Seal member and method for producing the same
A sealing member with a resin and polymerization inhibitor, optimized by SP value matching, addresses blooming and maintains polymerization reactivity by ensuring even dispersion and adherence, effectively preventing pipe clogging.
Patent Information
- Application Number
- JP2023061806
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
Existing sealing members, such as gaskets made from polytetrafluoroethylene (PTFE), suffer from the 'blooming phenomenon' where polymerizable monomers penetrate and polymerize within the gaps, causing pipe clogging, while polymerization inhibitors in PTFE-based gaskets either form clumps or desorb, leading to insufficient inhibition and potential inhibition of polymerization reactions.
A sealing member with a resin portion containing a polymerization inhibitor, where the difference in solubility parameter (SP) values between the resin and inhibitor satisfies a specific range (SPp-SPb ≤ 16.37), ensuring the inhibitor is evenly dispersed and adheres well to the resin, preventing blooming and maintaining polymerization reactivity.
The sealing member effectively prevents blooming for extended periods by ensuring the polymerization inhibitor remains adhered and active, without inhibiting polymerization reactions, thus maintaining pipe functionality.
Smart Images

Figure 2024148573000001 
Figure 2024148573000002 
Figure 2024148573000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a sealing member and a method for manufacturing the same. [Background technology]
[0002] Gaskets (or packings) are always used as sealing materials at the joints of pipes used in chemical plants, etc. When a polymerizable monomer is passed through the pipes, the monomer soaks into the resin gasket, polymerizes inside the gasket, and grows, causing the pipes to become clogged, creating an issue known as the "blooming phenomenon." To date, measures proposed to combat the blooming phenomenon include gaskets based on polytetrafluoroethylene (PTFE), which is more resistant to solvents and less susceptible to penetration, and gaskets containing inhibitors that suppress polymerization (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-196779 A [Patent Document 2] WO2015 / 151515 publication Summary of the Invention [Problem to be solved by the invention]
[0004] In the above Patent Document 1, even if the gasket is based on PTFE, which has high solvent resistance, gaps exist, and thus monomers penetrate into the gasket, causing the blooming phenomenon. On the other hand, in the above Patent Document 2, when a polymerization inhibitor is contained in a base material of highly solvent-resistant PTFE in order to maximize the effect of suppressing the blooming phenomenon, even if a polymerization inhibitor with a high polymerization inhibitor effect is used, the domains of the polymerization inhibitor in the gasket tend to be present as clumps, so the effect of suppressing the blooming phenomenon is insufficient. Furthermore, problems such as the desorption and elution of the polymerization inhibitor tend to occur, and there is a risk of inhibiting the polymerization reaction of polymerizable monomers in pipes and equipment. The object of the present invention is to provide a sealing material that prevents the blooming phenomenon over a long period of time even if a polymerizable compound penetrates into the gaps of a sealing material such as a gasket, and does not inhibit the polymerization reaction of polymerizable monomers in piping or equipment. [Means for solving the problem]
[0005] The present inventors have conducted extensive research to solve the above problems and have found the following method. That is, the present invention provides a sealing member having a resin portion containing a resin and a polymerization inhibitor, The SP value of the resin [(J / cm 3 ) 0.5 ] is SPb, the SP value of the polymerization inhibitor [(J / cm 3 ) 0.5 When SPp is taken as the value, the relationship of the following formula (1) is satisfied, SPp-SPb≦16.37...Equation (1) The present invention relates to a sealing member, characterized in that, in a cross-sectional observation of the resin part of the sealing member, when the area of the cross-section occupied by the polymerization inhibitor is taken as 100 area %, an area of domains of the polymerization inhibitor that are occupied by domains having a short axis of 5 μm or more is 25 area % or less. The present invention also provides a method for manufacturing the seal member having the above configuration, comprising the steps of: The present invention relates to a method for producing a sealing member, characterized in that the resin is molded to obtain an intermediate molded body, and then the intermediate molded body is impregnated with a solution of the polymerization inhibitor in an organic solvent to obtain the sealing member. Effect of the Invention
[0006] According to the present invention, the inhibitor is impregnated so that the difference between the SP value of the base material and that of the polymerization inhibitor falls within an appropriate range, and the dispersion state of the inhibitor is controlled to have few lumps, so that the inhibitor is evenly dispersed in the gaps in the gasket and has a certain degree of affinity with the base material, making it difficult for the inhibitor to be detached or eluted. Therefore, it is possible to provide a sealing member that prevents the blooming phenomenon for a long period of time even if a polymerizable compound permeates the gaps in the gasket and does not inhibit the polymerization reaction of polymerizable monomers in piping or equipment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The present invention will be described in detail below.
[0008] [Features of the present invention] A sealing member having a resin portion containing a resin and a polymerization inhibitor, the resin having an SP value [(J / cm 3 ) 0.5 ] is SPb, the SP value of the polymerization inhibitor [(J / cm 3 ) 0.5 When SPp is taken as the value, the relationship of the following formula (1) is satisfied, SPp-SPb≦16.37...Equation (1) The effects of the present invention can be obtained by using a sealing member characterized in that, when a cross-sectional observation of the resin part of the sealing member is performed, the area occupied by domains of the polymerization inhibitor having a short axis of 5 μm or more accounts for 25 area % or less when the area of the cross-section occupied by the polymerization inhibitor is taken as 100 area %.
[0009] Although the reason why the effects of the present invention are manifested is not necessarily clear, the present inventors believe it to be as follows.
[0010] Sealing members such as gaskets are used at the joints of pipes and the like. This does not cause problems with normal fluids, but in the case of a sealing member having a resin part, if the fluid is a polymerizable monomer, the polymerizable monomer will penetrate into the minute gaps in the resin part of the sealing member, polymerize inside the resin part, and ultimately cause a "blooming phenomenon" that blocks the pipes, etc. Therefore, by filling the minute gaps in the resin part of the sealing member with a polymerization inhibitor, it is possible to suppress the polymerization reaction there, even if the polymerizable monomer penetrates into the minute gaps in the sealing member. In this case, (i) The difference (SPp-SPb) between the SP value of the polymerization inhibitor (SPp) and the SP value of the resin part of the sealing material (SPb) must be 16.37 or less. (ii) in a cross-sectional observation of the resin part of the sealing member, when the area of the cross-section occupied by the polymerization inhibitor is taken as 100 area %, the area of domains of the polymerization inhibitor having a minor axis of 5 μm or more is 25 area % or less. The polymerization inhibitor is finely dispersed in the resin with few lumps, and can efficiently inhibit the polymerization reaction. Also, since the affinity between the resin and the polymerization inhibitor is high to a certain degree, the polymerization inhibitor does not come off from the resin and is retained for a long period of time, so that the blooming phenomenon can be suppressed even during long-term use. In addition, since the elution of the polymerization inhibitor is suppressed, the polymerization reaction in the device is not hindered.
[0011] Here, when the difference (SPp-SPb) between the SP value (SPp) of the polymerization inhibitor and the SP value (SPb) of the resin part of the sealing member exceeds 16.37, the polymerization inhibitor is easily detached from the resin part, and therefore the blooming phenomenon cannot be suppressed for a long period of time. In addition, when observing the cross section of the resin part of the sealing member, when the area occupied by the polymerization inhibitor in the cross section is taken as 100 area %, if the area occupied by domains of the polymerization inhibitor with a short diameter of 5 μm or more exceeds 25 area %, the polymerization inhibitor has many lumps in its dispersed state, which causes unevenness in the polymerization inhibition effect, and the specific surface area is small, which is not preferable because the polymerization inhibition efficiency is low. In addition, even if the difference (SPp-SPb) between the SP value (SPp) of the polymerization inhibitor and the SP value (SPb) of the resin part of the sealing member is 16.37 or less, the polymerization inhibitor is easily detached in the domains with a short diameter of 5 μm or more, which is not preferable because the contact area of the polymerization inhibitor with the resin part is small.
[0012] [Methods for identifying each component and measuring physical properties] Next, a method for identifying the above-mentioned constituent elements and measuring the physical properties according to the present invention will be described.
[0013] <Identification of resin part of sealing material> The composition and ratio of the constituent compounds of the resin portion of the sealing material are identified using a solid pyrolysis gas chromatography mass spectrometer (hereafter referred to as pyrolysis GC / MS) and NMR.
[0014] First, the resin portion is separated from the sealing material to obtain only the resin portion. The types of constituent compounds in the resin portion are analyzed using solid pyrolysis GC / MS.
[0015] The resin part is thermally decomposed at about 550°C to 700°C under the following measurement conditions. The mass spectrum of the decomposition products derived from the resin part is measured and the decomposition peaks are analyzed to identify the types of compounds that make up the resin part. [Measurement conditions for pyrolysis GC / MS] Pyrolysis device: JPS-700 (Japan Analysis Industry) Decomposition temperature: 590℃ GC / MS equipment: Focus GC / ISQ (Thermo Fisher) Column: HP-5MS, length 60 m, inner diameter 0.25 mm, film thickness 0.25 μm Inlet temperature: 200℃ Flow pressure: 100kPa Split: 50mL / min MS ionization: EI Ion source temperature: 200℃ Mass Range 45-650
[0016] Next, the abundance ratio of the identified constituent compounds in the resin part is determined according to the material. 29 Si-NMR, solid state 19 F-NMR, solid 13 C-NMR, 1 H-NMR, solid state high resolution 19 Measured and calculated using F-MAS NMR method etc.
[0017] For example, solid 29 In Si-NMR, peaks are detected in different shift regions depending on the number of functional groups bonded to the Si of the constituent compounds of the resin part. The number of functional groups can be identified by identifying the position of each peak using a standard sample. In addition, the abundance ratio of each constituent compound can be calculated from the obtained peak area.
[0018] solid 29 The measurement conditions for Si-NMR are, for example, as follows: Equipment: JNM-ECX5002 (JEOL RESONANCE) Temperature: room temperature Measurement method: DDMAS method 29Si 45° Sample tube: Zirconia 3.2mmφ Sample: Powdered material filled into test tube Sample rotation speed: 10kHz Relaxation delay: 180s Scan:2000
[0019] solid 19 The measurement conditions for F-NMR are, for example, as follows: Equipment: JNM-ECZ400S (JEOL Ltd.) Temperature: room temperature Measurement method: DDMAS method 29Si 45° Sample tube: Zirconia 3.2mmφ Sample: Powdered material filled into test tube Sample rotation speed: 10kHz Relaxation delay: 180s Scan:2000
[0020] <Identification of polymerization inhibitor, measurement of melting point and content> The composition and ratio of the constituent compounds of the polymerization inhibitor contained in the sealing material are identified using a solid pyrolysis gas chromatography mass spectrometer (hereafter referred to as pyrolysis GC / MS) and NMR.
[0021] First, when the sealing material contains substances other than the polymerization inhibitor, the sealing material is dispersed in a solvent such as tetrahydrofuran (THF), and then the supernatant liquid containing the polymerization inhibitor due to the difference in specific gravity is recovered by centrifugation or the like, and further separated by preparative liquid chromatography and further dried to obtain the polymerization inhibitor. The content of the polymerization inhibitor is calculated from the mass ratio of the obtained polymerization inhibitor to the mass of the sealing material.
[0022] Furthermore, 5 mg of the polymerization inhibitor separated by the above method was weighed out, and 600 μL of deuterated THF was added to dissolve it, 1H-NMR measurement is performed, and the composition ratio is calculated from the integral value of each peak. The specific instrument conditions are as follows: (Measurement conditions) Measuring device JNM-ECA400 FT-NMR(JEOL) Measured nuclides: 1 H Solvent: Deuterated THF Measurement frequency: 400MHz Pulse width: 3.125μs Frequency range: 7500Hz Number of times accumulated: 64 Measurement temperature: room temperature
[0023] The melting point of the polymerization inhibitor is the peak top temperature of the endothermic peak measured by DSC, and is measured by the following method. The peak top temperature of the endothermic peak in differential scanning calorimetry (DSC) is measured in accordance with ASTM D3418-82 using a differential scanning calorimeter "Q2000" (manufactured by TA Instruments). The melting points of indium and zinc are used for temperature correction of the detector of the device, and the heat of fusion of indium is used for heat correction.
[0024] Specifically, about 5 mg of the polymerization inhibitor separated by the above-mentioned method is precisely weighed as a measurement sample, placed in an aluminum pan, and measured at room temperature and humidity with a temperature rise rate of 10°C / min in the measurement temperature range of 30 to 200°C using an empty aluminum pan as a reference. In the measurement, the temperature is raised to 200°C once, then lowered to 30°C, and then raised again. In the DSC curve (temperature-endothermic amount curve) obtained during this temperature rise process, the peak top temperature of the maximum endothermic peak in the temperature range of 30°C to 200°C is obtained.
[0025] <How to calculate solubility parameter (SP value)> The solubility parameter (SP value) is calculated using the following Fedors formula (2). The values of Δei and Δvi below are based on the evaporation energies and molar volumes (25°C) of atoms and atomic groups listed in Table 3-9 of "Basic Science of Coatings, pp. 54-57, 1986 (Maki Shoten)".
[0026] In this application, the unit of SP value is (J / cm 3 ) 0.5 However, (cal / cm 3 ) 0.5 By multiplying the value by 2.046 (J / cm 3 ) 0.5 can be converted to units of δi=(Ev / V) 1 / 2 =(Δei / Δvi) 1 / 2 Formula (2) Ev: Evaporation energy V: Molar volume Δei: Evaporation energy of the atom or atomic group of the i component Δvi: Molar volume of the atom or atomic group of the i component
[0027] <Observation of the cross section of a sealing member using a scanning transmission electron microscope> The state of the polymerization inhibitor in the seal member is confirmed by observing the cross section of the seal member using a scanning transmission electron microscope. In the cross section image of the seal member using a scanning transmission electron microscope, the polymerization inhibitor is observed as domains. The state of the polymerization inhibitor is specified by measuring the number and shape of the domains of the polymerization inhibitor.
[0028] The procedure for observing the cross section of the sealing member is as follows.
[0029] The sealing member was embedded in a visible light curable embedding resin (D-800, manufactured by Nissin EM Co., Ltd.) and cut to a thickness of 70 nm using an ultrasonic ultramicrotome (UC7, manufactured by Leica).
[0030] Of the obtained thin sample pieces, ten samples are randomly selected which are cut along a plane (thickness direction) horizontal to the liquid-contacting surface of the sealing member.
[0031] The selected thin section sample is stained for 15 minutes in a 500 Pa RuO4 gas atmosphere using a vacuum staining device (VSC4R1H, Filgen), and a STEM image is created using the scanning image mode of a scanning transmission electron microscope (JEM2800, JEOL).
[0032] The STEM probe size was 1 nm, and the image size was 1024 × 1024 pixels. In addition, the contrast of the Detector Control panel for the bright-field image was adjusted to 1425, the brightness to 3750, and the contrast of the Image Control panel was adjusted to 0.0, the brightness to 0.5, and the Gamma to 1.00, to acquire a STEM image.
[0033] The obtained STEM image is binarized (threshold 120 / 255 levels) using the image processing software "Image-Pro Plus (Media Cybernetics)" to clearly distinguish the domains of the polymerization inhibitor and the binder resin.
[0034] When the binarization threshold is set to 210, the areas that appear white are the domains of the polymerization inhibitor.
[0035] <Calculation method for the area ratio of domains with a minimum diameter of 5 μm or more in polymerization inhibitor> In each of the STEM images of the cross sections of the 10 selected sealing members, an area of 2 μm x 2 μm was arbitrarily selected, and the shortest diameters of all the domains contained therein were measured. The area occupied by the polymerization inhibitor in the cross section was taken as 100 area %, and the total area % of the area occupied by domains whose shortest diameter is 5 μm or more was taken as the ratio of domains of the polymerization inhibitor whose short diameter is 5 μm or more.
[0036] [Preferred embodiment of the present invention] The present invention is based on the above-mentioned characteristics, but more preferred embodiments will be described below.
[0037] <Proportion of domains with minor axis of 5μm or more in polymerization inhibitor> In a cross-sectional observation of the resin part of the sealing member, when the area of the cross-section occupied by the polymerization inhibitor is taken as 100 area %, it is more preferable that the area of the domains of the polymerization inhibitor that are occupied by domains having a short axis of 5 μm or more is 15 area % or less.
[0038] This is because the polymerization inhibitor is distributed in a dispersed state with a large specific surface area, so that the polymerization inhibition efficiency is higher and the detachment of the polymerization inhibitor is more suppressed.Furthermore, in terms of the physical strength of the sealing member, if the polymerization inhibitor has few domains with a size of 5 μm or more, there are few locally weak parts, and even when pressure is applied, dents are less likely to occur.
[0039] <Polymerization inhibitor content> The content of the polymerization inhibitor in the seal member is preferably 0.1% by mass or more and 10.0% by mass or less, because when the content is 0.1% by mass or more and 10.0% by mass or less, the polymerization inhibitor effect is sufficiently obtained and the physical strength of the seal member is also excellent.
[0040] <Young's modulus of resin part> The Young's modulus of the resin portion is preferably 0.1 GPa or more and 30.0 GPa or less, because this allows the strength of the seal member and sufficient adhesion to piping and the like to be obtained.
[0041] (Measurement of Young's modulus of resin part) The method for measuring Young's modulus using the nanoindentation method involves measuring the relationship between the load and the indentation depth (amount of displacement) while pressing a tiny diamond indenter into a thin film, and calculating the plastic deformation hardness from the measured value. This method is characterized by being less susceptible to the effects of the physical properties of the base layer, particularly when measuring thin films of 1 mm or less, and by being less susceptible to cracking in the thin film when the indenter is pressed into it. This method is generally used to measure the physical properties of very thin thin films.
[0042] The Young's modulus Es of the sample is calculated based on the following formula. Er = [(1-νs 2 ) / Es+(1-νi 2) / Ei] -1 =√π / 2 S / β√A Here, Er is the composite Young's modulus, Es is the Young's modulus of the sample, Ei is the Young's modulus of the indenter, νs is the Poisson's ratio of the sample, νi is the Poisson's ratio of the indenter, and β is a constant related to the shape of the indenter. Note that here, the Young's modulus of the sample, Es, is also simply called the Young's modulus E, and the Poisson's ratio of the sample, νs, is also simply called the Poisson's ratio ν. Measurement conditions Measuring device: NANO Indenter XP / DCM (MTS Systems) Measurement indenter: Diamond Berkovich indenter with a triangular pyramid tip Measurement environment: 20℃, 60% RH Measurement sample: Cut the resin part of the seal material to a size of 5cm x 5cm to create a measurement sample. Maximum load setting: 25μN Pressing speed: The load is applied in proportion to time at a speed that reaches the maximum load of 25 μN in 5 seconds.
[0043] The measurement is carried out at 10 random points for each sample, and the average value is regarded as the Young's modulus measured by the nanoindentation method.
[0044] <SP value of each material> The SP value (SPb) of the resin of the sealing member [(J / cm 3 ) 0.5 ] is preferably 16.37 or less, and more preferably 14.32 or less, because this provides excellent solvent resistance to general polymerizable monomers having a vinyl group.
[0045] The SP value (SPp) of the polymerization inhibitor [(J / cm 3 ) 0.5] is preferably 21.48 or more and 28.64 or less. This is because the polarity of the polymerization inhibitor is not too low or too high, and the molecular size is not too bulky or too small, so the polymerization inhibitor easily adheres to the fine gaps of the resin part of the sealing member and is difficult to remove. The larger the SP value, the bulkier the molecule is, and the greater the polarity. Therefore, if the molecules of the polymerization inhibitor are not bulky, the affinity between the molecules is high, and a sufficient contact area can be obtained when adhering to the fine gaps of the resin part, which is preferable. In addition, since the molecules of the polymerization inhibitor are not too small, when the polymerizable monomer is impregnated into the fine gaps of the resin part, they are less likely to be washed away by the flow of the polymerizable monomer, and since the polarity is not too small, the polymerization inhibitors work together through the polarity, so the polymerization inhibitor is less likely to be liberated, and since the polarity is not too large, the polymerization inhibitors do not solidify too much with each other, and the polymerization inhibition effect on the polymerizable monomer is large, which is more preferable.
[0046] <Difference in SP values> The difference between the SP value of the polymerization inhibitor (SPp) and the SP value of the resin part of the sealing material (SPb) (SPp-SPb) [(J / cm 3 ) 0.5 ] is preferably 9.21 or greater and 16.37 or less.
[0047] This is because the polymerization inhibitor has a high affinity with the resin portion and is therefore unlikely to be detached from the resin portion; and because the affinity between the polymerization inhibitor and the resin portion is moderate, the polymerization inhibitor does not become too familiar with the resin portion, and the adhesion between the polymerization inhibitors is strong due to the affinity between the polymerization inhibitors, so that the blooming phenomenon can be suppressed for a long period of time.
[0048] In particular, the SP value (SPp) of the polymerization inhibitor [(J / cm 3 ) 0.5 ] is 21.48 or more and 28.64 or less, and (SPp-SPb) [(J / cm 3 ) 0.5 The effect is greater and it is more preferable that the ratio is 9.21 or more and 16.37 or less.
[0049] <Material of the resin part of the seal member> Possible resins for the resin portion of the sealing member include urethane resin, acrylic resin, polyester resin, polyvinyl chloride resin, epoxy resin, nylon, styrene butadiene rubber (SBR), isoprene, butadiene rubber, isobutylene rubber, silicone resin, and fluororesins such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkoxyethylene copolymer resin (PFA), tetrafluoroethylene-hexafluoropropylene copolymer resin (FEP), tetrafluoroethylene-ethylene copolymer resin (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and ethylene chlorotrifluoroethylene copolymer (ECTFE).
[0050] Among the above, from the viewpoint of solvent resistance, SBR, isoprene, butadiene rubber, isobutylene rubber, silicone resin, PTFE, PFA, FEP, ETFE, PVDF, PCTFE, and ECTFE are preferred, PTFE, PVDF, PCTFE, and ECTFE are more preferred, PTFE, PFA, FEP, and ETFE are even more preferred, and PTFE is even more preferred.
[0051] When using a polymer obtained by polymerizing a monomer having a fluorine atom and a vinyl group among the above-mentioned fluororesins, examples of the monomer to be used include 1,1,1,3,3,3-hexafluoroisopropyl methacrylate, 1H,1H,2H,2H-tridecafluoro-n-octyl methacrylate, 1,1,1,3,3,3-hexafluoroisopropyl acrylate, 2,2,3,3,3-pentafluoropropyl methacrylate, 1,1,2,2,3,3-hexafluoro-1-(trifluoromethoxy)-3-[(1,2,2-trifluorovinyl)oxy]propionate, and the like. Pan, 1H,1H,5H-octafluoropentyl acrylate, pentafluorophenyl methacrylate, 1H,1H,2H,2H-heptadecafluorodecyl acrylate, 2,2,3,3,4,4,5,5,6,6,7,7-dodecafluoroheptyl acrylate, 3,3,4,4,5,5,6,6,6-nonafluoro-1-hexene, 1H,1H,2H,2H-nonafluorohexyl methacrylate, (perfluorohexyl)ethylene, 1,1,1-trifluoro-2-(trifluoromethyl)-4-penten-2-ol, 1H,1H,2H, 2H-Tridecafluoro-n-octyl, 1H,1H-pentadecafluoro-n-octyl acrylate, pentafluorophenyl acrylate, 2,3,4,5,6-pentafluorostyrene, 4-bromo-3,3,4,4-tetrafluoro-1-butene, 1,6-bis(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, 2-(heptafluoropropoxy)hexafluoropropyl trifluorovinyl ether, 2,2,3,3-tetrafluoro-3-[[1,1,1,2,3,3-hexafluoro-3-[(1,2,2 -trifluorovinyl)oxy]propan-2-yl]oxy]propionitrile, pentafluorobenzyl methacrylate, 2,2,3,3-tetrafluoropropyl acrylate, 1H,1H,5H-octafluoropentyl methacrylate, 1H,1H,2H-heptadecafluoro-1-decene, 2,2,2-trifluoroethyl methacrylate, methyl 2-fluoroacrylate, 2,2,3,4,4,4-hexafluorobutyl methacrylate, 2,2,3,3,4,4,5,5,6,6,7,7-dodecafluoroheptyl methacrylate, 1H,Examples of the methacrylate include 1H,2H,2H-nonafluorohexyl, 2,2,3,3,4,4,4-heptafluorobutyl methacrylate, allyl pentafluorobenzene, 1-(3-butenyloxy)-2,3,3,4,4,5,5-heptafluorocyclopentene, vinyl trifluoroacetate, and 2-(trifluoromethyl)acrylic acid.
[0052] In particular, PTFE fine powder (also called PTFE aggregate dispersion) can be preferably used. PTFE fine powder is a PTFE powder produced by coagulating and drying an aqueous dispersion of PTFE fine particles (also called PTFE dispersion or PTFE aqueous dispersion) with an average particle size of 0.1 μm or more and 0.5 μm or less obtained by emulsion polymerization of tetrafluoroethylene. The average particle size of the PTFE powder is, for example, 200 μm or more and 1000 μm or less.
[0053] The number average molecular weight of PTFE is obtained by a method of determining the heat of crystallization of polymeric PTFE using a differential scanning calorimeter (DSC) and calculating the number average molecular weight based on the determined heat of crystallization. Specifically, a Shimadzu Corporation differential scanning calorimeter DSC-60A was used, and 9,400 mg of a sample of polymeric PTFE was weighed out, heated from room temperature to 380°C at a rate of 10°C / min, and then cooled to 200°C at a rate of 10°C / min. Then, the heat of crystallization (ΔHc: DSC heat of crystallization cal / g) was determined based on the peak area observed near 315°C during the temperature drop and the amount of the sample. The number average molecular weight Mn was then determined using the relationship between the number average molecular weight Mn and the heat of crystallization shown by the following formula (I). Mn = 2.1 × 10 10 ΔHc -5.16 (I)
[0054] <Structure of polymerization inhibitor> As the polymerization inhibitor contained in the sealing member of the present invention, an amine-based polymerization inhibitor and / or a phenol-based polymerization inhibitor can be used.
[0055] Examples of the amine-based polymerization inhibitor include phenothiazine, N,N'-di-naphthyl-p-phenylenediamine, poly(2,2,4-trimethyl-1,2-dihydroquinoline), di(4-octylphenyl)amine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, and N-(1,3-dimethylbutyl)-N'-phenyl-1,4-phenylenediamine.
[0056] In addition to the above, the amine-based polymerization inhibitor may be an aromatic secondary diamine compound such as N-phenyl-1-naphthylamine, octylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonylamide)diphenylamine, N,N'-diphenyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, or N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine. Nocrak ODA and Nocrak ODA-N (both manufactured by Ouchi Shinko Chemical Industry) may also be used.
[0057] Phenol-based polymerization inhibitors include catechol compounds such as 3,5-di-tert-butylcatechol and 4-tert-butylcatechol, phenol compounds such as 4-methylphenol, 4-methoxyphenol, 2,6-di-tert-butylphenol, 6-tert-butyl-2,4-xylenol, and 2,4-dinitrophenol, hydroquinone compounds such as hydroquinone, 2,5-di-tert-butylhydroquinone, and 2-tert-butylhydroquinone, and other compounds such as 2,6-di-tert-butyl-p-cresol, 2,2'-methylenebis(1,4-benzenediol), 4,4'-methylenebis(2-methylbenzene-1,3-diol), 2,2'-methylenebis(6-methyl-1,4-benzenediol), 2,2'-methylenebis(4-methylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), etc. can be used.
[0058] Also, compounds that have both a phenolic hydroxyl group and an amine group, such as 2-oxydiphenylamine, can be used.
[0059] The polymerization inhibitor is preferably a structure having two phenolic hydroxyl groups, and more preferably a structure having 1,4-benzenediol. This may be because the polymerization inhibitor has a strong polymerization inhibitory effect, but in addition, the affinity between the polymerization inhibitors is strong due to the π-π stacking between aromatics and the hydrogen bonds between hydroxyl groups, and the polymerization inhibitors are easy to coordinate, so that the retention is strong and the polymerization inhibitors are difficult to dissolve, which is preferable. In particular, when the resin portion is a fluorine atom-containing resin, the electron-attracting property of the fluorine atom is strong, so that the hydroxyl group of the polymerization inhibitor is electrostatically bonded to the hydroxyl group, and the polarization of the hydroxyl group is a phenolic hydroxyl group, so that the electrons are stabilized by the benzene ring, and the resin portion and the inhibitor and the inhibitors are each coordinated or electrostatically bonded to each other to form a network, so that the polymerization inhibitor is difficult to be removed, which is preferable. In particular, when the polymerization inhibitor has a structure having 1,4-benzenediol, the effect is high.
[0060] Furthermore, it is even more preferable that the resin portion of the sealing member is made of polytetrafluoroethylene and the polymerization inhibitor has a structure containing 1,4-benzenediol, since they have a higher affinity with each other and are less likely to be removed.
[0061] When the polymerization inhibitor has a structure having two phenolic hydroxyl groups, the electrostatic bonds between the polymerization inhibitors are not too strong, so that the polymerization inhibitor has excellent affinity with the sealing member, and the polarity of the polymerization inhibitor is not too high, so that the polymerization inhibitor is appropriately compatible with the polymerizable monomer, and therefore the polymerization inhibitor has excellent polymerization inhibition effect, which is more preferable, compared to when the polymerization inhibitor has a structure having three or more phenolic hydroxyl groups.
[0062] Therefore, when the resin portion of the sealing member is polytetrafluoroethylene, the polymerization inhibitor is preferably 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 3,5-di-tert-butylcatechol, 4-tert-butylcatechol, hydroquinone, 2-tert-butylhydroquinone, or 2,5-di-tert-hydroquinone, with 2-tert-butylhydroquinone or 2,5-di-tert-hydroquinone being particularly preferred.
[0063] In particular, the resin portion of the sealing member is polytetrafluoroethylene, and the SP value (SPp) of the polymerization inhibitor [(J / cm 3 ) 0.5 ] is 21.48 or more and 28.64 or less, and (SPp-SPb) [(J / cm 3 ) 0.5
[0046] It is particularly preferred that the polymerization inhibitor has a structure having 1,4-benzenediol and has a ratio of 1:1 to 1:1, since the polymerization inhibitor has a strong polymerization inhibitory effect, is less likely to be detached or eluted, and can suppress the blooming phenomenon for a long period of time.
[0064] <Melting point of polymerization inhibitor> From the viewpoint of heat resistance, the melting point of the polymerization inhibitor is preferably 70° C. or higher, more preferably 95° C. or higher, and even more preferably 120° C. or higher. In particular, a melting point of 120° C. or higher is preferable because it can be used not only in the polymerization reaction step but also in the distillation step and the like.
[0065] <Other fillers> The sealing member of the present invention may further contain a filler, such as alumina, titanium oxide, silica, barium sulfate, silicon carbide, silicon nitride, glass fiber, glass beads, mica, talc, graphite, carbon fiber, calcium carbonate, barium sulfate, kaolin, clay, etc. These fillers may be used alone or in combination of two or more.
[0066] Among the above fillers, alumina and / or titanium oxide are preferred. Alumina and titanium oxide are effective in improving the whiteness of the sealing member, and are also expected to improve heat resistance and inhibit polymerization.
[0067] The content of one or more fillers selected from alumina, titanium oxide, silica, barium sulfate, silicon carbide, silicon nitride, glass fiber, glass beads, and mica in the sealing member of the present invention is, for example, 0.5 mass% or more and 50 mass% or less, and preferably 1 mass% or more and 35 mass% or less.
[0068] The sealing member of the present invention may consist of, or may consist only of, polytetrafluoroethylene or modified polytetrafluoroethylene; an unmodified polymerization inhibitor; and, optionally, one or more fillers selected from alumina, titanium oxide, glass fibers, glass beads, and mica.
[0069] The PTFE composition may also contain an extrusion pressure reducing agent that reduces the extrusion pressure that increases due to the content of the filler. When the content of the filler in the PTFE composition is 40% by mass or more, the extrusion pressure increases significantly due to the content of the filler. For example, the extrusion pressure reducing agent may be a compound that reduces friction between the filler particles contained in the PTFE composition and particles of other compounds such as PTFE. Specifically, one or more compounds selected from the group consisting of an organic silane compound having a hydrocarbon group with 3 to 40 carbon atoms, an organic titanate compound, an organic aluminate compound, and a surfactant may be used. As the surfactant, a cationic surfactant, an anionic surfactant, a nonionic surfactant, or an amphoteric surfactant may be used.
[0070] The content of the extrusion pressure reducing agent in the PTFE composition may be, for example, 0.2% by mass or more and 10% by mass or less, 0.2% by mass or more and 8% by mass or less, or 0.5% by mass or more and 6% by mass or less.
[0071] <Sealing member configuration> The sealing member is preferably a packing, an O-ring, or a gasket, and more preferably a gasket, because a gasket, which is a sealing member used on a stationary surface, does not apply stress to the minute gaps in the resin part of the sealing member, and the polymerization inhibitor is not detached by an external force.
[0072] <Method of manufacturing the sealing member> The method for producing the sealing member of the present invention is preferably a method for producing a sealing member, characterized in that the resin part is molded to obtain an intermediate molded body, and then the intermediate molded body is impregnated with a solution of the polymerization inhibitor in an organic solvent to obtain the sealing member.
[0073] This is because the size of the gaps in the sealing member can be easily controlled and the occurrence of large gaps can be suppressed, and it is preferable for impregnating the gaps in the sealing member with a polymerization inhibitor dissolved in an organic solvent to sufficiently fill the gaps in the sealing member and to exert the effects of the present invention.
[0074] In addition, since the polymerization inhibitor to be filled is not exposed to high temperatures, the polymerization inhibitor does not undergo thermal decomposition, and the performance of the polymerization inhibitor does not deteriorate. Furthermore, even if a molding method is selected according to the material forming the resin part, the polymerization inhibitor can also be selected. Therefore, the shape of the resin part can be controlled as desired. As the organic solvent used in this case, alcohol, acetone, ether, etc., which are easy to remove later, are preferable.
[0075] In the method for producing the sealing member, the resin part may be formed by a conventional method. In particular, when PTFE is used, for example, a method of filling a mold with a raw material containing PTFE, compressing and molding the raw material at a surface pressure of 20 MPa to 60 MPa, and sintering the compression molded body at 350°C to 370°C, a method of producing the resin part using melt molding, or a method of cutting the outer peripheral surface of a sintered cylinder in the longitudinal direction to form a sheet, and then punching the sheet into an annular shape may be used.
[0076] [Configuration included in the embodiment of the present invention] The disclosure of this embodiment includes the following configuration. (Configuration 1) A sealing member having a resin portion containing a resin and a polymerization inhibitor, The SP value of the resin [(J / cm 3 ) 0.5 ] is SPb, the SP value of the polymerization inhibitor [(J / cm 3 ) 0.5 When SPp is taken as the value, the relationship of the following formula (1) is satisfied, SPp-SPb≦16.37...Equation (1) a sealing member characterized in that, in a cross-sectional observation of the resin part of the sealing member, when an area of the cross-section occupied by the polymerization inhibitor is taken as 100 area %, an area of domains of the polymerization inhibitor that are occupied by domains having a short axis of 5 μm or more is 25 area % or less. (Configuration 2) The sealing member according to configuration 1, wherein the content of the polymerization inhibitor in the sealing member is 0.1% by mass or more and 10.0% by mass or less. (Configuration 3) The sealing member according to Configuration 1 or 2, in which, upon cross-sectional observation of the resin part of the sealing member, when the area of the cross-section occupied by the polymerization inhibitor is taken as 100 area %, the area of domains of the polymerization inhibitor that are occupied by domains having a short axis of 5 μm or more is 15 area % or less. (Configuration 4) The sealing member according to any one of configurations 1 to 3, wherein the resin portion has a Young's modulus of 0.1 GPa or more and 30.0 GPa or less. (Configuration 5) The sealing member according to any one of configurations 1 to 4, wherein the resin is polytetrafluoroethylene. (Configuration 6) The sealing member according to any one of configurations 1 to 5, wherein the polymerization inhibitor has a structure having two phenolic hydroxyl groups. (Configuration 7) The sealing member according to any one of configurations 1 to 6, wherein the melting point of the polymerization inhibitor is 120° C. or higher. (Configuration 8) The sealing member according to any one of configurations 1 to 7, which is a gasket. (Configuration 9) A method for producing the sealing member according to any one of configurations 1 to 8, comprising the steps of: A method for producing a sealing member, comprising: molding the resin to obtain an intermediate molded body; and impregnating the intermediate molded body with a solution of the polymerization inhibitor in an organic solvent to obtain the sealing member. EXAMPLES
[0077] Example 1 (Production of intermediate molded body) The PTFE powder was filled into a mold and compression molded from above and below at a pressure of 40 MPa for 0.5 hours to obtain a preform (outer diameter 100 mm x height 20 mm).
[0078] The obtained preform was placed in a firing furnace and fired at 370° C. for 5 hours. The obtained cylindrical fired body (outer diameter 100 mm × height 20 mm) was turned on a lathe to produce a sheet with a thickness of 1.5 mm. The sheet was punched out to obtain a donut-shaped (annular) gasket intermediate.
[0079] (Gasket manufacturing) The intermediate molded body obtained was immersed in a solution of 2-tert-butylhydroquinone (polymerization inhibitor) dissolved in methanol at a concentration of 20% by mass, and left for 24 hours. The amount of the methanol solution of 2-tert-butylhydroquinone was 10 times the volume of the sheet. The sheet was then placed in a vacuum dryer in a temperature environment of 25°C to remove alcohol, and a gasket 1 was obtained.
[0080] [Examples 2 to 11, Examples 13 to 15, 19 to 22, 25 to 26, Comparative Examples 1 to 3] Gaskets 2 to 11, 13 to 15, 19 to 22, 25 to 26, and 27 to 29 were obtained in the same manner as in Example 1, except that the types and amounts of raw materials used were changed as shown in Tables 1 and 2.
[0081] Example 16 A gasket 16 was obtained in the same manner as in Example 1, except that the amount of polymerization inhibitor added was changed as shown in Table 2 and the pressing pressure was changed to 50 MPa.
[0082] Example 17 Gasket 17 was obtained in the same manner as in Example 1, except that the amount of polymerization inhibitor added was changed as shown in Table 2 and the pressing pressure was changed to 35 MPa.
[0083] Example 18 A gasket 18 was obtained in the same manner as in Example 1, except that the amount of polymerization inhibitor added was changed as shown in Table 2 and the pressing pressure was changed to 30 MPa.
[0084] [Examples 23 and 24] A packing 1 and an O-ring 1 were obtained in the same manner as in Example 1, except that the shapes were changed as shown in Table 2.
[0085] Example 12 (Production of acrylic resin 2) 100 parts by mass of propylene glycol monomethyl ether was heated under nitrogen substitution and refluxed at a liquid temperature of 120°C or higher, and a mixture of 250 parts by mass of 1H,1H,2H-heptadecafluorodecyl acrylate, 50 parts by mass of hydroxyethyl acrylate, and 1.00 parts by mass of tert-butyl peroxybenzoate [organic peroxide polymerization initiator, NOF Corp., product name "Perbutyl Z"] was added dropwise over 3 hours. After the dropwise addition, the solution was stirred for 3 hours, and then distilled at normal pressure while increasing the liquid temperature to 170°C. After the liquid temperature reached 170°C, the solvent was removed by distillation under reduced pressure at 1 hPa for 1 hour to obtain a resin solid. The solid was dissolved in tetrahydrofuran, reprecipitated with n-hexane, and the precipitated solid was filtered to obtain an acrylic resin 2. The physical properties of the obtained acrylic resin 2 are shown below. Weight average molecular weight (Mw) = 15,000, Mw / Mn = 2.4, glass transition temperature (Tg) = 70°C
[0086] (Production of intermediate molded body) 300 parts by mass of acrylic resin 2 and 50 parts by mass of hexamethylenediamine were placed in a mold and cured by urethane bonding at 80°C for 10 hours in a convection oven to obtain a cylindrical molded body. The obtained cylindrical fired body (outer diameter 100 mm x height 20 mm) was turned on a lathe to produce a sheet with a thickness of 1.5 mm. The sheet was punched out to obtain a donut-shaped (annular) gasket intermediate molded body.
[0087] (Gasket manufacturing) The intermediate molded body obtained was immersed in a solution of 20% by mass of 2-tert-butylhydroquinone dissolved in methanol and left for 24 hours. The amount of the 2-tert-butylhydroquinone methanol solution was 10 times the volume of the sheet. The sheet was then placed in a vacuum dryer at a temperature of 25°C to remove the alcohol, and a gasket 12 was obtained.
[0088] Comparative Example 4 A mixture of PTFE powder and 2-tert-butylhydroquinone in a mass ratio of 100:2 was filled into a mold and compression molded from above and below at a pressure of 50 MPa for 0.5 hours to obtain a preform (outer diameter 100 mm x height 20 mm).
[0089] The obtained preform was placed in a firing furnace and fired at 370° C. for 5 hours. The obtained cylindrical fired body (outer diameter 100 mm × height 20 mm) was turned on a lathe to produce a sheet with a thickness of 1.5 mm. The sheet was punched out to obtain a donut-shaped (annular) gasket 30.
[0090] [Comparative Examples 5 to 8] Gaskets 31 to 34 were obtained in the same manner as in Comparative Example 4, except that the pressing pressure was changed to 40 MPa and the types and amounts of raw materials were changed as shown in Table 2.
[0091] [Table 1]
[0092] [Table 2]
[0093] <Evaluation of sealing materials> The sealing members according to the respective Examples and Comparative Examples were evaluated for the following characteristics, and the results are shown in Table 3.
[0094] [Mass change rate before and after immersion] An ASTM micro dumbbell test piece was punched out from the obtained sealing member to prepare an immersion sample. The obtained immersion sample was set on the ceiling of a 2 L pressure vessel, and the vessel was filled with a 1:1 (v:v) mixture of styrene monomer and butadiene monomer that did not contain a polymerization inhibitor, so that the immersion sample did not come into contact with the mixture.
[0095] The container was kept at 75°C and 0.8MPa for 30 days, after which the sample was taken out and dried. The mass of the dried sample after immersion was measured, and the mass increase from the sample before the immersion test was measured. The increase was due to the solid content generated by polymerization of butadiene monomer gas in the sample.
[0096] Table 3 also shows the evaluation ranking based on the following criteria. (Evaluation Criteria) A: 1.0% by mass or less B: More than 1.0 mass% and 2.0 mass% or less C: More than 2.0% by mass and 3.0% by mass or less D: More than 3.0 mass% and 4.0 mass% or less E: More than 4.0% by mass
[0097] [Polymerization inhibitor residual rate] An ASTM micro dumbbell test piece was punched out from the obtained sealing member to prepare an immersion sample. The obtained immersion sample was set on the ceiling of a 2 L pressure vessel, and the vessel was filled with a 1:1 (v:v) mixture of styrene monomer and butadiene monomer that did not contain a polymerization inhibitor, so that the immersion sample did not come into contact with the mixture.
[0098] The container was kept at 50°C x 1.0 MPa and the sample was left for 5 days, then taken out and dried. The dried sample was cut out and used as a measurement sample. Measurement was performed using pyrolysis GC-MS under the following conditions, and the residual rate of polymerization inhibitor in the sheet was evaluated from the peak position and area of the obtained spectrum. (Measurement conditions) Thermal decomposition temperature and time: 445℃×5sec GC section Column: Ultra alloy-1 Temperature rise conditions: 50℃→300℃ (heat rise rate 20℃ / min)
[0099] Table 3 also shows the evaluation ranking based on the following criteria. (Evaluation Criteria) A: 92% by mass or more B: 87% by mass or more and less than 92% by mass C: 82% by mass or more and less than 87% by mass D: Less than 82% by mass
[0100] [Compression set] The compression set in the present invention is measured after compressing by 25% for 70 hours at 150° C., and the rate of non-recovery after release from compression is expressed as 100% compression. Specifically, the compression set is measured by the following procedure. (1) Prepare a test piece of 10 mm x 10 mm x 2 mmt from the sealing material. (2) The sealing member is compressed by 25% and kept at 150°C for 70 hours. (3) The force causing the compressive deformation is removed, i.e., the sealing member is released from compression. Temperature when released: 23℃, Release time: 0.5 hours (4) When released from compression, the hardened material will attempt to return to its pre-compression shape (recover).
[0101] Compression set is the deformation that remains after the force that caused the deformation is removed, expressed as a percentage. In other words, if the shape of the cured product after release from compression remains the same as the shape that was compressed before release, the compression set is 100%. On the other hand, if the cured product completely returns to the shape it was before compression, the compression set is 0%.
[0102] Table 3 also shows the evaluation ranking based on the following criteria. (Evaluation Criteria) A: 7% or less B: More than 7% and less than 14% C: More than 14%
[0103] [Table 3]
Claims
1. A sealing member having a resin portion containing a resin and a polymerization inhibitor, The SP value of the resin [(J / cm 3 ) 0.5 ] is SPb, the SP value of the polymerization inhibitor [(J / cm 3 ) 0.5 When SPp is taken as the value of the particle diameter, the relationship of the following formula (1) is satisfied: SPp-SPb≦16.37 ... formula (1). A sealing member characterized in that, in a cross-sectional observation of the resin part of the sealing member, when an area of the cross-section occupied by the polymerization inhibitor is taken as 100 area %, an area of domains of the polymerization inhibitor whose short axis is 5 μm or more is occupied by 25 area % or less.
2. The seal member according to claim 1 , wherein the content of the polymerization inhibitor in the seal member is from 0.1% by mass to 10.0% by mass.
3. 3. The sealing member according to claim 1, wherein, in a cross-sectional observation of the resin part of the sealing member, when an area occupied by the polymerization inhibitor in the cross section is taken as 100 area %, an area occupied by domains of the polymerization inhibitor having a minor axis of 5 μm or more is 15 area % or less.
4. 3. The sealing member according to claim 1, wherein the resin portion has a Young's modulus of 0.1 GPa or more and 30.0 GPa or less.
5. 3. The sealing member according to claim 1, wherein the resin is polytetrafluoroethylene.
6. 3. The sealing member according to claim 1, wherein the polymerization inhibitor has a structure having two phenolic hydroxyl groups.
7. 3. The sealing member according to claim 1, wherein the melting point of the polymerization inhibitor is 120° C. or higher.
8. The sealing member according to claim 1 or 2, which is a gasket.
9. A method for manufacturing the seal member according to claim 1 or 2, comprising the steps of: A method for producing a sealing member, comprising: molding the resin to obtain an intermediate molded body; and impregnating the intermediate molded body with a solution of the polymerization inhibitor in an organic solvent to obtain the sealing member.
Citation Information
Patent Citations
Fluororesin-made gasket for piping seal
JP2014196779A
Molded body and method for producing same
WO2015151515A1