

[0115] In addition, in order to control the bubble shape and size of Monolith A, alcohols such as methanol and stearyl alcohol, carboxylic acids such as stearic acid, hydrocarbons such as octane, dodecane, and toluene, and cyclic ethers such as tetrahydrofuran and dioxane may be coexisted in the system.

[0116] There is no particular restriction on the mixing method when forming a water-in-oil emulsion. A mixing method such as a method of mixing each component at once all at once, a method of dissolving oil-soluble components such as an oil-soluble monomer, a surfactant, and an oil-soluble polymerization initiator, and a water-soluble component such as water or a water-soluble polymerization initiator separately and then mixing each component can be adopted. There is no particular restriction on the mixing device for forming the emulsion, and in order to obtain the desired emulsion particle size, an appropriate device can be selected from a normal mixer, a homogenizer, a high-pressure homogenizer, and a so-called planetary mixing device in which the material to be processed is placed in a mixing container and rotated around the revolution axis while being tilted, thereby stirring and mixing the material to be processed. There is also no particular restriction on the mixing conditions, and the stirring rotation speed and stirring time can be set arbitrarily to obtain the desired emulsion particle size. Among these mixing devices, a planetary mixing device can uniformly generate water droplets in a W / O emulsion, and the average diameter can be arbitrarily set within a wide range.

[0117] The polymerization conditions for polymerizing the water-in-oil emulsion can be selected from various conditions depending on the type of monomer and the initiator system. For example, when azobisisobutyronitrile, benzoyl peroxide, potassium persulfate, etc. are used as the polymerization initiator, the polymerization can be carried out by heating in a sealed container under an inert atmosphere at 30 to 100°C for 1 to 48 hours. When hydrogen peroxide-ferrous chloride, sodium persulfate-acidic sodium sulfite, etc. are used as the polymerization initiator, the polymerization can be carried out in a sealed container under an inert atmosphere at 0 to 30°C for 1 to 48 hours. After the polymerization is completed, the contents are taken out and subjected to Soxhlet extraction with a solvent such as isopropanol to remove unreacted monomers and residual surfactants, thereby obtaining monolith A shown in the middle diagram of Figure 3.

[0118] Next, the monolith A (crosslinked polymer) is hydrolyzed to obtain absorbent A. The monolith A is immersed in dichloroethane containing zinc bromide and stirred at 40°C for 24 hours, and then contacted with methanol, 4% hydrochloric acid, 4% aqueous sodium hydroxide solution, and water in that order to hydrolyze the monolith A. After drying, the block-shaped absorbent A is crushed to a specified size to obtain particulate absorbent A.

[0119] There is no particular limitation on the method of hydrolysis of monolith A, and it can be carried out by various methods. For example, aromatic solvents such as toluene and xylene, halogen-based solvents such as chloroform and dichloroethane, ether-based solvents such as tetrahydrofuran and isopropyl ether, amide-based solvents such as dimethylformamide and dimethylacetamide, alcohol-based solvents such as methanol and ethanol, carboxylic acid-based solvents such as acetic acid and propionic acid, or water can be used as a solvent, and the solvent can be contacted with a strong base such as sodium hydroxide, a hydrohalic acid such as hydrochloric acid, a Bronsted acid such as sulfuric acid, nitric acid, trifluoroacetic acid, methanesulfonic acid, and p-toluenesulfonic acid, or a Lewis acid such as zinc bromide, aluminum chloride, aluminum bromide, titanium (IV) chloride, cerium chloride / sodium iodide, and magnesium iodide.

[0120] Among the polymerization raw materials of the organic polymer forming the continuous skeleton of the absorbent A, the (meth)acrylic acid ester is not particularly limited, but is preferably a C1-C10 alkyl ester of (meth)acrylic acid, and more preferably a C4 alkyl ester of (meth)acrylic acid. Examples of the C4 alkyl ester of (meth)acrylic acid include t-butyl (meth)acrylic acid ester, n-butyl (meth)acrylic acid ester, and iso-butyl (meth)acrylic acid ester.

[0121] The monomers used in the crosslinking polymerization may be only (meth)acrylic acid esters and divinylbenzene, or may contain other monomers other than (meth)acrylic acid esters and divinylbenzene in addition to (meth)acrylic acid esters and divinylbenzene. Examples of other monomers include styrene, α-methylstyrene, vinyltoluene, vinylbenzyl chloride, (meth)acrylate glycidyl, (meth)acrylate 2-ethylhexyl, isobutene, butadiene, isoprene, chloroprene, vinyl chloride, vinyl bromide, vinylidene chloride, tetrafluoroethylene, (meth)acrylonitrile, vinyl acetate, ethylene glycol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. In the total monomers used in the crosslinking polymerization, the proportion of monomers other than (meth)acrylic acid esters and divinylbenzene is preferably 0 to 80 mol%, more preferably 0 to 50 mol%.

[0122] The surfactant is not limited to sorbitan monooleate. Any surfactant may be used as long as it can form a water-in-oil type (W / O) emulsion when the crosslinking polymerization monomer is mixed with water. For example, nonionic surfactants such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan trioleate, polyoxyethylene nonylphenyl ether, polyoxyethylene stearyl ether, and polyoxyethylene sorbitan monooleate, anionic surfactants such as potassium oleate, sodium dodecylbenzenesulfonate, and dioctyl sodium sulfosuccinate, cationic surfactants such as distearyl dimethyl ammonium chloride, and amphoteric surfactants such as lauryl dimethyl betaine can be used. These surfactants may be used alone or in combination of two or more.

[0123] As the polymerization initiator, a compound that generates radicals by heat and light irradiation is preferably used. The polymerization initiator may be water-soluble or oil-soluble, and examples thereof include azobis(4-methoxy-2,4-dimethylvaleronitrile), azobisisobutyronitrile, azobisdimethylvaleronitrile, azobiscyclohexanenitrile, azobiscyclohexanecarbonitrile, azobis(2-methylpropionamidine)dihydrochloride, benzoyl peroxide, potassium persulfate, ammonium persulfate, hydrogen peroxide-ferrous chloride, sodium persulfate-acidic sodium sulfite, and tetramethylthiuram disulfide. However, in some cases, there are systems in which polymerization proceeds only by heating or light irradiation without the addition of a polymerization initiator, and in such systems, the addition of a polymerization initiator is not necessary.

[0124] As another example of absorbent A, absorbent b can be used in which 6.4 g of t-butyl methacrylate and 2.8 g of 2-ethylhexyl methacrylate are used instead of 9.2 g of t-butyl methacrylate in absorbent a. It is the same as absorbent a except that the oil-soluble monomers are 6.4 g of t-butyl methacrylate and 2.8 g of 2-ethylhexyl methacrylate. The ion exchange capacity of absorbent b in a dry state is 5.0 mg equivalent / g.

[0125] For absorbent b, an absorption speed test was conducted in the same manner as for absorbent a, using pure water as the absorption target liquid. Figure 13 is a graph showing the relationship between the absorption amount and time for absorbent a and absorbent b when the absorption target liquid is pure water. As shown in Figure 13, the saturated absorption amount was 18g / g-resin, and the immersion time to reach 90% of the saturated absorption amount was within 5 seconds.

[0126] ===Other embodiments=== The above-described embodiment is for the purpose of facilitating understanding of the present invention, and is not intended to limit the present invention. The present invention may be modified or improved without departing from the spirit thereof, and it goes without saying that the present invention includes equivalents thereof.

[0127] In the above-described embodiment, the absorbent 11 includes the absorbent A (absorbent a) and SAP, but this is not limited to the above. The absorbent 11 may be composed of only the absorbent A. Furthermore, the material used together with the absorbent A is not limited to SAP. For example, the absorbent 11 may include the absorbent A and pulp fibers, or the absorbent 11 may include the absorbent A, SAP, and pulp fibers. [Explanation of symbols]

[0128] 1 diaper (pants-type disposable diaper, absorbent article), 10 absorbent body, 10ea end, 10eb end, 11 absorbent body, 11c absorbent core, 13 top sheet, 15 back sheet, 30 abdominal member, 30a side, 31 skin-side sheet, 32 non-skin-side sheet, 35 rubber thread, 40 dorsal member, 40a side, 41 skin-side sheet, 42 non-skin-side sheet, 45 rubber thread, SS welded portion, LH leg opening, BH waist opening

Claims

1. An absorbent for absorbing body fluids, comprising: A polymeric absorbent having a continuous skeleton and continuous pores, The polymer absorbent is a hydrolyzate of a crosslinked polymer of a (meth)acrylic acid ester and a compound containing two or more vinyl groups in one molecule, and is characterized in that it contains at least one -COONa group.

2. The absorbent body according to claim 1, The absorbent body is characterized in that the polymer absorbent is a monolithic absorbent.

3. The absorbent body according to claim 1 or 2, A first absorption weight of the polymer absorbent per unit weight at which an NaCl aqueous solution having a concentration of 0.9 wt % is absorbed; Regarding a second absorption weight at which the polymer absorbent per unit weight absorbs an NaCl aqueous solution having a concentration of 0 to 2.0 wt %, An absorbent body, characterized in that the first absorption weight is 0.5 to 1.9 times the second absorption weight.

4. The absorbent body according to claim 3, Regarding a first polymer absorbent that absorbs a 0.9 wt % NaCl aqueous solution by the first absorption weight, and a second polymer absorbent that absorbs a 0 to 2.0 wt % NaCl aqueous solution by the second absorption weight, The absorbent is characterized in that after dehydration for 90 seconds using a centrifuge under conditions of 150 G and 850 rpm for each predetermined time, the weight of the NaCl aqueous solution with a concentration of 0.9 wt % absorbed by the first polymer absorbent is 0.5 to 1.6 times the weight of the NaCl aqueous solution with a concentration of 0 to 2.0 wt % absorbed by the second polymer absorbent.

5. The absorbent body according to claim 4, The weight of the NaCl aqueous solution having a concentration of 0.9 wt % absorbed in the first polymer absorbent after the dehydration is defined as a first water retention weight, The weight of the NaCl aqueous solution having a concentration of 0 to 2.0 wt % absorbed by the second polymer absorbent after the dehydration is defined as a second water retention weight; a value obtained by dividing the difference between the first absorption weight and the first water retention weight of the first polymer absorbent by the first absorption weight is 50 to 80%; An absorbent body, characterized in that the difference between the second absorption weight and the second water retention weight of the second polymer absorbent is divided by the second absorption weight, and the difference is 40 to 85%.

6. The absorbent body according to any one of claims 1 to 5, An absorbent, characterized in that the time required for 2.0 g of said polymer absorbent to absorb 50 g of an aqueous NaCl solution having a concentration of 0.9 wt % by a vortex method is 1.0 to 10.0 seconds.

7. 7. The absorbent body according to claim 1 , The polymer absorbent is CaCl having a concentration of 0.5 wt %. 2 The absorbent body has an absorption weight for absorbing an aqueous solution that is 13 times or more the weight of the polymer absorbent.

8. The absorbent body according to any one of claims 1 to 7, The absorbent body is characterized in that, after one minute has elapsed while the lower end of 1.0 g of the polymer absorbent is kept in contact with the water surface of a 0.9 wt % NaCl aqueous solution, the amount of the 0.9 wt % NaCl aqueous solution absorbed by the polymer absorbent is 15 ml or more.

9. 9. The absorbent body according to claim 1 , The lower end of 2.0 g of the polymer absorbent under a load of 600 gw was placed in contact with the water surface of a 0.9 wt % NaCl aqueous solution. After 2 minutes, the amount of the NaCl aqueous solution having a concentration of 0.9 wt % absorbed by the polymer absorbent is 1.0 ml or more; 1. An absorbent body, characterized in that after 15 minutes, the amount of NaCl aqueous solution having a concentration of 0.9 wt % absorbed by said polymer absorbent is 5.0 ml or more.

10. 10. The absorbent body according to claim 1 , An absorbent body, characterized in that the volume of voids of said pores per unit volume of said polymer absorbent is 85% or more.

11. The absorbent body according to any one of claims 1 to 10, The absorbent body is characterized in that the polymer absorbent contains 0.1 to 30.0% of crosslinked polymer residues.

12. 12. The absorbent body according to claim 1 , An absorbent body characterized in that the average diameter of the continuous pores is 1 to 1000 μm.

13. 13. The absorbent body according to claim 1, The absorbent body is characterized by comprising the polymer absorbent and a polymer compound having a water retention capacity higher than that of the polymer absorbent.

14. 14. The absorbent body according to claim 1, The absorbent body is characterized in that the total ion exchange capacity of -COONa groups per unit weight of the polymer absorbent is 4.0 mg equivalent / g or more.

15. An absorbent article comprising the absorbent body according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Water absorbing resin particles, method for manufacturing water absorbing resin particles, absorption body, absorptive article, and water-sealing material

    WO2013018571A1