Rubber composition for undertreads

The rubber composition for undertreads uses a blend of isoprene and unmodified butadiene rubbers with large particle size silica and carbon black to enhance handling stability, high-speed durability, and low heat generation, addressing the balance of properties in tire undertreads.

JP2024148178AActive Publication Date: 2024-10-18THE YOKOHAMA RUBBER CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023057958
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-18
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing rubber compositions for undertreads in tires face challenges in balancing handling stability, high-speed durability, and low heat generation, with methods like increasing vulcanizing agents or reducing fillers compromising these properties.

Method used

A rubber composition for undertreads comprising 60-90% isoprene rubber, 10-40% unmodified butadiene rubber, large particle size silica, and specific carbon black, along with a silane coupling agent, to enhance low heat generation, handling stability, and high-speed durability.

Benefits of technology

The composition achieves a well-balanced improvement in handling stability, high-speed durability, and low heat generation by optimizing the blend of isoprene and butadiene rubbers with large particle size silica and carbon black, ensuring excellent physical properties for tire performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148178000001_ABST
    Figure 2024148178000001_ABST
Patent Text Reader

Abstract

To provide a rubber composition for undertreads, which provides improved maneuvering stability and high-speed durability while ensuring good low-heat-generating properties and allows for a high level of balance among these properties.SOLUTION: In the present invention, 3-60 pts.mass of silica having a CTAB adsorption specific surface area of 60-100 m2 / g is added to 100 pts.mass of a rubber component containing 60-90 mass% of an isoprene rubber and 10-40 mass% of an unmodified butadiene rubber. As the unmodified butadiene rubber, one having a molecular weight distribution (Mw / Mn), as determined from the weight average molecular weight (Mw) and the number average molecular weight (Mn), of at most 2.8 is used.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an undertread rubber composition intended primarily for use in the undertread layer of a tire. [Background technology]

[0002] In pneumatic tires, there is a demand for improving fuel efficiency during driving in order to reduce the environmental load. For this reason, efforts have been made to suppress heat generation in rubber compositions constituting various parts of pneumatic tires. In recent years, in order to further improve fuel efficiency, for example, studies have been made on suppressing heat generation in rubber compositions constituting the undertread rubber layer of pneumatic tires (rubber compositions for undertread).

[0003] As an index of heat generation of a rubber composition, tan δ at 60°C (hereinafter referred to as "tan δ(60°C)") measured by dynamic viscoelasticity measurement is generally used, and the smaller the tan δ(60°C) of the rubber composition, the smaller the heat generation. Methods for decreasing the tan δ(60°C) of the rubber composition include, for example, increasing the amount of vulcanizing agent or decreasing the amount of filler such as carbon black (see, for example, Patent Document 1). However, these methods cannot sufficiently secure the breaking elongation required for the rubber composition for undertread, and there is a risk that the steering stability and high-speed durability of the tire are not necessarily sufficient. Therefore, further measures are required for improving the steering stability and high-speed durability while securing good low heat generation (tan δ(60°C)) in the rubber composition for undertread. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-177113 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a rubber composition for undertread which improves steering stability and high-speed durability while ensuring good low heat build-up properties, thereby enabling these performance properties to be simultaneously achieved in a well-balanced manner to a high degree. [Means for solving the problem]

[0006] The rubber composition for undertread of the present invention, which achieves the above object, has a CTAB adsorption specific surface area of ​​60 m for 100 parts by mass of a rubber component containing 60% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of unmodified butadiene rubber. 2 / g~100m 2 The unmodified butadiene rubber is characterized in that it contains 3 parts by mass to 60 parts by mass of silica having a molecular weight of 1.0 to 1.0 g / g, and has a molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of 2.8 or less. Effect of the Invention

[0007] The rubber composition for undertread of the present invention, which is made up of the above-mentioned blending, can improve the driving stability and high-speed durability while ensuring good low heat generation properties. Specifically, by using an isoprene-based rubber and an unmodified butadiene rubber in the above-mentioned blending ratio as the rubber component, it is possible to improve low heat generation properties and high-speed durability in a well-balanced manner. In addition, the rubber component is mixed with large particle size silica (CTAB adsorption specific surface area of ​​60 m 2 / g~100m 2 The rubber is formulated with an appropriate amount of 1.0% tungsten carbide (1.0% / g), which improves low heat buildup. Furthermore, the unmodified butadiene rubber used has a molecular weight distribution (Mw / Mn) of 2.8 or less, which effectively improves the handling stability and high-speed durability of the resulting tire while maintaining good low heat buildup. These two aspects work together to ensure good low heat buildup while improving handling stability and high-speed durability, achieving a good balance between these performance characteristics.

[0008] In the present invention, the CTAB adsorption specific surface area is 40 m per 100 parts by mass of the rubber component. 2 / g~120m 2 It is preferable that 20 to 70 parts by mass of carbon black having a particle size of 1 / g is blended. In addition to the large particle size silica described above, by blending an appropriate amount of carbon black having a specific particle size as a filler, the processability (rubber cohesion, adhesion to other materials, etc.) can be improved.

[0009] In the present invention, the unmodified butadiene rubber preferably has a cis-1,4 bond content of 95% or more. Furthermore, the unmodified butadiene rubber has a 5% by mass toluene solution viscosity Tcp (unit: cps) at 25° C. and a Mooney viscosity ML 1+4 Ratio of TCP / ML 1+4 It is preferable that the relationship between the ratio of the modified butadiene rubber and the axial length of the rubber is 2.0 to 7.0. In addition, it is preferable that the unmodified butadiene rubber is synthesized using a neodymium catalyst. By using an unmodified butadiene rubber that satisfies specific conditions in this way, the effect of improving the low heat buildup and high-speed durability described above can be enhanced, which is advantageous for improving the steering stability and high-speed durability while ensuring good low heat buildup.

[0010] In the present invention, a silane coupling agent can be blended, and in this case, the ratio of the blended amount of the silane coupling agent to the blended amount of silica is preferably 3.0% by mass to 10.0% by mass. This can improve the dispersion of silica, which is advantageous for improving low heat generation and high-speed durability.

[0011] The rubber composition for undertread of the present invention can be suitably used for the undertread layer of a tire. Specifically, a tire using the rubber composition for undertread of the present invention has a tread portion extending in the tire circumferential direction to form an annular shape, and a pair of sidewall portions arranged on both sides of the tread portion, and the tread portion is preferably constructed by laminating a cap tread layer constituting the tire tread surface and an undertread layer arranged on the inner circumferential side of the cap tread layer, and in such a tire, it is preferable that the undertread layer is constructed from the rubber composition for undertread of the present invention. In this way, a tire having an undertread layer made of the rubber composition for undertread of the present invention can improve steering stability and high-speed durability while ensuring good low heat generation due to the excellent physical properties of the rubber composition for undertread of the present invention.

[0012] At this time, the tensile stress M100 of the undertread rubber constituting the undertread layer at 100% elongation at 23°C UT [Unit: MPa] and the tensile stress M100 of the side rubber that constitutes the sidewall at 100% elongation at 23°C SW [Unit: MPa] Ratio to M100 UT / M100 SW It is preferable that the tensile stress (M100) is 1.5 to 4.0. By optimizing the relationship between the tensile stress (M100) of the undertread layer using the rubber composition for undertread of the present invention and the adjacent sidewall portion (side rubber) in this manner, it is advantageous to improve low heat build-up properties and high-speed durability.

[0013] In the present invention, the "CTAB adsorption specific surface area" is measured in accordance with ISO 5794. The "weight average molecular weight Mw" and the "number average molecular weight Mn" are measured by gel permeation chromatography (GPC) in terms of standard polystyrene. The "cis-1,4 bond content" is the proportion of cis-1,4-bonds among the cis-1,4-bonds, trans-1,4-bonds, and 1,2-vinyl bonds, which are the bonding modes of butadiene, and is measured by infrared spectroscopy (Hampton method). The "Mooney viscosity at 100°C ML1+4 " is measured in accordance with JIS K6300-1:2001 using a Mooney viscometer with an L-type rotor, with a preheating time of 1 minute, a rotor rotation time of 4 minutes, and at 100°C. "Viscosity, Tcp, of a 5% by mass toluene solution at 25°C" is the viscosity of a toluene solution containing 5% by weight of the target butadiene rubber, and is measured at 25°C using a Cannon-Fenske viscometer. "Tensile stress at 100% elongation at 23°C" is a value measured in accordance with JIS K6251 using a No. 3 dumbbell test piece at a tensile speed of 500 mm / min and a temperature of 23°C. [Brief description of the drawings]

[0014] [Figure 1] 1 is a meridian cross-sectional view showing an example of a pneumatic tire using the rubber composition for an undertread of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The configuration of the present invention will be described in detail below with reference to the accompanying drawings.

[0016] As shown in FIG. 1, a pneumatic tire in which the rubber composition for undertread of the present invention is used includes a tread portion 1, a pair of sidewall portions 2 arranged on both sides of the tread portion 1, and a pair of bead portions 3 arranged on the tire radially inner side of the sidewall portions 2. In FIG. 1, the symbol CL indicates the tire equator. Although not depicted in FIG. 1 because it is a meridian cross section, the tread portion 1, the sidewall portions 2, and the bead portions 3 each extend in the tire circumferential direction to form an annular shape, thereby forming a toroidal basic structure of a pneumatic tire. The following description using FIG. 1 is basically based on the meridian cross section shown in the figure, but each tire component extends in the tire circumferential direction to form an annular shape.

[0017] A carcass layer 4 is installed between a pair of left and right bead portions 3. This carcass layer 4 includes a plurality of reinforcing cords extending in the tire radial direction, and is folded back from the inner side to the outer side in the tire width direction around a bead core 5 arranged in each bead portion 3. A bead filler 6 is arranged on the outer periphery of the bead core 5, and this bead filler 6 is wrapped by the main body and the folded back portion of the carcass layer 4. Meanwhile, a plurality of belt layers 7 (two layers in FIG. 1) are embedded on the outer periphery side of the carcass layer 4 in the tread portion 1. Each belt layer 7 includes a plurality of reinforcing cords inclined with respect to the tire circumferential direction, and the reinforcing cords are arranged so as to cross each other between the layers. In these belt layers 7, the inclination angle of the reinforcing cords with respect to the tire circumferential direction is set to, for example, a range of 10° to 40°. Furthermore, a belt reinforcing layer 8 (two layers, a full cover 8a covering the entire width of the belt layer 7 and an edge cover 8b locally covering the end portion of the belt layer 7) is provided on the outer periphery side of the belt layer 7. The belt reinforcing layer 8 includes organic fiber cords oriented in the tire circumferential direction. In the belt reinforcing layer 8, the organic fiber cords are set at an angle of, for example, 0° to 5° with respect to the tire circumferential direction.

[0018] A tread rubber layer 10 is disposed on the outer peripheral side of the carcass layer 4 in the tread portion 1, a side rubber layer 20 is disposed on the outer peripheral side (outside in the tire width direction) of the carcass layer 4 in the sidewall portion 2, and a rim cushion rubber layer 30 is disposed on the outer peripheral side (outside in the tire width direction) of the carcass layer 4 in the bead portion 3. The tread rubber layer 11 has a structure in which two types of rubber layers with different physical properties (a cap tread 11 that forms the tread surface of the tread portion 1 and an undertread 12 disposed on its inner peripheral side) are laminated in the tire radial direction.

[0019] The tire in which the rubber composition for undertread of the present invention is used is preferably a pneumatic tire (a tire filled with air, an inert gas such as nitrogen, or other gas) as described above, but may be a non-pneumatic tire. In the case of a non-pneumatic tire, the rubber composition for undertread of the present invention can be used in a rubber layer (a portion corresponding to the undertread layer 12 in a pneumatic tire) arranged on the inner periphery side of a portion that contacts the road surface (a portion corresponding to the cap tread layer 11 in a pneumatic tire). As long as the tread portion 1 (tread rubber layer 10) of the tire to which the present invention is applied is composed of the cap tread 11 and the undertread 12, the basic structure of the other portions is not limited to the above-mentioned structure.

[0020] In the rubber composition for undertread of the present invention, the rubber component is a diene rubber, and necessarily contains an isoprene rubber and an unmodified butadiene rubber. By using the isoprene rubber and the unmodified butadiene rubber in this manner, it is advantageous to improve low heat generation while maintaining good elongation at break.

[0021] Examples of isoprene-based rubber include various natural rubbers, epoxidized natural rubbers, and various synthetic polyisoprene rubbers. Among these isoprene-based rubbers, natural rubbers are particularly suitable. The content of isoprene-based rubber is 60% by mass to 90% by mass, preferably 65% ​​by mass to 90% by mass, and more preferably 70% by mass to 90% by mass, based on 100% by mass of the rubber component. By including such an amount of isoprene-based rubber (particularly natural rubber), it is possible to improve the elongation at break and low heat build-up properties in a well-balanced manner. If the amount of isoprene-based rubber is less than 60% by mass, the elongation at break decreases. If the amount of isoprene-based rubber is more than 90% by mass, the low heat build-up properties deteriorate.

[0022] The unmodified butadiene rubber used has a molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of 2.8 or less, preferably 2.5 or less. By using an unmodified butadiene rubber having a suitable molecular weight distribution, the rubber physical properties become better, and the handling stability and high-speed durability of a tire can be effectively improved while maintaining low heat buildup. If the molecular weight distribution (Mw / Mn) of the unmodified butadiene rubber exceeds 2.8, the hysteresis loss increases, the heat buildup of the rubber increases, and the compression set resistance decreases.

[0023] The content of the unmodified butadiene rubber is 10% by mass to 40% by mass, preferably 15% by mass to 35% by mass, and more preferably 20% by mass to 35% by mass, based on 100% by mass of the rubber component. By appropriately including the unmodified butadiene rubber in this manner, it is advantageous to improve the elongation at break and the low heat build-up property in a well-balanced manner. If the amount of the unmodified butadiene rubber is less than 10% by mass, the low heat build-up property deteriorates. If the amount of the unmodified butadiene rubber is more than 40% by mass, the elongation at break decreases.

[0024] The cis-1,4 bond content of the unmodified butadiene rubber is preferably 95% or more, more preferably 96% to 99%. A high cis-1,4 bond content is advantageous for improving the breaking strength and breaking elongation. If the cis-1,4 bond content is less than 95%, the breaking strength and breaking elongation decrease. The cis-1,4 bond content of the butadiene rubber can be increased or decreased by a normal method such as a catalyst.

[0025] The viscosity of a 5% by mass toluene solution at 25°C, Tcp (unit: cps), and the Mooney viscosity at 100°C, ML 1+4 Ratio of TCP / ML 1+4 The ratio Tcp / ML preferably satisfies the relationship of 2.0 to 7.0, and more preferably 2.5 to 6.8. 1+4 By setting the ratio Tcp / ML within a specific range, it is advantageous to achieve low heat generation, breaking strength, and breaking elongation at the same time. 1+4If the ratio Tcp / ML is less than 2.0, the low heat generation property is deteriorated. 1+4 If it exceeds 7.0, the processability deteriorates.

[0026] The above ratio TCP / ML 1+4 When setting, the value of the viscosity Tcp of a 5% by mass toluene solution at 25°C is not particularly limited, but it can be set to preferably 50 cps to 200 cps, more preferably 80 cps to 180 cps. Similarly, the Mooney viscosity ML 1+4 The value itself is not particularly limited, but can be set preferably to 45-52, and more preferably to 45-50.

[0027] The unmodified butadiene rubber is preferably butadiene rubber synthesized using a neodymium catalyst (hereinafter, sometimes referred to as Nd-BR). Although the desired effect can be obtained by using butadiene rubber polymerized with other catalysts (e.g., nickel or cobalt), Nd-BR is preferably used from the viewpoint of achieving both low heat generation, breaking strength, and breaking elongation.

[0028] In addition, butadiene rubber polymerized using a neodymium-based catalyst (Nd-BR) is a known material, and is butadiene rubber polymerized using a neodymium-based catalyst such as simple neodymium, compounds of neodymium with other metals, or organic neodymium compounds. Butadiene rubber synthesized using these neodymium-based catalysts has the characteristics of a high molecular weight and a sharp molecular weight distribution. Commercially available Nd-BR can be used.

[0029] The rubber component constituting the rubber composition for undertread of the present invention includes at least two types of isoprene-based rubber (particularly natural rubber) and unmodified butadiene rubber as described above, but may optionally contain other diene-based rubber. As the other diene-based rubber, a rubber that can be generally used in rubber compositions for tires can be used. For example, unmodified styrene-butadiene rubber can be exemplified. In addition, when natural rubber is adopted as the isoprene-based rubber, isoprene rubber can also be used in combination as the other diene-based rubber. These other diene-based rubbers can be used alone or as an arbitrary blend.

[0030] In the present invention, silica is necessarily blended as a filler with the above-mentioned rubber component. As the silica used in the present invention, for example, silica usually used in rubber compositions for tires, such as wet process silica, dry process silica, or surface-treated silica, can be used. However, the CTAB adsorption specific surface area of ​​silica is 60 m 2 / g~100m 2 / g, preferably 70m 2 / g~90m 2 / g, more preferably 75m 2 / g~85m 2 / g. By using silica with such a large particle size, it is possible to improve low heat generation and wear resistance. 2 If the CTAB adsorption specific surface area of ​​silica is less than 100 m 2 If the silica satisfies the above-mentioned conditions, it may be appropriately selected from commercially available products and used, or silica obtained by a conventional manufacturing method may be used.

[0031] The amount of silica to be blended is 3 to 60 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 50 parts by mass, per 100 parts by mass of the rubber component. By blending an appropriate amount of silica in this manner, it is possible to improve the low heat build-up properties, steering stability, and high-speed durability of a tire in a well-balanced manner. If the amount of silica blended is less than 3 parts by mass, the elongation at break decreases. If the amount of silica blended exceeds 60 parts by mass, the low heat build-up properties deteriorate.

[0032] In the present invention, in addition to the above-mentioned silica, carbon black can also be blended as a filler. The carbon black used in the present invention is preferably a carbon black having a CTAB adsorption specific surface area of ​​40 m among the carbon blacks usually used in rubber compositions for tires. 2 / g~120m 2 / g, more preferably 70m 2 / g~100m 2 / g. Using such carbon black is advantageous in improving the balance of low heat generation, driving stability, and high-speed durability when made into a tire. The CTAB adsorption specific surface area of ​​carbon black is 40 m 2 If the CTAB adsorption specific surface area of ​​carbon black is less than 120 m 2 If it exceeds 1 / g, the low heat build-up property deteriorates.

[0033] When carbon black is used in addition to silica as described above, the total amount of silica and carbon black is preferably 40 to 95 parts by mass, more preferably 45 to 90 parts by mass, per 100 parts by mass of the rubber component. By mixing an appropriate amount of silica and carbon black in this way, it is advantageous to improve low heat build-up, steering stability, and high-speed durability in a well-balanced manner when the tire is made. If the total amount of silica and carbon black is less than 40 parts by mass, the breaking strength decreases and the high-speed durability deteriorates. If the total amount of silica and carbon black is more than 95 parts by mass, fuel efficiency deteriorates and the breaking elongation decreases.

[0034] Furthermore, when silica and carbon black are used in combination, the ratio Ms / Mc of the amount of silica to the amount of carbon black, Mc, is preferably 0.05 to 0.7, more preferably 0.1 to 0.6. In this way, by blending silica and carbon black in a suitable balance, and particularly by keeping the amount of silica in the filler low, it is possible to suppress the deterioration of tan δ(60°C) caused by blending large particle size silica, and to improve the elongation at break and low heat build-up in a well-balanced manner. If the ratio Ms / Mc of the amount of silica to the amount of carbon black exceeds 0.7, the processability (rubber cohesion, adhesion to other components, etc.) will deteriorate.

[0035] The rubber composition of the present invention may contain fillers other than silica and carbon black, such as clay, talc, calcium carbonate, mica, aluminum hydroxide, and other materials that are generally used in rubber compositions for tires.

[0036] In the rubber composition for undertread of the present invention, a silane coupling agent may be blended when blending the above-mentioned silica. Blending the silane coupling agent can improve the dispersibility of silica in the rubber component (diene rubber). Examples of the silane coupling agent include bis-(3-triethoxysilylpropyl) tetrasulfide, bis(3-triethoxysilylpropyl) disulfide, 3-trimethoxysilylpropyl benzothiazole tetrasulfide, γ-mercaptopropyl triethoxysilane, and 3-octanoylthiopropyl triethoxysilane. Among these, those having a tetrasulfide bond in the molecule can be preferably used. The blending amount of the silane coupling agent is preferably 3.0 mass% to 10 mass%, more preferably 4.0 mass% to 9.0 mass%, based on the blending amount of silica. If the blending amount of the silane coupling agent is less than 3.0 mass% of the blending amount of silica, the blending amount is so small that the effect of blending the silane coupling agent cannot be expected sufficiently. If the amount of the silane coupling agent exceeds 10 mass % of the amount of silica, the silane coupling agents will condense with each other, making it difficult to obtain the desired hardness and strength in the rubber composition.

[0037] Other compounding agents than those mentioned above can be added to the rubber composition for undertread of the present invention. Examples of other compounding agents include various compounding agents generally used in rubber compositions for tires, such as vulcanizing or crosslinking agents, vulcanization accelerators, antiaging agents, and liquid polymers. The compounding amounts of these compounding agents can be conventional general compounding amounts as long as they do not go against the object of the present invention. In addition, as the kneading machine, a normal rubber kneading machine, such as a Banbury mixer, a kneader, or a roll, can be used.

[0038] The rubber composition for undertread of the present invention can be suitably used in the undertread layer of a tire as described above, and a tire having an undertread layer made of the rubber composition for undertread of the present invention can improve the driving stability and high-speed durability while ensuring good low heat generation due to the excellent physical properties of the rubber composition for undertread of the present invention. When the rubber composition for undertread of the present invention is used in a tire, the tensile stress M100 at 100% elongation at 23°C of the undertread rubber constituting the undertread layer (i.e., the vulcanizate of the rubber composition for undertread of the present invention) is 0.01 to 0.01 mm. UT [Unit: MPa] and the tensile stress M100 of the side rubber that constitutes the sidewall at 100% elongation at 23°C SW [Unit: MPa] Ratio to M100 UT / M100 SW The ratio M100 is preferably 1.5 to 4.0, and more preferably 1.8 to 3.5. By optimizing the relationship of the tensile stress (M100) between the undertread layer using the rubber composition for undertread of the present invention and the adjacent sidewall portion (side rubber), it is advantageous to improve the driving stability and high-speed durability while ensuring low heat buildup. UT / M100 SW If the ratio is less than 1.5, the effects of improving low heat generation, steering stability, and high-speed durability are limited. UT / M100 SW If the value exceeds 4.0, the effects of improving low heat generation, driving stability, and high-speed durability become limited.

[0039] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES

[0040] The tire size is 245 / 45R18, and has the basic structure shown in FIG. 1. The compounding of the rubber composition for the undertread and the tensile stress (M100) at 100% elongation at 23°C of the undertread rubber and the side rubber are UT , M100 SW ) and its ratio M100UT / M100 SW Tires (test tires) of Standard Example 1, Comparative Examples 1 to 7, and Examples 1 to 8 were manufactured, each having a different value as shown in Tables 1 and 2.

[0041] Regarding the compounding of the rubber composition for undertread, the compounding common to all the examples is summarized in Table 3. The type of side rubber used in each example is also shown in Tables 1 and 2. The type of side rubber is indicated by the numbers of side rubbers A to B shown in Table 4, and the compounding of these side rubbers A to B is as shown in Table 4.

[0042] The tensile stress (M100 UT , M100 SW ) is the value (unit: MPa) measured using undertread rubber and side rubber, using a No. 3 dumbbell test piece prepared in accordance with JIS K6251, at a tensile speed of 500 mm / min and a temperature of 23°C.

[0043] Using each test tire, evaluations of steering stability, low rolling resistance, and high-speed durability were carried out by the methods described below.

[0044] Steering stability Each test tire was mounted on a wheel with a rim size of 18x7J, the air pressure was set to 240kPa, and the tire was mounted on a test vehicle with an engine displacement of 2000cc. The test driver performed a sensory evaluation of the handling stability on a test course consisting of a paved road surface. The evaluation results were evaluated on a 5-point scale, with the result of Standard Example 1 being 3 points (standard). The higher the score, the better the handling stability.

[0045] Low rolling resistance Each test tire was mounted on a wheel with a rim size of 18x7J, and the rolling resistance was measured using an indoor drum test machine (drum diameter: 1707.6mm) in accordance with ISO28580 under conditions of air pressure of 210kPa, load of 4.82kN, and speed of 80km / h. The evaluation results were expressed as an index using the reciprocal of the measured value, with standard example 1 being 100. The higher the index value, the lower the rolling resistance and the better the low rolling resistance.

[0046] fast durability Each test tire was mounted on a wheel with a rim size of 18x7J, and a running test was carried out on an indoor drum test machine (drum diameter: 1707.6mm) under the conditions of an air pressure of 340kPa, a load of 5kN, and a negative camber angle of 3°. Specifically, the initial speed was 250km / h, and the speed was increased by 10km / h every 20 minutes, and the tire was run until failure occurred, and the steps (speed) reached were measured. The evaluation results were expressed as an index with the measured value (speed) of standard example 1 set to 100. The higher the index value, the greater the steps (speed) reached until failure, meaning that the tire has excellent high-speed durability with a camber angle.

[0047] [Table 1]

[0048] [Table 2]

[0049] [Table 3]

[0050] The types of raw materials used in Tables 1 to 3 are shown below. NR: Natural rubber, RSS#3 BR1: Nipol 1220 manufactured by Zeon Corporation (butadiene rubber synthesized using a cobalt catalyst, cis-1,4 bond content: 98 mol%, Mw / Mn=2.9, Tcp / ML 1+4 =1.4) BR2: Nipol 1250H manufactured by Zeon Corporation (butadiene rubber synthesized using a lithium catalyst, cis-1,4 bond content: 35 mol%, Mw / Mn=1.4) BR3: UBEPOL BR360L manufactured by Ube Industries (butadiene rubber synthesized using a cobalt catalyst, cis-1,4 bond content: 98 mol%, Mw / Mn=2.2, Tcp / ML1+4 =2.8) BR4: ARLANXEO Buna CB22 (butadiene rubber synthesized using neodymium catalyst, cis-1,4 bond content: 98 mol%, Mw / Mn=2.3, Tcp / ML 1+4 =6.5) BR5: Buna CB24 manufactured by ARLANXEO (butadiene rubber synthesized using a neodymium catalyst, cis-1,4 bond content: 96 mol%, Mw / Mn=2.0) CB1: Carbon black (grade: ISAF), manufactured by Tokai Carbon Co., Ltd., SEAT 6 (CTAB adsorption specific surface area: 109 m 2 / g) CB2: Carbon black (grade: HAF), manufactured by Tokai Carbon Co., Ltd., SEAT 3 (CTAB adsorption specific surface area: 82 m 2 / g) CB3: Carbon black (grade: FEF), manufactured by Tokai Carbon Co., Ltd., SEAT F (CTAB adsorption specific surface area: 47 m 2 / g) ·Silica 1: Evonik ULTRASIL VN3GR (CTAB adsorption specific surface area: 175m 2 / g) Silica 2: Solvay ZEOSIL 115GR (CTAB adsorption specific surface area: 115 m 2 / g) Silica 3: Solvay Zeosil 1185GR (CTAB adsorption specific surface area: 80 m 2 / g) Silane coupling agent: Si69 manufactured by Evonik Industries AG Stearic acid: Stearic acid 50S manufactured by Nisshin Rika Co., Ltd. Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. · Anti-aging agent: PILFLEX 13 by NOCIL LIMITED Tackifier: Hitachi Chemical's Hitanol 1502Z Sulfur: Shikoku Chemical Industry Co., Ltd., Myucron OT-20 Vulcanization accelerator: Sancerer NS-G manufactured by Sanshin Chemical Industry Co., Ltd.

[0051] [Table 4]

[0052] The types of raw materials used in Table 4 are shown below. NR: Natural rubber, natural rubber, RSS#3 BR: Nippon Zeon Nipol 1220 CB: Carbon black (grade: FEF), manufactured by Tokai Carbon Co., Ltd., SEAT F (CTAB adsorption specific surface area: 47 m 2 / g) Tackifier: Hitachi Chemical's Hitanol 1502Z Zinc oxide: Three types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. · Anti-aging agent: PILFLEX 13 by NOCIL LIMITED Stearic acid: Stearic acid 50S manufactured by Nisshin Rika Co., Ltd. Aroma oil: Aromax T-DAE, manufactured by ENEOS Sulfur: Sulfax 5 manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator: Sancerer NS-G manufactured by Sanshin Chemical Industry Co., Ltd.

[0053] As is clear from Tables 1 and 2, Examples 1 to 8 improved the steering stability, low rolling resistance, and high-speed durability compared to Standard Example 1, and these performances were well balanced. On the other hand, in Comparative Example 1, the low rolling resistance was deteriorated because the CTAB specific surface area of ​​silica was large. In Comparative Example 2, the low rolling resistance was deteriorated because the CTAB specific surface area of ​​silica was large. In Comparative Example 3, the high-speed durability was deteriorated because a modified butadiene rubber was used. In Comparative Example 4, the high-speed durability was deteriorated because the compounding amount of silica was small. In Comparative Example 5, the steering stability was deteriorated because the compounding amount of silica was large. In Comparative Example 6, the compounding amount of isoprene-based rubber (natural rubber) was large and the compounding amount of unmodified butadiene rubber was small, so the low rolling resistance was deteriorated. In Comparative Example 7, the compounding amount of isoprene-based rubber (natural rubber) was small and the compounding amount of unmodified butadiene rubber was large, so the steering stability and high-speed durability were deteriorated.

[0054] The present disclosure includes the following inventions. Invention [1] A rubber composition having a CTAB adsorption specific surface area of ​​60 m for 100 parts by mass of a rubber component containing 60% by mass to 90% by mass of isoprene-based rubber and 10% by mass to 40% by mass of unmodified butadiene rubber. 2 / g~100m 2 and a molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of the unmodified butadiene rubber is 2.8 or less. Invention [2] The CTAB adsorption specific surface area is 40 m per 100 parts by mass of the rubber component. 2 / g~120m 2 The rubber composition for undertread according to the invention [1], characterized in that 20 parts by mass to 70 parts by mass of carbon black having a molecular weight of 1 / g are blended. Invention [3] The rubber composition for undertread according to invention [1] or [2], wherein the unmodified butadiene rubber has a cis-1,4 bond content of 95% or more. Invention [4] The unmodified butadiene rubber has a 5% by mass toluene solution viscosity Tcp (unit: cps) at 25°C and a Mooney viscosity ML 1+4 Ratio of TCP / ML 1+4 The rubber composition for undertread according to any one of inventions [1] to [3], wherein the relationship satisfies: Invention [5] The rubber composition for undertread according to any one of inventions [1] to [4], wherein the unmodified butadiene rubber is synthesized using a neodymium-based catalyst. Invention [6] The rubber composition for undertread according to any one of inventions [1] to [5], characterized in that a silane coupling agent is blended therein, and the ratio of the blending amount of the silane coupling agent to the blending amount of the silica is 3.0% by mass to 10.0% by mass. Invention [7] A tire comprising a tread portion extending in a circumferential direction of the tire to form an annular shape, and a pair of sidewall portions arranged on both sides of the tread portion, the tread portion being constructed by laminating a cap tread layer constituting the tire surface and an undertread layer arranged on its inner side, the undertread layer being constructed from the rubber composition for undertread according to any one of inventions [1] to [6]. Invention [8] The tensile stress M100 of the undertread rubber constituting the undertread layer at 100% elongation at 23°C UT [Unit: MPa] and the tensile stress M100 of the side rubber constituting the sidewall portion at 100% elongation at 23°C SW [Unit: MPa] Ratio to M100 UT / M100 SW The tire according to the invention [7], characterized in that the ratio of the axial length of the tire to the radial length of the tire is 1.5 to 4.0. [Explanation of symbols]

[0055] 1 Tread section 2 Sidewall 3 Bead section 4 Carcass layer 5 Bead Core 6 Bead Filler 7 Belt layer 8 Belt cover layer 10 Tread rubber layer 11 Cap tread layer 12 Undertread layer 20 Side rubber layer 30 Rim cushion rubber layer CL Tire Equator

Claims

1. A rubber component having a CTAB adsorption specific surface area of ​​60 m for 100 parts by mass of a rubber component containing 60% by mass to 90% by mass of an isoprene-based rubber and 10% by mass to 40% by mass of an unmodified butadiene rubber. 2 / g to 100m 2 and a molecular weight distribution (Mw / Mn) calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn) of the unmodified butadiene rubber is 2.8 or less.

2. A CTAB adsorption specific surface area of ​​40 m per 100 parts by mass of the rubber component. 2 / g ~ 120m 2 2. The rubber composition for undertread according to claim 1, characterized in that 20 to 70 parts by mass of carbon black having a viscosity of 1 / g is blended.

3. 3. The rubber composition for undertread according to claim 1, wherein the unmodified butadiene rubber has a cis-1,4 bond content of 95% or more.

4. The unmodified butadiene rubber has a 5% by mass toluene solution viscosity Tcp (unit: cps) at 25° C. and a Mooney viscosity ML at 100° C. 1+4 Ratio of Tcp / ML 1+4 The rubber composition for undertread according to claim 1 or 2, characterized in that the relationship of is 2.0 to 7.

0.

5. 3. The rubber composition for an undertread according to claim 1, wherein the unmodified butadiene rubber is synthesized using a neodymium-based catalyst.

6. 3. The rubber composition for undertread according to claim 1, further comprising a silane coupling agent, the ratio of the amount of the silane coupling agent to the amount of the silica being 3.0% by mass to 10.0% by mass.

7. A tire comprising a tread portion extending in a circumferential direction of the tire to form an annular shape and a pair of sidewall portions disposed on both sides of the tread portion, the tread portion being constructed by laminating a cap tread layer constituting the tire tread surface and an undertread layer disposed on an inner side of the cap tread layer, the undertread layer being constructed from the rubber composition for undertreads according to claim 1 or 2.

8. The tensile stress M100 of the undertread rubber constituting the undertread layer at 100% elongation at 23°C UT [Unit: MPa] and the tensile stress M100 of the side rubber constituting the sidewall portion at 100% elongation at 23°C SW Ratio M100 to [unit: MPa] UT / M100 SW 8. The tire according to claim 7, wherein the tread width is 1.5 to 4.0.

Citation Information

Patent Citations

  • Rubber composition for tire, and pneumatic tire

    JP2012219224A

  • Pneumatic tire

    JP2013177113A

  • Rubber composition for tire

    JP2019026757A

  • Rubber composition for tread, and tire

    JP2019151738A

  • Rubber composition and tire made therefrom

    JP2023069115A