Exterior material for power storage device
The exterior material for power storage devices addresses deformation and pressure distribution issues in all-solid-state batteries by optimizing layer stiffness and thickness ratios, ensuring stable performance in high-temperature conditions.
Patent Information
- Application Number
- JP2023060921
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2043-04-04
AI Technical Summary
All-solid-state batteries face issues with excessive deformation and non-uniform pressure distribution due to temperature changes, leading to insufficient output when pressurized in high-temperature environments.
An exterior material for power storage devices is designed with specific loop stiffness values and thickness ratios for its layers, including a base material layer, barrier layer, and sealant layer, to maintain structural integrity and uniform pressure distribution even in high-temperature conditions.
The exterior material effectively suppresses excessive deformation and ensures uniform pressure application, enhancing the performance and output of all-solid-state batteries in high-temperature environments.
Smart Images

Figure 2024148040000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an exterior material for an electricity storage device. [Background technology]
[0002] Known examples of power storage devices include secondary batteries such as lithium ion batteries, nickel metal hydride batteries, and lead storage batteries, as well as electrochemical capacitors such as electric double layer capacitors. Due to the miniaturization of portable devices or the limitations of installation space, there is a demand for further miniaturization of power storage devices, and lithium ion batteries with high energy density have attracted attention. Metallic cans have traditionally been used as exterior materials for lithium ion batteries, but multilayer films that are lightweight, have high heat dissipation properties, and can be produced at low cost have come to be used.
[0003] A lithium ion battery using the above multilayer film as an exterior material is called a laminated lithium ion battery. A laminated lithium ion battery includes an electric storage element having a positive electrode, a liquid electrolyte, and a negative electrode, and an exterior bag that houses the electric storage element, and prevents moisture from penetrating into the battery. The exterior bag has an exterior material, and the exterior material includes a base layer, a barrier layer, an adhesive layer, and a sealant layer in this order. The exterior material covers the electric storage element with the sealant layer facing inward and the base layer facing outward. A laminated lithium ion battery is manufactured, for example, by forming a recess in a part of the exterior material by cold molding, housing the electric storage element in the recess, folding back the remaining part of the exterior material, and sealing the edge portion by heat sealing (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-101765 A Summary of the Invention [Problem to be solved by the invention]
[0005] Meanwhile, as a next-generation battery of lithium-ion batteries, for example, a power storage device called an all-solid-state battery has been researched and developed. The all-solid-state battery includes, for example, a power storage element and an outer bag that houses the power storage element. In the all-solid-state battery, peeling may occur between the solid electrolyte and the positive electrode active material, or between the solid electrolyte and the negative electrode active material, due to expansion or contraction of the negative electrode and the positive electrode accompanying charging and discharging. This may cause the output of the all-solid-state battery to be insufficient. For this reason, in order to improve the output of the all-solid-state battery, unlike the liquid-type lithium-ion battery, the power storage element may be pressurized through the outer bag. However, if the outer bag is excessively deformed due to the pressurization, uniform pressurization of the power storage element through the outer bag may not be performed.
[0006] Here, the temperature range of the all-solid-state battery is, for example, from -40°C to 100°C. This range is wider than the temperature range of a liquid lithium-ion battery (for example, from -40°C to 60°C). When an all-solid-state battery pressurized by an outer bag in a high-temperature environment (for example, 70°C or higher) is used to improve the output of the all-solid-state battery, the above-mentioned deformation of the outer bag is likely to occur. Therefore, even when the all-solid-state battery is used in a high-temperature environment, the output of the all-solid-state battery may be insufficient.
[0007] An object of one aspect of the present disclosure is to provide an exterior material for an electricity storage device that is less likely to deform excessively even when pressurized in a high-temperature environment. [Means for solving the problem]
[0008] An exterior material for an electricity storage device according to one aspect of the present disclosure comprises a base material layer, a barrier layer, a thermal adhesive resin layer or an adhesive layer, and a sealant layer, which are laminated in this order, and when the thermal adhesive resin layer and the sealant layer, or the sealant layer, are (I) and the base material layer is (II), the loop stiffness value of (I) is 10 mN or more and 80 mN or less, the loop stiffness value of (II) is 2 mN or more and 20 mN or less, the loop stiffness value ratio (I / II) of (I) to (II) is 1.0 or more and 15 or less, and the thickness ratio (I / II) of (I) to (II) is 1.0 or more and 8.0 or less.
[0009] According to the electrical storage device exterior material, the ratio (I / II) of the loop stiffness value of (I) to (II) is 1.0 or more and 15 or less, and the ratio (I / II) of the thickness of (I) to (II) is 1.0 or more and 8.0 or less. By satisfying these parameters, an electrical storage device exterior material that is unlikely to deform excessively even when pressurized in a high-temperature environment is provided.
[0010] The thickness of the above (I) may be 30 μm or more and 120 μm or less, and the thickness of the above (II) may be 10 μm or more and 60 μm or less. In this case, the durability of the exterior material can be ensured while suppressing the thickness of the exterior material. In addition, the loop stiffness value of the above (I) and the loop stiffness value of the above (II) can be reliably set within the above range.
[0011] The ratio (I / II) of the loop stiffness value of (I) to that of (II) may be 2.5 or more and 11.0 or less. In this case, deformation of the exterior material for an electricity storage device is further suppressed even when pressure is applied in a high-temperature environment.
[0012] The ratio (I / II) of the loop stiffness value of (I) above to that of (II) above may be 3.5 or more and 10 or less. In this case, even when pressure is applied in a high-temperature environment, deformation of the exterior material for an electricity storage device is more effectively suppressed.
[0013] The sealant layer may contain a polypropylene-based resin as a base resin, and the polypropylene-based resin may be composed of homopropylene or block polypropylene. In this case, melting of the sealant layer in a high-temperature environment can be suppressed.
[0014] The sealant layer may further contain an additive resin containing a polyethylene-based resin or a block copolymer that is compatible with the polypropylene-based resin, in which case deformation of the electrical storage device packaging material is further suppressed.
[0015] The sealant layer may further include an additive resin containing a polyethylene-based resin, and a compatibilizer having a portion compatible with the polypropylene-based resin and a portion compatible with the polyethylene-based resin, whereby deformation of the electrical storage device packaging material is more effectively suppressed.
[0016] The compatibilizer may include a block copolymer of polypropylene and polyethylene, or a block copolymer of polyethylene and polyethylenebutylene.
[0017] The electrical storage device exterior material may be an all-solid-state battery exterior material. The electrical storage device exterior material is highly suitable as an exterior material for all-solid-state batteries because it can suppress deformation even when pressurized in a high-temperature environment. Effect of the Invention
[0018] According to the present disclosure, it is possible to provide an exterior material for an electricity storage device that is not prone to excessive deformation even when pressurized in a high-temperature environment. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a schematic cross-sectional view of an exterior material for an electricity storage device according to one embodiment. [Diagram 2] FIG. 2 is a perspective view illustrating an electricity accumulation device according to one embodiment. [Diagram 3]FIG. 3(a) is a schematic cross-sectional view of a comparative exterior material when pressed against a rigid body, and FIG. 3(b) is a schematic cross-sectional view of an exterior material for an electricity storage device according to one embodiment when pressed against a rigid body. [Figure 4] FIG. 4 is a schematic cross-sectional view of an exterior material for an electricity storage device according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0021] [Exterior materials for energy storage devices] FIG. 1 is a schematic cross-sectional view of an exterior material for an electricity storage device according to an embodiment. As shown in FIG. 1, an exterior material 10 (exterior material for an electricity storage device) according to an embodiment is an exterior material used for an electricity storage device, and includes a base layer 11, a barrier layer 13, a thermal adhesive resin layer 15, and a sealant layer 16, which are laminated in this order. When a laminate of the thermal adhesive resin layer 15 and the sealant layer 16 is (I) and the base layer 11 is (II), the loop stiffness value of (I) is 10 mN or more and 80 mN or less, the loop stiffness value of (II) is 2 mN or more and 20 mN or less, the ratio (I / II) of the loop stiffness values of (I) and (II) is 1.0 or more and 15 or less, and the ratio (I / II) of the thicknesses of (I) and (II) is 1.0 or more and 8.0 or less. According to this exterior material 10, deformation can be suppressed even when pressure is applied in a high-temperature environment.
[0022] In one embodiment, in the packaging material 10, the barrier layer 13 has a first corrosion prevention treatment layer 14a on the substrate layer 11 side via a first adhesive layer 12a, and a second corrosion prevention treatment layer 14b on the sealant layer 16 side. When the packaging material 10 is used as an exterior bag for an electricity storage device, the substrate layer 11 is the outermost layer and the sealant layer 16 is the innermost layer in the packaging material 10. That is, the packaging material 10 is used with the substrate layer 11 facing the outside of the electricity storage device and the sealant layer 16 facing the inside of the electricity storage device.
[0023] Each layer constituting the packaging material 10 will now be described in detail.
[0024] <Base material layer> The base layer 11 imparts heat resistance in a sealing process when manufacturing an electricity storage device and plays a role in suppressing the occurrence of pinholes that may occur during molding and distribution. In particular, in the case of an exterior material for a large-scale electricity storage device, the base layer 11 can also impart scratch resistance, chemical resistance, insulation, and the like.
[0025] The base layer 11 is preferably a layer formed of an insulating resin, such as polyester resin, polyamide resin, polyimide resin, polyamideimide resin, polyetherketone resin, polyphenylene sulfide resin, polyetherimide resin, polysulfone resin, fluororesin, phenol resin, melamine resin, urethane resin, allyl resin, silicone resin, epoxy resin, furan resin, acetyl cellulose resin, or the like.
[0026] Among these resins, polyester resin and polyamide resin are preferable for the base layer 11 because of their excellent moldability. Examples of polyester resin include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyamide resin include nylon 6, nylon 6,6, a copolymer of nylon 6 and nylon 6,6, nylon 9T, nylon 10, polymetaxylylene adipamide (MXD6), nylon 11, and nylon 12.
[0027] The substrate layer 11 may be in the form of a stretched or unstretched film, or in the form of a coating film. The substrate layer 11 may be a single layer or a multilayer. When the substrate layer 11 is a multilayer, it is formed by laminating layers made of different resins. When the substrate layer 11 is in the form of a film, it may be a co-extruded film or a laminated film using an adhesive. When the substrate layer 11 is a coating film, it may be a coating film obtained by coating a composition for forming a coating film multiple times. The substrate layer 11 may be a multilayer film by combining a film and a coating film.
[0028] When the above-mentioned resin is used in the form of a film, the base layer 11 is preferably a biaxially stretched film. In this case, the moldability of the packaging material 10 is improved. Examples of the stretching method for the biaxially stretched film include a sequential biaxial stretching method, a tubular biaxial stretching method, and a simultaneous biaxial stretching method. From the viewpoint of obtaining better deep-draw moldability, the biaxially stretched film is preferably a film stretched by a tubular biaxial stretching method.
[0029] The thickness of the base layer 11 is 10 μm or more and 60 μm or less. The thickness of the base layer 11 may be 15 μm or more, 20 μm or more, 25 μm or more, 50 μm or less, 40 μm or less, or 35 μm or less. When the thickness of the base layer 11 is within the above range, the loop stiffness value of the base layer 11 can be easily controlled within a suitable range.
[0030] From the viewpoint of stiffness of the exterior material 10, resistance to deformation due to heat, etc., the loop stiffness value of the base material layer 11 is 2 mN or more and 20 mN or less. The loop stiffness value of the base material layer 11 may be 2.5 mN or more and 17 mN or less, 3 mN or more and 15 mN or less, or 4.5 mN or more and 14.5 mN or less. The loop stiffness value of the base material layer 11 corresponds to the stress when the base material layer 11 is folded into a loop shape and compressed in the diameter direction of the loop. In general, the stiffer the film, the higher the loop stiffness value. The loop stiffness value of the base material layer 11 is obtained, for example, by a loop stiffness tester described in the examples described later.
[0031] <First adhesive layer> The first adhesive layer 12a is a layer that bonds the base material layer 11 and the barrier layer 13. Specific examples of materials constituting the first adhesive layer 12a include polyurethane resins in which a bifunctional or higher isocyanate compound (polyfunctional isocyanate compound) acts as a curing agent on a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol. The above-mentioned various polyols can be used alone or in combination of two or more types depending on the functions and performance required for the exterior material 10. In addition, materials constituting the first adhesive layer 12a can also be used that use an epoxy resin as a base material and a curing agent in addition to the above.
[0032] The first adhesive layer 12a is formed using an adhesive composition containing the above-mentioned base agent and curing agent. In addition, the first adhesive layer 12a may be formed by blending various other additives and stabilizers into the above-mentioned adhesive composition according to the performance required for the adhesive layer. As an additive, for example, a tin-based, titanium-based, or zirconium-based urethane catalyst may be blended to promote curing, and a visible curing agent or a latent curing agent may be blended. As the visible curing agent or the latent curing agent, for example, an amine-based compound may be mentioned. These may be blended alone or in combination of multiple types.
[0033] The adhesive composition preferably contains at least one polyfunctional isocyanate compound selected from the group consisting of alicyclic isocyanate polymers and isocyanate polymers containing an aromatic ring in the molecular structure as a curing agent. Examples of the polyfunctional isocyanate compound include a nurate of isophorone diisocyanate, an adduct of tolylene diisocyanate, an adduct of hexamethylene diisocyanate, a biuret and a nurate of hexamethylene diisocyanate, a biuret and a nurate of tolylene diisocyanate, an adduct, a biuret and a nurate of diphenylmethane diisocyanate, and an adduct, a biuret and a nurate of xylylene diisocyanate.
[0034] As the curing agent, an alicyclic isocyanate polymer may be used in combination with an isocyanate polymer containing an aromatic ring in the molecular structure. By using these in combination, the heat resistance tends to be further improved.
[0035] From the viewpoint of further improving heat resistance, the adhesive composition preferably contains at least one polyol selected from the group consisting of polyester polyol, acrylic polyol, and polycarbonate diol. Among these, from the viewpoint of further improving heat resistance, polyester polyol is more preferable.
[0036] In the adhesive composition, the ratio (NCO / OH) of the number of isocyanate groups contained in the polyfunctional isocyanate compound to the number of hydroxyl groups contained in the polyol may be 1.5 or more and 40.0 or less, or 15.0 or more and 30.0 or less. If this ratio is 1.5 or more, the curing agents react with each other, and by-products such as urea resin and biuret resin are easily generated. Since these by-products contain active hydrogen groups, they interact with polar groups of adjacent layers, and the interfacial adhesion between the first adhesive layer 12a and the base material layer 11 and the barrier layer 13 is further improved. Therefore, the heat resistance of the packaging material 10 tends to be improved. On the other hand, if the ratio is 40.0 or less, the laminate strength of the packaging material 10 can be further improved in room temperature and high temperature environments.
[0037] The thickness of the first adhesive layer 12a is not particularly limited, but from the viewpoint of obtaining the desired adhesive strength, followability, processability, etc., it is, for example, 1 μm or more and 10 μm or less, or 2 μm or more and 7 μm or less.
[0038] The mass per unit area of the first adhesive layer 12a is set to 2.0 g / m from the viewpoint of ensuring superior lamination strength both at room temperature and at high temperatures and obtaining superior deep drawability. 2 More than 6.0g / m 2 or less, and 2 More than 5.0g / m 2 or less, 3.0 g / m 2 More than 4.0g / m 2 It may be the following.
[0039] <Barrier layer> The barrier layer 13 has a water vapor barrier property that prevents moisture from penetrating into the inside of the electricity storage device. The barrier layer 13 may also have extensibility for deep drawing. As the barrier layer 13, for example, various metal foils such as aluminum, stainless steel, copper, etc., or metal vapor deposition films, inorganic oxide vapor deposition films, carbon-containing inorganic oxide vapor deposition films, films provided with these vapor deposition films, etc. can be used. As the film provided with the vapor deposition film, for example, an aluminum vapor deposition film or an inorganic oxide vapor deposition film can be used. These can be used alone or in combination of two or more. As the barrier layer 13, a metal foil is preferable, and an aluminum foil or a stainless steel foil is more preferable in terms of mass (specific gravity), barrier properties such as moisture resistance, processability, and cost.
[0040] As the aluminum foil, a soft aluminum foil that has been annealed can be preferably used in terms of imparting desired ductility during molding. In order to impart further pinhole resistance and ductility during molding, it is more preferable to use an aluminum foil containing iron. The content of iron in the aluminum foil is preferably 0.1% by mass or more and 9.0% by mass or less, and more preferably 0.5% by mass or more and 2.0% by mass or less, based on 100% by mass of the aluminum foil. When the iron content is 0.1% by mass or more, an exterior material 10 having better pinhole resistance and ductility can be obtained. When the iron content is 9.0% by mass or less, an exterior material 10 having better flexibility can be obtained. As the aluminum foil, an untreated aluminum foil may be used, but it is preferable to use an aluminum foil that has been degreased in terms of imparting corrosion resistance. When the aluminum foil is degreased, the degreased treatment may be performed on only one side of the aluminum foil, or on both sides.
[0041] The thickness of the barrier layer 13 is not particularly limited, but taking into consideration the barrier properties, pinhole resistance, and processability, it is preferably from 9 μm to 200 μm, more preferably from 15 μm to 100 μm, even more preferably from 30 μm to 80 μm, and particularly preferably from 40 μm to 60 μm.
[0042] <First and second corrosion prevention treatment layers> The first and second corrosion prevention layers 14a and 14b are layers provided to prevent corrosion of the metal foil (metal foil layer) constituting the barrier layer 13. The first corrosion prevention layer 14a plays a role in increasing the adhesion between the barrier layer 13 and the first adhesive layer 12a. The second corrosion prevention layer 14b plays a role in increasing the adhesion between the barrier layer 13 and the thermal adhesive resin layer 15. The first corrosion prevention layer 14a and the second corrosion prevention layer 14b may be layers of the same configuration or layers of different configurations. The first and second corrosion prevention layers 14a and 14b (hereinafter also simply referred to as "corrosion prevention layers 14a and 14b") are formed, for example, by degreasing treatment, hydrothermal conversion treatment, anodizing treatment, chemical conversion treatment, or a combination of these treatments.
[0043] Examples of the degreasing treatment include acid degreasing and alkaline degreasing. Examples of the acid degreasing include a method using an inorganic acid such as sulfuric acid, nitric acid, hydrochloric acid, or hydrofluoric acid alone or a mixture of these. In addition, in the acid degreasing, it is preferable to use an acid degreasing agent in which a fluorine-containing compound such as monosodium ammonium difluoride is dissolved in the inorganic acid. In this case, the degreasing effect of aluminum can be obtained, especially when an aluminum foil is used for the barrier layer 13. Furthermore, the acid degreasing agent can form a fluoride of aluminum, which is a passive state, and is effective in terms of corrosion resistance. Examples of the alkaline degreasing include a method using sodium hydroxide or the like.
[0044] An example of the hydrothermal modification treatment is boehmite treatment in which an aluminum foil is immersed in boiling water containing triethanolamine. An example of the anodization treatment is alumite treatment.
[0045] The chemical conversion treatment may be of the immersion type or the coating type. Examples of the immersion type chemical conversion treatment include chromate treatment, zirconium treatment, titanium treatment, vanadium treatment, molybdenum treatment, calcium phosphate treatment, strontium hydroxide treatment, cerium treatment, ruthenium treatment, and various chemical conversion treatments consisting of a mixture of these. On the other hand, examples of the coating type chemical conversion treatment include a method in which a coating agent having corrosion prevention properties is applied onto the barrier layer 13.
[0046] When forming at least a part of the corrosion prevention layer by any of these corrosion prevention treatments, namely, hydrothermal conversion treatment, anodizing treatment, and chemical conversion treatment, it is preferable to perform the above-mentioned degreasing treatment in advance. When using a degreased metal foil, such as a metal foil that has been subjected to an annealing process, as the barrier layer 13, there is no need to perform a degreasing treatment again in forming the corrosion prevention layers 14a and 14b.
[0047] The coating agent used in the spray-type chemical conversion treatment preferably contains trivalent chromium. The coating agent may also contain at least one polymer selected from the group consisting of cationic polymers and anionic polymers, which will be described later.
[0048] Among the above treatments, particularly hydrothermal conversion treatment and anodization treatment dissolve the aluminum foil surface with a treatment agent to form aluminum compounds (boehmite, alumite) with excellent corrosion resistance. Therefore, a form in which a bicontinuous structure is formed from the barrier layer 13 using the aluminum foil to the corrosion prevention treatment layers 14a, 14b is obtained, so the above treatments are included in the definition of chemical conversion treatment. On the other hand, as described later, it is also possible to form the corrosion prevention treatment layers 14a, 14b only by a pure coating method that is not included in the definition of chemical conversion treatment. As an example of this method, a method using a sol of a rare earth element oxide such as cerium oxide with an average particle size of 100 nm or less can be mentioned, which has an aluminum corrosion prevention effect (inhibitor effect) and is also environmentally friendly. By using this method, it is possible to impart a corrosion prevention effect to metal foils such as aluminum foils even with a general coating method.
[0049] Examples of the rare earth element oxide sol include sols using various solvents such as water-based, alcohol-based, hydrocarbon-based, ketone-based, ester-based, ether-based, etc. Among these, water-based sols are preferred.
[0050] In order to stabilize the dispersion of the rare earth element oxide sol, inorganic acids such as nitric acid, hydrochloric acid, phosphoric acid, etc. or their salts, and organic acids such as acetic acid, malic acid, ascorbic acid, lactic acid, etc. are usually used as dispersion stabilizers. Among these dispersion stabilizers, phosphoric acid in particular is expected to provide the following effects (1) to (4) in the exterior packaging material 10. (1) Dispersion stabilization of sol (2) Improved adhesion to the barrier layer 13 by utilizing the aluminum chelating ability of phosphoric acid (3) Imparting corrosion resistance by capturing aluminum ions (passivation) (4) The dehydration and condensation of phosphoric acid occurs easily even at low temperatures, improving the cohesive strength of the corrosion prevention treatment layers (oxide layers) 14a and 14b.
[0051] The corrosion prevention layers 14a and 14b formed from the rare earth oxide sol are aggregates of inorganic particles, and therefore may lose their cohesive strength even after the drying and curing process. Therefore, it is preferable that the corrosion prevention layers 14a and 14b in this case are compounded with an anionic polymer or a cationic polymer to compensate for the cohesive strength.
[0052] The corrosion prevention treatment layers 14a, 14b are not limited to the above-mentioned layers. For example, they may be formed using a treatment agent in which phosphoric acid and a chromium compound are mixed with a resin binder (such as aminophenol), as in the case of coating-type chromate, which is a known technology. By using this treatment agent, a layer having both corrosion prevention function and adhesion can be formed. In addition, although it is necessary to consider the stability of the coating liquid, a coating agent in which a rare earth oxide sol and a polycationic polymer or a polyanionic polymer are mixed in advance into a one-component solution can be used to form a layer having both corrosion prevention function and adhesion.
[0053] The mass per unit area of the corrosion prevention treatment layers 14a and 14b is 0.005 g / m2 regardless of whether the layer has a multi-layer structure or a single-layer structure. 2 More than 0.200g / m 2 It is preferable that the content is 0.010 g / m or less. 2 More than 0.100g / m 2 It is more preferable that the mass per unit area is 0.005 g / m or less. 2 If the mass per unit area is 0.200 g / m or more, it is easy to impart a corrosion prevention function to the barrier layer 13. 2 Even if the thickness exceeds 100 mm, the corrosion prevention function does not change much. On the other hand, when a rare earth oxide sol is used, if the coating is thick, the heat curing during drying may be insufficient, which may result in a decrease in cohesive force. The thickness of the corrosion prevention layers 14a and 14b can be calculated from their specific gravity.
[0054] From the viewpoint of easily maintaining adhesion between the sealant layer 16 and the barrier layer 13, the corrosion prevention treatment layers 14a, 14b may be in an embodiment containing, for example, cerium oxide, 1 part by mass or more and 100 parts by mass or less of phosphoric acid or a phosphate salt per 100 parts by mass of the cerium oxide, and a cationic polymer, or may be formed by subjecting the barrier layer 13 to a chemical conversion treatment, or may be formed by subjecting the barrier layer 13 to a chemical conversion treatment and contain a cationic polymer.
[0055] <Sealant layer and thermal adhesive resin layer> The sealant layer 16 is a layer that imparts heat sealing properties to the exterior material 10, and is a layer that is placed on the inside and heat sealed (thermally fused) when assembling the electricity storage device. The thermal adhesive resin layer 15 is a layer that bonds the sealant layer 16 and the barrier layer 13, and contains an adhesive resin.
[0056] In one embodiment, the sealant layer 16 includes a polypropylene-based resin as a base resin. The polypropylene-based resin is a resin obtained from a polymerized monomer including propylene. Examples of the polypropylene-based resin include homopolypropylene, block polypropylene, and random polypropylene. These may be used alone or in combination of two or more. From the viewpoint of stiffness of the sealant layer 16, the polypropylene-based resin may include at least one of homopolypropylene and block polypropylene.
[0057] The content of the polypropylene resin in the sealant layer 16 is not particularly limited and is, for example, 30% by mass or more and 100% by mass or less. From the viewpoint of stiffness of the sealant layer 16, the content may be 50% by mass or more and 95% by mass or less, or 70% by mass or more and 90% by mass or less.
[0058] The sealant layer 16 may contain, in addition to the base resin, an additive resin containing a polyethylene resin, or a block copolymer compatible with a polypropylene resin. The polyethylene resin is a resin obtained from a polymer monomer containing ethylene, and serves to impart softness (stress relaxation properties). Examples of the polyethylene resin include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and a polyethylene elastomer. These may be used alone or in combination of two or more. Since the polyethylene resin can impart softness in particular, it is preferable that the polyethylene elastomer is included. The block copolymer compatible with a polypropylene resin is only required to be compatible with at least a polypropylene resin, and is, for example, a type of compatibilizer described later.
[0059] The polyethylene elastomer may be an elastomer having an α-olefin as a comonomer. Specifically, such a polyethylene elastomer may be a compound obtained by copolymerizing ethylene with at least one α-olefin selected from 1-butene, 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene.
[0060] When the sealant layer 16 contains a polyethylene-based resin as an added resin, the content of the polyethylene-based resin in the sealant layer 16 is not particularly limited, and is, for example, 1% by mass or more and 70% by mass or less. From the viewpoint of stiffness of the sealant layer 16, the content may be 5% by mass or more and 50% by mass or less, 10% by mass or more and 30% by mass or less, or 10% by mass or more and 20% by mass or less. When the sealant layer 16 contains a block copolymer that is compatible with a polypropylene-based resin, the content of the block copolymer in the sealant layer 16 is not particularly limited, and is, for example, 1% by mass or more and 70% by mass or less. From the viewpoint of stiffness of the sealant layer 16, the content may be 5% by mass or more and 50% by mass or less, 10% by mass or more and 30% by mass or less, or 10% by mass or more and 20% by mass or less.
[0061] The sealant layer 16 may contain the above-mentioned additive resin and a compatibilizer in addition to the base resin. The compatibilizer plays a role of efficiently imparting softness by finely dispersing the polyethylene resin in the base resin made of the polypropylene resin. In one embodiment, the compatibilizer has a portion compatible with the polypropylene resin (hereinafter also referred to as the "PP compatible portion") and a portion compatible with the polyethylene resin (hereinafter also referred to as the "PE compatible portion"). Specific examples of the compatibilizer include a graft copolymer in which the PP compatible portion is the main chain and the PE compatible portion is the side chain, a graft copolymer in which the PE compatible portion is the main chain and the PP compatible portion is the side chain, and a block copolymer in which the PP compatible portion and the PE compatible portion each exist as a block. From the viewpoint of improving the dispersibility of the compatibilizer, the compatibilizer may be a block copolymer in which at least the PP compatible portion exists as a block, a block copolymer in which the PP compatible portion and the PE compatible portion each exist as a block, and the like. Examples of such block copolymers include block copolymers of polypropylene and polyethylene (PP·PE block copolymers), block copolymers of polyethylene and polyethylenebutylene (PE·PE-butylene block copolymers), etc. In the PE·PE-butylene block copolymers, the butylene portion corresponds to the PP compatible portion.
[0062] The content of the compatibilizer in the sealant layer 16 is not particularly limited and is, for example, 1% by mass or more and 50% by mass or less. From the viewpoint of stiffness of the sealant layer 16, the content may be 2% by mass or more and 30% by mass or less, 5% by mass or more and 15% by mass or less, or 6% by mass or more and 10% by mass or less.
[0063] The total content of the additive resin containing the polyethylene resin and the compatibilizer in the sealant layer 16 may be from 1% by mass to 70% by mass, from 2% by mass to 50% by mass, or from 5% by mass to 30% by mass.
[0064] The mass ratio of the compatibilizer to the additive resin containing a polyethylene resin is, for example, 5:1 to 1:5 (additive resin containing a polyethylene resin: compatibilizer). The mass ratio may be 2:1 to 1:4, or 1:1.1 to 1:3.
[0065] The sealant layer 16 may contain other additive components as necessary, such as slip agents, antiblocking agents, antioxidants, light stabilizers, crystal nucleating agents, flame retardants, etc. The content of these additive components is, for example, 5% by mass or less, assuming that the total mass of the sealant layer 16 is 100% by mass.
[0066] The thermal adhesive resin layer 15 is not particularly limited as long as it contains a resin that bonds the sealant layer 16 and the barrier layer 13, and examples of such resins include acid-modified polyolefin resins.
[0067] The acid-modified polyolefin resin may be a polyolefin resin modified with maleic anhydride, carboxylic acid, sulfonic acid, or a derivative thereof. The acid-modified polyolefin resin may be, for example, a graft copolymer, a block copolymer, or a random copolymer. From the viewpoint of adhesion to the barrier layer 13, the acid-modified polyolefin resin is preferably a polyolefin resin graft-modified with maleic anhydride.
[0068] The thermal adhesive resin layer 15 may contain various additives, such as various compatible and incompatible elastomers, flame retardants, slip agents, antiblocking agents, antioxidants, light stabilizers, crystal nucleating agents, and tackifiers, as necessary.
[0069] The ratio of the thickness of the sealant layer 16 to the thickness of the thermal adhesive resin layer 15 (thickness of sealant layer 16 / thickness of thermal adhesive resin layer 15) is preferably 1 or more, more preferably 1.1 or more, and even more preferably 1.5 or more. The ratio of the thickness of the sealant layer 16 to the thickness of the thermal adhesive resin layer 15 (thickness of sealant layer 16 / thickness of thermal adhesive resin layer 15) is preferably 10 or less, more preferably 3 or less, and even more preferably 2.2 or less.
[0070] As described later, since the sealant layer 16 and the thermal adhesive resin layer 15 are formed at the same time, it is difficult to separate the sealant layer 16 and the thermal adhesive resin layer 15. Therefore, in one embodiment, the physical properties of the innermost layer of the packaging material 10 are considered to be the physical properties of a laminate of the sealant layer 16 and the thermal adhesive resin layer 15. The total thickness of the sealant layer 16 and the thermal adhesive resin layer 15 (i.e., the thickness of the laminate) is greater than the thickness of the base material layer 11, which is the outermost layer of the packaging material 10, and is 30 μm or more and 120 μm or less. The thickness of the laminate may be 45 μm or more and 100 μm or less, 65 μm or more and 85 μm or less, or 70 μm or more and 80 μm or less. By having the total thickness of the sealant layer 16 and the thermal adhesive resin layer 15 within the above range, it is easy to control the loop stiffness value of the laminate to a suitable range. In addition, since the occurrence of pinholes in the sealant layer 16 can be suppressed, the risk of breakage of the packaging material 10 can be reduced. The loop stiffness value of the laminate is, for example, 10 mN or more and 80 mN or less. The loop stiffness value of the laminate may be greater than the loop stiffness value of the base layer 11. The loop stiffness value may be 15 mN or more, 25 mN or more, 35 mN or more, 40 mN or more, 80 mN or less, 70 mN or less, 60 mN or less, 50 mN or less, or 45 mN or less.
[0071] In one embodiment, when the laminate of the sealant layer 16 and the thermal adhesive resin layer 15 is (I) and the base layer 11 is (II), the ratio (I / II) of the thicknesses of (I) and (II) is 1.0 or more and 8.0 or less. In addition, the ratio (I / II) of the loop stiffness values of (I) and (II) is, for example, 1.0 or more and 15 or less. In this case, the balance between the hardness (stiffness) of (I) and the hardness (stiffness) of (II) is good. Therefore, when pressure is applied from the base layer 11 toward the sealant layer 16 with the sealant layer 16 in close contact with the electricity storage device, the distribution of the pressure can be made uniform at the stage of transmission to the electricity storage device.
[0072] The ratio (I / II) of the thickness of (I) to (II) may be 1.5 to 6.5, 2.0 to 5.0, or 2.3 to 3.2. The ratio (I / II) of the loop stiffness value of (I) to (II) may be 2.5 to 11.0, 3.0 to 11.0, 3.5 to 10, 7.0 to 10, 7.5 to 9.0, 8.0 to 10.0, or 8.0 to 8.7.
[0073] Fig. 2 is a perspective view showing an electricity storage device according to an embodiment of the present disclosure. As shown in Fig. 2, an all-solid-state battery 50 as an electricity storage device includes an electricity storage element 52, two metal terminals (current extraction terminals) 53 for extracting current from the electricity storage element 52 to the outside, and an exterior bag 54 for housing the electricity storage element 52 in an airtight state.
[0074] The exterior bag 54 is formed using the exterior material 10 to have a bag main body 54a and a seal portion 54b provided on the bag main body 54a, and is used as a container for accommodating the energy storage element 52. In the exterior material 10, the base material layer 11 is the outermost layer, and the sealant layer 16 is the innermost layer. That is, the exterior bag 54 can accommodate the energy storage element 52 inside by folding one exterior material 10 in half and heat-sealing the peripheral portions, or by stacking two exterior materials 10 and heat-sealing the peripheral portions, so that the base material layer 11 is on the outside of the all-solid-state battery 50 and the sealant layer 16 is on the inside of the all-solid-state battery 50.
[0075] Metal terminal 53 is sandwiched by exterior bag 54 with sealant layer 16 on the inside. Metal terminal 53 may be sandwiched by exterior bag 54 via tab sealant. Metal terminal 53 is a part of the current collector taken out to the outside of exterior material 10, and is made of metal foil such as copper foil or aluminum foil.
[0076] The energy storage element 52 has a pair of electrodes and a solid electrolyte sandwiched between the pair of electrodes. One of the pair of electrodes is a positive electrode, and the other is a negative electrode. Examples of the solid electrolyte include a sulfide-based solid electrolyte and an oxide-based solid electrolyte.
[0077] [Exterior material manufacturing method] Next, there will be described an example of a method for manufacturing the exterior packaging material 10 shown in Fig. 1. Note that the method for manufacturing the exterior packaging material 10 is not limited to the following method.
[0078] A manufacturing method of an exterior material 10 of one embodiment is roughly composed of a step of providing corrosion prevention treatment layers 14a, 14b on a barrier layer 13, a step of bonding the base material layer 11 and the barrier layer 13 using a first adhesive layer 12a, a step of further laminating a thermal adhesive resin layer 15 and a sealant layer 16 on the surface of the barrier layer 13 facing the corrosion prevention treatment layer 14b, and a step of performing an aging treatment, if necessary.
[0079] (Laminating process of corrosion prevention treatment layer onto barrier layer) This step is a step of forming the corrosion prevention treatment layers 14a, 14b on the barrier layer 13. As described above, examples of the method include subjecting the barrier layer 13 to a degreasing treatment, a hydrothermal conversion treatment, an anodizing treatment, or a chemical conversion treatment, or applying a coating agent having corrosion prevention properties.
[0080] Furthermore, when the corrosion prevention treatment layers 14a, 14b are multiple layers, for example, a coating liquid (coating agent) constituting the lower corrosion prevention treatment layer (barrier layer 13 side) may be applied to the barrier layer 13 and baked to form a first layer, and then a coating liquid (coating agent) constituting the upper corrosion prevention treatment layer may be applied to the first layer and baked to form a second layer.
[0081] The degreasing treatment may be performed by spraying or immersion. The hydrothermal conversion treatment and anodizing treatment may be performed by immersion. The chemical conversion treatment may be performed by an appropriate method such as immersion, spraying, or coating, depending on the type of chemical conversion treatment.
[0082] Regarding the coating method of the coating agent having corrosion prevention properties, various methods such as gravure coating, reverse coating, roll coating, bar coating, etc. can be used.
[0083] As described above, the various treatments for the barrier layer 13 may be performed on either one or both sides of the metal foil, but in the case of one-sided treatment, the treated side is preferably the side on which the sealant layer 16 is laminated. If required, the surface of the base layer 11 may also be subjected to the above treatments.
[0084] The coating amount of the coating agent for forming the first layer and the second layer is 0.005 g / m 2 More than 0.200g / m 2 It is preferable that the content is 0.010 g / m or less. 2 More than 0.100g / m 2 It is more preferable that:
[0085] Furthermore, when dry curing is required, it can be performed at a base material temperature in the range of 60° C. or more and 300° C. or less, depending on the drying conditions of the corrosion prevention treatment layers 14a, 14b used.
[0086] (Laminating process of substrate layer and barrier layer) This step is a step of bonding the barrier layer 13 provided with the anti-corrosion treatment layers 14a and 14b to the base material layer 11 via the first adhesive layer 12a. The base material layer 11 is bonded to the surface of the barrier layer 13 on the side of the anti-corrosion treatment layer 14a. The bonding method may be dry lamination, non-solvent lamination, wet lamination, or the like, and the two are bonded together using the material constituting the first adhesive layer 12a described above. The first adhesive layer 12a is preferably applied in a dry coating amount of 1 g / m. 2 More than 10g / m 2 The range is preferably 2 g / m 2 More than 7g / m 2 It is set within the following range.
[0087] (Lamination process of thermal adhesive resin layer and sealant layer) The lamination process of the thermal adhesive resin layer and the sealant layer is a process of forming the thermal adhesive resin layer 15 and the sealant layer 16 on the surface of the barrier layer 13 on the corrosion prevention treatment layer 14b side. The method includes a method of sand laminating the thermal adhesive resin layer 15 together with the sealant layer 16 using an extrusion laminator. Furthermore, lamination is also possible by a tandem lamination method in which the thermal adhesive resin layer 15 and the sealant layer 16 are extruded, or a co-extrusion method. In forming the thermal adhesive resin layer 15 and the sealant layer 16, for example, each component is blended so as to satisfy the above-mentioned configuration of the thermal adhesive resin layer 15 and the sealant layer 16. The thermal adhesive resin layer 15 is formed using a resin composition for forming a thermal adhesive resin layer containing the above-mentioned components of the thermal adhesive resin layer 15. The sealant layer 16 is formed using a resin composition for forming a sealant layer containing the above-mentioned components of the sealant layer 16.
[0088] By the lamination process of the thermal adhesive resin layer and the sealant layer, a laminated structure is obtained in which the layers are laminated in the following order: base layer 11 / first adhesive layer 12a / first corrosion prevention treatment layer 14a / barrier layer 13 / second corrosion prevention treatment layer 14b / thermal adhesive resin layer 15 / sealant layer 16, as shown in Figure 1.
[0089] The thermal adhesive resin layer 15 may be laminated by directly extruding the materials dry-blended to have the above-mentioned material composition using an extrusion laminator. Alternatively, the thermal adhesive resin layer 15 may be laminated by extruding the granulated material, which has been previously melt-blended using a melt kneading device such as a single-screw extruder, a twin-screw extruder, or a Brabender mixer, using an extrusion laminator.
[0090] The sealant layer 16 may be laminated by directly extruding a material obtained by dry blending the components of the resin composition for forming a sealant layer with an extrusion laminator. Alternatively, the thermal adhesive resin layer 15 and the sealant layer 16 may be laminated by a tandem lamination method in which the thermal adhesive resin layer 15 and the sealant layer 16 are extruded with an extrusion laminator using a granulated product obtained by melt blending in advance using a melt kneading device such as a single screw extruder, a twin screw extruder, or a Brabender mixer, or by a co-extrusion method. The thermal adhesive resin layer 15 and the sealant layer 16 may also be laminated by a method in which the sealant layer is formed in advance as a cast film using the resin composition for forming a sealant layer, and this sealant layer is sandwich-laminated with an adhesive resin. The forming speed (processing speed) of the thermal adhesive resin layer 15 and the sealant layer 16 can be, for example, 80 m / min or more from the viewpoint of productivity.
[0091] (Aging process) The aging treatment step is a step of aging (curing) the laminated structure. By aging the laminated structure, the adhesion between the base material layer 11 / the first adhesive layer 12a / the first corrosion prevention treatment layer 14a / the barrier layer 13 and the adhesion between the barrier layer 13 / the second corrosion prevention treatment layer 14b / the thermal adhesive resin layer 15 / the sealant layer 16 can be promoted. The aging temperature may be 80°C or more, 100°C or more, or 120°C or more, and may be 140°C or less, 150°C or less, or 160°C or less. The aging time may be 1 hour or more, 2 hours or more, or 3 hours or more, and may be 24 hours or less, 48 hours or less, or 72 hours or less.
[0092] In this manner, an exterior packaging material 10 according to one embodiment as shown in FIG. 1 can be manufactured.
[0093] The effects of the exterior material 10 according to one embodiment will be described below with reference to Figs. 3(a) and (b). Fig. 3(a) is a schematic cross-sectional view of a comparative exterior material pressed against a rigid body, and Fig. 3(b) is a schematic cross-sectional view of an exterior material for an electricity storage device according to one embodiment pressed against a rigid body. The comparative exterior material 100 shown in Fig. 3(a) is different from the exterior material 10 in that the ratio of the loop stiffness value of the laminate of the sealant layer 116 and the thermal adhesive resin layer 115 to the loop stiffness value of the base layer 11 is less than 1 or greater than 15. Therefore, the loop stiffness value of the base layer 11 and the loop stiffness value of the laminate are significantly different. For this reason, the stiffness of the laminate of the sealant layer 116 and the thermal adhesive resin layer 115, which are the innermost layers of the packaging material 100, is too low (i.e., too soft) or too high (i.e., too hard) compared to the stiffness of the base material layer 11, which is the outermost layer of the packaging material 100.
[0094] When the exterior material 100 including the laminate with too low stiffness is pressed against the rigid body 200, for example, the resin included in the sealant layer 116 easily flows. With this flow of the resin, the sealant layer 116 is deformed as shown in FIG. 3(a). This may cause the thickness of the sealant layer 116 and the like to vary greatly, and as a result, the rigid body 200 is likely to be pressurized non-uniformly via the exterior material 100. Here, since the above deformation is likely to occur in a high-temperature environment (for example, 70°C or higher), the above pressurization tends to be more likely to be non-uniform. On the other hand, when the exterior material 100 including the laminate with too high stiffness is pressed against the rigid body 200, force is likely to concentrate on a portion of the exterior material 100 that contacts the end 200a (pressurized end, see FIG. 3(a)) of the rigid body 200. Alternatively, the convex portion provided on the surface of the sealant layer 116 according to the unevenness of the base layer 11 is unlikely to deform, and force is likely to concentrate on the convex portion. Such concentration of force tends to cause the pressure applied to the rigid body 200 via the exterior material 100 to be localized. Therefore, not only when the stiffness is too low, but also when the stiffness is too high, the pressure applied to the rigid body via the exterior material tends to be uneven.
[0095] In contrast, in the exterior packaging material 10 according to one embodiment, when the laminate of the thermal adhesive resin layer 15 and the sealant layer 16 is (I) and the base material layer 11 is (II), the loop stiffness value of (I) is 10 mN or more and 80 mN or less, the loop stiffness value of (II) is 2 mN or more and 20 mN or less, the ratio (I / II) of the loop stiffness values of (I) and (II) is 1.0 or more and 15 or less, and the ratio (I / II) of the thicknesses of (I) and (II) is 1.0 or more and 8.0 or less. This allows the stiffness of the innermost layer in the exterior packaging material 10, the stiffness of the outermost layer in the exterior packaging material 10, and the balance between them to be set in appropriate ranges. As a result, as shown in FIG. 3(b), even when the rigid body 200 is pressed through the exterior packaging material 10 in a high-temperature environment, the exterior packaging material 10 is unlikely to deform excessively. Therefore, even when pressure is applied to the rigid body 200 via the outer packaging material 10 in a high-temperature environment, pressure can be applied to the rigid body 200 uniformly via the outer packaging material 10.
[0096] The loop stiffness value of the resin layer (substrate layer 11, sealant layer 16, etc.) in the exterior packaging material 10 can be adjusted, for example, by the layer thickness, the crystallinity of the resin, the type of resin, etc. In general, the loop stiffness value increases as the thickness of the resin layer increases. However, if the loop stiffness value is adjusted by simply adjusting the thickness of the resin layer, the thickness of the exterior packaging material may become excessive and the durability of the exterior packaging material may become insufficient. In contrast, in one embodiment, the thickness of the above (I) is 30 μm or more and 120 μm or less, and the thickness of the above (II) is 10 μm or more and 60 μm or less. In this case, the durability of the exterior packaging material 10 can be ensured while suppressing the thickness of the exterior packaging material 10. Therefore, even when pressure is applied in a high-temperature environment, for example, pinholes, breakage, etc. of the exterior packaging material 10 are unlikely to occur. In addition, the loop stiffness value of the above (I) and the loop stiffness value of the above (II) can be reliably set within the above range.
[0097] In one embodiment, the ratio (I / II) of the loop stiffness values of (I) and (II) may be 2.5 or more and 11.0 or less. In this case, the ratio (I / II) of the thicknesses of (I) and (II) may be 1.0 or more and 6.5 or less, the thickness of (I) may be 45 μm or more and 100 μm or less, and the thickness of (II) may be 15 μm or more and 50 μm or less. In this case, even when pressure is applied in a high-temperature environment, deformation of the exterior material 10 is well suppressed.
[0098] In one embodiment, the ratio (I / II) of the loop stiffness values of (I) and (II) may be 3.5 or more and 10.0 or less. In this case, the ratio (I / II) of the thicknesses of (I) and (II) may be 2.0 or more and 5.0 or less, the thickness of (I) may be 65 μm or more and 85 μm or less, and the thickness of (II) may be 20 μm or more and 40 μm or less. In this case, even when pressure is applied in a high-temperature environment, deformation of the exterior material 10 is more effectively suppressed.
[0099] In one embodiment, the sealant layer 16 includes a polypropylene-based resin as a base resin, and the polypropylene-based resin may be composed of homopropylene or block polypropylene. In this case, melting of the sealant layer 16 in a high-temperature environment can be suppressed.
[0100] In one embodiment, the sealant layer 16 may further contain an additive resin containing a polyethylene-based resin or a block copolymer that is compatible with the polypropylene-based resin. In this case, deformation of the exterior material 10 is further suppressed.
[0101] In one embodiment, the sealant layer 16 may further include an additive resin containing a polyethylene-based resin, and a compatibilizer having a portion compatible with the polypropylene-based resin and a portion compatible with the polyethylene-based resin. In this case, deformation of the exterior packaging material 10 is more effectively suppressed.
[0102] In one embodiment, the exterior material 10 may be an exterior material for an all-solid-state battery. In this case, even when the all-solid-state battery 50 is pressurized through the exterior material 10 in a high-temperature environment, the pressurization can be performed uniformly. This can satisfactorily improve the output of the all-solid-state battery 50. Therefore, the exterior material 10 can be highly suitable as an exterior material for the all-solid-state battery 50.
[0103] Hereinafter, an exterior material according to a modified example of the above embodiment will be described with reference to Fig. 4. In the modified example, the description that overlaps with the above embodiment will be omitted. Fig. 4 is a schematic cross-sectional view of an exterior material for an electricity storage device according to a modified example. As shown in Fig. 4, an exterior material 20 is an exterior material used for an electricity storage device, and includes a base layer 11, a barrier layer 13, a second adhesive layer 12b, and a sealant layer 16, which are laminated in this order.
[0104] In the exterior material 20, the barrier layer 13 has a first corrosion prevention treatment layer 14a on the base material layer 11 side via a first adhesive layer 12a, and has a second corrosion prevention treatment layer 14b on the sealant layer 16 side.
[0105] The exterior material 20 differs from the exterior material 10 in that a second adhesive layer 12b is used instead of the thermal adhesive resin layer 15. The thickness of the second adhesive layer 12b in the exterior material 20 is significantly smaller than the thickness of the sealant layer 16, and therefore has almost no effect on the physical properties of the sealant layer 16. Therefore, in the modified example, the sealant layer 16 is designated as (I) and the base material layer 11 is designated as (II). In the modified example, the ratio of the thickness of (I) to the thickness of (II) and the ratio of the loop stiffness value of (I) to the loop stiffness value of (II) are each within the same range as in the above embodiment.
[0106] <Second adhesive layer> The second adhesive layer 12b will now be described. The second adhesive layer 12b is a layer that bonds the barrier layer 13 and the sealant layer 16. For the second adhesive layer 12b, a general adhesive for bonding the barrier layer 13 and the sealant layer 16 can be used.
[0107] When a corrosion prevention treatment layer 14b is provided on the barrier layer 13 and the second corrosion prevention treatment layer 14b has a layer containing at least one polymer selected from the group consisting of the above-mentioned cationic polymers and anionic polymers, the second adhesive layer 12b is preferably a layer containing a compound (hereinafter also referred to as a "reactive compound") that is reactive with the above-mentioned polymer contained in the second corrosion prevention treatment layer 14b.
[0108] For example, when the second corrosion prevention treatment layer 14b contains a cationic polymer, the second adhesive layer 12b preferably contains a compound reactive with the cationic polymer. When the second corrosion prevention treatment layer 14b contains an anionic polymer, the second adhesive layer 12b preferably contains a compound reactive with the anionic polymer. When the second corrosion prevention treatment layer 14b contains a cationic polymer and an anionic polymer, the second adhesive layer 12b preferably contains a compound reactive with the cationic polymer and a compound reactive with the anionic polymer. However, the second adhesive layer 12b does not necessarily have to contain the above two types of compounds, and may contain a compound reactive with both the cationic polymer and the anionic polymer. Here, "reactive" means to form a covalent bond with the cationic polymer or the anionic polymer. The second adhesive layer 12b may further contain an acid-modified polyolefin resin.
[0109] The compound reactive with the cationic polymer may be at least one compound selected from the group consisting of a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxy group, and a compound having an oxazoline group.
[0110] Examples of the polyfunctional isocyanate compound, glycidyl compound, compound having a carboxy group, and compound having an oxazoline group include the polyfunctional isocyanate compound, glycidyl compound, compound having a carboxy group, and compound having an oxazoline group, which are exemplified above as crosslinking agents for forming a crosslinked structure from a cationic polymer. Among these, the polyfunctional isocyanate compound is preferred in terms of high reactivity with the cationic polymer and ease of forming a crosslinked structure.
[0111] The compound reactive with anionic polymers includes at least one compound selected from the group consisting of glycidyl compounds and compounds having oxazoline groups.These glycidyl compounds and compounds having oxazoline groups include the glycidyl compounds and compounds having oxazoline groups exemplified above as crosslinking agents for forming cationic polymers into crosslinked structures.Among these, glycidyl compounds are preferred because of their high reactivity with anionic polymers.
[0112] When the second adhesive layer 12b contains an acid-modified polyolefin resin, it is preferable that the reactive compound is also reactive with the acidic group in the acid-modified polyolefin resin (i.e., forms a covalent bond with the acidic group). This further enhances the adhesion to the second corrosion prevention treatment layer 14b. In addition, the acid-modified polyolefin resin has a crosslinked structure, which further improves the solvent resistance of the exterior material 20.
[0113] The content of the reactive compound is preferably from 1 to 10 times the equivalent of the acid group in the acid-modified polyolefin resin. If it is equal to or more than 10 times the equivalent, the reactive compound reacts sufficiently with the acid group in the acid-modified polyolefin resin. On the other hand, if it exceeds 10 times the equivalent, the crosslinking reaction with the acid-modified polyolefin resin is sufficiently saturated, so that there is a concern of the presence of unreacted substances and the deterioration of various performances. Therefore, for example, the content of the reactive compound is preferably 5 to 20 parts by mass (solid content ratio) per 100 parts by mass of the acid-modified polyolefin resin.
[0114] The acid-modified polyolefin resin is a polyolefin resin to which an acidic group has been introduced. Examples of the acidic group include a carboxyl group, a sulfonic acid group, and an acid anhydride group, and maleic anhydride groups and (meth)acrylic acid groups are particularly preferred. For example, the acid-modified polyolefin resin may be the same as the modified polyolefin resin used in the sealant layer 16.
[0115] The second adhesive layer 12b may contain various additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, and a tackifier.
[0116] The second adhesive layer 12b may contain, for example, an acid-modified polyolefin and at least one curing agent selected from the group consisting of a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxy group, a compound having an oxazoline group, and a carbodiimide compound, from the viewpoint of suppressing a decrease in heat seal strength when corrosive gases such as hydrogen sulfide or an electrolyte are involved and from the viewpoint of further suppressing a decrease in insulating properties. Examples of the carbodiimide compound include N,N'-di-o-toluylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-di-2,6-dimethylphenylcarbodiimide, N,N'-bis(2,6-diisopropylphenyl)carbodiimide, N,N'-dioctyldecylcarbodiimide, N-triyl-N'-cyclohexylcarbodiimide, N,N'-di-2,2-di-t-butylphenylcarbodiimide, N-triyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-di-cyclohexylcarbodiimide, and N,N'-di-p-toluylcarbodiimide.
[0117] In addition, as the adhesive for forming the second adhesive layer 12b, for example, a polyurethane adhesive obtained by blending polyester polyol made of hydrogenated dimer fatty acid and diol with polyisocyanate can be used. Examples of the adhesive include polyurethane resins obtained by reacting a bifunctional or higher isocyanate compound with a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol, and epoxy resins obtained by reacting an amine compound with a base material having an epoxy group. These are preferable from the viewpoint of heat resistance.
[0118] The thickness of the second adhesive layer 12b is not particularly limited, but from the viewpoint of obtaining the desired adhesive strength, processability, etc., it is preferably 1 μm or more and 10 μm or less, and more preferably 2 μm or more and 7 μm or less.
[0119] Next, a description will be given of an example of a method for manufacturing the exterior material 20 shown in Fig. 4. Note that the method for manufacturing the exterior material 20 is not limited to the following method.
[0120] The manufacturing method of the exterior material 20 according to the modified example is generally configured to include a step of providing the corrosion prevention treatment layers 14a, 14b on the barrier layer 13, a step of bonding the base material layer 11 and the barrier layer 13 with the first adhesive layer 12a, a step of bonding the sealant layer 16 to the side of the corrosion prevention treatment layer 14b of the barrier layer 13 via the second adhesive layer 12b to obtain a laminated structure, and a step of aging the obtained laminated structure, if necessary. The steps up to the step of bonding the base material layer 11 and the barrier layer 13 with the first adhesive layer 12a can be performed in the same manner as the manufacturing method of the exterior material 10 described above. The step of aging the obtained laminated structure can be performed in the same manner as the manufacturing method of the exterior material 10 described above.
[0121] (Lamination process of second adhesive layer and sealant layer) The lamination step of the second adhesive layer and the sealant layer is a step of obtaining a laminated structure by laminating the sealant layer 16 via the second adhesive layer 12b to the corrosion prevention treatment layer 14b side of the barrier layer 13. Examples of the lamination method include a wet process and dry lamination.
[0122] In the case of a wet process, a solution or dispersion of the adhesive constituting the second adhesive layer 12b is applied onto the corrosion prevention treatment layer 14b, and the solvent is removed at a predetermined temperature to form a dry film, or a baking process is performed as necessary after the dry film is formed. Then, the sealant layer 16 is laminated to produce the exterior material 20. Examples of the coating method include the various coating methods exemplified above. The preferred dry coating amount of the second adhesive layer 12b is the same as that of the first adhesive layer 12a.
[0123] In this case, the sealant layer 16 can be produced, for example, by a melt extrusion molding machine using a resin composition for forming a sealant layer containing the above-mentioned base resin, additive resin, and compatibilizer. In the melt extrusion molding machine, the processing speed can be set to 80 m / min or more from the viewpoint of productivity.
[0124] The exterior packaging material 20 according to the modified example described above also exerts the same effects as those of the above embodiment.
[0125] An exterior material for an electricity storage device according to one aspect of the present disclosure is as described in the following [1] to [9], and has been described in detail based on the above embodiment and the above modified example. [1] An exterior material for an electricity storage device comprising a base material layer, a barrier layer, a thermal adhesive resin layer or an adhesive layer, and a sealant layer, which are laminated in this order, wherein when the thermal adhesive resin layer and the sealant layer, or the sealant layer, are (I) and the base material layer is (II), the loop stiffness value of (I) is 10 mN or more and 80 mN or less, the loop stiffness value of (II) is 2 mN or more and 20 mN or less, the loop stiffness value ratio (I / II) of (I) to (II) is 1.0 or more and 15 or less, and the thickness ratio (I / II) of (I) to (II) is 1.0 or more and 8.0 or less. [2] The exterior packaging material for an electricity storage device according to [1], wherein the thickness of (I) is 30 μm or more and 120 μm or less, and the thickness of (II) is 10 μm or more and 60 μm or less. [3] The exterior material for an electricity storage device according to [1] or [2], wherein a ratio (I / II) of loop stiffness values of (I) and (II) is 2.5 or more and 11.0 or less. [4] The exterior material for an electricity storage device according to any one of [1] to [3], wherein a ratio (I / II) of loop stiffness values of the above (I) and the above (II) is 3.5 or more and 10 or less. [5] The exterior packaging material for an electricity storage device according to any one of [1] to [4], wherein the sealant layer contains a polypropylene-based resin as a base resin, and the polypropylene-based resin is composed of homopropylene or block polypropylene. [6] The exterior packaging material for an electricity storage device according to [5], wherein the sealant layer further contains an additive resin containing a polyethylene-based resin, or a block copolymer exhibiting compatibility with the polypropylene-based resin. [7] The exterior material for an electricity storage device according to [5], wherein the sealant layer further contains an additive resin containing a polyethylene-based resin, and a compatibilizer having a portion compatible with the polypropylene-based resin and a portion compatible with the polyethylene-based resin. [8] The exterior packaging material for an electricity storage device according to [7], wherein the compatibilizer contains a block copolymer of polypropylene and polyethylene, or a block copolymer of polyethylene and polyethylenebutylene. [9] The exterior material for an electricity storage device according to any one of [1] to [8], which is an exterior material for an all-solid-state battery.
[0126] However, one aspect of the present disclosure is not limited to the above embodiment, the above modification, and the above [1] to [9]. One aspect of the present disclosure can be further modified within the scope of the gist. For example, in the above embodiment and the above modification, a corrosion prevention treatment layer is provided on each of both sides of the barrier layer, but this is not limited. The exterior material may have only one corrosion prevention treatment layer, or may not have a corrosion prevention treatment layer.
[0127] The exterior material for an electric storage device of the present disclosure can be used as an exterior material for an electric storage device such as a secondary battery such as a lithium ion battery, a nickel hydrogen battery, and a lead storage battery, and an electrochemical capacitor such as an electric double layer capacitor, but the exterior material for an electric storage device of the present disclosure can be particularly suitably used as an exterior material for an electric storage device made of an all-solid-state battery. The exterior material for an electric storage device has an adjusted loop stiffness value ratio between a thermal adhesive resin layer and a sealant layer provided in the exterior material, or between a sealant layer and a base material layer. Therefore, when the exterior material for an electric storage device is used as an exterior material for an all-solid-state battery provided with an electric storage element, and the electric storage element is pressurized through the exterior material, not only is the exterior material difficult to deform due to heat and pressure, but the presence of a portion where the pressure is large and a portion where the pressure is small on the pressurized surface of the electric storage element is suppressed, and the pressurized surface of the electric storage element is uniformly pressurized. As a result, the all-solid-state battery can be operated efficiently. EXAMPLES
[0128] The present disclosure will be described more specifically below based on examples, but the present disclosure is not limited to the following examples.
[0129] [Materials used] The materials used as the barrier layer, the thermal adhesive resin layer, the first adhesive layer, the second adhesive layer, the material for forming the first corrosion prevention treatment layer, and the material for forming the second corrosion prevention treatment layer are as follows.
[0130] <Barrier layer (thickness 40 μm)> Annealed and degreased soft aluminum foil (manufactured by Toyo Aluminum, "8079 material")
[0131] <Resin composition for forming a thermal adhesive resin layer> A resin composition for forming a thermal adhesive resin layer, which is a dry blend of a maleic anhydride-modified homopolypropylene and a polyethylene-based elastomer.
[0132] <First adhesive layer (mass per unit area: 4.0 g / m2 ) to form the first adhesive> An adhesive (first adhesive) prepared by mixing polyester polyol (manufactured by Showa Denko Materials Co., Ltd., product name: Teslac 2505-63, hydroxyl value: 7 to 11 mgKOH / g) and a nurate of isophorone diisocyanate (manufactured by Mitsui Chemicals, Inc., product name: Takenate 600) so that the NCO / OH ratio is 20.0, and diluting with ethyl acetate to a solid content of 26 mass%.
[0133] <Second adhesive layer (mass per unit area 3.0 g / m 2 ) to form a second adhesive> An adhesive (second adhesive) made by mixing 100 parts by mass of acid-modified polyolefin resin dissolved in toluene with 10 parts by mass (solid content ratio) of a polyisocyanate compound with an isocyanurate structure.
[0134] <Material for forming first corrosion prevention treatment layer and material for forming second corrosion prevention treatment layer> The first corrosion prevention treatment layer forming material (substrate layer side) and the second corrosion prevention treatment layer forming material (sealant layer side) are as follows (CL-1) and (CL-2). (CL-1): Sodium polyphosphate-stabilized cerium oxide sol adjusted to a solid content of 10% by mass using distilled water as a solvent. (CL-2): A composition prepared by using distilled water as a solvent and adjusting the solid content concentration to 5% by mass.
[0135] The sodium polyphosphate-stabilized cerium oxide sol was prepared by blending 100 parts by mass of cerium oxide with 10 parts by mass of sodium salt of phosphoric acid. In the composition, the mass ratio of "polyallylamine (manufactured by Nitto Boseki Co., Ltd.)" to "polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation)" was 90:10.
[0136] <Sealant layer> The base resin, additive resin, and compatibilizer used in the sealant layer are as shown in the following Table 1. In the following Table 1, "PP" stands for "polypropylene" and "PE" stands for "polyethylene."
[0137] [Table 1]
[0138] As the substrate layer, the following (D1) or (D2) was used. (D1): Polyethylene terephthalate film with corona treatment on one side (D2): Nylon film
[0139] [Creating exterior materials] Example 1 First, a first and a second corrosion prevention treatment layer were provided on the barrier layer. Specifically, (CL-1) was applied to both surfaces of the barrier layer in a dry coating amount of 70 mg / m 2 The layer was then coated by microgravure coating so that the thickness of the layer was 200 mm, and the layer was baked at 200° C. in a drying unit. Next, (CL-2) was applied onto the layer obtained in a dry coating amount of 20 mg / m 2 By applying the coating by microgravure coating so that the above-mentioned coating conditions were satisfied, a composite layer consisting of (CL-1) and (CL-2) was formed as the first and second corrosion prevention treatment layers. This composite layer exhibits corrosion prevention performance by combining the two types of materials, (CL-1) and (CL-2).
[0140] Next, the first corrosion prevention layer side of the barrier layer provided with the first corrosion prevention layer and the second corrosion prevention layer was attached to the substrate layer by dry lamination using the first adhesive to form the first adhesive layer, to obtain a first laminate (substrate layer / first adhesive layer / first corrosion prevention layer / barrier layer / second corrosion prevention layer). Specifically, the first adhesive was applied to the surface of the barrier layer facing the first corrosion prevention layer so that the thickness after curing was 4 μm, and the layer was dried at 80° C. for 1 minute, and then laminated with the substrate layer and aged at 80° C. for 120 hours to obtain a first laminate. At this time, the substrate layer shown in Table 2 was used as the substrate layer.
[0141] Next, the first laminate was set at the unwinding section of the extrusion laminator. On the second corrosion prevention treatment layer of the first laminate, a thermal adhesive resin layer and a sealant layer were laminated in this order by co-extrusion from a T-die under processing conditions of 270 ° C. and 80 m / min, to obtain an exterior material (a laminate of a base layer / a first adhesive layer / a first corrosion prevention treatment layer / a barrier layer / a second corrosion prevention treatment layer / a thermal adhesive resin layer / a sealant layer). At this time, the thicknesses of the thermal adhesive resin layer and the sealant layer were 25 μm and 55 μm, respectively. At this time, for the sealant layer, a resin composition for forming a sealant layer, which is obtained by dry-blending the base resin, the additive resin, and the compatibilizer shown in Table 2 in advance so as to have the content shown in Table 2, was prepared, and this resin composition was used. In addition, for the thermal adhesive resin layer, a resin composition for forming a thermal adhesive resin layer was prepared, and this resin composition was used.
[0142] (Examples 2 to 8) Except for using a sealant layer with a composition as shown in Table 2, the same procedure as in Example 1 was followed to prepare an exterior material.
[0143] Example 9 An exterior material was produced in the same manner as in Example 1, except that the thickness of the substrate layer was changed to 35 μm.
[0144] Example 10 A first laminate (substrate layer / first adhesive layer / first corrosion prevention treatment layer / barrier layer / second corrosion prevention treatment layer) was obtained in the same manner as in Example 1. A sealant layer was formed under the same processing conditions as in Example 1. Next, a sealant layer shown in Table 2 was attached to the second corrosion prevention treatment layer of the first laminate by dry lamination using a second adhesive for forming a second adhesive layer. At this time, lamination of the first laminate and the sealant layer was performed by applying the second adhesive to the second corrosion prevention treatment layer so that the thickness after drying was 3 μm, drying at 80 ° C. for 1 minute, laminating with the sealant layer, and aging at 120 ° C. for 3 hours. In this manner, an exterior material (a laminate of substrate layer / first adhesive layer / first corrosion prevention treatment layer / barrier layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) was produced.
[0145] Comparative Example 1 Except for using the materials for the base layer and the compositions for the sealant layer as shown in Table 2, the same procedure as in Example 1 was followed to prepare exterior materials.
[0146] Comparative Example 2 Except for using the materials for the base material layer as shown in Table 2, exterior materials were produced by the dry lamination method in the same manner as in Example 10.
[0147] Comparative Example 3 Except for using a sealant layer with a composition as shown in Table 2, an exterior material was produced in the same manner as in Example 9.
[0148] Comparative Example 4 An exterior material was produced in the same manner as in Example 1, except that the thicknesses of the thermal adhesive resin layer and the sealant layer were changed to 5 μm and 15 μm, respectively.
[0149] <Loop stiffness value> The loop stiffness value was measured using a loop stiffness tester DA-S manufactured by Toyo Seiki Seisakusho Co., Ltd. The loop stiffness value was specifically measured as follows. First, a test film having a width direction (TD direction) of 15 mm and a flow direction (MD direction) of 200 mm was prepared. Next, both ends of the test film were fixed with chucks to form a loop with a loop length of 85 mm, and this loop was compressed with an indenter under the conditions of a compression speed of 3.3 mm / min, a compression time of 3 seconds, and a compression distance of 20 mm, and the load of the indenter at that time was measured. The maximum load measured in this test was adopted as the loop stiffness value. The compression distance represents the distance when the indenter and the chuck are closest to each other. Table 2 shows the measurement results of the loop stiffness values of the thermal adhesive resin layer and the sealant layer in Examples 1 to 9 and Comparative Examples 1 and 3 to 4, the measurement results of the loop stiffness value of the sealant layer in Example 10 and Comparative Example 2, and the measurement results of the loop stiffness value of the base layer in Examples 1 to 10 and Comparative Examples 1 to 4.
[0150] <Deformation rate of exterior materials> The deformation rate was evaluated for the exterior materials obtained in Examples 1 to 10 and Comparative Examples 1 to 4. Specifically, first, the exterior material was placed on a SUS plate. At this time, the exterior material was placed so that the sealant layer was in contact with the SUS plate. Next, a SUS block having a bottom surface with a short side of 10 mm and a long side of 40 mm was placed on the exterior material. At this time, the SUS block was placed so that the base layer was in contact with the bottom surface of the SUS block. The SUS plate and the SUS block can each be heated by a heater. Next, while the SUS plate and the SUS block were each maintained at 100°C, the SUS block pressed the exterior material with a force of 5 MPa for 1 hour along the lamination direction of the SUS plate, exterior material, and SUS block. Thereafter, the exterior material after pressing was solidified using an epoxy resin, and the cross section was exposed with a grinder, and then the cross section of the exterior material was observed with a microscope. The thickness (X) of the thermal adhesive resin layer and sealant layer of the exterior packaging materials in Examples 1 to 9 and Comparative Examples 1, 3 to 4, or the sealant layer of the exterior packaging materials in Example 10 and Comparative Example 2, at the location where the thickness change was greatest, was measured. The deformation rate ((XY) / Y×100) was calculated from the thickness (Y) of the thermal adhesive resin layer and sealant layer of the exterior packaging materials in Examples 1 to 9 and Comparative Examples 1, 3 to 4, or the sealant layer of the exterior packaging materials in Example 10 and Comparative Example 2, before heating and pressurization. The deformation rate was evaluated based on the following evaluation criteria. The evaluation results are shown in Table 2. [Evaluation Criteria] A: When the deformation rate is less than 5% B: When the deformation rate is 5% or more but less than 10% C: When the deformation rate is 10% or more but less than 15% D: When the deformation rate is 15% or more
[0151] [Table 2] [Explanation of symbols]
[0152] Reference Signs List 10, 20, 100...outer packaging material (outer packaging material for electricity storage device), 11...base material layer, 12a...first adhesive layer, 12b...second adhesive layer (adhesive layer), 13...barrier layer, 14a...first corrosion prevention treatment layer, 14b...second corrosion prevention treatment layer, 15, 115...thermal adhesive resin layer, 16, 116...sealant layer, 50...all-solid-state battery (electricity storage device), 52...electricity storage element, 54...outer packaging bag, 54a...bag main body, 54b...sealing portion.
Claims
1. The laminated laminate includes a base layer, a barrier layer, a thermal adhesive resin layer or an adhesive layer, and a sealant layer, When the thermal adhesive resin layer and the sealant layer, or the sealant layer is (I) and the base layer is (II), The loop stiffness value of (I) is 10 mN or more and 80 mN or less, The loop stiffness value of (II) is 2 mN or more and 20 mN or less, The ratio (I / II) of the loop stiffness values of (I) and (II) is 1.0 or more and 15 or less, The ratio (I / II) of the thickness of the (I) to the thickness of the (II) is 1.0 or more and 8.0 or less; Exterior material for electricity storage devices.
2. The thickness of the (I) is 30 μm or more and 120 μm or less, The exterior material for an electricity storage device according to claim 1, wherein the thickness of the (II) is 10 μm or more and 60 μm or less.
3. The exterior material for an electricity storage device according to claim 1, wherein a ratio (I / II) of loop stiffness values of the (I) and the (II) is 2.5 or more and 11.0 or less.
4. The exterior material for an electricity storage device according to claim 1, wherein a ratio (I / II) of loop stiffness values of the (I) and the (II) is 3.5 or more and 10 or less.
5. the sealant layer contains a polypropylene-based resin as a base resin, The exterior material for an electricity storage device according to claim 1 , wherein the polypropylene-based resin is composed of homopropylene or block polypropylene.
6. The exterior packaging material for an electricity storage device according to claim 5 , wherein the sealant layer further contains an additive resin containing a polyethylene-based resin, or a block copolymer exhibiting compatibility with the polypropylene-based resin.
7. The exterior material for an electricity storage device according to claim 5 , wherein the sealant layer further comprises an additive resin containing a polyethylene-based resin, and a compatibilizer having a portion compatible with the polypropylene-based resin and a portion compatible with the polyethylene-based resin.
8. The exterior material for an electricity storage device according to claim 7 , wherein the compatibilizer contains a block copolymer of polypropylene and polyethylene, or a block copolymer of polyethylene and polyethylenebutylene.
9. The electrical storage device exterior material according to any one of claims 1 to 8, which is an exterior material for an all-solid-state battery.
Citation Information
Patent Citations
Polylactic acid-containing polypropylene based resin composition
JP2013087160A
Aromatic-containing resin composition and production method thereof
JP2015044771A
Method of manufacturing battery
JP2016126826A
Sheath material for power storage device and power storage device using the same
JP2016162622A
Sheath material for power storage device
JP2017168355A