Method for producing pitch for carbon material production and naphthalene
The method of heat treating ethylene bottom oil, separating and recovering naphthalene from low-boiling components, addresses the inefficiencies in pitch production by enhancing the yield of high-value naphthalene and pitch for carbon materials.
Patent Information
- Application Number
- JP2023061675
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Existing methods for producing pitch from ethylene bottom oil yield low-boiling components as low-value by-products, with little investigation into their effective utilization, while the production of high-value naphthalene from these components is not adequately addressed.
A method involving heat treatment of ethylene bottom oil, followed by distillation to separate high-boiling pitch and low-boiling components, with a step to recover naphthalene from the latter, optimizing conditions such as temperature and time to enhance naphthalene recovery.
Efficient production of pitch suitable for carbon materials and high-purity naphthalene from ethylene bottom oil, increasing the value of the process by utilizing low-boiling components effectively.
Smart Images

Figure 2024148495000003 
Figure 2024148495000001 
Figure 2024148495000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing pitch for producing carbon materials and naphthalene. [Background technology]
[0002] Heavy residual oil (ethylene bottom oil) produced as a by-product when olefins such as ethylene and propylene are produced by steam cracking or thermal cracking of petroleum hydrocarbons such as naphtha is mostly used as fuel, with only a portion of it being used as a raw material for carbon black. Therefore, converting this ethylene bottom oil into a product with high added value is a problem in the technical field. In order to solve this problem, attempts have been made to produce pitch for producing carbon materials from ethylene bottom oil by taking advantage of the characteristics of ethylene bottom oil that contains a large amount of aromatic compounds. Various methods for producing pitch for producing carbon materials from ethylene bottom oil have been reported, but one of the most common methods is a method for producing pitch for producing carbon materials that includes a step of heat treating ethylene bottom oil (heat treatment step) and a step of distilling the heat-treated product obtained in the heat treatment step to obtain pitch as a high-boiling point component (distillation step) (Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 53-60927 [Patent Document 2] Japanese Patent Application Publication No. 49-35420 [Patent Document 3] Japanese Patent Publication No. 51-83622 Summary of the Invention [Problem to be solved by the invention]
[0004] In the methods for producing pitch for carbon material production from ethylene bottom oil, as typified by Patent Documents 1 to 3, the yield of pitch for carbon material production is about 20% by mass to 50% by mass, depending on the composition of the raw materials used, the conditions of each process, etc. The remaining low-boiling point components produced as by-products are still low-added-value fractions, but as far as the present inventors know, there have been almost no studies conducted on methods for effectively utilizing these low-boiling point components.
[0005] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing pitch for carbon material production and naphthalene, which can produce pitch for carbon material production from ethylene bottom oil and can also produce high added value naphthalene from the by-produced low boiling point component. [Means for solving the problem]
[0006] The present inventors conducted extensive research to achieve the above object, and as a result, obtained the following findings. For the purpose of producing pitch for carbon material production, ethylene bottom oil was heat-treated, and the heat-treated product was distilled to produce pitch for carbon material production as a high-boiling component. The low-boiling components by-produced during the process were analyzed in detail, and it was found that the low-boiling components contain a large amount of naphthalene. Based on this finding, the inventors further investigated the production of naphthalene as a chemical product in parallel with the production of pitch for carbon material production from ethylene bottom oil, and as a result, the present invention was completed.
[0007] That is, the present invention relates to the following [1] to [5].
[0008] [1] A method for producing pitch and naphthalene for use in producing carbon materials, comprising the steps of: heat-treating petroleum heavy oil (step 1); distilling the heat-treated product obtained in step 1 and separating it into pitch, which is a high-boiling component, and low-boiling components (step 2); and recovering naphthalene from the low-boiling components obtained in step 2 (step 3). [2] The method for producing pitch for producing carbon materials and naphthalene according to [1], wherein the petroleum heavy oil is at least one selected from the group consisting of ethylene bottom oil and ethylene bottom oil light fraction. [3] The method for producing pitch for producing carbon materials and naphthalene according to [1] or [2], wherein the naphthalene concentration in the petroleum heavy oil is 5% by mass to 60% by mass. [4] The method for producing pitch for producing carbon materials and naphthalene according to any one of [1] to [3], wherein the heat treatment temperature in the step 1 is 360° C. to 480° C., and the heat treatment time is 0.5 hours to 48 hours. [5] The method for producing pitch for producing a carbon material and naphthalene according to any one of [1] to [4], wherein the carbon material is a graphite electrode. Effect of the Invention
[0009] According to the present invention, pitch for producing carbon materials and naphthalene can be obtained from petroleum heavy oil. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a flow diagram showing a petrochemical process for thermally cracking naphtha or the like and a process for producing ethylene bottom oil.
[0011] Preferred embodiments of the present invention will be described below, but it should be understood that the present invention is not limited to these embodiments and that various applications are possible within the spirit and scope of the present invention.
[0012] In this specification, when "to" is used to describe a numerical range, the numerical values at both ends are the upper and lower limits, respectively, and are included in the numerical range.
[0013] A method for producing pitch and naphthalene for producing a carbon material according to one embodiment includes at least the following steps 1 to 3 in this order, and other steps may be added. Process 1 (heat treatment process): Process for heat treating petroleum-based heavy oil Step 2 (distillation step): The heat-treated product obtained in step 1 is distilled and separated into pitch, which is a high-boiling component, and low-boiling components. Step 3 (naphthalene recovery step): A step of recovering naphthalene from the low boiling point components obtained in step 2.
[0014] The naphthalene concentration in the petroleum heavy oil used as the raw material is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The naphthalene concentration in the petroleum heavy oil used as the raw material is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less. These upper and lower limit values can be arbitrarily combined. A preferred range is 5% by mass to 60% by mass, more preferably 10% by mass to 50% by mass, and even more preferably 15% by mass to 40% by mass. If the naphthalene concentration in the petroleum heavy oil is 5% by mass to 60% by mass, depending on the heat treatment conditions in step 1, the distillation conditions in step 2, and the like, a low-boiling point component containing naphthalene at a relatively high concentration can be obtained in step 2, so that naphthalene can be efficiently recovered in step 3. The method for measuring the naphthalene concentration is not particularly limited, but for example, an internal standard method using gas chromatography can be used.
[0015] The petroleum heavy oil used as the raw material is not particularly limited, but is preferably one that satisfies the above naphthalene concentration, and is preferably ethylene bottom oil or an ethylene bottom oil light fraction obtained by separating an arbitrary ratio (for example, 5% by mass to 70% by mass) of light fractions from ethylene bottom oil by distillation or the like. At least one selected from the group consisting of ethylene bottom oil and ethylene bottom oil light fractions may be used with the addition of heavy oils such as fluid catalytic cracking oil (FCC decant oil), atmospheric distillation residual oil, vacuum distillation residual oil, various petroleum heavy oils hydrotreated, cracked kerosene, and coal tar. In this case, the amount of heavy oil added is preferably within a range that satisfies the above naphthalene concentration. In one embodiment, the petroleum heavy oil is preferably at least one selected from the group consisting of ethylene bottom oil and ethylene bottom oil light fractions.
[0016] In the petrochemical industry, naphtha and other fuels are generally cracked at high temperatures, and the resulting cracked material is distilled to separate it into various fractions, such as ethylene, propylene and other olefins, aromatic compounds such as benzene, toluene and xylene, cracked gasoline, cracked kerosene, etc., to produce the final products. Of these fractions, the heavy fraction with the highest boiling point is called ethylene bottom oil, and is used as a raw material and fuel for carbon black and other products (see Figure 1). Thermal cracking plants for naphtha and other fuels are often called ethylene plants, so the aforementioned heavy fraction is called ethylene bottom oil.
[0017] The properties of ethylene bottom oil obtained by thermal cracking of naphtha-containing raw materials vary depending on the type of naphtha-containing raw material, thermal cracking conditions, operating conditions of the refining distillation column, etc., but the general properties are as follows: 50% distillation temperature is 200°C to 400°C, aromatic carbon content is 50 mass% or more, flash point is 70°C to 100°C, 50°C kinematic viscosity is 40mm 2 / s and the naphthalene concentration is 5% by mass to 25% by mass. However, since ethylene bottom oil is a mixture of hydrocarbon compounds, the above values may vary to some extent.
[0018] (Step 1: Heat treatment step) Step 1 is a step of heat treating petroleum heavy oil. The heat treatment is preferably carried out in a closed vessel in a non-oxidizing gas atmosphere. Examples of non-oxidizing gases include nitrogen gas, argon gas, hydrogen gas, lower alkanes such as methane and ethane, and mixed gases of these non-oxidizing gases. From the viewpoints of cost and ease of handling, nitrogen gas is preferred.
[0019] The heat treatment temperature is preferably 360° C. or higher, and more preferably 380° C. or higher. The heat treatment temperature is preferably 480° C. or lower, and more preferably 450° C. or lower. These upper and lower limit values can be combined arbitrarily. A preferred range is 360° C. to 480° C., and more preferably 380° C. to 450° C.
[0020] The heat treatment time is preferably 0.5 hours or more, and more preferably 1 hour or more, from the time when the predetermined heat treatment temperature is reached. The heat treatment time is preferably 48 hours or less, more preferably 24 hours or less, and even more preferably 12 hours or less, from the time when the predetermined heat treatment temperature is reached. These upper and lower limit values can be arbitrarily combined. The preferred range is 0.5 hours to 48 hours, more preferably 0.5 hours to 24 hours, and even more preferably 1 hour to 12 hours.
[0021] By performing heat treatment under conditions that satisfy the above heat treatment temperature and heat treatment time, it is possible to obtain pitch having properties that are particularly suitable for producing carbon materials such as graphite electrodes. This pitch can be used as a binder pitch and an impregnating pitch in the production of carbon materials such as graphite electrodes.
[0022] The pressure at the start of the heat treatment (initial pressure) is preferably 0 MPaG, but there is no particular limit. The pressure inside the sealed container rises due to hydrogen gas generated by thermal decomposition during the heat treatment, and lower alkanes such as methane and ethane. There is no limit to the pressure inside the sealed container, but it is possible to release the pressure as necessary.
[0023] (Step 2: Distillation step) Step 2 is a step of obtaining pitch, which is a high-boiling component, and low-boiling components by distilling the heat-treated product obtained in step 1. The distillation method in step 2 may be any of atmospheric distillation, reduced-pressure distillation (vacuum distillation), or a combination of atmospheric distillation and reduced-pressure distillation, and can be appropriately selected. It is preferable that the internal temperature of the distillation apparatus does not exceed 360°C. If the temperature exceeds 360°C, reactions such as polymerization are likely to occur, and coking may occur on the inner wall of the distillation apparatus. The lower limit temperature does not affect the characteristics of the pitch, but if the temperature is low, the distillation pressure must be lowered to distill off the low-boiling components, so that from the viewpoint of economy, 200°C or higher is preferable. The preferred distillation conditions vary depending on the softening point of the pitch to be produced. In general, the more the amount of low-boiling components removed, the higher the softening point of the pitch obtained.
[0024] Since the petroleum heavy oil after heat treatment, which is the distillation target, is a mixture of components with different boiling points, the distillation conditions in step 2 cannot be determined uniquely. Therefore, in step 2, 50 to 75 mass% of the petroleum heavy oil after heat treatment may be distilled off to obtain a "low boiling point component". The 5 mass% distillation temperature of the "low boiling point component" at normal pressure is preferably 250°C or less, more preferably 220°C or less, and even more preferably 200°C or less. The 90 mass% distillation temperature of the "low boiling point component" at normal pressure is preferably 360°C or less, more preferably 330°C or less, and even more preferably 300°C or less. The method for measuring the distillation properties of the "low boiling point component" is not particularly limited, but it is preferable to select an appropriate method from JIS K 2254:2018, ASTM D7500-15, and ASTM D7169-16 according to the type of the low boiling point component and measure it. The "high boiling point component" refers to the component remaining in the distillation apparatus after the distillation process (so-called bottom residue). It is possible to directly introduce the distilled low boiling point components into step 3, but if an intermediate boiling point fraction with a boiling point of about 190°C to 230°C, which contains naphthalene at a high concentration, is introduced into step 3, naphthalene can be recovered more efficiently.
[0025] (Process 3: Naphthalene recovery process) Step 3 is a step of recovering naphthalene from the low boiling point components obtained in step 2, preferably from the intermediate boiling point fraction of the low boiling point components. The method of recovering naphthalene is not particularly limited, but for example, a distillation method, a crystallization method, or the like that is commonly used as a method of recovering naphthalene from naphthalene oil in the coal tar industry can be used. In one embodiment, the method of recovering naphthalene is a crystallization method.
[0026] <Graphite electrode manufacturing process> The carbon material refers to various molded carbon materials such as graphite tubes, graphite crucibles, graphite boats, graphite electrodes, etc. The general manufacturing process for graphite electrodes is described below. 1. Mixing process Mixing and kneading the needle coke and the binder pitch together 2. Molding process A process of forming the kneaded material into a molded body of a predetermined size and shape. 3. Firing process A step of sintering the molded body to obtain a sintered body. 4.Impregnation process A process of filling the fired body with impregnated pitch 5. Re-firing process A process of re-firing the fired body filled with impregnated pitch to obtain a re-fired body. 6.Graphitization process A step of graphitizing the refired body to obtain a graphitized body. 7. Processing process A process in which the graphitized body is formed into a predetermined shape by cutting or the like to produce a graphite electrode.
[0027] 1. Mixing process The needle coke that has been crushed, classified, and blended in a predetermined particle size ratio is mixed and kneaded with the binder pitch. The blending amount of the binder pitch varies depending on the blending method and the molding method, but is generally about 20 parts by mass to 30 parts by mass per 100 parts by mass of the needle coke.
[0028] The kneaded material may contain a puffing inhibitor such as iron oxide.
[0029] A commercially available mixer or kneader can be used for mixing and kneading. Specific examples include mixers and kneaders such as mixers and kneaders. The kneading temperature varies depending on the binder pitch used, but is generally about 140°C to 180°C. After kneading, the kneaded product is cooled to a temperature suitable for subsequent molding (for example, 100°C to 130°C).
[0030] Although it varies depending on the type of carbon material produced and the production method, the softening point of the binder pitch used is preferably 80° C. to 120° C. The amount of fixed carbon is preferably 45% by mass or more, and more preferably 50% by mass or more.
[0031] 2. Molding process The kneaded material is molded to obtain a molded product of a desired size and shape. The molding method can be appropriately selected from extrusion molding, molding, etc., depending on the target carbon material. When the target carbon material is a graphite electrode, extrusion molding into a cylindrical shape is generally used.
[0032] 3. Firing process The molded body from the previous step is heated and fired at 700°C to 1000°C to obtain a fired body. The firing step is preferably carried out in a non-oxidizing atmosphere of combustion exhaust gas. The molded body softens at the beginning of the temperature rise, and at 200°C to 500°C, a large amount of decomposition gas is generated by thermal decomposition and polycondensation of the binder pitch, resulting in the formation of pores and volumetric shrinkage. At 500°C to 600°C, the binder pitch is carbonized. The firing step, including cooling, often takes about one month.
[0033] 4.Impregnation process In the firing process, generally, 35% to 45% of the mass of the binder pitch is lost as a volatile matter. At that time, a large number of pores are generated in the fired body. The impregnation process is to fill these pores with impregnation pitch. Impregnation is carried out, for example, by placing the fired body in an autoclave, degassing it under reduced pressure, and then injecting the molten impregnation pitch into the pores at about 200°C with a gas pressure of about 1 MPa.
[0034] Although it differs depending on the type of carbon material produced and the production method, the softening point of the impregnation pitch used is preferably 80° C. to 120° C. The amount of fixed carbon is preferably 45% by mass or more, more preferably 50% by mass or more.
[0035] 5. Re-firing process The fired body filled with the impregnated pitch is fired again to obtain a refired body. The refire can be performed under the same conditions as the firing step. The impregnation step and the refire step can be repeated as necessary.
[0036] 6.Graphitization process The re-burned body is placed in a furnace (such as an Acheson furnace or an LWG furnace) surrounded by an insulating material, and the re-burned body is subjected to a heat treatment using packing coke or resistance heating of the re-burned body due to electrical current. The graphitization temperature is 2000°C to 3000°C. This temperature is necessary to convert the amorphous carbon in the re-burned body into crystalline graphite. It is preferable to heat treat the re-burned body for several days to convert it into a graphitized body.
[0037] 7. Processing process The graphitized body is machined, for example by cutting, to form a graphite electrode product of a desired shape. EXAMPLES
[0038] The present invention will be further described with reference to the following examples and comparative examples. However, these examples are merely illustrative of the present invention, and the present invention is not limited to these examples.
[0039] <Method of measuring softening point> The softening point was measured in accordance with "8. Measurement method for softening point of tar pitch (ring and ball method)" of JIS K 2425:2006 "Test methods for creosote oil, processed tar and tar pitch".
[0040] <Method of measuring fixed carbon amount> The amount of fixed carbon was measured in accordance with "11. Quantitative method for fixed carbon content" in JIS K 2425:2006 "Test methods for creosote oil, processed tar and tar pitch."
[0041] <Method of measuring naphthalene concentration and purity> The concentration and purity of naphthalene were calculated by the internal standard method using a gas chromatograph mass spectrometer (GC-MS). n-Hexadecane (Tokyo Chemical Industry Co., Ltd., GC standard grade) was used as the internal standard. The GC-MS equipment used was a 6890N Network Gas Chromatograph and a 5975C inert XL MSD manufactured by Agilent Technologies, Inc., and a HP-5MS (0.25 mmφ×30 m×0.25 μm) manufactured by Agilent Technologies, Inc., as the column. The analytical conditions were as follows. [GC conditions] Column: HP-5MS (0.25 mmφ×30 m×0.25 μm) Sample injection volume: 1 μL Sample vaporizer temperature: 270℃ Oven temperature: 50℃(1min)→(3℃ / min)→200℃(1min)→(10℃ / min)→310℃(1min) Carrier gas: Helium [MS conditions] Measurement mode: SIM Ion source temperature: 230℃ Quadrupole temperature: 150℃
[0042] <Measurement of 5% by mass and 90% by mass distillation temperatures of the raw material (recovery process raw material) provided to step 3> The 5% by mass and 90% by mass distillation temperatures of the raw material used in step 3 were measured in accordance with the method described in ASTM D7500-15 "Standard Test Method for Determination of Boiling Range Distribution of Distillates and Lubricating Base Oils-in Boiling Range from 100° C. to 735° C. by Gas Chromatography". For the measurement, an AC SIMDIS Analyzer manufactured by PAC was used.
[0043] <Method for preparing light ethylene bottom oil fraction> 894 kg of ethylene bottom oil (naphthalene concentration: 9.1% by mass) was used as a raw material and purified by distillation at a distillation temperature of 101°C and an operating pressure of 533 to 1067 PaA in a distillation apparatus with 15 theoretical plates (Sulzer packing), to obtain 544 kg of ethylene bottom oil heavy fraction as a bottom liquid. The initial boiling point of the obtained ethylene bottom oil heavy fraction was 218°C. About 350 kg of components obtained as a distillate were used as an ethylene bottom oil light fraction. The naphthalene concentration in the obtained ethylene bottom oil light fraction was 23.3% by mass.
[0044] <Electrode evaluation> The binder pitch and needle coke were mixed (needle coke: binder pitch = 8:2, mass ratio) using a laboratory kneader (TDR200-3 model, manufactured by Toshin Co., Ltd.), and molded into the shape of an electrode piece (cylindrical; 50 mmΦ x 35 mm) to produce a green body. The green body was fired at approximately 1000°C to produce a fired body. The bulk density of the green body and the fired body was measured in accordance with JIS R 7222:2017 "Method of measuring physical properties of graphite material 7. Method of measuring bulk density". The carbonization rate was calculated using formula (1).
[0045]
number
[0046] Example 1 300 g of ethylene bottom oil light fraction having a naphthalene concentration of 23.3% by mass obtained by the above-mentioned method for preparing ethylene bottom oil light fraction was introduced into a SUS autoclave with a capacity of 0.98 L. The autoclave was sealed under a nitrogen gas atmosphere, and the inside of the container was heated to 430 ° C. at a rate of 4 ° C. / min while stirring, and heat treatment was performed. After 6 hours had passed since reaching 430 ° C., it was allowed to cool to room temperature, and the heat-treated product was taken out. The heat-treated product was subjected to vacuum distillation using a vacuum distillation apparatus, and 217 g (yield: 72 mass%) of low boiling point components and 71 g (yield: 24 mass%) of pitch as a high boiling point component were obtained. The remaining 12 g was the amount lost during the heat-treated product recovery operation and vacuum distillation operation. The vacuum distillation was performed by keeping the pressure constant at 5 mmHg and gradually increasing the pot temperature from room temperature until the steam temperature at the top of the distillation tube reached 340 ° C. in terms of normal pressure. The naphthalene concentration in the obtained low boiling point component was 44.2% by mass. 217 g of this low boiling point component was left to stand at 10°C for 10 hours to crystallize naphthalene. The obtained slurry was filtered at room temperature, and the obtained residue (crystallized material) was sandwiched between two pieces of filter paper and pressed and squeezed at a pressure of 5 MPa using an electric compressor (BRE-32 manufactured by Mayekawa Test Machinery Co., Ltd.) to obtain 46 g of naphthalene (yield: 15% by mass relative to the ethylene bottom oil light fraction). The obtained naphthalene was white and had a purity of 97.9% by mass. The physical properties of the obtained pitch were as shown in Table 1.
[0047] The resulting pitch was used as a binder pitch to perform electrode evaluation. The bulk density of the resulting molded body was 1.848 g / cm 3 The carbonization rate was 60%, and the bulk density of the fired body was 1.583 g / cm 3 It was.
[0048] Example 2 Pitch and naphthalene were obtained according to the method described in Example 1, except that the heat treatment conditions and distillation conditions were changed as shown in Table 1.
[0049] Example 3 Pitch and naphthalene were obtained in the same manner as in Example 1, except that the heat treatment raw material, heat treatment conditions, and distillation conditions were changed as shown in Table 1.
[0050] Comparative Example 1 200 g of ethylene bottom oil light fraction with a naphthalene concentration of 23.3% by mass obtained by the above-mentioned method for preparing ethylene bottom oil light fraction was distilled under reduced pressure, and a fraction with a boiling point of about 200°C or less was distilled off, thereby obtaining 122 g of ethylene bottom oil light fraction in which naphthalene was concentrated as a high boiling point component. The reduced pressure distillation was performed by keeping the pressure constant at 65 mmHg and gradually increasing the vessel temperature from room temperature until the steam temperature at the top of the distillation tube reached 195°C in terms of normal pressure. The naphthalene concentration in this ethylene bottom oil light fraction in which naphthalene was concentrated was 30.7% by mass. This 122 g of ethylene bottom oil light fraction in which naphthalene was concentrated was left to stand at 10°C for 10 hours to crystallize naphthalene. The obtained slurry was treated in the same manner as in Example 1 to obtain 16 g of naphthalene (yield 8%). The obtained naphthalene was pale purple and had a purity of 96.6%.
[0051] Comparative Example 2 150 g of ethylene bottom oil light fraction having a naphthalene concentration of 23.3 mass% obtained by the above-mentioned method for preparing ethylene bottom oil light fraction was left to stand at 10° C. for 20 hours, but naphthalene did not precipitate. This result shows that naphthalene cannot be obtained at 10° C. even if the ethylene bottom oil light fraction is crystallized as it is without concentrating naphthalene by distillation. A lower temperature is required to crystallize naphthalene from this ethylene bottom oil light fraction.
[0052] [Table 1]
[0053] It has been found that pitch obtained as a high boiling point component by heat treating ethylene bottom oil or a light fraction of ethylene bottom oil and distilling the heat treated product has physical properties suitable for use in the production of carbon materials such as graphite electrodes. By recovering naphthalene from the low boiling point components obtained together with the pitch in the distillation process, high purity naphthalene without coloration can be obtained.
Claims
1. A method for producing pitch and naphthalene for producing carbon materials, comprising the steps of: heat-treating petroleum heavy oil (step 1); distilling the heat-treated product obtained in step 1 and separating it into pitch, which is a high-boiling component, and a low-boiling component (step 2); and recovering naphthalene from the low-boiling component obtained in step 2 (step 3).
2. 2. The method for producing pitch for producing carbon materials and naphthalene according to claim 1, wherein the petroleum heavy oil is at least one selected from the group consisting of ethylene bottom oil and ethylene bottom oil light fraction.
3. The method for producing pitch for producing carbon materials and naphthalene according to claim 1 or 2, wherein the naphthalene concentration in the petroleum heavy oil is 5% by mass to 60% by mass.
4. 3. The method for producing pitch and naphthalene for producing carbon materials according to claim 1, wherein the heat treatment temperature in step 1 is 360° C. to 480° C., and the heat treatment time is 0.5 hours to 48 hours.
5. 3. The method for producing pitch for producing carbon materials and naphthalene according to claim 1 or 2, wherein the carbon material is a graphite electrode.
Citation Information
Patent Citations
JP1974035420A
kemikarupitsuchi
JP1976083622A
Continuous method of manufacturing petroleum pitch
JP1978060927A