Perfluoropolyether group-containing phosphonate compound, surface treatment agent, and article treated with surface treatment agent

A perfluoropolyether group-containing phosphonate compound with a specific structure addresses the issues of water and oil repellency, heat resistance, and synthesis complexity in existing surface treatment agents, providing durable films with enhanced properties.

JP2024147937AActive Publication Date: 2024-10-17HARVES CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023060696
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Existing surface treatment agents using fluorine-containing compounds suffer from insufficient water and oil repellency, heat resistance, and complex synthesis processes, with issues such as reduced molecular mobility, poor thermal and chemical stability, and cumbersome production methods.

Method used

A perfluoropolyether group-containing phosphonate compound with a specific structure, represented by the general formula A-O-Rf-(CF2)x-L-(CH2)y-P(=O)(OR1)2-z(OH)z, forms a cured film with excellent water and oil repellency, abrasion resistance, and heat resistance, utilizing a phosphonate bond for improved stability and ease of synthesis.

Benefits of technology

The compound achieves durable films with high water and oil repellency, excellent abrasion resistance, and heat resistance, along with ease of fingerprint stain removal and mold releasability, addressing the limitations of previous compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147937000001
    Figure 2024147937000001
Patent Text Reader

Abstract

To provide a perfluoropolyether group-containing phosphonate compound which is capable of forming a cured film on the surface of a base material when used in a surface treatment agent, the cured film having excellent water and oil repellency, wear resistance, antifouling properties, lubricity, fingerprint stain removal easiness, mold releasability and heat resistance.SOLUTION: According to the present invention, there is provided a perfluoropolyether group-containing phosphonate compound represented by formula (1). (1): A-O-Rf-(CF2)x-L-(CH2)y-P(=O)(OR1)2-z(OH)z. In formula (1), A represents a perfluoroalkyl group having 1 to 4 carbon atoms, Rf represents a perfluoropolyether group, and L represents a linking group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a perfluoropolyether group-containing phosphonate compound, a surface treatment agent, and an article treated with the surface treatment agent. [Background technology]

[0002] It is known that certain fluorine-containing compounds have very small surface free energy, and therefore, when used for surface treatment of a substrate, they can provide excellent water and oil repellency, antifouling properties, mold releasing properties, lubricity, etc. When used for surface treatment, excellent water and oil repellency, abrasion resistance, antifouling properties, lubricity, ease of removing fingerprint stains, and durability are required. As a technique for improving the surface of a metal substrate, a surface treatment technique using a phosphonate compound is known, and examples of its use include antifouling treatment applications for design parts such as stainless steel, automobile parts, home appliances, interior building materials, etc., and applications as mold release agents.

[0003] As a surface treatment agent for satisfying the above requirements, for example, a fluorine-containing polyether phosphonic acid ester compound represented by the following formula (I) has been proposed (Patent Document 1). (RO)(RO)P(O)(CH2) a CF(CF3)〔OCF2CF(CF3)〕 b O(CF2) c O〔CF(CF3)CF2O〕 d CF(CF3)(CH2) e P(O)(OR3)(OR4)···(I) (wherein R1, R2, R3 and R4 are hydrogen atoms, alkyl groups, cycloalkyl groups, aryl groups, alkylaryl groups, aralkyl groups or groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms, and a, b, c, d and e are integers satisfying the conditions 2≦a+e≦8, b+d≦28 and 1≦c≦10, and b and d can be 0).

[0004] The following has been proposed as a surface treatment agent with improved water and oil repellency, ease of removing fingerprint stains, and abrasion resistance (Patent Document 2). The surface treatment agent is a surface treatment agent for substrates that contains a perfluoropolyether group-containing phosphate compound, and the perfluoropolyether group-containing phosphate compound is a compound represented by the following formula (II). B 1 -(C m F 2m O) n1 -A 1 (II) During the ceremony, A 1 is a monovalent organic group having one or more terminal phosphate groups, B 1 is R F1 -O-, D 1 -Q 1 -O-CH2- or A 2 -O-, Here, R F1 is a perfluoroalkyl group having 1 to 6 carbon atoms, D 1 is CF3- or CF3-O-, Q 1 represents a fluoroalkylene group having 1 to 20 carbon atoms containing one or more hydrogen atoms, a fluoroalkylene group having 2 to 20 carbon atoms containing one or more hydrogen atoms and having an ethereal oxygen atom between the carbon-carbon atoms, an alkylene group having 1 to 20 carbon atoms, or an alkylene group having 2 to 20 carbon atoms having an ethereal oxygen atom between the carbon-carbon atoms, A 2 is a monovalent organic group having one or more terminal phosphate groups, m is an integer from 1 to 6; n1 is an integer from 2 to 200; (C m F 2m O) n1 is a group represented by the following formula (2-1-a). (CF2CF2O) n4 (CF2CF2CF2CF2O) n5 (2-1-a) During the ceremony, n4 is an integer equal to or greater than 1, n5 is an integer equal to or greater than 1, Here, n4+n5 is an integer between 2 and 200. (CF2CF2O) and (CF2CF2CF2CF2O) are arranged alternately.

[0005] In addition, a compound represented by the following formula (III) has been disclosed as a surface treatment agent for metals (Patent Document 3). [R f -O-CFY-LO] m P(=O)(O - Z + ) 3-m (III) [Wherein, L is (a) -CH2-(OCH2CH2)n- (n is an integer of 0 to 3) and (b) -CO-NR'-(CH2) q -(R' is H or C 1-4 alkyl, and q is an integer from 1 to 4), m is 1, Y is -F or -CF3, Z+ is H+, M+ (M is an alkali metal), N(R)4+ (R are the same or different and are H or C 1-6 alkyl), R f is a polyperfluoroalkylene oxide chain]

[0006] Furthermore, the following have been proposed as surface treatment agents with improved water and oil repellency, fingerprint stain removability, and abrasion resistance (Patent Document 4). A-Rf 1 -Q 1 -Q 2 -(CH2) a -P(=O)(OX)2(IV) In formula (IV), A is a -CF group, a -CF2CF3 group, or a group represented by the following formula (IV-2), and Rf 1 Ha-(CF2) d -(OCF2) p (OCF2CF2) q (OCF2CF2CF2) r (OCF2CF2CF2CF2) s (OCF(CF3)CF2) t -O(CF2) d-, each d is independently an integer of 0 to 5, p, q, r, s, and t are independently an integer of 0 to 200, and p+q+r+s+t is 3 to 200, and each unit shown in parentheses may be randomly bonded. Q 1 is a divalent linking group, Q 2 is a divalent linking group having silicon atoms at both ends, Each X is independently a hydrogen atom, an alkali metal atom, an unsubstituted or substituted alkyl group having 1 to 5 carbon atoms, an aryl group, or a monovalent group represented by JSi- (J is independently an unsubstituted or substituted alkyl group or aryl group having 1 to 5 carbon atoms), and a is an integer of 2 to 20. -Q 1 -Q 2 -(CH2) a -P(=O)(OX)2(IV-2) [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 4245050 [Patent Document 2] Patent No. 6769304 [Patent Document 3] Patent No. 3574222 [Patent Document 4] Patent No. 6488890 Summary of the Invention [Problem to be solved by the invention]

[0008] However, there were cases where the water / oil repellency or heat resistance was insufficient. For example, it was found that the compound represented by the above formula (I) in Patent Document 1 had insufficient water / oil repellency. It was also found that the compound represented by the above formula (II) in Patent Document 2 or the formula (III) in Patent Document 3 had poor heat resistance. It was also found that the compound represented by formula (IV) in Patent Document 4 had a complicated synthesis process.

[0009] More specifically, it was found that the compound represented by formula (I) has a bulky CF3 group in the side chain of the fluorine chain portion, and therefore has a large dynamic friction coefficient, poor antifouling properties, and poor ease of removing fingerprint stains. In addition, it was found that the compound has phosphonate functional groups at both ends of the molecule, which reduces molecular mobility, resulting in insufficient water / oil repellency and abrasion resistance. In addition, the compounds represented by formulas (II) and (III) have a phosphate ester bond (COP) between the fluorine chain and the phosphonate functional group, which has a low bond energy and is prone to hydrolysis and has poor thermal and chemical stability. Furthermore, the compound represented by formula (IV) contains a silicon atom between the fluorine chain and the phosphonate functional group, and the synthesis process is complicated, which poses a production problem.

[0010] The present invention has been made in view of the above circumstances, and provides a perfluoropolyether group-containing phosphonate compound capable of forming a cured film excellent in water and oil repellency, abrasion resistance, antifouling properties, lubricity, ease of fingerprint stain removal, releasability, and heat resistance on the surface of a substrate when used in a surface treatment agent. Also provided is a surface treatment agent capable of forming a cured film excellent in water and oil repellency, abrasion resistance, antifouling properties, lubricity, ease of fingerprint stain removal, releasability, and heat resistance on the surface of a substrate, and an article provided with a cured film of the surface treatment agent. [Means for solving the problem]

[0011] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and discovered that when a perfluoropolyether group-containing phosphonate compound having a specific structure is used as a surface treatment agent, it is possible to form a coating film on the surface of a substrate which has excellent water and oil repellency, abrasion resistance, stain resistance, lubricity, ease of removing fingerprint stains, release properties and heat resistance, and thus completed the present invention.

[0012] The following invention is provided: [1] A perfluoropolyether group-containing phosphonate compound represented by the following general formula (1): AO-Rf-(CF2) x-L-(CH2) y -P(=O)(OR 1 ) 2-z (OH) z (1) In the general formula (1), A is a perfluoroalkyl group having 1 to 4 carbon atoms, Rf is a structure represented by the following general formula (2), and each bonding unit in the parentheses may be bonded randomly: (CF2O) p (CF2CF2O) q (CF2CF2CF2O) r (CF2CF2CF2CF2O) s (CF(CF3)CF2O) t (2) In the general formula (2), p, q, r, s, and t are each independently an integer of 0 to 100, and p+q+r+s+t is an integer of 10 to 100; L is a single bond, C(=O)NR 2 , CH2O or CH2, and R 2 is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, or an aryl group, x is an integer from 1 to 2; y is an integer from 1 to 4; z is an integer from 0 to 2; R 1 is a hydrocarbon group having 1 to 4 carbon atoms, or SiR 3 3, R 3 is a hydrocarbon group having 1 to 4 carbon atoms; compound. [2] The compound according to [1], wherein in the general formula (2), p is an integer of 1 or more, and q is an integer of 1 or more. [3] In the general formula (1), A is a CF group; Rf is a structure represented by the following general formula (2-1), and each bonding unit in the parentheses may be bonded randomly. (CF2O) p (CF2CF2O) q (2-1) L is CH2O or CH2; In the general formula (2-1), p and q each independently represent an integer of 1 to 30, The compound according to [1] or [2], wherein p+q is an integer of 10 to 50. [4] The compound according to any one of [1] to [3], which has a number average molecular weight of more than 1,500. [5] A surface treatment agent comprising the compound according to any one of [1] to [4] and a volatile solvent. [6] An article comprising a substrate and a cured film of the surface treatment agent of [5] on the surface of the substrate. [7] The article described in [6], wherein the substrate is a metal. [8] The article described in [6], wherein the substrate is a metal oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present invention will be described. Various features shown in the following embodiments can be combined with each other. Also, each feature can be an invention independently.

[0014] 1. Perfluoropolyether group-containing phosphonate compound A compound according to one embodiment of the present invention (hereinafter also referred to as "compound P") is a perfluoropolyether group-containing phosphonate compound represented by the following general formula (1). Each element in general formula (1) will be described below. AO-Rf-(CF2) x -L-(CH2) y -P(=O)(OR 1 ) 2-z (OH) z (1)

[0015] A is a perfluoroalkyl group having 1 to 4 carbon atoms. The perfluoroalkyl group preferably has a straight-chain structure from the viewpoint of water repellency. The straight-chain perfluoroalkyl group is, for example, a CF3 group (CF3-), a CF3CF2 group (CF3CF2-), a CF3CF2CF2 group (CF3CF2CF2-), or a CF3CF2CF2CF2 group (CF3CF2CF2CF2-). The perfluoroalkyl group is preferably a CF3 group (CF3-).

[0016] Rf is a structure represented by the following general formula (2). (CF2O) p (CF2CF2O) q (CF2CF2CF2O) r (CF2CF2CF2CF2O) s (CF(CF3)CF2O) t (2)

[0017] In the structure of formula (2), the bonding units in the parentheses, i.e., one or more bonding units contained in Rf among "CF2O", "CF2CF2O", "CF2CF2CF2O", "CF2CF2CF2CF2O", and "CF(CF3)CF2O", are not particularly limited in the bonding order in Rf, and each bonding unit may be bonded randomly with no regularity, or may have a structure with a predetermined regularity (for example, a structure in which the bonding units are bonded alternately, or a block structure for each type of bonding unit). Each bonding unit in the parentheses is preferably bonded randomly. When each of these bonding units is bonded randomly, Rf may include a portion in which the same type of bonding unit is continuously repeated, a portion in which the same type of bonding unit is not continuously repeated, etc. In addition, the perfluoroalkylene group contained in each bonding unit in the structure of formula (2) preferably has 1 to 4 carbon atoms, more preferably has 1 to 2 carbon atoms.

[0018] When Rf has a structure represented by formula (2), it has excellent lubricity, antifouling properties, ease of fingerprint stain removal, and mold releasability. Although the relationship between the structure and these effects is not yet clear, it is speculated that the surface free energy is reduced because the perfluoropolyether group has a flexible structure in which the rigid perfluoroalkylene group is divided by oxygen atoms with high mobility. In addition, as for compound P, a structure having phosphonate functional groups at both ends of the molecule is not preferable from the viewpoint of wear resistance, etc., because molecular mobility may be reduced.

[0019] In one embodiment, the bond unit constituting Rf preferably does not have a CF3 group in the side chain. For example, the structure of formula (2) preferably does not have "CF(CF3)CF2O" as a bond unit (i.e., t is 0). When the structure is a straight chain structure without a bulky CF3 group in the side chain of the fluorine chain portion, the lubricity, antifouling property, ease of removing fingerprint stains, and wear resistance are particularly excellent.

[0020] In formula (2), p, q, r, s, and t are each independently an integer of 0 to 100, and preferably an integer of 1 to 30. In formula (2), p is preferably an integer of 1 or more, and q is preferably an integer of 1 or more.

[0021] In the formula (2), p+q+r+s+t is an integer of 10 to 100, and preferably 10 to 60.

[0022] From the viewpoint of antifouling properties, Rf is preferably a structure represented by the following general formula (2-1). (CF2O) p (CF2CF2O) q (2-1)

[0023] In the structure of formula (2-1), the order of bonding of each bond unit in parentheses in Rf is not particularly limited, and each bond unit may be bonded randomly with no regularity, or may have a structure with a predetermined regularity (for example, a structure in which they are bonded alternately, or a block structure for each type of bond unit, etc.). Rf in the structure represented by formula (2-1) has "CF2O" and "CF2CF2O" as bond units, and is composed only of these units.

[0024] In formula (2-1), p and q each independently represent an integer of 1 to 30, and preferably an integer of 5 to 25.

[0025] In formula (2-1), p+q is an integer of 10 to 50, and preferably an integer of 15 to 45. When p+q is less than 10, the abrasion resistance, antifouling property, and releasability are poor. When p+q is more than 50, the ratio of phosphonate groups present per unit molecule is small, the adhesion to the substrate surface is weak, and the abrasion resistance is poor. Furthermore, the molecular weight is large, so that the solubility in a solvent is low, and the compatibility when other components are blended is also poor.

[0026] L is a single bond, C(=O)NR 2 , CH2O or CH2. L is preferably CH2O or CH2. From the viewpoints of thermal stability (heat resistance) and chemical stability, L is more preferably CH2.

[0027] A single bond directly connects adjacent structural units. When L is a single bond, the structure in formula (1) is "-(CF2) x -(CH2) y -".

[0028] C(=O)NR 2 R in 2is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, or an aryl group. The substituted or unsubstituted alkyl group having 1 to 5 carbon atoms may be a linear, branched, or cyclic alkyl group, and is preferably a linear alkyl group. Specific examples of the unsubstituted alkyl group having 1 to 5 carbon atoms include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, and n-pentyl groups; branched alkyl groups such as isopropyl, isobutyl, tert-butyl, isopentyl, and tert-pentyl groups; and cyclic alkyl groups such as cyclopropyl, cyclobutyl, and cyclopentyl groups.

[0029] x is an integer of 1 to 2, and is preferably 1.

[0030] y is an integer of 1 to 4, and preferably 2 or 3. In addition, since the phosphonate functional group is bonded via a phosphonate bond (CP) and not via a phosphate ester bond (COP) which has a small bond energy, hydrolysis is unlikely to occur and the thermal or chemical stability is high.

[0031] z is an integer of 0 to 2, and is preferably 2 from the viewpoint of adhesion between the cured film and the substrate.

[0032] R 1 is a hydrocarbon group having 1 to 4 carbon atoms, or SiR 3 3. Compound P is R 1 If there are multiple R 1 may be different or the same. 3 Multiple R's in 3 3 may be different or the same

[0033] R 1 Examples of the hydrocarbon group having 1 to 4 carbon atoms as R include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an isopropyl group, an isobutyl group, a tert-butyl group, a cyclopropyl group, and a cyclobutyl group. 1From the viewpoint of ease of synthesis, R is preferably a methyl group. 3 The hydrocarbon group having 1 to 4 carbon atoms as R 1 R is a hydrocarbon group having 1 to 4 carbon atoms. 1 may be selected independently of R. 3 From the viewpoint of ease of synthesis, etc., is preferably a methyl group.

[0034] The number average molecular weight of compound P is preferably more than 1500, more preferably more than 1500 and not more than 5000. If it is not more than 1500, the fluorine chain is short, so that the water and oil repellency and the mold releasability are inferior. If it is not less than 5000, the content of the functional group is small, so that the adhesion is weak and the abrasion resistance is deteriorated.

[0035] <Method of producing compound P> Compound P can be synthesized, for example, by using a perfluoropolyether group-containing compound having a modifiable functional group at its terminal as a starting material. The perfluoropolyether group-containing compound can be produced by a known method (for example, International Publication No. 2009-008380, Japanese Patent No. 6107659). Specifically, the following perfluoropolyether group-containing compounds [1a] to [1f] can be used as starting materials. [1a] AO-Rf-(CF2) x -C(=O)F [1b] AO-Rf-(CF2) x -C(=O)OR 4 (R 4 : Hydrocarbons with 1 to 4 carbon atoms) [1c] AO-Rf-(CF2) x -C(=O)OH [1d] AO-Rf-(CF2) x -CHOH [1e] AO-Rf-(CF2) x -Br [1f] AO-Rf-(CF2) x -I

[0036] Using any one of the above starting materials [1a] to [1f], a compound having an unsaturated group at the end can be obtained by a known method. For example, the following intermediate [2d] can be obtained by reacting the starting material [1d] with allyl bromide in the presence of a basic compound. [2d] AO-Rf-(CF2) x -L-(CH2) y -CH=CH2

[0037] From the intermediate [2d], a compound having a terminal phosphonate group can be obtained by a known method. For example, the following compound [3d] can be obtained as compound P by reacting with dimethyl phosphite in the presence of peroxide. [3d] AO-Rf-(CF2) x -L-(CH2) y -P(=O)(OCH3)2

[0038] Furthermore, the phosphonate group of compound [3d] can be silylated by a known method to obtain compound [4d-1], or dealkylated by a known method to obtain compound [4d-2] as compound P. [4d-1] AO-Rf-(CF2) x -L-(CH2) y -P(=O)(OSiR 3 )2 [4d-2] AO-Rf-(CF2) x -L-(CH2) y -P(=O)(OH)2

[0039] 2. Surface treatment agent The compound P can be used as a component of a surface treatment agent, and the surface treatment agent according to one embodiment of the present invention is a composition containing the compound P and a volatile solvent. The compound P contained in the surface treatment agent may be one type or two or more types in combination.

[0040] The surface treatment agent contains compound P in an amount of preferably 0.1 to 5 mass %, more preferably 0.1 to 2 mass %, based on 100 mass % of the total amount of the surface treatment agent. By making it 0.1 mass % or more, the coating film has a sufficient thickness, and is excellent in initial water repellency (contact angle), weather resistance, and abrasion resistance. In addition, by making it 5 mass % or less, the coating film does not become too thick, and the workability when spreading is good, and the coating film has excellent uniformity and transparency. In addition, the cost of the surface treatment agent can be reduced.

[0041] <Volatile solvent> The volatile solvent is not limited as long as it is a solvent in which the compound P is soluble, and examples thereof include fluorine-modified solvents, non-fluorine-based solvents, and mixtures thereof.

[0042] Examples of fluorine-modified solvents include hydrofluoroethers, perfluorocarbons, perfluoroalkylamines, hydrofluorocarbons, perfluoropolyethers, hydrofluorochlorocarbons, hydrofluoroolefins, and fluorine-modified aromatic hydrocarbons.

[0043] Examples of non-fluorinated solvents include lower alcohols such as ethyl alcohol and isopropyl alcohol; ketones such as methyl ethyl ketone and methyl isobutyl ketone; esters such as ethyl acetate and butyl acetate; hydrocarbon solvents such as hexane, toluene, benzene and xylene; and ethers such as diethyl ether and diisopropyl ether.

[0044] These volatile solvents may be used alone or in combination of two or more. Among these volatile solvents, from the viewpoints of solubility, wettability, etc., the volatile solvent preferably includes a fluorine-modified solvent. In one embodiment, the volatile solvent is a fluorine-modified solvent.

[0045] Furthermore, the volatile solvent may be a mixed solution of a fluorine-modified solvent and a non-fluorine-based solvent, if necessary, and may be mixed in any ratio. For example, the volatile solvent may contain 50 to 100 mass% of the fluorine-modified solvent in a total of 100 mass% of the fluorine-modified solvent and the non-fluorine-based solvent.

[0046] <Other ingredients> The surface treatment agent may contain other components within the range not impairing the effects of the present invention. Examples of the other components include a perfluoropolyether compound having no phosphonate group and a catalyst.

[0047] Examples of the perfluoropolyether compound include commercially available perfluoropolyether oils such as FOMBLIN M, FOMBLIN Y, and FOMBLIN Z (manufactured by Solvay Solexis), Krytox (manufactured by DuPont), and Demnum (manufactured by Daikin Industries, Ltd.).

[0048] The catalyst is added for the purpose of promoting the hydrolysis reaction of the phosphonate functional group or the condensation reaction between the functional group and the base material, and includes acid catalysts and basic catalysts. Examples of the acid catalyst include hydrochloric acid, nitric acid, acetic acid, sulfuric acid, phosphoric acid, sulfonic acid, methanesulfonic acid, p-toluenesulfonic acid, etc. Examples of the basic catalyst include sodium hydroxide and potassium hydroxide, etc.

[0049] A surface treatment agent according to another embodiment of the present invention is a composition containing a neutralized salt of compound P and water. Compound P can be used in the surface treatment agent in the form of an aqueous solution as a neutralized salt. For example, compound P can be used by reacting it with sodium hydroxide, ammonium hydroxide, zinc sulfate, zinc acetate, zinc oxide, triethylamine, morpholine, triethanolamine, or the like to form a metal salt, an amine salt, or an ammonium salt. The neutralized salt of compound P contained in the surface treatment agent may be used alone or in combination of two or more kinds. The aqueous solution may further contain an organic solvent compatible with water, a catalyst, and other additives, as necessary.

[0050] <Method of manufacturing surface treatment agent> The surface treatment agent is obtained by dissolving the compound P in a volatile solvent. In addition, the surface treatment agent may be produced by dissolving other components such as a catalyst together with the compound P in a volatile solvent, if necessary.

[0051] In another embodiment, the compound P may be obtained by converting it into a metal salt, an amine salt, or an ammonium salt and dissolving it in water.

[0052] 3.Goods An article according to one embodiment of the present invention is an article including a substrate and a cured film provided on the substrate. The cured film is a coating obtained by curing the above-mentioned surface treatment agent. The cured film is a coating having water repellency and oil repellency. The cured film is, for example, a film obtained by applying a surface treatment agent to the surface of a substrate and curing the surface treatment agent.

[0053] The substrate material may be an inorganic material or an organic material. Inorganic materials include metals, metal oxides, single crystal materials, stone, glass, and composite materials thereof. Metals include, for example, iron, iron alloys (stainless steel, etc.), aluminum, aluminum alloys, etc. Metal oxides include, for example, sapphire, etc. Organic materials include, for example, resins, etc. Resins include, for example, acrylic resins, polycarbonate resins, etc.

[0054] The article is not particularly limited as long as the substrate (surface) to be treated has a heat resistance higher than the curing temperature. The curing temperature is, for example, a temperature for curing the applied surface treatment agent. Examples of the article include design parts, ornaments, cookers, water-related products, building materials, automobiles, precision molds, displays such as smartphones, wearable terminals, and tablet terminals, optical parts such as eyeglass lenses and protective films, and medical devices such as endoscopes.

[0055] <Production method> As a coating method for coating the above-mentioned surface treatment agent on the surface of the substrate, a known method such as a hand coating method, a nozzle flow coating method, a dipping method, a spray method, a reverse coating method, a flow coating method, a spin coating method, a roll coating method, or a vacuum deposition method can be appropriately adopted.

[0056] In addition, the substrate surface may be subjected to a treatment (pretreatment) to improve the adhesive strength between the substrate and the cured coating. Examples of pretreatment include polishing, cleaning, and drying with various polishing liquids, surface modification treatment with an acidic or basic solution, primer treatment, plasma irradiation, corona discharge, high-pressure mercury lamp irradiation, etc., which generate active groups on the substrate surface. In particular, primer treatment is preferable because it can form active groups on the substrate and increase the number of active groups on the surface to which the surface treatment agent is applied.

[0057] Next, the treatment after applying the surface treatment agent to the substrate will be described. After applying the surface treatment agent to the substrate, it can be cured at room temperature or by heating at 50 to 150°C. In one embodiment, room temperature means, for example, less than 50°C (or 10 to 30°C). By heating, the phosphonate group of compound P and the binding group such as a hydroxyl group present on the substrate surface can be bonded more strongly than in the case where heat treatment is not performed, and a cured film having excellent durability can be formed on the substrate surface. Heating may be performed under normal pressure, under pressure, under reduced pressure, or in an inert atmosphere.

[0058] The thickness of the cured film is preferably 50 nm or less, more preferably 2 to 20 nm, and even more preferably 4 to 15 nm.

[0059] If the excess portion dries and remains on the substrate, the excess portion can be wiped off with a paper towel or cloth moistened with an organic solvent or a dry paper towel or cloth to obtain an article on which a cured film has been formed.

[0060] <Surface characteristics> The cured film of the surface treatment agent formed on the substrate preferably has the following properties:

[0061] (contact angle) A contact angle meter (NICK LSE-B100W) is used to generate a 2 μL droplet and measure the contact angle with the test substrate. Measurements are performed at five different points on the surface, and the average value is taken as the contact angle.

[0062] The contact angle of water is preferably 110 degrees (deg) or more, more preferably 114 degrees or more, and further preferably 115 degrees or more.

[0063] The contact angle of hexadecane is preferably 70 degrees or more, more preferably 72 degrees or more, and even more preferably 73 degrees or more.

[0064] The contact angle of oleic acid is preferably 76 degrees or more, more preferably 78 degrees or more, and even more preferably 79 degrees or more.

[0065] (Fall angle) Using a contact angle meter (NICK LSE-B100W), a 20μL droplet is dropped, the horizontally placed test substrate is gradually tilted, and the angle between the test substrate and the horizontal plane is measured when the droplet begins to slide down. Measurements are taken at five different points on the surface, and the average value is taken as the slide angle.

[0066] The water fall angle is preferably 20 degrees or less, more preferably 18 degrees or less, and even more preferably 16 degrees or less.

[0067] The sliding angle of hexadecane is preferably 15 degrees or less, more preferably 11 degrees or less, and even more preferably 9 degrees or less.

[0068] The sliding angle of oleic acid is preferably 22 degrees or less, more preferably 21 degrees or less, and further preferably 20 degrees or less. EXAMPLES

[0069] The present invention will be specifically described below with reference to Synthesis Examples, Examples, and Comparative Examples, but the present invention is not limited to the following Examples.

[0070] The phosphonate compounds 1 to 7 (also referred to as compounds [1] to [7]) used in the study as components of the surface treatment agent are shown below. Phosphonate compounds 1 to 5 and 7 were synthesized by the methods shown below, and phosphonate compound 6 was a commercially available product. Phosphonate compound 1: CF3O(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(=O)(OH)2 p / q≒0.9, p+q≒25 Phosphonate compound 2: CF3O(CF2O) p (CF2CF2O) q CF2CH2CH2CH2CH2P(=O)(OH)2 p / q≒0.9, p+q≒25 Phosphonate compound 3: CF3O(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(=O)(OH)2 p / q≒0.9, p+q≒45 Phosphonate compound 4: CF3O(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(=O)(OH)2 p / q≒0.9, p+q≒15 Phosphonate compound 5: (OH)2(O=)PCH2CH2CH2OCH2CF2(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(=O)(OH)2 p / q≒0.9, p+q≒45 Phosphonate compound 6: CF3O(CF2O) p (CF2CF2O) q CF2CH2O(CH2CH2O) n P(=O)(OH)2 Mn=2,400 Phosphonate compound 7: CF3CF2CF2CF2O(CF2CF2O)2CF2CH2CH2CH2P(=O)(OH)2

[0071] <Synthesis Example> Synthesis of phosphonate compound 1 (Process 1-1) Sodium hydride (4.2 g) and meta-xylene hexafluoride (100 g) were mixed in a 0.5 L flask equipped with a stirrer, a reflux condenser, a thermometer, a dry nitrogen inlet tube, and a dropping funnel, and the mixture was stirred for 20 minutes in an ice bath. Then, an alcohol (100 g) represented by the following formula [1-1] and meta-xylene hexafluoride (50 g) were dropped, and the mixture was stirred at room temperature for 20 minutes. Then, allyl bromide (21 g) and meta-xylene hexafluoride (50 g) were dropped, and the mixture was reacted at room temperature for 1 hour. Then, the mixture was reacted at 60°C for 1 hour, 80°C for 1 hour, and 100°C for 4 hours in sequence. Then, the reaction product was cooled, 50 g of SV110 (a fluorine-based solvent manufactured by Solvay) was added, and the mixture was washed with 10 g of normal heptane and 10 g of methanol, and the lower layer was separated. This washing procedure was repeated four times, and the solvent in the separated lower layer was distilled off to obtain 101 g (yield 99%) of a colorless, transparent liquid represented by the following formula [1-2]. Compound [1-1]:CF3O(CF2O) p (CF2CF2O) q CF2CH2OH p / q≒0.9, p+q≒25 Compound [1-2]:CF3O(CF2O) p (CF2CF2O) q CF2CH2OCH2CH=CH2

[0072] (Step 1-2) Compound [1-2] (50 g), dimethyl phosphite (3.5 g), t-butyl peroxyoctoate (1.4 g), and meta-xylene hexafluoride (50 g) were mixed in a 0.2 L flask equipped with a stirrer, reflux condenser, thermometer, and dry nitrogen inlet tube, and stirred at 80° C. for 7 hours. The low boiling point components in the reaction solution were distilled off to obtain 47 g of a colorless, transparent liquid represented by the following formula [1-3] (yield 90%). Compound [1-3]: CF3O(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(O)(OCH3)2

[0073] (Step 1-3) In a 0.1 L flask equipped with a stirrer, reflux condenser, thermometer, and dry nitrogen inlet tube, compound [1-3] (30 g), trimethylsilyl iodide (6.1 g), and meta-xylene hexafluoride (30 g) were mixed and stirred at 50° C. for 7 hours. Then, 30 g of methanol was added and stirred at 50° C. for 7 hours. By carrying out the same purification operation as in (Step 1-1), 28 g of a colorless transparent liquid represented by the following formula [1] was obtained (yield 95%). Compound [1]:CF3O(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(O)(OH)2

[0074] The results of NMR measurement are as follows. The structures corresponding to each shift value are indicated with "". compound [1] 1 H-NMR(CDCl3,TMS,δ):1.9-2.0 (4H,m,CF2CH2OCH2"CH2CH2"P(O)(OH)2),3.8-3.9(4H,m, CF2"CH2"O"CH2"CH2CH2P(O)(OH)2)

[0075] Synthesis of phosphonate compound 2 (Step 2-1) In a 1L flask equipped with a stirrer, reflux condenser, thermometer, and dry nitrogen inlet tube, the alcohol represented by [1-1] (200 g), triphenylphosphine (46 g), carbon tetrabromide (58 g), imidazole (12 g), meta-xylene hexafluoride (250 g), and N,N'-dimethylformamide (250 g) were mixed and stirred at 100°C for 24 hours. By carrying out the same purification procedure as in (Step 1-1), 201 g of a pale yellow transparent liquid represented by the following formula [2-1] was obtained (yield 98%). Compound [2-1]:CF3O(CF2O) p (CF2CF2O) q CF2CH2Br

[0076] (Step 2-2) In a 0.5 L flask equipped with a stirrer, reflux condenser, thermometer, and dry nitrogen inlet tube, the compound represented by [2-1] (100 g), allyltributyltin (15 g), azobisisobutyronitrile (0.73 g), and metaxylenehexafluoride (100 g) were mixed and stirred at 90° C. for 7 hours. After carrying out the same purification procedure as in (Step 1-1), the recovered layer was treated with silica gel and concentrated to obtain 74 g of a colorless, transparent liquid represented by the following formula [2-2] (yield 75%). Compound [2-2]:CF3O(CF2O) p (CF2CF2O) q CF2CH2CH2CH=CH2

[0077] (Step 2-3) Using compound [2-2] as a raw material, compound [2-3] represented by the following formula was synthesized in the same manner as in (step 1-2). (Colorless transparent liquid, yield 88%) Compound [2-3]: CF3O(CF2O) p (CF2CF2O) q CF2CH2CH2CH2CH2P(O)(OCH3)2

[0078] (Step 2-4) Using the compound [2-3] as a raw material, the compound represented by the following formula was synthesized in the same manner as in (Step 1-3) (colorless transparent liquid, 93% yield). Compound [2]:CF3O(CF2O) p (CF2CF2O) q CF2CH2CH2CH2CH2P(O)(OH)2

[0079] The results of NMR measurement are as follows. The structures corresponding to each shift value are indicated with "". compound [2] 1 H-NMR(CDCl3,TMS,δ):1.8-2.0(6H,m,CF2CH2"CH2CH2CH2"P(O)(OH)2), 2.1-2.3(2H,m,CF2"CH2"CH2CH2CH2P(O)(OH)2)

[0080] Synthesis of phosphonate compound 3 Compound [3-1] was used as a raw material and reacted in the same manner as in (Step 1-1) to (Step 1-3). Compound [3] represented by the following formula was synthesized (colorless transparent liquid, total yield 90%). The structure and purity of the obtained compound are 1 This was confirmed by H-NMR measurement. Compound [3-1]:CF3O(CF2O) p (CF2CF2O) q CF2CH2OH p / q≒0.9, p+q≒45 Compound [3]:CF3O(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(O)(OH)2

[0081] Synthesis of phosphonate compound 4 Compound [4-1] was used as a raw material and reacted in the same manner as in (Step 1-1) to (Step 1-3). Compound [4] represented by the following formula was synthesized (colorless transparent liquid, total yield 89%). The structure and purity of the obtained compound are 1 This was confirmed by H-NMR measurement. Compound [4-1]:CF3O(CF2O) p (CF2CF2O) q CF2CH2OH p / q≒0.9, p+q≒15 Compound [4]:CF3O(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(O)(OH)2

[0082] Synthesis of phosphonate compound 5 Compound [5-1] was used as a raw material and reacted in the same manner as in (Step 1-1) to (Step 1-3). Compound [5] represented by the following formula was synthesized (colorless transparent liquid, total yield 86%). The structure and purity of the obtained compound are 1 This was confirmed by H-NMR measurement. Compound [5-1]: HOCH2CF2(CF2O) p (CF2CF2O) q CF2CH2OH p / q≒0.9, p+q≒45 Compound [5]: (OH)2(O=)PCH2CH2CH2OCH2CF2(CF2O) p (CF2CF2O) q CF2CH2OCH2CH2CH2P(=O)(OH)2

[0083] Synthesis of phosphonate compound 7 Compound [7-1] was used as a raw material and reacted in the same manner as in (Step 2-2) to (Step 2-4). Compound [7] represented by the following formula was synthesized (colorless transparent liquid, total yield 81%). The structure and purity of the obtained compound are 1 This was confirmed by H-NMR measurement. Compound [7-1]: CF3CF2CF2CF2O(CF2CF2O)2CF2Br Compound [7]: CF3CF2CF2CF2O(CF2CF2O)2CF2CH2CH2CH2P(O)(OH)2

[0084] <Preparation of surface treatment agent> 0.5 g of each phosphonate compound and 99.5 g of Novec 7200 (a fluorine-based solvent manufactured by 3M) were mixed and thoroughly stirred to obtain surface treatment agents 1 to 7 containing 0.5 mass % of the active ingredient relative to 100 mass % of the total amount of the surface treatment agent.

[0085] <Preparation of test substrate> Each test piece of stainless steel plate (SUS304, 26mm x 76mm) was immersed in normal heptane and subjected to ultrasonic treatment (5 minutes). The same operation was then performed with acetone. Next, the test pieces were subjected to VUV treatment (λ max = 254 nm, gap 2 mm, 6 times). The test pieces were dip-coated with a surface treatment agent (pulling speed: 10 mm / s). Finally, they were heated and cured at 100°C for 1 hour to obtain test substrates 1 to 7 having a cured film.

[0086] <Evaluation of test substrates using each surface treatment agent> The cured films of the test substrates 1 to 7 were evaluated by the following tests (1) to (7). Each test was carried out on the surface-treated surface of the test substrate.

[0087] (1) Contact angle measurement (water and oil repellency test) A contact angle meter (NICK LSE-B100W) was used to generate 2 μL droplets and measure the contact angle with the test substrate. Measurements were performed at five different points on the surface, and the average value was shown. Water, hexadecane, and oleic acid were used as droplets.

[0088] (2) Falling angle measurement (water and oil repellency test) Using a contact angle meter (NICK LSE-B100W), a 20μL droplet was dropped, and the test substrate placed horizontally was gradually tilted, and the angle (sliding angle) between the test substrate and the horizontal plane when the droplet started to slide was measured. Measurements were taken at five different points on the surface, and the average value was shown. Water, hexadecane, and oleic acid were used as droplets.

[0089] (3) Pen writing test (anti-stain test) The test board was written on with an oil-based marking pen (product name: Mackie, manufactured by Zebra Co., Ltd.), and the ink repellency was visually evaluated. The evaluation criteria were as follows: 1. Repels ink well 2: Repels ink but has slow coagulation speed 3: Ink repellency is weak 4: Ink repellency is weak and coagulation speed is slow 5: The ink is barely repelled, leaving ink streaks behind 6: Does not repel ink at all

[0090] (4) Abrasion resistance test A nonwoven fabric (Bencotto) was attached to an abrasion resistance tester (API-3DT manufactured by API Corporation) and subjected to a test at 1 kgf / cm 2 The test substrate was slid at a speed of 40 mm x 60 reciprocations / min under a load of 1.0 mm. After every 1,000 reciprocations, the contact angle of water was measured in the same manner as in "(1) Contact angle measurement" above, and the test was continued until the contact angle fell below 100 degrees or the number of reciprocations reached 10,000.

[0091] (5) Heat resistance test The test substrate was exposed to a thermostatic chamber (WFO-420 manufactured by Tokyo Rikakikai Co., Ltd.) set at 200°C. After every 24 hours, the substrate was removed and allowed to cool, after which the surface of the test substrate was rinsed with Asahiklin AK-225 (a fluorine-based solvent manufactured by AGC), and the water contact angle was measured in the same manner as in "(1) Contact angle measurement" above. The test was continued until the contact angle fell below 100 degrees or the exposure time reached 200 hours.

[0092] (6) Friction test (lubricity test) A surface texture measuring instrument (Shinto Scientific Co., Ltd., TYPE: 14FW) was placed on an ABS ball (1 cm 3 ) was attached, and the test substrate was slid 1 cm at a speed of 500 mm / min under a load of 100 gf to measure the dynamic friction coefficient.

[0093] (7) Mold releasability / mold release durability test An epoxy adhesive (TOA Gosei Co., Ltd.; one-part curing epoxy resin AP-0021HW) was applied to the test board, and a hook-shaped jig (cross-sectional area: 1 cm 2 ) was placed on the plate. The adhesive was cured by heating at 100°C for 30 minutes. Next, the metal substrate was fixed on a tensile tester (A&D benchtop tensile compression tester MCT-2150), and the hook was pulled up in the 90° direction at a speed of 60 mm / min. The release load at this time was taken as the mold releasability, and was evaluated according to the following evaluation criteria (A and B were considered to be pass, and C was considered to be fail). The above series of operations was repeated, and the number of times that release was possible under a release load of less than 50 N with the formation of a cured film by applying the surface treatment agent once was measured, and the number of times was used as an index of release durability. A: Less than 1N B: 1N or more, less than 10N C: 10N or more

[0094] Table 1 shows the evaluation results of the surface properties for each of the Examples and Comparative Examples.

[0095] [Table 1]

[0096] As shown in Table 1, the test substrates treated with the surface treatment agents using phosphonate compounds 1 to 4 showed good results in terms of water and oil repellency, abrasion resistance, antifouling, lubricity, ease of removing fingerprint stains, heat resistance, and release properties and release durability. In addition, the dynamic friction coefficients were small.

[0097] The test substrate treated with the surface treatment agent using phosphonate compound 5 had insufficient water and oil repellency, and also had poor abrasion resistance and lubricity. This is presumably because the presence of phosphonate functional groups at both ends of the molecule limits the molecular mobility of the perfluoropolyether chain.

[0098] The test substrate treated with the surface treatment agent using phosphonate compound 6 had insufficient heat resistance and poor release durability. This is presumably due to the weak bond energy of the phosphate ester bond (COP) between the perfluoropolyether group and the phosphonate functional group and the ether bond in the ethylene oxide chain.

[0099] The test substrate treated with the surface treatment agent using phosphonate compound 7 showed poor abrasion resistance, antifouling properties, lubricity, and releasability. This is presumably because the molecular weight of the perfluoropolyether group is small and the function of the perfluoropolyether group is not fully exerted. Possible industrial applications

[0100] The article treated with the surface treatment agent of the present invention has good water and oil repellency, abrasion resistance, antifouling property, release property, lubricity, ease of removing fingerprint stains, and heat resistance. Due to such properties, it can be used as a surface treatment agent for articles such as design parts, ornaments, cookers, water-related products, building materials, automobiles, precision molds, displays of smartphones, wearable terminals, tablet terminals, optical parts such as eyeglass lenses and protective films, and medical devices such as endoscopes.

Claims

1. A perfluoropolyether group-containing phosphonate compound represented by the following general formula (1): A-O-Rf-(CF 2 ) x -L-(CH 2 ) y -P(=O)(OR 1 ) 2-z (OH) z (1) In the general formula (1), A is a perfluoroalkyl group having 1 to 4 carbon atoms; Rf is a structure represented by the following general formula (2), and each bonding unit in the parentheses may be bonded randomly: (CF 2 O) p (CF 2 CF 2 O) q (CF 2 CF 2 CF 2 O) r (CF 2 CF 2 CF 2 CF 2 O) s (CF(CF 3 )CF 2 O) t (2) In the general formula (2), p, q, r, s, and t each independently represent an integer from 0 to 100, and p+q+r+s+t represents an integer from 10 to 100; L is a single bond, C(=O)NR 2 , C.H. 2 O or CH 2 and R 2 is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 5 carbon atoms, or an aryl group, x is an integer from 1 to 2; y is an integer from 1 to 4, z is an integer from 0 to 2; R 1 is a hydrocarbon group having 1 to 4 carbon atoms, or SiR 3 3 and R 3 is a hydrocarbon group having 1 to 4 carbon atoms; compound.

2. The compound according to claim 1 , wherein, in the general formula (2), p is an integer of 1 or more, and q is an integer of 1 or more.

3. In the general formula (1), A is CF 3 It is based on Rf is a structure represented by the following general formula (2-1), and each bonding unit in the parentheses may be bonded randomly: (CF 2 O) p (CF 2 CF 2 O) q (2-1) L is CH 2 O or CH 2 and In the general formula (2-1), p and q each independently represent an integer of 1 to 30, p+q is an integer from 10 to 50; The compound of claim 1.

4. The compound of claim 1 having a number average molecular weight of greater than 1500.

5. A surface treatment agent comprising the compound according to any one of claims 1 to 4 and a volatile solvent.

6. An article comprising a substrate and a cured film of the surface treatment agent of claim 5 on the surface of the substrate.

7. The article of claim 6 , wherein the substrate is a metal.

8. The article of claim 6 , wherein the substrate is a metal oxide.

Citation Information

Patent Citations

  • Low-surface-energy composition and application thereof

    CN105647363A

  • Magnetic fluid and manufacture thereof

    JP1986263202A

  • Acrylic elastomer cured molded product

    JP1996198975A

  • Vulcanized acrylic elastomer molding

    JP1996283519A

  • Perfluoropolyetheramide-linked phosphonates, phosphates and their derivatives

    JP2007502814A