Mud material for blocking blast furnace tap hole
By integrating alumina shot blast powder into the mud material, the strength and porosity of blast furnace tap hole blocking materials are optimized, addressing the structural challenges of conventional materials and enhancing their performance.
Patent Information
- Application Number
- JP2024113489
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-16
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional mud materials for blocking blast furnace tap holes exhibit strong structures that hinder easy opening and compromise pore opening properties, affecting hot metal resistance and slag resistance.
Incorporation of alumina shot blast powder, a recycled material from post-use processing, into the mud material composition to enhance porosity and maintain corrosion resistance.
The inclusion of alumina shot blast powder improves pore opening properties and corrosion resistance while reducing waste, resulting in a mud material with enhanced fluidity and reduced binder usage.
Smart Images

Figure 2024147692000001 
Figure 2024147692000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a mud material for plugging a blast furnace taphole. [Background technology]
[0002] Blast furnace taphole plugging mud is a clay-like material used to fill and plug the taphole of a blast furnace. In the iron-making process in the production of iron, iron ore is melted in a blast furnace whose taphole is plugged with mud to produce pig iron, and then the mud is broken to open the taphole and the pig iron is extracted.
[0003] Conventional mud materials for plugging the taphole of a blast furnace are disclosed in, for example, Patent Document 1 and Patent Document 2 listed below. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 08-119754 [Patent Document 2] Japanese Patent Application Publication No. 11-029366 Summary of the Invention [Problem to be solved by the invention]
[0005] Patent Document 1 discloses a mud material for blocking blast furnace tapholes, which is made by adding 10 to 17 weight percent liquid tar as a binder to 100% refractory aggregate composed of 30 to 50 weight percent alumina raw materials, 2 to 5 weight percent silica raw materials, 15 to 25 weight percent silicon carbide, 5 to 10 weight percent carbonaceous raw materials, 15 to 30 weight percent nitrides, and 5 to 15 weight percent metal powder.
[0006] Patent Document 2 describes a powder containing 30 to 50% by weight of an alumina-based raw material including calcined alumina, 2 to 5% by weight of a silica-based raw material, 15 to 25% by weight of silicon carbide, 5 to 10% by weight of a carbonaceous raw material, 15 to 30% by weight of a nitride, and 5 to 15% by weight of a metal powder, with 5% by weight or less of particles having a particle size of more than 1 mm and a particle size of less than 0.075 mm (excluding calcined alumina having a particle size of 2 μm or less). The present invention discloses a mud material for plugging a blast furnace tap hole, which is made by adding 100% by weight of refractory aggregate having a particle size composition consisting of 60-70% by weight of calcined alumina, 5-15% by weight of calcined alumina with a particle size of 2 μm or less, and the remainder with a particle size of 1-0.075 mm, to which 10-17% by weight of liquid tar as a binder is added by outer coating.
[0007] The mud material for plugging blast furnace tap holes disclosed in Patent Document 1 is expected to have improved strength and corrosion resistance, and is said to have good hole opening properties, but its strength may be so high that it may take a long time to open holes.
[0008] The mud material for plugging blast furnace tap holes disclosed in Patent Document 2 is characterized by a particle size composition that uses a large amount of fine raw materials, and by using a large amount of alumina components, it has excellent resistance to molten iron and slag. However, it has high strength and a dense structure, making it difficult to open holes.
[0009] As described above, while conventional mud materials for plugging blast furnace tapholes have excellent resistance to molten iron and slag, they have the problem that their structure is hard and they have poor hole opening properties. [Means for solving the problem]
[0010] The mud material for plugging a blast furnace tap hole according to the present invention is characterized in that it contains used alumina shot blast powder.
[0011] The mud material for plugging a blast furnace tap hole according to the present invention preferably contains 2% by mass or more and 50% by mass or less of the used alumina shot blast powder.
[0012] In the mud material for plugging a blast furnace tap hole according to the present invention, it is preferable that the maximum particle size of the used alumina shot blast powder is 3 mm or less. Effect of the Invention
[0013] In the ironworks and non-ferrous metals industries, alumina shot (alumina blasting) processing is carried out by spraying aluminum oxide abrasives (polishing agents) onto products to smooth their surface roughness, remove rust and dirt, etc. The alumina used in this processing is called used alumina shot blast powder.
[0014] As a result of the inventors' investigation into mud materials with excellent porosity, they discovered that by applying used alumina shot blast powder generated after the application of alumina shot to mud materials, mud materials with excellent porosity while maintaining the corrosion resistance of conventional mud materials can be obtained.
[0015] In addition, since used alumina shot blast powder is discharged and discarded on a monthly basis in the large-scale steel product manufacturing industry, for example, by using the used alumina shot blast powder as a recycled raw material for mud material, it is possible to significantly reduce the amount of waste. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The mud material for plugging a blast furnace tap hole of the present invention comprises a known refractory aggregate and used alumina shot blast powder.
[0017] The used alumina shot blast dust in this invention means the shot blast dust generated after processing such as deburring, surface polishing, precision grinding, etc., by projecting granular alumina onto the surface of a workpiece made of steel material, etc. Note that the mechanism by which the effect of the present invention is achieved is not completely clear, but it is presumed that the metal powder adhering to the alumina surface contributes to this.
[0018] The preferred Fe content, as well as the preferred Al2O3 content, particle size, and particle shape, when the used alumina shot blast powder contains, for example, Fe in the present invention, will be described in detail below.
[0019] <Fe content> The Fe content in the used alumina shot blast powder is preferably 2 to 25% by mass, more preferably 5 to 20% by mass. Incidentally, the Fe content can be measured using the bromine methanol method or the like. The matte material during tapping will be exposed to 1400 °C or higher. However, when the used alumina shot blast powder contains an Fe component, it is considered that the Fe component functions as a reaction catalyst for the reaction between silicon nitride and carbon contained in the matte material, promoting the following reaction to generate SiC and nitrogen gas. Reaction formula: 3Fe + Si3N4 + 2C → Fe3Si + 2SiC + 2N2 (reaction temperature range: about 1400 °C)
[0020] The generation of SiC bonds in the matrix part of the matte material is promoted, improving the corrosion resistance of the matte material. At the same time, the generated nitrogen gas makes the matte material porous, improving the porosity. Therefore, when the used alumina shot blast powder contains an Fe component, it becomes easier to obtain a matte material excellent in corrosion resistance and porosity.
[0021] <Al2O3 content> The Al2O3 content in the used alumina shot blast powder is preferably 70 to 98% by mass, more preferably 80 to 95% by mass. Incidentally, the Al2O3 content can be measured by fluorescence X-ray analysis using glass beads according to the provisions of Japanese Industrial Standard JIS R 2216. The Al2O3 component contained in the used alumina shot blast powder improves the corrosion resistance and slag resistance of the matte material.
[0022] <Particle size> The maximum particle size of the used alumina shot blast powder is not particularly limited, but is preferably 3 mm or less, more preferably 1 mm or less, and even more preferably 0.075 mm or less. The reactivity of the used alumina shot blast powder with silicon nitride, iron, and carbon is favorable when the maximum particle size of the used alumina shot blast powder is 3 mm or less, because the used alumina shot blast powder disperses well in the mud material. The particle size at this time is determined by sieving using a JIS Z 8801-1 sieve.
[0023] <Particle shape> The particle shape of the used alumina shot blast powder is preferably rounded, and for example, in terms of roundness, an average of 0.3 or more is preferable, and an average of 0.5 or more is more preferable. The average roundness of the used alumina shot blast powder can be calculated by comparing each particle one by one with Krumbein's roundness impression diagram. If the average roundness is 0.3 or more, it is easy to exert a ball bearing effect that increases fluidity by reducing friction between the raw materials during kneading, and the amount of binder added to obtain the plasticity required for the mud material can be reduced. In the structure of the mud material with reduced binder addition, the distance between the raw materials is closer, and the reactivity of the used alumina shot blast powder, silicon nitride iron, and carbon is increased.
[0024] The mud material for plugging a blast furnace tap hole of the present invention preferably contains 2 to 50 mass % of used alumina shot blast powder.
[0025] Examples of the refractory aggregate applicable to the mud material for plugging a blast furnace tap hole of the present invention include one or more oxide refractory raw materials selected from alumina raw materials, alumina-silica raw materials, clay raw materials and silica raw materials, carbonaceous raw materials, silicon carbide raw materials, silicon nitride raw materials, etc. Only one of these raw materials may be selected, or two or more may be used in combination.
[0026] The amount of the oxide refractory raw material is preferably 5% by mass or more and 85% by mass or less, more preferably 30% by mass or more and 75% by mass or less. If the amount exceeds 85% by mass, the corrosion resistance decreases, and if it is less than 5% by mass, the porosity tends to be too high. Examples of the oxide refractory raw material that can be used include sintered alumina, fused alumina, aluminium shale, bauxite, chamotte raw material, pyrite, mullite, andalusite, and silica fume.
[0027] Examples of carbonaceous raw materials constituting the refractory aggregate include graphite, amorphous graphite, coal coke, petroleum coke and powders of these cokes, graphite electrode scraps, carbon black, coal pitch, petroleum pitch, etc. The carbonaceous raw materials are added for the purpose of suppressing the penetration of slag and suppressing over-sintering, and the blending amount is preferably 3% by mass or more and 20% by mass or less, more preferably 4% by mass or more and 16% by mass or less. If the blending amount of the carbonaceous raw materials is less than 3% by mass, it is not preferable because it will result in over-sintering, while if it exceeds 20% by mass, it is not preferable because the strength will decrease.
[0028] As the silicon carbide raw material constituting the refractory aggregate, for example, a silicon carbide raw material produced by the Acheson process or a silicon carbide raw material obtained by reducing and carbonizing silica can be used. The silicon carbide raw material is added for the purpose of improving corrosion resistance against slag, and the blending amount is preferably 5% by mass or more and 50% by mass or less, more preferably 10% by mass or more and 30% by mass or less. The blending amount of the silicon carbide raw material is desirably 5% by mass or more and 50% by mass or less. If the blending amount is less than 5% by mass, the contribution to improving corrosion resistance is small, and if it exceeds 50% by mass, the strength after sintering decreases.
[0029] If necessary, silicon nitride raw materials may be blended to improve corrosion resistance. Examples of such silicon nitride raw materials include silicon nitride obtained by reducing and nitriding silica, silicon nitride obtained by directly nitriding metal silicon, and silicon ferronitride obtained by directly nitriding ferrosilicon. The blending amount is preferably 3% by mass or more and 45% by mass or less, and more preferably 10% by mass or more and 40% by mass or less. The blending amount of silicon nitride raw materials is desirably 3% by mass or more and 45% by mass or less. If it is less than 3% by mass, it is difficult to obtain a sufficient effect on improving corrosion resistance, while if it exceeds 45% by mass, the silicon nitride raw materials are somewhat expensive among the raw materials of the mud material, and it is difficult to obtain an effect of adding them that is commensurate with the cost of the mud material.
[0030] If necessary, one or more kinds of metal powders may be added, such as aluminum metal, silicon metal, and aluminum metal-silicon alloy.
[0031] If necessary, coal tar or phenol resin for mud materials may be used as an organic binder. The amount of organic binder added can be appropriately adjusted depending on the usage situation of the mud material and the required performance.
[0032] The mud material for plugging the tap hole of a blast furnace according to the present invention can be produced by mixing at least the above-mentioned refractory aggregate and used alumina shot blast powder using a known mixing device and mixing method. Such a mixing device is not particularly limited, but for example, a Fukai-type Conner mixer, an upper mixer, an Eirich mixer, etc. can be used.
[0033] The method for filling and plugging the taphole of a blast furnace using the mud material for plugging the taphole of a blast furnace according to the present invention is not particularly limited, and any commonly used filling and plugging method may be used. EXAMPLES
[0034] The following Table 1 shows an example of the mud material for blocking blast furnace tap holes of the present invention, which contains used alumina shot blast powder, and a comparative example of the mud material not containing used alumina shot blast powder. [Table 1]
[0035] Each of Examples 1 to 4 in Table 1 is a mud material made by mixing alumina shot blast powder after use with a refractory aggregate based on a mixture of rosewood, alumina, carbon, silicon carbide, clay, and silicon ferronitride, and adding anhydrous tar as an organic binder. Comparative Examples 1 and 2 are mud materials with a mixture that does not contain alumina shot blast powder after use.
[0036] The mud material obtained above was placed in a 40 x 40 x 160 mm mold, molded under a pressure of 5.0 MPa, and dried in a dryer at 300°C for 12 hours. After drying, the sample was buried in coke breeze and heated at 1500°C for 3 hours to prepare a test piece.
[0037] <Bending strength> A bending test was conducted to evaluate the hole opening property. In the bending test, the test pieces were measured in accordance with JIS R 2553. When the bending strength was 10 MPa or more, the strength was judged to be high and excellent in corrosion resistance, but the strength was too high and the hole opening property was judged to be poor, and when the bending strength was less than 10 MPa, the hole opening property was judged to be excellent.
[0038] The mud materials of Examples 1 to 4 containing used alumina shot blast powder were found to have better pore opening properties than the mud materials of Comparative Examples 1 and 2 containing no used alumina shot blast powder.
[0039] Next, the compositions and test results of Examples 5 to 22 and Comparative Examples 3 to 5, which were tested with a focus on the particle size composition of the raw materials, are shown in Table 2 below. [Table 2]
[0040] The bending test was carried out in the same manner as in Table 1. The corrosion resistance was evaluated by carrying out tests on the molten iron resistance index and the slag resistance index as described below.
[0041] <Hot metal resistance index> A test of molten iron resistance was performed, and an index was calculated and evaluated. The corrosion resistance against molten iron was evaluated by a sample lining test using a high-frequency induction furnace. A form was filled with mud material, and the test piece was heated at 800 ° C for 3 hours while being buried in coke breeze. Each test piece was combined into a crucible shape, 20 kg of pig iron was put into the crucible as an erosion agent, and the test was performed by holding it at 1550 to 1600 ° C for 4 hours. The erosion volume of the sample after the test was measured, and an index was calculated and evaluated. The erosion volume of the comparative product 1 was set to 100, and the index of each example and comparative example was calculated by the following formula. The smaller the index, the better the molten iron resistance. Molten iron resistance index = (erosion volume of each test piece ÷ erosion volume of Comparative Example 1) × 100
[0042] <Slag resistance index> A test of slag resistance was carried out, and an index was calculated and evaluated. The corrosion resistance against blast furnace slag was evaluated by a rotating drum corrosion test method. The mud material was filled into a formwork, and the test piece was heated at 800 ° C for 3 hours while being buried in coke breeze. Each test piece was combined into a drum shape, and 1 kg of blast furnace slag was put into the drum as an erosion agent, and the test piece was held at 1550 to 1600 ° C for 4 hours. The erosion agent was replaced every hour. The melting depth of the mud material sample after the test was measured, and an index was calculated and evaluated. Comparative product 1 was set to 100, and the index of each example and comparative example was calculated using the following formula. The smaller the index, the better the slag resistance. Slag resistance index = (erosion depth of each test piece ÷ erosion depth of Comparative Example 1) × 100
[0043] In Examples 5 to 9, used alumina shot blast powder with a particle size of more than 1 mm was used and the blending amount was changed. In Examples 10 to 14, used alumina shot blast powder with a particle size of 0.075 mm to 1 mm was used and the blending amount was changed. In Examples 15 to 22, used alumina shot blast powder with a particle size of less than 0.075 mm was used and the blending amount was changed.
[0044] As shown in Table 2, all of Examples 5 to 22 were excellent in corrosion resistance and pore opening property. [Industrial Applicability]
[0045] The mud material according to the present invention can be suitably used, in particular, as a mud material for plugging a taphole of a blast furnace.
Claims
[Claim 1] A mud material for plugging a blast furnace taphole, comprising used alumina shot blast powder.
Citation Information
Patent Citations
Material for sealing iron spout
JP1996119754A
Mud material for closing iron notch of blast furnace
JP1999029366A