Steel material

A steel material with a tailored chemical composition and controlled oxide inclusions addresses the challenge of achieving high yield strength and fracture toughness in low temperatures, ensuring stability in CO2 storage applications.

JP2024148631APending Publication Date: 2024-10-18NIPPON STEEL CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023061948
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing steel materials used for carbon dioxide storage in depleted oil wells lack both high yield strength and excellent fracture toughness in extremely low temperature environments, particularly at -100°C, as they are not designed to handle the sudden pressure and temperature changes associated with supercritical CO2 storage.

Method used

A steel material with a specific chemical composition and controlled oxide inclusions, including a yield strength of 110 ksi class (758 to 862 MPa) and a reduced number density of coarse Al and Si oxides, specifically 30 pieces/200 mm² and 5 pieces/200 mm² respectively, to enhance fracture toughness in cryogenic conditions.

Benefits of technology

The steel material achieves both high yield strength and excellent fracture toughness in extremely low temperatures, maintaining stability and performance in environments as low as -100°C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148631000001_ABST
    Figure 2024148631000001_ABST
Patent Text Reader

Abstract

To provide a steel material which achieves both yield strength of 110 ksi, and excellent fracture toughness at ultra-low temperature environment of -100°C.SOLUTION: A steel material contains, by mass%, 0.15 to 0.45% of C, 0.05 to 1.00% of Si, 0.05 to 1.00% of Mn, 0.030% or less of P, 0.0050% or less of S, 0.005 to 0.100% of Al, 0.30 to 1.50% of Cr, 0.40 to 2.00% of Mo, 0.002 to 0.020% of Ti, 0.002 to 0.100% of Nb, 0.05 to 0.30% of V, 0.0005 to 0.0040% of B, 0.0100% or less of N, 0.0040% or less of O, and the balance Fe with unavoidable impurities, and has a yield strength of 758 or more and less than 862 MPa, wherein number density of Al oxide having a major axis of 5.0 μm or more is less than 30 pieces / 200 mm2 in the steel material, and the number density of Si oxide having a major axis of 5.0 μm or more is 5 pieces / 200 mm2 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to steel products, and more particularly to steel products used in CO2 storage technology. [Background technology]

[0002] Currently, the rise in carbon dioxide (CO2) concentrations on land has become a global problem. As a result, efforts to curb CO2 emissions are underway. Among these efforts to curb CO2 emissions, CCUS in particular has been attracting attention.

[0003] CCUS is an abbreviation for Carbon dioxide Capture, Utilization and Storage. In other words, CCUS includes three technologies: capture, utilization, and storage of CO2. Of these, a technology that stores CO2 has been attracting attention, which involves capturing CO2 emitted from industrial facilities such as power plants and factories, and injecting the CO2 into depleted oil wells for storage.

[0004] Steel materials used in such CO2 storage technologies are required to have a yield strength of, for example, 110 ksi class (110 to less than 125 ksi, i.e., 758 to less than 862 MPa). To date, steel materials having a yield strength of 110 ksi or more have been proposed in WO 2015 / 190377 (Patent Document 1), WO 2016 / 038809 (Patent Document 2), and WO 2017 / 149572 (Patent Document 3).

[0005] The steel material disclosed in Patent Document 1 is a low-alloy oil well steel pipe having a chemical composition, in mass%, of C: 0.15% or more and less than 0.30%, Si: 0.05 to 1.00%, Mn: 0.05 to 1.00%, P: 0.030% or less, S: 0.0050% or less, Al: 0.005 to 0.100%, O: 0.005% or less, N: 0.007% or less, Cr: 0.10% or more and less than 1.00%, Mo: more than 1.0% and 2.5% or less, V: 0.01 to 0.30%, Ti: 0.002 to 0.009%, Nb: 0 to 0.050%, B: 0 to 0.0050%, Ca: 0 to 0.0050%, and the balance: Fe and impurities, satisfying the formula (Mo / Cr≧2.0). This steel further has a prior austenite grain size number of 7.0 or more according to ASTM E112, and cementite with a circle equivalent diameter of 200 nm or more is present in the matrix of 100 μm. 2 There are more than 50 M2C alloy carbides per μm, and the number density of M2C alloy carbides is 25 / μm 2 and the yield strength is 758 MPa or more. Patent Document 1 discloses that this steel material has a yield strength of 110 ksi (758 MPa) or more and excellent resistance to sulfide stress corrosion cracking.

[0006] The steel material disclosed in Patent Document 2 is a high-strength seamless steel pipe for oil wells, and has a chemical composition, in mass%, of C: 0.20-0.50%, Si: 0.05-0.40%, Mn: 0.3-0.9%, P: 0.015% or less, S: 0.005% or less, Al: 0.005-0.1%, N: 0.008% or less, Cr: 0.6-1.7%, Mo: 0.4-1.0%, V: 0.01-0.30%, Nb: 0.01-0.06%, B: 0.0003-0.0030%, O: 0.0030% or less, and the balance: Fe and unavoidable impurities. This steel material further has a tempered martensite phase of 95% or more by volume, and a structure in which prior austenite grains have a grain size number of 8.5 or more. The ratio of the segregation content to the average content obtained by surface analysis of each element using an electron beam microanalyzer is determined by centering on the 1 / 4t position (t: pipe thickness) from the inner surface of the steel pipe. X M The segregation index Ps(=8.1(X Si +X Mn +X Mo )+1.2XP ) is less than 65 and the yield strength is 758 MPa or more. This steel material has a yield strength of 758 MPa or more and is disclosed in Patent Document 2 as being excellent in resistance to sulfide stress corrosion cracking.

[0007] The steel material disclosed in Patent Document 3 is a low-alloy, high-strength, thick-walled seamless steel pipe for oil wells, and has a chemical composition, in mass%, of C: 0.25 to 0.31%, Si: 0.01 to 0.35%, Mn: 0.55 to 0.70%, P: 0.010% or less, S: 0.001% or less, O: 0.0015% or less, Al: 0.015 to 0.040%, Cu: 0.02 to 0.09%, ... The steel material contains r: 0.8-1.5%, Mo: 0.9-1.6%, V: 0.04-0.10%, Nb: 0.005-0.05%, B: 0.0015-0.0030%, Ti: 0.005-0.020%, N: 0.005% or less, the ratio of the Ti content to the N content (Ti / N) is 3.0-4.0, and the balance is Fe and unavoidable impurities. The steel material further has a cumulative frequency rate of 1% or less of measurement points with a Mo segregation degree of 1.5 or more in the entire thickness of a cross section perpendicular to the longitudinal direction of the pipe, a ratio of the stress at 0.7% strain to the stress at 0.4% strain in a stress-strain curve is 1.02 or less, a wall thickness of 40 mm or more, and a yield strength of 758 MPa or more. Patent Document 3 discloses that this steel material has a yield strength of 758 MPa or more and also exhibits excellent resistance to sulfide stress corrosion cracking. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2015 / 190377 [Patent Document 2] International Publication No. 2016 / 038809 [Patent Document 3] International Publication No. 2017 / 149572 Summary of the Invention [Problem to be solved by the invention]

[0009] Incidentally, when injecting CO2 into a depleted oil well, the CO2 gas may be compressed and pressurized to a supercritical state in order to increase the injection efficiency. On the other hand, if CO2 leaks, the temperature of the CO2 gas that has turned from the supercritical state to gas is rapidly reduced due to a sudden drop in pressure. In this case, the temperature of the environment may fall far below normal, even to -80°C or lower. Therefore, steel materials that are expected to be applied to such carbon dioxide storage technology are required to have not only high strength but also fracture toughness in a cryogenic environment of -80°C or lower, specifically -100°C. On the other hand, the above Patent Documents 1 to 3 do not consider fracture toughness in a cryogenic environment of -100°C.

[0010] An object of the present disclosure is to provide a steel material that combines a 110 ksi-class (758 to less than 862 MPa) yield strength with excellent fracture toughness in a cryogenic environment of -100°C. [Means for solving the problem]

[0011] The steel material according to the present disclosure is In mass%, C: 0.15-0.45%, Si: 0.05 to 1.00%, Mn: 0.05 to 1.00%, P:0.030% or less, S: 0.0050% or less, Al: 0.005 to 0.100%, Cr: 0.30~1.50%, Mo: 0.40-2.00%, Ti: 0.002 to 0.020%, Nb: 0.002 to 0.100%, V: 0.05-0.30%, B: 0.0005~0.0040%, N: 0.0100% or less, O: 0.0040% or less, Cu: 0-0.50%, Ni: 0 to 0.50%, W: 0 to 0.50%, Ca: 0 to 0.0100%, Mg: 0 to 0.0100%, Zr: 0 to 0.0100%, Rare earth elements: 0 to 0.0100%, and the balance being Fe and impurities, The yield strength is less than 758 to 862 MPa, In the steel material, The Al content is 20% or more, the O content is 10% or more, and the number density of Al oxides with a major axis of 5.0 μm or more is 30 / 200 mm 2 is less than In mass%, the Al content is less than 20%, the Si content is 20% or more, the O content is 10% or more, and the number density of silicon oxides having a major axis of 5.0 μm or more is 5 pieces / 200 mm 2 The following is the result. Effect of the Invention

[0012] The steel material according to the present disclosure can achieve both a 110 ksi-class (758 to less than 862 MPa) yield strength and excellent fracture toughness in an extremely low temperature environment of -100°C. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a diagram showing the relationship between the number density (pieces / 200 mm2) of coarse Si oxides (Si oxides with a major axis of 5.0 μm or more) in this example and the CTOD value (mm), which is an index of fracture toughness in a cryogenic environment. [Diagram 2] FIG. 2 is a schematic diagram of a CT test piece used in a CTOD test for evaluating the fracture toughness of a steel material in a cryogenic environment in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] First, the inventors focused on the chemical composition and investigated how to obtain a steel material that combines a 110 ksi-class yield strength with excellent fracture toughness in a cryogenic environment of -100° C. As a result, the inventors found that the composition of the steel material is, by mass%, C: 0.15-0.45%, Si: 0.05-1.00%, Mn: 0.05-1.00%, P: 0.030% or less, S: 0.0050% or less, Al: 0.005-0.100%, Cr: 0.30-1.50%, Mo: 0.40-2.00%, Ti: 0.002-0.020%, Nb: 0.002-0.100%, V: 0.05-0.30%, B: 0.0005-0.0040%. %, N: 0.0100% or less, O: 0.0040% or less, Cu: 0-0.50%, Ni: 0-0.50%, W: 0-0.50%, Ca: 0-0.0100%, Mg: 0-0.0100%, Zr: 0-0.0100%, rare earth elements: 0-0.0100%, and the balance being Fe and impurities, it was thought that a steel material consisting of the following components could potentially achieve both a 110 ksi-class yield strength and excellent fracture toughness in cryogenic environments.

[0015] Next, the inventors of the present invention investigated various methods for improving the fracture toughness in a cryogenic environment for a steel material having the above-mentioned chemical composition and a 110 ksi-class yield strength. Specifically, the inventors of the present invention considered that if coarse oxide-based inclusions could be reduced, it would be possible to improve the fracture toughness in a cryogenic environment while maintaining the yield strength. Here, in a steel material having the above-mentioned chemical composition, Al oxides mainly composed of Al2O3 tend to coarsen. Therefore, the inventors of the present invention first focused on the coarse Al oxides.

[0016] As a result of the investigation by the present inventors, in a steel material having the above-mentioned chemical composition and a yield strength of 110 ksi class, the number density of Al oxide particles having a major axis of 5.0 μm or more is 30 particles / 200 mm 2 It has been revealed that if the particle size is less than 1.0 μm, the fracture toughness can be improved. Here, in this specification, particles having an Al content of 20% or more and an O content of 10% or more, in mass%, are also referred to as "Al oxides". Furthermore, in this specification, Al oxides having a major axis of 5.0 μm or more are also referred to as "coarse Al oxides".

[0017] Here, Al oxides are hard oxides and tend to reduce the toughness of steel materials. In particular, in an extremely low temperature environment of -100°C, the effect of coarse Al oxides is likely to become apparent, and fracture toughness is likely to decrease significantly. Therefore, in the steel material according to this embodiment having the above-mentioned chemical composition and a yield strength of 110 ksi, the number density of coarse Al oxides is set to 30 particles / 200 mm 2 Less than.

[0018] On the other hand, the above-mentioned chemical composition and the yield strength of 110 ksi class, the number density of the coarse Al oxides is 30 pieces / 200 mm 2 In some cases, even if the steel material has a temperature of less than 100°C, it may not be possible to obtain stable and excellent fracture toughness in an extremely low temperature environment of -100°C. Therefore, the inventors have developed a steel material having the above-mentioned chemical composition, a yield strength of 110 ksi, and a number density of coarse Al oxides of 30 / 200 mm 2 As a result of detailed investigations by the inventors, it was found that a steel material having the above-mentioned chemical composition, a yield strength of 110 ksi class, and a number density of coarse Al oxides of 30 particles / 200 mm 2 It has become clear that in steel materials with a temperature below -100°C, if not only the coarse Al oxides in the steel material but also the coarse Si oxides can be reduced, it may be possible to stably obtain excellent fracture toughness even in an extremely low temperature environment of -100°C.

[0019] Herein, in this specification, particles having an Al content of less than 20%, a Si content of 20% or more, and an O content of 10% or more, in mass%, are also referred to as "Si oxides". Furthermore, in this specification, Si oxides having a major axis of 5.0 μm or more are also referred to as "coarse Si oxides". Hereinafter, particles having the above-mentioned chemical composition, a yield strength of 110 ksi class, and a number density of coarse Al oxides of 30 particles / 200 mm 2 The relationship between coarse Si oxides and fracture toughness in a cryogenic environment for steel materials having a melting point of less than 1000 mm will be specifically explained with reference to the drawings.

[0020] FIG. 1 shows the number density (pieces / 200 mm ) of coarse Si oxides (Si oxides with a major axis of 5.0 μm or more) in this example. 21 is a graph showing the relationship between the CTOD value (mm), which is an index of fracture toughness in a cryogenic environment, and the number density of coarse Al oxides of 30 / 200 mm. 2 The number density (pieces / 200 mm ) of coarse Si oxides was determined by the method described below for steel products with a diameter of less than 1 mm. 2 ) and the CTOD value (mm) obtained in a CTOD test carried out at -100°C using the method described below.

[0021] With reference to FIG. 1, a sintered product having the above-mentioned chemical composition and a yield strength of 110 ksi class and a number density of coarse Al oxide particles of 30 particles / 200 mm 2 In steels with a particle density of less than 5 particles / 200 mm 2 If the CTOD value was 0.250 mm or more, the fracture toughness was excellent. Therefore, in this embodiment, the alloy has the above-mentioned chemical composition and a yield strength of 110 ksi, and the number density of the coarse Al oxides is 30 / 200 mm. 2 The number density of coarse Si oxides is set to less than 5 pieces / 200 mm 2 As a result, the steel material according to this embodiment can achieve both a 110 ksi-class yield strength and excellent fracture toughness in an extremely low temperature environment of -100°C.

[0022] The reason why the fracture toughness of steel in a cryogenic environment is improved by reducing the number density of coarse Si oxides is not clear in detail. However, the present inventors speculate as follows. When manufacturing steel having the above-mentioned chemical composition, deoxidation is mainly performed with aluminum (Al) in the steelmaking process. Therefore, in the steel having the above-mentioned chemical composition, Al oxides represented by Al2O3 have been studied, and Si oxides, which are few in number, have not been paid attention. However, in a cryogenic environment of -100°C, not only coarse Al oxides but also coarse Si oxides, which are few in number, may easily cause a decrease in fracture toughness. Therefore, the number density of coarse Al oxides is set to 30 / 200 mm 2Not only to reduce the number density of coarse silicon oxide particles to less than 5 particles / 200 mm 2 The present inventors speculate that by doing the above, it will be possible to stably obtain excellent fracture toughness even in an extremely low temperature environment of -100°C.

[0023] It is possible that the fracture toughness of steel materials in cryogenic environments is increased by a mechanism different from that presumed by the present inventors. However, in the case of steels having the above-mentioned chemical composition and a yield strength of 110 ksi, and a number density of coarse Al oxides of 30 particles / 200 mm 2 In steels with a particle density of less than 5 particles / 200 mm 2 By satisfying the following conditions, excellent fracture toughness in a cryogenic environment can be obtained, as will be demonstrated by the examples described later.

[0024] The gist of the steel material according to this embodiment, which was completed based on the above findings, is as follows.

[0025] [1] A steel material, In mass%, C: 0.15-0.45%, Si: 0.05 to 1.00%, Mn: 0.05 to 1.00%, P: 0.030% or less, S: 0.0050% or less, Al: 0.005 to 0.100%, Cr: 0.30~1.50%, Mo: 0.40-2.00%, Ti: 0.002 to 0.020%, Nb: 0.002 to 0.100%, V: 0.05-0.30%, B: 0.0005~0.0040%, N: 0.0100% or less, O: 0.0040% or less, Cu: 0-0.50%, Ni: 0 to 0.50%, W: 0 to 0.50%, Ca: 0 to 0.0100%, Mg: 0 to 0.0100%, Zr: 0 to 0.0100%, Rare earth elements: 0 to 0.0100%, and the balance being Fe and impurities, The yield strength is less than 758 to 862 MPa, In the steel material, The Al content is 20% or more, the O content is 10% or more, and the number density of Al oxides with a major axis of 5.0 μm or more is 30 / 200 mm 2 is less than In mass%, the Al content is less than 20%, the Si content is 20% or more, the O content is 10% or more, and the number density of silicon oxides having a major axis of 5.0 μm or more is 5 pieces / 200 mm 2 Below is the Steel material.

[0026] [2] The steel material according to [1], Cu: 0.01 to 0.50%, Ni: 0.01 to 0.50%, W: 0.01 to 0.50%, Ca: 0.0001 to 0.0100%, Mg: 0.0001 to 0.0100%, Zr: 0.0001 to 0.0100%, and Rare earth elements: containing one or more elements selected from the group consisting of 0.0001 to 0.0100%; Steel material.

[0027] [3] The steel material according to [1] or [2], The steel material is a seamless steel pipe. Steel material.

[0028] The shape of the steel material according to this embodiment is not particularly limited. The steel material according to this embodiment may be a steel pipe, a round bar (solid material), or a steel plate. The round bar means a steel bar having a circular cross section perpendicular to the axial direction. The steel pipe may be a seamless steel pipe or a welded steel pipe.

[0029] The steel material according to this embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.

[0030] [Chemical composition] The chemical composition of the steel material according to this embodiment contains the following elements.

[0031] C: 0.15-0.45% Carbon (C) improves the hardenability of steel material and increases its strength. Furthermore, C promotes spheroidization of carbides during tempering in the manufacturing process, and increases the fracture toughness of the steel material. If the C content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the C content is too high, even if the contents of other elements are within the range of this embodiment, the amount of carbides becomes too large, and the fracture toughness of the steel material decreases. Therefore, the C content is 0.15 to 0.45%. The preferred lower limit of the C content is 0.18%, more preferably 0.20%, more preferably 0.22%, and more preferably 0.25%. The preferred upper limit of the C content is 0.40%, more preferably 0.38%, and more preferably 0.35%.

[0032] Silicon: 0.05 to 1.00% Silicon (Si) deoxidizes steel. If the Si content is too low, the above effect cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Si content is too high, a large number of coarse Si oxides are generated, and the fracture toughness of the steel material may decrease even if the contents of other elements are within the range of this embodiment. Therefore, the Si content is 0.05 to 1.00%. The preferred lower limit of the Si content is 0.10%, more preferably 0.15%, and more preferably 0.20%. The preferred upper limit of the Si content is 0.85%, more preferably 0.75%, more preferably 0.60%, more preferably 0.50%, and more preferably 0.40%.

[0033] Mn: 0.05 to 1.00% Manganese (Mn) deoxidizes steel. Mn also enhances the hardenability of steel. If the Mn content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mn content is too high, coarse sulfide-based inclusions are generated, and the fracture toughness of the steel is reduced, even if the contents of other elements are within the range of this embodiment. Therefore, the Mn content is 0.05 to 1.00%. The preferred lower limit of the Mn content is 0.06%, more preferably 0.08%, and more preferably 0.10%. The preferred upper limit of the Mn content is 0.90%, more preferably 0.80%, more preferably 0.70%, more preferably 0.60%, and more preferably 0.50%.

[0034] P:0.030% or less Phosphorus (P) is an impurity. That is, the lower limit of the P content is more than 0%. If the P content is too high, even if the contents of other elements are within the range of this embodiment, P will segregate to grain boundaries, and the fracture toughness of the steel material will decrease. Therefore, the P content is 0.030% or less. A preferred upper limit of the P content is 0.025%, more preferably 0.020%, and even more preferably 0.015%. The P content is preferably as low as possible. However, an extreme reduction in the P content significantly increases the manufacturing cost. Therefore, in consideration of industrial production, a preferred lower limit of the P content is 0.001%, more preferably 0.002%, and even more preferably 0.003%.

[0035] S: 0.0050% or less Sulfur (S) is an impurity. That is, the lower limit of the S content is more than 0%. If the S content is too high, even if the contents of other elements are within the range of this embodiment, S will segregate to grain boundaries, and the fracture toughness of the steel material in a cryogenic environment will decrease. Therefore, the S content is 0.0050% or less. A preferred upper limit of the S content is 0.0040%, more preferably 0.0030%, and even more preferably 0.0020%. The S content is preferably as low as possible. However, an extreme reduction in the S content significantly increases the manufacturing cost. Therefore, in consideration of industrial production, a preferred lower limit of the S content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%.

[0036] Al: 0.005 to 0.100% Aluminum (Al) deoxidizes steel. If the Al content is too low, the above effect is not sufficiently obtained even if the contents of other elements are within the range of this embodiment, and the fracture toughness of the steel material is reduced. On the other hand, if the Al content is too high, a large number of coarse Al oxides are generated even if the contents of other elements are within the range of this embodiment, and the fracture toughness of the steel material is reduced. Therefore, the Al content is 0.005 to 0.100%. The preferred lower limit of the Al content is 0.010%, more preferably 0.015%, and more preferably 0.020%. The preferred upper limit of the Al content is 0.080%, more preferably 0.060%, and more preferably 0.040%. The "Al" content in this specification means the content of "acid-soluble Al", that is, "sol.Al".

[0037] Cr: 0.30~1.50% Chromium (Cr) enhances the hardenability of steel. Cr also enhances the temper softening resistance of steel, making high-temperature tempering possible. As a result, the fracture toughness of the steel is enhanced. If the Cr content is too low, the above effects are not sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Cr content is too high, the fracture toughness of the steel is reduced even if the contents of other elements are within the range of this embodiment. Therefore, the Cr content is 0.30 to 1.50%. The preferred lower limit of the Cr content is 0.35%, more preferably 0.40%, and more preferably 0.50%. The preferred upper limit of the Cr content is 1.40%, more preferably 1.30%, more preferably 1.20%, more preferably 1.10%, and more preferably 1.05%.

[0038] Mo: 0.40~2.00% Molybdenum (Mo) enhances the hardenability of steel. Mo also enhances the temper softening resistance of steel, making high-temperature tempering possible. As a result, the fracture toughness of steel is enhanced. If the Mo content is too low, the above effects are not sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Mo content is too high, the above effects are saturated. Therefore, the Mo content is 0.40 to 2.00%. The preferred lower limit of the Mo content is 0.45%, more preferably 0.50%, and even more preferably 0.60%. The preferred upper limit of the Mo content is 1.80%, more preferably 1.60%, more preferably 1.40%, and even more preferably 1.30%.

[0039] Ti: 0.002 to 0.020% Titanium (Ti) combines with N to form nitrides, which refine the grains of the steel material by the pinning effect. As a result, the strength of the steel material is increased. If the Ti content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Ti content is too high, even if the contents of other elements are within the range of this embodiment, the Ti nitrides become coarse, and the fracture toughness of the steel material decreases. Therefore, the Ti content is 0.002 to 0.020%. The preferred lower limit of the Ti content is 0.003%, and more preferably 0.004%. The preferred upper limit of the Ti content is 0.018%, and more preferably 0.015%, and more preferably 0.010%, and more preferably 0.008%.

[0040] Nb: 0.002 to 0.100% Niobium (Nb) combines with C and / or N to form carbides, nitrides, or carbonitrides (hereinafter referred to as "carbonitrides, etc."). Carbonitrides, etc., refine the grains of steel by a pinning effect, and increase the fracture toughness of the steel. Nb also forms fine carbides during tempering to increase the temper softening resistance of the steel, and increase the strength of the steel. If the Nb content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the Nb content is too high, even if the contents of other elements are within the range of this embodiment, excessive carbonitrides, etc. are generated, and the fracture toughness of the steel decreases. Therefore, the Nb content is 0.002 to 0.100%. The preferable lower limit of the Nb content is 0.005%, more preferably 0.010%, more preferably 0.015%, and even more preferably 0.020%. The upper limit of the Nb content is preferably 0.080%, more preferably 0.060%, and further preferably 0.040%.

[0041] V: 0.05~0.30% Vanadium (V) forms carbonitrides and the like. Carbonitrides and the like refine the grains of steel by pinning effect, and increase the fracture toughness of the steel. V also forms fine carbides during tempering, increasing the temper softening resistance of the steel, and increasing the strength of the steel. If the V content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the V content is too high, even if the contents of other elements are within the range of this embodiment, excessive carbonitrides and the like are generated, and the fracture toughness of the steel decreases. Therefore, the V content is 0.05 to 0.30%. The preferred lower limit of the V content is 0.06%, more preferably 0.07%, and more preferably 0.08%. The preferred upper limit of the V content is 0.25%, more preferably 0.20%, and more preferably 0.15%.

[0042] B: 0.0005~0.0040% Boron (B) dissolves in steel to improve the hardenability of the steel material and increase the strength of the steel material. If the B content is too low, the above effects cannot be sufficiently obtained even if the contents of other elements are within the range of this embodiment. On the other hand, if the B content is too high, coarse nitrides are generated and the fracture toughness of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the B content is 0.0005 to 0.0040%. The preferred lower limit of the B content is 0.0006%, and more preferably 0.0008%. The preferred upper limit of the B content is 0.0035%, more preferably 0.0030%, more preferably 0.0025%, and more preferably 0.0020%.

[0043] N: 0.0100% or less Nitrogen (N) is inevitably contained. That is, the lower limit of the N content is more than 0%. N combines with Ti to form nitrides, and the grains of the steel are refined by the pinning effect. As a result, the strength of the steel is increased. However, if the N content is too high, even if the contents of other elements are within the range of this embodiment, coarse nitrides are formed, and the fracture toughness of the steel is reduced. Therefore, the N content is 0.0100% or less. The preferred upper limit of the N content is 0.0080%, more preferably 0.0060%, more preferably 0.0050%, and more preferably 0.0040%. The preferred lower limit of the N content for more effectively obtaining the above effects is 0.0005%, more preferably 0.0010%, more preferably 0.0015%, and more preferably 0.0020%.

[0044] O: 0.0040% or less Oxygen (O) is an impurity. That is, the lower limit of the O content is more than 0%. If the O content is too high, even if the contents of other elements are within the range of this embodiment, coarse oxides are formed, and the fracture toughness of the steel material decreases. Therefore, the O content is 0.0040% or less. A preferred upper limit of the O content is 0.0035%, more preferably 0.0030%, more preferably 0.0025%, and even more preferably 0.0020%. The O content is preferably as low as possible. However, an extreme reduction in the O content significantly increases the manufacturing cost. Therefore, in consideration of industrial production, a preferred lower limit of the O content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%.

[0045] The balance of the chemical composition of the steel material according to the present embodiment is composed of Fe and impurities. Here, the term "impurities" refers to substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the steel material, and that are permissible within a range that does not adversely affect the steel material according to the present embodiment.

[0046] [Optional element] The chemical composition of the steel material described above may further contain one or more elements selected from the group consisting of Cu and Ni in place of a portion of Fe. All of these elements are optional elements and improve the hardenability of the steel material.

[0047] Cu: 0-0.50% Copper (Cu) is an optional element and may not be contained. That is, the Cu content may be 0%. When contained, Cu enhances the hardenability of the steel material and enhances the strength of the steel material. If even a small amount of Cu is contained, the above effect can be obtained to some extent. However, if the Cu content is too high, even if the contents of other elements are within the range of this embodiment, the hardenability of the steel material becomes too high, and the fracture toughness of the steel material decreases. Therefore, the Cu content is 0 to 0.50%. The preferred lower limit of the Cu content is more than 0%, more preferably 0.01%, more preferably 0.02%, and more preferably 0.03%. The preferred upper limit of the Cu content is 0.35%, more preferably 0.25%, more preferably 0.15%, more preferably 0.10%, and more preferably 0.05%.

[0048] Ni: 0 to 0.50% Nickel (Ni) is an optional element and may not be contained. That is, the Ni content may be 0%. When contained, Ni improves the hardenability of the steel material and increases the strength of the steel material. Ni also dissolves in the steel material to increase the fracture toughness of the steel material. Even if even a small amount of Ni is contained, these effects can be obtained to a certain extent. However, if the Ni content is too high, local corrosion is promoted and the fracture toughness of the steel material decreases even if the contents of other elements are within the range of this embodiment. Therefore, the Ni content is 0 to 0.50%. The preferred lower limit of the Ni content is more than 0%, more preferably 0.01%, and more preferably 0.02%. The preferred upper limit of the Ni content is 0.30%, more preferably 0.20%, more preferably 0.10%, and more preferably 0.05%.

[0049] The chemical composition of the above-mentioned steel material may further contain W instead of a portion of Fe.

[0050] W: 0~0.50% Tungsten (W) is an optional element and may not be contained. That is, the W content may be 0%. When W is contained, W forms a protective corrosion film in a sour environment and suppresses the penetration of hydrogen into the steel material. This increases the fracture toughness of the steel material. If even a small amount of W is contained, the above effect can be obtained to a certain extent. However, if the W content is too high, even if the contents of other elements are within the range of this embodiment, coarse carbides are generated in the steel material, and the fracture toughness of the steel material decreases. Therefore, the W content is 0 to 0.50%. The preferred lower limit of the W content is more than 0%, more preferably 0.01%, more preferably 0.03%, and more preferably 0.05%. The preferred upper limit of the W content is less than 0.50%, and more preferably 0.48%.

[0051] The chemical composition of the steel material described above may further contain, instead of a part of Fe, one or more elements selected from the group consisting of Ca, Mg, Zr, and rare earth elements. All of these elements are optional elements, and render S in the steel material harmless as sulfides. As a result, these elements increase the fracture toughness of the steel material.

[0052] Ca: 0 to 0.0100% Calcium (Ca) is an optional element and may not be contained. That is, the Ca content may be 0%. When contained, Ca renders S in the steel harmless as sulfide, and increases the fracture toughness of the steel. If even a small amount of Ca is contained, the above effect can be obtained to some extent. However, if the Ca content is too high, even if the contents of other elements are within the range of this embodiment, the oxides in the steel will coarsen, and the fracture toughness of the steel will decrease. Therefore, the Ca content is 0 to 0.0100%. The preferred lower limit of the Ca content is more than 0%, more preferably 0.0001%, more preferably 0.0003%, and more preferably 0.0006%. The preferred upper limit of the Ca content is 0.0040%, more preferably 0.0025%, and more preferably 0.0020%.

[0053] Magnesium: 0 to 0.0100% Magnesium (Mg) is an optional element and may not be contained. That is, the Mg content may be 0%. When contained, Mg renders S in the steel harmless as sulfide, and increases the fracture toughness of the steel. If even a small amount of Mg is contained, the above effect can be obtained to some extent. However, if the Mg content is too high, even if the contents of other elements are within the range of this embodiment, the oxides in the steel will coarsen, and the fracture toughness of the steel will decrease. Therefore, the Mg content is 0 to 0.0100%. The preferable lower limit of the Mg content is more than 0%, more preferably 0.0001%, more preferably 0.0003%, and more preferably 0.0006%. The preferable upper limit of the Mg content is 0.0040%, more preferably 0.0025%, and more preferably 0.0020%.

[0054] Zr: 0 to 0.0100% Zirconium (Zr) is an optional element and may not be contained. That is, the Zr content may be 0%. When contained, Zr renders S in the steel harmless as sulfide, and increases the fracture toughness of the steel. If even a small amount of Zr is contained, the above effect can be obtained to some extent. However, if the Zr content is too high, even if the contents of other elements are within the range of this embodiment, the oxides in the steel will coarsen, and the fracture toughness of the steel will decrease. Therefore, the Zr content is 0 to 0.0100%. The preferable lower limit of the Zr content is more than 0%, more preferably 0.0001%, more preferably 0.0003%, and more preferably 0.0006%. The preferable upper limit of the Zr content is 0.0040%, more preferably 0.0025%, and more preferably 0.0020%.

[0055] Rare earth elements (REM): 0~0.0100% Rare earth elements (REM) are optional elements and may not be contained. That is, the REM content may be 0%. When contained, REM renders S in the steel harmless as sulfides, and increases the fracture toughness of the steel. REM further binds to P in the steel and suppresses the segregation of P at the grain boundaries. Therefore, the decrease in the fracture toughness of the steel caused by the segregation of P is suppressed. If even a small amount of REM is contained, the above effect can be obtained to some extent even if the contents of other elements are within the range of this embodiment. However, if the REM content is too high, the oxides in the steel become coarse, and the fracture toughness of the steel decreases, even if the contents of other elements are within the range of this embodiment. Therefore, the REM content is 0 to 0.0100%. The preferable lower limit of the REM content is more than 0%, more preferably 0.0001%, more preferably 0.0003%, and even more preferably 0.0006%. The upper limit of the REM content is preferably 0.0040%, more preferably 0.0025%, and even more preferably 0.0020%.

[0056] In this specification, REM refers to one or more elements selected from the group consisting of scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and the lanthanides lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. In addition, in this specification, the REM content refers to the total content of these elements.

[0057] [Yield strength] The yield strength of the steel material according to this embodiment is 758 to less than 862 MPa (110 ksi class, 110 to less than 125 ksi). The yield strength in this specification means the stress at 0.7% total elongation (0.7% total elongation yield strength) obtained in a tensile test at room temperature (25 ° C.) in accordance with ASTM E8 / E8M (2021). The steel material according to this embodiment has the above-mentioned chemical composition and satisfies the number density of coarse Al oxides and the number density of coarse Si oxides described later, so that even if the yield strength is less than 758 to 862 MPa, it has excellent fracture toughness in a cryogenic environment.

[0058] The yield strength of the steel material according to this embodiment is determined by the following method. First, a round bar test piece is prepared from the steel material according to this embodiment. When the steel material is a steel plate, the round bar test piece is prepared from the center of the plate thickness. In this case, the axial direction of the round bar test piece is parallel to the rolling direction of the steel plate. When the steel material is a steel pipe, the round bar test piece is prepared from the center of the wall thickness. In this case, the axial direction of the round bar test piece is parallel to the axial direction of the steel pipe. When the steel material is a round steel bar, the round bar test piece is prepared from the R / 2 position. In this specification, the R / 2 position means the center position of the radius R in a cross section perpendicular to the axial direction of the round steel bar. In this case, the axial direction of the round bar test piece is parallel to the axial direction of the round steel bar. The size of the round bar test piece is, for example, 8.9 mm in parallel part diameter and 35.6 mm in gauge length. Using the prepared round bar test piece, a tensile test is performed at room temperature (25 ° C) in air in accordance with a method conforming to ASTM E8 / E8M (2021), and the obtained stress at 0.7% total elongation (0.7% total elongation yield strength) is defined as the yield strength (MPa). In this embodiment, the yield strength (MPa) is obtained by rounding the obtained value to the first decimal place.

[0059] [Number density of coarse Al oxide particles] The steel material according to the present embodiment has the above-mentioned chemical composition and a yield strength of 110 ksi class, and further has a number density of coarse Al oxides of 30 particles / 200 mm 2 As described above, in this specification, particles having an Al content of 20% or more and an O content of 10% or more, in mass%, are also referred to as "Al oxides". As described above, in this specification, Al oxides having a major axis of 5.0 μm or more are also referred to as "coarse Al oxides". In other words, coarse Al oxides refer to particles having an Al content of 20% or more, an O content of 10% or more, and a major axis of 5.0 μm or more, in mass%.

[0060] As described above, when manufacturing a steel material having the above-mentioned chemical composition, deoxidation is mainly performed with aluminum (Al) in the steelmaking process. Therefore, a large amount of Al oxides is likely to be formed in the steel material having the above-mentioned chemical composition. Furthermore, Al oxides are hard oxides and are likely to reduce the toughness of the steel material. In particular, in an extremely low temperature environment of -100°C, the effect of coarse Al oxides is likely to become apparent, and the fracture toughness is likely to decrease significantly. Therefore, in the steel material according to this embodiment having the above-mentioned chemical composition and a yield strength of 110 ksi class, the number density of coarse Al oxides is set to 30 particles / 200 mm 2 Less than.

[0061] In this embodiment, the preferred upper limit of the number density of the coarse Al oxide particles is 28 particles / 200 mm. 2 and more preferably 25 pieces / 200 mm 2 More preferably, 22 pieces / 200 mm 2 In this embodiment, the lower limit of the number density of the coarse Al oxides is not particularly limited, and is 0 particles / 200 mm 2 The lower limit of the number density of the coarse Al oxides may be, for example, 5 pieces / 200 mm 2 It may be 7 pieces / 200mm 2 Can be 9 pieces / 200mm 2 The method for determining the number density of the coarse Al oxide particles will be described later.

[0062] [Number density of coarse Si oxides] The steel material according to the present embodiment has the above-mentioned chemical composition, a yield strength of 110 ksi, and a number density of coarse Al oxides of 30 particles / 200 mm 2 The density of the coarse Si oxide particles is less than 5 particles / 200 mm. 2 As described above, in this specification, particles having an Al content of less than 20%, a Si content of 20% or more, and an O content of 10% or more, in mass%, are also referred to as "Si oxides". As described above, in this specification, Si oxides having a major axis of 5.0 μm or more are also referred to as "coarse Si oxides". In other words, coarse Si oxides refer to particles having an Al content of less than 20%, a Si content of 20% or more, an O content of 10% or more, and a major axis of 5.0 μm or more, in mass%,.

[0063] As mentioned above, silicon oxides have not received much attention because of their small number. However, in an extremely low temperature environment of -100°C, not only coarse aluminum oxides but also coarse silicon oxides, which are few in number, may easily cause a decrease in fracture toughness. Therefore, we set the number density of coarse aluminum oxides to 30 / 200 mm 2 Not only to reduce the number density of coarse silicon oxide particles to less than 5 particles / 200 mm 2 By setting the temperature at or below 100° C., it is possible to stably obtain excellent fracture toughness even in an extremely low temperature environment of −100° C. Therefore, the steel material according to the present embodiment has the above-mentioned chemical composition and a yield strength of 110 ksi class, and the number density of coarse Al oxides in the steel material is 30 pieces / 200 mm 2 The density of the coarse Si oxide particles is less than 5 particles / 200 mm. 2 The following applies.

[0064] In this embodiment, the preferred upper limit of the density of the coarse Si oxide particles is 4 particles / 200 mm. 2 and more preferably 3 pieces / 200 mm 2 In this embodiment, the lower limit of the number density of the coarse Si oxides is not particularly limited, and is 0 pieces / 200 mm 2The lower limit of the density of the coarse Si oxide particles may be, for example, 1 particle / 200 mm. 2 may be also possible.

[0065] In this embodiment, the number density of coarse Al oxides and the number density of coarse Si oxides in the steel material can be obtained by the following method. First, a test piece is prepared from the steel material according to this embodiment, with the surface including the rolling direction and the rolling down direction as the observation surface. Specifically, when the steel material is a steel plate, a test piece is prepared from the center of the plate thickness, with the surface including the rolling direction and the plate thickness direction as the observation surface. When the steel material is a steel pipe, a test piece is prepared from the center of the plate thickness, with the surface including the pipe axial direction and the pipe radial direction as the observation surface. When the steel material is a round bar, a test piece is prepared with the R / 2 position in the center and the surface including the axial direction and the radial direction as the observation surface.

[0066] The observation surface of the prepared test piece is polished to a mirror finish before measurement. The area of ​​the observation surface is not limited, but for example, 300 mm 2 (20mm x 15mm). The number of Si oxides with a major axis of 5.0μm or more is counted on the observation surface. Specifically, the particles on the observation surface are first identified from the contrast. An element concentration analysis (EDS analysis) is performed on each identified particle. In the EDS analysis, the acceleration voltage is set to 20kV, and the target elements are quantified as N, O, Mg, Al, Si, P, S, Ca, Ti, Cr, Mn, Fe, Cu, Zr, and Nb. If the EDS analysis result of each particle shows that the Al content is 20% or more by mass% and the O content is 10% or more by mass%, the particle is identified as an "Al oxide". If the EDS analysis result of each particle shows that the Al content is less than 20% by mass, the Si content is 20% or more by mass, and the O content is 10% or more by mass, the particle is identified as an "Si oxide".

[0067] Among the Al oxides identified on the observation surface, Al oxides (coarse Al oxides) with a major axis of 5.0 μm or more are identified, and the total number of coarse Al oxides is calculated. Furthermore, among the Si oxides identified on the observation surface, Si oxides (coarse Si oxides) with a major axis of 5.0 μm or more are identified, and the total number of coarse Si oxides is calculated. The major axes of Al oxides and Si oxides can be calculated by known methods. In this specification, the major axis of Al oxides and Si oxides means the longest line segment (μm) among the line segments connecting any two points on the periphery of Al oxides and Si oxides on the observation surface.

[0068] Based on the total number of coarse Al oxides and the total area of ​​the observation surface, the number density of the coarse Al oxides (pieces / 200 mm 2 Furthermore, the number density of the coarse Si oxides (pieces / 200 mm2) was calculated based on the total number of the coarse Si oxides and the total area of ​​the observation surface. 2 In this embodiment, the number density (pieces / 200 mm 2 ), and the number density of coarse Si oxides (pieces / 200 mm 2 ) are all calculated by rounding off the obtained numerical value to the nearest tenth. The number density of the coarse Al oxides and the coarse Si oxides can be measured using a scanning electron microscope equipped with a composition analysis function (SEM-EDS device). For example, an automatic analyzer manufactured by FEI (ASPEX) under the trade name Metals Quality Analyzer can be used as the SEM-EDS device.

[0069] [Fracture toughness] The steel material according to the present embodiment has the above-mentioned chemical composition, a yield strength of 110 ksi, and a number density of coarse Al oxides of 30 particles / 200 mm 2 The density of the coarse Si oxide particles is less than 5 particles / 200 mm. 2As a result, the steel material according to this embodiment has excellent fracture toughness even when the yield strength is less than 758 to 862 MPa and in a cryogenic environment of -100 ° C. In this embodiment, excellent fracture toughness means that the CTOD value obtained by a CTOD test at cryogenic temperatures (-100 ° C.) in accordance with ISO 12135 (2021) described below is 0.250 mm or more.

[0070] Specifically, in this embodiment, the fracture toughness of a steel material is evaluated by the following method. First, a CT (Compact Tension) test piece shown in FIG. 2 is prepared from the steel material according to this embodiment. FIG. 2 is a schematic diagram of a CT test piece used in a CTOD test for evaluating the fracture toughness of a steel material in a cryogenic environment in this embodiment. With reference to FIG. 2, the size of the CT test piece is a thickness B of 25.4 mm, a length L (vertical direction in FIG. 2) of 60.96 mm, and a width W (horizontal direction in FIG. 2) of 50.8 mm. The web thickness Bn of the CT test piece is 22 mm.

[0071] If the steel material is a steel plate, the CT test piece is prepared from the center position of the plate thickness. In this case, the length L direction of the CT test piece is parallel to the rolling direction of the steel plate. If the steel material is a steel pipe, the CT test piece is prepared from the center position of the wall thickness. In this case, the length L direction of the CT test piece is parallel to the axial direction of the steel pipe. If the steel material is a round bar, the CT test piece is prepared from the R / 2 position. In this case, the length L direction of the CT test piece is parallel to the axial direction of the round bar.

[0072] Referring to FIG. 2, the CT test piece has a notch formed in the width W direction at the center position in the length L direction. The notch is formed by machining, and has a width of 3 mm and a depth of 23 mm. A fatigue test is performed on the prepared CT test piece to introduce a pre-crack. In this embodiment, the initial relative crack length a0 / W is set to 0.51. Specifically, the fatigue test is performed at room temperature (25° C.) so that the fatigue pre-crack introduced at the tip of the notch is 3.0 mm.

[0073] The CT test piece in which the fatigue pre-crack is introduced is cooled to -100 ° C. with liquid nitrogen. The cooled CT test piece is subjected to a CTOD test at -100 ° C. in accordance with ISO 12135 (2021). The CTOD value (mm) is obtained based on ISO 12135 (2021) from the load at break in the load-opening amount curve and the plastic component amount of the clip gauge opening displacement obtained by the CTOD test. The same test is performed three times, and the smallest CTOD value (mm) is defined as the CTOD value (mm) of the steel material. In this embodiment, the CTOD value of the steel material is obtained by rounding off the fourth decimal place of the obtained value.

[0074] [Microstructure] The microstructure of the steel material according to this embodiment has a total volume fraction of tempered martensite and tempered bainite of 90% or more. The remainder of the microstructure is, for example, ferrite or pearlite. If the microstructure of the steel material having the above-mentioned chemical composition contains a total volume fraction of tempered martensite and tempered bainite of 90% or more, it can achieve both a 110 ksi-class yield strength and excellent fracture toughness in a cryogenic environment, provided that other configurations of this embodiment are satisfied. That is, in this embodiment, if the steel material has a 110 ksi-class yield strength and excellent fracture toughness in a cryogenic environment, it is determined that the microstructure has a total volume fraction of tempered martensite and tempered bainite of 90% or more.

[0075] When the volume fractions of tempered martensite and tempered bainite are determined by observation, they can be determined by the following method. First, a test piece having an observation surface is prepared from the steel material according to this embodiment. When the steel material is a steel plate, a test piece is prepared from the center of the plate thickness, with a surface including the rolling direction and the plate thickness direction as the observation surface. When the steel material is a steel pipe, a test piece is prepared from the center of the plate thickness, with a surface including the pipe axial direction and the pipe radial direction as the observation surface. When the steel material is a round bar, a test piece is prepared that includes the R / 2 position in the center and has a surface including the axial direction and the radial direction as the observation surface.

[0076] The observation surface of the test piece is polished to a mirror finish, and then immersed in a nital etching solution for about 10 seconds to reveal the structure by etching. The etched observation surface is observed in 10 fields of view using a scanning electron microscope (SEM) in secondary electron images. The field area is, for example, 0.01 mm 2 (magnification 1000x). In each field of view, tempered martensite and tempered bainite are identified from the contrast. The area ratios of the identified tempered martensite and tempered bainite are determined. The method for determining the area ratios is not particularly limited, and any known method may be used. For example, the area ratios of tempered martensite and tempered bainite can be determined by image analysis. In this embodiment, the arithmetic average value of the area ratios of tempered martensite and tempered bainite determined in all fields of view is defined as the volume ratios of tempered martensite and tempered bainite.

[0077] [Manufacturing method] A method for manufacturing a steel material according to this embodiment will be described below. A method for manufacturing a seamless steel pipe will be described below as an example of a steel material according to this embodiment. The method for manufacturing a seamless steel pipe includes a process for preparing a material (steelmaking process), a process for hot working the material to manufacture a mother pipe (hot working process), and a process for quenching and tempering the mother pipe to produce a seamless steel pipe (quenching process and tempering process). Note that the manufacturing method according to this embodiment is not limited to the manufacturing method described below. Each process will be described in detail below.

[0078] [Steel manufacturing process] In the steelmaking process, first, molten pig iron produced by a known method is refined in a converter (primary refining). The molten steel produced by the primary refining is then subjected to secondary refining. In the secondary refining, alloy elements are added to adjust the composition, and molten steel satisfying the above-mentioned chemical composition is produced.

[0079] In the secondary refining, for example, a Ruhrstahl-Hausen (RH) vacuum degassing treatment is performed. Then, the alloy components are finally adjusted. In the secondary refining, a composite refining may be performed. In this case, a refining treatment using, for example, a Ladle Furnace (LF) or a Vacuum Arc Degassing (VAD) is performed before the RH vacuum degassing treatment.

[0080] A material is manufactured using the molten steel that has been subjected to secondary refinement. Specifically, a cast piece (slab, bloom, or billet) is manufactured by continuous casting using the molten steel that has been subjected to secondary refinement. In the continuous casting method, first, the molten steel is poured from a ladle into a tundish. At this time, packing sand is usually enclosed in the nozzle of the ladle to seal the nozzle. Therefore, packing sand may be mixed with the molten steel from the ladle into the tundish. Also, when manufacturing a material having the above-mentioned chemical composition, silicon oxide may be used as packing sand. In this case, there is a concern that silicon oxide may be introduced into the manufactured material.

[0081] Therefore, in this embodiment, in order to prevent the Si oxide sealed in the nozzle of the ladle from being introduced into the tundish, the molten steel and the Si oxide are separated. The method of separating the Si oxide is not particularly limited, but the following method can be used, for example. A metal plate with an inclination is placed below the nozzle of the ladle and above the opening of the tundish. When the nozzle of the ladle is opened, the Si oxide is discharged from the nozzle first, and then the molten steel is discharged. Here, the Si oxide is lighter than the molten steel. Therefore, the Si oxide discharged from the nozzle is guided to the outside of the opening of the tundish along the inclination of the metal plate. The inclination of the metal plate may be provided, for example, by disposing a metal plate processed into a cone shape without a bottom surface so that the apex is located directly below the nozzle of the ladle, or may be provided by other methods. In addition, one metal plate may be used, or multiple metal plates may be used in a stacked manner. Furthermore, the thickness of the metal plate is not particularly limited, but is, for example, about 1 to 10 mm.

[0082] After the Si oxide is discharged from the nozzle, the molten steel is discharged. At this time, the molten steel discharged from the nozzle is introduced into the tundish through the opening together with the metal plate. That is, in this embodiment, a part or all of the metal plate may be introduced into the tundish and mixed into the molten steel. Therefore, the metal plate in this embodiment is preferably a metal plate made of alloy elements contained in the molten steel. As the metal plate made of alloy elements contained in the molten steel, for example, an aluminum plate can be used. In this specification, the aluminum plate means a metal plate made of aluminum and the balance of impurities.

[0083] Preferably, after the Si oxide is discharged from the nozzle, the metal plate is removed from below the nozzle before the molten steel is discharged. In this case, it is possible to prevent the Si oxide attached to the metal plate from being mixed into the molten steel. The method for removing the metal plate from below the nozzle is not particularly limited, but for example, a hole may be formed in a part of the metal plate, and the metal plate may be removed using a rod with a hook at its tip. In this case, the hook at the tip of the rod can be hooked into the hole in the metal plate and the rod can be pulled to remove the metal plate. By the above method, the Si oxide can be separated from the molten steel and the molten steel can be introduced into the tundish. The method for separating the Si oxide from the molten steel is not limited to the above method.

[0084] Next, the prepared molten steel is cast to produce a material. The casting method is not particularly limited, but may be, for example, a continuous casting method. When producing a material by a continuous casting method, it is preferable to carry out the following method.

[0085] The casting speed in the continuous casting machine is preferably 1.0 to 3.0 m / min. If the casting speed is too slow, an accumulation zone of Al oxides may be formed in the material. In this case, the produced steel material contains a large amount of coarse Al oxides, and the fracture toughness in a cryogenic environment is reduced. On the other hand, if the casting speed is too fast, the Al oxides may not float up, and a large amount of Al oxides may remain in the material. In this case, the produced steel material contains a large amount of coarse Al oxides, and the fracture toughness in a cryogenic environment is reduced. Therefore, the casting speed in the continuous casting machine is preferably 1.0 to 3.0 m / min.

[0086] When the material is manufactured by the continuous casting method, it is preferable to further electromagnetically stir the molten steel in the mold. Specifically, by performing the electromagnetic stirring in the mold with a current value of 330 to 450A, it becomes difficult for an accumulation zone of Al oxide to be formed in the material. If the current value of the electromagnetic stirring in the mold is too low, the stirring of the molten steel is insufficient, and an accumulation zone of Al oxide may be formed in the material. In this case, a large number of coarse Al oxides are contained in the manufactured steel material, and the fracture toughness in a cryogenic environment decreases. On the other hand, if the current value of the electromagnetic stirring in the mold is too high, the manufacturing equipment may be overloaded. Therefore, in this embodiment, it is preferable to set the current value of the electromagnetic stirring in the mold to 330 to 450A. By the above method, the molten steel is cast to manufacture the material.

[0087] [Hot processing process] In the hot working process, the prepared material is hot worked to produce an intermediate steel material. When the steel material is a seamless steel pipe, the intermediate steel material corresponds to a mother pipe. First, the billet is heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The billet extracted from the heating furnace is hot worked to produce a mother pipe (seamless steel pipe). The method of hot working is not particularly limited, and may be a well-known method.

[0088] For example, the Mannesmann process may be carried out as the hot working to produce a mother pipe. In this case, a round billet is pierced and rolled using a piercing machine. When piercing and rolling is performed, the piercing ratio is not particularly limited, but is, for example, 1.0 to 4.0. The pierced and rolled round billet is further hot rolled using a mandrel mill, a reducer, a sizing mill, or the like to produce a mother pipe. The cumulative reduction in area in the hot working process is, for example, 20 to 70%.

[0089] Other hot working methods may be used to produce a mother pipe from the billet. For example, in the case of a short, thick-walled steel material such as a coupling, the mother pipe may be produced by forging using the Erhardt method or the like. The mother pipe is produced by the above steps. The thickness of the mother pipe is not particularly limited, but is, for example, 9 to 60 mm.

[0090] When the steel material is round steel, the material is first heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300°C. The material extracted from the heating furnace is subjected to hot processing to produce an intermediate steel material having a circular cross section perpendicular to the axial direction. The hot processing is, for example, blooming rolling by a blooming mill, or hot rolling by a continuous rolling mill. In the continuous rolling mill, a horizontal stand having a pair of grooved rolls arranged side by side in the vertical direction and a vertical stand having a pair of grooved rolls arranged side by side in the horizontal direction are alternately arranged.

[0091] When the steel material is a steel plate, the material is first heated in a heating furnace. The heating temperature is not particularly limited, but is, for example, 1100 to 1300° C. The material removed from the heating furnace is subjected to hot rolling using a blooming mill and a continuous rolling mill to produce an intermediate steel material in the shape of a steel plate.

[0092] The mother pipe produced by hot working may be air-cooled (as-rolled). The mother pipe produced by hot working may be quenched directly after the hot working without being cooled to room temperature, or may be quenched after being reheated after the hot working.

[0093] When quenching is performed directly after hot working, or after reheating, cooling may be stopped or slow cooling may be performed during quenching. In this case, it is possible to prevent quench cracks from occurring in the mother pipe. When quenching is performed directly after hot working, or after reheating, stress relief annealing (SR) may be performed after quenching and before the next heat treatment. In this case, residual stress in the mother pipe is removed.

[0094] As described above, in the hot working process, the prepared material is hot worked to produce an intermediate steel material. The quenching process will be described in detail below.

[0095] [Quenching process] In the quenching process, quenching is performed on the prepared intermediate steel material (blank pipe). In this specification, "quenching" means rapidly cooling the intermediate steel material at the A3 point or higher. The preferred quenching temperature is 800 to 1000°C. If the quenching temperature is too high, the prior γ grains may become coarse, and the fracture toughness of the steel material may decrease. Therefore, the quenching temperature is preferably 800 to 1000°C.

[0096] In this specification, the quenching temperature corresponds to the surface temperature of the intermediate steel material measured by a thermometer installed at the outlet side of the device performing the final hot working when quenching is performed directly after hot working. Furthermore, the quenching temperature corresponds to the temperature of the furnace where quenching or reheating is performed when quenching is performed after reheating or reheating after hot working.

[0097] The quenching method is, for example, to continuously cool the intermediate steel material (mother pipe) from the quenching start temperature to continuously lower the surface temperature of the mother pipe. The method of continuous cooling is not particularly limited and may be a well-known method. For example, the method of continuous cooling is a method of immersing the mother pipe in a water tank for cooling, or a method of accelerating cooling the mother pipe by shower water cooling or mist cooling.

[0098] If the cooling rate during quenching is too slow, the microstructure will not be mainly martensite and bainite, and the mechanical properties (yield strength of 110 ksi) specified in this embodiment will not be obtained. In this case, furthermore, excellent fracture toughness will not be obtained.

[0099] Therefore, as described above, in the steel manufacturing method according to the present embodiment, the intermediate steel is quenched during quenching. Specifically, in the quenching step, the average cooling rate in the range of the surface temperature of the intermediate steel (blank pipe) during quenching from 800 to 500°C is defined as the quenching cooling rate CR. 800-500 More specifically, the cooling rate during quenching, CR 800-500 is determined from the temperature measured at the slowest cooling location in the cross section of the intermediate steel being quenched (e.g., the center of the intermediate steel thickness when both surfaces are forced cooled).

[0100] Preferred cooling rate during quenching: CR 800-500 The cooling rate during quenching is preferably 300°C / min or more. 800-500 The lower limit of the cooling rate during quenching is 450° C. / min, and more preferably 600° C. / min. 800-500 The upper limit is not particularly specified, but is, for example, 60,000° C. / min.

[0101] Preferably, the mother tube is heated in the austenite region multiple times and then quenched. In this case, the austenite grains before quenching are refined, thereby increasing the fracture toughness of the steel material. By performing quenching multiple times, heating in the austenite region may be repeated multiple times, or by performing normalizing and quenching, heating in the austenite region may be repeated multiple times. Furthermore, quenching and tempering, which will be described later, may be combined and performed multiple times. That is, quenching and tempering may be performed multiple times. In this case, the fracture toughness of the steel material is further increased. The tempering process will be described in detail below.

[0102] [Tempering process] In the tempering process, the above-mentioned quenched blank pipe is tempered. In this specification, "tempering" refers to the process of tempering the intermediate steel material after quenching to Ac1 The term "tempering temperature" refers to the temperature of a furnace in which the intermediate steel material is heated and held after quenching at a temperature lower than the tempering temperature. The term "tempering time" refers to the time from when the temperature of the intermediate steel material reaches a predetermined tempering temperature until it is extracted from the heat treatment furnace.

[0103] The tempering temperature is appropriately adjusted according to the chemical composition of the seamless steel pipe and the yield strength to be obtained. That is, the tempering temperature is adjusted for a mother pipe having the chemical composition of this embodiment to adjust the yield strength of the seamless steel pipe to 110 ksi class (758 to less than 862 MPa). It is naturally possible for a person skilled in the art to adjust the yield strength of the seamless steel pipe to 110 ksi class by adjusting the tempering temperature. Specifically, in the tempering process according to this embodiment, the preferred tempering temperature is 690 to 730°C.

[0104] If the tempering time is too short, a microstructure mainly composed of tempered martensite and tempered bainite may not be obtained. On the other hand, if the tempering time is too long, the above effects are saturated. Therefore, in the tempering step of this embodiment, the tempering time is preferably 10 to 90 minutes. A more preferable lower limit of the tempering time is 15 minutes. A more preferable upper limit of the tempering time is 80 minutes.

[0105] The steel material according to this embodiment can be manufactured by the above manufacturing method. In the above manufacturing method, a method for manufacturing a seamless steel pipe has been described as one example. However, the steel material according to this embodiment may be a steel plate or other shape. Similar to the above manufacturing method, the manufacturing method for steel plate or other shape also includes, for example, a preparation step, a quenching step, and a tempering step. Furthermore, the above manufacturing method is one example, and the steel material may be manufactured by other manufacturing methods.

[0106] The present invention will now be described in more detail with reference to examples. EXAMPLES

[0107] Molten steels having the chemical compositions shown in Tables 1-1 and 1-2 were produced. In Table 1-2, "-" means that the content of each element is at the impurity level. Specifically, the Cu content, Ni content, and W content of Steel A were rounded off to two decimal places and were 0%. Furthermore, the Ca content, Mg content, Zr content, and rare earth element (REM) content of Steel A were rounded off to five decimal places and were 0%.

[0108] [Table 1-1]

[0109] [Table 1-2]

[0110] Using the above molten steel, a round billet was produced by a continuous casting method. In the continuous casting method, when molten steel was introduced from a ladle to a tundish, a metal plate processed into a bottomless cone shape was placed above the opening of the tundish so that its apex was located directly below the nozzle of the ladle. Table 2 shows whether or not a metal plate of the above shape was placed above the opening of the tundish. Specifically, when a metal plate of the above shape was placed above the opening of the tundish, "A" is indicated in the "Metal Plate" column of Table 2. When a metal plate of the above shape was not placed above the opening of the tundish, "B" is indicated in the "Metal Plate" column of Table 2. The metal plate of the above shape placed above the opening of the tundish was an aluminum plate. Specifically, three aluminum plates with a thickness of 2 mm were used in a stack. When a metal plate was placed, after the Si oxide was discharged from the nozzle and before the molten steel was discharged, the metal plate was removed from below the nozzle using a rod with a hook formed at its tip. Furthermore, the molten steel was cast into a round billet at the casting speed shown in Table 2. At this time, electromagnetic stirring was performed in the mold at the current value shown in Table 2.

[0111] [Table 2]

[0112] The manufactured round billet of each test number was held at 1250°C for 1 hour, and then hot rolling was performed using the Mannesmann-mandrel method to manufacture a blank pipe (seamless steel pipe) of each test number. Furthermore, the obtained blank pipe of each test number was quenched. Specifically, the blank pipe of each test number was held at the temperature (°C) for the time (minutes) specified in the "Quenching process" column in Table 2, and then quenched by shower water cooling. Note that for each test number, the cooling rate during quenching, CR 800-500 The quenching rates were all within the range of 480 to 30,000°C / min. The quenching temperatures (°C) shown in Table 2 were the temperatures (°C) of the heat treatment furnace in which the mother tube was heated. Furthermore, the quenching times (min) shown in Table 2 were the times (min) the mother tube was held at the quenching temperature.

[0113] The obtained mother pipes of each test number were tempered. Specifically, the mother pipes of each test number were tempered by holding them at the temperature (°C) for the time (minutes) listed in the "Tempering process" column in Table 2. Here, the tempering temperature (°C) listed in Table 2 is the temperature (°C) of the tempering furnace in which the mother pipes were heated. Furthermore, the tempering time (minutes) listed in Table 2 is the time (minutes) during which the mother pipes were held at the tempering temperature. Through the above manufacturing process, seamless steel pipes of each test number were obtained.

[0114] [Evaluation test] The seamless steel pipes having the respective test numbers after tempering were subjected to a tensile test, a test for measuring the number density of coarse Al oxides and coarse Si oxides, and a CTOD test, which will be described below.

[0115] [Tensile test] A tensile test was performed on the seamless steel pipe of each test number to determine the yield strength. The tensile test was performed in accordance with ASTM E8 / E8M (2021). A round bar test piece with a parallel part diameter of 8.9 mm and a gauge length of 35.6 mm was prepared from the center of the wall thickness of the seamless steel pipe of each test number. The axial direction of the round bar test piece was parallel to the pipe axial direction of the seamless steel pipe. Using the prepared round bar test piece, a tensile test was performed at room temperature (25 ° C.) in air to obtain the yield strength (MPa) of the seamless steel pipe of each test number. In this embodiment, the stress at 0.7% total elongation obtained in the tensile test (0.7% total elongation yield strength) was defined as the yield strength. The obtained yield strength (MPa) is shown in Table 3 as "YS (MPa)".

[0116] [Table 3]

[0117] [Measurement of the number and density of coarse Al oxides and coarse Si oxides] A number density measurement test of coarse Al oxides and coarse Si oxides was carried out on the seamless steel pipes of each test number to determine the number density of Al oxides with a major axis of 5.0 μm or more (coarse Al oxides) and Si oxides with a major axis of 5.0 μm or more (coarse Si oxides). The number density of coarse Al oxides and coarse Si oxides was determined by the above-mentioned method using test pieces prepared from the center of the wall thickness of the seamless steel pipes of each test number. The number density of the obtained coarse Al oxides (particles / 200 mm 2 ) in Table 3, "Coarse Al oxide (pieces / 200 mm 2 The number density (pieces / 200 mm) of the obtained coarse Si oxides is shown in the " 2 ) in Table 3, "Large Si oxide (pieces / 200 mm 2 ) column.

[0118] [CTOD test] A CTOD test was performed on the seamless steel pipe of each test number to obtain the CTOD value in a cryogenic environment of -100 ° C. Specifically, a CTOD test was performed using a CT test piece prepared from the center of the wall thickness of the seamless steel pipe of each test number by the above-mentioned method. The CTOD value (mm) was obtained based on ISO 12135 (2021) from the load at break in the load-opening amount curve obtained by the CTOD test and the plastic component amount of the clip gauge opening displacement. In this example, the load application rate in the CTOD test was 20.94 kN / min, and the Young's modulus was 212000 MPa. The same test was performed three times, and the minimum CTOD value (mm) was defined as the CTOD value (mm) of the seamless steel pipe. The obtained CTOD value (mm) is shown in the "CTOD value (mm)" column of Table 3.

[0119] [Evaluation Results] With reference to Tables 1-1, 1-2, 2, and 3, the seamless steel pipes of test numbers 1 to 12 had appropriate chemical compositions, and the manufacturing methods also satisfied the above-mentioned preferable conditions. As a result, these seamless steel pipes had a yield strength of 758 to less than 862 MPa and a number density of coarse Al oxides of 30 particles / 200 mm 2 The density of the coarse Si oxide particles is less than 5 particles / 200 mm. 2 As a result, the seamless steel pipes had a CTOD value of 0.250 mm or more in the CTOD test carried out at -100°C. That is, the seamless steel pipes of test numbers 1 to 12 had a yield strength of 758 to less than 862 MPa and excellent fracture toughness in an extremely low temperature environment of -100°C. It was determined that the total volume fraction of tempered martensite and tempered bainite in the microstructure of these seamless steel pipes was 90% or more.

[0120] On the other hand, the seamless steel pipes of test numbers 13 and 14 were cast at too high a speed in the steelmaking process. As a result, the number density of coarse Al oxides in these seamless steel pipes was 30 pieces / 200 mm 2As a result, in the CTOD test carried out at -100℃, these seamless steel pipes had a CTOD value of less than 0.250 mm, and did not have excellent fracture toughness in the cryogenic environment of -100℃.

[0121] For the seamless steel pipes of test numbers 15 to 17, no metal plate was used in the steelmaking process. As a result, the number density of coarse Si oxides in these seamless steel pipes was 5 pieces / 200 mm 2 As a result, in the CTOD test carried out at -100℃, these seamless steel pipes had a CTOD value of less than 0.250 mm, and did not have excellent fracture toughness in the cryogenic environment of -100℃.

[0122] The seamless steel pipe of test number 18 had an excessively high O content. As a result, the seamless steel pipe had a CTOD value of less than 0.250 mm in the CTOD test carried out at -100°C, and did not have excellent fracture toughness in the cryogenic environment of -100°C.

[0123] The seamless steel pipe of test number 19 had a too low Mo content. As a result, the seamless steel pipe had a CTOD value of less than 0.250 mm in the CTOD test carried out at -100°C, and did not have excellent fracture toughness in the cryogenic environment of -100°C.

[0124] The seamless steel pipe of test number 20 had an excessively high S content. As a result, the seamless steel pipe had a CTOD value of less than 0.250 mm in the CTOD test carried out at -100°C, and did not have excellent fracture toughness in the cryogenic environment of -100°C.

[0125] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.

Claims

1. A steel material, In mass percent, C: 0.15-0.45%, Si: 0.05-1.00%, Mn: 0.05-1.00%, P: 0.030% or less, S: 0.0050% or less, Al: 0.005-0.100%, Cr: 0.30-1.50%, Mo: 0.40-2.00%, Ti: 0.002 to 0.020%, Nb: 0.002 to 0.100%, V: 0.05-0.30%, B: 0.0005-0.0040%, N: 0.0100% or less, O: 0.0040% or less, Cu: 0 to 0.50%, Ni: 0 to 0.50%, W: 0-0.50%, Ca: 0-0.0100%, Mg: 0 to 0.0100%, Zr: 0 to 0.0100%, Rare earth elements: 0 to 0.0100%, and The balance is Fe and impurities, The yield strength is less than 758 to 862 MPa; In the steel material, The Al content is 20% or more, the O content is 10% or more, and the number density of Al oxides having a major axis of 5.0 μm or more is 30 / 200 mm 2 is less than In the case where the Al content is less than 20%, the Si content is 20% or more, the O content is 10% or more, and the number density of Si oxides having a major axis of 5.0 μm or more is 5 pieces / 200 mm 2 Below is the Steel material.

2. The steel material according to claim 1, Cu: 0.01 to 0.50%, Ni: 0.01-0.50%, W: 0.01-0.50%, Ca: 0.0001-0.0100%, Mg: 0.0001 to 0.0100%, Zr: 0.0001 to 0.0100%, and Rare earth elements: containing one or more elements selected from the group consisting of 0.0001 to 0.0100%; Steel material.

3. The steel material according to claim 1 or 2, The steel material is a seamless steel pipe. Steel material.

Citation Information

Patent Citations

  • Low alloy steel pipe for oil well

    WO2015190377A1

  • High strength seamless steel pipe for use in oil wells and manufacturing method thereof

    WO2016038809A1

  • Low-alloy, high-strength thick-walled seamless steel pipe for oil well

    WO2017149572A1