Nitrided steel component and method for manufacturing nitrided steel component

The nitrided steel component with a quenched hardened layer and nitrided hardened layer improves wear resistance and lifespan by employing a multi-layered structure with optimized hardness and toughness through instant quenching.

JP2024148619APending Publication Date: 2024-10-18HITACHI CONSTRUCTION MACHINERY CO LTD

Patent Information

Application Number
JP2023061921
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Conventional nitrided steel parts require improved wear resistance to extend their lifespan.

Method used

A nitrided steel component with a nitrided layer that includes a quenched hardened layer extending from the surface in the depth direction, featuring a pearlite structure and martensitic structure with fine carbides, and a nitrided hardened layer with a ferrite structure, both having higher hardness than the core, achieved through instant quenching using a laser.

Benefits of technology

Enhances wear resistance and extends the lifespan of nitrided steel components by incorporating a multi-layered structure with optimized hardness and toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148619000001_ABST
    Figure 2024148619000001_ABST
Patent Text Reader

Abstract

To provide a nitrided steel component that can improve wear resistance.SOLUTION: A nitrided steel component includes: a nitrided steel member provided with a nitrided layer at the surface layer part thereof. The nitrided layer includes: a quench-hardened layer in a depth direction from the surface. The quench-hardened layer has hardness that is harder than that of the surface layer part of the nitrided steel member and a center part on a center side.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nitrided steel part used as a machine structural part and a method for manufacturing the nitrided steel part. [Background technology]

[0002] Conventionally, for example, steel mechanical structural parts such as gears, pistons, axles, shafts, and cams have been subjected to surface hardening treatments such as carburizing and quenching, nitriding, and quenching in order to improve mechanical strength such as surface pressure strength, wear resistance, and bending fatigue strength. Various techniques are known for steel parts obtained by surface hardening treatment and methods of surface hardening treatment.

[0003] For example, a reprocessed part obtained by further performing flash quenching on a carburized part and a manufacturing method for the reprocessed part including the flash quenching method are known (Patent Document 1). The reprocessed part has a carburized layer on its surface, and in the carburized layer, three layers, a first hardened layer, a second hardened layer, and a third hardened layer, each of which has a higher hardness than the core, are adjacent to each other in the depth direction from the surface, and the first hardened layer has the highest hardness of the three layers, and the second hardened layer has the lowest hardness of the three layers. The manufacturing method includes a step of preparing a carburized part having a carburized layer on its surface, and a step of performing flash quenching on the carburized part to form the three layers in the carburized layer. According to these, the life of the carburized part can be extended by a simple and inexpensive method using only heat treatment.

[0004] Also, a quenched steel member obtained by carrying out a composite heat treatment method, which is a type of surface hardening treatment, and the composite heat treatment method thereof are known (Patent Document 2). The composite heat treatment method includes a step of forming a nitrogen compound layer on the surface of a steel base material by nitriding treatment and diffusing nitrogen into the surface layer portion of the steel base material covered with the nitrogen compound layer, and a step of forming a hardened layer containing diffused nitrogen and a fine martensite structure on the surface side of the surface layer portion of the steel base material directly below the nitrogen compound layer by high-frequency hardening in ammonia gas or the like, with an effective hardened layer depth of 200 μm or more from the surface (Patent Document 2). According to these, in the quenched steel member, mechanical strength, sliding resistance, wear resistance, etc. based on the characteristics of the nitrogen compound layer are maintained, and the formation of the nitrogen compound layer increases the hardness of the surface layer portion of the steel base material, improving the hardenability. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2022 / 230937 [Patent Document 2] International Publication No. 2011 / 013559 Summary of the Invention [Problem to be solved by the invention]

[0006] Among steel parts obtained by conventional surface hardening treatment, nitrided steel parts obtained by nitriding treatment include parts in which the surface layer of the steel member is hardened, as described in Patent Document 2. On the other hand, there is a demand for nitriding steel parts that have a longer life than ever before by improving the wear resistance through hardening the surface layer of the steel member.

[0007] The present invention has been made in view of the above-mentioned problems, and has as its main object to provide a nitrided steel part and a manufacturing method for a nitrided steel part that can improve wear resistance. [Means for solving the problem]

[0008] In order to solve the above problems, the nitriding steel part of the present invention is a nitriding steel part comprising a nitriding steel member having a nitrided layer provided on a surface layer portion, the nitriding layer having a quench-hardened layer in a depth direction from the surface, and the quench-hardened layer having a higher hardness than a core portion of the nitriding steel member that is closer to the center than the surface layer portion.

[0009] Furthermore, the manufacturing method of the nitriding steel part of the present invention is a method for manufacturing the above-mentioned nitriding steel part, and is characterized in that it comprises the steps of: preparing a steel member made of a nitriding steel; performing a nitriding treatment on the steel member to convert the steel member into a nitriding steel member having a nitrided layer formed on a surface layer portion; and performing flash quenching on the nitriding steel member to convert the nitrided layer into a layer having the quench-hardened layer in the depth direction from the surface. Effect of the Invention

[0010] According to the present invention, the wear resistance can be improved.

[0011] Objects, configurations, and effects of the present invention other than those described above will become apparent from the following description of the preferred embodiments of the present invention. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1(a) is a schematic cross-sectional view showing a nitrided steel part according to the first embodiment, FIG. 1(b) is a schematic cross-sectional view showing the cross-sectional structure of the quench-hardened layer of the nitrided steel part according to the first embodiment, and FIG. 1(c) is a schematic cross-sectional view showing the cross-sectional structure of the nitrided hardened layer of the nitrided steel part according to the first embodiment. [Diagram 2] 1(a) to 1(d) are schematic cross-sectional views illustrating steps of a manufacturing method for a nitriding steel part according to a first embodiment. [Diagram 3] 1(a) and 1(b) are schematic diagrams illustrating a flash quenching step in a manufacturing method for a nitrided steel part according to a first embodiment. [Figure 4] FIG. 5 is a schematic cross-sectional view showing a nitrided steel part according to a second embodiment. [Diagram 5] 6(a) to 6(c) are schematic cross-sectional views illustrating steps of a manufacturing method for a nitrided steel part according to a second embodiment. [Figure 6] 1 is a graph showing the wear amounts and the average amounts of the two test samples of the embodiment and the seven test samples of the comparative example. [Figure 7] 1 is a graph showing hardness distribution in the cross-sectional depth direction of a test sample of an example and a test sample of a comparative example. [Figure 8] 1 is a photograph of the cross-sectional structure of a region with a cross-sectional depth of less than 300 μm in a test sample of an example and a test sample of a comparative example, observed by SEM. [Figure 9] FIG. 9 is a diagram showing a schematic cross-sectional structure of the test sample of the example and the test sample of the comparative example shown in FIG. 8. [Figure 10] 1 is a graph showing the half-value widths of X-ray diffraction peaks of the diffraction plane of the martensite phase of each sample of the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, a nitrided steel part and a method for manufacturing a nitrided steel part according to an embodiment of the present invention will be described. First, an overview of the nitrided steel part and the manufacturing method of the nitrided steel part according to the embodiment will be described by taking as examples the nitrided steel part and the manufacturing method of the nitrided steel part according to the first and second embodiments.

[0014] (First embodiment) FIG. 1(a) is a schematic cross-sectional view showing a nitrided steel part according to the first embodiment, FIG. 1(b) is a schematic cross-sectional view showing the cross-sectional structure of the quench-hardened layer of the nitrided steel part according to the first embodiment, and FIG. 1(c) is a schematic cross-sectional view showing the cross-sectional structure of the nitrided hardened layer of the nitrided steel part according to the first embodiment.

[0015] As shown in Fig. 1(a), the nitrided steel part 10 according to the first embodiment comprises a nitrided steel member 11 consisting of a surface layer 11P facing a surface 11S and a core portion 11C closer to the center than the surface layer 11P, with a nitrided layer 12 provided on the surface layer 11P. The nitrided layer 12 has a quench hardened layer 14 and a nitrided hardened layer 16, in this order, in the depth direction from the surface 12S. That is, the nitrided layer 12 has the quench hardened layer 14 in the depth direction from the surface 12S, and further has a nitrided hardened layer 16 in the depth direction from the end of the quench hardened layer 14 on the core portion 11C side of the nitrided steel member 11.

[0016] As shown in FIG. 1(b), the quench hardened layer 14 includes a pearlite structure and a martensite structure. The pearlite structure has a lamellar structure in which ferrite and cementite are alternately arranged. Fine carbides are precipitated in the ferrite of the pearlite structure. The martensite structure has a structure in which many fine lath martensites are assembled. In the martensite structure, fine carbides are precipitated mainly at the lath boundaries (boundaries between lath martensites). The quench hardened layer 14 has a higher dislocation density than the nitrided hardened layer 16.

[0017] As shown in FIG. 1(c), the nitrided layer 16 includes a pearlite structure and a ferrite structure. The pearlite structure has a lamellar structure in which ferrite and cementite are arranged alternately. The ferrite structure is composed of ferrite. In addition, unlike the quench hardened layer 14, the nitrided layer 16 does not have fine carbides precipitated therein.

[0018] Both the quench hardened layer 14 and the nitrided layer 16 have a higher hardness than the core 11C of the nitrided steel member 11. The quench hardened layer 14 has a higher hardness than the nitrided layer 16.

[0019] As described above, the nitrided steel part 10 according to the first embodiment includes a nitrided steel member 11 having a nitrided layer 12 provided on the surface layer 11P, and the nitrided layer 12 has a quenched hardened layer 14 in the depth direction from the surface 12S. The quenched hardened layer 14 includes a pearlite structure having a lamellar structure in which ferrite and cementite are alternately arranged, thereby achieving composite strengthening, and fine carbides are precipitated in the ferrite of the pearlite structure, thereby achieving precipitation strengthening. In addition, the quenched hardened layer 14 includes a martensite structure having a structure in which a large number of fine lath martensites are assembled, thereby achieving fine grain strengthening, and fine carbides are precipitated in the martensite structure, thereby achieving precipitation strengthening. Furthermore, the dislocation density is higher than that of the nitrided hardened layer 16, thereby achieving dislocation strengthening. As a result, the quenched hardened layer 14 has a higher hardness than the nitrided hardened layer 16, and can maintain high toughness. Therefore, the wear resistance of the nitrided steel part 10 can be improved.

[0020] In addition, the nitrided layer 12 further has a nitrided layer 16 in the depth direction from the end of the quench hardened layer 14 on the side of the core 11C of the nitrided steel member 11. Unlike the quench hardened layer 14, the nitrided layer 16 does not contain a martensite structure and does not have fine carbides precipitated therein. As a result, the hardness of the nitrided layer 16 is lower than that of the quench hardened layer 14. This makes it possible to increase the toughness of the nitrided layer 12 compared to when the nitrided layer 12 is composed only of the quench hardened layer 14. This makes it possible to further improve the wear resistance of the nitrided steel part 10.

[0021] A method for manufacturing a nitrided steel part 10 according to the first embodiment will now be described. Figures 2(a) to 2(d) are schematic cross-sectional views illustrating the steps of the method for manufacturing a nitrided steel part according to the first embodiment.

[0022] In the manufacturing method of the nitriding steel part according to the first embodiment, first, as shown in FIG. 2(a), a steel member 1 made of steel for nitriding is prepared (preparation step).

[0023] Next, as shown in Fig. 2(b), the steel member 1 is subjected to a nitriding treatment to turn the steel member 1 into a nitrided steel member 11 having a nitride layer 12 formed on a surface layer portion 1P facing the surface 1S (nitriding treatment step). At this time, a nitrogen compound layer 5 is formed on the surface 11S of the nitriding steel member 11. Note that the surface layer portion 1P of the steel member 1 corresponds to the surface layer portion 11P of the nitriding steel member 11, and the core portion 1C of the steel member 1 corresponds to the core portion 11C of the nitriding steel member 11. Next, as shown in Fig. 2(c), the nitrogen compound layer 5 is removed by a method such as mechanical polishing (removal step).

[0024] 2(d), the nitrided steel member 11 is flash-hardened by a laser to turn the nitrided layer 12 into a layer having a quench-hardened layer 14 and a nitrided layer 16 in this order in the depth direction from the surface 12S (flash-hardening process). That is, the nitrided layer 12 is turned into a layer having a quench-hardened layer 14 in the depth direction from the surface 12S, and further having a nitrided layer 16 in the depth direction from the end of the quench-hardened layer 14 on the core 11C side of the nitrided steel member 11.

[0025] Here, Fig. 3(a) and Fig. 3(b) are schematic diagrams for explaining the instantaneous quenching step in the manufacturing method of the nitrided steel part according to the first embodiment. In the instantaneous quenching step, as shown in Fig. 3(a), a laser irradiation device 100 is used, and laser light from a laser oscillator 101 is conveyed by an optical fiber 102 and converged by a condenser lens 103, and the surface 11S of the nitrided steel component 11 is irradiated with the laser light L so as to scan the surface 11S of the nitrided steel component 11 with the converged laser light L. This causes instantaneous heating in which the temperature of the area near the laser light irradiated portion of the nitrided steel component 11 rises locally and in a very short time to the heat treatment temperature. Then, as shown in Fig. 3(b), after irradiation with the laser light L, heat is rapidly conducted from the area near the laser light irradiated portion of the nitrided steel component 11 to the center side, and the area near the laser light irradiated portion is rapidly cooled naturally. As a result, the area near the laser light irradiated portion of the nitrided steel component 11 is quenched, and the area near the laser light irradiated portion becomes a quench-hardened layer 14.

[0026] The above steps are used to manufacture the nitrided steel part 10. Therefore, the wear resistance of the nitrided steel part 10 can be improved by the simple and inexpensive method of flash quenching the nitrided steel member 11.

[0027] Second embodiment 4 is a schematic cross-sectional view showing a nitriding steel part according to the second embodiment. The nitriding steel part 10 according to the second embodiment includes, in addition to the nitriding steel member 11 similar to that of the nitriding steel part 10 according to the first embodiment, a nitrogen compound layer 5 provided on the surface 11S of the nitriding steel part 11. As a result, the nitriding steel part 10 according to the second embodiment not only achieves the same effects as the nitriding steel part 10 according to the first embodiment, but also achieves the effects of improving wear resistance due to structural modification and improved hardness.

[0028] A method for manufacturing a nitrided steel part 10 according to the second embodiment will now be described. Figures 5(a) to 5(c) are schematic cross-sectional views illustrating the steps of the method for manufacturing a nitrided steel part according to the second embodiment.

[0029] In the manufacturing method of the nitrided steel part according to the second embodiment, first, as shown in Fig. 5(a) and Fig. 5(b), a steel member 1 made of a steel for nitriding is prepared in the same manner as in the manufacturing method according to the first embodiment, and the steel member 1 is subjected to a nitriding treatment to form a nitrided steel member 11 having a nitrided layer 12 formed on a surface layer portion 1P (preparation step and nitriding treatment step). Next, as shown in Fig. 5(c), while the nitrogen compound layer 5 is maintained, the nitrided steel member 11 is subjected to instantaneous quenching by a laser, so that the nitrided layer 12 is formed into a layer having a quenched hardened layer 14 and a nitrided hardened layer 16 in this order in the depth direction from the surface 12S (instantaneous quenching step). At this time, the surface 5S of the nitrogen compound layer 5 is irradiated with the laser light L so as to scan the surface 5S of the nitrogen compound layer 5 with the laser light L, thereby performing instantaneous heating and instantaneous cooling of the area of ​​the nitrided steel member 11 near the laser light irradiated portion. Through the above steps, the nitrided steel part 10 is manufactured.

[0030] As described above, according to the nitrided steel part of the embodiment, it is possible to improve the wear resistance of the nitrided steel part and extend its life, as with the nitrided steel parts of the first and second embodiments. Also, according to the manufacturing method of the nitrided steel part of the embodiment, it is possible to improve the wear resistance of the nitrided steel part and extend its life, as with the manufacturing methods of the first and second embodiments, by using a simple and inexpensive method of flash quenching the nitriding steel member.

[0031] Next, the nitrided steel part and the method for manufacturing the nitrided steel part according to the embodiment will be described in more detail.

[0032] 1.Nitrided steel parts A nitriding steel part is a nitriding steel part comprising a nitriding steel member having a nitrided layer provided on a surface layer portion, the nitriding layer having a quench-hardened layer extending in a depth direction from the surface, and the quench-hardened layer having a higher hardness than a core portion of the nitriding steel member that is closer to the center than the surface layer portion.

[0033] The nitrided layer is not particularly limited as long as it has a quench-hardened layer extending in the depth direction from the surface, but it is preferable that the quench-hardened layer further has a nitrided hardened layer extending in the depth direction from the end of the quench-hardened layer on the core side of the nitriding steel member, the nitrided hardened layer having a higher hardness than the core of the nitriding steel member, and the quench-hardened layer having a higher hardness than the nitrided hardened layer.

[0034] The nitrided layer can be confirmed, for example, by measuring the mass concentration of nitrogen in a cross section intersecting with the surface of the nitrided steel part using EDS (Energy Dispersive X-ray spectrometry) or EPMA (Electron Probe Micro Analyzer). The quench hardened layer and the nitrided hardened layer can be confirmed, for example, by observing a cross section intersecting with the surface of the nitrided steel part using an SEM (Scanning Electron Microscope).

[0035] The quench hardened layer is not particularly limited as long as it has a higher hardness than the core of the nitriding steel member, but as in the first and second embodiments, it is preferable that the quench hardened layer contains a pearlite structure and fine carbides are precipitated in the ferrite of the pearlite structure. This is because the wear resistance of the nitrided steel part is effectively improved. Also, as in the first and second embodiments, it is preferable that the quench hardened layer contains a martensite structure and fine carbides are precipitated in the martensite structure. This is because the wear resistance of the nitrided steel part is effectively improved.

[0036] The thickness of the quench hardened layer is preferably, for example, 50 μm or more and 500 μm or less, and more preferably 250 μm or more and 350 μm or less. When the thickness of the quench hardened layer is equal to or more than these lower limits, the life of the nitriding steel parts used in construction machines can be sufficiently extended. When the thickness of the quench hardened layer is equal to or less than these upper limits, the quench hardened layer can be formed by flash quenching without difficulty.

[0037] The nitrided hardened layer is not particularly limited as long as it has a higher hardness than the core of the nitrided steel member, but it is preferable that the nitrided hardened layer contains a pearlite structure and a ferrite structure as in the first and second embodiments, because this effectively improves the wear resistance of the nitrided steel part.

[0038] The thickness of the nitrided hardened layer is, for example, preferably 50 μm or more and 500 μm or less, more preferably 50 μm or more and 400 μm or less, and particularly preferably 50 μm or more and 300 μm or less. When the thickness of the nitrided hardened layer is equal to or more than these lower limits, the life of the nitrided steel parts used in construction machines can be sufficiently extended. When the thickness of the nitrided hardened layer is equal to or less than these upper limits, the nitrided hardened layer can be formed by nitriding without difficulty.

[0039] As for the quench hardened layer and the nitrided hardened layer, the quench hardened layer preferably has a Vickers hardness of 600 Hv or more, because this effectively improves the wear resistance of the nitrided steel part. Also, the nitrided hardened layer preferably has a Vickers hardness of 400 Hv or more and less than 600 Hv, because this effectively improves the wear resistance of the nitrided steel part.

[0040] The nitrided steel part may be one in which the nitrogen compound layer formed on the surface of the nitrided steel member by nitriding has been removed, as in the first embodiment, or one in which the nitrogen compound layer has not been removed but which still further comprises a nitrogen compound layer, as in the second embodiment.

[0041] The nitrided steel part is not particularly limited as long as it is used as a mechanical structural part, but for example, a gear or a piston is preferable. As the piston, a piston of a hydraulic part used in a hydraulic pump or a hydraulic motor of a hydraulic device is preferable. As the piston of a gear or hydraulic part, a piston of a gear or hydraulic part used in a construction machine is preferable. As the method for producing the nitrided steel part, it is not particularly limited, but for example, the method for producing a nitrided steel part described below is preferable.

[0042] 2. Manufacturing method of nitrided steel parts The manufacturing method of a nitriding steel part is a method for manufacturing the above-mentioned nitriding steel part, and includes the steps of: preparing a steel member made of a steel for nitriding (preparation step); performing a nitriding treatment on the steel member to turn the steel member into a nitriding steel member having a nitride layer formed on the surface portion (nitriding treatment step); and performing flash quenching on the nitriding steel member to turn the nitrided layer into a layer having the quench-hardened layer in the depth direction from the surface (flash quenching step).

[0043] The steel member prepared in the preparation step is processed into the shape of the nitriding steel part and has been subjected to pretreatment including, for example, quenching and tempering. The nitriding steel constituting the steel member is not particularly limited, and examples thereof include alloy steels containing alloy components such as Al, Cr, V, and Ti. This is because these alloy components have a strong chemical affinity with nitrogen. Examples of such alloy steels include Al-Cr-Mo alloy steels such as nitriding steel SACM645 specified in JIS, Al-Cr alloy steels, Al-Cr-V alloy steels, Cr-Mo alloy steels, Cr-Mo-V alloy steels, Ni-Cr-Al alloy steels, and Ni-Cr-Mo-Al alloy steels.

[0044] The nitriding treatment performed in the nitriding step is not particularly limited, and examples thereof include gas nitriding and gas soft nitriding. The gas nitriding is a treatment in which nitrogen is allowed to penetrate and diffuse from the surface of the steel member, and the nitrogen is reacted with metal atoms such as iron to generate a compound such as iron nitride, thereby forming a nitride layer on the surface layer of the steel member. The method of the gas nitriding is not particularly limited, and may be a general method, and examples thereof include a method in which the steel member is heated to a predetermined temperature in an atmosphere of ammonia gas or the like and maintained for a predetermined time. The gas soft nitriding is a treatment in which carbon is allowed to penetrate and diffuse from the surface of the nitriding steel material, together with nitrogen, to react with metal atoms such as iron to generate a compound such as iron nitride, thereby forming a nitride layer on the surface layer of the steel member. The method of the gas soft nitriding is not particularly limited, and may be a general method, and examples thereof include a method in which the steel member is heated to a predetermined temperature in an atmosphere of ammonia gas, nitrogen, and carbon dioxide mixed gas, and maintained for a predetermined time. In the gas nitriding and gas soft nitriding treatments, the depth of the nitrided layer and the nitrogen concentration can be adjusted by controlling conditions such as the concentration of each gas in the atmosphere, the heating temperature, and the treatment time.

[0045] The nitriding treatment may be any of gas nitriding treatment, gas soft nitriding treatment, etc., but gas nitriding treatment is preferred. Gas nitriding treatment requires a long time of about 10 to 30 hours, but the hardness of the nitrided layer increases and the hardened region of the nitrided layer becomes deep. Therefore, the wear resistance of the nitrided steel part can be effectively improved.

[0046] The method for producing a nitrided steel part is not particularly limited, but may further include, for example, a step of removing a nitrogen compound layer formed on the surface of the nitrided steel part by the nitriding treatment (a removal step) after the nitriding treatment step and before the flash quenching step, as in the first embodiment, or may not include the removal step, as in the second embodiment.

[0047] The "instantaneous quenching" performed in the instantaneous quenching process refers to quenching in which a particle beam such as a laser beam, an electron beam, or a neutron beam (hereinafter collectively referred to as "laser beam, etc.") is irradiated onto the surface of a nitriding steel member, thereby performing instantaneous heating and instantaneous cooling to harden the surface. The principle of instantaneous quenching is that the surface of the nitriding steel member or the nitrogen compound layer is irradiated with a laser beam, etc. so as to scan the surface of the nitriding steel member or the nitrogen compound layer with the laser beam, thereby performing instantaneous heating in which the temperature of the area near the laser beam irradiated area of ​​the nitriding steel member rises locally and in a very short time to the heat treatment temperature, and after the irradiation of the laser beam, etc., heat is rapidly conducted from the area near the laser beam irradiated area of ​​the nitriding steel member to the center, and the area is rapidly cooled naturally, thereby performing instantaneous cooling to harden the area. As a result, the area near the area becomes a quench-hardened layer.

[0048] The instantaneous hardening process is not particularly limited, but a process in which the instantaneous hardening is performed by a laser is preferred because it is advantageous from the viewpoints of simplicity and cost. A known device can be used as a laser irradiation device for performing instantaneous hardening by a laser. Incidentally, instantaneous hardening performed by a laser is sometimes called "laser hardening".

[0049] The laser used in the laser hardening is not particularly limited, but examples thereof include semiconductor laser, YAG laser, CO2, etc., among which semiconductor laser, etc. are preferred. The conditions for the laser hardening are not particularly limited as long as a hardened layer can be formed, but the conditions under which the hardened layer can be formed as a layer containing the above-mentioned pearlite structure or martensite structure and in which fine carbides are precipitated, with a thickness in the above-mentioned preferred range, are preferred.

[0050] As the flash quenching process, a process in which flash quenching can be performed without specially controlling the atmosphere and in which flash quenching is performed in air is preferable.

[0051] Although there is no particular limitation on the manufacturing method of the nitrided steel part, a method in which the Vickers hardness of the nitrided layer before the flash quenching is 400 Hv or more and less than 600 Hv, and the Vickers hardness of the quench-hardened layer is 600 Hv or more is preferred, because this effectively improves the wear resistance of the nitrided steel part.

[0052] A preferred method for manufacturing a nitrided steel part is one in which the wear amount of the nitrided steel member after the flash quenching in a lubricating oil wear test (reciprocating sliding test) conducted under conditions of a load of 400 N, a reciprocating frequency of 50 Hz, a reciprocating stroke of 1 mm, and a friction time of 2 hours, using a steel ball of 10 mm diameter made of SUJ2 specified in JIS (Japanese Industrial Standards) G4805 as the mating material, is 33% to 50% lower than the wear amount of the nitrided steel member before the flash quenching in the lubricating oil wear test. EXAMPLES

[0053] EXAMPLES Hereinafter, the nitrided steel part and the method for manufacturing the nitrided steel part according to the embodiment will be described more specifically with reference to examples and comparative examples.

[0054] [Example] Two test samples of the nitriding steel part according to the embodiment were manufactured. When manufacturing each test sample, first, a steel member made of nitriding steel (SCM435) was prepared (preparation step).

[0055] Next, the steel member was subjected to a nitriding treatment to form a nitrided steel member having a nitrided layer formed on the surface layer (nitriding treatment step). During this treatment, a nitrogen compound layer was formed on the surface of the nitrided steel member. Next, the nitrogen compound layer was removed by a method such as mechanical polishing (removal step).

[0056] Next, the nitrided steel member was flash-hardened by laser to form the nitrided layer into a layer having a hardened layer and a nitrided layer in that order from the surface in the depth direction (flash-hardening process). In the laser hardening, a semiconductor laser was used as the laser, the output (peak output) of the laser light was 1.6 kW, and the scanning speed of the laser light was 100 mm / min. Each test sample was manufactured by the above process.

[0057] [Comparative Example] Seven test samples of the nitrided steel parts were produced by a manufacturing method similar to that of the test samples of the Examples, except that no flash quenching was performed.

[0058] [Evaluation of wear resistance] A lubricating oil wear test (reciprocating sliding test) was carried out on two test samples of the nitrided steel parts manufactured in the embodiment and seven test samples of the nitrided steel parts manufactured in the comparative example. The test samples were circular flat steel members with a diameter and a plate thickness of 24 mm x 7.9 mm. The lubricating oil wear test was carried out under the following conditions: a load of 400 N, a reciprocating frequency of 50 Hz, a reciprocating stroke of 1 mm, a friction time of 2 hours, lubricating oil of 0.25 ml, a lubricating oil temperature of 100°C, and a friction time of 2 hours, with a counter material being a steel ball made of SUJ2 as specified in JIS (Japanese Industrial Standards) G4805. The depth of the wear marks on each test sample after the wear test was measured as the amount of wear, and the wear resistance was evaluated. FIG. 6 is a graph showing the amount of wear and the average amount of wear of two test samples of the embodiment and seven test samples of the comparative example.

[0059] As shown in Fig. 6, the wear amounts of both of the two test samples of the embodiment were smaller than the wear amounts of all of the seven test samples of the comparative example. In addition, the reduction rate of the maximum wear amount of the two test samples of the embodiment relative to the minimum wear amount of the seven test samples of the comparative example was 33%, and the reduction rate of the minimum wear amount of the two test samples of the embodiment relative to the maximum wear amount of the seven test samples of the comparative example was 50%.

[0060] [Evaluation of hardness distribution in the cross-sectional depth direction] For one test sample selected from two test samples of the nitrided steel parts manufactured in the Example and one test sample selected from seven test samples of the nitrided steel parts manufactured in the Comparative Example, the Vickers hardness [Hv] was measured at each position in the cross-sectional depth direction to evaluate the hardness distribution in the cross-sectional depth direction. Figure 7 is a graph showing the hardness distribution in the cross-sectional depth direction of the test sample of the Example and the test sample of the Comparative Example.

[0061] As shown in Fig. 7, in the region where the cross-sectional depth is 800 μm or more, the Vickers hardness of the test sample of the embodiment and the Vickers hardness of the test sample of the comparative example were both approximately the same and did not change. In the region where the cross-sectional depth is 300 μm or more and less than 800 μm, the Vickers hardness of the test sample of the embodiment and the Vickers hardness of the test sample of the comparative example both increased while taking approximately the same value as approaching the surface. In the region where the cross-sectional depth is less than 300 μm, the Vickers hardness of the test sample of the embodiment and the Vickers hardness of the test sample of the comparative example both increased as approaching the surface, but the Vickers hardness of the test sample of the embodiment was higher.

[0062] From these results, it is considered that a nitrided layer is formed in the region with a cross-sectional depth of less than 800 μm in both the test sample of the example and the test sample of the comparative example, whereas a quench-hardened layer is formed in the region with a cross-sectional depth of less than 300 μm in the test sample of the example, and a nitrided hardened layer is formed in the region with a cross-sectional depth of 300 μm or more and less than 800 μm.

[0063] [Evaluation of cross-sectional structure] For one test sample selected from the two test samples of the nitrided steel parts produced in the examples, and one test sample selected from the seven test samples of the nitrided steel parts produced in the comparative examples, the cross-sectional structures of the regions with a cross-sectional depth of less than 300 μm were observed by SEM (Scanning Electron Microscope). Fig. 8 is a photograph of the cross-sectional structures of the regions with a cross-sectional depth of less than 300 μm in the test sample of the example and the test sample of the comparative example observed by SEM. Fig. 9 is a schematic diagram showing the cross-sectional structures of the test sample of the example and the test sample of the comparative example shown in Fig. 8.

[0064] As shown in FIG. 8 and FIG. 9, the cross-sectional structure of the test sample of the comparative example in the region with a cross-sectional depth of less than 300 μm includes a pearlite structure and a ferrite structure. The pearlite structure has a lamellar structure in which ferrite and cementite are alternately arranged. The ferrite structure is composed of ferrite. On the other hand, the cross-sectional structure of the test sample of the embodiment in the region with a cross-sectional depth of less than 300 μm includes a pearlite structure and a martensite structure. The pearlite structure has a lamellar structure in which ferrite and cementite are alternately arranged. Fine carbides are precipitated in the ferrite of the pearlite structure. The martensite structure has a structure in which many fine lath martensites are assembled. In the martensite structure, fine carbides are precipitated mainly at the lath boundaries (boundaries between lath martensites).

[0065] From the observation results of these cross-sectional structures, it is considered that in the region (quench-hardened layer) of the test sample of the embodiment where the cross-sectional depth is less than 300 μm, the pearlite structure of the corresponding region (nitrided layer) of the test sample of the comparative example remains, and an untransformed structure including a lamellar structure is maintained. In addition, it is considered that the martensite structure of the corresponding region of the test sample of the embodiment is the ferrite structure of the corresponding region of the test sample of the comparative example that has been transformed by laser quenching and has fine crystals. Furthermore, it is considered that the fine carbides of the pearlite structure and martensite structure in the corresponding region of the test sample of the embodiment are precipitated by laser quenching.

[0066] [Evaluation by XRD measurement] XRD (X-ray diffraction) measurements were performed on the surface portions of one test sample selected from two test samples of the nitrided steel parts manufactured in the examples, a sample after flash quenching, a sample after a wear test of the sample, and a sample (nitrided steel member) obtained during the manufacture of the selected test sample after nitriding before flash quenching. In addition, XRD measurements were performed on the surface portions of one test sample selected from seven test samples of the nitrided steel parts manufactured in the comparative examples, a sample after nitriding, and a sample after a wear test of the sample. In the XRD measurements, CuKα rays were used as a radiation source to measure the X-ray diffraction pattern, which is the diffraction intensity profile of the diffraction plane of the martensite phase contained in each sample. Then, the half-value width [deg] of the X-ray diffraction peak (156°) of the diffraction plane of the martensite phase of each sample was obtained.

[0067] 10 is a graph showing the half-width of the X-ray diffraction peak of the diffraction plane of the martensite phase of each sample of the embodiment and the comparative example. As shown in FIG. 10, the half-width of the sample after the flash quenching of the embodiment is larger than that of the sample after the nitriding treatment of the comparative example. The half-width of the sample after the wear test of the embodiment is also larger than that of the sample after the wear test of the comparative example. From this, it is estimated that the dislocation density is higher in the region of the test sample of the embodiment where the cross-sectional depth is less than 300 μm compared to the corresponding region of the test sample of the comparative example.

[0068] [Considerations from the evaluation results] From the above evaluation results, it is considered that in the region (quench-hardened layer) of the test sample of the example having a cross-sectional depth of less than 300 μm, the structure is modified by laser quenching, and the hardness and toughness are increased by composite strengthening, precipitation strengthening, fine grain strengthening, and dislocation strengthening. Also, in the region (nitrided hardened layer) of the test sample of the example having a cross-sectional depth of 300 μm or more and less than 800 μm, unlike the region having a cross-sectional depth of less than 300 μm, a ferrite structure exists instead of a martensite structure, and fine carbides do not precipitate, which is considered to be the reason for the low hardness.

[0069] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present invention and that provides similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0070] 1 Steel parts 1S surface 1P surface layer 1C Heart 5. Nitrogen Compound Layer 10 Nitrided steel parts 11 Nitrided steel components 11S surface 11P surface layer 11C heart 12 Nitrided layer 12S surface 14 Hardened layer 16 Nitriding hardened layer

Claims

1. A nitriding steel part including a nitriding steel member having a nitriding layer provided on a surface layer portion, The nitrided layer has a quench-hardened layer in a depth direction from a surface thereof, A nitrided steel part, wherein the quench-hardened layer has a higher hardness than a core portion closer to the center than the surface layer portion of the nitrided steel member.

2. 2. The nitrided steel part according to claim 1, wherein the quench hardened layer has a Vickers hardness of 600 Hv or more.

3. 3. The nitrided steel part according to claim 1, wherein the quench hardened layer contains a pearlite structure, and fine carbides are precipitated in ferrite of the pearlite structure.

4. 3. The nitrided steel part according to claim 1, wherein the quench hardened layer contains a martensite structure, and fine carbides are precipitated in the martensite structure.

5. The nitrided layer further includes a nitrided hardened layer extending in the depth direction from an end of the quench hardened layer on the core side of the nitrided steel member, the nitrided hardened layer has a hardness higher than that of the core of the nitrided steel member, The nitrided steel part according to claim 1 or 2, wherein the quench-hardened layer has a higher hardness than the nitrided hardened layer.

6. 6. The nitrided steel part according to claim 5, wherein the Vickers hardness of the nitrided hardened layer is 400 Hv or more and less than 600 Hv.

7. The nitrided steel part according to claim 1 or 2, wherein the nitrided steel part is a gear or a piston.

8. A method for manufacturing a nitriding steel part according to claim 1 or 2, comprising the steps of: A step of preparing a steel member made of a nitriding steel; a step of subjecting the steel member to a nitriding treatment to convert the steel member into a nitrided steel member having a nitrided layer formed on a surface layer portion; and performing flash quenching on the nitriding steel member to convert the nitrided layer into a layer having the quench-hardened layer in a depth direction from the surface.

9. A method for producing a nitrided steel part according to claim 8, wherein the flash hardening is performed by means of a laser.

10. 9. The method for producing a nitrided steel part according to claim 8, wherein the Vickers hardness of the nitrided layer before the flash quenching is 400 Hv or more and less than 600 Hv, and the Vickers hardness of the quench-hardened layer is 600 Hv or more.

Citation Information

Patent Citations

  • Method of combined heat treatment and quench-hardened steel member

    WO2011013559A1

  • Reprocessed component and method for manufacturing reprocessed component

    WO2022230937A1

Cited By

  • Laser nitriding method for surface of die steel

    CN121023418A