Process for producing long-term color stable superabsorbent polymer particles
Thermal surface post-crosslinking with hydrogen peroxide enhances the color stability of superabsorbent polymer particles, addressing discoloration issues under high temperature and humidity, and maintains high absorbency and retention capacity.
Patent Information
- Application Number
- JP2024118485
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-10-29
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-16
AI Technical Summary
Superabsorbent polymer particles tend to discolor during storage under high temperatures or high humidity, particularly turning yellow, brown, or black, which is undesirable for sanitary products.
A method involving thermal surface post-crosslinking of polymer particles with hydrogen peroxide prior to thermal surface post-crosslinking, along with specific crosslinking agents and initiators, to enhance long-term color stability.
The method produces superabsorbent polymer particles with improved color stability, maintaining a yellowness index of 54 or less after 14 days at 70°C and 80% humidity, while maintaining high absorbency under pressure and centrifugal retention capacity.
Smart Images

Figure 2024147775000001 
Figure 2024147775000002 
Figure 2024147775000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing long-term color stable superabsorbent polymer particles, comprising the steps of polymerizing a monomer solution, drying the resulting polymer gel, optionally grinding and classifying the resulting dried polymer gel, and thermally surface post-crosslinking the resulting polymer particles and cooling, wherein a thermal surface post-crosslinker and hydrogen peroxide are added to the polymer particles prior to the thermal surface post-crosslinking. [Background technology]
[0002] Superabsorbent polymer particles are also used to make diapers, tampons, sanitary napkins, and other hygiene articles, as well as water retention agents in market gardens. Superabsorbent polymer particles are also often referred to as "absorbent resins," "superabsorbents," "superabsorbent polymers," "absorbent polymers," "absorbent gelling materials," "hydrophilic polymers," or "hydrogels."
[0003] The preparation of superabsorbent polymer particles is described in the monograph "Modern Superabsorbent Polymer Technology", FL Buchholz and AT Graham, Wiley-VCH, 1998, pages 71 to 103.
[0004] The properties of the superabsorbent polymer particles can be adjusted, for example, by the amount of crosslinker used. With increasing amounts of crosslinker, the centrifuge retention capacity (CRC) decreases, reaching 21.0 g / cm 2 The absorbency under pressure (AUL) passes through a maximum value.
[0005] Application properties, such as permeability of swollen gel bed (SFC) in diapers and 49.2 g / cm 2To improve absorbency under pressures of up to 49.2 g / cm (AUHL), superabsorbent polymer particles are generally surface postcrosslinked. This increases the degree of crosslinking on the particle surface, which in turn increases the absorbency under pressures of up to 49.2 g / cm 2 The absorbency under pressure (AUHL) and centrifuge retention capacity (CRC) can be at least partially separated. This surface postcrosslinking can be carried out in aqueous gel phase. However, preferably, the dried, ground and sieved polymer particles (base polymer) are surface-coated with a surface postcrosslinking agent, thermally surface postcrosslinked and dried. Crosslinking agents suitable for this purpose are compounds that can form covalent bonds with at least two carboxylate groups of superabsorbent polymer particles.
[0006] A problem that frequently occurs with superabsorbent polymer particles is that of discoloration during storage at high temperatures or high air humidity. Such conditions often occur during storage in tropical or subtropical countries. Under these conditions, superabsorbent polymer particles tend to yellow, and they may even take on a brown or even almost black color. This discoloration of practically colorless superabsorbent polymer particles is visible, especially in desired thin sanitary products, which is unsightly and undesirable, and consumers reject unsightly sanitary products. The cause of discoloration is not completely clear, but it seems that reactive compounds, such as monomers remaining from polymerization, the use of some initiators, impurities in the monomers or neutralizers, surface postcrosslinkers, or stabilizers in the monomers used, play a role.
[0007] EP1770113A1 discloses surface post-crosslinking in the presence of peroxides for the reduction of residual monomers.
[0008] WO2006 / 062258A2 discloses a method of surface post-crosslinking by adding a water-soluble polymerization initiator and irradiating the mixture with active energy rays. This method does not require heating.
[0009] WO2010 / 096595A2 discloses a superabsorbent polymer having antibacterial properties, which is coated with 0.5-20% by weight of hydrogen peroxide and dried.
[0010] EP 2 915 548 A1 discloses a method for the preparation of superabsorbent particles which involves the addition of peroxide after polymerization. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] EP1770113A1 [Patent Document 2] WO2006 / 062258A2 [Patent Document 3] WO2010 / 096595A2 [Patent Document 4] EP2915548A1 [Non-patent literature]
[0012] [Non-Patent Document 1] "Modern Superabsorbent Polymer Technology", FL Buchholz and AT Graham, Wiley-VCH, 1998, pages 71 to 103 Summary of the Invention [Problem to be solved by the invention]
[0013] It was an object of the present invention to provide a method for producing superabsorbent polymer particles having improved long-term color stability. [Means for solving the problem]
[0014] The object is to provide a method for producing long-term color-stable superabsorbent polymer particles, comprising: a) partially neutralized acrylic acid, b) optionally, at least one crosslinker, and c) at least one initiator the step of polymerizing a monomer solution containing the above-mentioned, the step of drying the obtained polymer gel, the step of optionally grinding and classifying the obtained dried polymer gel, and the step of thermally surface postcrosslinking the obtained polymer particles and cooling, wherein a thermal surface postcrosslinker and 0.014 to 0.095 wt % hydrogen peroxide based on the polymer particles are added to the polymer particles before the thermal surface postcrosslinking.
[0015] The thermal surface postcrosslinking agent is added to the polymer particles prior to thermal surface postcrosslinking, preferably in an amount of 0.005 to 5% by weight, more preferably 0.010 to 2% by weight, and most preferably 0.015 to 1% by weight, based on the polymer particles.
[0016] Suitable surface postcrosslinkers are, for example, polyfunctional amines, polyfunctional amidoamines, polyfunctional epoxides, di- or polyfunctional alcohols, β-hydroxyalkylamides, cyclic carbonates, 2-oxazolinones and derivatives thereof, bis- and poly-2-oxazolinones, 2-oxotetra-hydro-1,3-oxazines and derivatives thereof, cyclic ureas, bicyclic amide acetals, oxetanes, cyclic ureas, and morpholine-2,3-dione and derivatives thereof.
[0017] Hydrogen peroxide is added to the polymer particles prior to thermal surface post-crosslinking, preferably in an amount of 0.016-0.080% by weight, more preferably 0.018-0.065% by weight, most preferably 0.020-0.050% by weight, based on the polymer particles.
[0018] The temperature of the polymer particles during thermal surface postcrosslinking is preferably 110-220° C., more preferably 120-200° C., most preferably 130-190° C. Lower temperatures may be possible during the heating of the polymer particles.
[0019] The residence time of the polymer particles during the thermal surface post-crosslinking is preferably 10 to 120 minutes, more preferably 15 to 90 minutes, and most preferably 20 to 60 minutes. This residence time is the residence time of the polymer particles in the device used for the thermal surface post-crosslinking.
[0020] In a preferred embodiment of the present invention, the monomer solution contains a polymerization inhibitor in an amount of preferably 0.001 to 0.020% by weight, more preferably 0.002 to 0.015% by weight, and most preferably 0.004 to 0.010% by weight, based on the acrylic acid before neutralization.
[0021] Suitable polymerization inhibitors are, for example, hydroquinone monomethyl ether (MEHQ) and alpha-tocopherol (vitamin E). Hydroquinone monomethyl ether (MEHQ) is preferred.
[0022] In a preferred embodiment of the present invention, the chelating agent is added to the polymer particles during or after cooling, preferably in an amount of 0.005 to 1.0 wt %, more preferably 0.010 to 0.7 wt %, and most preferably 0.015 to 0.5 wt %, based on the polymer particles.
[0023] Suitable chelating agents are, for example, citric acid, tartaric acid, iminodiacetic acid, hydroxyethyliminodiacetic acid, nitrilotriacetic acid, nitrilotripropionic acid, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, triethylenetetraaminehexaacetic acid, N,N-bis(2-hydroxyethyl)glycine, trans-1,2-diaminocyclohexanepentaacetic acid, and 1-hydroxyethane-1,1-diphosphonic acid and / or its salts. 1-Hydroxyethane-1,1-diphosphonic acid and / or its salts are preferred.
[0024] Surface post-crosslinking is carried out by heating, no irradiation with active energy rays is required.
[0025] The present invention is based on the discovery that the long-term color stability of superabsorbent polymers can be increased by treating with hydrogen peroxide prior to thermal postcrosslinking. Too much hydrogen peroxide has a detrimental effect on absorbency under high load (AUHL).
[0026] The addition of hydrogen peroxide after thermal post-crosslinking, or the use of other peroxides, is less effective.
[0027] The present invention further provides superabsorbent polymer particles obtainable by the process according to the invention.
[0028] The superabsorbent polymer particles produced by the process according to the invention preferably have a centrifuge retention capacity (CRC) of at least 40 g / g, more preferably at least 41 g / g, and most preferably at least 42 g / g. The centrifuge retention capacity (CRC) of the superabsorbent polymer particles is typically less than 60 g / g.
[0029] The superabsorbent polymer particles produced by the process according to the invention preferably have an absorbent capacity under high load (AUHL) of at least 20 g / g, more preferably at least 22 g / g, and most preferably at least 24 g / g. The absorbent capacity under high load (AUHL) of the superabsorbent polymer particles is typically less than 50 g / g.
[0030] The superabsorbent polymer particles produced by the process according to the present invention preferably have a Yellowness Index (YI) (2 / C) of YI D1925 of 54 or less, more preferably 52 or less, and most preferably 50 or less, after aging for 14 days at 70° C. and 80% relative humidity.
[0031] The preparation of the superabsorbent is described in detail below.
[0032] Superabsorbents are made by polymerizing a monomer solution and are typically water-insoluble.
[0033] Suitable crosslinking agents b) are compounds that have at least two groups suitable for crosslinking.Such groups are, for example, ethylenically unsaturated groups that can be polymerized into polymer chains by free radicals, and functional groups that can form covalent bonds with the acid groups of acrylic acid.In addition, polyvalent metal salts that can form coordinate bonds with at least two acid groups of acrylic acid are also suitable as crosslinking agents b).
[0034] The crosslinking agent b) is preferably a compound having at least two polymerizable groups, which can be polymerized by free radicals into a polymer network.Suitable crosslinking agents b) are, for example, ethylene glycol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, allyl methacrylate, trimethylolpropane triacrylate, triallylamine, tetraallyl ammonium chloride, tetraallyloxyethane, as described in EP 0530438 A1, EP 0547847 A1, EP 0559476 A1, EP 0632068 A1, WO 93 / 21237 A1, WO 2003 / 104299 A, etc. 1, di- and triacrylates, as described in WO 2003 / 104300 A1, WO 2003 / 104301 A1, and DE 10331450 A1, mixed acrylates which contain further ethylenically unsaturated groups in addition to acrylate groups, as described in DE 10331456 A1 and DE 10355401 A1, or mixtures of crosslinkers, as described, for example, in DE 19543368 A1, DE 19646484 A1, WO 90 / 15830 A1, and WO 2002 / 032962 A2.
[0035] Preferred crosslinkers b) are pentaerythrityl triallyl ether, tetraallyloxyethane, methylene bismethacrylamide, 15-tuply ethoxylated trimethylolpropane triacrylate, polyethylene glycol diacrylate, trimethylolpropane triacrylate, and triallylamine.
[0036] Very particularly preferred crosslinkers b) are polyethoxylated and / or propoxylated glycerols which are esterified with acrylic or methacrylic acid to give di- or triacrylates, as described, for example, in WO 2003 / 104301 A1. Di- and / or triacrylates of 3- to 10-tuply ethoxylated glycerol are particularly advantageous. Di- or triacrylates of 1- to 5-tuply ethoxylated and / or propoxylated glycerol are very particularly preferred. Most preferred are triacrylates of 3- to 5-tuply ethoxylated and / or propoxylated glycerol, especially triacrylates of 3-tuply ethoxylated glycerol.
[0037] The amount of crosslinker b) is preferably 0.05 to 1.5% by weight, more preferably 0.1 to 1% by weight, most preferably 0.3 to 0.6% by weight, based on the acrylic acid before neutralization in each case. With increasing crosslinker content, the centrifuge retention capacity (CRC) decreases, reaching 21.0 g / cm 2 The absorbency under pressure passes through a maximum value.
[0038] The initiators c) used may be all compounds which generate free radicals under the polymerization conditions, for example thermal initiators, redox initiators, photoinitiators. Suitable redox initiators are sodium peroxodisulfate / ascorbic acid, hydrogen peroxide / ascorbic acid, sodium peroxodisulfate / sodium bisulfite and hydrogen peroxide / sodium bisulfite. It is preferred to use mixtures of thermal and redox initiators, for example sodium peroxodisulfate / hydrogen peroxide / ascorbic acid. However, the reducing component used is preferably disodium 2-hydroxy-2-sulfonatoacetate or a mixture of disodium 2-hydroxy-2-sulfinatoacetate, disodium 2-hydroxy-2-sulfonatoacetate and sodium bisulfite. Such mixtures are available as Brueggolite® FF6 and Brueggolite® FF7 (Brueggemann Chemicals (Heilbronn; Germany)).
[0039] Typically, an aqueous monomer solution is used. The water content of the monomer solution is preferably 40-75% by weight, more preferably 45-70% by weight, most preferably 50-65% by weight. A monomer suspension, i.e. a monomer solution containing excess sodium acrylate, can also be used. With increasing water content, the energy requirements for subsequent drying increase, and with decreasing water content, the heat of polymerization may be only insufficiently removed.
[0040] For optimal action, the preferred polymerization inhibitors require dissolved oxygen, so the monomer solution may be freed of dissolved oxygen prior to polymerization by inertization, i.e., by flushing with an inert gas, preferably nitrogen or carbon dioxide. The oxygen content of the monomer solution is preferably reduced to less than 1 ppm by weight, more preferably less than 0.5 ppm by weight, and most preferably less than 0.1 ppm by weight prior to polymerization.
[0041] In order to better control the polymerization reaction, any known chelating agent can be optionally added to the monomer solution or suspension or to its raw materials. Suitable chelating agents are, for example, phosphoric acid, diphosphoric acid, triphosphoric acid, polyphosphoric acid, citric acid, tartaric acid, or salts thereof.
[0042] Further suitable examples are iminodiacetic acid, hydroxyethyliminodiacetic acid, nitrilotriacetic acid, nitrilotripropionic acid, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, triethylenetetraaminehexaacetic acid, N,N-bis(2-hydroxyethyl)glycine, and trans-1,2-diaminocyclohexanetetraacetic acid, and salts thereof. The amount used is typically 1 to 30000 ppm, preferably 10 to 1000 ppm, preferentially 20 to 600 ppm, more preferably 50 to 400 ppm, and most preferably 100 to 300 ppm, based on monomer a).
[0043] The monomer solution is polymerized. Suitable reactors are, for example, kneader reactors or belt reactors. In kneaders, the polymer gel formed in the polymerization of aqueous monomer solution or suspension is continuously comminuted by a counter-rotating stirring shaft, for example, as described in WO2001 / 038402A1. Polymerization on a belt is described, for example, in DE3825366A1 and US Pat. No. 6,241,928. Polymerization in a belt reactor forms a polymer gel, which must be comminuted in a further process step, for example, in an extruder or kneader.
[0044] To improve the drying properties, the ground polymer gel obtained by the kneader can be additionally extruded.
[0045] The acid groups of the resulting polymer gel are typically partially neutralized. Neutralization is preferably carried out at the monomer stage. This is typically achieved by mixing in a neutralizing agent, either as an aqueous solution or, preferably, also as a solid. The degree of neutralization is preferably 50-85 mol%, more preferably 60-80 mol%, most preferably 65-75 mol%, and for the neutralization customary neutralizing agents can also be used, preferably alkali metal hydroxides, alkali metal oxides, alkali metal carbonates or alkali metal hydrogen carbonates, and mixtures thereof. Instead of the alkali metal salts, ammonium salts can also be used. Particularly preferred alkali metals are sodium and potassium, but sodium hydroxide, potassium hydroxide, and also mixtures thereof are very particularly preferred.
[0046] The resulting polymer gel is dried. The dryer is not subject to any restrictions. However, the drying of the polymer gel is preferably carried out by a belt dryer until the residual moisture content is preferably 0.5-10% by weight, more preferably 1-7% by weight, and most preferably 2-5% by weight, the residual moisture content being determined by EDANA recommended test method No. WSP230.2(05) "Mass Loss Upon Heating". If the residual moisture content is too high, the dried polymer gel will have a too low glass transition temperature Tg If the residual moisture content is too low, the dried polymer gel will be too brittle and in the subsequent grinding step will undesirably give a large amount of polymer particles with an excessively small particle size (fines). The solids content of the gel before drying is preferably 25-90% by weight, more preferably 35-70% by weight, most preferably 40-60% by weight. However, fluidized bed dryers or paddle dryers may also be used for drying purposes, if desired.
[0047] The dried polymer gel is then crushed and classified. The apparatus used for crushing may typically be a single-stage or multi-stage roll mill, preferably a two-stage or three-stage roll mill, a pin mill, a hammer mill, or a vibrating mill.
[0048] The average particle size of the polymer particles taken as product fraction is preferably at least 200 μm, more preferably between 250 and 600 μm, very particularly between 300 and 500 μm. The average particle size of the product fraction can be determined by EDANA Recommended Test Method No. WSP220.2(05) "Particle Size Distribution", where the percentages by mass of the sieved fractions are plotted in cumulative form and the average particle size is determined graphically. The average particle size here is the mesh size value that gives rise to a cumulative 50% by weight.
[0049] The proportion of particles having a particle size of at least 150 μm is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
[0050] Polymer particles with too small a particle size reduce saline flow conductivity (SFC), so the proportion of excessively small polymer particles ("fines") should be kept low.
[0051] Therefore, excessively small polymer particles are typically removed and recycled into the process, preferably before, during, or immediately after polymerization, i.e., before drying of the polymer gel. The excessively small polymer particles can be moistened with water and / or aqueous surfactants before or during recycling.
[0052] It is also possible to remove the excessively small polymer particles in a later process step, for example after a surface postcrosslinking or another coating step, in which case the recycled excessively small polymer particles are surface postcrosslinked or coated by another method, for example by fumed or precipitated silica.
[0053] When a kneading reactor is used for the polymerization, the excessively small polymer particles are preferably added in the last third of the polymerization.
[0054] If too small polymer particles are added at a very early stage, for example to the monomer solution, this will reduce the centrifuge retention capacity (CRC) of the resulting superabsorbent. However, this can be compensated for, for example, by adjusting the amount of crosslinker b) used.
[0055] If excessively small polymer particles are added at a very late stage, for example not until the equipment connected downstream of the polymerization reactor, for example an extruder, the excessively small polymer particles can be incorporated into the resulting polymer gel, but only with difficulty. However, the insufficiently incorporated excessively small polymer particles are again detached from the dry polymer gel during grinding, and are therefore again taken up in the classification process, increasing the amount of excessively small polymer particles to be recycled.
[0056] The proportion of particles having a particle size of up to 850 μm is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
[0057] The proportion of particles having a particle size of up to 600 μm is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
[0058] Polymer particles with excessively large particle size reduce the free swell rate (FSR), so the proportion of excessively large polymer particles should be kept low as well.
[0059] Therefore, the excessively large polymer particles are typically removed and recycled to the grinding of the dried polymer gel.
[0060] However, it is also possible to form an aqueous monomer solution into droplets and polymerize the resulting droplets in a heated carrier gas stream, where the process steps of polymerization and drying can be combined, as described in WO 2008 / 052971 A1 and WO 2011 / 026876 A1.
[0061] For this purpose, the monomer solution is metered into the reaction chamber by means of at least one hole for forming the droplets, which may for example be in a dropletizing plate.
[0062] A dropletizer plate is a plate with at least one hole through which liquid passes from above. The dropletizer plate or the liquid can be vibrated, which generates chains of ideally monodisperse droplets in each hole on the lower surface of the dropletizer plate. In a preferred embodiment, the dropletizer plate is not rocked.
[0063] The number and size of the holes are selected according to the desired capacity and droplet size. The diameter of the droplets is typically 1.9 times the diameter of the holes. What is important here is that the liquid to be dropletized does not pass through the holes too quickly and that the pressure loss at both ends of the holes is not too large. Otherwise the liquid will not be dropletized, but rather the jet of liquid will break up (atomize) due to the high kinetic energy. The Reynolds number based on the throughput per hole and the diameter of the holes is preferably less than 2000, more preferably less than 1600, particularly preferably less than 1400, and most preferably less than 1200.
[0064] The dropletizing plate preferably has at least 5 holes, more preferably at least 25 holes, and most preferably at least 50 holes, and preferably up to 750 holes, more preferably up to 500 holes, and most preferably up to 250 holes. The diameter of the holes is selected depending on the desired droplet size.
[0065] The diameter of the pores is preferably 50 to 500 μm, more preferably 100 to 300 μm, and most preferably 150 to 250 μm.
[0066] The temperature of the monomer solution when passing through the holes is preferably 5 to 80°C, more preferably 10 to 70°C, and most preferably 30 to 60°C.
[0067] The distance between the holes is preferably 10 to 50 mm, more preferably 12 to 40 mm, most preferably 15 to 30 mm. An excessively short distance will result in the formation of agglomerates.
[0068] Carrier gas flows through the polymerization reactor. This carrier gas can be guided through the reaction chamber in cocurrent or countercurrent, preferably in cocurrent, i.e. from the bottom upwards, with respect to the droplets of the monomer solution that are falling freely. After one pass, the carrier gas is preferably at least partially, preferably to the extent of at least 50%, more preferably to the extent of at least 75%, recycled to the reaction chamber as cycle gas. Typically, a portion of the carrier gas, preferably at most 10%, more preferably at most 3%, most preferably at most 1%, is discharged after each pass.
[0069] The oxygen content of the carrier gas is preferably 0.5 to 15% by volume, more preferably 1 to 10% by volume, and most preferably 2 to 7% by weight.
[0070] In addition to oxygen, the carrier gas preferably contains nitrogen. The nitrogen content of the carrier gas is preferably at least 80% by volume, more preferably at least 90% by volume, and most preferably at least 95% by volume. Further suitable carrier gases are carbon dioxide, argon, xenon, krypton, neon, and helium. Gas mixtures can also be used. The carrier gas can also be loaded with steam and / or acrylic acid vapor.
[0071] The gas velocity is preferably set so that the flow in the polymerization reactor is guided, for example, so that there is no convection current opposite to the overall flow direction, and is typically 0.1 to 2.5 m / sec, preferably 0.3 to 1.5 m / sec, more preferably 0.5 to 1.2 m / sec, particularly preferably 0.6 to 1.0 m / sec, and most preferably 0.7 to 0.9 m / sec.
[0072] The carrier gas flowing through the reactor is suitably preheated to the reaction temperature upstream of the reactor.
[0073] Advantageously, the gas inlet temperature is adjusted so that the gas outlet temperature, i.e. the temperature at which the carrier gas leaves the reaction chamber, is typically 90-150°C, preferably 100-140°C, more preferably 105-135°C, especially preferably 110-130°C, and most preferably 115-125°C.
[0074] The reaction can be carried out under elevated or reduced pressure, preferably under reduced pressure up to 100 mbar relative to ambient pressure.
[0075] The reaction off-gas, i.e. the gas leaving the reaction chamber, can be cooled, for example, in a heat exchanger. This condenses water and unconverted monomers a). The reaction off-gas can then be at least partially reheated and recycled to the reactor as cycle gas. A portion of the reaction off-gas can be discharged and replaced by fresh carrier gas, in which case the water and unconverted monomers a) present in the reaction off-gas can be removed and recycled.
[0076] Particularly preferred is an integrated heating system, which means that some of the waste heat in cooling the off-gas is used to heat the cycle gas.
[0077] The reactor may be trace heated, the trace heating being adjusted to ensure that the wall temperature is at least 5° C. above the internal reactor temperature to prevent condensation on the reactor walls.
[0078] The reaction product is subsequently thermally post-treated and, optionally, dried to the desired moisture content.
[0079] To improve the properties, the polymer particles (base polymer) are subsequently thermally surface crosslinked.Suitable surface crosslinking agents are compounds that contain groups that can form covalent bonds with at least two acid groups of the polymer particles.Suitable compounds are, for example, the polyfunctional amines, polyfunctional amidoamines, polyfunctional epoxides described in EP0083022A2, EP0543303A1 and EP0937736A2, the difunctional or polyfunctional alcohols described in DE3314019A1, DE3523617A1 and EP0450922A2, or the β-hydroxyalkylamides described in DE10204938A1 and US Patent No. 6,239,230.
[0080] Cyclic carbonates in DE 4020780 C1, 2-oxazolidinones and derivatives thereof, such as 2-hydroxyethyl-2-oxazolidinone in DE 19807502 A1, bis- and poly-2-oxazolidinones in DE 19807992 C1, 2-oxotetrahydro-1,3-oxazines and derivatives thereof in DE 19854573 A1, N-acyl-2-oxazolidinones in DE 19854574 A1, cyclic ureas in DE 10204937 A1, bicyclic amide acetals in DE 10334584 A1, oxetanes and cyclic ureas in EP 1199327 A2, and morpholine-2,3-diones and derivatives thereof in WO 2003 / 031482 A1 are additionally described as suitable surface postcrosslinkers.
[0081] Preferred surface postcrosslinkers are ethylene carbonate, ethylene glycol diglycidyl ether, reaction products of polyamides with epichlorohydrin, and mixtures of propylene glycol and 1,4-butanediol.
[0082] Very particularly preferred surface postcrosslinkers are 2-hydroxyethyloxazolidin-2-one, oxazolidin-2-one and 1,3-propanediol.
[0083] In addition, surface postcrosslinkers which contain additional polymerizable ethylenically unsaturated groups, as described in DE 3713601 A1, can also be used.
[0084] The amount of surface postcrosslinker is preferably 0.005 to 5% by weight, more preferably 0.01 to 2% by weight, most preferably 0.015 to 1% by weight, based on the polymer particles in each case.
[0085] In a preferred embodiment of the present invention, polyvalent cations are applied to the particle surface in addition to the surface postcrosslinking agent before, during or after the surface postcrosslinking.
[0086] The polyvalent cations that can be used in the method according to the invention are, for example, divalent cations, such as zinc, magnesium, calcium, iron and strontium cations, trivalent cations, such as aluminum, iron, chromium, rare earth and manganese cations, tetravalent cations, such as titanium and zirconium cations.Possible counterions are chloride, bromide, sulfate, hydrogen sulfide, carbonate, hydrogen carbonate, nitrate, phosphate, hydrogen phosphate, dihydrogen phosphate and carboxylate ions, such as acetate and lactate.Aluminum sulfate and aluminum lactate are preferred.Besides metal salts, polyvalent amines can also be used as polyvalent cations.
[0087] The amount of the polyvalent cation used is, for example, 0.001 to 1.5% by weight, preferably 0.005 to 1% by weight, and more preferably 0.02 to 0.8% by weight, based on the polymer particles.
[0088] Surface postcrosslinking is typically carried out by spraying the solution of surface postcrosslinking agent onto dry polymer particles.After spray application, the polymer particles coated with surface postcrosslinking agent are dried by heat, and surface postcrosslinking reaction can occur either before or during drying.
[0089] The spray application of the solution of the surface postcrosslinker is preferably carried out with a mixer having a moving mixing tool, such as a screw mixer, a disk mixer, and a paddle mixer.Horizontal mixers, such as a paddle mixer, are particularly preferred, and vertical mixers are very particularly preferred.The distinction between horizontal mixers and vertical mixers is made by the position of the mixing shaft, i.e. horizontal mixers have a horizontally mounted mixing shaft, and vertical mixers have a vertically mounted mixing shaft.Suitable mixers are, for example, horizontal Pflugschar® ploughshare mixer (Gebr. Loedige Maschinenbau GmbH; Paderborn; Germany), Vrieco-Nauta continuous mixer (Hosokawa Micron BV; Doetinchem; The Netherlands), Processall Mixmill mixer (Processall Incorporated; Cincinnati; USA), and Schugi Flexomix® (Hosokawa Micron BV; Doetinchem; The Netherlands). However, spraying of the surface postcrosslinker solution can also be carried out in a fluidized bed.
[0090] The surface post-crosslinking agent is typically used in the form of an aqueous solution. The penetration depth of the surface post-crosslinking agent into the polymer particles can be adjusted by the content of the non-aqueous solvent and the total amount of the solvent.
[0091] When using excess water as solvent, it is advantageous to add a surfactant, which improves the wetting behavior and reduces the tendency to form lumps. However, it is preferred to use solvent mixtures, such as isopropanol / water, 1,3-propanediol / water and propylene glycol / water, the mixing ratio by weight being preferably 20:80 to 40:60.
[0092] Surface post-crosslinking by heat is preferably carried out in contact dryer, more preferably in paddle dryer, most preferably in disk dryer.Suitable dryers are, for example, Hosokawa Bepex® Horizontal Paddle Dryer (Hosokawa Micron GmbH; Leingarten; Germany), Hosokawa Bepex® Disc Dryer (Hosokawa Micron GmbH; Leingarten; Germany) and Nara Paddle Dryer (NARA Machinery Europe; Frechen; Germany).Furthermore, fluidized bed dryer can also be used.
[0093] Thermal surface postcrosslinking can also be carried out in the mixer itself by heating the jacket or blowing in warm air.Downflow dryers, such as tray dryers, rotary tube ovens or heatable screws, are also suitable.It is particularly advantageous to carry out mixing and drying in a fluidized bed dryer.
[0094] The surface postcrosslinking temperature is preferably within the range of 110 to 220° C., more preferably 120 to 200° C., and most preferably 130 to 190° C. The residence time of the polymer particles during thermal surface postcrosslinking is preferably 10 to 120 minutes, more preferably 15 to 90 minutes, and most preferably 20 to 60 minutes.
[0095] The surface postcrosslinked polymer particles can then be classified again and the excessively small and / or excessively large polymer particles removed and recycled into the process.
[0096] To further improve the properties, the surface postcrosslinked polymer particles can be coated or remoisturized.
[0097] The remoistening is preferably carried out at 30-80°C, more preferably at 35-70°C, most preferably at 40-60°C. At too low a temperature the superabsorbent tends to form lumps, at high temperatures the water has already evaporated to a visible extent. The amount of water used for the remoistening is preferably 1-15% by weight, more preferably 2-10% by weight, most preferably 3-5% by weight, based on the polymer particles. Remoistening increases the mechanical stability of the polymer particles and reduces their tendency to become electrostatically charged.
[0098] Suitable coatings for improving the free swell rate and saline flow conductivity (SFC) are, for example, inorganic inert substances, such as water-insoluble metal salts, organic polymers, cationic polymers, and divalent or polyvalent metal cations. Suitable coatings for binding dust are, for example, polyols. Suitable coatings for suppressing the undesirable caking tendency of polymer particles are, for example, fumed silica, such as Aerosil® 200, or precipitated silica, such as Sipernat® D17, and surfactants, such as Span® 20.
[0099] method Measurements shall be made at an ambient temperature of 23±2°C and a relative atmospheric humidity of 50±10%, unless otherwise specified. The superabsorbent polymer is thoroughly mixed prior to the measurements.
[0100] Residual Monomer (RAA) Residual monomers in superabsorbent polymer particles are determined by EDANA Recommended Test Method No. WSP210.2(04) "Determination of the Amount of Residual Monomers in Superabsorbent Materials."
[0101] Particle Size Distribution The particle size distribution of the superabsorbent polymer particles is determined by EDANA Recommended Test Method No. WSP220.2(05) "Determination of Polyacrylate Superabsorbent Powders and Particle Size Distribution - Sieve Fractionation."
[0102] Circularity Circularity is determined by a PartAn® 3001 L Particle Analysator (Microtrac Europe GmbH; Meerbusch; Germany).
[0103]
number
[0104] For the measurement, the superabsorbent polymer particles are introduced through a funnel and transported to a drop shaft with a measurement channel. The particles are selectively recorded by a camera while they fall through an illuminated wall. The recorded images are evaluated by software according to the selected parameters.
[0105] Moisture content (MC) The moisture content of superabsorbent polymer particles is determined by EDANA Recommended Test Method No. WSP230.2(05) "Moisture Content - Weight Loss Upon Heating."
[0106] Centrifuge retention capacity (CRC) The centrifuge retention capacity of superabsorbent polymer particles is determined by EDANA Recommended Test Method No. WSP241.2(05) "Gravimetric Determination of Fluid Retention Capacity in Saline Solution After Centrifugation", for larger centrifuge retention capacity values, larger tea bags should be used.
[0107] Absorption capacity under load (AUL) The absorbency under load of superabsorbent polymer particles is determined by EDANA Recommended Test Method No. WSP242.2(05) "Gravimetric Determination of Absorption Under Pressure."
[0108] Absorbency under high load (AUHL) The absorbency of the superabsorbent polymer particles under high load is 21.0 g / cm 2 Weight instead of 49.2g / cm 2 The determination is made in the same manner as EDANA Recommended Test Method No. WSP242.2(05) “Gravimetric Determination of Absorption Under Pressure”, except that the weight of the specimen is used.
[0109] flow rate The flow rate of superabsorbent polymer particles is determined by EDANA Recommended Test Method No. WSP250.2(05) "Gravimetric Determination of Flowrate."
[0110] Bulk Density The bulk density of the superabsorbent polymer particles is determined by EDANA Recommended Test Method No. WSP260.2(05), "Gravimetric Determination of Density."
[0111] Extractables (Ext.16h) The content of extractable components in superabsorbent polymer particles is determined by EDANA Recommended Test Method No. WSP270.2(05) "Determination of Extractable Polymer Content by Potentiometric Titration."
[0112] Caking (40℃ / 80% relative humidity / 1 hour) 5g of superabsorbent polymer particles is placed in an aluminum weighing dish (57mm x 15mm) and stored at 40°C and 80% relative humidity for 1 hour. The sample is cooled to ambient temperature and weighed. After sieving through a 1.68mm sieve (ASTM No.12, sieve diameter greater than 57mm and less than 100mm), the amount that passes through the sieve is weighed to determine the mass of non-caking polymer particles. The sieving process is as follows:
[0113] Carefully take the aluminum dish containing the hydrated polymer and hold it vertically with one hand. Invert the sieve pan assembly on the dish and gently invert the sieve, pan, and weighing dish containing the polymer in one continuous motion so that the dish is inverted on the sieve mesh. Place a lid on the sieve mesh containing the aluminum weighing dish and place the assembly on a sieve shaker. Vibrate the sieve assembly for 1 minute with a Retsch® Vibratory Sieve Shaker AS 200 control at an amplitude of 0.20 mm.
[0114] The percentage of non-caking particles is then calculated using the following formula:
[0115]
number
[0116] Color value (CIE color number [L,a,b]) The measurement of color values is carried out by a colorimeter model "LabScan XE Spectrometer" (HunterLab; Reston; USA) according to the CIELAB procedure (Hunterlab, Vol. 8, 1996, No. 7, pp. 1-4). Colors are described by the coordinates L, a, and b in a three-dimensional system. L describes the lightness, L=0 is black and L=100 is white. The a and b values describe the position of the color on the red / green and yellow / blue color axes, respectively, with positive a values representing red, negative a values representing green, positive b values representing yellow, and negative b values representing blue.
[0117] Yellowness Index (YI) (2 / C) of YI D1925 is measured according to ASTM D-1925, 2 degrees / lll.°C. The higher the value, the darker and more yellow the color is.
[0118] Tests were performed using tissue culture dishes (35 mm diameter and 10 mm height) and a 0.5 inch port plate opening.
[0119] The measurement of the colour values follows the tristimulus method according to DIN 5033-6. EXAMPLES
[0120] Example 1 (Base Polymer) This example was carried out similarly to Example 1 of WO2016 / 134905A1.
[0121] The process was carried out in a simultaneous spray drying plant with an integrated fluidized bed (27) as shown in Figure 1 of WO2016 / 134905A1. The reaction zone (5) had a height of 22 m and a diameter of 3.4 m. The internal fluidized bed (IFB) had a diameter of 3 m and a weir height of 0.25 m.
[0122] Drying gas was fed through a gas distributor (3) at the top of the spray dryer. It was partially recycled (drying gas loop) via a cyclone as dust separation unit (9) and a condensation tower (12). The drying gas was nitrogen containing 1% to 4% by volume of residual oxygen. Before starting the polymerization, the drying gas loop was filled with nitrogen until the residual oxygen was below 4% by volume. The gas velocity of the drying gas in the reaction zone (5) was 0.79 m / s. The pressure inside the spray dryer was 4 mbar below ambient pressure.
[0123] The temperature of the gas leaving the reaction zone (5) was measured at three points around the circumference of the end of the cylindrical section of the spray dryer as shown in Figure 3 of WO2016 / 134905A1. The three individual measurements (43) were used to calculate the average temperature (spray dryer outlet temperature). The drying gas loop is heated and the addition of the monomer solution is started. From this point on, the spray dryer outlet temperature was controlled at 114°C by adjusting the gas inlet temperature through the heat exchanger (20). The gas inlet temperature was 167°C.
[0124] The product accumulated in the internal fluidized bed (27) reached the weir height. A conditioned internal fluidized bed gas having a temperature of 105° C. was fed to the internal fluidized bed (27) through the line (25). The gas velocity of the internal fluidized bed gas in the internal fluidized bed (27) was 0.65 m / s. The residence time of the product was 150 minutes. The temperature of the superabsorbent polymer particles in the internal fluidized bed (27) was 71° C.
[0125] The spray dryer exhaust gas was filtered in a cyclone as dust separation unit (9) and sent to a condensation tower (12) for quenching / cooling. Excess water was pumped out of the condensation tower (12) by controlling a (constant) filling level in the condensation tower (12). The water in the condensation tower (12) was cooled by a heat exchanger (13) and pumped countercurrent to the gas. To wash out the acrylic acid vapors, the water in the condensation tower (12) was brought to an alkaline pH by adding sodium hydroxide solution.
[0126] The gas leaving the condensation tower (12) was split into the drying gas inlet pipe (1) and the conditioned internal fluidized bed gas (25). The gas temperature was controlled by heat exchangers (20) and (22). The hot drying gas was fed to the simultaneous spray dryer through the gas distributor (3). The gas distributor (3) consists of a series of plates and provides a pressure drop of 2-4 mbar depending on the amount of drying gas.
[0127] The product was discharged from the internal fluidized bed (27) via a rotary valve (28) onto a sieve (29) which was used to screen out the overs / lumps having a particle diameter of more than 800 μm.
[0128] A monomer solution was prepared by first mixing acrylic acid with 3 times ethoxylated glycerol triacrylate (internal crosslinker), secondly with a 37.3 wt.% sodium acrylate solution, and thirdly with an aqueous solution of the disodium salt of 1-hydroxyethane-1,1-diphosphonic acid (HDPA). The temperature of the resulting monomer solution was controlled at 10° C. by using a heat exchanger and by pumping in a loop. In a loop after the pump, a filter unit with a mesh size of 250 μm was used. The initiator was metered into the monomer solution upstream of the dropper by static mixers (31) and (32) via lines (33) and (34), as shown in FIG. 1 of WO2016 / 134905A1. Sodium peroxodisulfate solution having a temperature of 20° C. was added via line (33) together with [2,2′-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride solution via line (34). Each initiator was pumped in a loop and added to each dropletization unit via a control valve. After the static mixer (32), a second filter unit with a mesh size of 140 μm was used. To add the monomer solution to the top of the spray dryer, three dropletization units were used, as shown in FIG. 4 of WO2016 / 134905A1.
[0129] As shown in FIG. 5 of WO2016 / 134905A1, the dropletization unit consisted of an outer pipe (47) with an opening into a dropletization cassette (49). The dropletization cassette (49) was connected to an inner pipe (48). The inner pipe (48), which terminated with a PTFE block (50) as a sealing, could be pushed in and out of the outer pipe (47) during operation of the process for maintenance purposes.
[0130] The dropwise cassette (49) had 256 perforations with a diameter of 170 μm and a perforation spacing of 15 mm. The dropwise cassette (49) consisted of a flow path (56) with no stagnation volume, essential for uniform distribution of the premixed monomer and initiator solutions, and one dropwise plate (53). The dropwise plate (53) had a tilted configuration with an angle of 3°. The dropwise plate (53) was made of stainless steel and had a length of 630 mm, a width of 128 mm, and a thickness of 1 mm.
[0131] The feed to the spray dryer consisted of 10.45% by weight of acrylic acid, 33.40% by weight of sodium acrylate, 0.018% by weight of 3 times ethoxylated glycerol triacrylate, 0.108% by weight of the disodium salt of 1-hydroxyethane-1,1-diphosphonic acid (HDPA), 0.072% by weight of [2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 0.072% by weight of a sodium peroxodisulfate solution (15% by weight in water), and water. The degree of neutralization was 71%. The feed per hole was 1.4 kg / h.
[0132] The resulting superabsorbent polymer particles were analyzed. The conditions and results are summarized in Tables 1-3.
[0133] Example 2 (not the present invention) 1200g of water-absorbing polymer particles (base polymer) prepared in Example 1 was placed in a laboratory plowshare mixer (model MR5, manufactured by Gebrueder Loedige Maschinenbau GmbH, Paderborn, Germany). A surface postcrosslinker solution was prepared in a beaker by mixing 30g of ethylene carbonate, 1.2g of aluminum sulfate, and 60g of deionized water, as described in Table 4. At a mixer speed of 200 rpm, the aqueous solution was sprayed onto the polymer particles by a spray nozzle within 1 minute. Mixing was continued for an additional 5 minutes. The product was removed and transferred to another plowshare mixer (model MR5, manufactured by Gebrueder Loedige Maschinenbau GmbH, Paderborn, Germany) that had been preheated to 150°C. After mixing for another 40 minutes at 150°C, the product was removed from the mixer and sieved through a 850 μm sieve.
[0134] A rewetting solution was prepared in a beaker by mixing 3 g of aluminum lactate, 25 mg of sorbitan monododecanoate (Span® 20), and 80 g of deionized water, as described in Table 8. 1000 g of this product was transferred to another ploughshare mixer (model MR5, manufactured by Gebrueder Loedige Maschinenbau GmbH, Paderborn, Germany) that was preheated to 80° C. After reaching a final temperature of 80° C., the heat of the ploughshare mixer was turned off and the aqueous rewetting solution was sprayed onto the polymer particles by a spray nozzle within 2 minutes at a mixer speed of 200 rpm. Mixing was continued for an additional 13 minutes. The product was removed and sieved through an 850 μm sieve.
[0135] The samples were analyzed and the formulations, conditions and results are summarized in Tables 4 and 5.
[0136] Example 3 (invention) This example was carried out similarly to Example 2, except that an additional 0.18 g of hydrogen peroxide was added to the surface postcrosslinker solution.
[0137] Example 4 (Invention) This example was run similarly to Example 2, except that an additional 0.36 g of hydrogen peroxide was added to the surface postcrosslinker solution.
[0138] Example 5 (Invention) This example was run similarly to Example 2, except that an additional 0.72 g of hydrogen peroxide was added to the surface postcrosslinker solution.
[0139] Example 6 (Invention) This example was run similarly to Example 2, except that an additional 1.08 g of hydrogen peroxide was added to the surface postcrosslinker solution.
[0140] Example 7 (not the present invention) This example was run similarly to Example 2, except that an additional 1.80 g of hydrogen peroxide was added to the surface postcrosslinker solution.
[0141] Example 8 (not of the present invention) This example was run similarly to Example 2, except that an additional 3.60 g of hydrogen peroxide was added to the surface postcrosslinker solution.
[0142] Example 9 (not the present invention) This example was carried out similarly to Example 2, except that an additional 0.18 g of sodium persulfate was added to the surface postcrosslinker solution.
[0143] Example 10 (not the present invention) This example was carried out similarly to Example 2, except that an additional 0.36 g of sodium persulfate was added to the surface postcrosslinker solution.
[0144] Example 11 (not the present invention) This example was carried out similarly to Example 2, except that an additional 0.72 g of sodium persulfate was added to the surface postcrosslinker solution.
[0145] Example 12 (not of the present invention) This example was run similarly to Example 2, except that an additional 0.15 g of hydrogen peroxide was added to the rewet solution.
[0146] Example 13 (not of the present invention) This example was run similarly to Example 2, except that an additional 0.30 g of hydrogen peroxide was added to the rewet solution.
[0147] Example 14 (not of the present invention) This example was run similarly to Example 2, except that an additional 0.60 g of hydrogen peroxide was added to the rewet solution.
[0148] [Table 1]
[0149] [Table 2]
[0150] [Table 3]
[0151] [Table 4]
[0152] [Table 5]
[0153] FIG. 1 shows the yellowness index (YI D1925) after storage for 14 days in a weathering cabinet at 70° C. and 80% relative humidity, depending on the hydrogen peroxide content in the surface postcrosslinker solution (Examples 2-8).
[0154] FIG. 2 shows the absorbency under high load (AUHL) depending on the hydrogen peroxide content in the surface postcrosslinker solution (Examples 2-8).
Claims
1. 1. A method for producing long-term color stable superabsorbent polymer particles, comprising: a) partially neutralized acrylic acid; b) optionally, at least one crosslinker, and c) at least one initiator polymerizing a monomer solution comprising: drying the resulting polymer gel; optionally grinding and classifying the resulting dried polymer gel; and thermally post-crosslinking the resulting polymer particles and cooling, A process in which a thermal post-crosslinking agent and 0.014 to 0.095% by weight of hydrogen peroxide, based on the polymer particles, are added to the polymer particles prior to thermal post-crosslinking.
2. 2. The method according to claim 1, wherein 0.005 to 5% by weight, based on the polymer particles, of a thermal postcrosslinker is added to the polymer particles before postcrosslinking.
3. 3. The process according to claim 1, wherein 0.02 to 0.05% by weight, based on the polymer particles, of peroxide is added to the polymer particles before post-crosslinking.
4. 4. The process according to claim 1, wherein the post-crosslinking temperature is from 130 to 190° C.
5. 5. The process according to claim 1, wherein the residence time of the postcrosslinking is from 20 to 60 minutes.
6. The method of claim 1 , wherein the monomer solution comprises a polymerization inhibitor.
7. 7. The method according to claim 1, wherein the monomer solution comprises 0.004 to 0.010% by weight of a polymerization inhibitor, based on acrylic acid.
8. 8. The method according to claim 6 or 7, wherein hydroquinone monomethyl ether is used as the polymerization inhibitor.
9. 9. The method of claim 1, wherein at least one chelating agent is added to the polymer particles during or after cooling.
10. 10. The method according to any one of claims 1 to 9, wherein 0.005 to 1% by weight, based on the polymer particles, of at least one chelating agent is added to the polymer particles during or after cooling.
11. The method according to claim 9 or 10, wherein 1-hydroxyethane-1,1-diphosphonic acid and / or a salt thereof is used as a chelating agent.
12. The method according to claim 1 , wherein the post-crosslinking step is substantially free of irradiation with active energy rays.
13. 13. Superabsorbent polymer particles obtainable by the method according to any one of claims 1 to 12, having a centrifuge retention capacity of at least 40 g / g and an absorbent capacity under high load of at least 20 g / g.
14. 14. The superabsorbent polymer particles of claim 13, having a Yellowness Index of 54 or less after aging for 14 days at 70°C and 80% relative humidity.
15. 15. Superabsorbent polymer particles according to claim 13 or 14, having a yellowness index of 50 or less after aging for 14 days at 70°C and 80% relative humidity.
Citation Information
Patent Citations
Manufacturing method of high whiteness water absorption resin
CN101045789A
Method for producing particle-formed water-absorbing agent, and particle-formed water-absorbing agent
JP2007119757A
Particulate water-absorbing agent mainly composed of polyacrylic acid (salt)-based water-absorbing resin, method for producing the same, absorbent body and absorbent article using this particulate water-absorbing agent
JP2008535640A
Classification method for superabsorbent polymer particles
JP2010504211A
Method for producing superabsorbent polymer particles
JP2013520539A