Resin-ceramic direct joining method, resin-ceramic joined body, and resin-ceramic member

Laser-induced surface modification on ceramics forms oxide particle aggregates for strong bonding with resins, addressing bonding challenges and enabling efficient, durable ceramic-resin joints.

JP2024148648APending Publication Date: 2024-10-18HIROTEC CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023061974
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing methods for bonding ceramics and resins face challenges due to differences in electronic and physical properties, leading to weak bonding interfaces, limited applicability of adhesives, and complex processing requirements, especially when precise bonding and high strength are needed.

Method used

A method involving laser irradiation in an oxidizing atmosphere to form a surface-modified region on ceramics, followed by contact with a resin material and external heating to create a strong bond, utilizing oxide particle aggregates for enhanced bonding without adhesives.

Benefits of technology

This method enables high-strength, homogeneous, and efficient bonding of ceramics and resins, suitable for various shapes and sizes, with improved durability and reliability, suitable for applications like roof and outer wall members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148648000001_ABST
    Figure 2024148648000001_ABST
Patent Text Reader

Abstract

To provide a method for directly joining a ceramic material and a resin material, that is a simple method for directly joining ceramic material and resin material without using an adhesive, that is applicable regardless of a size and a shape of the materials to be joined, does not include a wet process, and can mass-produce homogeneous, high-strength joints with high efficiency, and also to provide a ceramic-resin joined body in which the ceramic material and the resin material are firmly and directly joined, and a roof member and an exterior wall member having the ceramic-resin joined body.SOLUTION: A ceramic-resin direct joining method for directly joining a ceramic material and a resin material includes: a first step of irradiating a surface of the ceramic material with a laser in an oxidizing atmosphere to form a surface modified area; a second step of contacting the surface modified area with the resin material to form a joined interface; and a third step of heating the joined interface by external heating means to achieve joining.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for joining a resin material and a ceramic material, a resin-ceramic joined body obtained by the joining method, and a resin-ceramic member having the resin-ceramic joined body; more specifically, the present invention relates to a method for directly and firmly joining a resin material and a ceramic material without using an adhesive, mechanical fastening, or the like, a resin-ceramic joined body obtained by the joining method, and a resin-ceramic member having the resin-ceramic joined body. [Background technology]

[0002] In recent years, multi-material structures in which different materials are placed in the right places have been attracting attention, and joining technologies for joining different materials are being actively studied. However, since ceramics and resins, among the different materials, have significantly different electronic bonds and physical properties, it is not possible to form a good joining interface, and joining is generally achieved by the physical or chemical adsorption forces of adhesives.

[0003] However, when using adhesives, the adhesive spreads and is not suitable for precise bonding, which limits the bonding area, and there are problems in that the bonding strength is greatly affected by the state of the bonded surfaces (surface roughness, etc.). Furthermore, there are problems such as the time required for the adhesive to harden limiting productivity, and the difficulty of maintaining and managing the state of the adhesive. In addition, the strength and reliability of the bonding interface depend on the properties of the adhesive, and it is not possible to obtain a bonded body that fully utilizes the properties of ceramics and resins.

[0004] In contrast, for example, Patent Document 1 (JP 2021-195419 A) discloses a bonded body having a functional group-bearing adherend surface (A) having one or more functional groups selected from the group consisting of amino groups, epoxy groups, mercapto groups, styryl groups, (meth)acryloyl groups, isocyanato groups, and alkenyl groups on the surface of the adherend, and a functional group-bearing resin surface (B) having one or more functional groups selected from the group consisting of amino groups, epoxy groups, mercapto groups, styryl groups, (meth)acryloyl groups, isocyanato groups, and alkenyl groups on the surface of the resin, wherein at least one of the functional group-bearing adherend surface (A) and the functional group-bearing resin surface (B) has a mixture of two-dimensional monomolecular structures and three-dimensional multimolecular structures, and the adherend is at least one of glass and ceramics.

[0005] In the bonded body described in Patent Document 1, the functional groups on the directly bonded adherend surface (A) and resin surface (B) bond with each other through at least one of chemical bonds, hydrogen bonds, and van der Waals forces. Therefore, it is said that the adherend (glass and / or ceramics) and resin can be bonded with sufficient bonding strength without using conventional adhesives.

[0006] In addition, Patent Document 2 (JP 2022-14112 A) discloses a bonded body having a rubber surface having one or more functional groups selected from the group consisting of amino groups, epoxy groups, mercapto groups, styryl groups, (meth)acryloyl groups, isocyanato groups, and alkenyl groups, and a functional group-attached surface B having one or more functional groups selected from the group consisting of amino groups, epoxy groups, mercapto groups, styryl groups, (meth)acryloyl groups, isocyanato groups, and alkenyl groups, which is directly bonded to the surface of at least one adherend selected from the group consisting of metals, glass, ceramics, resins, and rubber, and a two-dimensional monomolecular structure and a three-dimensional multimolecular structure are mixed on at least one of the functional group-attached rubber surface A and the functional group-attached surface B.

[0007] In the bonded body described in Patent Document 2, chemical bonds between functional groups, hydrogen bonds, and bonds due to van der Waals forces are generated at the bonded surface formed by directly bonding the functional group-bearing rubber surface A and the functional group-bearing adherend surface B. It is said that these bonding forces enable the rubber to be bonded with at least one adherend selected from the group consisting of metal, glass, ceramic, resin, and rubber with sufficient bonding strength without using an adhesive. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2021-195419 A [Patent Document 2] Patent Publication No. 2022-14112 Summary of the Invention [Problem to be solved by the invention]

[0009] However, in the bonded body described in Patent Document 1, it is essential that both the adherend surface (A) and the resin surface (B) have specific functional groups, which limits the types of bonded materials that can be used. In addition, in order to impart specific functional groups, it may be necessary to perform a functional group imparting treatment by immersion or spray coating, which makes the bonding process complicated. In addition, in order to achieve bonding, it is said that the distance between the functional group on the adherend surface (A) and the functional group on the resin surface (B) needs to be within about 0.3 nm, which requires precise control of the bonding process.

[0010] In addition, in the joined body described in Patent Document 2, one of the joined materials is limited to rubber, and it is essential that both the rubber surface A and the adherend surface B have specific functional groups on their surfaces, so that, similar to the case of Patent Document 1, the applicable joined materials are limited and the joining process is complicated. Furthermore, in order to achieve joining, it is necessary to bring the functional groups on the rubber surface and the functional groups on the ceramic or other surface within 3 angstroms, and precise control of the joining process is required.

[0011] In view of the problems in the conventional techniques as described above, an object of the present invention is to provide a method for directly joining ceramic materials and resin materials, which is a simple method for directly joining ceramic materials and resin materials without using an adhesive, which is applicable regardless of the size and shape of the materials to be joined, does not include a wet process, and can mass-produce homogeneous and high-strength joints with high efficiency. Another object of the present invention is to provide a ceramic-resin joined body in which a ceramic material and a resin material are directly and firmly joined, and a roof member and an exterior wall member having the ceramic-resin joined body. [Means for solving the problem]

[0012] In order to achieve the above-mentioned object, the inventors conducted extensive research into methods for joining thermoplastic resin materials and metal materials, and discovered that it is effective to form an appropriate surface-modified area on the surface of a ceramic material by irradiating a laser, thereby arriving at the present invention.

[0013] That is, the present invention provides: A method for directly bonding a ceramic material and a resin material, comprising the steps of: A first step of irradiating a surface of the ceramic material with a laser in an oxidizing atmosphere to form a surface modified region; a second step of contacting the resin material with the surface modified region to form a bonded interface; and a third step of heating the interface to be joined by an external heating means to achieve joining. The present invention provides a method for directly bonding ceramics to resin, comprising the steps of:

[0014] The greatest feature of the ceramic resin direct bonding method of the present invention is that a surface modified region is formed at the interface of the ceramic material to be bonded by using laser irradiation in an oxidizing atmosphere. Although the ceramic material is basically stable, a surface state suitable for direct bonding with the resin material can be obtained by irradiating the ceramic material with a high energy density laser under appropriate conditions. More specifically, the contaminants (mainly C) adsorbed on the surface of the ceramic material can be removed, and the interface to be bonded can be cleaned. Here, the ceramic material is not particularly limited as long as it does not impair the effects of the present invention, and can be various non-oxide ceramics, oxide ceramics, and composite materials containing these.

[0015] In the ceramic resin direct bonding method of the present invention, it is preferable to form an oxide particle aggregate in the surface modified region. The oxide particle aggregate is made of oxide particles containing at least one of the elements constituting the ceramic material, and a large number of fine oxide particles are aggregated together to cover the surface of the ceramic material. Here, the degree of aggregation is not particularly limited as long as it does not impair the effects of the present invention, and the oxide particles may be in a state of being necked together as sintering progresses due to heat input during laser irradiation. The particle size of the oxide particles is preferably 1 to 1000 nm, more preferably 1 to 500 nm, and most preferably 1 to 200 nm.

[0016] Although the reason why the formation of oxide particle aggregates made of fine oxide particles can firmly bond ceramic materials and resin materials is not entirely clear, it is believed that the oxide particle aggregates can obtain a lower state energy at the bonded interface with the resin material, compared to ceramic materials that are extremely stable chemically and have poor bondability (binding ability). As a result, it is believed that a good bonded interface can be formed even in cases where untreated ceramic materials and resin materials cannot be bonded.

[0017] In addition, in the ceramic resin direct bonding method of the present invention, it is preferable to use a pulsed laser as the laser in the first step. By using a pulsed laser, it is possible to appropriately control the local heating and cooling of the ceramic material surface, and it is possible to easily and efficiently form an oxide particle aggregate consisting of fine oxide particles on the nanometer order. It is preferable that the irradiation energy of one pulse of the pulsed laser is 0.2 to 1.0 mJ. By setting the irradiation energy of one pulse of the pulsed laser to 0.2 to 1.0 mJ, it is possible to suitably obtain an oxide particle aggregate consisting of oxide particles having a particle size of 1 to 1000 nm on the surface of the ceramic material. In addition, when the ceramic has a white color, for example, and the energy absorption rate by the laser irradiation is low, it is preferable to overlap the laser irradiation multiple times.

[0018] In the ceramic resin direct bonding method of the present invention, the resin material is preferably a fluororesin material. The C-F bond of the fluororesin material is strong, and it is a typical resin material that is difficult to bond because it is chemically stable like ceramic materials. However, a strong bonded interface can be obtained by forming a bonded interface through an oxide particle aggregate. The mechanism by which a strong bonded interface is formed is not necessarily clear, but it is thought that fine oxide particles on the nanometer order have a catalytic effect and dissociate the C-F bond.

[0019] Furthermore, in the ceramic resin direct bonding method of the present invention, it is preferable that a bonding pressure is applied to the bonded interface in the third step. By applying the bonding pressure, the surface modified region (oxide particle aggregate) and the resin material can be closely attached to each other, and a strong bond can be obtained. In addition, even if bubbles are formed in the bonded portion due to the temperature rise, the bubbles can be discharged outside the system.

[0020] In addition, when the resin material is a fluororesin, it is preferable to apply a pressure of 2 MPa or more to the interface to be joined in the third step. By applying a pressure of 2 MPa or more to the interface to be joined in the third step, the fluororesin material and the surface modified region can be reliably adhered to each other. On the other hand, when the resin material is a thermoplastic resin other than a fluororesin, it is preferable to apply a pressure of more than 0 and 0.8 MPa or less to the interface to be joined in the third step. By applying pressure to the interface to be joined in the third step, the adhesion between the ceramic material and the thermoplastic resin material is improved, the formation of defects can be suppressed, and the bonding strength of the bonding interface can be improved. On the other hand, by applying a pressure of 0.8 MPa or less, it is possible to suppress the formation of a skin layer and a bulk layer of the thermoplastic resin in the vicinity of the bonding interface, and the progression of fracture from between the skin layer and the bulk layer can be suppressed.

[0021] More specifically, since the strength of the resin main chain of general thermoplastic resins such as polypropylene (PP) and polyacetal (POM) is not very high, the shape change caused by the expansion and contraction of the thermoplastic resin during heat bonding causes the bond between the skin layer and the bulk of the thermoplastic resin to break, making it difficult to maintain the bond.In contrast, a good bond can be formed by applying an appropriate bonding pressure (pressure of 0.8 MPa or less) that does not cause internal destruction of the thermoplastic resin.

[0022] The external heating means in the third step is not particularly limited as long as it does not impair the effects of the present invention, and various external heating means known in the art can be used, but it is preferable to use, for example, laser irradiation or a heating stage. When the ceramic material is colored, the temperature of the interface to be joined can be easily and efficiently increased by laser irradiation. In addition, when the ceramic material is white, for example, and the energy absorption rate by laser irradiation is low, the ceramic material can be placed on a heating stage to control the temperature of the interface to be joined.

[0023] The present invention also provides a ceramic-resin joined body in which a ceramic material and a resin material are directly joined, the ceramic material and the resin material being integrated together at the joint via an oxide layer.

[0024] Here, the ceramic material is not particularly limited as long as it does not impair the effects of the present invention, and may be various non-oxide ceramics, oxide ceramics, and composite materials containing these. The oxide layer is formed by irradiating the surface of the ceramic material with a laser, and contains at least one of the elements that constitute the ceramic material. In addition, when the ceramic material is an oxide ceramic, the oxide layer has a structure and / or a microstructure different from the surface of the oxide ceramic itself.

[0025] In the ceramic resin bonded body of the present invention, the oxide layer is preferably made of an oxide particle aggregate. The oxide particle aggregate is a large number of fine oxide particles aggregated together to cover the surface of the ceramic material. The degree of aggregation is not particularly limited as long as it does not impair the effects of the present invention, and the oxide particles may be in a necked state as a result of sintering proceeding due to heat input during laser irradiation. The particle size of the oxide particles is preferably 1 to 1000 nm, more preferably 1 to 500 nm, and most preferably 1 to 200 nm.

[0026] In the ceramic-resin bonded body of the present invention, the resin material is preferably a fluororesin material. Although a fluororesin material is a typical resin material that is difficult to bond, it is chemically stable and has excellent properties such as heat resistance, slipperiness, non-adhesiveness, chemical resistance, low friction, and insulation. On the other hand, a ceramic material is also chemically stable and has excellent mechanical properties, heat resistance, and chemical resistance, and by combining a fluororesin material and a ceramic material in an appropriate place, it can be more suitably used in many fields such as food, chemistry, semiconductors, liquid crystals, physicochemical equipment, and transportation.

[0027] As the resin material, thermoplastic resins other than fluororesins can also be suitably used. As the thermoplastic resin other than fluororesins, any of general-purpose plastics, engineering plastics, and super engineering plastics is preferably used. The type of thermoplastic resin material is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known thermoplastic resin materials can be used. By using the ceramic-resin direct bonding method of the present invention, a good bonded body in which these resin materials and ceramic materials are directly bonded can be obtained.

[0028] In addition, in the ceramic-resin bonded body of the present invention, it is preferable that the base material of the resin material is fractured in a 90° peel test based on JIS-Z0237. It is extremely difficult to impart high strength to a bonded interface where a ceramic material and a resin material, which have poor bondability, are directly bonded, but in the ceramic-resin bonded body of the present invention, the ceramic material and the resin material are firmly bonded via an oxide layer, so that the base material of the resin material is fractured in a 90° peel test based on JIS-Z0237, and the bonded body can be suitably used for applications requiring high strength and long-term reliability.

[0029] The present invention further provides a ceramic resin member, which comprises the ceramic resin joined body of the present invention and is used as a roof member or an exterior wall member.

[0030] The ceramic-resin bonded body of the present invention has a ceramic material and a resin material firmly bonded via an oxide layer, and does not have an adhesive layer or the like that has poor environmental resistance, and therefore has high strength and long-term reliability, and can be suitably used as a roofing member or an exterior wall member. In particular, by using a ceramic-resin bonded body formed by bonding a fluororesin material and a ceramic material and arranging the fluororesin material on the outside, adhesion of dirt can be suppressed and cleaning work can be simplified. In addition, by using a fluororesin material on the outside of the roofing member, snow accumulation can be suppressed, and snow removal work can be omitted in areas with heavy snowfall. Effect of the Invention

[0031] According to the present invention, it is possible to provide a method for directly joining ceramics and resin, which is a simple method for directly joining ceramics and resin without using an adhesive, is applicable regardless of the size and shape of the materials to be joined, does not include a wet process, and can mass-produce homogeneous and high-strength joints with high efficiency. Also, according to the present invention, it is possible to provide a ceramic-resin joined body in which a ceramic material and a resin material are firmly and directly joined, and a roof member and an exterior wall member having the ceramic-resin joined body. [Brief description of the drawings]

[0032] [Figure 1] 1 is a process diagram of a ceramic resin direct bonding method according to the present invention. [Diagram 2] 5A to 5C are schematic diagrams showing an example of patterning by laser irradiation in a first step. [Diagram 3] 1 is a schematic cross-sectional view showing an example of a joint obtained by the ceramic-resin direct bonding method of the present invention. [Figure 4] 1 is a schematic cross-sectional view showing an example of a ceramic-resin bonding member of the present invention. [Diagram 5] 1 is a SEM photograph of a surface modified region obtained in Example 1 with a laser irradiation interval of 60 μm. [Figure 6] 1 shows the results of a wide scan of a silicon nitride plate before surface modification in Example 1. [Figure 7] 1 shows the results of a wide scan of the surface modified region in Example 1. [Figure 8] FIG. 2 is a schematic diagram showing a joining state in Example 1. [Figure 9] 1 is a photograph showing the appearance of a ceramic-resin bonded body (laser irradiation interval: 60 μm) obtained in Example 1. [Figure 10] 3 is a photograph showing the state during a 90° peel test in Example 1. [Figure 11] 4 is a graph showing the test force at break of each ceramic-resin bonded body in Example 1. [Figure 12]13 is a graph showing the test force at break of each ceramic-resin bonded body in Example 2. [Figure 13] 13 is a graph showing the test force at break of each ceramic-resin joined body in Example 3. [Figure 14] 1 is a photograph showing the appearance of a ceramic-resin bonded body obtained at 3 MPa in Example 3 after a 90° peel test. [Figure 15] 13 is a graph showing the test force at break of a ceramic-resin bonded body before and after a temperature cycle test in Example 4. [Figure 16] 11 is a photograph showing a state of a three-point bending test in Example 4. [Figure 17] 13 is a photograph showing the appearance of a ceramic-resin bonded body after a three-point bending test in Example 4. [Figure 18] 1 is a SEM photograph of the surface-modified region obtained in Example 5. [Figure 19] 13 is a photograph showing the appearance of a pressure bonding device used in Example 5. [Figure 20] FIG. 13 is a schematic diagram showing a state during joining in Example 5. [Figure 21] 1 is a photograph showing the appearance of a ceramic-resin bonded body obtained in Example 5. [Figure 22] FIG. 13 is a test force-displacement diagram during a 90° peel test in Example 5. [Figure 23] FIG. 13 is a test force-displacement diagram in a 90° peel test of the ceramic-resin bonded body in Example 5 before and after the temperature cycle test. [Figure 24] 13 is a wide scan result of an alumina plate before surface modification in Example 5. [Diagram 25] 1 shows the result of a narrow scan of an alumina plate before surface modification in Example 5. [Figure 26] 13 is a wide scan result of the alumina plate after surface modification in Example 5. [Figure 27] 1 shows the narrow scan results of the alumina plate after surface modification in Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] Representative embodiments of the ceramic-resin direct bonding method, ceramic-resin bonded body, and ceramic-resin member of the present invention will be described in detail below with reference to the drawings, but the present invention is not limited to these. In the following description, the same or corresponding parts are given the same reference numerals, and duplicated descriptions may be omitted. In addition, since the drawings are intended to conceptually explain the present invention, the dimensions of each component shown and their ratios may differ from the actual ones.

[0034] 1. Direct ceramic-resin bonding method 1 is a process diagram of the ceramic resin direct bonding method of the present invention. The ceramic resin direct bonding method of the present invention includes a first step (S01) of forming a surface modified region on a ceramic material, a second step (S02) of forming a bonding interface, and a third step (S03) of raising the temperature of the bonding interface to achieve bonding. Each step will be described in detail below.

[0035] (1-1) First step (S01: Surface modified region formation step) The first step (S01) is a step for obtaining a surface-modified region that contributes to the formation of a strong bonded interface. The first step (S01) can remove contaminants (mainly C) adsorbed on the surface of the ceramic material, and clean the bonded interface. In addition, it is preferable to form an oxide particle aggregate in the surface-modified region. The oxide particle aggregate is a large number of fine oxide particles that are aggregated together and cover the surface of the ceramic material. Here, the degree of aggregation is not particularly limited as long as it does not impair the effects of the present invention, and sintering (bonding between oxide particles) progresses due to the heat input during laser irradiation, and the oxide particles may be in a state of being necked together. The particle size of the oxide particles is preferably 1 to 1000 nm, more preferably 1 to 500 nm, and most preferably 1 to 200 nm.

[0036] Although the reason why the formation of an oxide particle aggregate made of fine oxide particles can firmly bond a ceramic material to a resin material is not entirely clear, the oxide particle aggregate can obtain a lower state energy at the bonded interface with the resin material, compared to a ceramic material that is extremely stable chemically and has poor bondability (binding ability). As a result, even in cases where untreated ceramic material and resin material cannot be bonded, a good bonded interface can be formed.

[0037] In the first step (S01), specifically, a pulsed laser is irradiated onto the surface of the ceramic material in an oxidizing atmosphere. The laser used in the first step is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known lasers can be used, for example, a semiconductor laser can be preferably used.

[0038] The irradiation energy of one pulse of the pulsed laser is preferably 0.2 to 1.0 mJ. By setting the irradiation energy of one pulse of the pulsed laser to 0.2 to 1.0 mJ, it is possible to form oxide particle aggregates (oxide particle clusters) in which oxide particles having particle sizes of 5 to 500 nm are continuously bonded in the irradiated region.

[0039] Furthermore, the type of oxidizing atmosphere is not particularly limited as long as it does not impair the effects of the present invention, and it is sufficient that the atmosphere is one in which oxide particle aggregates are formed on the surface of the ceramic material by irradiation with a pulsed laser, for example, the treatment may be performed in air.

[0040] The surface-modified region may be formed on the interface of the ceramic material to be joined, and it is preferable that the surface-modified region occupies 20% or more of the area of ​​the interface to be joined. By making the surface-modified region occupy 20% or more of the area of ​​the interface to be joined, high joint strength and reliability can be ensured for the entire joint. The surface-modified region may be formed in a planar shape, or may be formed into an appropriate pattern such as a line shape.

[0041] It is also preferable to pattern the laser irradiation so that at least a portion of the irradiated areas of the pulsed laser (beam diameter of the pulsed laser on the surface of the ceramic material) overlaps. An example of patterning of the laser irradiation is shown in FIG. 2. (a) to (c) in FIG. 2 are preferable patterning, and (d) is an inappropriate patterning in which the irradiated areas do not overlap. By performing the laser treatment so that at least a portion of the irradiated areas overlap, a high bonded interface strength can be obtained.

[0042] (1-2) Second process (S02: bonded interface formation process) The second step (S02) is a step for forming a joining interface by bringing the ceramic material having the surface modified region formed in the first step (S01) into contact with a resin material.

[0043] Here, the ceramic material and the resin material may be in a general overlapping state with their flat surfaces abutting against each other, or, for example, the end face of the ceramic material may be abutted against the surface of the resin material to form a so-called T-shaped joint.

[0044] In addition, when a ceramic material and a resin material are to be joined in a lap joint, a heat-resistant glass plate or the like can be placed on the surface of one or both of the materials to be joined to fully restrain them, thereby making it possible to bring the materials into closer contact with each other and suppressing the displacement of the interface to be joined during laser irradiation. It is preferable to use heat-resistant glass with excellent laser transparency.

[0045] When a fluororesin is used as the material to be joined, the fluororesin is not particularly limited as long as it does not impair the effects of the present invention, and any conventionally known fluororesin can be used. Examples of the fluororesin include polytetrafluoroethylene (PTFE, melting point: 327°C), polychlorotrifluoroethylene (PCTFE, melting point: 220°C), polyvinylidene fluoride (PVDF, melting point: 151 to 178°C), polyvinyl fluoride (PVF, melting point: 203°C), tetrafluoroethylene-hexafluoropropylene copolymer (FEP, melting point: 250 to 275°C), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA, melting point: 302 to 310°C), Examples of suitable materials include tetrafluoroethylene-ethylene copolymer (ETFE, melting point: 218 to 270°C), tetrafluoroethylene-perfluorodioxole copolymer (TFE / PDD), and chlorotrifluoroethylene-ethylene copolymer (ECTFE, melting point: 245°C). However, since the direct ceramic-resin bonding method of the present invention can obtain a bonded joint with excellent high-temperature strength without using an adhesive, it is preferable to use polytetrafluoroethylene (PTFE, melting point: 327°C), which has a high melting point.

[0046] In addition, when a thermoplastic resin other than fluororesin is used as the material to be joined, the thermoplastic resin is not particularly limited as long as it does not impair the effects of the present invention, and conventionally known general-purpose plastics, engineering plastics, and super engineering plastics can be suitably used. More specifically, for example, polyethylene (PE), polypropylene (PP), polystyrene (PS), polyacetal (POM), polyvinyl chloride (PVC), polyethylene terephthalate (PET), ABS resin (ABS), polyamide (PA), polycarbonate (PC), PET (Polyethylene Terephthalate), and various carbon fiber reinforced plastics (CFRP) and glass fiber reinforced plastics (GFRP), etc. can be used.

[0047] The ceramic material used as the joined material is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known ceramic materials can be used, including non-oxide ceramics, oxide ceramics, and composite materials containing these. The oxide layer is formed by irradiating the surface of the ceramic material with a laser, and contains at least one of the elements that constitute the ceramic material. In addition, when the ceramic material is an oxide ceramic, the oxide layer has a structure and / or a microstructure different from the surface of the oxide ceramic.

[0048] (1-3) Third process (S03: heating process) The third step (S03) is a step of increasing the temperature of the interface to be joined formed in the second step (S02) by an external heating means to achieve joining.

[0049] When laser irradiation is used as the external heating means, it is preferable to irradiate the resin material with a pulsed laser from the resin material side when the resin material is transparent, and to irradiate the ceramic material side when the resin material is opaque. By irradiating the resin material with a pulsed laser from the resin material side when the resin material is transparent, and by irradiating the resin material with a pulsed laser from the ceramic material side when the resin material is opaque, the temperature of the interface to be joined can be efficiently increased. In addition, by irradiating the ceramic material with a laser from the ceramic material side, the resin material can be used as the joined material regardless of the type. Furthermore, by heating from the ceramic material side, a space can be provided on the resin material side, and pressure can be applied from the surface of the resin material as necessary. Here, the laser used in the third step (S03) is not limited to a pulsed laser, and various conventionally known lasers can be used.

[0050] In the third step (S03), when a fluororesin is used as the resin material, it is preferable to apply a pressure of 2 MPa or more to the interface to be joined. By applying a pressure of 2 MPa or more to the interface to be joined, the fluororesin material and the ceramic material (oxide particle aggregate) can be bonded closely to each other, and a strong bond can be obtained. In addition, even if bubbles are formed in the bond as the temperature rises, the bubbles can be discharged outside the system.

[0051] The bonded portion obtained by the ceramic-resin direct bonding method of the present invention has a sufficiently high strength, but the variation in quality can be reduced by adding a pressurizing step. The pressurizing, for example, causes the softened fluororesin material to extend beyond the range of the heat-affected zone of the ceramic material, thereby expanding the bonding interface between the ceramic material and the fluororesin material.

[0052] In addition, when a thermoplastic resin other than fluororesin is used as the resin material, it is preferable that the temperature (T) of the interface to be joined in the third step (S03) satisfies the relational expression (1): melting point (°C) of the thermoplastic resin material ≦ T ≦ thermal decomposition temperature of the thermoplastic resin material. By setting the temperature (T) of the interface to be joined to the melting point (°C) of the thermoplastic resin material or higher, the surface modification region formed on the surface of the ceramic material and the thermoplastic resin material are well adhered to each other, and dissociation of CH bonds and the like of the thermoplastic resin material is promoted by the oxide particle aggregates, so that a strong joint can be efficiently obtained. On the other hand, by setting the temperature (T) of the interface to be joined to the thermal decomposition temperature of the thermoplastic resin material or lower, it is possible to suppress a decrease in the strength of the thermoplastic resin material due to excessive heat input. Here, the temperature (T) of the interface to be joined can be measured, for example, by attaching a K-type thermocouple to the center of the interface to be joined on the ceramic side.

[0053] In addition, when a thermoplastic resin other than fluororesin is used as the resin material, it is preferable to apply a pressure of more than 0 and 0.8 MPa or less to the bonded interface in the third step (S03). By applying pressure to the bonded interface, the adhesion between the ceramic material and the thermoplastic resin material is improved, the formation of defects is suppressed, and the bond strength of the bonded interface can be improved. On the other hand, by applying a pressure of 0.8 MPa or less, the formation of a skin layer and a bulk layer of the thermoplastic resin in the vicinity of the bonded interface can be suppressed, and the progression of breakage from between the skin layer and the bulk layer can be suppressed. Here, the pressure applied to the bonded interface can be measured, for example, by placing a heat-resistant pressure-sensitive sheet on the bonded portion.

[0054] The bonded portion obtained by the ceramic resin direct bonding method of the present invention has a sufficiently high strength, but the variation in quality can be reduced by adding a pressurizing step. The pressurizing step can expand the bonded interface between the ceramic material and the resin material, for example, by softening the resin material and expanding it beyond the range of the heat-affected zone of the ceramic material.

[0055] When applying pressure to the interface to be joined, in the second step (S02), a heat-resistant glass plate or the like is brought into contact with the surface of one or both of the materials to be joined to completely restrain the surface, thereby making it easier to press the interface to be joined.

[0056] Moreover, the third step (S03) is preferably performed in a state where the interfaces to be joined of the ceramic material and the resin material are in close contact with each other, and the close contact state is preferably maintained after the third step (S03) until the temperature of the interface becomes 80% or less of the melting point (°C) of the resin material. In order to make the interfaces to be joined in close contact during the joining process, it is preferable to restrain the positions of the ceramic material and the resin material using an appropriate jig in the third step (S03). However, if the temperature of the interface is equal to or higher than the melting point of the resin material or close to the melting point, the state of the interface is unstable, and if the restraint is removed in this state, sufficient joining strength cannot be obtained. In contrast, by maintaining the restraint until the temperature of the interface becomes 80% or less of the melting point (°C) of the resin material, a stable high-strength joint interface can be obtained.

[0057] In addition, the process parameters of the external heating means in the third step (S03) (when laser irradiation is used, the laser output, scanning speed, focal length, etc.) may be appropriately selected depending on the type and size of the materials to be joined, the area of ​​the interface to be joined, and the mechanical properties required of the joint, etc.

[0058] 2. Ceramic-resin joint 3 is a schematic cross-sectional view showing an example of a joint obtained by the ceramic-resin direct bonding method of the present invention. The ceramic-resin bonded body 2 is a laminated bonded member of a resin material 4 and a ceramic material 6, and the resin material 4 and the ceramic material 6 are directly bonded via a thin oxide layer (not shown). The ceramic-resin bonded body 2 is formed by directly bonding the resin material 4 and the ceramic material 6, and no adhesive, rivets, etc. are used at the bonded portion (bonded interface) 8. The ceramic-resin bonded body 2 can be suitably manufactured by the above-mentioned ceramic-resin direct bonding method of the present invention.

[0059] In the ceramic-resin bonded body 2, the resin material 4 and the ceramic material 6 are firmly bonded together. For example, when the resin material 4 is a fluororesin, when the resin material 4 and the ceramic material 6 are forcibly peeled away from each other, the fluororesin material elongated into a fibrous form can be observed at the bonded interface by TEM observation or high-magnification SEM observation. Furthermore, when a shear tensile test is performed on the ceramic-resin bonded body 2, it shows excellent tensile properties to the extent that the resin material 4 elongates. Furthermore, when a 90-degree peel test based on JIS-Z0237 is performed, the base material of the resin material 4 breaks.

[0060] It is preferable to conduct the tensile test based on ISO19095, the international standard for evaluation test methods for resin-metal bonding properties. In a typical tensile test, the resin part, which is weaker than the bonded part, breaks first, making it difficult to quantify the bonding properties. However, with ISO19095, by optimizing the test piece shape and using auxiliary tools, it is possible to prevent the resin part from breaking, and therefore to measure the strength of the bonded interface.

[0061] Furthermore, when the resin material 4 is a fluororesin, the C-F bonds of the fluororesin material at the bonding interface are changed to bonds such as COO, CO, and C=O. As a result, for example, when the above-mentioned fluororesin material stretched into a fibrous form is subjected to elemental analysis, the amount of F detected is extremely small compared to C and O.

[0062] 3. Ceramic resin bonding materials The ceramic-resin bonded member of the present invention is used as a roof member or an exterior wall member, and is most characterized in that it has the ceramic-resin bonded body of the present invention. Fig. 4 is a schematic cross-sectional view showing an example of the ceramic-resin bonded member of the present invention.

[0063] In the ceramic resin joint member 10, the ceramic material 6 and the resin material 4 are firmly joined via a thin oxide layer (not shown) and there is no adhesive layer or the like that has poor environmental resistance, so that it has high strength and long-term reliability and can be suitably used as a roofing material or an exterior wall material. In particular, by using a fluororesin as the resin material 4 and arranging the fluororesin material on the outside, adhesion of dirt is suppressed and cleaning work can be simplified. In addition, by using a fluororesin material on the outside of the roofing material, snow accumulation is suppressed, and snow removal work in areas with heavy snowfall can be omitted.

[0064] Representative embodiments of the present invention have been described above, but the present invention is not limited to these, and various design modifications are possible, all of which are included in the technical scope of the present invention. EXAMPLES

[0065] Example 1: Bonding of non-oxide ceramics and resin (examination of surface modification conditions) Using the ceramic-resin direct bonding method of the present invention, a non-oxide ceramic material was directly bonded to a fluororesin material. The non-oxide ceramic material was a silicon nitride (Si3N4) plate with a thickness of 3 mm, width of 30 mm, and length of 80 mm, and the fluororesin material was a tetrafluoroethylene-ethylene copolymer (ETFE) sheet with a thickness of 100 μm.

[0066] The silicon nitride plate was irradiated with laser in the atmosphere to form a surface modified region (first step). A 50W nanosecond pulse laser (YLPN-1-100-50-50) manufactured by IPG was used as the laser, and the laser irradiation conditions were average output: 50W (energy of 1 pulse: 1mj), focus diameter: 59μm, and scanning speed: 15000588.5μm / s. The laser irradiation intervals were 30μm, 42μm, 60μm, 75μm, and 90μm, and a surface modified region was formed over the entire area of ​​the bonded interface. Here, the irradiation intervals of 30μm, 42μm, 60μm, and 75μm correspond to the states (a), (b), (c), and (d) in Figure 2, respectively.

[0067] Figure 5 shows an SEM photograph of the surface modified region obtained with a laser irradiation interval of 60 μm. A JSM-7200F manufactured by JEOL Ltd. was used for the SEM observation. Figure 5 shows that oxide particle aggregates, which are the aggregates of oxide particles having a particle size of about 1 to 50 nm, were formed in the surface modified region. Here, similar oxide particle aggregates were observed in all surface modified regions, regardless of the laser irradiation interval.

[0068] XPS analysis was performed on the surface of the silicon nitride plate before and after surface modification. For the XPS analysis, a PHI Quantera SXM was used, and the excitation X-rays were monochromatic AlKα 1,2 The X-ray energy was 1486.6 eV, the X-ray diameter was 200 μm, and the photoelectron detection angle was 45°. Data was processed by 9-point smoothing, and the horizontal axis was adjusted to 284.6 eV for the C1s main peak. In addition, XPS analysis was performed on a sample in which the SiOH group had been modified with a fluorine-based silane treatment agent, and it was assumed that all the fluorine detected from the modified sample was derived from the reaction with SiOH. 2p Peak area and F 1s The SiOH group was quantitatively evaluated from the peak area.

[0069] The results of the wide scan before surface modification and the wide scan of the surface modified area are shown in Figures 6 and 7, respectively. Table 1 shows the elemental composition obtained for the silicon nitride substrate surface before surface modification and the surface modified area obtained with a laser irradiation interval of 60 μm.

[0070] [Table 1]

[0071] Compared to the untreated surface, the surface-modified region has more oxygen and silicon, and less carbon and nitrogen. Furthermore, the sodium, magnesium, potassium, calcium, etc., found on the untreated surface were below the lower detection limit of XPS (0.1 to 0.3 atomic %) in the surface-modified region. These results show that carbon is effectively removed from the surface of the silicon nitride plate by laser irradiation.

[0072] Regarding the chemical state, carbon is CH x The main component was N-Si, and components attributable to CO (ether, hydroxyl group), CN, C=O (carbonyl group), COO (ester, carboxyl group, carboxylate, etc.) were also observed. Regarding the chemical state of nitrogen, before surface modification, components attributable to N-Si and organic nitrogen such as ON-Si or amine / amide were observed. On the other hand, the main component of nitrogen observed in the surface modified area was N-Si. Regarding the chemical state of silicon, before surface modification, N-Si, SiON, SiO x On the other hand, the silicon detected in the surface modified region is attributed to SiO2 (including Si-OH).

[0073] The ratio of SiOH groups to the total silicon (SiOH / Si) is shown in Table 2. Measurements were taken at two locations both before and after the surface modification treatment. The SiOH / Si value was higher in the surface modified area than before the treatment, indicating that silanol groups were generated by the surface modification.

[0074] [Table 2]

[0075] Next, the silicon nitride plate and the fluororesin sheet with the surface modified regions formed at each laser irradiation interval were stacked as shown in Fig. 8 (second step), pressed with a glass roller to bring the bonding interfaces into close contact with each other, and the silicon nitride plate side was irradiated with a laser to obtain a ceramic resin bonded body (third step). In the third step, a 4kW semiconductor laser (LDF-4000-40) manufactured by Laserline was used, and a two-axis zoom homogenizer was used in the optical system to make a rectangular laser with a width of 33 mm and a length of 5 mm. The output was adjusted using a temperature feedback system, and the laser heating temperature was set to 320°C. The average laser output during irradiation was about 7% (280 W), and the laser was scanned for 60 mm at a scanning speed of 3 mm / s. In the third step, a pressure of 2 MPa was applied to the bonding interface. A photograph of the appearance of the obtained ceramic resin bonded body (laser irradiation interval: 60 μm) is shown in Fig. 9.

[0076] The strength of the joint was evaluated by a 90° peel test for the ceramic-resin joints obtained using each laser irradiation interval. The 90° peel test was conducted at a test speed of 300 mm / min using a Shimadzu Corporation precision universal testing machine Autograph (AGS-10KNX) based on JIS Z0237. Figure 10 shows the state of the joint during the 90° peel test.

[0077] Figure 11 shows the test force at fracture for each ceramic-resin bonded body. When the laser irradiation interval was 60 μm or less, all ceramic-resin bonded bodies showed a high test force, and the resin fractured at the boundary region between the unbonded and bonded parts. In contrast, when the laser irradiation interval was greater than 60 μm, the test force decreased, and when the laser irradiation interval was 75 μm and 90 μm, the interfacial fracture occurred at the bonded interface. When a surface-modified region was not formed in the ceramic material by laser irradiation, the ceramic material and the resin material were not bonded at all.

[0078] Example 2: Joining non-oxide ceramics and resin (examination of laser heating temperature) Based on the results of Example 1, a ceramic resin bonded body was obtained in the same manner as in Example 1, except that the laser irradiation interval in the first step was set to 60 μm, and the laser output was controlled so that the laser heating temperature in the third step was 280° C., 320° C., and 360° C. The laser heating temperature was measured using a temperature feedback system (LPC03) manufactured by Dr. Mergenthaler. The average output during laser irradiation when the laser heating temperature was 280° C. was about 6% (240 W), the average output during laser irradiation when the laser heating temperature was 320° C. was about 7% (280 W), and the average output during laser irradiation when the laser heating temperature was 360° C. was about 8% (320 W).

[0079] A 90° peel test was carried out on each of the obtained ceramic-resin joined bodies in the same manner as in Example 1. The laser heating temperature in the third step and the test force at which each ceramic-resin joined body broke are shown in Fig. 12. The ceramic-resin joined body obtained at 280°C showed interfacial peeling, while the ceramic-resin joined body obtained at 320°C or higher showed resin fracture in the boundary region between the unjoined part and the joined part.

[0080] Example 3: Joining of non-oxide ceramics and resin (examination of applied pressure) Based on the results of Examples 1 and 2, ceramic-resin joined bodies were obtained in the same manner as in Example 1, except that the laser irradiation interval in the first step was set to 60 μm, the laser heating temperature in the third step was set to 320° C., and the joining pressures applied to the joined interfaces in the third step were set to 1 MPa, 2 MPa, and 3 MPa.

[0081] A 90° peel test was carried out on each of the obtained ceramic-resin joined bodies in the same manner as in Example 1. The pressure applied in the third step and the test force at which each ceramic-resin joined body broke are shown in FIG. 13. In the ceramic-resin joined body obtained with a pressure of 1 MPa, unjoined parts were generated, and the test force was accordingly reduced. In contrast, the ceramic-resin joined body obtained with a pressure of 2 MPa or more showed a high test force, with the resin breaking at the boundary between the unjoined parts and the joined parts. FIG. 14 shows an external view of the ceramic-resin joined body obtained with a pressure of 3 MPa after the 90° peel test, and it can be seen that wrinkles were generated in the resin film.

[0082] Example 4: Bonding of non-oxide ceramics and resin (evaluation of durability, etc.) Based on the results of Examples 1 to 3, a ceramic resin joint was obtained in the same manner as in Example 1, except that the laser irradiation interval in the first step was 60 μm, the laser heating temperature in the third step was 320° C., and the pressure in the third step was 2 MPa.

[0083] Furthermore, the obtained ceramic-resin bonded body was subjected to a temperature cycle test, and then a 90° peel test was performed in the same manner as in Example 1. The temperature cycle test was performed for 10 cycles and 25 cycles, with one cycle being "cooling the ceramic-resin bonded body from room temperature and holding it at -30°C for 3 hours, and then heating it to 100°C and holding it there for 3 hours."

[0084] The test force at fracture of the ceramic-resin bonded bodies before and after the temperature cycle test is shown in Figure 15. No decrease in the test force due to the temperature cycle test was observed, and the resin fracture occurred at the boundary between the unbonded part and the bonded part in all ceramic-resin bonded bodies. The bond strength did not decrease even in an extremely low temperature environment of -30°C, and it was revealed that the ceramic-resin bonded body of the present invention can be suitably used in extremely low temperature environments such as those in heavy snowfall areas.

[0085] A bending stress was applied to the ceramic-resin bonded body before the temperature cycle test using a universal testing machine and a three-point bending jig as shown in Figure 16, and the influence of secondary processing such as bending on the bonded part was evaluated. Figure 17 shows a photograph of the appearance of the ceramic-resin bonded body after the stress was applied. It can be seen that even when the ceramic-resin bonded body was cracked, the fluororesin material did not peel off at the bonded part.

[0086] Example 5: Bonding of oxide ceramics and resin Using the ceramic-resin direct bonding method of the present invention, an oxide-based ceramic material and a fluororesin material were directly bonded to each other. The oxide-based ceramic material was an alumina (Al2O3) plate with a thickness of 2 mm, width of 25 mm, and length of 90 mm, and the fluororesin material was a tetrafluoroethylene-ethylene copolymer (ETFE) sheet with a thickness of 100 μm.

[0087] The area of ​​the alumina plate that would become the interface to be bonded was irradiated with a laser in the atmosphere to form a surface modified area (first step). A 50W nanosecond pulse laser (YLPN-1-100-50-50) manufactured by IPG was used as the laser, and the laser irradiation conditions were average output: 50W (energy per pulse: 1mj), focus diameter: 59μm, and scanning speed: 15000588.5μm / s.

[0088] Here, since alumina is white, its energy absorption rate by laser irradiation is low, and the laser irradiation conditions applied to the silicon nitride plate do not allow for the formation of a sufficient surface modified area. Therefore, the laser irradiation interval was set to 5 μm in the row direction and 50 μm in the column direction, and the angle was changed by 90° to perform two laser irradiations.

[0089] An SEM photograph of the obtained surface-modified region is shown in FIG. 18. For SEM observation, a JSM-7200F manufactured by JEOL Ltd. was used. From FIG. 18, it can be seen that oxide particle aggregates formed in the surface-modified region are formed by agglomerating oxide particles having a particle size of about 1 to 50 nm. Here, compared to the surface-modified region formed on the silicon nitride plate, it is clear that the form is an aggregate of oxide particles having an ultrafine particle size.

[0090] Since it is difficult to heat up the alumina plate by laser irradiation, a ceramic resin bonded body was obtained using the pressure bonding device shown in Figure 19. The state during bonding is shown typically in Figure 20, where the alumina plate with the surface modified region formed and the fluororesin sheet were placed on top of each other on a heater table (second step), and bonding pressure was applied using a hydraulic cylinder press. The bonding temperature was set to 290°C, and a bonding pressure of 1 MPa was applied for 3 seconds. A photograph of the appearance of the obtained ceramic resin bonded body is shown in Figure 21.

[0091] Next, a 90° peel test was performed on each of the obtained ceramic-resin bonded bodies in the same manner as in Example 1. The test force-displacement diagram during the 90° peel test is shown in FIG. 22. For comparison, a 90° peel test was also performed on a ceramic-resin bonded body obtained by forming a surface-modified region by laser irradiation similar to that in Example 1, and the results are shown in FIG. 22. It should be noted that when the surface-modified region was not formed (when the first step was not performed), a ceramic-resin bonded body could not be obtained. It can be seen from FIG. 22 that a higher test force was obtained when the surface-modified region was formed by two laser irradiations, compared to when the surface-modified region was formed under the same conditions as the silicon nitride plate.

[0092] Next, the ceramic-resin bonded bodies were subjected to a temperature cycle test 25 times in the same manner as in Example 4, and the test force at the time of fracture of the ceramic-resin bonded bodies was measured before and after the temperature cycle test. The obtained test force-displacement diagram is shown in FIG. 23. No decrease in the test force due to the temperature cycle test was observed, and the resin fracture occurred at the boundary region between the unbonded part and the bonded part in all the ceramic-resin bonded bodies. The bond strength did not decrease even in an extremely low temperature environment of -30°C, and it was revealed that the ceramic-resin bonded body of the present invention can be suitably used in an extremely low temperature environment such as a heavy snowfall area, regardless of the type of ceramic.

[0093] XPS analysis was performed on the surface of the alumina plate before and after surface modification. For the XPS analysis, an AXIS ULTRA DLD manufactured by Kratos was used, and the excitation X-rays were monochromatic AlKα1,2 rays at 60 W (12 kV, 5 mA), with pass energies of 160 eV (wide spectrum) and 40 eV (narrow spectrum). Data processing was carried out by C 1s The peak top was corrected to 284.5 eV.

[0094] The results of the wide scan and narrow scan of each spectrum before surface modification are shown in Figures 24 and 25, respectively. The results of the wide scan and narrow scan of each spectrum after surface modification are shown in Figures 26 and 27, respectively. It can be seen that the peak intensity of C is reduced by laser irradiation, and the peaks of contaminants (Si and N) that are not included in the composition of the alumina plate have disappeared. [Explanation of symbols]

[0095] 2. Ceramic resin joint, 4. Resin material, 6. Ceramic materials, 8...Joint part (joint interface), 10. Ceramic resin joining material.

Claims

1. A method for directly bonding a ceramic material and a resin material, comprising the steps of: A first step of irradiating a surface of the ceramic material with a laser in an oxidizing atmosphere to form a surface modified region; a second step of contacting the resin material with the surface modified region to form a bonded interface; and a third step of heating the interface to be joined by an external heating means to achieve joining. A method for directly bonding ceramics to resin, comprising the steps of:

2. forming oxide particle aggregates in the surface modified region; 2. The method for directly bonding ceramics to resin according to claim 1,

3. using a pulsed laser as the laser in the first step; 3. The method for directly bonding ceramics to resin according to claim 1 or 2,

4. The resin material is a fluororesin material; 3. The method for directly bonding ceramics to resin according to claim 1 or 2,

5. applying a bonding pressure to the bonded interface in the third step; 3. The method for directly bonding ceramics to resin according to claim 1 or 2,

6. A ceramic-resin bonded body in which a ceramic material and a resin material are directly bonded to each other, At the joint, the ceramic material and the resin material are integrated via an oxide layer; A ceramic resin bonded body characterized by the above.

7. the oxide layer is made of oxide particle aggregates; 7. The ceramic-resin bonded body according to claim 6,

8. The resin material is a fluororesin material; 8. The ceramic-resin bonded body according to claim 6 or 7,

9. The resin base material is broken in a 90-degree peel test based on JIS-Z0237.

8. The ceramic-resin bonded body according to claim 6 or 7,

10. The ceramic-resin bonded body according to claim 6 or 7, To be used as a roofing material or an exterior wall material; A ceramic resin component characterized by the above.

11. The ceramic-resin bonded body according to claim 8, To be used as a roofing material or an exterior wall material; A ceramic resin component characterized by the above.

Citation Information

Patent Citations

  • Laser joining method

    JP2017164986A

  • Electron beam curing in a composite having a flow resistant adhesive layer

    US20060003127A1

  • Method for joining metal and resin and metal-resin composite, method for joining glass and resin and glass-resin composite, and method for joining ceramic and resin and ceramic-resin composite

    WO2007029440A1

  • Method for roughening substrate, method for surface-treating substrate, method for producing spray-coated member, and spray-coated member