Hydrogen cyanide production method
The use of a molybdenum-titanium mixed oxide catalyst in a fixed bed flow reactor initiates and maintains hydrogen cyanide production at lower temperatures, addressing high-cost equipment issues by leveraging reaction heat, thus reducing costs and maintaining efficiency.
Patent Information
- Application Number
- JP2023062343
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
Gas-phase ammoxidation reactions of hydrocarbons require high reaction temperatures, leading to increased equipment costs due to the need for specialized heating media capable of reaching and maintaining high temperatures, such as molten salts.
A method using a mixed oxide catalyst of molybdenum and titanium, with a molybdenum content between 50 to 97 mol%, is employed in a fixed bed flow reactor, where the reaction initiation temperature is 200 to 300°C, allowing the reaction to be initiated and maintained through the heat generated by the exothermic reaction itself, eliminating the need for high-temperature heating media.
This approach reduces the temperature requirements for the heating medium, lowering equipment and heating medium costs while maintaining efficient production of hydrogen cyanide, and allows for normal temperature control without specialized heating media.
Smart Images

Figure 2024148850000001 
Figure 2024148850000002 
Figure 2024148850000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing hydrogen cyanide. [Background technology]
[0002] Nitrile compounds are useful compounds for use as pharmaceutical and agrochemical intermediates, as raw materials for functional resins, dyes, pigments, etc. The most inexpensive method for producing these compounds is the gas phase ammoxidation method of organic compounds having alkyl groups. Various ammoxidation catalysts have been studied and many improvements have been proposed. Hydrogen cyanide is an important compound used in the production of many fine and specialty chemicals and is also produced by ammoxidation, for example, using methanol, ammonia and air as feedstocks in a catalytic fluidized bed reactor. There are various reports on catalysts used in the ammoxidation of methanol. For example, Patent Document 1 proposes a method for producing hydrogen cyanide using a molybdenum-bismuth (Mo-Bi) catalyst as a composite oxide catalyst, and Patent Document 2 proposes a method for producing hydrogen cyanide using a catalyst made by calcining a metal oxide containing iron-antimony (Fe-Sb). Patent Document 3 proposes a method for producing hydrogen cyanide using a catalyst mainly composed of manganese (Mn) and phosphorus (P), and Patent Document 4 proposes a method for producing hydrogen cyanide using a catalyst mainly composed of vanadium (V) and phosphorus (P). The above-mentioned ammoxidation of methanol is carried out at high temperatures of 400° C. or higher in all cases. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-97017 A [Patent Document 2] Japanese Patent Application Publication No. 10-251012 [Patent Document 3] Special Publication No. 2010-531290 [Patent Document 4] Japanese Patent Application Publication No. 7-206427 Summary of the Invention [Problem to be solved by the invention]
[0004] Normally, a high reaction temperature is required for the gas phase ammoxidation reaction of hydrocarbons. The ammoxidation of methanol is carried out at a high temperature of 400°C or more. For this reason, the reaction vessel is heated to 400°C or more using a heat transfer medium before the reaction starts. For this reason, the heat transfer medium used in the early stage of the ammoxidation reaction must be a special one that can be heated to a high temperature of 400°C or more. This increases the equipment costs.
[0005] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a method for producing hydrogen cyanide that can reduce the temperature of a heat medium used compared to conventional methods and reduce the costs of the heat medium and equipment. [Means for solving the problem]
[0006] As a result of intensive research aimed at solving the above problems, the present inventors have found that the above problems can be solved by the following invention.
[0007] That is, the present invention relates to the following. [1] A step (A) of reacting methanol and oxygen in a gas phase while supplying them to a reactor in the presence of a catalyst containing a molybdenum oxide; Following the step (A), a step (B) is performed in a gas phase while supplying methanol, oxygen, and ammonia to the reactor, 1. A method for producing hydrogen cyanide, comprising the steps (A) and (B) being carried out in a flow manner in the presence of a mixed oxide of molybdenum and titanium having a molybdenum content of more than 50 mol % and not more than 97 mol %. [2] In the step (A), the reaction initiation temperature is 200 to 300° C.; The method for producing hydrogen cyanide according to the above-mentioned [1], wherein the reaction temperature of the ammoxidation reaction in the step (B) is 270 to 600°C. [3] The method for producing hydrogen cyanide according to the above [1] or [2], wherein in the step (A), the reaction between the methanol and oxygen is initiated in a heated state using a heat transfer medium. [4] The method for producing hydrogen cyanide according to the above [3], wherein the gas phase reactions in the step (A) and the step (B) are carried out in a fixed bed flow type reactor. Effect of the Invention
[0008] According to the present invention, it is possible to provide a method for producing hydrogen cyanide in which the temperature of the heat medium used can be lowered compared to conventional methods, thereby reducing the heat medium costs and equipment costs. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the present invention will be described in detail with reference to an embodiment. <How to manufacture hydrogen cyanide> The method for producing hydrogen cyanide of the present embodiment includes a step (A) of reacting methanol and oxygen in a gas phase while supplying them to a reactor in the presence of a mixed oxide catalyst of molybdenum and titanium having a molybdenum content of 45 mol % or more and 97 mol % or less, and a step (B) of, subsequent to the step (A), carrying out an ammoxidation reaction in the gas phase while supplying methanol, oxygen, and ammonia to the reactor, and is characterized in that the steps (A) and (B) are carried out in a flow mode.
[0010] [Process (A)] In step (A), methanol and oxygen are supplied to a reactor in the presence of a catalyst containing molybdenum oxide and reacted in a gas phase. This reaction is an exothermic reaction and is represented by the following formula (1). CH3OH+O2→HCHO+H2O (1) The reactor is heated by the heat of reaction generated in the reaction, and the temperature of the reactor rises to a temperature at which the reaction in the subsequent step (B) can take place. This allows the temperature of the heat transfer medium used in the initial stage of the reaction to be lower than in the past. Therefore, in this embodiment, it is not necessary to use a special heat transfer medium that can be used at high temperatures, such as molten salt. This makes it possible to produce hydrogen cyanide at low cost. Once the temperature of the reactor rises to a temperature at which the reaction in step (B) can take place, the temperature in step (B) is maintained by the heat of reaction, so normal control can be performed and there is no need to perform a new step (A).
[0011] The mixed oxide catalyst of molybdenum and titanium used for hydrogen cyanide has a molybdenum content of more than 50 mol% and not more than 97 mol% relative to the total amount of molybdenum and titanium. By using this oxide catalyst, the reaction represented by the above formula (1) can be efficiently carried out. By using the mixed oxide catalyst of molybdenum and titanium, a sufficient heating effect can be obtained in step (A). However, if the ratio of molybdenum is 50 mol% or less, the amount of hydrogen cyanide obtained in step (B) is insufficient, which is not preferable. In addition, if the content of molybdenum is more than 97 mol%, the amount of hydrogen cyanide obtained decreases, which is not preferable. The content of molybdenum in the mixed oxide catalyst of molybdenum and titanium is more preferably more than 50 mol% and not more than 95 mol%, and even more preferably 80 mol% or more and not more than 95 mol%. The ratio of molybdenum and titanium almost reflects the ratio of the respective raw materials charged during the production of the catalyst, but it can be confirmed by measuring the contents of molybdenum and titanium contained in the catalyst using a fluorescent X-ray analyzer. Specifically, it can be measured by the method described in the Examples.
[0012] The catalyst can be produced by a known complex polymerization method, for example, as disclosed in JP-A-6-115934. The complex polymerization method uses a metal salt as a raw material of a metal complex, an oxycarboxylic acid that functions as a ligand, and a polyol for forming a complex polymer. For example, the raw materials of the molybdenum oxide and titanium oxide used in this embodiment are not particularly limited as long as they can be completely dissolved in a solvent, and the oxides may be used as they are, or various compounds that can easily become oxides may be used. As the raw material of molybdenum oxide, heteropolyacids such as molybdenum trioxide, molybdic silicate, and phosphomolybdic acid; molybdenum compounds that can be easily converted into oxides such as ammonium molybdate (para) tetrahydrate are preferably used. Among these, ammonium molybdate (para) tetrahydrate is particularly preferred. As the raw material of titanium oxide, titanium tetrachloride, ammonium titanium oxalate, potassium oxalate titanate, and tetraisopropyl orthotitanate are preferably used. Among these, titanium tetrachloride is particularly preferred. Preferred examples of oxycarboxylic acids include citric acid, tartaric acid, oxalic acid, malic acid, tartronic acid, glyceric acid, oxybutyric acid, hydroacrylic acid, lactic acid, and glycolic acid. Of these, citric acid is particularly preferred. As the polyol, ethylene glycol, propylene glycol, trimethylene glycol, 1,4-butanediol, etc. are preferably used, of which ethylene glycol is particularly preferred.
[0013] A metal complex obtained by reacting a raw material of an oxide of molybdenum with a raw material of an oxide of titanium and an oxycarboxylic acid is polymerized with a polyol in a solvent to form a complex polymer, which is then calcined in an oxygen gas atmosphere. The solvent is not particularly limited, but water and alcohol are preferred. The firing is carried out at 300 to 800° C. for 1 to 10 hours while passing a gas containing oxygen gas. The firing temperature is preferably 400 to 650° C., more preferably 450 to 600° C. There is no limitation on the gas containing oxygen gas, but air is preferred. Pre-firing may be carried out prior to the firing.
[0014] In this embodiment, steps (A) and (B) are carried out in a flow-through manner in the same reactor without replacing the catalyst. In step (A), the temperature of the reactor is raised by the reaction heat of oxidizing methanol, thereby ensuring the reaction temperature required for the ammoxidation of methanol in the subsequent step (B). Therefore, a reactor with a large heat storage capacity is preferred. The material of the reactor depends on the type of raw material and the reaction conditions, but generally, stainless steel such as SUS316; nickel, Inconel (registered trademark), Monel, Hastelloy (registered trademark) C, and other nickel-containing metals are used.
[0015] A fixed-bed flow-type reactor is preferably used as the reactor. Any known fixed-bed flow-type reactor can be used as the reactor for gas reaction without any particular limitation. The fixed-bed flow-type reactor is composed of a gas supply and a reactor filled with a catalyst. The reactor is heated from the outside by a heat medium. The gasified methanol and oxygen gas in the gas supply vessel are introduced into a reactor heated by a heat medium, and the mixed gas containing the methanol gas and the oxygen gas comes into contact with a catalyst and reacts continuously in the gas phase.
[0016] In the step (A), the reaction initiation temperature is preferably 200 to 300° C., more preferably 200 to 270° C., even more preferably 210 to 250° C., and still more preferably 210 to 240° C. The reaction initiation temperature can be appropriately adjusted by the heat medium.
[0017] Examples of the heat transfer medium include silicone oil, high-pressure water, ionic liquid, sand bath, etc. Among them, silicone oil is preferred from the viewpoints of ease of handling, heat removal / uniform heating, and heat resistance. The temperature of the heat medium is preferably 200 to 300° C., more preferably 200 to 270° C., even more preferably 210 to 250° C., and still more preferably 210 to 240° C. When the temperature of the heat medium is 200° C. or higher, the reaction can proceed, and when the temperature is 300° C. or lower, side reactions due to an increase in reaction temperature can be suppressed. The temperature of the heat medium can be appropriately adjusted by adjusting the temperature setting of the heater of the heat medium.
[0018] The feed composition of methanol and oxygen gas [O2 / CH3OH] is preferably 0.5 to 10.0, more preferably 0.5 to 2.0, and even more preferably 1.0 to 1.2, in terms of molar ratio. When the feed composition of methanol and oxygen gas [O2 / CH3OH] is 0.5 or more, the reaction can be maintained without deactivating the catalyst, and when it is 10.0 or less, excessive oxidation can be suppressed.
[0019] The mixed gas containing methanol and oxygen gas may contain gases other than ammonia as long as they are inert to the reaction. If ammonia is mixed into the mixed gas containing methanol and oxygen gas in step (A), the ammonia competitively inhibits the adsorption of methanol onto the catalyst surface, lowering the reaction temperature, which may make it difficult for ammoxidation to proceed in the subsequent step (B). Examples of the gas other than ammonia contained in the mixed gas include inert gases such as nitrogen gas, carbon dioxide, helium, argon, etc. Among these, nitrogen gas is preferred from the viewpoints of cost and safety.
[0020] The linear velocity (LV) of the mixed gas is usually 0.25 to 5.2 m / min, and preferably 0.5 to 2.0 m / min. The reaction in step (A) varies depending on the operating conditions, but is usually carried out for 30 to 60 minutes before step (B). The by-product gases including oxygen gas and unreacted methanol gas may be rendered harmless by a prescribed method and discharged outside the system, or a part or all of the by-product gases may be reused as a mixed gas to be introduced into the reactor.
[0021] During the step (A), the temperature of the catalyst packed in the reactor (catalyst layer temperature) is measured. The measurement can be performed by moving a thermocouple up and down inside an inner tube attached to the reactor. When the catalyst layer temperature in the reactor reaches 250 to 430°C and stabilizes, it is preferable to end the step (A) and move to the step (B) immediately. The temperature of the catalyst layer in the reactor at the time of moving to step (B) is preferably 260 to 370° C., more preferably 270 to 330° C. When the catalyst layer temperature is 250° C. or higher, the ammoxidation reaction in the subsequent step (B) can proceed sufficiently, and when the catalyst layer temperature is 430° C. or lower, side reactions can be suppressed. The catalyst layer temperature can be appropriately adjusted depending on the type of catalyst, the amount of catalyst, and the inner diameter of the reactor.
[0022] [Process (B)] In the step (B), subsequent to the step (A), an ammoxidation reaction is carried out in a gas phase while supplying methanol, oxygen gas and ammonia to the reactor. Ammonia is further introduced from a gas supplying device into the reactor heated in the step (A), and the raw material mixed gas containing methanol, oxygen gas, and ammonia is brought into contact with the catalyst to continuously carry out an ammoxidation reaction in the gas phase. The ammoxidation reaction is initiated under the catalyst layer temperature conditions achieved by the reaction in step (A). When the reaction in step (B) is carried out, the reaction temperature (catalyst layer temperature) is increased to a temperature higher than that in step (A) due to the heat of reaction caused by ammoxidation. The reaction temperature of ammoxidation is preferably 270 to 600°C, more preferably 300 to 600°C, even more preferably 320 to 500°C, and still more preferably 320 to 450°C. When the reaction temperature of ammoxidation is 270°C or higher, the reaction can be maintained, and when the reaction temperature is 600°C or lower, sublimation of molybdenum and side reactions can be suppressed.
[0023] From the viewpoint of improving the reaction rate, the concentration of methanol in the raw material mixed gas in step (B) is preferably 1 to 15 mol %, more preferably 5 to 15 mol %, and even more preferably 5 to 12 mol %. The amount of oxygen gas used, in terms of the molar ratio to methanol [O2 / CH3OH], is preferably 1 to 10, more preferably 1 to 6, and further preferably 1 to 4. When the amount of oxygen gas used is within the above range, the reaction can be maintained without reducing the catalyst. The amount of ammonia used, in terms of the molar ratio to methanol [NH3 / CH3OH], is preferably 0.5 to 3.0, more preferably 0.6 to 2.5, and further preferably 0.8 to 2.0. When the amount of ammonia used is within the above range, the ammoxidation reaction can be maintained.
[0024] The contact time between the raw material mixed gas and the catalyst is preferably 0.1 to 25 seconds, more preferably 0.1 to 10 seconds. The gas hourly space velocity (SV) is preferably 1,000 to 20,000 Hr. -1 More preferably, it is 2000 to 9000Hr -1 It is. The ammoxidation reaction can be carried out under any of normal pressure, elevated pressure, and reduced pressure, but is preferably carried out within a range of normal pressure to 300 kPaG (gauge pressure).
[0025] The reaction product can be collected, for example, by washing the reaction product gas with a solvent such as water and collecting it. The collected reaction product can be purified by a known method such as distillation to obtain the target product, hydrogen cyanide. EXAMPLES
[0026] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples in any way.
[0027] [Catalyst production] <Catalyst 1, synthesis example of a mixed oxide catalyst of molybdenum and titanium containing 90 mol % of molybdenum> 9.93g of ethylene glycol (FUJIFILM Wako Pure Chemical Co., Ltd.), 3.18g of ammonium molybdate (para) tetrahydrate (FUJIFILM Wako Pure Chemical Co., Ltd.), 7.68g of citric acid (Kanto Chemical Co., Ltd.), and 25ml of water were placed in a silica-alumina container, and the mixture was heated and stirred at 60°C to dissolve. The mixture was then cooled to room temperature (25°C), and 0.58g of titanium (IV) chloride solution (FUJIFILM Wako Pure Chemical Co., Ltd.) was added, and the mixture was heated and stirred at 100°C to dissolve. Here, the amount of molybdenum metal was 90mol% of the total metal, and the molar ratio of total metal / citric acid / ethylene glycol was 1 / 2 / 8. The mixture was then heated at 150°C until it became a viscous polymer-like solid. The heating temperature was gradually increased to 350°C, and the polymer was carbonized to obtain a catalyst precursor. The obtained catalyst precursor was heated in a muffle furnace from room temperature (25°C) to 500°C over 50 minutes in an air atmosphere, and then calcined at 500°C for 6 hours to prepare an ammoxidation catalyst. It was then ground in a mortar to obtain catalyst 1, which is a mixed oxide of molybdenum and titanium containing 90 mol% molybdenum.
[0028] <Other catalysts 2-7> A catalyst was produced in the same manner as in the synthesis example of a mixed oxide catalyst of molybdenum and titanium containing 90 mol % of molybdenum, except that the amounts of ammonium molybdate (para) tetrahydrate and titanium chloride were as shown in Table 1. (No titanium (IV) chloride solution was added to catalyst 6.) In this way, mixed oxide catalysts of molybdenum and titanium with different molybdenum ratios were obtained, 2 to 7.
[0029] [Table 1]
[0030] [Catalyst analysis] For catalysts 1 to 5, composition analysis was performed by the fundamental parameter (FP) method using an XRF (X-ray fluorescence analyzer) (manufactured by Rigaku Corporation, product name: X-ray fluorescence analyzer RIGAKU ZSX PrimusIV), and the molybdenum metal content [mol%] and titanium content [mol%] relative to the total metals were calculated. In addition, the specific surface area of catalysts 1 to 5 was measured by the BET one-point method using nitrogen adsorption using a specific surface area measurement device (manufactured by Microtrack Bell Corporation, product name: BELSORP MINI II). The results obtained are shown in Table 1 below.
[0031] [Table 2]
[0032] [Production of hydrogen cyanide] In the following examples and comparative examples, a normal pressure fixed bed flow type reactor was used as the reactor. The reactor tube was a stainless steel tube with an outer diameter of 19.1 mm and a length of 27.0 mm, into which a stainless steel tube with an outer diameter of 3.0 mm was inserted and fixed so that the reaction temperature in the catalyst layer could be measured. The reactor tube was heated from the outside with a silicone oil bath.
[0033] Example 1 The reaction tube was filled with 1.0 g of the mixed oxide catalyst 1 of molybdenum and titanium containing 90 mol% of molybdenum prepared above, and the flow rates of oxygen gas and nitrogen gas were adjusted. After passing through a vaporizer heated to 200°C, the gas was sent to the catalyst layer from the side of the reactor. The temperature of the catalyst layer at this time was 230°C, which was the reaction start temperature. After the temperature stabilized, methanol gasified through a vaporizer heated to 200°C was additionally sent to the catalyst layer. At this time, the reaction temperature rose due to the oxidation of methanol, and the catalyst layer temperature (methanol oxidation reaction temperature) reached 313°C. The total amount of the supplied gas was CH3OH:O2:N2=1:1.2:6.7 at a supply composition (molar ratio) of 196 mL / min.
[0034] Next, after the temperature had stabilized, ammonia gasified by passing it through a vaporizer heated to 200°C was added to the mixed gas containing oxygen gas, nitrogen gas, and methanol, and the resulting mixture was sent to the catalyst layer as the raw material mixed gas. The reaction temperature rose due to the ammoxidation of methanol, and the catalyst layer temperature (methanol ammoxidation reaction temperature) reached 338°C. The total amount of the raw material mixed gas was CH3OH:NH3:O2:N2=1:1.1:1.2:6.7 in terms of feed composition (molar ratio) at 220mL / min. The gas hourly space velocity (SV) was 4519Hr -1 The contact time between the raw material mixed gas and the catalyst was 0.44 seconds. The reaction gas passing through the reaction tube was trapped with an acidic aqueous solution of hydrochloric acid, and the gas passing through the trap was collected. The reaction gas was analyzed. 82.0% of the methanol fed in was reacted and converted to hydrogen cyanide. The yield of hydrogen cyanide was 62.1%.
[0035] (Examples 2 to 5, Comparative Examples 1 to 2) Hydrogen cyanide was obtained by carrying out a reaction in the same manner as in Example 1, except that catalysts 2 to 7 having different molybdenum ratios were used instead of catalyst 1. The results are shown in Table 3 together with the results of Example 1.
[0036] [Methanol conversion rate] The methanol conversion was calculated from the following formula (1). Conversion rate of methanol (%) = Concentration of reacted methanol (mol%) / Concentration of supplied methanol (mol%) × 100 (1)
[0037] [Hydrogen cyanide yield] The yield of hydrogen cyanide (HCN) was calculated from the following formula (2). Hydrogen cyanide yield (%) = hydrogen cyanide concentration (mol%) produced / methanol concentration (mol%) fed x 100 (2)
[0038] [Selectivity for hydrogen cyanide] The selectivity of hydrogen cyanide (HCN) was calculated from the following formula (3). Selectivity of hydrogen cyanide (%) = yield of hydrogen cyanide (%) / conversion of methanol (%) × 100 (3)
[0039] [Table 3]
Claims
1. A step (A) of reacting methanol and oxygen in a gas phase while supplying them to a reactor in the presence of a catalyst containing an oxide of molybdenum; Following the step (A), a step (B) is performed in a gas phase while supplying methanol, oxygen, and ammonia to the reactor, 1. A method for producing hydrogen cyanide, comprising the steps of: (A) and (B) being carried out in a flow manner in the presence of a mixed oxide catalyst of molybdenum and titanium, the mixed oxide catalyst having a molybdenum content of more than 50 mol % and not more than 97 mol % relative to the total amount of molybdenum and titanium.
2. In the step (A), the reaction initiation temperature is 200 to 300° C., 2. The method for producing hydrogen cyanide according to claim 1, wherein the reaction temperature of the ammoxidation reaction in the step (B) is 270 to 600° C.
3. In the step (A), the reaction between the methanol and oxygen is started in a heated state using a heat transfer medium. The method for producing hydrogen cyanide according to claim 1 or 2.
4. The method for producing hydrogen cyanide according to claim 3, wherein the gas phase reactions in the steps (A) and (B) are carried out in a fixed bed flow type reactor.
Citation Information
Patent Citations
Preparation method capable of improving yield of hydrocyanic acid
CN107500313A
Iron-antimony-molybdenum-containing oxide catalyst composition and its manufacture
JP1992118051A
Catalyst compositions and methods for the direct production of hydrogen cyanide in acrylonitrile reactor feed streams
JP2019502546A
Ammoxidation of methanol to produce hydrogen cyanide
US4485079A
Production of hydrocyanic acid
JP1995206427A