Photosensitive resin composition, cured product, and semiconductor element
The photosensitive resin composition, with specific components, addresses the need for flexible and dielectric insulating films in semiconductor devices by enhancing elongation and microprocessability, suitable for semiconductor elements with improved rewiring layers.
Patent Information
- Application Number
- JP2023060587
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-17
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Photosensitive resin compositions used to form insulating films in semiconductor devices require improved flexibility (elongation) while maintaining sufficient microprocessability and dielectric properties.
A photosensitive resin composition containing a maleimide compound, crosslinking agent, and photopolymerization initiator, with specific components like tetracarboxylic dianhydride, amine, and polymerizable crosslinking agents with allyl groups, to enhance flexibility and dielectric properties.
The composition forms insulating films with high elongation rates and maintains microfabricability, providing semiconductor elements with improved rewiring layers.
Smart Images

Figure 2024147881000001 
Figure 2024147881000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a photosensitive resin composition, a cured product, and a semiconductor device. [Background technology]
[0002] With the high integration, miniaturization, and miniaturization of semiconductor elements, insulating films used in surface protection layers, interlayer insulating layers, rewiring layers, etc. of semiconductor elements are required to have better electrical properties, heat resistance, mechanical properties, etc. As a material for forming an insulating film having such properties, a photosensitive resin composition containing an alkali-soluble resin has been developed (see, for example, Patent Documents 1, 2, and 3). These photosensitive resin compositions are applied to a substrate and dried to form a resin film, and the resin film is exposed to light and developed to obtain a patterned resin film (a resin film having a pattern). The patterned resin film is then heated and cured to form a patterned cured film (a cured film having a pattern), and the patterned cured film can be used as an insulating film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2008-309885 A [Patent Document 2] JP 2007-057595 A [Patent Document 3] International Publication No. 2010 / 073948 Summary of the Invention [Problem to be solved by the invention]
[0004] Photosensitive resin compositions for forming insulating films such as redistribution layers are required to have high flexibility (elongation in particular) while maintaining sufficient micro-processability and dielectric properties. Therefore, the present disclosure aims to provide a photosensitive resin composition capable of forming an insulating film having a high elongation while maintaining sufficient micro-processability and dielectric properties. [Means for solving the problem]
[0005] One aspect of the present disclosure relates to the following photosensitive resin composition, cured product, and semiconductor element. [1] A photosensitive resin composition comprising a maleimide compound, a crosslinking agent, and a photopolymerization initiator, wherein the maleimide compound is a reaction product of a tetracarboxylic dianhydride, an amine, and maleic anhydride, the amine includes a dimer diamine and a second amine other than the dimer diamine, and the crosslinking agent includes a polymerizable crosslinking agent having an allyl group. [2] The photosensitive resin composition according to the above [1], wherein the tetracarboxylic dianhydride comprises at least one selected from the group consisting of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride, 4,4'-oxydiphthalic anhydride, 1,2,3,4-butanetetracarboxylic dianhydride, and 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-C]furan-1,3-dione. [3] The photosensitive resin composition according to the above [1] or [2], wherein the second amine comprises at least one selected from the group consisting of metaxylylenediamine, 4,4'-diaminodiphenylmethane, 1,3-diaminopropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and norbornanediamine. [4] The photosensitive resin composition according to any one of the above [1] to [3], wherein the polymerizable crosslinking agent having an allyl group includes at least one selected from the group consisting of 1,3,4,6-tetraallyl glycol uril, triallyl isocyanurate, and diallyl isocyanurate. [5] The photosensitive resin composition according to any one of the above [1] to [4], wherein the crosslinking agent further comprises a polymerizable crosslinking agent having a (meth)acryloyl group. [6] The photosensitive resin composition according to any one of the above [1] to [5], further comprising a thermal polymerization initiator. [7] A cured product of the photosensitive resin composition according to any one of [1] to [6] above. [8] A semiconductor device having a rewiring layer comprising a cured product of the photosensitive resin composition according to any one of [1] to [6] above. Effect of the Invention
[0006] According to the present disclosure, it is possible to provide a photosensitive resin composition capable of forming an insulating film having a high elongation rate while sufficiently maintaining fine processability and dielectric properties, a cured product of the photosensitive resin composition having low dielectric properties, and a semiconductor element having a redistribution layer including the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Preferred embodiments of the present disclosure will be described in detail below. However, the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0008] In this specification, a numerical range indicated using "~" indicates a range including the numerical values described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of a numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. "A or B" may include either A or B, or may include both. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more types. The content of each component in the composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified.
[0009] In this specification, the terms "layer" and "film" include structures that are formed over the entire surface as well as structures that are formed only partially when observed in a plan view. The term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0010] In this specification, "(meth)acryloyl" means at least one of "acryloyl" and the corresponding "methacryloyl", and the same applies to other similar expressions such as (meth)acrylic acid, (meth)acrylate, etc. In this specification, "solid content" refers to the non-volatile content excluding volatile substances (water, solvent, etc.) contained in the photosensitive resin composition, and also includes components that are liquid, syrup-like, or wax-like at room temperature (around 25°C).
[0011] [Photosensitive resin composition] The photosensitive resin composition according to the present embodiment contains, as essential components, a maleimide compound, a crosslinking agent, and a photopolymerization initiator. The maleimide compound is a reaction product of a tetracarboxylic dianhydride, an amine, and maleic anhydride. The amine contains a dimer diamine and a second amine other than the dimer diamine. The crosslinking agent contains a polymerizable crosslinking agent having an allyl group.
[0012] The photosensitive resin composition according to the present embodiment may further contain a thermal polymerization initiator, a coupling agent, a rust inhibitor, a polymerization inhibitor, etc., as necessary. The photosensitive resin composition according to the present embodiment is a negative photosensitive resin composition, and the cured product of the photosensitive resin composition can be suitably used as an insulating film for a rewiring layer. Hereinafter, each component used in the photosensitive resin composition according to the present embodiment will be described in more detail.
[0013] (Maleimide compounds) The maleimide compound according to this embodiment (hereinafter also referred to as "component (A)") is a reaction product of a tetracarboxylic dianhydride (a1) (hereinafter also referred to as "component (a1)"), an amine (a2) (hereinafter also referred to as "component (a2)"), and maleic anhydride (a3) (hereinafter also referred to as "component (a3)"). That is, the component (A) is a maleimide compound obtained by reacting the components (a1), (a2), and (a3).
[0014] Examples of the component (a1) include pyromellitic anhydride, 4,4'-oxydiphthalic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 1,2,3,4-butanetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride, 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-C]furan-1,3-dione, bis(1,3-dioxo-1,3-dihydro ...hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-C]furan-1,3-dione, bis(1,3-dioxo Benzofuran-5-carboxylic acid)1,4-phenylene, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, 4,4'-(ethyne-1,2-diyl)diphthalic anhydride, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, 3,4'-oxydiphthalic anhydride, and 3,4'-biphthalic anhydride can be used. The (a1) component may be used alone or in combination of two or more.
[0015] From the viewpoint of low dielectric properties, the (a1) component may include at least one selected from the group consisting of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (BPADA), 4,4'-oxydiphthalic anhydride (ODPA), and 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-C]furan-1,3-dione (TDA), and from the viewpoints of dielectric properties, fine processability, and heat resistance, it may include TDA.
[0016] The (a2) component contains a dimer diamine (first amine) and a second amine other than the dimer diamine. By using the dimer diamine as the (a2) component, a cured product with excellent dielectric properties can be obtained. On the other hand, when only the dimer diamine is used as the (a2) component, the elastic modulus and Tg of the cured product are decreased. In contrast, by using the second amine in combination with the dimer diamine, the elastic modulus and Tg of the cured product can be improved.
[0017] As described in JP-A-9-12712, for example, dimer diamine is a compound derived from a dimer acid, which is a dimer of an unsaturated fatty acid such as oleic acid. In this embodiment, any known dimer diamine can be used without any particular limitation. The dimer diamine may be a branched aliphatic diamine.
[0018] As the dimer diamine, a diamine represented by the following formula (1) may be used. [ka]
[0019] In formula (1), R 2 and R 3 each independently represents an alkylene group having 4 to 50 carbon atoms; R 4 represents an alkyl group having 4 to 50 carbon atoms, and R 5 represents an alkyl group having 2 to 50 carbon atoms.
[0020] From the viewpoint of improving flexibility and ease of synthesis, R 2 and R 3 are each independently preferably an alkylene group having 5 to 25 carbon atoms, more preferably an alkylene group having 6 to 10 carbon atoms, and further preferably an alkylene group having 7 to 10 carbon atoms. From the same viewpoint, R 4 is preferably an alkyl group having 5 to 25 carbon atoms, more preferably an alkyl group having 6 to 10 carbon atoms, and further preferably an alkyl group having 7 to 10 carbon atoms. 5is preferably an alkyl group having 3 to 25 carbon atoms, more preferably an alkyl group having 4 to 10 carbon atoms, and further preferably an alkyl group having 5 to 8 carbon atoms.
[0021] Commercially available dimer diamines include, for example, PRIAMINE 1075 and PRIAMINE 1074 (both manufactured by Croda Japan Ltd.).
[0022] The second amine is an amine that does not fall under the above-mentioned dimer diamine. The second amine may be a diamine or a linear diamine. The second amine may be used alone or in combination of two or more.
[0023] Examples of the second amine include 1,3-diaminopropane, norbornane diamine, metaxylylene diamine, 4,4'-diaminodiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(aminomethyl)norbornane, 4,4'-(hexafluoroisopropylidene)dianiline, 3(4),8(9)-bis(aminomethyl)tricyclohexane, [5.2.1.02,6] Decane, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), 4,4'-ethylenedianiline, 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2-ethyl-6-methylaniline), 2,2'-dimethylbenzidine, 4,4'-diaminodiphenyl ether, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 1,3'-bis(3-aminophenoxy)benzene, and 1,4'-bis(4-aminophenoxy)benzene.
[0024] From the viewpoint of improving the glass transition temperature (Tg) of the cured product, the second amine may include at least one selected from the group consisting of norbornanediamine, metaxylylenediamine, 4,4'-diaminodiphenylmethane, and 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and from the viewpoints of dielectric properties, fine processability, and heat resistance, the second amine may include norbornanediamine.
[0025] In component (a2), the molar ratio of the second amine (moles of second amine / (moles of dimer diamine+moles of second amine)) may be 5 to 90 mol%, 10 to 85 mol%, 20 to 80 mol%, 25 to 75 mol%, 30 to 70 mol%, or 30 to 50 mol%. When this ratio is 5 mol% or more, the elastic modulus and Tg of the cured product are easily increased, and when it is 90 mol% or less, a cured product with lower dielectric properties can be formed.
[0026] The method for producing component (A) is not limited. Component (A) may be produced, for example, by reacting components (a1) and (a2) to synthesize an amine-terminated compound, and then reacting the amine-terminated compound with an excess of component (a3).
[0027] The (A) component can be produced by various known methods. For example, first, the (a1) component and the (a2) component are polyaddition reacted at about 60 to 120°C, preferably 70 to 90°C, for about 0.1 to 2 hours, preferably 0.1 to 1.0 hours. The resulting polyaddition product is then subjected to an imidization reaction, i.e., a dehydration ring-closing reaction, at about 80 to 250°C, preferably 100 to 200°C, for about 0.5 to 30 hours, preferably 0.5 to 10 hours. The product obtained by the dehydration ring-closing reaction is then subjected to a maleimidization reaction, i.e., a dehydration ring-closing reaction, with the (a3) component at about 60 to 250°C, preferably 80 to 200°C, for about 0.5 to 30 hours, preferably 0.5 to 10 hours, to obtain the desired (A) component.
[0028] In the imidization reaction or maleimidization reaction, various known reaction catalysts, dehydrating agents, and organic solvents can be used.
[0029] Examples of the reaction catalyst include aliphatic tertiary amines such as triethylamine, aromatic tertiary amines such as dimethylaniline, heterocyclic tertiary amines such as pyridine, picoline, isoquinoline, and organic acids such as methanesulfonic acid and paratoluenesulfonic acid monohydrate. The reaction catalyst can be used alone or in combination of two or more. Examples of the dehydrating agent include aliphatic acid anhydrides such as acetic anhydride, and aromatic acid anhydrides such as benzoic anhydride.
[0030] Examples of organic solvents include aromatic hydrocarbons such as benzene, toluene, xylene, and mesitylene; alcohol-based solvents such as methanol, ethanol, isopropyl alcohol, butanol, pentanol, hexanol, propanediol, and phenol; ketone-based solvents such as acetone, methyl isobutyl ketone, methyl ethyl ketone, pentanone, hexanone, cyclopentanone, cyclohexanone, isophorone, and acetophenone; cellosolves such as methyl cellosolve and ethyl cellosolve, ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl propionate, and butyl formate; and ethylene glycol mono-n n-butyl ether, ethylene glycol mono-iso-butyl ether, ethylene glycol mono-tert-butyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-iso-butyl ether, triethylene glycol mono-n-butyl ether, tetraethylene glycol mono-n-butyl ether, and other glycol ether-based solvents; and N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, and other nitrogen-containing compounds. The organic solvents can be used alone or in combination of two or more.
[0031] The component (A) can be purified by various known methods to increase its purity. For example, first, the component (A) dissolved in an organic solvent and pure water are placed in a separatory funnel. The separatory funnel is then shaken and allowed to stand. After the aqueous layer and the organic layer are separated, only the organic layer is collected to purify the component (A).
[0032] The molecular weight of the (A) component can be controlled by the number of moles of the (a1) component and the (a2) component, and the smaller the number of moles of the (a1) component is compared with the number of moles of the (a2) component, the smaller the molecular weight can be. For the purpose of easily achieving the effects of the present disclosure, the ratio of [the number of moles of the (a1) component] / [the number of moles of the (a2) component] is usually in the range of about 0.30 to 0.85, preferably 0.50 to 0.80.
[0033] From the viewpoints of solubility in solvents and heat resistance, the molecular weight of the component (A) may be a weight average molecular weight (Mw) of 3,000 to 100,000, 4,000 to 80,000, 5,000 to 60,000, 6,000 to 40,000, or 7,000 to 20,000. Mw can be measured by gel permeation chromatography (GPC) and converted using a calibration curve of standard polystyrene.
[0034] (Crosslinking agent) The resin composition according to the present embodiment contains a polymerizable crosslinking agent having an allyl group as a crosslinking agent (hereinafter also referred to as "component (B)") from the viewpoint of flexibility and heat resistance. The component (B) can crosslink not only with itself but also with the component (A) during exposure of the photosensitive layer, for example. In addition, the crosslinking agent can crosslink with itself during heating of the resin film after pattern formation, for example. The polymerizable crosslinking agent having an allyl group can crosslink with itself during heating of the resin film after pattern formation, for example.
[0035] The polymerizable crosslinking agent having an allyl group may be, for example, a compound having two or more allyl groups. The number of allyl groups may be 2 to 8, 2 to 6, 2 to 4, or 3 to 4.
[0036] Examples of polymerizable crosslinking agents having an allyl group include 1,3,4,6-tetraallyl glycoluril, triallyl isocyanurate, diallyl monoglycidyl isocyanurate, diallyl monomethyl isocyanurate, diallyl isocyanurate, triallyl trimellitate, and triallyl orthoformate.
[0037] From the viewpoint of further increasing the elongation of the cured product of the photosensitive resin composition, the polymerizable crosslinking agent having an allyl group may contain at least one selected from the group consisting of 1,3,4,6-tetraallyl glycol uril, triallyl isocyanurate, and diallyl isocyanurate.
[0038] From the viewpoint of fine processing, the (B) component may further contain a polymerizable crosslinking agent having a (meth)acryloyl group as a crosslinking agent. The polymerizable crosslinking agent having a (meth)acryloyl group can crosslink not only with itself but also with the (A) component, for example, during exposure of the photosensitive layer. The polymerizable crosslinking agent having a (meth)acryloyl group may be an acrylate compound or a methacrylate compound. From the viewpoint of dielectric properties, the (B) component may contain a methacrylate compound.
[0039] Examples of polymerizable crosslinking agents having a (meth)acryloyl group include tricyclodecane dimethanol di(meth)acrylate, tris-(2-(meth)acryloyloxyethyl)isocyanurate, dioxane glycol di(meth)acrylate, pentaerythritol tetra(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, propoxylated ethoxylated bisphenol A (meth)acrylate, dipentaerythritol poly(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, and polyethylene glycol di(meth)acrylate.
[0040] The polymerizable crosslinking agent having a (meth)acryloyl group may contain at least one selected from the group consisting of tricyclodecane dimethanol di(meth)acrylate, tris-(2-(meth)acryloyloxyethyl)isocyanurate, and dioxane glycol di(meth)acrylate, from the viewpoints of heat resistance, dielectric properties, and fine processability, and may contain tris-(2-(meth)acryloyloxyethyl)isocyanurate from the viewpoints of heat resistance and dielectric properties.
[0041] From the viewpoint of further improving the balance between low dielectric properties and fine processability, the content of the (B) component is preferably less than 50 parts by mass, and may be 1 to 45 parts by mass, 5 to 40 parts by mass, 8 to 30 parts by mass, or 10 to 20 parts by mass, when the total amount of the (A) component and the (B) component is 100 parts by mass.
[0042] (Photopolymerization initiator) The photopolymerization initiator (hereinafter also referred to as "component (C)") is not particularly limited as long as it is a compound that initiates polymerization upon irradiation with actinic rays (ultraviolet rays, etc.); examples of the photopolymerization initiator include alkylphenone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, intramolecular hydrogen abstraction photopolymerization initiators, and oxime ester-based photopolymerization initiators.
[0043] Alkylphenone-based photopolymerization initiators can be purchased, for example, from IGM Resins BV under the names Omnirad 651, Omnirad 184, Omnirad 1173, Omnirad 2959, Omnirad 127, Omnirad 907, Omnirad 369, and Omnirad 379EG. Acylphosphine oxide-based photopolymerization initiators can be purchased, for example, from IGM Resins BV under the names Omnirad 819 and Omnirad TPO H. Intramolecular hydrogen abstraction photopolymerization initiators can be purchased, for example, from IGM Resins BV under the names Omnirad MBF and Omnirad 754. Oxime ester-based photopolymerization initiators can be purchased, for example, from BASF Japan Ltd. under the names Irgacure OXE01 and Irgacure OXE02. In order to promote the photoreaction, a titanocene-based photopolymerization initiator (for example, Irgacure 784 manufactured by BASF Japan Ltd.) may be used in combination.
[0044] The content of the (C) component may be 0.1 to 10 parts by mass, 0.5 to 8 parts by mass, or 1 to 5 parts by mass per 100 parts by mass of the total amount of the (A) and (B) components, because excellent micro-processability is easily obtained.
[0045] (Thermal polymerization initiator) The photosensitive resin composition according to the present embodiment may further contain a thermal polymerization initiator as component (D) from the viewpoint of promoting the polymerization reaction of the thermally polymerizable crosslinking agent. As component (D), a compound that decomposes by heating during curing to generate radicals and promote the polymerization reaction of components (A) and (B) is preferable. As component (D), for example, an organic peroxide can be mentioned.
[0046] Examples of organic peroxides include methyl ethyl ketone peroxide, methylcyclohexanone peroxide, methylacetoacetate peroxide, acetylacetone peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(4,4-di-t-butylperoxy)cyclohexane, t-butylperoxycyclohexyl)propane, 1,1-bis(t-butylperoxy)cyclododecane, n-butyl-4,4-bis(t-butylperoxy)valerate, 2,2-bis(t-butylperoxy)butane, 1,1-bis(t-butylperoxy)-2-methylcyclohexane, t-butyl hydroperoxide, p-menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, t-hexyl hydroperoxide, dicumyl peroxide, 2,5-dimethyl -2,5-bis(t-butylperoxy)hexane, α,α'-bis(t-butylperoxy)diisopropylbenzene, t-butylcumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3, isobutyryl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, lauroyl peroxide, cinnamic acid peroxide, m-toluoyl peroxide, benzoyl peroxide, diisopropyl Peroxydicarbonate, bis(4-t-butylcyclohexyl) peroxydicarbonate, di-3-methoxybutyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, di(4-t-butylcyclohexyl) peroxydicarbonate, α,α'-bis(neodecanoylperoxy)diisopropylbenzene, cumyl peroxyneodecanoate, 1,1,3,3,-Tetramethylbutylperoxyneodecanoate, 1-cyclohexyl-1-methylethylperoxyneodecanoate, t-hexylperoxyneodecanoate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 1-cyclohexyl-1-methylethylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxyisobutyrate, Examples of the peroxyalkylene compounds include tert-butyl peroxymaleic acid, t-butyl peroxy laurate, t-butyl peroxy-3,5,5-trimethylhexanoate, t-butyl peroxy isopropyl monocarbonate, t-butyl peroxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, t-butyl peroxy acetate, t-hexyl peroxy benzoate, t-butyl peroxy-m-toluoyl benzoate, t-butyl peroxy benzoate, bis(t-butylperoxy) isophthalate, t-butyl peroxy allyl monocarbonate, and 3,3',4,4'-tetra(t-butylperoxycarbonyl) benzophenone. These compounds may be used alone or in combination of two or more.
[0047] The content of the (D) component is not particularly limited, but may be 0.1 to 10.0 parts by mass, 0.5 to 5.0 parts by mass, or 0.7 to 3.0 parts by mass relative to 100 parts by mass of the total amount of the (A) and (B) components.
[0048] (Coupling Agent) The photosensitive resin composition according to the present embodiment may further contain a coupling agent. The coupling agent may be a silane coupling agent. The silane coupling agent may have, for example, a vinyl group, an epoxy group, a styryl group, an acryloyl group, a methacryloyl group, an amino group, a ureido group, an isocyanate group, an isocyanurate group, a mercapto group, or the like.
[0049] Examples of silane coupling agents having a vinyl group include KBM-1003 and KBE-1003 (trade names of Shin-Etsu Chemical Co., Ltd.; the same applies below). Examples of silane coupling agents having an epoxy group include KBM-303, 402, 403, KBE-402, 403, X-12-981S, and X-12-984S. Examples of silane coupling agents having a styryl group include KBM-1403. Examples of silane coupling agents having a methacryloyl group include KBM-502, 503, KBE-502, and 503. Examples of silane coupling agents having an acryloyl group include KBM-5103, X-12-1048, and X-12-1050. Examples of silane coupling agents having an amino group include KBM-602, 603, 903, 573, 575, KBE-903, 9103P, and X-12-972F. Examples of silane coupling agents having a ureido group include KBE-585. Examples of silane coupling agents having an isocyanate group include KBE-9007 and X-12-1159L. Examples of silane coupling agents having an isocyanurate group include KBM-9659. Examples of silane coupling agents having a mercapto group include KBM-802, 803, X-12-1154, and X-12-1156. The silane coupling agent may be a silane coupling agent having a methacryloyl group. The silane coupling agents may be used alone or in combination of two or more.
[0050] The content of the silane coupling agent may be 0.01 to 10 parts by mass, 0.1 to 8 parts by mass, or 0.5 to 5 parts by mass, relative to 100 parts by mass of the total amount of the components (A) and (B).
[0051] (rust inhibitor) The photosensitive resin composition according to the present embodiment may further contain a rust inhibitor in order to suppress corrosion or prevent discoloration of copper wiring. Examples of the rust inhibitor include triazole derivatives such as benzotriazole, and tetrazole derivatives. The rust inhibitor may be used alone or in combination of two or more.
[0052] The content of the rust inhibitor may be 0.01 to 10 parts by mass, 0.1 to 5 parts by mass, or 0.5 to 3 parts by mass, relative to 100 parts by mass of the total amount of the components (A) and (B).
[0053] (Polymerization inhibitor) The photosensitive resin composition according to this embodiment may further contain a polymerization inhibitor from the viewpoint of storage stability.
[0054] Examples of the polymerization inhibitor include 4-tert-butylcatechol, 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxy radical, p-methoxyphenol, diphenyl-p-benzoquinone, benzoquinone, hydroquinone, pyrogallol, phenothiazine, resorcinol, orthodinitrobenzene, paradinitrobenzene, metadinitrobenzene, phenanthraquinone, N-phenyl-2-naphthylamine, cupferron, 2,5-toluquinone, tannic acid, parabenzylaminophenol, tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, and nitrosamines. The polymerization inhibitor may be used alone or in combination of two or more.
[0055] The content of the polymerization inhibitor may be 0.01 to 10 parts by mass, 0.05 to 5 parts by mass, or 0.10 to 2 parts by mass, relative to 100 parts by mass of the total amount of the components (A) and (B).
[0056] (solvent) The photosensitive resin composition according to this embodiment contains a solvent for dissolving and dispersing each component, which makes it easy to apply the composition to a substrate and forms a coating film of uniform thickness. The solvent may be used alone or in combination of two or more kinds.
[0057] Examples of the solvent include ketones such as methyl ethyl ketone, cyclohexanone, and cyclopentanone; aromatic hydrocarbons such as toluene, xylene, mesitylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate; and nitrogen-containing compounds such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, and 3-butoxy-N,N-dimethylpropanamide.
[0058] The amount of the solvent is not particularly limited, but may be an amount such that the solid content in the photosensitive resin composition is 5 to 60 mass %, 10 to 50 mass %, or 15 to 40 mass %.
[0059] The preparation means, conditions, etc. of the photosensitive resin composition are not particularly limited. For example, a method in which each main component in a predetermined amount is thoroughly and uniformly stirred and mixed by a mixer or the like, and then kneaded using a mixing roll, an extruder, a kneader, a roll, an extruder, etc. is mentioned. The kneading method is not particularly limited.
[0060] The dielectric constant at 10 GHz of the cured product of the photosensitive resin composition according to this embodiment may be 2.80 or less, 2.70 or less, 2.65 or less, or 2.60 or less. The dielectric loss tangent at 10 GHz of the cured product of the photosensitive resin composition may be 0.0050 or less, 0.0045 or less, 0.0040 or less, or 0.0030 or less. The dielectric constant and the dielectric loss tangent can be measured by the method described in the examples using a cured film of the photosensitive resin composition.
[0061] The photosensitive resin composition according to the present embodiment is capable of forming a fine pattern. The photosensitive resin composition according to the present embodiment is capable of forming an insulating film that exhibits low dielectric properties and has excellent insulation reliability. A semiconductor element having an interlayer insulating layer formed from the cured product of the above-mentioned photosensitive resin composition, and an electronic device including the semiconductor element can be produced. The semiconductor element can improve high-frequency characteristics by having a rewiring layer including the cured product of the photosensitive resin composition according to the present embodiment. The semiconductor element may be, for example, a memory, a package, etc. having a multilayer wiring structure, a rewiring structure, etc. Examples of electronic devices include mobile phones, smartphones, tablet terminals, personal computers, and hard disk suspensions. By providing a patterned cured film formed by the photosensitive resin composition of the present embodiment, a semiconductor element and an electronic device having excellent reliability can be provided. EXAMPLES
[0062] The present disclosure will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0063] (Synthesis Example 1) Into a 1L flask equipped with a condenser, a nitrogen inlet tube, a thermocouple, and a stirrer, 24.35 parts by mass of 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho [1,2-C] furan-1,3-dione (manufactured by New Japan Chemical Co., Ltd., trade name "TDA-100"), 132.69 parts by mass of T-SOL100 (manufactured by ENEOS Corporation, aromatic high boiling point solvent), and 29.33 parts by mass of Solmix A-11 (manufactured by Japan Alcohol Sales Co., Ltd., alcohol-based solvent) were added. After addition, the temperature was raised to 80 ° C. and kept at 40.68 parts by mass of dimer diamine (trade name "PRIAMINE 1075", manufactured by Croda Japan Co., Ltd.) was added dropwise. After the addition, 5.01 parts by mass of norbornane diamine (manufactured by Mitsui Chemicals Fine Co., Ltd.) was added. After the addition, 2.08 parts by mass of an aqueous methanesulfonic acid solution (manufactured by BASF, trade name "Lutropur MSA") was added, and the temperature was raised to 160°C. After the temperature was raised, 40.00 parts by mass of toluene (manufactured by Yamaichi Chemical Industry Co., Ltd.) was added, and a dehydration ring-closing reaction was carried out at 160°C for 1 hour, and water and alcohol in the reaction solution were removed to obtain an intermediate polyimide. Subsequently, the obtained polyimide was cooled to 130°C, 7.96 parts by mass of maleic anhydride (manufactured by Fuso Chemical Industry Co., Ltd.) was added, and the temperature was raised to 160°C. A dehydration ring-closing reaction was carried out at 160°C for 4 hours, and water in the reaction solution was removed to obtain a maleimide compound.
[0064] The obtained maleimide compound was placed in a separatory funnel, 500 parts by mass of pure water was added, the separatory funnel was shaken, and the mixture was allowed to stand. After standing, the aqueous layer and the organic layer were separated, and only the organic layer was collected. The collected organic layer was placed in a 1 L glass vessel equipped with a cooler, a nitrogen inlet tube, a thermocouple, a stirrer, and a vacuum pump, and the temperature was raised to 88 to 93°C. After removing water, the temperature was raised to 100°C. The solvent was removed for 0.5 hours under a reduced pressure of 0.1 MPa from atmospheric pressure, to obtain a maleimide compound (A-1) of the component (A).
[0065] The molecular weight of the maleimide compound (A-1) was measured by GPC. A sample in which the maleimide compound was dissolved in tetrahydrofuran (THF) to a concentration of 3% by mass was injected in an amount of 50 μL into a column (GL-R420 (Hitachi High-Tech Fielding Corporation) x 1, GL-R430 (Hitachi High-Tech Fielding Corporation) x 1, GL-R440 (Hitachi High-Tech Fielding Corporation) x 1) heated to 30 ° C., and the measurement was performed under the condition of a flow rate of 1.6 mL / min using THF as a developing solvent. The detector used was an L-3350 RI detector (Hitachi, Ltd.), and the weight average molecular weight (Mw) was calculated from the elution time using a molecular weight / elution time curve created using standard polystyrene (Tosoh Corporation). The Mw of (A-1) was 10900.
[0066] As component (B), the following compounds were prepared. TA-G: 1,3,4,6-tetraallyl glycol uril (manufactured by Shikoku Chemical Industry Co., Ltd., product name, number of allyl groups: 4) TAIC: Triallyl isocyanurate (product name, manufactured by Mitsubishi Chemical Corporation, number of allyl groups: 3) L-DAIC: Isocyanurate with allyl groups (manufactured by Shikoku Chemical Industry Co., Ltd., product name, number of allyl groups: 2 or more) A-9300: Tris-(2-acryloyloxyethyl)isocyanurate (product name, manufactured by Shin-Nakamura Chemical Co., Ltd., number of acryloyl groups: 3)
[0067] The following compounds were prepared as component (C), component (D), coupling agent, polymerization inhibitor, rust inhibitor, and solvent. Component (C): Oxime ester photopolymerization initiator (manufactured by BASF Japan Ltd., product name "Irgacure OXE01") Component (D): α,α'-bis(t-butylperoxy)diisopropylbenzene (manufactured by NOF Corporation, trade name "Perbutyl P") Coupling agent: 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-503") Polymerization inhibitor: 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPOL) (Tokyo Chemical Industry Co., Ltd.) Rust inhibitor: 1,2,3-benzotriazole (manufactured by Johoku Chemical Industry Co., Ltd., product name "BT-120") Solvent: Mesitylene (manufactured by Toyo Gosei Co., Ltd.)
[0068] [Photosensitive resin composition] Each component in the amounts (parts by weight, solid content) shown in Table 1 was mixed with 210 parts by weight of the solvent, stirred at 25°C for 30 minutes or more, and then filtered through a #200 nylon mesh (mesh opening: 75 μm) to prepare a photosensitive resin composition.
[0069] (Dielectric properties) The photosensitive resin composition was applied onto copper foil using a knife coater, and then air-dried for 15 minutes and dried in a dryer at 90°C for 15 minutes to form a coating film. The coating film was exposed to light using a high-pressure mercury lamp (exposure amount: 1000 mJ / cm 2 ) and post-exposure baking (100°C, 1 minute) on a hot plate to form a resin film with a thickness of 100 μm. The resin film was then cured in a nitrogen atmosphere using a clean oven at 200°C for 2 hours. The copper foil was then dissolved and removed with ammonium persulfate to obtain a cured film.
[0070] The cured film was cut into a length of 80 mm and a width of 80 mm to prepare an evaluation sample. The dielectric constant (Dk) and dielectric loss tangent (Df) of the evaluation sample were measured at room temperature and 10 GHz using a SPDR dielectric resonator (manufactured by QWED) and an analyzer (manufactured by Agilent Technologies, product name "PNA Network Analyzer N5227A").
[0071] (5% weight loss temperature) The cured film was weighed out in an amount of 6.0 to 10.0 mg and placed in an open-type sample container (Hitachi High-Tech Science Corporation, product name "GCA-0055") and measured at a 5% weight loss temperature (T d5) was measured. The measurement device used was NEXTA STA200RV (manufactured by Hitachi High-Tech Science Corporation).
[0072] (Elongation at break) The photosensitive resin composition was spin-coated on a silicon wafer with a Cu sputtered film, and then heated and dried at 90°C for 5 minutes using a hot plate to form a resin film with a thickness of 14 µm. Then, a mask aligner exposure machine (manufactured by Mikasa Corporation, product name "MA-20") was used to expose the film to an exposure dose of 1000 mJ / cm. 2 After pattern exposure under the above conditions to obtain a resin film with a width of 10 mm, the wafer was heated at 100°C for 1 minute using a hot plate. The wafer was then immersed in a developer (a mixture of cyclopentanone and propylene glycol monomethyl ether acetate) at 25°C for 30 seconds, and washed with propylene glycol monomethyl ether acetate to form a patterned resin film on the silicon wafer. The silicon wafer on which the patterned resin film was formed was heated under conditions of 200°C and 2 hours in a nitrogen atmosphere to obtain a silicon wafer with a patterned cured film. The silicon wafer with the patterned cured film was immersed in an aqueous solution of ammonium persulfate, and the peeled cured film was washed with pure water to prepare an evaluation sample with a width of 10 mm. The evaluation sample was measured for breaking elongation at room temperature using a small tabletop tester (manufactured by Shimadzu Corporation, product name "EZ-S") at a chuck distance of 20 mm and a tensile speed of 5 mm / min.
[0073] (Micro-processability) The photosensitive resin composition was spin-coated on a silicon wafer and dried by heating at 90° C. for 5 minutes using a hot plate to form a resin film with a thickness of 8 μm. Then, an i-line stepper exposure machine (manufactured by Therma Precision Co., Ltd., product name "Sc6k") was used to expose the film to an exposure dose of 300 mJ / cm. 2After the resin film was exposed to light under the above conditions, it was heated at 100°C for 1 minute using a hot plate. It was then immersed in a developer (a mixture of cyclopentanone and propylene glycol monomethyl ether acetate) at 25°C for 20 seconds and washed with propylene glycol monomethyl ether acetate. After development, the resin film was checked using a metallurgical microscope for peeling from the silicon wafer, cracks in the resin film, roughness at the edge of the pattern, and the presence or absence of residue at the bottom of the pattern where the resin film was developed. Cases where the minimum via diameter was 20 μm or less and where these defects were not confirmed were evaluated as "A," and cases where the minimum via diameter was more than 20 μm were evaluated as "B."
[0074] [Table 1]
Claims
1. Contains a maleimide compound, a crosslinking agent, and a photopolymerization initiator; the maleimide compound is a reaction product of a tetracarboxylic dianhydride, an amine, and maleic anhydride, the amine containing a dimer diamine and a second amine other than the dimer diamine, The photosensitive resin composition, wherein the crosslinking agent comprises a polymerizable crosslinking agent having an allyl group.
2. The photosensitive resin composition according to claim 1, wherein the tetracarboxylic dianhydride comprises at least one selected from the group consisting of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride, 4,4'-oxydiphthalic anhydride, 1,2,3,4-butanetetracarboxylic dianhydride, and 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-C]furan-1,3-dione.
3. The photosensitive resin composition according to claim 1, wherein the second amine comprises at least one selected from the group consisting of metaxylylenediamine, 4,4'-diaminodiphenylmethane, 1,3-diaminopropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and norbornanediamine.
4. 2. The photosensitive resin composition according to claim 1, wherein the polymerizable crosslinking agent having an allyl group comprises at least one selected from the group consisting of 1,3,4,6-tetraallyl glycol uril, triallyl isocyanurate, and diallyl isocyanurate.
5. The photosensitive resin composition according to claim 1 , wherein the crosslinking agent further comprises a polymerizable crosslinking agent having a (meth)acryloyl group.
6. The photosensitive resin composition according to claim 1 , further comprising a thermal polymerization initiator.
7. A cured product of the photosensitive resin composition according to any one of claims 1 to 6.
8. A semiconductor device having a rewiring layer comprising a cured product of the photosensitive resin composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Positive photosensitive insulating resin composition and cured product of the same
JP2007057595A
Positive photosensitive resin composition, method for producing resist pattern and electronic device
JP2008309885A
Positive-type photosensitive resin composition, method for producing resist pattern, semiconductor device, and electronic device
WO2010073948A1
Cited By
Photosensitive resin composition, cured product, and semiconductor element
WO2025134897A1