Processing method for wafer
By forming a protective film with narrowing sidewalls and applying plasma treatment to stabilize the mask, the method addresses the issue of sidewall tilt during plasma etching, ensuring precise and high-quality wafer processing.
Patent Information
- Application Number
- JP2023061915
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
The formation of laser-processed grooves with inclined sidewalls leads to a thinner protective film at the bottom edge, causing the mask to tilt and recede during plasma etching, resulting in increased etched width and deteriorated processing quality due to changes in mask shape.
A method involving the formation of a first protective film, followed by laser irradiation to create a groove with narrowing sidewalls, application of a second protective film through plasma treatment to reduce sidewall slope, and subsequent plasma etching using a second gas to expose the wafer, with optional repetition of deposition and removal steps to maintain sidewall integrity.
The method improves plasma etching quality by maintaining sidewall stability and reducing the etched width, preventing mask shape changes and enhancing processing precision.
Smart Images

Figure 2024148615000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a wafer processing method. [Background technology]
[0002] A known method for processing a wafer involves forming a protective film on the upper surface of the wafer, removing the protective film by irradiating it with a laser beam, forming a laser-processed groove that exposes the wafer, and then processing the wafer by plasma etching along the laser-processed groove using the protective film as a mask (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-027889 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, because the sidewalls of the laser-machined grooves are formed at an incline, the protective film formed on the edge of the bottom of the groove is thinner than the protective film formed on the surface of the wafer, and is removed during plasma etching and retreats to the outside of the groove, exposing the wafer. When the protective film near the bottom of the laser-machined groove is removed, the sidewalls of the mask formed by the protective film also retreat at an incline, resulting in a problem that the width of the wafer etched becomes large, making it impossible to realize a narrow kerf, and a problem that the processing quality of the chip deteriorates due to a change in the mask shape during etching.
[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a wafer processing method capable of improving processing quality in plasma etching. [Means for solving the problem]
[0006] In order to solve the above-mentioned problems and achieve the object, the wafer processing method of the present invention is a processing method for processing a wafer, comprising: a first protective film forming step of forming a first protective film on a front surface of a wafer; a processed groove forming step of removing the first protective film by irradiating a laser beam after the first protective film forming step to expose the wafer and forming a processed groove whose sidewall is inclined in a direction in which the opening width narrows from the front surface to the back surface; and a plasma treatment using a first gas after the processed groove forming step. the deposition step of depositing a second protective film on the sidewalls and bottom surface of the processed groove to form a second protective film that reduces the inclination of the sidewalls of the processed groove; a second protective film removal step of removing the second protective film deposited on the bottom surface of the processed groove by plasma etching using a second gas after the deposition step to expose the wafer; and a wafer processing step of processing the wafer along the processed groove covered with the second protective film by plasma etching using a third gas.
[0007] The depositing step and the second protective film removing step may be performed repeatedly.
[0008] In the groove forming step, the groove may be formed so that the width of the groove is equal to or less than twice the depth of the groove.
[0009] The second protective film may be removed by ashing using a fourth gas in plasma form.
[0010] The first protective film is a water-soluble resin and may be removed with a liquid. Effect of the Invention
[0011] The present invention forms a second protective film that reduces the slope of the sidewall of the processed groove, so that the sidewall of the second protective film can be maintained in an optimal state while the wafer exposed at the bottom of the processed groove can be excavated toward the back side, thereby improving the processing quality in plasma etching. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a perspective view that illustrates a wafer to be processed by a wafer processing method according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view that typically shows a main part of the wafer shown in FIG. [Diagram 3] FIG. 3 is a flowchart showing a flow of the wafer processing method according to the embodiment. [Figure 4] FIG. 4 is a cross-sectional view that illustrates a schematic view of a main part of the wafer after the first protective film forming step of the wafer processing method illustrated in FIG. [Diagram 5] FIG. 5 is a cross-sectional view that illustrates a schematic view of a main part of a wafer after a groove forming step in the wafer processing method shown in FIG. [Figure 6] FIG. 6 is a schematic partial cross-sectional view of a main portion of the wafer during the deposition step of the wafer processing method shown in FIG. [Figure 7] FIG. 7 is a schematic partial cross-sectional view of a main portion of a wafer during the second protective film removal step of the wafer processing method shown in FIG. [Figure 8] FIG. 8 is a schematic partial cross-sectional view of a main portion of a wafer during the wafer processing step of the wafer processing method shown in FIG. [Figure 9] FIG. 9 is a cross-sectional view that typically shows a main part of the wafer after the protective film removing step in the wafer processing method shown in FIG. [Figure 10] FIG. 10 is a schematic partial cross-sectional view of a main portion of a wafer during the wafer processing method according to the comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.
[0014] [Embodiment] A wafer processing method according to an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a perspective view that typically shows a wafer 1 to be processed by the wafer processing method according to the embodiment. Fig. 2 is a cross-sectional view that typically shows a main part of the wafer 1 shown in Fig. 1. Fig. 3 is a flow chart showing the flow of the wafer processing method according to the embodiment.
[0015] (Wafer) The wafer processing method according to the embodiment is a method for processing a wafer 1 shown in Fig. 1. In this embodiment, the wafer 1 is a wafer such as a disk-shaped semiconductor wafer having a substrate 2 made of silicon, glass, SiC, sapphire, gallium arsenide, or the like. As shown in Fig. 1, the wafer 1 has devices 5 formed in areas partitioned in a lattice pattern by a plurality of planned division lines 4 formed in a lattice pattern on a surface 3.
[0016] The device 5 is, for example, an integrated circuit such as an IC (Integrated Circuit) or an LSI (Large Scale Integration), a CCD (Charge Coupled Device), or a memory (semiconductor memory device).
[0017] In this embodiment, the wafer 1 has a functional layer 6 laminated on the surface of the substrate 2, as shown in Figures 1 and 2. The functional layer 6 includes a low dielectric constant insulator coating (hereinafter referred to as a Low-k film) made of an inorganic film such as SiOF, BSG (SiOB), or an organic film such as a polymer film of a polyimide system or parylene system, or carbon-containing silicon oxide (SiOCH), and a circuit layer including a conductive metal pattern or metal film.
[0018] The low-k film is laminated with a circuit layer to form the device 5. The circuit layer constitutes the circuit of the device 5. For this purpose, the device 5 is constituted by the mutually laminated low-k films of the functional layer 6 laminated on the substrate 2, and the circuit layer laminated between the low-k films. At the planned division line 4, the functional layer 6 is constituted by the low-k film laminated on the substrate 2.
[0019] The functional layer 6 such as a low-k film is easily peeled off from the substrate 2 when the wafer 1 is cut from the front surface 3 side with a cutting blade. Thus, in this embodiment, the wafer 1 has the devices 5 formed on the front surface 3 by the functional layer 6 laminated on the substrate 2.
[0020] (Wafer Processing Method) The wafer processing method according to the embodiment is a method of processing a wafer 1, on which a plurality of devices 5 are formed by a functional layer 6 laminated on the surface of a substrate 2, along a planned division line 4 that divides the plurality of devices 5. Note that in this embodiment, the wafer processing method is also a method of dividing (corresponding to processing) the wafer 1 along the planned division lines 4 into individual device chips 10 (shown in FIG. 1). Note that the device chip 10 includes a part of the substrate 2 and a device 5. Note that although this embodiment is described with a configuration in which a functional layer 6 is laminated on the surface of the substrate 2, the functional layer 6 may not be formed.
[0021] As shown in Fig. 3, the wafer processing method includes a first protective film forming step 101, a processed groove forming step 102, a deposition step 103, a second protective film removing step 104, a wafer processing step 105, and a protective film removing step 106. In this embodiment, the wafer processing method includes adhering a disk-shaped tape 11 having a larger diameter than the wafer 1 to the back surface 9 behind the front surface 3, adhering an annular frame 12 to the outer edge of the tape 11, and processing the wafer 1 supported by the frame 12, as shown in Fig. 1.
[0022] (First protective film forming step) Fig. 4 is a cross-sectional view showing a schematic view of a main part of the wafer 1 after a first protective film forming step 101 of the wafer processing method shown in Fig. 3. Fig. 4 is a cross-sectional view in a cross section perpendicular to the front surface 3 and back surface 9 of the wafer 1, i.e., in a cross section parallel to the thickness direction of the wafer 1. The first protective film forming step 101 is a step of forming a first protective film 13 (shown in Fig. 4) on the front surface 3 of the wafer 1 before the processing groove forming step 102 is performed.
[0023] In this embodiment, in the first protective film forming step 101, a resin coating device (not shown) suction-holds the back surface 9 of the wafer 1 on the holding surface of the spinner table via the tape 11, clamps the frame 12 with a clamping section, rotates the spinner table about its axis, and drips liquid water-soluble resin from a water-soluble resin supply nozzle onto the center of the front surface 3 of the wafer 1. The dripped water-soluble resin flows from the center to the outer periphery on the front surface 3 of the wafer 1 due to centrifugal force generated by the rotation of the spinner table, and is applied to the entire surface of the front surface 3 of the wafer 1. Note that although this embodiment is described as including the frame 12, the frame 12 need not be used.
[0024] The water-soluble resin contains a water-soluble resin such as polyvinyl alcohol (PVA) or polyvinylpyrrolidone (PVP). In the first protective film forming step 101, the water-soluble resin applied to the entire surface of the front surface 3 of the wafer 1 is dried, so that the entire surface of the front surface 3 of the wafer 1 is covered with a first protective film 13 containing a water-soluble resin, as shown in FIG. 4. Thus, in this embodiment, the first protective film 13 is made of a water-soluble resin. Furthermore, when dried, the water-soluble resin constituting the first protective film 13 has a lower etching rate than the substrate 2 with respect to the third gas 18 (shown in FIG. 8) that is made into plasma and is used in the wafer processing step 105, and has resistance.
[0025] (Groove formation step) FIG. 5 is a cross-sectional view showing a schematic view of a main part of the wafer 1 after the processing groove forming step 102 of the wafer processing method shown in FIG. 3. FIG. 5 and FIGS. 6 to 9 described later are all cross-sectional views in a cross section parallel to the thickness direction of the wafer 1 and perpendicular to the extension direction of the processing groove 14. The processing groove forming step 102 is a step in which, after the first protective film forming step 101, a laser beam (not shown) is irradiated from the front surface 3 of the wafer 1 along the dividing line 4, the first protective film 13 is removed by the irradiation of the laser beam to expose the substrate 2 of the wafer 1, and a processing groove 14 (shown in FIG. 5) is formed in which the side wall 14-2 is inclined in a direction in which the opening width 14-1 narrows from the front surface 3 toward the back surface 9. In this embodiment, in the processing groove forming step 102, the functional layer 6 formed on the dividing line 4 is also removed by the irradiation of the laser beam.
[0026] In this embodiment, in the processed groove forming step 102, a laser processing device (not shown) suction-holds the back surface 9 of the wafer 1 on the holding surface of a holding table via tape 11, and clamps the frame 12 with a clamp section. In this embodiment, in the processed groove forming step 102, the laser processing device images the front surface 3 of the wafer 1 with an imaging unit (not shown), detects the planned division lines 4, and performs alignment to align the laser beam application unit with the planned division lines 4.
[0027] In this embodiment, in the processed groove forming step 102, the laser processing device irradiates the wafer 1 along the planned dividing lines 4 with a laser beam having a wavelength absorbed by the wafer 1 from the laser beam application unit while moving the wafer 1 and the laser beam application unit relatively along the planned dividing lines 4. Note that in this embodiment, in the processed groove forming step 102, the laser processing device sets the focusing point of the laser beam on the surface of the first protective film 13 or the surface of the substrate 2, and irradiates the wafer 1 with the laser beam along each planned dividing line 4.
[0028] In this embodiment, in the groove formation step 102, a laser processing device performs ablation processing on the first protective film 13, functional layer 6 and substrate 2 on each planned division line 4 to remove portions of these, thereby forming grooves 14, which are laser grooving (LG) grooves that divide the first protective film 13 and functional layer 6 at each planned division line 4, as shown in Figure 5.
[0029] In this embodiment, in the groove forming step 102, a laser beam is irradiated to both edges in the width direction of each division line 4 to ablate the first protective film 13, the functional layer 6 and the substrate 2 at both edges in the width direction of each division line 4 to form a groove, and then a laser beam is irradiated between the grooves of each division line 4 to ablate the first protective film 13, the functional layer 6 and the substrate 2 between the grooves of each division line 4 to form a groove 14. In this embodiment, in the groove forming step 102, a laser beam having a wavelength of 355 nm (not limited to 355 nm, a wavelength in the ultraviolet region is preferable) and a repetition frequency of 200 kHz to 2000 kHz is irradiated.
[0030] In this embodiment, in the processed groove forming step 102, the laser beam is branched to form two both edge processed grooves on both edges in the width direction of the dividing line 4, and when performing the ablation processing, the average output of the laser beam is set to 0.5 W, the relative moving speed between the laser beam application unit and the wafer 1 (hereinafter referred to as the processing feed speed) is set to 100 mm / sec to 400 mm / sec, and the spot of the focusing point of the laser beam is set to a circle with a diameter of 5 μm. In this embodiment, in the processed groove forming step 102, when performing the ablation processing between the both edge processed grooves of the dividing line 4, the average output of the laser beam is set to 10.0 W, the processing feed speed is set to 200 mm / sec to 1000 mm / sec, and the spot of the focusing point of the laser beam is set to a rectangle with a width of 60 μm.
[0031] In this embodiment, all the grooves 14 have the same opening width 14-1, and the sidewalls 14-2 have a tapered inclination in the direction in which the opening width 14-1 narrows from the same front surface 3 to the back surface 9. Here, the opening width 14-1 of the groove 14 in this embodiment refers to the width between both ends of the groove 14 along a direction parallel to the front surface 3 and the back surface 9 of the wafer 1 and perpendicular to the extension direction of the groove 14. In this embodiment, the inclination of the sidewalls 14-2 of the groove 14 is expressed by, for example, a width by which the opening width 14-1 narrows (a length by which it decreases) when it becomes deeper by a predetermined unit length along the thickness direction of the wafer 1 from the front surface 3 to the back surface 9.
[0032] In the groove forming step 102, it is preferable to form the groove 14 so that the opening width 14-1 of the groove 14 is not more than twice the depth 14-4 of the groove 14. In the groove forming step 102, it is preferable to form the groove 14 so that the opening width 14-1 at the bottom surface 14-3 of the groove 14 is not more than twice the depth 14-4 of the groove 14, and it is more preferable to form the groove 14 so that the opening width 14-1 of the groove 14 at the upper surface of the wafer 1 (upper surface of the first protective film 13) is not more than twice the depth 14-4 of the groove 14. In such a case, in the deposition step 103, the components of the deposited film based on the plasmatized first gas 15 (shown in Figure 6) are less likely to deposit on the bottom surface 14-3 of the groove 14 than on the top surface of the wafer 1, and are more difficult to deposit on the side wall 14-2 of the groove 14 as the depth increases. This makes it possible to more significantly form a second protective film 16 (shown in Figure 6) that reduces the slope of the side wall 14-2 of the groove 14 in the deposition step 103 described below.
[0033] (Deposition step) Fig. 6 is a schematic partial cross-sectional view of a main part of the wafer 1 during a deposition step 103 of the wafer processing method shown in Fig. 3. The deposition step 103 is a step of depositing a second protective film 16 (shown in Fig. 6) on the upper surface of the wafer 1, the sidewall 14-2 of the groove 14, and the bottom surface 14-3 of the groove 14 by plasma processing using a first gas 15 (shown in Fig. 6) that has been made plasmatized after the groove formation step 102, thereby forming the second protective film 16 that reduces the inclination of the sidewall 14-2 of the groove 14.
[0034] In this embodiment, in the deposition step 103, a plasma processing device (not shown) holds the back surface 9 of the wafer 1 on the holding surface of the holding table via a tape 11. In this embodiment, in the deposition step 103, high frequency power for creating and maintaining plasma is applied to the upper electrode, and high frequency power for attracting ions is applied to the holding table, which is the lower electrode, while supplying the plasmatized first gas 15 to the front surface 3 of the wafer 1. In this embodiment, in the deposition step 103, the first gas 15 is, for example, C4F8, and the second protective film 16 formed on the inner surface of the processed groove 14 by the plasma treatment using the plasmatized first gas 15 is a deposition film of a CF-based gas component based on the C4F8 of the plasmatized first gas 15.
[0035] In this embodiment, in the deposition step 103, the components of the deposition film based on the plasmatized first gas 15 are less likely to deposit on the bottom surface 14-3 of the groove 14 than on the top surface of the wafer 1, and are less likely to deposit on the sidewall 14-2 of the groove 14 as the deposition position deepens. Therefore, the second protective film 16 becomes thinner as the deposition position deepens on the sidewall 14-2 of the groove 14. As a result, the inclination of the tapered shape of the sidewall 16-2 of the second protective film 16 is smaller than the inclination of the sidewall 14-2 of the groove 14. Here, the inclination of the sidewall 16-2 of the second protective film 16 is represented by the width by which the opening width 16-1 narrows (the length by which it decreases) when the sidewall 16-2 of the second protective film 16 becomes deeper by a predetermined unit length from the front surface 3 toward the back surface 9 along the thickness direction of the wafer 1. In this embodiment, the opening width 16-1 of the second protective film 16 refers to the width between both ends of a groove formed by the surface of the second protective film 16, which is parallel to the front surface 3 and back surface 9 of the wafer 1 and perpendicular to the extension direction of the groove 14. Thus, in this embodiment, in the deposition step 103, the second protective film 16 is formed on the inner surface of the groove 14, thereby mitigating, i.e., reducing, the inclination of the sidewall 14-2 of the groove 14.
[0036] The inclination of the sidewall 14-2 of the groove 14 and the inclination of the sidewall 16-2 of the second protective film 16 may be expressed by the angle (inclination angle) of the inner surface of the sidewall 14-2, 16-2 with respect to a reference plane parallel to the thickness direction of the wafer 1 and the extension direction of the groove 14, instead of being expressed by the width (reduced length) of the opening widths 14-1, 16-1 as described above. Even when expressed in this way, the inclination angle of the sidewall 16-2 of the second protective film 16 is smaller than the inclination angle of the sidewall 14-2 of the groove 14.
[0037] (Second protective film removal step) Fig. 7 is a schematic partial cross-sectional view of a main part of the wafer 1 during a second protective film removing step 104 of the wafer processing method shown in Fig. 3. The second protective film removing step 104 is a step in which the second protective film 16 deposited on the bottom surface 14-3 of the processed groove 14 is removed by plasma etching using a second gas 17 (shown in Fig. 7) that has been made into plasma after the deposition step 103, thereby exposing the substrate 2 of the wafer 1.
[0038] In this embodiment, in the second protective film removal step 104, a plasma processing device (not shown) holds the back surface 9 of the wafer 1 on the holding surface of the holding table via a tape 11. In this embodiment, in the second protective film removal step 104, high frequency power for creating and maintaining plasma is applied to the upper electrode, and high frequency power for attracting ions is applied to the holding table, which is the lower electrode, while supplying the plasmatized second gas 17 to the front surface 3 of the wafer 1. In this embodiment, in the second protective film removal step 104, the second gas 17 is, for example, O2. In this embodiment, in the second protective film removal step 104, anisotropic etching is performed using the plasmatized second gas 17 to selectively etch and remove the bottom surface 16-3 of the second protective film 16 deposited on the bottom surface 14-3 of the processed groove 14 while maintaining the side wall 16-2 of the second protective film 16 deposited on the side wall 14-2 of the processed groove 14.
[0039] In this embodiment, in the second protective film removing step 104, anisotropic etching is performed with the second gas 17 made into plasma, so that as the inclination of the sidewall 16-2 of the second protective film 16 becomes smaller, the risk of etching the second protective film 16 deposited on the sidewall 14-2 of the processed groove 14 is reduced. In this embodiment, since the second protective film 16 that reduces the inclination of the sidewall 14-2 of the processed groove 14 is formed in the depositing step 103, in the second protective film removing step 104, the second protective film 16 deposited on the bottom surface 14-3 of the processed groove 14 can be selectively etched and removed while favorably maintaining the sidewall 14-2 of the second protective film 16 deposited on the sidewall 14-2 of the processed groove 14.
[0040] In this embodiment, the deposition step 103 and the second protective film removal step 104 may be performed once, or may be repeated multiple times. Each time the deposition step 103 and the second protective film removal step 104 are performed once, the slope of the sidewall 16-2 of the second protective film 16 is reduced. Therefore, the deposition step 103 and the second protective film removal step 104 can be repeatedly performed until the slope of the sidewall 16-2 of the second protective film 16 is reduced to a desired value or less.
[0041] (Wafer processing step) Fig. 8 is a schematic partial cross-sectional view of a main part of the wafer 1 in a wafer processing step 105 of the wafer processing method shown in Fig. 3. The wafer processing step 105 is a step of processing the substrate 2 of the wafer 1 along the processing groove 14 covered with the second protective film 16 after the second protective film removing step 104.
[0042] In this embodiment, the wafer processing step 105 includes a deposition reinforcement step in which a second protective film 16 is further deposited on the side wall 16-2 of the second protective film 16 to reinforce it, and a deep engraving processing step in which the substrate 2 of the wafer 1 exposed on the bottom surface 14-3 of the processing groove 14 is excavated toward the back surface 9 by plasma etching using a third gas 18 that has been converted into plasma.
[0043] In this embodiment, in the deposition reinforcement step of the wafer processing step 105, similar to the deposition step 103, a plasma treatment device (not shown) supplies the first gas 15, which has been converted into plasma, to the front surface 3 side of the wafer 1 to reinforce the side wall 16-2 of the second protective film 16. Therefore, in the deposition reinforcement step of the wafer processing step 105, similar to the deposition step 103, the side wall 16-2 of the second protective film 16 that reduces the inclination of the side wall 14-2 of the processed groove 14 is re-formed.
[0044] In this embodiment, in the deep engraving step of the wafer processing step 105, a plasma processing apparatus (not shown) holds the back surface 9 of the wafer 1 on the holding surface of a holding table via a tape 11. In this embodiment, in the deep engraving step of the wafer processing step 105, high frequency power for generating and maintaining plasma is applied to the upper electrode, and high frequency power for attracting ions is applied to the holding table, which is the lower electrode, while supplying a plasmatized third gas 18 (shown in FIG. 8) to the front surface 3 side of the wafer 1. In this embodiment, in the deep engraving step of the wafer processing step 105, the third gas 18 is, for example, C4F8 and SF6.
[0045] In this embodiment, in the wafer processing step 105, a so-called Bosch process is carried out in which a deposition reinforcement step and a deep excavation processing step are alternately and repeatedly performed in separate processes, so that the etching amount of the sidewall 16-2 of the second protective film 16 is made sufficiently smaller than the etching amount of the substrate 2 of the wafer 1 exposed on the bottom surface 14-3 of the processed groove 14, and a high aspect ratio is maintained, and the substrate 2 of the wafer 1 exposed on the bottom surface 14-3 of the processed groove 14 can be excavated toward the back surface 9. Note that, in the wafer processing step 105, the present invention is not limited to this, and the deposition reinforcement step and the deep excavation processing step may be simultaneously performed in parallel to maintain a high aspect ratio, and the substrate 2 of the wafer 1 exposed on the bottom surface 14-3 of the processed groove 14 can be excavated toward the back surface 9.
[0046] In this embodiment, in the deep engraving processing step of the wafer processing step 105, etching is performed using the third gas 18 that has been converted into plasma. Therefore, as the inclination of the side wall 16-2 of the second protective film 16 becomes smaller, the risk of etching the second protective film 16 deposited on the side wall 14-2 of the processed groove 14 is reduced. In this embodiment, a second protective film 16 that reduces the slope of the side wall 14-2 of the processed groove 14 is formed in the deposition step 103, and the side wall 16-2 of the second protective film 16 that reduces the slope of the side wall 14-2 of the processed groove 14 is re-formed in the deposition reinforcement step of the wafer processing step 105.Therefore, in the deep engraving processing step of the wafer processing step 105, the side wall 16-2 of the second protective film 16 deposited on the side wall 14-2 of the processed groove 14 can be favorably maintained while maintaining a high aspect ratio, and the substrate 2 of the wafer 1 exposed on the bottom surface 14-3 of the processed groove 14 can be engraven toward the back surface 9.
[0047] In this embodiment, in the wafer processing step 105, the plasma processing apparatus performs plasma etching on the wafer 1 until the processed grooves 14 open on the back surface 9 side and the wafer 1 is divided into device chips 10, as shown in Fig. 8. Thus, in this embodiment, in the wafer processing step 105, the wafer 1 is divided to manufacture a plurality of device chips 10.
[0048] (Protection film removal step) Fig. 9 is a cross-sectional view showing a schematic view of a main part of the wafer 1 after the protective film removing step 106 of the wafer processing method shown in Fig. 3. The protective film removing step 106 is a step of removing the first protective film 13 and the second protective film 16 after the wafer processing step 105 is performed.
[0049] In this embodiment, the protective film removal step 106 includes an ashing step of removing the second protective film 16 by ashing using a plasmatized fourth gas (not shown), and a cleaning step of removing the first protective film 13 by cleaning with a liquid after the ashing step is performed.
[0050] In this embodiment, in the ashing step of the protective film removal step 106, a plasma processing device (not shown) holds the back surface 9 of the wafer 1 on the holding surface of the holding table via tape 11. In this embodiment, in the ashing step of the protective film removal step 106, high frequency power is applied to the upper electrode to generate and maintain plasma, and high frequency power is applied to the lower electrode, which is the holding table, to attract ions while supplying a fourth gas that has been made into plasma to the front surface 3 of the wafer 1. In this embodiment, in the ashing step of the protective film removal step 106, the fourth gas is, for example, O2. In this embodiment, in the ashing step of the protective film removal step 106, the second protective film 16 is decomposed and removed by the fourth gas that has been made into plasma.
[0051] In this embodiment, in the cleaning step of the protective film removal step 106, a cleaning device (not shown) suction-holds the back surface 9 of the wafer 1 on the holding surface of the spinner table via the tape 11, clamps the frame 12 with a clamping section, and supplies a cleaning liquid consisting of pure water or pure water containing a surfactant from a cleaning liquid supply nozzle to the center of the front surface 3 of the wafer 1 while rotating the spinner table around its axis. The cleaning liquid supplied to the front surface 3 of the wafer 1 flows from the center side to the outer periphery side on the front surface 3 of the wafer 1 due to centrifugal force generated by the rotation of the spinner table, cleaning the front surface 3 of the wafer 1, and removes the first protective film 13 containing a water-soluble resin from the front surface 3 of the wafer 1 together with foreign matter such as debris, as shown in FIG. 9.
[0052] FIG. 10 is a schematic partial cross-sectional view of a main part of a wafer 1 during the wafer processing method according to the comparative example. In order to more clearly explain this embodiment, a comparative example based on the conventional technology will be described in comparison with this embodiment. In the comparative example, the deposition step 103 and the second protective film removal step 104, which are the main parts of this embodiment, are omitted, and the wafer processing step 105 is performed. In such a comparative example, for a wafer 1 in which the surface 3 is covered with the first protective film 13 and the first protective film 13, the functional layer 6, and the substrate 2 are formed with a processed groove 14 by ablation processing, if the deposition step 103 and the second protective film removal step 104 are omitted and the processed groove 14 is dug in the same manner as the wafer processing step 105, as shown in FIG. 10, the functional layer 6 and the substrate 2 in the region close to the bottom surface 14-3 on the side wall 14-2 of the processed groove 14 are easily removed during the wafer processing step 105 because the deposition amount of the second protective film 16 is small. Furthermore, during this wafer processing step 105, the functional layer 6 located on the sidewall 14-2 of the processed groove 14 may be damaged, and coupled with the thin thickness of the functional layer 6 itself, the functional layer 6 is removed faster than the first protective film 13. For this reason, during this wafer processing step 105, the sidewall 14-2 of the mask that protects the upper part of the substrate 2, which is essentially formed of the first protective film 13 and the functional layer 6, recedes at an incline, so that the shape of the mask changes during the process, and the groove width 14-5 in which the substrate 2 is etched gradually increases, and there is a risk of the etching quality deteriorating.
[0053] In contrast to such comparative examples, in this embodiment, in order to perform the deposition step 103 and the second protective film removal step 104, the second protective film 16 is formed, which reduces the risk of the functional layer 6 and substrate 2 in the area close to the bottom surface 14-3 on the side wall 14-2 of the processing groove 14 being removed during the wafer processing step 105, and reduces the risk of the side wall 14-2 of the mask protecting the upper part of the substrate 2, which is essentially formed by the first protective film 13 and the functional layer 6, tilting and retreating.
[0054] In the wafer processing method according to the embodiment described above, a second protective film 16 that reduces the slope of the side wall 14-2 of the processed groove 14 is formed in the deposition step 103, so that in the second protective film removal step 104, the second protective film 16 deposited on the bottom surface 14-3 of the processed groove 14 can be selectively etched and removed while favorably maintaining the side wall 16-2 of the second protective film 16 deposited on the side wall 14-2 of the processed groove 14, and in the wafer processing step 105, the substrate 2 of the wafer 1 exposed on the bottom surface 14-3 of the processed groove 14 can be excavated toward the back surface 9 while favorably maintaining the side wall 16-2 of the second protective film 16 deposited on the side wall 14-2 of the processed groove 14 and maintaining a high aspect ratio. Therefore, the wafer processing method according to the embodiment can suppress the risk of the sidewall 16-2 of the second protective film 16 being etched and tilted, thereby making it possible to maintain the width of the substrate 2 of the wafer 1 etched narrow and large to realize a narrow kerf, and can suppress the mask shape from changing during etching, thereby suppressing the risk of quality defects such as unevenness in the shape of the sidewall of the substrate 2 of the processed wafer 1. In this way, the wafer processing method according to the embodiment can improve the processing quality in plasma etching.
[0055] Moreover, in the wafer processing method according to the embodiment, since the deposition step 103 and the second protective film removal step 104 are repeatedly performed, the inclination of the sidewall 16-2 of the second protective film 16 can be reduced to a desired value or less. As a result, the wafer processing method according to the embodiment can further improve the processing quality in plasma etching.
[0056] Furthermore, in the wafer processing method of the embodiment, in the groove formation step 102, the groove is formed so that the opening width 14-1 of the groove 14 is less than twice the depth 14-4 of the groove 14. Therefore, in the subsequent deposition step 103, the components of the deposited film based on the plasmatized first gas 15 are less likely to deposit on the bottom surface 14-3 of the groove 14 than on the top surface of the wafer 1, and are more difficult to deposit on the side wall 14-2 of the groove 14 as the depth increases. As a result, a second protective film 16 can be formed which more significantly reduces the slope of the side wall 14-2 of the groove 14.
[0057] In addition, in the wafer processing method according to the embodiment, the second protective film 16 is removed by ashing using the fourth gas that has been made into plasma. Therefore, in the wafer processing method according to the embodiment, the second protective film 16 is suitably removed, thereby improving the processing quality in plasma etching.
[0058] In the wafer processing method according to the embodiment, the first protective film 13 is a water-soluble resin and is removed by washing with a liquid. Therefore, the wafer processing method according to the embodiment can improve processing quality in plasma etching by suitably removing the first protective film 13.
[0059] It should be noted that the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the gist of the present invention. [Explanation of symbols]
[0060] 1 wafer 2. Board 3 surface 9 Back side 13 1st protective film 14 Machining groove 14-1,16-1 Opening width 14-2,16-2 Side wall 14-3,16-3 Bottom 14-4 Depth 15 First Gas 16 Second protective film 17 Second Gas 18 The Third Gas 101 First protective film formation step 102 Groove formation step 103 Deposition Step 104 Second protective film removal step 105 Wafer Processing Steps 106 Protective film removal step
Claims
1. A processing method for processing a wafer, comprising the steps of: a first protective film forming step of forming a first protective film on a surface of the wafer; a groove forming step of removing the first protective film by irradiating the wafer with a laser beam to expose the wafer after the first protective film forming step, and forming a groove having a sidewall that is inclined in a direction in which an opening width narrows from the front surface to the back surface; a deposition step of depositing a second protective film on the upper surface of the wafer, the sidewall of the groove, and the bottom surface of the groove by plasma processing using a first gas after the groove formation step, thereby forming a second protective film that reduces the inclination of the sidewall of the groove; a second protective film removing step of removing the second protective film deposited on the bottom surface of the groove by plasma etching using a second gas after the depositing step, thereby exposing the wafer; a wafer processing step of processing the wafer along the processing groove covered with the second protective film by plasma etching using a third gas; A wafer processing method comprising the steps of:
2. 2. The wafer processing method according to claim 1, wherein the depositing step and the second protective film removing step are repeatedly performed.
3. 2. The wafer processing method according to claim 1, wherein in the groove forming step, the groove is formed so that the width of the groove is not more than twice the depth of the groove.
4. 2. The method for processing a wafer according to claim 1, wherein the second protective film is removed by ashing using a fourth gas in the form of plasma.
5. 2. The method for processing a wafer according to claim 1, wherein the first protective film is a water-soluble resin and is removed by a liquid.
Citation Information
Patent Citations
Processing method of work piece
JP2020027889A