Laminated film and method for producing laminated film
Patent Information
- Application Number
- JP2024024649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-04
- Filing Date
- 2024-02-21
- Publication Date
- 2024-10-17
Smart Images

Figure 2024148141000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate film and a method for producing the laminate film. [Background technology]
[0002] Conventionally, a laminated film has been known that includes a base layer, a surface layer disposed on the base layer, and a bonding layer disposed between the base layer and the surface layer to bond the base layer and the surface layer (for example, Patent Document 1 below).
[0003] The following Patent Document 1 describes that the base layer (transparent base material) is made of a resin film made of triacetyl cellulose, the surface layer (low refractive index layer) is made of a curable resin composition containing a binder matrix made of an ionizing radiation curable material (e.g., an acrylic material, etc.), and the bonding layer (hard coat layer) is made as a mixed layer in which a portion of the triacetyl cellulose contained in the base layer (transparent base material) and a portion of the binder matrix contained in the surface layer (low refractive index layer) are mixed together. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-205644 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the laminated film configured as above, the bonding layer is required to have a function of sufficiently bonding the base layer and the surface layer. However, when the bonding layer is formed as a mixed layer of a part of the components of the base material layer and a part of the components of the surface layer, it cannot be said that sufficient consideration has been given to ensuring that the mixed layer serving as the bonding layer exhibits sufficient bonding function.
[0006] Therefore, an object of the present invention is to provide a laminated film that can provide a sufficient bonding function in a bonding layer that is formed as a mixed layer of a part of the components of a base layer and a part of the components of a surface layer, and to provide a method for manufacturing the laminated film. [Means for solving the problem]
[0007] As a result of intensive research by the present inventors, in a laminate film in which a bonding layer is configured as a mixed layer containing a part of the constituent components of a base layer and a part of the constituent components of a surface layer, when the thickness of the bonding layer is T μm and imaging Raman measurement is performed on the bonding layer by Raman spectroscopy, the peak top is at a wave number of 1730 cm -1 The intensity of the peak observed at I A , the peak top is 1635cm -1 The intensity of the peak observed at I B When T and I are A , and the above I B It has been found that the bonding layer exhibits a sufficient bonding function by satisfying a specific relational expression. As a result, the present invention was achieved.
[0008] That is, the laminated film according to the present invention is A substrate layer, a surface layer disposed on the substrate layer, and a bonding layer disposed between the substrate layer and the surface layer to bond the substrate layer and the surface layer, The base layer is made of a resin film containing triacetyl cellulose, The surface layer is made of a resin composition containing a photocurable resin, the bonding layer is configured as a compatible layer in which a part of the triacetyl cellulose contained in the base material layer and a part of the photocurable resin contained in the surface layer are compatible with each other, The thickness of the bonding layer is T J μm, When imaging Raman measurement was performed on the bonding layer by Raman spectroscopy, the peak top was at a wave number of 1730 cm -1The intensity of the peak observed at I A The peak top is at wavenumber 1635 cm -1 The intensity of the peak observed at I B When Said T J , I A , and the above I B satisfies the following relation: T J ×I B / I A ≧15.0μm
[0009] The method for producing a laminated film according to the present invention further comprises the steps of: A resin composition containing an organic solvent capable of dissolving triacetyl cellulose and a photocurable resin is applied onto a base layer composed of a resin film containing triacetyl cellulose to form a coating layer; and heat-treating the base layer and the coating layer, The heat treatment is carried out so that the maximum temperature is 130° C. or higher. Effect of the Invention
[0010] According to the laminated film of the present invention, the bonding layer, which is constituted as a mixed layer of a part of the constituent components of the base layer and a part of the constituent components of the surface layer, can exhibit a sufficient bonding function. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a cross-sectional view showing the configuration of the laminated film according to the present embodiment. [Figure 2A] 3A to 3C are cross-sectional views showing a process for forming the laminated film according to the embodiment. [Figure 2B] 6A to 6C are cross-sectional views showing another process for forming the laminated film according to the embodiment. [Figure 2C] 6A to 6C are cross-sectional views showing still another process for forming the laminated film according to the embodiment. [Figure 2D] 6A to 6C are cross-sectional views showing still another process for forming the laminated film according to the embodiment. [Diagram 3]1A to 1C are schematic diagrams illustrating a method for producing a laminated film according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] [Laminated film] Hereinafter, a laminate film according to one embodiment of the present invention will be described with reference to Fig. 1. In addition, hereinafter, a laminate film according to a specific example of one embodiment of the present invention may be simply referred to as a laminate film according to this embodiment.
[0013] The laminated film 10 of this embodiment comprises a base layer 1, a surface layer 2 arranged on the base layer 1, and a bonding layer 3 arranged between the base layer 1 and the surface layer 2 to bond the base layer 1 and the surface layer 2. In the laminated film 10 according to this embodiment, the base layer 1 is made of a resin film containing triacetyl cellulose (TAC). In the laminate film 10 according to this embodiment, the surface layer 2 is made of a resin composition containing a photocurable resin. In the laminated film 10 of this embodiment, the bonding layer 3 is configured as a compatible layer in which a portion of the triacetyl cellulose (TAC) contained in the base layer 1 and a portion of the photocurable resin contained in the surface layer 2 are compatible with each other. In the laminated film 10 according to this embodiment, the thickness of the bonding layer 3 is T J μm, and when imaging Raman measurement was performed on the bonding layer 3 by Raman spectroscopy, the peak top was at a wave number of 1730 cm -1 The intensity of the peak observed at I A The peak top is at wavenumber 1635 cm -1 The intensity of the peak observed at I B When the above T J , I A , and the above I B satisfies the following relation: ·Relationship T J ×[I B / I A ]≧15.0μm
[0014] The peak top is at wave number 1730 cm -1 The peak intensity I of the peak observed in A is derived from the carbon-oxygen double bond (C=O) of triacetyl cellulose. The peak top is at a wavenumber of 1635 cm -1 The peak intensity I of the peak observed in B comes from the carbon-carbon double bond (C=C) of the photocurable resin.
[0015] The term "miscible" refers to a state in which two or more substances are mixed together without being separated from each other.
[0016] Here, the laminate film 10 according to this embodiment is obtained by applying a resin composition containing a photocurable resin and an organic solvent capable of dissolving triacetyl cellulose (TAC) onto a substrate layer 1 to form a coating layer, and then heat-treating the coating layer, as described below. In the laminated film 10 according to this embodiment, the surface layer 2 and the bonding layer 3 are formed by the coating layer and triacetyl cellulose (TAC) that diffuses from the base layer 1 into the coating layer. More specifically, in the laminate film 10 of this embodiment, the portion of the coating layer in which triacetyl cellulose is not diffused constitutes a surface layer 2, and the portion of the coating layer in which triacetyl cellulose is diffused constitutes a bonding layer 3. The bonding layer 3 forms a compatible layer in which the triacetyl cellulose derived from the base layer 1 and the photocurable resin derived from the coating layer are mixed together without being separated from each other. That is, the bonding layer 3 forms a compatible layer in which the triacetyl cellulose derived from the base layer 1 and the photocurable resin derived from the coating layer are firmly entangled with each other.
[0017] As described above, the base layer 1 is made of a resin film containing triacetyl cellulose (TAC). The triacetyl cellulose is a cellulose in which all three hydroxyl groups present in the β-glucose unit constituting the cellulose are acetylated. More specifically, the triacetyl cellulose is a cellulose in which all the secondary hydroxyl groups at the 2- and 3-positions and the primary hydroxyl group at the 6-position present in the β-glucose unit are acetylated. An example of a commercially available resin film containing triacetyl cellulose is "TJ40UL" manufactured by Fuji Film Corporation. The glass transition temperature Tg of the triacetyl cellulose (TAC) is 130°C.
[0018] The glass transition temperature Tg can be measured, for example, using a DSC device. More specifically, the glass transition temperature Tg can be obtained from a DSC curve obtained when a sample (triacetyl cellulose) is heated at a temperature rise rate of 5° C. / min while flowing nitrogen gas between a temperature 30 K or more lower and a temperature 30 K or more higher than the expected glass transition temperature Tg. The glass transition temperature Tg can be determined based on the method described in JIS K7121:1987 "Method of measuring glass transition temperature of plastics."
[0019] The resin film as the base layer 1 can be obtained by, for example, forming a resin composition containing triacetyl cellulose (TAC) into a film. When forming the resin composition into a film, it is preferable not to perform a stretching treatment. That is, it is preferable that the resin film is a non-stretched film.
[0020] As described above, the surface layer 2 is composed of a resin composition containing a photocurable resin. Examples of the photocurable resin include a resin that can be cured by irradiation with active energy rays (hereinafter, also referred to as an active energy ray curable resin). Examples of active energy ray curable resins include resins that are cured by irradiation with electron beams, ultraviolet rays, α rays, β rays, γ rays, or X-rays. Among these, ultraviolet ray curable resins that are cured by irradiation with light such as ultraviolet rays are preferred. The irradiation with active energy rays may be irradiation with light including ultraviolet light (light irradiation).
[0021] Examples of the photocurable resin include polyester-based resins, (meth)acrylic-based resins, urethane-based resins, amide-based resins, silicone-based resins, epoxy-based resins, and urethane (meth)acrylate-based resins. Among these, it is preferable to use at least one of a (meth)acrylic resin and a urethane (meth)acrylate resin as the photocurable resin, and it is more preferable to use a urethane (meth)acrylate resin. An example of a commercially available urethane (meth)acrylate resin is "LUXYDIR 17-806" manufactured by DIC Corporation.
[0022] The photocurable resin may be a copolymer of an oligomer having a functional group and a monomer having a functional group. The oligomer having a functional group may be, for example, a curable urethane (meth)acrylate. The curable urethane (meth)acrylate may be 6 or more functional, or 8 or more functional. The curable urethane (meth)acrylate may be 10 or less functional. Examples of the monomer having a functional group include polyfunctional (meth)acrylates. The polyfunctional (meth)acrylates may be bifunctional or higher, or trifunctional or higher.
[0023] The resin composition may contain a photopolymerization initiator. When the resin composition contains a photopolymerization initiator, the polymerization reaction of the photocurable resin can be more easily initiated when the surface layer 2 is cured by irradiating the surface layer 2 with active energy rays (e.g., ultraviolet rays). The photopolymerization initiator may be appropriately selected depending on the type of the photocurable resin.
[0024] Examples of the photopolymerization initiator include 4,4'-bis(diethylamino)benzophenone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, ethyl-4-(dimethylamino)-benzoate, [4-(methylphenylthio)phenyl]-phenylmethane, ethylhexyl-4-dimethylaminobenzoate, methyl-o-benzoylbenzoate, methylbenzoylformate, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)diphenylphosphine oxide, and 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane. When the (meth)acrylic resin or the urethane (meth)acrylate resin is used as the photocurable resin, it is preferable to use 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)diphenylphosphine oxide, or 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane as a photopolymerization initiator, and it is particularly preferable to use 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane. An example of a commercially available product of 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane is the product name "OMNIRAD907" manufactured by BASF.
[0025] When the surface layer 2 is irradiated with light from the surface side, the curing of the surface layer 2 can be sufficiently promoted by a polymerization reaction of the carbon-carbon bonds (C=C) of the photocurable resin. On the other hand, as described above, in the bonding layer 3, the photocurable resin and the triacetyl cellulose are firmly entangled with each other. Therefore, when the surface layer 2 is irradiated with light or the like, the strong entanglement between the photocurable resin and triacetyl cellulose may cause the polymerization reaction of the carbon-carbon bonds (C=C) of the photocurable resin to not necessarily proceed sufficiently in the bonding layer 3. In other words, the curing in the bonding layer 3 proceeds more slowly than the curing in the surface layer 2. As a result, even after light irradiation is performed from the surface side of the surface layer 2, carbon-carbon double bonds (C=C) derived from the photocurable resin remain in the bonding layer 3. Therefore, when imaging Raman measurement by Raman spectroscopy is performed on the bonding layer 3 after the active energy ray irradiation, a peak derived from the carbon-carbon double bond (C=C) is observed. Specifically, in the bonding layer 3 after the active energy ray irradiation, the peak top is at a wave number of 1635 cm -1 A peak with a peak intensity I B is observed.
[0026] The resin composition may contain 1 part by mass or more, 2 parts by mass or more, or 4 parts by mass or more of the photopolymerization initiator relative to 100 parts by mass of the photocurable resin. The resin composition may contain 10 parts by mass or less of the photopolymerization initiator relative to 100 parts by mass of the photocurable resin.
[0027] The resin composition may contain an organic solvent for dissolving and suspending the photocurable resin. Examples of the organic solvent include monohydric alcohol solvents such as methanol, ethanol, isopropyl alcohol, butanol, and 2-methoxyethanol, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclopentanone, ester solvents such as methyl acetate, ethyl acetate, and butyl acetate, ether solvents such as diisopropyl ether and propylene glycol monomethyl ether, polyol solvents such as ethylene glycol and propylene glycol, acyclic aliphatic hydrocarbon solvents such as hexane, heptane, and octane, cyclic aliphatic hydrocarbons such as cyclohexane and cycloheptane, and aromatic hydrocarbon solvents such as benzene, toluene, and xylene. These may be used alone or in combination.
[0028] As shown in Figures 2A to 2D, the surface layer 2 is formed by applying the resin composition onto a base layer 1 to form a coating layer 4 (see Figure 2A), and then heat-treating the base layer 1 and the coating layer 4 (see Figures 2B to 2D). Furthermore, when forming the coating layer 4, the surface portion of the base material layer 1 is dissolved by the organic solvent contained in the resin composition, and by heat-treating the base material layer 1 and the coating layer 4, the molecular motion of a portion of the triacetyl cellulose C contained in the base material layer 1 becomes active (see Figure 2B), and a portion of the triacetyl cellulose C diffuses into the coating layer 4 (see Figure 2C). In order to activate the molecular motion of triacetyl cellulose C, it is necessary to transition the triacetyl cellulose C from a glassy state to a rubbery state. Therefore, the heat treatment is carried out at a temperature equal to or higher than the glass transition temperature Tg (130° C.) of triacetyl cellulose C.
[0029] As described above, in the portion in which the triacetyl cellulose C is dispersed in the coating layer 4, the triacetyl cellulose C and the photocurable resin are not separated from each other but are mixed together to form a compatible layer. That is, as described above, the coating layer 4 forms the surface layer 2 made of the photocurable resin and the compatible layer of the photocurable resin and triacetyl cellulose C. As described above, the organic solvent contained in the coating layer 4 volatilizes during the heat treatment of the base layer 1 and the coating layer 4. After the organic solvent has volatilized, the compatible layer functions as a bonding layer 3 for bonding the base layer 1 and the surface layer 2 (see FIG. 2D). The bonding layer 3 can bond the base layer 1 and the surface layer 2 more firmly by being irradiated with active energy rays (ultraviolet rays, etc.). This is because the light irradiation causes a polymerization reaction in part of the photocurable resin to proceed, making it possible to sufficiently retain the triacetyl cellulose in a state where it is entangled with the photocurable resin.
[0030] From the viewpoint of allowing the compatible layer to exhibit sufficient bonding properties, it is preferable that the boiling point of the organic solvent is within ±10° C. of the maximum temperature during the heat treatment of the coating layer. For example, when the maximum temperature during heat treatment of the coating layer is 130° C., it is preferable to use cyclopentanone, which has a boiling point of 140° C., as the organic solvent. Since the difference between the maximum temperature and the boiling point of the organic solvent is small, the organic solvent can be gradually evaporated from the coating layer formed by the resin composition. Therefore, a compatible layer in which triacetyl cellulose and the photocurable resin are sufficiently compatible can be formed between the base layer 1 and the surface layer 2. That is, a bonding layer 3 that can exhibit sufficient bonding properties to the base layer 1 and the surface layer 2 can be formed. When the resin composition contains two or more organic solvents and the two or more organic solvents form an azeotropic mixture, the azeotropic point is the boiling point.
[0031] From the viewpoint of sufficiently dissolving the surface layer portion of the base layer 1 and sufficiently diffusing a portion of the triacetyl cellulose into the coating layer, the organic solvent is preferably ethyl acetate or cyclohexane. In addition, when the resin composition contains a thickener as described later, ethyl acetate cannot sufficiently dissolve the thickener, so that if ethyl acetate is used alone as the organic solvent, agglomerates of the thickener may occur in the bonding layer 3. If agglomerates of the thickener occur in the bonding layer 3, this is undesirable in that the appearance of the laminated film 10 is deteriorated. Here, since the thickener usually exhibits high solubility in toluene, it is preferable to use ethyl acetate and toluene in combination. By using ethyl acetate and toluene in combination, the surface layer portion of the base layer 1 can be sufficiently dissolved, and the triacetyl cellulose contained in the surface layer portion can be sufficiently diffused into the coating layer, while the thickener can be dissolved with toluene. That is, in the laminated film 10, the adhesion between the base layer 1 and the surface layer 2 by the bonding layer 3 can be sufficiently ensured, and the occurrence of poor appearance due to aggregation of the thickener can be suppressed.
[0032] The resin composition may contain a thickener, such as organoclay, talc, bentonite, montmorillonite, kaolinite, or the like. Smectite that has been highly purified by hydrothermal treatment is also called smectone.
[0033] The resin composition may contain 0.5 parts by mass or more, 1.0 parts by mass or more, or 2.5 parts by mass or more of a thickener per 100 parts by mass of the photocurable resin, or 5 parts by mass or less of a thickener per 100 parts by mass of the photocurable resin.
[0034] The resin composition may contain a filler. The filler may be an inorganic filler or an organic filler.
[0035] Examples of the inorganic filler include silicon oxide particles, titanium oxide particles, aluminum oxide particles, zinc oxide particles, tin oxide particles, calcium carbonate particles, barium sulfate particles, talc particles, kaolin particles, and calcium sulfate particles. Examples of the organic filler include polymethyl methacrylate resin particles (PMMA particles), silicone resin particles, polystyrene resin particles, polycarbonate resin particles, acrylic styrene resin particles, benzoguanamine resin particles, melamine resin particles, polyolefin resin particles, polyester resin particles, polyamide resin particles, polyimide resin particles, and polyethylene fluoride resin particles. The inorganic filler and the organic filler may each be used alone or in combination of two or more kinds. In addition, when the resin composition contains the filler, the filler is naturally also contained in the surface layer 2. Since the filler may have a property of absorbing light, the surface layer 2 can fully exhibit the function as an antireflection layer.
[0036] The resin composition may contain 5 parts by mass or more, 7 parts by mass or more, or 10 parts by mass or more of the filler relative to 100 parts by mass of the photocurable resin. The resin composition may contain 30 parts by mass or less, or 20 parts by mass or less of the filler relative to 100 parts by mass of the photocurable resin.
[0037] The resin composition may contain a leveling agent (surface modifier). The leveling agent may be a fluorine-based surfactant. A commercially available fluorine-based surfactant may be, for example, "Megafac F-556" manufactured by DIC Corporation.
[0038] The resin composition may contain 0.1 parts by mass or more, 0.2 parts by mass or more, or 0.4 parts by mass or more of the leveling agent relative to 100 parts by mass of the photocurable resin. The resin composition may contain 2 parts by mass or less, or 1 part by mass or less, of the leveling agent relative to 100 parts by mass of the photocurable resin.
[0039] In the laminate film 10 according to this embodiment, the surface layer 2 may have a function as a hard coat layer, an antiglare layer, or an antireflection layer.
[0040] The hard coat layer is a layer that imparts scratch resistance, chemical resistance, etc. to the surface of the laminate film 10. Therefore, the laminate film 10 having the surface layer 2 functioning as a hard coat layer can be used by being attached to an image display unit in an image display device such as a tablet personal computer. The antiglare layer is a layer for preventing external light from being reflected by scattering and reflecting light. Therefore, the laminated film 10 having the surface layer 2 as an antiglare layer can be used by being attached to the image display part of the image display device of a car navigation system, for example. The anti-reflection layer is a layer for preventing reflection of external light. Therefore, the laminate film 10 having the surface layer 2 as an anti-reflection layer can be used by being attached to the image display section of an image display device of a car navigation system, for example.
[0041] In the laminated film 10 according to this embodiment, the thickness T B The thickness T of the base layer 1 may be 10 μm or more, 20 μm or more, or 30 μm or more. B may be 100 μm or less, may be 80 μm or less, or may be 50 μm or less. Thickness T of base layer 1 B can be obtained using a digital linear gauge (product name "MODEL D-10HS", manufactured by Ozaki Manufacturing Co., Ltd.) as a measuring device. B The thickness T of the base layer 1 can be calculated by measuring the thickness at any five points in the width direction of the base layer 1 using the digital linear gauge and arithmetically averaging the measured values. B is the thickness T of the surface layer 2 described below S It can be measured in the same manner.
[0042] In the laminated film 10 according to this embodiment, the thickness T of the surface layer 2 S The thickness T of the surface layer 2 may be 1.0 μm or more, 2.0 μm or more, or 3.0 μm or more. S may be 10.0 μm or less, may be 8.0 μm or less, or may be 5.0 μm or less. Thickness T of surface layer 2 S The thickness T of the surface layer 2 can be measured using, for example, a transmission electron microscope (TEM) (product name "HT7820" manufactured by Hitachi High-Technologies Corporation) under conditions of a magnification of 10,000 times and an acceleration voltage of 100 kV. The arithmetic average of the thickness measurements at at least five randomly selected points is taken as the thickness T of the surface layer 2. S It can be adopted as.
[0043] In the laminated film 10 according to this embodiment, the thickness T of the bonding layer 3 J The thickness T of the bonding layer 3 may be 3.0 μm or more, 4.0 μm or more, or 5.0 μm or more. J It is particularly preferable that the thickness T is 6.1 μm or more. J When the thickness is 6.1 μm or more, the bonding layer 3 exhibits particularly strong bonding properties. In addition, the thickness T of the bonding layer 3 J may be 10.0 μm or less, may be 8.0 μm or less, or may be 7 μm or less. Thickness T of bonding layer 3 J is the thickness T of the surface layer 2 S can be calculated in the same manner.
[0044] In the laminated film 10 according to this embodiment, the thickness T of the surface layer 2 S and the thickness T of the bonding layer 3 J The combined value of T S +T J may be 6.0 μm or more, 8.0 μm or more, or 9.0 μm or more. In addition, the above total value T S +T Jmay be 15.0 μm or less, may be 12.0 μm or less, or may be 10.0 μm or less.
[0045] In the laminated film 10 according to this embodiment, the thickness T of the surface layer 2 S and the thickness T of the bonding layer 3 J The combined value of T S +T J The thickness T of the bonding layer 3 J The ratio [T J / (T S +T J )] may be 0.30 or more, may be 0.40 or more, or may be 0.50 or more. In addition, the above ratio [T J / (T S +T J ) may be 1.00 or less, 0.80 or less, 0.70 or less, or 0.65 or less.
[0046] As described above, in the laminated film 10 according to this embodiment, the thickness of the bonding layer 3 is T J μm, and when imaging Raman measurement by Raman spectroscopy was performed on the bonding layer 3 after irradiation with active energy rays, the peak top was at a wave number of 1730 cm -1 The intensity of the peak observed at I A The peak top is at wavenumber 1635 cm -1 The intensity of the peak observed at I B When T and I are A , and the above I B satisfies the following relation: ·Relationship T J ×(I B / I A )≧15.0μm
[0047] In the laminated film 10 according to this embodiment, the above [T J ×(I B / I A The above [T J ×(I B / IA )] may be 30.0 μm or less, 25.0 μm or less, 22.0 μm or less, or 20.0 μm or less.
[0048] In the laminated film 10 according to this embodiment, I B / I A may be 1.00 or more, 2.00 or more, or 3.00 or more. B / I A may be 5.00 or less, or may be 4.00 or less.
[0049] In the laminated film 10 according to this embodiment, I A / I B may be 0.10 or more, 0.20 or more, 0.30 or more, or more than 0.30. A / I B may be 0.60 or less, may be 0.50 or less, or may be 0.4 or less.
[0050] In the laminated film 10 according to this embodiment, [T J / (T S +T J )]×[I B / I A ] may be 0.50 or more, 1.00 or more, or 1.50 or more. J / (T S +T J )]×[I B / I A ] may be 5.00 or less, 4.00 or less, 3.00 or less, 2.50 or less, or 2.00 or less.
[0051] The imaging Raman measurement by Raman spectroscopy can be carried out by measuring the Raman spectrum using a Raman microscope spectrometer (product name "alpha300RSA", manufactured by WITec). In the measurement of the Raman spectrum, a Raman spectrum is obtained for 30,000 points on the cross section of the laminate film 10 in an area of 20 μm×15 μm under conditions of an objective lens of 100 times and an excitation wavelength of 532 nm. In the obtained Raman spectrum, the wave number was 75 cm -1 ~3780cm -1 The baseline was corrected by linear approximation using the baseline, and the peak top was at wavenumber 1730 cm -1 Intensity of the peak observed in I A The peak top is 1635 cm -1 Intensity of the peak observed in I B We ask for:
[0052] In the laminate film 10 according to this embodiment, it is preferable that the bonding layer 3 has a bonding strength that does not peel off from the surface layer 2 even after the surface layer 2 is exposed to light irradiation for 144 hours or more. As a result, in the laminated film 10 according to this embodiment, the bonding layer 3 exhibits particularly strong bonding properties.
[0053] (Laminated Film Manufacturing Method) The manufacturing method of the laminated film according to this embodiment includes applying a resin composition containing an organic solvent capable of dissolving triacetyl cellulose and a photocurable resin onto a substrate layer composed of a resin film containing triacetyl cellulose to form a coating layer, and heat-treating the coating layer. In the method for producing a laminated film according to this embodiment, the heat treatment is carried out so that the maximum temperature becomes 130° C. or higher.
[0054] The laminated film according to this embodiment is manufactured, for example, by using a laminated film manufacturing apparatus 2000 as shown in FIG. As explained in the manufacturing method below, at least a part of the base material roll 1A becomes the base material layer.
[0055] As shown in FIG. 3, the laminated film manufacturing apparatus 2000 includes a first unwinding section 100 that unwinds a base material raw web 1A containing triacetyl cellulose wound in a roll toward the downstream side, a pre-annealing section 200 that is disposed downstream of the first unwinding section 100 and pre-anneals the base material raw web 1A unwound from the first unwinding section 100, a first roller 300 that is disposed downstream of the pre-annealing section 200 and transports the base material raw web 1A after pre-annealing further downstream, and a die coater 400 that is disposed opposite the transport surface of the base material raw web 1A on the first roller 300 and coats the exposed surface of the base material raw web 1A being transported by the first roller 300 with a resin composition containing an organic solvent capable of dissolving the triacetyl cellulose and a photocurable resin. The apparatus includes an oven 500 disposed downstream of the first roller 300 for heat-treating the base material raw fabric 1A on which a coating layer of the resin composition has been formed, a light irradiation section 600 disposed downstream of the oven 500 for irradiating the coating layer formed on the base material raw fabric 1A with light (active energy rays) such as ultraviolet rays, a second roller 700 and a third roller 800 disposed opposite each other downstream of the light irradiation section 600, the second roller 700 and the third roller 800 holding the coating layer and the base material raw fabric 1A after light irradiation and transporting them further downstream, and a winding section 900 disposed downstream of the second roller 700 and the third roller 800 for winding up the coating layer and the base material raw fabric 1A after irradiation with light such as ultraviolet rays. As shown in FIG. 3, the laminated film manufacturing apparatus 2000 also includes a storage tank 1000 for storing the resin composition to be applied by the die coater 400, and a second unwinding section 1100 for unwinding a roll of protective film P for protecting the exposed surface of the coating layer after irradiation with light such as ultraviolet light, toward the second roller 700 and the third roller 800.
[0056] Hereinafter, the method for producing a laminated film according to this embodiment will be described using the laminated film production apparatus 2000 shown in FIG.
[0057] (Pre-annealed) In the laminated film manufacturing method according to this embodiment, the base material raw web 1A fed from the first feed-out section 100 is pre-annealed in the pre-annealing section 200. By pre-annealing in the pre-annealing section 200, stresses such as tensile residual stress or compressive residual stress remaining in the base material raw web 1A can be removed from the base material raw web 1A. This makes it possible to prevent damage such as cracks from occurring in the base material raw web 1A due to residual stress in the base material raw web 1A during the manufacturing of the laminated film. In this embodiment, the base material raw material 1A is a base material raw material containing triacetyl cellulose, and therefore, pre-annealing in the pre-annealing section 200 is preferably performed at a temperature in the range of 80°C or more and 100°C or less.
[0058] (Formation of coating layer) Next, the pre-annealed base material raw material 1A is conveyed toward the first roller 300. The conveying speed (line speed) of the pre-annealed base material raw material 1A is preferably 20 m / h or more and 50 m / h or less. The conveying speed can be adjusted by appropriately adjusting the rotation speed of the first roller 300. Then, using a die coater 400 arranged opposite the first roller 300, a resin composition containing an organic solvent capable of dissolving the triacetyl cellulose and a photocurable resin is applied to the exposed surface of the pre-annealed base material raw material 1A to form a coating layer. Since the resin composition contains an organic solvent capable of dissolving the triacetyl cellulose, the triacetyl cellulose is dissolved by the organic solvent in the surface portion of the base material 1A on which the coating layer is formed. Coating by the die coater 400 is carried out, for example, by using a 50 μm thick PET shim to set the thickness of the coating liquid discharge section of the die coater 400 to 50 μm, and preferably by setting the die gap, which is the distance between the die lip of the die coater 400 and the substrate original roll 1A, to 300 μm or more and 400 μm or less. The thickness of the coating layer is preferably 10 μm or more and 30 μm or less. In addition, by setting the conveying speed of the pre-annealed base material raw material 1A within the above-mentioned numerical range, it becomes easier to apply the resin composition to the exposed surface of the pre-annealed base material raw material 1A with a thickness that is nearly uniform.
[0059] Examples of the organic solvent include those described above. Among these, it is preferable to use cyclopentanone. Examples of the photocurable resin include those described above, and among these, it is preferable to use a urethane (meth)acrylate resin. In addition, the resin composition preferably contains a photopolymerization initiator to initiate a polymerization reaction of the photocurable resin by irradiation with light such as ultraviolet light. When the photocurable resin is a urethane (meth)acrylate resin, the photopolymerization initiator is preferably 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propane. The resin composition preferably contains a thickener so that the resin composition has a viscosity suitable for application. The thickener preferably contains smectite. The resin composition can be prepared, for example, by stirring and mixing the organic solvent, the photocurable resin, the photopolymerization initiator, the thickener, and the like in a storage tank 1000.
[0060] (Heat treatment) Next, the base material roll 1A with the formed coating layer attached thereto is transported toward the oven 500. The conveying speed (line speed) of the base material roll 1A having the coating layer attached thereto is preferably 20 m / h or more and 50 m / h or less, as described above. By setting the conveying speed within the above-mentioned range, the coating layer can be efficiently heat-treated in the oven 500 . In this embodiment, the heat treatment in the oven 500 is carried out so that the maximum temperature in the oven is 130° C. or higher. As described above, the triacetyl cellulose contained in the base material raw material 1A has a glass transition temperature Tg of 130° C. By setting the maximum temperature in the oven to 130° C. or higher, the triacetyl cellulose dissolved by the organic solvent in the surface layer portion of the base material raw material 1A can be transitioned from a glassy state to a rubbery state. As a result, the molecular motion of the triacetyl cellulose can be made active in the surface layer portion of the base material web 1A. This allows a portion of the triacetyl cellulose present in the surface layer portion of the base material web 1A to be diffused into the coating layer. In the portion of the coating layer where the triacetyl cellulose is dispersed, the triacetyl cellulose and the photocurable resin are not separated from each other but are mixed together to form a compatible layer. The portion of the coating layer into which the triacetyl cellulose has not diffused constitutes a surface layer.
[0061] The drying time required to reach a maximum temperature of 130° C. or higher is preferably 10 seconds or longer, more preferably 20 seconds or longer, and even more preferably 30 seconds or longer. Furthermore, the drying time required for the maximum temperature to reach 130° C. or higher may be 60 seconds or less, 50 seconds or less, or 40 seconds or less. By setting the drying time at which the maximum temperature reaches 130°C or higher within the above-mentioned numerical range, a portion of the triacetyl cellulose contained in the surface layer portion of the base material raw material 1A dissolved by the organic solvent can be efficiently diffused into the coating layer. Moreover, the maximum temperature in the heat treatment is preferably 200° C. or lower, more preferably 180° C. or lower, and even more preferably 150° C. or lower. By carrying out the heat treatment in this manner, a laminated film can be obtained in which the bonding layer (compatible layer) and the surface layer are laminated in this order on the base material roll 1A.
[0062] The heat treatment may be carried out in several stages at different temperatures, for example, a first stage of heat treatment may be carried out at a temperature of 50° C. to 90° C., a second stage of heat treatment may be carried out at a temperature of 130° C. or higher, and a third stage of heat treatment may be carried out at a temperature of 50° C. to 90° C. In this way, by performing the heat treatment in multiple steps at different temperatures, it is possible to prevent the organic solvent from bumping in the coating layer due to a sudden increase in temperature, and therefore to prevent the coating layer from having a poor appearance due to the bumping.
[0063] (Light irradiation) Next, the coated layer and the original substrate 1A after the heat treatment are transported toward the light irradiation section 600. The conveying speed (line speed) of the coating layer and the base material roll 1A after the heat treatment is preferably 20 m / h or more and 50 m / h or less, as described above. By setting the conveying speed within the above-mentioned range, the coating layer after the heat treatment can be efficiently irradiated with light in the light irradiating section 600 . The light irradiation unit 600 preferably irradiates active energy rays, and among active energy rays, it is preferable that the light irradiation unit 600 irradiates ultraviolet rays (for example, ultraviolet rays having a wavelength of 365 nm). Hereinafter, irradiation of active energy rays may be simply referred to as light irradiation. The active energy rays have an integrated light amount of 100 mJ / cm 2 It is preferable to irradiate the light at a dose of 150 mJ / cm or more. 2 More preferably, the irradiation is performed at a dose of 200 mJ / cm or more. 2 It is more preferable that the irradiation is performed so as to achieve the above value. The upper limit of the integrated light amount is usually 500 mJ / cm 2 It is.
[0064] As described above, by irradiating the coating layer and the base material 1A after the heat treatment with light, a curing reaction can be carried out by the photocurable resin entangled with the triacetyl cellulose in the portion of the coating layer where the triacetyl cellulose is diffused (corresponding to the bonding layer). On the other hand, in the portion of the coating layer where the triacetyl cellulose is not diffused (corresponding to the surface layer), the curing reaction can be promoted by the photocurable resin that is not entangled with the triacetyl cellulose, which allows the surface layer in the laminate film according to the present embodiment to have sufficient strength. Furthermore, in the bonding layer, a polymerization reaction of the photocurable resin in a state in which it is entangled with the triacetyl cellulose proceeds, so that the bonding layer can be hardened while the triacetyl cellulose is suitably retained in the bonding layer. Since the hardened bonding layer is formed while the triacetyl cellulose is favorably held, the bonding layer can exhibit favorable bonding properties to the base material roll 1A. In addition, since the photocurable resin is continuous as a matrix resin in the surface layer and the bonding layer, good bonding properties are also exhibited between the surface layer and the bonding layer.
[0065] (Winding of laminated film) Next, the laminated film after light irradiation is transported by a second roller 700 and a third roller 800 to a winding section 900, where the laminated film is wound up. The transport speed (line speed) of the laminated film after the light irradiation is preferably 20 m / h or more and 50 m / h or less, as described above. In the laminated film manufacturing method according to this embodiment, the laminated film after light irradiation is wound up while the protective film P is being paid out from the second pay-out section 1100 to the second roller 700 and the third roller 800 . The protective film P is unwound so as to cover the exposed surface of the coating layer in the laminated film (ie, the exposed surface of the surface layer). In order to suitably cover the exposed surface of the surface layer with the protective film P, the payout speed of the protective film P is preferably set to the same speed as the transport speed (line speed) of the laminated film after light irradiation. As a result of the above, the laminated film according to this embodiment can be obtained in which the bonding layer and the surface layer are arranged in this order on the base material raw material 1A, and further, a protective film P is arranged on the surface of the surface layer.
[0066] The matters disclosed in this specification include the following.
[0067] (1) A substrate layer, a surface layer disposed on the substrate layer, and a bonding layer disposed between the substrate layer and the surface layer to bond the substrate layer and the surface layer, The base layer is made of a resin film containing triacetyl cellulose, The surface layer is made of a resin composition containing a photocurable resin, the bonding layer is configured as a compatible layer in which a part of the triacetyl cellulose contained in the base material layer and a part of the photocurable resin contained in the surface layer are compatible with each other, The thickness of the bonding layer is T J μm, When imaging Raman measurement was performed on the bonding layer by Raman spectroscopy, the peak top was at a wave number of 1730 cm -1 The intensity of the peak observed at I A The peak top is at wavenumber 1635 cm -1 The intensity of the peak observed at I B When Said T J , I A , and the above I B A laminated film, which satisfies the following relational expression: T J ×I B / I A ≧15.0μm
[0068] (2) The bonding layer has a thickness of 6.1 μm or more. The laminate film described in (1) above.
[0069] (3) The bonding layer has a bonding strength such that it does not peel off from the surface layer even after the surface layer is exposed to light irradiation for 144 hours or more. The laminate film according to (1) or (2) above.
[0070] (4) The surface layer has a function of a hard coat layer. The laminate film according to any one of (1) to (3) above.
[0071] (5) A resin composition containing an organic solvent capable of dissolving triacetyl cellulose and a photocurable resin is applied onto a base layer composed of a resin film containing triacetyl cellulose to form a coating layer; and drying the coating layer by heating; The heat drying is carried out so that the maximum temperature is 130° C. or higher. A method for manufacturing a laminated film.
[0072] (6) In the heat drying, heating at the maximum temperature is carried out for 20 seconds or more. A method for producing the laminated film according to (5) above.
[0073] The laminated film and the method for producing the laminated film according to the present invention are not limited to the above-described embodiment. Furthermore, the laminated film and the method for producing the laminated film according to the present invention are not limited to the above-mentioned effects. The laminated film and the method for producing the laminated film according to the present invention can be modified in various ways without departing from the gist of the present invention. EXAMPLES
[0074] The present invention will now be described in more detail with reference to examples. The following examples are provided to further explain the present invention in detail, and are not intended to limit the scope of the present invention.
[0075] <Example 1> (base material layer) As the substrate layer, a triacetyl cellulose substrate (manufactured by Fuji Film Corporation under the trade name "TJ40UL", thickness 40 μm) was used. (Preparation of Resin Composition) To a mixed solvent (PGM:CPN=60:40) of organic solvents propylene glycol monomethyl ether (PGM), 3 parts by mass of a photopolymerization initiator (BASF product name "OMNIRAD907"), 100 parts by mass of an ultraviolet-curable urethane acrylate resin (DIC product name "LUXYDIR 17-806", solids concentration 80%) as a photocurable resin, and 0.01 parts by mass of a leveling agent (DIC product name "GRANDIC PC4100") were added, and the mixture was stirred for 15 minutes with a disperser to prepare the resin composition of Example 1. (Preparation of bonding layer and surface layer) A triacetyl cellulose substrate as a substrate layer was conveyed at a conveying speed (line speed) of 25 m / s, and the resin composition of Example 1 was applied onto the triacetyl cellulose substrate to form a coating layer, followed by a heat treatment in an oven. The coating layer was formed using an apparatus as shown in FIG. The heat treatment consisted of a first heating at 90° C. for 25 seconds, then a second heating at 130° C. for 25 seconds, and finally a third heating at 90° C. for 25 seconds. This allowed the coating layer to dry. The resin composition according to Example 1 was applied onto the triacetyl cellulose substrate so that the thickness after drying was 9.8 μm. The dried coating layer was irradiated with a high-pressure mercury lamp at an integrated light dose of 245 mJ / cm 2 The sample was irradiated with ultraviolet light having a wavelength of 365 nm so as to obtain the following: In this way, the bonding layer and the surface layer were formed in this order on the triacetyl cellulose base material. That is, a laminated film according to Example 1 was obtained in which a bonding layer and a surface layer were laminated in this order on a base layer.
[0076] <Example 2> In preparing the bonding layer and the surface layer, a first drying step was performed at 60°C for 25 seconds, and the resin composition was applied onto the base layer so that the thickness after drying was 9.4 µm. In the same manner as in Example 1, a laminated film of Example 2 was obtained in which the bonding layer and the surface layer were laminated in this order on the base layer.
[0077] <Example 3> In the preparation of the bonding layer and the surface layer, a second drying was performed at 140°C for 25 seconds, and the resin composition was applied onto the base layer so that the thickness after drying was 9.5 µm. In the same manner as in Example 1, a laminated film of Example 3 was obtained in which the bonding layer and the surface layer were laminated in this order on the base layer.
[0078] <Example 4> In preparing the bonding layer and the surface layer, the conveying speed (line speed) was set to 30 m / s, and the resin composition was applied onto the base layer so that the thickness after drying would be 9.0 μm. In the same manner as in Example 1, a laminated film of Example 4 was obtained in which the bonding layer and the surface layer were laminated in this order on the base layer.
[0079] <Comparative Example 1> In the preparation of the bonding layer and the surface layer, a second drying was performed at 120°C for 25 seconds, and the resin composition was applied onto the base layer so that the thickness after drying was 10.1 µm. In the same manner as in Example 1, a laminated film of Comparative Example 1 was obtained in which the bonding layer and the surface layer were laminated in this order on the base layer.
[0080] <Comparative Example 2> In preparing the bonding layer and the surface layer, a second drying step was performed at 110°C for 25 seconds, and the resin composition was applied onto the base layer so that the thickness after drying was 9.7 µm. In the same manner as in Example 1, a laminated film according to Comparative Example 2 was obtained in which the bonding layer and the surface layer were laminated in this order on the base layer.
[0081] <Comparative Example 3> In the preparation of the bonding layer and the surface layer, a second drying was performed at 100°C for 25 seconds, and the resin composition was applied onto the base layer so that the thickness after drying was 9.6 µm. In the same manner as in Example 1, a laminated film of Comparative Example 3 was obtained in which the bonding layer and the surface layer were laminated in this order on the base layer.
[0082] The manufacturing conditions for the laminated film in each example are shown in Table 1 below.
[0083] [Table 1]
[0084] (Thickness measurement) For each example of the laminated film, the thickness T S and the thickness of the bonding layer T J The thickness of the surface layer T S and the thickness of the bonding layer T J were measured according to the method described in the above embodiment section, and the results are shown in Table 2 below. In addition, in Table 2 below, the thickness of the surface layer T S and the thickness of the bonding layer T J The sum of these values and the thickness of the surface layer T S and the thickness of the bonding layer T J The thickness of the bonding layer T J It also shows:
[0085] (Imaging Raman measurement) The bonding layer of the laminated film according to each example was subjected to imaging Raman measurement by Raman spectroscopy, and the peak top was at a wave number of 1730 cm -1 The peak intensity I of the peak observed inA , and the peak top is at wavenumber 1635 cm -1 The peak intensity I of the peak observed in B The imaging Raman measurements were performed according to the method described in the Examples section above. And, for the laminated film according to each example, the peak intensity I B Peak intensity I A The ratio (I A / I B ), and peak intensity I A Peak intensity I B The ratio (I B / I A ) was calculated. In addition, for the laminated film in each example, T J ×I B / I A , and [T J / (T S +T J )]×[I B / I A ] were also calculated. The results are shown in Table 2 below.
[0086] (Durable adhesion) The laminated film according to each example was evaluated for durable adhesion. The evaluation of durable adhesion was carried out by a fade adhesion test. The fade adhesion test is a test for evaluating durable adhesion (weather resistance) under irradiation with ultraviolet light. In the tests herein, the laminate film according to each example was placed in an ultraviolet long-life fade meter (manufactured by Suga Test Instruments, model "U48HB"), and the laminate film was irradiated with ultraviolet light for a predetermined period of time. In the fade test, a carbon arc lamp was used as the light source, the black panel temperature was set to 63°C, and the radiation intensity (integrated illuminance at 300-700 nm) was set to 500 W / m 2 The environmental temperature was set to 40° C., and the environmental humidity was set to a range of 10% RH to 40% RH. The laminated films were subjected to the below-described cross-cut peel test 48 hours, 96 hours, 144 hours, 192 hours, 240 hours, and 500 hours after the start of UV irradiation to evaluate the adhesion of the bonding layer to the surface layer. The laminated film used had a planar dimension of 10 mm×10 mm.
[0087] (Cross-cut peel test) Using a utility knife, 100 (10×10) squares with 1 mm sides were formed in a grid pattern on the exposed surface of the surface layer. Next, an adhesive tape (manufactured by Sekisui Chemical Co., Ltd., product name "Cellotape (registered trademark) No. 252") was attached to the exposed surface of the surface layer, and then peeled off. This procedure was repeated twice, and the UV irradiation time required for none of the 100 1 mm square pieces to peel off was determined. For example, if the evaluation result is 48 hours (h), it means that when UV irradiation was performed for 48 hours (h), none of the 100 1 mm square squares peeled off, but when UV irradiation was performed for 96 hours (h), at least one of the 100 1 mm square squares peeled off. The same applies to evaluation results at 96 hours (h) and 144 hours (h). When the evaluation time is 500 hours (h), it means that even when ultraviolet irradiation was performed for 500 hours (h), not a single 1 mm square was peeled off. Although the above-mentioned grid peel test conforms to JIS K5600, it is different in that it uses 100 1 mm squares (JIS K5600 requires 25 1 mm squares). The results are shown in Table 2 below.
[0088] (Steel wool (SW) resistance) The laminated film according to each example was evaluated for steel wool (SW) resistance under a load of 400 g or 800 g. The SW resistance evaluation was carried out according to the following procedure. (1) The laminate film according to each example is placed on a glass plate with the side on which the surface layer is not formed facing down. (2) Steel wool #0000 was evenly attached to the side (smooth surface) of a cylinder with an outer diameter of 11 mm to obtain a cylinder with steel wool attached, and then the side of the cylinder with the steel wool was moved back and forth 10 times on the surface (exposed surface) of the surface layer of the laminate film of each example. The conditions for reciprocating the side surface of the cylinder with the steel wool are a load of 400 g or 800 g and a speed of approximately 100 mm / sec. (3) For each example of the laminate film, the state of scratches on the surface of the surface layer was visually inspected and evaluated according to the following criteria. The results are shown in Table 2 below. Excellent: No scratches were found on the surface of the surface layer upon visual inspection. Unacceptable: Any scratches are visible on the surface of the surface layer.
[0089] (exterior) The appearance of the laminated film of each example was evaluated. The appearance of the laminated film according to each example was evaluated by irradiating the surface layer side with light from a sodium lamp in a dark room and visually inspecting the reflection. Specifically, the test was performed by visually checking whether or not there were any defects on the surface layer caused by air bubbles or foreign matter of 100 μm or more. The sodium lamp light was irradiated from a position 50 cm above the surface layer. The appearance was evaluated according to the following criteria, and the results are shown in Table 2 below. Excellent: No defects observed at all. No: Any defects are observed.
[0090] [Table 2]
[0091] From Table 2, the thickness of the bonding layer is T JWhen imaging Raman measurement was performed on the bonding layer after ultraviolet irradiation using Raman spectroscopy, the peak top was measured at a wave number of 1730 cm -1 The intensity of the peak observed at I A The peak top is at wavenumber 1635 cm -1 The intensity of the peak observed at I B When the above T J , I A , and the above I B But the relation T J ×I B / I A It is understood that the laminated films according to the examples, which satisfy the condition of ≧15 μm, are excellent in durable adhesion. That is, it is understood that the laminated film according to each example has a bonding layer having sufficient bonding strength. [Explanation of symbols]
[0092] 1 Base material layer, 2 Surface layer, 3 Bonding layer, 10 Laminated film.
Claims
1. A substrate layer, a surface layer disposed on the substrate layer, and a bonding layer disposed between the substrate layer and the surface layer to bond the substrate layer and the surface layer, The base layer is made of a resin film containing triacetyl cellulose, The surface layer is made of a resin composition containing a photocurable resin, the bonding layer is configured as a compatible layer in which a part of the triacetyl cellulose contained in the base material layer and a part of the photocurable resin contained in the surface layer are compatible with each other, The thickness of the bonding layer is T J μm, When imaging Raman measurement was performed on the bonding layer by Raman spectroscopy, the peak top was at a wave number of 1730 cm -1 The intensity of the peak observed at I A The peak top is at wave number 1635 cm -1 The intensity of the peak observed at I B When Said T J , the above I A , and the I B satisfies the following relation: T J ×I B / I A ≧15.0 μm Laminated film.
2. The thickness T of the bonding layer J is 6.1 μm or more; The laminated film according to claim 1 .
3. The bonding layer has a bonding strength such that it does not peel off from the surface layer even after the surface layer is exposed to light irradiation for 144 hours or more. The laminated film according to claim 1 or 2.
4. The surface layer has a function of a hard coat layer. The laminated film according to claim 1 or 2.
5. A resin composition containing an organic solvent capable of dissolving triacetyl cellulose and a photocurable resin is applied onto a base layer composed of a resin film containing triacetyl cellulose to form a coating layer; and heat-treating the base layer and the coating layer, The heat treatment is carried out so that the maximum temperature is 130° C. or higher. A method for manufacturing a laminated film.
6. In the heat treatment, heating at the maximum temperature is carried out for 20 seconds or more. A method for producing the laminated film according to claim 5.
Citation Information
Patent Citations
Curable composition for forming antireflection film, antireflection film and method for manufacturing the same, polarizing plate, and display device
JP2013205644A