Method for manufacturing bond magnet and compound for bond magnet

By using a thermosetting resin and curing agent with a controlled reactive group ratio, the bonded magnet compound's fluidity and mechanical properties are enhanced, addressing moldability issues and resulting in stronger magnets with improved moldability.

JP2024147593AActive Publication Date: 2024-10-16NICHIA CORP

Patent Information

Application Number
JP2024106295
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-07-22
Filing Date
2024-07-01
Publication Date
2024-10-16
Estimated Expiration
2040-06-17

AI Technical Summary

Technical Problem

Existing bonded magnet production methods face challenges in improving the fluidity and mechanical properties of bonded magnet compounds due to reactive group interactions between thermoplastic and thermosetting resins, leading to poor moldability and mechanical performance.

Method used

Incorporating a thermosetting resin and curing agent with a specific reactive group ratio of 2 to 11, and using a bonded magnet additive that includes a cured product of these components, along with a magnetic material and thermoplastic resin, to enhance fluidity and mechanical properties through controlled reaction and injection molding.

Benefits of technology

The method improves the fluidity and mechanical properties of bonded magnets, allowing for lower injection pressures and enhanced mechanical strength, thereby improving moldability and overall magnet performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147593000001
    Figure 2024147593000001
  • Figure 2024147593000002
    Figure 2024147593000002
Patent Text Reader

Abstract

To provide an additive for a bond magnet which can improve flowability of a compound for a bond magnet containing a thermoplastic resin, and mechanical characteristics of a bond magnet, and a compound for a bond magnet which improves these characteristics, and a method for manufacturing a bond magnet.SOLUTION: An additive for a bond magnet containing a thermoplastic resin contains a cured product of a thermosetting resin, and a curing agent having a ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin of 2 or more and 11 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an additive for bonded magnets and a method for producing a compound for bonded magnets. [Background technology]

[0002] Patent Documents 1 and 2 disclose a method for producing a bonded magnet in which a thermoplastic resin and SmFeN particles are melt-kneaded, then compression-molded to produce a compound, which is then injection-molded.

[0003] On the other hand, Patent Document 3 discloses a bonded magnet that uses NdFeB magnetic powder, epoxy resin, and an amine-based hardener as a hardener for the epoxy resin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-43804 A [Patent Document 2] JP 2004-115921 A [Patent Document 3] JP 2010-232468 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide an additive for bonded magnets that can improve the fluidity of bonded magnet compounds containing thermoplastic resins and the mechanical properties of bonded magnets, as well as a compound for bonded magnets with improved properties and a method for producing the bonded magnets. [Means for solving the problem]

[0006] An additive for bonded magnets containing a thermoplastic resin according to one embodiment of the present invention contains a cured product of a thermosetting resin and a curing agent in which the ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin is 2 or more and 11 or less.

[0007] A manufacturing method for a bonded magnet compound according to one embodiment of the present invention includes a step of thermally curing a thermosetting resin and a curing agent, the ratio of which to the number of reactive groups of the thermosetting resin is 2 or more and 11 or less, to obtain a bonded magnet additive, and a kneading step of kneading the bonded magnet additive, a magnetic material, and a thermoplastic resin.

[0008] A method for producing a bonded magnet according to one embodiment of the present invention includes a step of thermally curing a thermosetting resin and a curing agent in which the ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin is 2 or more and 11 or less to obtain an additive for a bonded magnet, a kneading step of kneading the additive for a bonded magnet, a magnetic material, and a thermoplastic resin, and an injection molding step of injection molding the obtained compound for a bonded magnet. Effect of the Invention

[0009] According to the above embodiment, it is possible to improve the flowability of the bonded magnet compound containing a thermoplastic resin, and the mechanical properties of the bonded magnet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present invention will be described in detail. However, the embodiments shown below are examples for embodying the technical idea of ​​the present invention, and the present invention is not limited to the following. In this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.

[0011] The additive for bonded magnets containing thermoplastic resin of the present invention is characterized by containing a cured product of a thermosetting resin and a curing agent having a ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin of 2 or more and 11 or less. Conventionally, when making a bonded magnet containing a thermoplastic resin, if a mixture of a thermosetting resin and a thermosetting resin is injection molded, the reactive groups of the thermosetting resin (e.g., glycidyl groups in the case of epoxy resin) react with the reactive groups of the thermoplastic resin (e.g., amide groups in the case of nylon 12), which may cause the fluidity of the resin to decrease and the moldability to deteriorate. In the cured product of the thermosetting resin of this embodiment and a curing agent having an equivalent ratio to the equivalent of the thermosetting resin of 2 or more and 11 or less, the reactive groups of the thermosetting resin are sufficiently deactivated by the reactive groups of the curing agent (e.g., amino groups in the case of DDS (diaminodiphenylsulfone)), so that the reaction with the reactive groups of the thermoplastic resin is unlikely to occur and the decrease in the fluidity of the resin can be suppressed, and therefore it can be used as an additive for bonded magnets containing thermoplastic resin. Furthermore, when a bonded magnet is produced by injection molding using a bonded magnet compound made from the bonded magnet additive containing the thermoplastic resin of this embodiment, the injection pressure can be reduced, thereby improving the mechanical properties of the resulting bonded magnet.

[0012] The thermosetting resin is not particularly limited as long as it is thermosetting, and examples thereof include epoxy resin, phenol resin, urea resin, melamine resin, guanamine resin, unsaturated polyester, vinyl ester resin, diallyl phthalate resin, polyurethane resin, silicone resin, polyimide resin, alkyd resin, furan resin, dicyclopentadiene resin, acrylic resin, and allyl carbonate resin. Among them, epoxy resin is preferable in terms of mechanical properties and heat resistance. The thermosetting resin is preferably a liquid at room temperature or a solid that dissolves in a solvent and becomes liquid.

[0013] The curing agent is not particularly limited as long as it can thermally cure the selected thermosetting resin, and when the thermosetting resin is an epoxy resin, examples of the curing agent include amine-based curing agents, acid anhydride-based curing agents, polyamide-based curing agents, imidazole-based curing agents, phenolic resin-based curing agents, polymercaptan resin-based curing agents, polysulfide resin-based curing agents, organic acid hydrazide-based curing agents, etc. Examples of the amine-based curing agents include diaminodiphenylsulfone, metaphenylenediamine, diaminodiphenylmethane, diethylenetriamine, triethylenetetramine, etc.

[0014] The amount of the curing agent is adjusted by the ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin (the ratio of the equivalent of the curing agent to the equivalent of the thermosetting resin). The ratio of the number of reactive groups of the curing agent to the number of reactive groups of the thermosetting resin is 2 or more and 11 or less, preferably 2 or more and 10 or less, and more preferably 2 or more and 7 or less. The lower limit of the number of reactive groups is preferably more than 2.5, more preferably 3 or more. If the ratio exceeds 11, the mechanical properties of the bonded magnet are reduced, and if it is less than 2, the ratio of the reactive groups of the curing agent to the reactive groups of the thermosetting resin is small, so that the reactive groups of the thermosetting resin remain. When kneaded with the thermoplastic resin in the subsequent process, the reactive groups of the thermoplastic resin react with the remaining reactive groups of the thermosetting resin, causing an increase in viscosity during injection molding, and the moldability of the bonded magnet and the mechanical properties of the obtained molded product are worse than those of the thermoplastic resin alone. Here, the equivalent of a thermosetting resin species refers to the number of grams of resin containing 1 gram equivalent of reactive groups, and the equivalent of a hardener species refers to the active hydrogen equivalent.

[0015] The cured product can be obtained by mixing the above-mentioned thermosetting resin with a curing agent and then thermally curing the mixture. The temperature for thermal curing can be set according to the characteristics of the thermosetting resin used, but in order to suppress the magnetic deterioration of the magnetic material due to heat and to perform thermal curing, a temperature of 60°C or higher and 250°C or lower is preferable, and 180°C or higher and 220°C or lower is even more preferable.

[0016] The cured product can be pulverized as necessary. The method for pulverizing the cured product is not particularly limited, and a sample mill, a ball mill, a stamp mill, a mortar, a mixer pulverization, or the like can be used. If necessary, the pulverized product can be classified using a sieve or the like. The average particle size of the pulverized product is preferably 1000 μm or less, more preferably 500 μm or less, from the viewpoint of compatibility with the thermoplastic resin.

[0017] The additive for bonded magnets can also be cured by mixing a curing accelerator with the thermosetting resin and the curing agent. Examples of the curing accelerator include 1,8-diazabicyclo(5,4,0)-undecene-7, 1,5-diazabicyclo(4,3,0)-nonene-5, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-methyl-4-methylimidazole, triphenylphosphine, and sulfonium salts. The amount of the curing accelerator is not particularly limited, but is generally added in an amount of 0.01% by mass or more and 10% by mass or less based on the total amount of the thermosetting resin and the curing agent.

[0018] The manufacturing method for the bonded magnet compound of this embodiment is characterized by including a step of thermally curing a thermosetting resin and a curing agent whose equivalent ratio to the equivalent weight of the thermosetting resin is 2 or more and 11 or less to obtain an additive for the bonded magnet, and a kneading step of kneading the additive for the bonded magnet, a magnetic material, and a thermoplastic resin.

[0019] The process for obtaining the bonded magnet additive of this embodiment is as described above.

[0020] In the kneading process, the bond magnet additive, magnetic material, and thermoplastic resin are melt-kneaded to prepare a bond magnet compound to be used in injection molding. The melt kneader is not particularly limited, but a single screw kneader, twin screw kneader, mixing roll, kneader, Banbury mixer, intermeshing twin screw extruder, non-intermeshing twin screw extruder, etc. can be used. The melt kneading temperature is not particularly limited and can be set according to the characteristics of the thermoplastic resin used, but it is preferably 180°C or higher and 250°C or lower.

[0021] The thermoplastic resin is not particularly limited as long as it is an injection moldable resin, and examples thereof include nylon resin (polyamide resin), polyolefins such as polypropylene (PP) and polyethylene (PE), polyester, polycarbonate (PC), polyphenylene sulfide resin (PPS), polyether ether ketone (PEEK), polyacetal (POM), liquid crystal polymer (LCP), etc. Examples of the nylon resin include polylactams such as nylon 6, nylon 11, and nylon 12, condensates of dicarboxylic acid and diamine such as nylon 6,6, nylon 6,10, and nylon 6,12, copolymer polyamides such as nylon 6 / 6,6, nylon 6 / 6,10, nylon 6 / 12, nylon 6 / 6,12, nylon 6 / 6,10 / 6,10, nylon 6 / 6,6 / 6,12, and nylon 6 / polyether, nylon 6T, nylon 9T, nylon MXD6, aromatic nylon, and amorphous nylon. Among these, nylon resin is preferred, and nylon 12 is particularly preferred, because of its low water absorption rate, moldability, and mechanical properties.

[0022] The magnetic material is not particularly limited, but examples thereof include rare earth magnetic materials of SmFeN, NdFeB, and SmCo. Among them, SmFeN is preferable because of its heat resistance and the absence of rare metals. As the SmFeN magnetic material, Th2Zn 17 It has a crystal structure of the type Sm x Fe 100-x-y N y It is a nitride composed of rare earth metal Sm, iron Fe, and nitrogen N, represented by the formula: Here, it is preferable that x is 8.1 atomic % or more and 10 atomic % or less, y is 13.5 atomic % or more and 13.9 atomic % or less, and the remainder is mainly Fe.

[0023] The SmFeN magnetic material can be produced by the method disclosed in Japanese Patent Application Laid-Open No. 11-189811. The NdFeB magnetic material can be produced by the HDDR method disclosed in International Publication No. 2003 / 85147. The SmCo magnetic material can be produced by the method disclosed in Japanese Patent Application Laid-Open No. 08-260083. In addition, the magnetic material can be surface-treated with a silane coupling agent by the method shown in Patent Document 1, for example.

[0024] The average particle size of the magnetic material is preferably 10 μm or less, more preferably 6 μm or less, and even more preferably 4 μm or less. The average particle size is measured as the particle size that corresponds to 50% of the cumulative volume from the small particle size side in the particle size distribution. The particle size distribution of the magnetic material used in the bonded magnet compound is preferably monodisperse from the viewpoint of the squareness of the demagnetization characteristics.

[0025] The magnetic material can also be surface-treated with a silane coupling agent, which enhances the bond between the magnetic material and the resin, making it possible to suppress an increase in viscosity during injection molding.

[0026] The silane coupling agent has the general formula: X-Si-(OR) n (wherein X is an alkyl group having a polar group at the end, R is an alkyl group having 1 to 3 carbon atoms, and n is an integer of 1 to 3), and it is preferable that the polar group in X has an amino group, a ureido group, an epoxy group, a thiol group, or a methacryloxy group. When using a nylon resin as the thermoplastic resin, it is preferable to use a coupling agent having an amino group that has high affinity with the nylon resin, and it is particularly preferable to use 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, or 3-(2-aminoethyl)aminopropylmethyltriethoxysilane.

[0027] The amount of magnetic material added in the kneading step is preferably 93.2% by mass or less, and more preferably 75% to 92.5% by mass, in terms of the content of magnetic material in the bonded magnet compound. If it exceeds 93.2% by mass, the viscosity during injection molding increases, decreasing moldability, and if it is less than 75% by mass, the residual magnetic flux density of the bonded magnet decreases.

[0028] The amount of the bond magnet additive added in the kneading step is preferably 0.1% by mass or more and 2.5% by mass or less, and more preferably 0.2% by mass or more and 2.0% by mass or less, as the content of the bond magnet additive in the bond magnet compound. If the content of the bond magnet additive exceeds 2.5% by mass, the mechanical properties will decrease, and if it is less than 0.1% by mass, the effect of adding the bond magnet additive will be small.

[0029] The amount of thermoplastic resin added in the kneading step is preferably 6.3% by mass or more, more preferably 7.0% by mass or more and 24.5% by mass or less, in terms of the content of thermoplastic resin in the bond magnet compound. If the amount of thermoplastic resin added exceeds 24.5% by mass, the residual magnetic flux density decreases, and if it is less than 6.3% by mass, the viscosity during injection molding increases, resulting in reduced moldability.

[0030] The compound for bonded magnets of this embodiment is obtained by the manufacturing method described above.

[0031] The method for producing the bonded magnet of this embodiment is as follows: A step of thermally curing a thermosetting resin with a curing agent having a ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin of 2 or more and 11 or less to obtain an additive for bonded magnets; A kneading step of kneading the additive for the bonded magnet, the magnetic material, and the thermoplastic resin; and an injection molding process for injection molding the resulting bonded magnet compound. The present invention is characterized by comprising:

[0032] The process for obtaining the additive for a bonded magnet and the kneading process are as described above.

[0033] In the injection molding process, the bonded magnet compound is injection molded to obtain an injection molded product. The cylinder temperature of the injection molding machine may be within the temperature range in which the bonded magnet compound melts, and is preferably 260°C or less in order to suppress magnetic deterioration of the magnetic material due to heat. The injection pressure may be any pressure that allows the molten compound to be injected, but for example, when the cylinder temperature of the injection molding machine is 260°C and injection molding is performed into a cavity with a width of 10 mm, a thickness of 4 mm, and a length of 80 mm, it is preferable that the cavity can be completely filled at less than 162 MPa in terms of moldability.

[0034] The bonded magnet of this embodiment is obtained by the manufacturing method described above. EXAMPLES

[0035] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples.

[0036] In the examples and comparative examples, the following materials were used. Epoxy resin: Biphenyl type (epoxy equivalent: 186g / eq) Hardener: DDS (diaminodiphenyl sulfone) (active hydrogen equivalent: 62.0 g / eq) Curing accelerator: TPP (triphenylphosphine) Magnetic material: Surface-treated SmFeN-based magnetic material (Average particle size 3μm (particle size distribution is monodisperse), residual magnetic flux density of magnetic powder alone Br=1.31T)

[0037] Manufacturing Example 1 100 parts by mass of the SmFeN magnetic material was surface-treated using 1.875 parts by mass of ethyl silicate and 0.4 parts by mass of 3-aminopropyltriethoxysilane silane (Z-6011, manufactured by Dow Corning Toray Co., Ltd.) to prepare a surface-treated SmFeN magnetic material.

[0038] Example 1 (Preparation of additives for bonded magnets) 12 parts by mass of epoxy resin, 8.9 parts by mass of hardener, and 0.4 parts by mass of hardening accelerator were dissolved and mixed in 100 parts by mass of acetone. After volatilizing the acetone, the mixture was hardened in a shelf dryer at 200°C for 6 hours under a nitrogen atmosphere. The hardened product was pulverized in a mixer and classified using a sieve with 500 μm openings to produce an additive for bonded magnets.

[0039] (Making compounds for bonded magnets) 100 parts by mass of the surface-treated SmFeN magnetic material produced in Example 1 was mixed with 0.5 parts by mass of an additive for bonded magnets and 8.8 parts by mass of polyamide 12, and the mixture was melt-extruded and mixed in a twin-screw mixer at 230°C to obtain a compound for bonded magnets.

[0040] (Production of bonded magnets) The bonded magnet compound was injection molded at a cylinder temperature of 260°C, a mold temperature of 90°C, and an injection pressure of 152 MPa to obtain a bonded magnet strength test piece having a width of 10 mm, a thickness of 4 mm, and a length of 116 mm.

[0041] Comparative Example 1 9.2 parts by mass of polyamide 12 was mixed with 100 parts by mass of the surface-treated SmFeN magnetic material, and melt-extruded and kneaded in a twin-screw kneader at 230°C to obtain a bonded magnet compound. Next, a bonded magnet was produced using the obtained bonded magnet compound in the same manner as in Example 1. The bending strength was measured. The injection pressure during injection molding is shown in Table 1.

[0042] Examples 2 and 3 and Comparative Example 2 A compound for bonded magnets and a bonded magnet were obtained in the same manner as in Example 1, except that the composition when preparing the additive for bonded magnets was changed as shown in Table 1.

[0043] In the examples and comparative examples, the injection pressure used during injection molding of the bonded magnets is shown in Table 1. Additionally, the bending strength of the bonded magnets was measured using an Instron universal testing machine, and the results are shown in Table 2.

[0044] [Table 1]

[0045] As can be seen from Table 1, the compositions of Examples 1 to 3 had lower injection pressures compared to the compositions of Comparative Examples 1 and 2, which shows that compositions containing an additive for bonded magnets that contains a cured product of a thermosetting resin and a curing agent whose equivalent ratio to the equivalent of the thermosetting resin is in a specific range improve the fluidity of the compound for bonded magnets.

[0046] [Table 2]

[0047] As can be seen from Table 2, the bonded magnets of Examples 1 to 3 have higher bending strength than the bonded magnets of Comparative Examples 1 and 2, and it was therefore confirmed that the mechanical properties are also improved in bonded magnets made from compositions containing additives for bonded magnets that contain a cured product of a thermosetting resin and a curing agent whose equivalent ratio to the equivalent of the thermosetting resin is within a specific range. [Industrial Applicability]

[0048] The additive for bonded magnets of the present invention can greatly improve the flowability of the compound for bonded magnets and can also improve the mechanical properties of the resulting bonded magnets. The resulting bonded magnets can be suitably used as composite materials and bonded magnets in motors and other applications.

Claims

1. An additive for bonded magnets containing thermoplastic resins, characterized in that it contains a cured product of a thermosetting resin and a curing agent in which the ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin is 2 or more and 11 or less.

2. 2. The additive for bonded magnets according to claim 1, wherein said thermoplastic resin is a nylon resin.

3. A step of thermally curing a thermosetting resin and a curing agent having a ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin of 2 to 11 to obtain an additive for bonded magnets; A kneading process for kneading the additives for bonded magnets, the magnetic material, and the thermoplastic resin. A method for producing a compound for a bonded magnet comprising the steps of:

4. 4. The method for producing a compound for a bonded magnet according to claim 3, wherein said thermoplastic resin is a nylon resin.

5. 5. The method for producing a compound for a bonded magnet according to claim 3, wherein the magnetic material has a monodisperse particle size distribution.

6. The method for producing a compound for a bonded magnet according to any one of claims 3 to 5, wherein the magnetic material contains Sm, Fe and N.

7. A compound for bonded magnets obtained by the manufacturing method according to any one of claims 3 to 6.

8. A step of thermally curing a thermosetting resin with a curing agent having a ratio of the number of reactive groups to the number of reactive groups of the thermosetting resin of 2 or more and 11 or less to obtain an additive for bonded magnets; A kneading step of kneading the additive for the bonded magnet, the magnetic material, and the thermoplastic resin; and an injection molding step of injection molding the obtained bonded magnet compound.

9. A bonded magnet obtained by the manufacturing method according to claim 8.

Citation Information

Patent Citations

  • Metal element-containing powder, mold, and method for manufacturing metal element-containing powder

    JP2019106431A

  • Powdered metals and structural metals having improved resistance to heat and corrosive fluids and b-stage powders for making such powdered metals

    US20090010784A1

  • Additive for bonded magnet and method for manufacturing compound for bonded magnet

    WO2021014837A1

  • Sm-Fe-N BASED ALLOY POWDER AND METHOD FOR MANUFACTURING THE SAME

    JP2004115921A

  • Rare earth bonded magnet

    JP2010232468A

Cited By

  • Eco-friendly high-performance and high-heat-resistant hybrid bond magnet compound, bond magnet using the same, and method for manufacturing the same

    KR103007900B1