Laminate

A laminate structure combining crystalline and amorphous resin coatings addresses the challenge of achieving both high heat seal strength and transparency by laminating amorphous resin over crystalline resin, enhancing both properties effectively.

JP2024148558AInactive Publication Date: 2024-10-18CHUKYO YUSHI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023061778
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing aqueous dispersions of crystalline resins like polycaprolactone exhibit high heat seal strength but low transparency, while amorphous resins such as polylactic acid have excellent transparency but low heat seal strength, making it difficult to achieve both properties simultaneously in a coating film.

Method used

A laminate structure is developed where a first coating film from an aqueous dispersion of crystalline resin is laminated on a base material, followed by a second coating film from an aqueous dispersion of amorphous resin, enhancing both high heat seal strength and transparency.

Benefits of technology

The laminate achieves high heat seal strength and transparency by smoothing the rough surface of the crystalline resin with the amorphous resin, maintaining transparency while improving heat seal strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148558000001
    Figure 2024148558000001
  • Figure 2024148558000002
    Figure 2024148558000002
  • Figure 2024148558000003
    Figure 2024148558000003
Patent Text Reader

Abstract

To create a coating film on a base sheet, the coating film having both high heat-seal strength and high transparency, by using a water-dispersed biodegradable resin.SOLUTION: A laminate includes: a first coating film obtained from a water-dispersed crystalline resin laminated on a base sheet; and a second coating film obtained from a water-dispersed non-crystalline resin laminated on the first coating film.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate. The laminate relates to a base sheet such as a film or paper and a coating film laminated thereon that has both high heat sealability and transparency. [Background technology]

[0002] Food packaging materials not only need heat sealability for bag making, but also often need transparency so as not to spoil the appearance of the product inside. Generally, plastic films such as OPP film are used as packaging materials that have both heat seal strength and transparency. However, in recent years, as the problem of environmental pollution caused by plastic waste has become more serious, there has been an active movement to develop packaging materials such as paper, biodegradable film, etc. As a method for imparting heat sealability to paper and biodegradable film without impairing their biodegradability, products have been developed in which thermoplastic biodegradable resins are laminated onto paper or biodegradable film substrates (see Patent Documents 1 and 2).

[0003] In the lamination technique disclosed in this document, the amount of biodegradable resin used is approximately 20 to 50 g / m 2 Because of the large number of options and the high cost of raw materials, this method is not widely used. Therefore, research and development of aqueous dispersions of biodegradable resins that can be easily controlled to a low coating weight has been actively conducted. The present inventors have developed aqueous dispersions of crystalline resins such as polycaprolactone and aqueous dispersions of non-crystalline resins such as polylactic acid, and have applied them to various film substrates and evaluated them (Patent Document 3). Please also refer to Patent Document 4, which discloses technology related to the present invention. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-272712 A [Patent Document 2] JP 2011-743 A [Patent Document 3] JP 2022-055374 A [Patent Document 4] Patent Publication No. 2022-150809 Summary of the Invention [Problem to be solved by the invention]

[0005] The inventors who carried out the above development noticed the following problems. Aqueous dispersions of crystalline resins such as polycaprolactone exhibit high heat seal strength but low transparency, whereas aqueous dispersions of non-crystalline resins such as polylactic acid exhibit excellent transparency but low heat seal strength. Therefore, it has been difficult to form a coating film that has both high heat seal strength and high transparency. [Means for solving the problem]

[0006] The present inventors have been conducting intensive research to solve the above problems. As a result, it has been found that high heat seal strength and high transparency can be achieved by laminating a second coating film obtained from an aqueous dispersion of a non-crystalline resin on a first coating film obtained from an aqueous dispersion of a crystalline resin, and the present invention has been conceived. In this specification, a crystalline resin refers to a resin having an oriented molecular chain portion (crystalline portion). In contrast, an amorphous resin refers to a resin that does not have the above-mentioned crystalline portion, or that has the above-mentioned crystalline portion in an extremely small amount. Whether or not a resin has a crystalline portion to the extent that it has crystallinity can be determined by whether or not the resin has a melting point, that is, whether or not it has a clear melting peak in differential scanning calorimetry (DSC) in which the temperature is increased at a constant rate. In this specification, if the peak area of ​​the melting peak in DSC is 20 J / g or more, it is determined that the resin has a clear melting peak, and a resin having such characteristics is considered to be a crystalline resin. A first aspect of the present invention is defined as follows. A laminate comprising: a first coating film obtained from an aqueous dispersion of a crystalline resin that is laminated on a substrate; and a second coating film obtained from an aqueous dispersion of a non-crystalline resin that is laminated on the first coating film.

[0007] The laminate of the first aspect thus defined maintains the high heat seal strength of the first coating film obtained from the aqueous dispersion of the crystalline resin and the high transparency of the second coating film obtained from the aqueous dispersion of the non-crystalline resin. On the other hand, a composite coating film formed by laminating a first coating film obtained from an aqueous dispersion of a crystalline resin onto a second coating film obtained from an aqueous dispersion of a non-crystalline resin has poor heat seal strength and transparency.

[0008] The reason why the transparency of the first coating film obtained from the aqueous dispersion of the crystalline resin is poor is thought to be because the surface is rough, which causes diffuse reflection of light. When the aqueous dispersion of the amorphous resin is applied to such a rough surface, the rough surface is repaired and the diffuse reflection of light is suppressed. The transparency of the second coating film obtained from the aqueous dispersion of the amorphous resin is maintained as it is. Heat seal strength is evaluated by placing a pair of substrates laminated with a composite coating film facing each other and hot pressing them. However, in composite coatings in which the second coating film containing a non-crystalline resin is in contact with the substrate, sufficient strength may not be secured between the composite coating film and the substrate.

[0009] The substrate is not particularly limited as long as the first coating film can be laminated thereon. In this embodiment, a transparent sheet-like substrate is used, but it may be opaque paper, or it may be a plate-like or block-like substrate. When a sheet-like substrate is used, the sheet may be formed of multiple layers. For example, a first sheet having a rough surface such as graft paper may have transparency when coated with an aqueous dispersion of a non-crystalline resin and dried. In this case, the coating film laminated on the surface of the first sheet is a part of the sheet-like substrate even if it is obtained from an aqueous dispersion of a non-crystalline resin.

[0010] A coating film obtained from an aqueous dispersion of a non-crystalline resin can be laminated on the second coating film. Furthermore, a coating film obtained from an aqueous dispersion of a crystalline resin and a coating film obtained from an aqueous dispersion of a non-crystalline resin can be laminated in this order on the second coating film.

[0011] In the above, it is preferable that both the crystalline resin and the non-crystalline resin contain a biodegradable resin. Of the biodegradable resins, it is preferable that the crystalline resin contains polycaprolactone and the non-crystalline resin contains polylactic acid.

[0012] Another aspect of the present invention is defined as follows: Providing a substrate; A step of preparing a first water dispersion in which a crystalline resin is dispersed; A step of preparing a second aqueous dispersion in which an amorphous resin is dispersed; forming a first coating film from the first aqueous dispersion on a surface of the substrate; forming a second coating film from the second aqueous dispersion on the surface of the first coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The laminate according to the embodiment of the present invention is formed by sequentially laminating a first coating film and a second coating film on a transparent substrate sheet. The first coating film is obtained from an aqueous dispersion of a crystalline resin, and the second coating film is obtained from an aqueous dispersion of a non-crystalline resin. Examples of the crystalline resin constituting the first coating film include dibasic acid polyesters such as polycaprolactone, copolymers of caprolactone and other hydroxycarboxylic acids, polylactic acid, polybutylene succinate, polybutylene succinate adipate, polyethylene succinate, polyethylene terephthalate succinate, polybutylene adipate, polybutylene adipate terephthalate, polyhydroxybutyrate, copolymers of polyhydroxybutyrate and other hydroxycarboxylic acids, etc. These may be used alone or in combination of two or more. When polycaprolactone is selected as the crystalline resin for the first coating, the coating weight (dry mass) is 2-15g / m 2 It is preferable to set the thickness to 3-10g / m 2 It is.

[0014] Examples of the amorphous resin constituting the second coating film include polylactic acid and thermoplastic starch. When polylactic acid is selected as the amorphous resin for the second coating, the coating weight after drying is 1-10g / m 2 It is preferable to set the thickness to 2-5 g / m 2 It is.

[0015] The base sheet can be made of food packaging materials (food packaging paper such as craft paper, pure white roll paper, and fine paper, food packaging films made of PE, PP, PET, cellophane, biodegradable resins, etc.). When the base sheet is paper, the combination of the first coating film and the second coating film of the present invention has the effect of imparting high heat seal strength without compromising the design of the pattern or the like drawn on the paper surface. Also, when the base sheet is a highly transparent biodegradable film such as cellophane, it has the effect of imparting high heat seal strength without significantly impairing transparency.

[0016] The method of forming the first coating film and the second coating film is not particularly limited. For example, a water-based dispersion of a crystalline resin or a composition containing the same can be laminated to a uniform thickness on the surface of a substrate sheet by a known method, and then dried to obtain a first coating film. After drying of the first coating film is completed, a water-based dispersion of a non-crystalline resin or a composition containing the same can be laminated to a uniform thickness on the surface by a known method, and then dried to obtain a second coating film. EXAMPLES

[0017] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Example 1 (Preparation of base sheet) Plain cellophane, PT#300 (manufactured by Rengo Co., Ltd.), was used as the base sheet, as it has high transparency but does not have heat-sealing properties by itself.

[0018] (Preparation of Water Dispersions A and B) Polycaprolactone water dispersion A was prepared as follows. 47.2 parts by mass of polycaprolactone was mixed with an aqueous solution in which 2.8 parts by mass of polyvinyl alcohol was dissolved in 50 parts by mass of water, and the former was converted into a solid dispersoid by a general phase inversion emulsification method, and the solid was dispersed in the latter as an aqueous dispersion medium, thereby obtaining a 50% by mass first aqueous dispersion A, which is an aqueous dispersion of polycaprolactone.

[0019] Aqueous dispersion B of polylactic acid was prepared as follows. 47.2 parts by mass of polylactic acid was mixed with an aqueous solution in which 2.8 parts by mass of polyvinyl alcohol was dissolved in 50 parts by mass of water, and the former was converted into a solid dispersoid by a general phase inversion emulsification method, and the solid was dispersed in the latter as an aqueous dispersion medium, to obtain a 50% by mass aqueous dispersion B of polylactic acid.

[0020] (Preparation of Coating Fluid) A coating liquid for a first coating layer with a solid content of 40% by mass was prepared by adding water to the polycaprolactone aqueous dispersion A. A coating liquid for a second coating layer with a solid content of 10% by mass was prepared by adding water to the polylactic acid aqueous dispersion B.

[0021] (Preparation of coating film) A coating solution of polycaprolactone aqueous dispersion A (solid content 40 mass%) was applied to one side of plain cellophane using a wire bar (No. 03 / wet film thickness 6.86 μm), and the coating was dried in a dryer at 120°C for 1 minute to obtain a first coating film containing polycaprolactone. A coating solution of polylactic acid aqueous dispersion B (solid content 10% by mass) was applied onto the first coating film using a wire bar (No. 03 / wet film thickness 6.86 μm), and the coating was dried in a dryer at 120°C for 1 minute to obtain a second coating film. As a result, a laminate was obtained in which the first coating film and the second coating film were laminated in this order on the plain cellophane. Here, the first coating film contained polycaprolactone as a biodegradable crystalline resin, and the coating amount was 4 g / m 2 (dry mass). The second coating contains polylactic acid as a biodegradable amorphous resin, and the coating weight is 1 g / m 2 (dry mass).

[0022] Example 2 Water was added to the polylactic acid aqueous dispersion B to prepare a coating solution with a solid content of 20% by mass, and the coating was applied with a wire bar (No. 03 / wet film thickness 6.86 μm) to obtain a coating weight of 2 g / m 2( The other conditions were the same as in Example 1.

[0023] Example 3 Water was added to the polylactic acid aqueous dispersion B to prepare a coating solution with a solid content of 40% by mass, and the coating amount of the second coating was 5 g / m2 by applying it with a wire bar (No. 04 / wet film thickness 9.14 μm). 2 (dry weight) The other conditions were the same as in Example 1.

[0024] Example 4 Water was added to the polylactic acid aqueous dispersion B to prepare a coating solution with a solid content of 40% by mass, and the coating was applied with a wire bar (No. 10 / wet film thickness 22.6 μm) to obtain a coating weight of 10 g / m 2 (dry weight) The other conditions were the same as in Example 1.

[0025] Example 5 A coating solution of polycaprolactone (solid content 40% by mass) was applied using a wire bar (No. 6 / wet film thickness 13.7 μm), and a coating solution of 20% solid content was prepared by adding water to the aqueous dispersion B of polylactic acid, and this was then applied using a wire bar (No. 03 / wet film thickness 6.86 μm). The coating weight of the first coating was 7 g / m 2 (dry weight), coating weight of second coating is 2g / m 2 The same as Example 1, except that the coating was performed so that the dry weight was 100 g.

[0026] Example 6 A coating solution of polycaprolactone (solid content 40% by mass) was applied using a wire bar (No. 10 / wet film thickness 22.6 μm), and a coating solution of 20% solid content was prepared by adding water to the aqueous dispersion B of polylactic acid, and this was then applied using a wire bar (No. 03 / wet film thickness 6.86 μm) to obtain a coating weight of 10 g / m 2 (dry weight), coating weight of second coating is 2g / m 2 The same as Example 1, except that the coating was performed so that the dry weight was 100 g.

[0027] Example 7 A coating solution of polycaprolactone (solid content 40% by mass) was applied using a wire bar (No. 16 / wet film thickness 36.6 μm), and a coating solution of 20% solid content was prepared by adding water to the aqueous dispersion B of polylactic acid, and this was then applied using a wire bar (No. 03 / wet film thickness 6.86 μm). The coating weight of the first coating was 15 g / m 2 (dry weight), coating weight of second coating is 2g / m 2 The same as Example 1, except that the coating was performed so that the dry weight was 100 g.

[0028] Example 8 Water was added to the polycaprolactone aqueous dispersion A to prepare a coating solution with a solid content of 20% by mass, and the coating amount of the first coating was set to 2 g / m by applying it with a wire bar (No. 03 / wet film thickness 6.86 μm). 2 The coating weight of the second coating was 2 g / m2 by adding water to the polylactic acid aqueous dispersion B to prepare a coating solution with a solid content of 20% by mass, and applying it with a wire bar (No. 03 / wet film thickness 6.86 μm). 2 The other conditions were the same as in Example 1.

[0029] Example 9 Water was added to the polycaprolactone aqueous dispersion A to prepare a coating solution with a solid content of 30% by mass, and the coating amount of the first coating was 3 g / m2 by applying it with a wire bar (No. 03 / wet film thickness 6.86 μm). 2The coating liquid was prepared by adding water to the polylactic acid aqueous dispersion B to obtain a solid content of 20% by mass, and the coating amount of the second coating was 2 g / m2 by applying the coating liquid with a wire bar (No. 03 / wet film thickness 6.86 μm). 2 The other conditions were the same as in Example 1.

[0030] Comparative Example 1 It consists of only a base sheet (plain cellophane manufactured by Rengo Co., Ltd.), and the first coating film and the second coating film are not laminated. Comparative Example 2 Only the first coating containing polycaprolactone (dry mass: 4 g / m 2 ) is coated onto a base sheet. Comparative Example 3 A coating containing polylactic acid (dry mass: 2g / m2) was applied to the base sheet as the second coating. 2 ) was formed, and then the first coating film containing polycaprolactone (dry mass: 4 g / m 2 ) is formed.

[0031] (Evaluation method) The obtained laminates of the examples and comparative examples were evaluated as follows. <Transparency: Haze> Measurements were carried out in accordance with JIS K7136:2000. The transparency of the laminate was evaluated based on the following criteria. [Table 1]

[0032] <Heat seal strength> The second coating films of the laminate were thermally pressed together using a heat sealer. The heat sealing conditions were a temperature of 120°C, a press pressure of 0.2 MPa, and a press time of 3 seconds. The heat seal strength was evaluated using a tensile tester (A&D Co., Ltd.: universal material testing machine), and the heat seal strength was evaluated based on the following criteria. The tensile speed was 300 mm / min, and the peeling condition was 180 degree peeling. [Table 2]

[0033] [Table 3] From a comparison of Comparative Examples 2 and 3 with Examples 1 to 9 in Table 3 above, it can be seen that by laminating a second coating film containing polylactic acid on a first coating film containing polycaprolactone, the transparency of the laminate is improved while maintaining the heat seal strength.

[0034] The coating weight of the first coating is 2g / m 2 The upper limit of the coating amount of the first coating film is not particularly limited, but it is set to 15 g / m from the viewpoints of ensuring transparency and reducing material costs. 2 It can be as follows: The coating weight of the second coating is 1g / m 2 The upper limit of the coating amount of the second coating film is not particularly limited, but it is set to 10 g / m from the viewpoint of ensuring transparency and reducing material costs. 2 It can be as follows:

[0035] When the first coating contains polycaprolactone, the coating weight of the second coating is 2 g / m 2 (See Examples 1 and 2.) In this case, the upper limit of the coating amount of the second coating film is not particularly limited, but from the viewpoints of material cost and ensuring transparency, it is preferably 8 g / m 2 It is more preferably 5 g / m or less (see Examples 3 and 4). 2 The following is the result. When the first coating contains polycaprolactone, the coating weight of the first coating containing polycaprolactone is set to 3 g / m2 in order to improve the heat seal strength. 2 In this case, the upper limit of the coating amount of the first coating film is not particularly limited, but it is preferably 10 g / m from the viewpoint of material cost and ensuring transparency. 2 The following can be done (see Example 6):

[0036] The present invention is not limited to the above-mentioned aspects and embodiments. Various modifications within the scope of the claims and within the scope that can be easily conceived by a person skilled in the art are also included in the present invention. The contents of papers, published patent publications, patent publications, etc. specified in this specification are all incorporated by reference.

Claims

1. A laminate comprising: a first coating film obtained from an aqueous dispersion of a crystalline resin that is laminated on a substrate; and a second coating film obtained from an aqueous dispersion of a non-crystalline resin that is laminated on the first coating film.

2. The laminate according to claim 1 , wherein the crystalline resin and the amorphous resin comprise a biodegradable resin.

3. The laminate according to claim 2 , wherein the crystalline resin comprises polycaprolactone and the non-crystalline resin comprises polylactic acid.

4. The coating amount (dry mass) of the first coating film is 2 g / m 2 15g / m or more 2 The coating amount (dry mass) of the second coating film is 1 g / m or less. 2 10g / m or more 2 The laminate according to claim 2, wherein:

5. The crystalline resin contains polycaprolactone, and the coating amount (dry mass) of the first coating film is 2 g / m 2 15g / m or more 2 the amorphous resin contains polylactic acid, and the coating amount (dry mass) of the second coating film is 1 g / m or less. 2 10g / m or more 2 4. The laminate of claim 3, wherein:

6. The coating amount (dry mass) of the first coating film is 3 g / m 2 10g / m or more 2 The coating amount (dry mass) of the second coating film is 2 g / m or less. 2 Above 5g / m 2 6. The laminate of claim 5, wherein:

7. 7. The laminate according to claim 2, wherein the substrate comprises a biodegradable sheet and is used as a food sheet.

8. Providing a substrate; A step of preparing a first water dispersion in which a crystalline resin is dispersed; A step of preparing a second aqueous dispersion in which an amorphous resin is dispersed; forming a first coating film from the first aqueous dispersion on a surface of the substrate; and forming a second coating film from the second aqueous dispersion on the surface of the first coating film.

9. A method for producing a food sheet, comprising the steps of producing a laminate according to the method described in claim 7, wherein the substrate comprises a sheet having biodegradability, the crystalline resin and the non-crystalline resin comprise biodegradable resins, and the coated surfaces of the laminate are placed opposite each other and heat sealed.

Citation Information

Patent Citations

  • Manufacturing method of film laminated with polybutylene succinate

    JP2006272712A

  • Biodegradable lamination sheet and processed article of the same

    JP2011000743A

  • Aqueous dispersion, coating liquid containing the aqueous dispersion, method for producing biodegradable resin film using the coating liquid, method for manufacturing laminated sheet for food packaging, method for manufacturing packaging bag, and dispersoid contained in the aqueous dispersion

    JP2022055374A

  • Coated paper

    JP2022150809A