Steel plate for hot stamp and hot stamp member using the same
A hot stamping steel plate with balanced chemical compositions and a targeted metal structure addresses the challenge of achieving high strength and complex shapes in vehicle parts, enhancing impact energy absorption and crack resistance.
Patent Information
- Application Number
- JP2023062285
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
Existing hot-stamping technologies face challenges in achieving both high strength and complex shapes in vehicle parts while ensuring sufficient impact energy absorption, with issues such as early crack initiation and propagation due to ferrite content and strict process conditions.
A hot stamping steel plate with specific chemical compositions and a metal structure comprising 70% or more martensite and bainite, and 30% or less ferrite, adhering to a formula that balances elements like C, Si, Mn, Ti, and B, allowing for general hot-stamping conditions to achieve tensile strength of 800 to 1300 MPa.
The solution enables hot-stamped members with excellent impact energy absorption characteristics, suppressing crack initiation and propagation, and maintaining strength within the desired range.
Smart Images

Figure 2024148818000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a steel sheet for hot stamping and a hot stamped member using the same. [Background technology]
[0002] Conventionally, there has been a demand for improving the safety of vehicle occupants in vehicles, and for this purpose, the shapes of parts used in the vehicle body have been made complex to improve rigidity, etc. On the other hand, against the background of the worsening of global warming problems, etc., there has been an accelerating movement to improve the fuel efficiency of automobiles. It is known that reducing the weight of the vehicle body is effective in improving fuel efficiency. For this reason, there is a demand for both high strength and complex shapes in automotive parts. As a technology that can achieve both high strength and complex shapes, hot stamping has been proposed, in which a steel sheet is press-formed at high temperatures using a die and then quenched to obtain a desired shape. Hot stamped components manufactured by the hot stamping process generally have a tensile strength (TS) of 1500 MPa or more. Hot stamped components with a tensile strength of 1500 MPa or more are used in non-deformable parts that suppress deformation of the cabin during an automobile collision. As the strength increases, the deformation resistance of the component increases and the initial load during a collision becomes higher, which not only causes the impact of the collision to propagate to the cabin, but also makes it easier for cracks to occur and grow during deformation, resulting in a problem that sufficient collision energy absorption effect cannot be obtained.
[0003] For this reason, it is known that the collision characteristics of the entire vehicle body can be improved by disposing a hot stamped part having a tensile strength of less than 1500 MPa and an enhanced energy absorption effect in a predetermined location. In particular, in recent years, various hot stamped parts having a tensile strength of less than 1500 MPa, such as 800 to 1300 MPa, have been proposed.
[0004] Patent Document 1 discloses a hot stamped component that has high strength and can improve the hole expansion ratio, which is correlated with impact properties, by making the metal structure 40% or more and 90% or less of ferrite and 10% or more and 60% or less of martensite.
[0005] Patent Document 2 discloses a hot stamped member having a gradient structure in the thickness direction, which comprises an internal hard layer, a surface soft phase obtained by decarburizing the surface, and a transition layer between these two layers, thereby achieving both high strength and high bendability. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2013 / 105633 [Patent Document 2] International Publication No. 2018 / 179839 Summary of the Invention [Problem to be solved by the invention]
[0007] The metal structure of the hot stamped member of Patent Document 1 is mostly ferrite, and it is difficult to achieve a tensile strength of 800 to 1300 MPa. If 40% or more of ferrite coexists with martensite, which can improve tensile strength, strain due to deformation during collision is concentrated in ferrite, making it easier for cracks to occur and progress early, and there is a problem that a sufficient collision energy absorption effect cannot be obtained.
[0008] The hot stamped member of Patent Document 2 is required to have a soft layer formed by decarburization. Since it is necessary to decarburize the material before hot stamping and maintain the decarburized state during the hot stamping process, there is a problem that the process conditions are severely limited, such as the soaking temperature and soaking time, as well as the cooling rate and forming temperature until forming for forming the surface soft layer. In addition, although a strength in the range of 800 to 1300 MPa can be obtained, there is still a problem that a sufficient impact energy absorption effect cannot be obtained.
[0009] The present disclosure has been made in consideration of the above circumstances, and has an object to provide a steel sheet for hot stamping which can provide a hot stamped component having excellent collision energy absorption effect, and a hot stamped component having excellent collision energy absorption effect. [Means for solving the problem]
[0010] Aspect 1 of the present invention is C:0.050~0.12% by mass Si:0.50~2.0% by mass Mn:2.1~3.0% by mass P: 0.10% by mass or less (including 0% by mass) S: 0.010% by mass or less (including 0% by mass) Al: 0.01~0.10% by mass Ti:0.010~0.100% by mass B:0.0010~0.0100% by mass N: 0.010% by mass or less (including 0% by mass) The remainder is Fe and unavoidable impurities, and the steel sheet for hot stamping satisfies the following formula (1): α=[%C] / 21 - [%Si] / 334 + [%Mn] / 81 - [%Ti] / 11 + 10 × <%B> ≧ 0.03 ···(1) Here, [%C], [%Si], [%Mn] and [%Ti] are the contents of C, Si, Mn and Ti, respectively, expressed in mass%, and <%B> is the amount of solute B expressed in mass%.
[0011] A second aspect of the present invention is the steel sheet for hot stamping according to the first aspect, wherein the steel sheet for hot stamping is a hot-rolled steel sheet.
[0012] A third aspect of the present invention is the steel sheet for hot stamping according to the first aspect, wherein the steel sheet for hot stamping is a cold-rolled steel sheet.
[0013] A fourth aspect of the present invention is a hot stamped member using the steel sheet for hot stamping according to any one of the first to third aspects, The metal structure has an area ratio of martensite and bainite totaling 70% or more and ferrite totaling 30% or less, The hot stamped member has a tensile strength of 800 MPa or more and 1,300 MPa or less. Effect of the Invention
[0014] According to one embodiment of the present invention, a steel sheet for hot stamping capable of obtaining a hot stamped member having an excellent collision energy absorption effect can be provided, and according to another embodiment of the present invention, a hot stamped member having an excellent collision energy absorption effect can be provided. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a diagram showing a cross-sectional shape of a hot-stamped member according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram of a crush test specimen. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present inventors have conducted extensive research to solve the above problems. As a result of detailed research focusing particularly on the structure after hot stamping, it has been found that it is necessary to suppress the amount of ferrite in the metal structure after hot stamping, i.e., in the state of the hot stamped member. More specifically, it has been found that by not only setting the contents of C, Si, Mn, P, S, Al, Ti, B, and N within a predetermined range, but also satisfying the following formula (1), the metal structure of the hot stamped member can be made to have an area ratio of martensite and bainite of 70% or more in total and ferrite of 30% or less, and a tensile strength of 800 to 1300 MPa, and as a result, an excellent collision energy absorption effect can be obtained. α=[%C] / 21 - [%Si] / 334 + [%Mn] / 81 - [%Ti] / 11 + 10 × <%B> ≧ 0.03 ···(1) Here, [%C], [%Si], [%Mn] and [%Ti] are the contents of C, Si, Mn and Ti, respectively, expressed in mass%, and <%B> is the amount of solute B expressed in mass%.
[0017] By using a steel sheet according to an embodiment of the present invention in which not only the contents of C, Si, Mn, P, S, Al, Ti, B, and N are within predetermined ranges but also the value of α calculated by formula (1) is within a predetermined range, the hot stamped material obtained can have an excellent collision energy absorption effect even when general hot stamping conditions are applied instead of special hot stamping conditions. Each requirement defined in the embodiment of the present invention will be described in detail below.
[0018] 1.Chemical composition The steel plate and hot stamped member according to the embodiment of the present invention have a chemical composition described below, and thus can have an excellent collision energy absorption effect after hot stamping (i.e., in the state of the hot stamped member).
[0019] [C: 0.050 mass% or more, 0.12 mass% or less] In the present invention, C is an important element. In order to suppress excessive strength while ensuring a certain degree of hardenability and suppressing the generation of ferrite, it is necessary to set the C content within an appropriate range. If the C content is excessively reduced, the strength and hardenability of the hot stamped member cannot be ensured, so the C content is set to 0.050 mass% or more. The C content is preferably 0.060 mass% or more, and more preferably 0.070 mass% or more. On the other hand, if the C content is excessive, the strength after hot stamping becomes excessive and the toughness of the hot stamped member is insufficient, which makes it easier for cracks to occur and progress due to deformation during collision, and the collision energy absorption characteristics deteriorate, so the upper limit of the C content is set to 0.12 mass%. The C content is preferably 0.11 mass% or less, and more preferably 0.10 mass% or less.
[0020] [Si: 0.50 mass% or more, 2.0 mass% or less] Si is an important element for ensuring the strength of hot stamped members. By adding Si, it is possible to ensure the strength by suppressing the precipitation of C as carbides during cooling after hot stamping. In order to achieve such an effect, the Si content is set to 0.50 mass% or more. The Si content is preferably 0.60 mass% or more, and more preferably 0.70 mass% or more. However, if the Si content is excessive, it causes deterioration of pickling properties due to an increase in oxide scale during steel sheet production, an increase in Ac3 transformation point, a decrease in cross tensile strength of spot welds, and the like. Therefore, the Si content is set to 2.0 mass% or less. The Si content is preferably 1.8 mass% or less, and more preferably 1.6 mass% or less.
[0021] [Mn: 2.1% by mass or more, 3.0% by mass or less] In the present invention, Mn is an important element. With the C content adjusted to the above range, it is useful for improving the hardenability of the steel sheet and making the main phase of the metal structure after hot stamping martensite-bainite. In order to exert such effects, the Mn content is set to 2.1 mass% or more. However, if the Mn content exceeds 3.0 mass%, the effect is saturated, which not only causes an increase in cost but also excessively increases the strength of the hot-rolled sheet during the production of the steel sheet before hot stamping, leading to a decrease in the subsequent cold rolling property. Therefore, the Mn content is set to 3.0 mass% or less. The Mn content is preferably 2.8 mass% or less, more preferably 2.6 mass% or less.
[0022] [P: 0.10% by mass or less (including 0% by mass)] P is an inevitable impurity element that deteriorates the weldability of steel plate, so it is desirable to limit its content as much as possible. In order not to deteriorate the weldability of steel plate, the P content is set to 0.10 mass% or less. The P content is preferably 0.050 mass% or less, and more preferably 0.020 mass% or less. P is an impurity that is inevitably mixed into steel, and it is difficult in industrial production to reduce its content to 0 mass%, so it is usually contained at 0.0005 mass% or more. In this specification, "including 0 mass%" means that it includes embodiments in which it is not added intentionally, i.e., the content is below the unavoidable impurity level (it does not exclude the case where it is added intentionally).
[0023] [S: 0.010% by mass or less (including 0% by mass)] S is an inevitable impurity element that deteriorates the weldability of steel sheets. Therefore, the S content is set to 0.010 mass% or less. The S content is preferably 0.0080 mass% or less, and more preferably 0.0050 mass% or less. The S content should be as low as possible, but it is difficult to reduce the S content to 0 mass% in industrial production, so the S content is usually 0.0001 mass% or more.
[0024] [Al: 0.01 mass% or more, 0.10 mass% or less] Al is an element that acts as a deoxidizer. In order to exert such an effect, the Al content is set to 0.01 mass% or more. The Al content is preferably 0.015 mass% or more, and more preferably 0.020 mass% or more. However, since excessive Al content leads to an increase in manufacturing costs, the Al content is set to 0.10 mass% or less. The Al content is preferably 0.08 mass% or less, and more preferably 0.07 mass% or less.
[0025] [Ti: 0.010 mass% or more, 0.100 mass% or less] In the present invention, Ti is an important element. The inclusion of Ti promotes the formation of TiN and increases the amount of solute B, which improves hardenability (it is possible to suppress the bonding of N with B). In order to achieve such effects, the Ti content is set to 0.010 mass% or more. The Ti content is preferably 0.012 mass% or more, and more preferably 0.015 mass% or more. However, if the Ti content is excessive, TiC is easily formed, the steel structure becomes fine, and the hardenability is rather reduced. Therefore, the Ti content is set to 0.100 mass% or less, preferably 0.095 mass% or less, and more preferably 0.090 mass% or less.
[0026] [B: 0.0010 mass% or more, 0.0100 mass% or less] In the present invention, B is an important element. B is known as an element that strengthens grain boundaries, and is contained as an element that is effective in improving hardenability. In order to obtain such an effect, the B content needs to be 0.0010% by mass or more. The B content is preferably 0.0012% by mass or more, and more preferably 0.0015% by mass or more. However, if the B content is excessive, it can cause surface cracks during casting due to the generation of B compounds, etc. Therefore, the B content needs to be 0.0100% by mass or less, preferably 0.0090% by mass or less, and more preferably 0.0085% by mass or less.
[0027] [N: 0.010% by mass or less (including 0% by mass)] N is an inevitable impurity element, and if it is contained in excess, BN is easily generated, which reduces the amount of solute B. Therefore, the N content is set to 0.010 mass% or less. The N content is preferably 0.008 mass% or less, and more preferably 0.005 mass% or less. Since the N content is preferably as small as possible, there is no particular lower limit, but it is difficult to reduce the N content to 0 mass% in industrial production, and it is usually contained at 0.0001 mass% or more.
[0028] [Remainder] The basic components of the hot stamping steel plate and hot stamping member according to the embodiment of the present invention are as described above, with the balance being iron and inevitable impurities. Examples of inevitable impurities include O, which is preferably suppressed as described below, as well as tramp elements (Pb, Bi, Sb, Sn, V, etc.) that are introduced depending on the conditions of raw materials, materials, manufacturing facilities, etc., within a range that does not impair the effects of the present invention. Like P, S, and N, the lower the content, the better, and therefore these elements are unavoidable impurities, but the composition ranges of some elements are separately specified as above. Therefore, in this specification, the "unavoidable impurities" that make up the balance are a concept that excludes elements whose composition ranges are separately specified. In addition, O is an inevitable impurity element, and if contained in excess, it forms an oxide and reduces the solid solution Si. Therefore, the O content is preferably 0.010 mass% or less. The O content is more preferably 0.005 mass% or less, and even more preferably 0.003 mass% or less. Since the O content is preferably as small as possible, there is no particular lower limit, but it is difficult to reduce the O content to 0 mass% in industrial production, and it is usually contained in an amount of 0.0001 mass% or more.
[0029] [Value α of Equation (1)] In order to make the metal structure of the hot stamped member obtained when applying general hot stamping conditions to the steel sheet for hot stamping of the present invention have an area ratio of martensite and bainite of 70% or more in total and ferrite of 30% or less, it is necessary not only to set the contents of C, Si, Mn, P, S, Al, Ti, B and N within the above-mentioned specified ranges, but also to satisfy the following formula (1). α=[%C] / 21 - [%Si] / 334 + [%Mn] / 81 - [%Ti] / 11 + 10 × <%B> ≧ 0.03 ···(1) Here, [%C], [%Si], [%Mn] and [%Ti] are the contents of C, Si, Mn and Ti, respectively, expressed in mass%, and <%B> is the amount of solute B expressed in mass%.
[0030] The value α calculated by the above formula (1) is an index showing the hardenability of the steel sheet. The ferrite fraction of various samples obtained by applying general hot stamping conditions was measured, and multiple regression analysis was performed with the ferrite fraction as the objective variable and each component value as the explanatory variable, and the following formula (2) was obtained from the relation between the ferrite fraction and the components. α=[%C] / 21 - [%Si] / 334 + [%Mn] / 81 - [%Ti] / 11 + 10 × <%B> - [%Nb] / 2 ≧ 0.03 ···(2) Here, [%C], [%Si], [%Mn], [%Ti] and [%Nb] are the contents of C, Si, Mn, Ti and Nb, respectively, expressed in mass%, and <%B> is the amount of solute B expressed in mass%.
[0031] In the Nb term, the denominator of the coefficient is small, and in the useful amount of Nb added, it is difficult to ensure α≧0.03. In consideration of this, Nb is not contained in formula (2) (i.e., Nb is not added), thereby arriving at formula (1).
[0032] The amount of dissolved B <%B> can be calculated as follows. N present in steel bonds more easily with Ti than with B. In order for all N to bond with Ti to become TiN, that is, since TiN has a stoichiometric ratio of 1:1, if the following formula (3) is satisfied based on the atomic weights of Ti and N of 47.8 and 14, respectively, then all N has become TiN, no BN is formed, and all added B (B amount) is judged to be dissolved B. In other words, dissolved B amount <%B> is equal to the B amount. [%Ti] ≧ (47.8 / 14) × [%N] ···(3) Here, [%Ti] and [%N] are the Ti and N contents expressed in mass% respectively.
[0033] On the other hand, if the above formula (3) is not satisfied, N that did not form TiN will form BN, so the amount of dissolved B <%B> is calculated using the following formula (4) using the atomic weight of B, 10.8. However, if the value of formula (4) is negative, <%B> should be set to zero. <%B> = 10.8 × ([%B] / 10.8 -([%N] / 14 - [%Ti] / 47.8)) ···(4) Here, [%B], [%Ti] and [%N] are the contents of B, Ti and N, respectively, expressed in mass%.
[0034] The above-mentioned "general hot stamping conditions" are conditions that satisfy: (1) heating to a soaking temperature of Ac3 point or higher and holding at the soaking temperature (soaking), (2) an average cooling rate from the soaking temperature to the forming temperature that is equal to or higher than the cooling rate due to natural cooling, and (3) a forming temperature of 500 to 750°C. Note that "forming temperature" refers to the temperature of the steel sheet just before forming with a die, and "equal to or higher than the cooling rate due to natural cooling" refers to a cooling rate that is equal to or higher than the cooling rate when the steel sheet is left in the air naturally after being removed from a heating furnace without being heated to reduce the cooling rate.
[0035] 2.Metal structure (1) Metal structure of steel sheets for hot stamping The steel sheet for hot stamping according to the embodiment of the present invention is a steel sheet that can be processed into a desired shape by applying the above-mentioned "general hot stamping conditions". Since the steel sheet is heated to a temperature of Ac3 point or higher during hot stamping, there is no particular restriction on the metal structure in the state of the steel sheet. The steel sheet for hot stamping according to the embodiment of the present invention may be a hot-rolled steel sheet or a cold-rolled steel sheet. A hot-rolled steel sheet is excellent in productivity because it does not require cold rolling after hot rolling, whereas a cold-rolled steel sheet has an advantage that a thin steel sheet can be easily obtained.
[0036] (2) Hot stamping parts The hot stamped member according to the embodiment of the present invention can be obtained by applying "general hot stamping conditions" to the above-mentioned steel sheet for hot stamping according to the embodiment of the present invention. The metal structure of the obtained hot stamped member is, in terms of area ratio, 70% or more of martensite and bainite in total, 30% or less of ferrite, and less than 1% of other structures. Examples of other structures include pearlite and retained austenite. Preferably, it does not contain other structures. In other words, the metal structure is preferably composed of only 70% or more of martensite and bainite in total, and 30% or less of ferrite in terms of area ratio.
[0037] By making the total area ratio of martensite and bainite 70% or more, the tensile strength of the obtained hot stamped part can be made 800 MPa or more and 1300 MPa or less. This makes it possible to ensure a sufficient amount of energy absorption during a collision. The total area ratio of martensite and bainite is preferably 80% or more, more preferably 90% or more. The martensite and bainite may include both or only one of them. The martensite may be one or more selected from the group consisting of as-quenched martensite without carbides, tempered martensite with carbides, and self-tempered martensite. The bainite may be either or both of upper bainite containing cementite and retained austenite between laths and lower bainite containing carbides within the laths.
[0038] Ferrite is an equiaxed crystal grain that does not contain iron-based carbides. By making the area ratio of ferrite 30% or less, the structure in which strain caused by deformation during a collision is concentrated can be reduced, and early generation and propagation of cracks can be suppressed. The area ratio of ferrite is preferably 20% or less, more preferably 10% or less.
[0039] The metal structure is observed at a representative location, that is, the plate thickness t / 4 position (a position located a quarter of the plate thickness t from the surface (main surface) of the steel plate constituting the hot stamped component toward the center), on the flat surface of the hot stamped component (a portion without hot deformation such as bending).
[0040] The surface of the steel sheet for hot stamping and the hot stamp member according to the embodiment of the present invention may or may not have a plating layer such as hot-dip galvanizing or galvannealing. By having such a plating layer, for example, it is possible to suppress the generation of scale during hot stamp heating. On the other hand, if there is no plating layer, the manufacturing cost of the steel sheet can be suppressed. Furthermore, the steel sheet for hot stamping and the hot stamp member according to the embodiment of the present invention may have a decarburized layer on the surface in order to improve formability during hot stamping.
[0041] 3. Manufacturing method As described above, the hot stamping steel sheet according to the embodiment of the present invention is not particularly limited in terms of its metal structure. Therefore, as long as the chemical composition specified in the above "1. Chemical composition" including formula (1) is satisfied, the hot stamping steel sheet can be easily manufactured by using a known method for manufacturing a hot rolled steel sheet and a cold rolled steel sheet.
[0042] The steel sheet for hot stamping according to the embodiment of the present invention can be obtained by hot stamping under the above-mentioned "general hot stamping conditions" which satisfy: (1) heating to a soaking temperature of Ac3 point or higher and holding at the soaking temperature (soaking), (2) an average cooling rate from the soaking temperature to the forming temperature is equal to or higher than the cooling rate by natural cooling, and (3) a forming temperature of 500 to 750°C.
[0043] An example of such a soaking temperature of the Ac3 point or higher is a temperature of 850 to 1000° C. Furthermore, an example of a soaking time (holding time) for holding at such a soaking temperature is 50 to 300 seconds. Furthermore, the average cooling rate from the soaking temperature to the molding temperature, which is "greater than the cooling rate by natural cooling", can be exemplified by natural cooling (for example, 2°C / sec) to 50°C / sec. EXAMPLES
[0044] 1. Example 1 In Example 1, the relationship between the composition, the value of α calculated from the formula (1), and the metal structure of the sample after hot stamping (hot stamped member) was clarified.
[0045] (1) Preparation of steel sheet samples for hot stamping Steel having the composition shown in Table 1 was melted and made into a slab. In addition to the chemical composition, Table 1 also shows the value α calculated using formula (1). In addition, for steel types A, D, E, and I that contain B, the value of the right hand side of formula (3) and whether or not formula (3) is satisfied are also shown. As can be seen from Table 1, steel types A, D, E, and I all satisfy formula (3), so when calculating α using formula (1), the amount of solute B was used. The B content of each steel type was used as the value of The obtained slab was heated to 1100 to 1300 ° C, hot-rolled so that the finish rolling temperature was 890 to 950 ° C, and held at 500 to 700 ° C. After holding, it was cooled to room temperature to obtain a hot-rolled steel sheet. The obtained hot-rolled steel sheet was pickled to remove surface scale, and then cold-rolled to produce a cold-rolled steel sheet. The sheet thickness of the cold-rolled steel sheet sample thus obtained is shown in Table 2. The cold-rolled steel sheet sample was subjected to additional annealing as necessary, and hot-dip galvanizing treatment or alloyed hot-dip galvanizing treatment.
[0046] [Table 1]
[0047] From the steel plate samples thus obtained, blanks of the sizes shown in Table 2 were cut out, and the obtained blanks were subjected to hot stamping under the conditions (soaking temperature, soaking time, average cooling rate from the soaking temperature to the forming temperature, and forming temperature) shown in Table 2 to obtain hot stamped component samples.
[0048] [Table 2]
[0049] The obtained hot stamped member samples were subjected to microstructural observation and measurement of the ferrite fraction. The results are shown in Table 2. The structure was observed by observing a nital-etched region of 100 μm vertical×130 μm horizontal field of view at the sheet thickness t / 4 position on a surface parallel to the rolling direction at 1000 to 3000 magnifications using a scanning electron microscope (SEM). In all samples, no structures other than ferrite, martensite, and bainite were observed, i.e., all structures other than ferrite were martensite or bainite. The ferrite fraction was determined by a point counting method in which a grid of 100 or more intersections of evenly spaced vertical and horizontal lines was placed on the 1000 to 3000x SEM images used for microstructural observation, and the number of intersections on each phase was counted.
[0050] The chemical compositions of samples A1, A2, H1, and H2 satisfy the prescribed component range. In addition, after hot stamping performed under typical hot stamping conditions, the ferrite fraction was 0% (martensite and bainite were 100% in total), and the α value was also satisfied. Samples B1, B2, C1, C2, D1, E1, E2, F1, F2, G1 and G2 do not satisfy the chemical composition regulations, do not satisfy the α value, and have a ferrite fraction exceeding 30%. Sample D-2 has lower Si and Mn than the specified values. Due to this, the ferrite fraction was below 30% even though the α value was out of range. However, it is believed that sufficient strength cannot be obtained because the Si value is low. In samples I1 and I2, the value of α was within the specified range, and the ferrite fraction was 0. However, the C content was too large, and the strength was too high to obtain sufficient collision energy absorption characteristics (see also Example 2).
[0051] 2. Example 2 In Example 2, in addition to samples H1 and I1 of Example 1, the collision energy absorption properties were evaluated for three types (steel types J, K, and L) of general-purpose high-tensile steel (cold-rolled steel sheet) for cold forming, whose chemical compositions are shown in Table 3, as comparative materials.
[0052] [Table 3]
[0053] (1) Preparation of samples for crushing test Blank samples for samples H1-1 and H1-2, measuring 217 mm wide x 300 mm long x 1.2 mm thick, were prepared in the same manner as for H1 in Example 1. As shown in Table 4, the blanks for sample H1-1 and sample H1-2 are the same except that the former is not plated and the latter is zinc alloy plated. Blank samples for samples I1-1 and I1-2, each having a width of 217 mm, length of 300 mm, and thickness of 1.2 mm, were prepared in the same manner as in I1 of Example 1. As shown in Table 4, the blanks for sample I1-1 and I1-2 are the same except that the former is galvannealed and plated with zinc, and the latter has a surface decarburized layer in addition to the galvannealed plating.
[0054] These blank samples were used to produce hot stamped member samples having the cross-sectional shape shown in Fig. 1, as in Example 1. The hot stamping conditions for samples H1-1 and H1-2 were the same as those for sample H1 in Example 1, and the hot stamping conditions for samples I1-1 and I1-2 were the same as those for sample I1 in Example 1.
[0055] In addition, cold forming samples J-1, K-1, and L-1 measuring 217 mm wide x 300 mm long x 1.2 mm thick were cut out from each of the high tensile steel samples for cold forming of steel types J, K, and L. The obtained cold forming samples were cold formed to obtain high tensile steel cold formed samples having the cross section shown in Figure 1.
[0056] Next, both ends of the obtained hot stamped parts and high tensile cold formed samples (the hot stamped parts and high tensile cold formed samples are sometimes collectively referred to as "hat parts") were cut to a length of 200 mm. Furthermore, a 590Ma-class steel plate of the same thickness was attached to the flange part of the 200 mm long hat part by spot welding to form a closed cross-section structure. Furthermore, a top plate was attached to the upper end of the hat component by arc welding, and a bottom plate was attached to the lower end by arc welding. The top plate was 200mm x 200mm in size, and the bottom plate was 250mm x 250mm in size, with a thickness of 9mm for both. Both the top plate and the bottom plate were positioned so that their centers of gravity were aligned with the hat component. Figure 2 is a schematic diagram showing the crush test specimen thus obtained. In Figure 2, the plates attached to the flange of the hat member by spot welding are omitted so that the shape of the hat member can be easily recognized, but the positions of the spot welds at 25 mm intervals are shown.
[0057] (2) Crush test Using the obtained crush test specimen, a dynamic axial crush test was conducted in which a 190 kg weight was dropped from a height of 10 m. A stopper to receive the weight was placed 105 mm downward from the top plate of the crush test specimen. The load was measured using a load cell, and the displacement was measured with a laser displacement meter by marking the weight.
[0058] The stroke was 0% when the weight contacted the crushing specimen and the load was recorded on the load cell, and the stroke was 100% when the displacement was 100 mm. The recorded data was averaged over 21 points. The load between 0 and 100% of the stroke and the load between 80 and 100% of the stroke were integrated, and the amount of absorbed energy was calculated. The amount of energy absorbed between 80-100% of the stroke is divided by the amount of energy absorbed between 0-100% of the stroke and expressed as a percentage. R The test was performed at least three times for each sample, and the average values are shown in Table 4 as the measurement results for each sample. R Samples with a value of 18% or more were judged to have high absorbed energy.
[0059] The crushing state of each sample was observed and is shown in Table 4. Samples that developed a large crack and broke even once out of multiple tests are recorded in Table 4 as "large crack and breakage," and samples where all samples showed bellows-like deformation, which is the normal crushing mode, are recorded in Table 4 as "bellows-like deformation." Total energy absorption is 5.5kJ or more, EA R The samples with a crushing deformation of 18% or more and all of which showed a bellows-like deformation were judged to have excellent collision energy absorption properties.
[0060] [Table 4]
[0061] (Tensile strength) A No. 5 test piece (JIS No. 5 test piece) specified by JIS Z 2241 was taken from the flat part of the hat member of each sample (a part without hot deformation such as bending) and the tensile strength was measured. The measurement results are shown in Table 4.
[0062] Samples H1-1 and H1-2 according to the embodiment of the present invention exhibited excellent collision absorption energy characteristics. The tensile strength of the samples I1-1 and I1-2 was too high, and the EA of the crush test R The strength was low, and large cracks occurred, causing the specimen to break. Sample J-1 had low tensile strength and low total energy absorption. Samples K-1 and L-1 are EA of the crush test R The strength was low, and large cracks occurred, causing the specimen to break.
Claims
1. C: 0.050 to 0.12% by mass Si: 0.50 to 2.0% by mass Mn: 2.1 to 3.0% by mass P: 0.10% by mass or less (including 0% by mass) S: 0.010% by mass or less (including 0% by mass) Al: 0.01 to 0.10% by mass Ti: 0.010 to 0.100% by mass B: 0.0010 to 0.0100% by mass N: 0.010% by mass or less (including 0% by mass) and the balance being Fe and unavoidable impurities, and satisfying the following formula (1): α=[%C] / 21 - [%Si] / 334 + [%Mn] / 81 - [%Ti] / 11 + 10 × <%B> ≧ 0.03 ... (1) Here, [%C], [%Si], [%Mn] and [%Ti] are the contents of C, Si, Mn and Ti, respectively, expressed in mass%, and <%B> is the amount of solute B expressed in mass%.
2. The steel sheet for hot stamping according to claim 1, which is a hot-rolled steel sheet.
3. The steel sheet for hot stamping according to claim 1, which is a cold-rolled steel sheet.
4. A hot stamped member using the steel sheet for hot stamping according to any one of claims 1 to 3, The metal structure has an area ratio of martensite and bainite totaling 70% or more and ferrite totaling 30% or less, A hot stamped member having a tensile strength of 800 MPa or more and 1300 MPa or less.
Citation Information
Patent Citations
Galvanized steel sheet for hot stamping, hot stamped part, and method for producing hot-stamped part
JP2021120483A
Steel plate for hot stamping, method for manufacturing same, hot stamp member, and method for manufacturing same
WO2022080489A1
A cold-rolled and hot-press formed high strength steel product with excellent hole expandability and process of producing the same
WO2022189606A1
Steel sheet for hot stamping, method for manufacturing steel sheet for hot stamping, and hot stamp molded body
WO2023132349A1