Method for curing ultraviolet curable resin composition and method for manufacturing laminate
A two-step UV-LED irradiation process with specific wavelength ranges and photopolymerization initiators addresses the power consumption and reaction rate issues in UV-LED devices, enhancing the curing efficiency of ultraviolet curable resin compositions.
Patent Information
- Application Number
- JP2023062522
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
UV-LED irradiation devices with densely integrated UV-LED chips of 300 nm or less increase power consumption and environmental burden, while reducing the number of chips decreases the reaction rate of ultraviolet curable resin compositions.
A method involving a two-step irradiation process using UV-LED devices with different wavelength ranges (250-300 nm and 350-400 nm) to cure ultraviolet curable resin compositions, incorporating photopolymerization initiators with specific absorption wavelengths, to balance power consumption and reaction rate.
The method effectively suppresses power consumption and enhances the reaction rate of ultraviolet curable resin compositions, improving the physical properties of cured products.
Smart Images

Figure 2024148930000002 
Figure 2024148930000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for curing an ultraviolet-curable resin composition and a method for producing a laminate. [Background technology]
[0002] Articles containing a cured product of an ultraviolet-curable resin composition are widely used in optical material applications, building material applications, etc. Such articles can be produced, for example, by forming a coating film containing an ultraviolet-curable resin composition on a substrate, and then irradiating the coating film with ultraviolet light to cure the ultraviolet-curable resin composition.
[0003] Conventionally, ultraviolet irradiation devices that include ultraviolet lamps using mercury, such as low-pressure mercury lamps and high-pressure mercury lamps, have been used as ultraviolet irradiation devices because they can increase the irradiation intensity of ultraviolet rays. However, ultraviolet irradiation devices including ultraviolet lamps using mercury have problems in that they place a large burden on the environment due to the use of mercury, and they also have problems in that they consume a large amount of energy.
[0004] For this reason, a method of irradiating ultraviolet rays using an irradiation device including a UV-LED chip has been proposed (Patent Documents 1 and 2). A UV-LED chip is an LED chip that emits ultraviolet rays. An LED chip is the smallest component unit that functions as an LED. In this specification, an "irradiation device including a UV-LED chip" may be referred to as a "UV-LED irradiation device." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-112986 A [Patent Document 2] JP 2015-166770 A Summary of the Invention [Problem to be solved by the invention]
[0006] The ultraviolet-curable resin composition contains an ultraviolet-curable compound and a photopolymerization initiator. Most photopolymerization initiators have a maximum absorption wavelength of 300 nm or less. Therefore, in order to cure the ultraviolet-curable resin composition using a UV-LED irradiation device, it is necessary to use a UV-LED chip with an emission peak wavelength (center wavelength) of 300 nm or less. However, UV-LED chips with a central wavelength of 300 nm or less have low output. Therefore, in the current situation, it is necessary to irradiate ultraviolet rays using a UV-LED irradiation device in which UV-LED chips with a central wavelength of 300 nm or less are densely integrated. However, when a UV-LED irradiation device in which UV-LED chips are densely integrated is used, there is a problem that power consumption increases and the environmental load cannot be reduced. On the other hand, when the number of UV-LED chips is reduced, the reaction rate of the ultraviolet-curable resin composition cannot be increased. Patent Documents 1 and 2 do not consider these problems at all.
[0007] The present disclosure has been made in consideration of the above-mentioned circumstances, and aims to provide a method for curing an ultraviolet-curable resin composition using a UV-LED irradiation device, which can reduce power consumption and improve the reaction rate of the ultraviolet-curable resin composition. [Means for solving the problem]
[0008] The present disclosure provides the following [1] to [2]. [1] A method for curing an ultraviolet-curable resin composition containing an ultraviolet-curable compound and a photopolymerization initiator by irradiating the composition with ultraviolet light, comprising the steps of: The photopolymerization initiator includes a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less, A method for curing an ultraviolet-curable resin composition, comprising the following first and second steps: -First step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device. [2] A coating step of coating a functional layer ink containing an ultraviolet-curable resin composition containing an ultraviolet-curable compound and a photopolymerization initiator on a substrate to form a coating film containing the ultraviolet-curable resin composition; and a curing step of irradiating the coating film with ultraviolet light to cure the ultraviolet-curable resin composition to form a functional layer, As the photopolymerization initiator, a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less is used, A method for producing a laminate, wherein the curing step includes the following first and second steps: -First step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide a method for curing an ultraviolet-curable resin composition, which can reduce power consumption and improve the reaction rate of the ultraviolet-curable resin composition. Also, according to the present disclosure, it is possible to provide a method for manufacturing a laminate, which can reduce power consumption and improve the reaction rate of the ultraviolet-curable resin composition. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram for explaining a method for curing an ultraviolet-curable resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, embodiments of the present disclosure will be described.
[0012] [Method of curing ultraviolet-curable resin composition] The method for curing the ultraviolet-curable resin composition of the present disclosure includes the steps of: A method for curing an ultraviolet-curable resin composition containing an ultraviolet-curable compound and a photopolymerization initiator by irradiating the composition with ultraviolet light, comprising the steps of: The photopolymerization initiator includes a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less, The method includes the following first and second steps. -First step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device.
[0013] FIG. 1 is a diagram for explaining the curing method of the ultraviolet curable resin composition of the present disclosure. In FIG. 1, a coating film containing an ultraviolet curable resin composition is formed on a substrate 10 by a coating device 200. In FIG. 1, after forming a coating film on the substrate 10, the ultraviolet curable resin composition contained in the coating film is cured by irradiating ultraviolet rays by UV-LED irradiation devices 301 and 302 to form a functional layer 20. In FIG. 1, a laminate 100 having a functional layer 20 on the substrate 10 is obtained. Reference numerals 401 and 402 in FIG. 1 denote conveying rolls.
[0014] <Ultraviolet curable resin composition> The ultraviolet-curable resin composition contains an ultraviolet-curable compound and a photopolymerization initiator.
[0015] 《Ultraviolet curable compound》 The ultraviolet-curable resin composition of the present disclosure is required to contain an ultraviolet-curable compound. In this specification, the ultraviolet-curable compound refers to a compound having an ultraviolet-curable functional group, such as an ethylenically unsaturated bond group such as a (meth)acryloyl group, a vinyl group, or an allyl group, an epoxy group, or an oxetanyl group. The ultraviolet curable compound is preferably a compound having an ethylenically unsaturated bond group, more preferably a compound having two or more ethylenically unsaturated bond groups, and even more preferably a compound having two or more (meth)acryloyl groups. In this specification, a compound having two or more (meth)acryloyl groups is referred to as a polyfunctional (meth)acrylate compound. As the polyfunctional (meth)acrylate compound, either a monomer or an oligomer can be used.
[0016] Among the polyfunctional (meth)acrylate compounds, examples of bifunctional (meth)acrylate monomers include ethylene glycol di(meth)acrylate, bisphenol A tetraethoxydiacrylate, bisphenol A tetrapropoxydiacrylate, and 1,6-hexanediol diacrylate. Examples of trifunctional or higher (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and isocyanuric acid-modified tri(meth)acrylate. The (meth)acrylate monomer may have a part of its molecular skeleton modified, for example, with ethylene oxide, propylene oxide, caprolactone, isocyanuric acid, alkyl, cyclic alkyl, aromatic, bisphenol, or the like.
[0017] Examples of the polyfunctional (meth)acrylate oligomer include acrylate polymers such as urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, and polyether (meth)acrylate. The urethane (meth)acrylate can be obtained, for example, by reacting a polyhydric alcohol and an organic diisocyanate with a hydroxy (meth)acrylate. Preferred epoxy (meth)acrylates are (meth)acrylates obtained by reacting a tri- or higher functional aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like, with (meth)acrylic acid, (meth)acrylates obtained by reacting a di- or higher functional aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like, with a polybasic acid and (meth)acrylic acid, and (meth)acrylates obtained by reacting a di- or higher functional aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like, with a phenol and (meth)acrylic acid.
[0018] The weight average molecular weight of the polyfunctional (meth)acrylate oligomer is preferably 500 or more and 3,000 or less, and more preferably 700 or more and 2,500 or less. In this specification, the weight average molecular weight is an average molecular weight measured by GPC analysis and converted into standard polystyrene.
[0019] <Photopolymerization initiator> The ultraviolet curable resin composition of the present disclosure is required to contain a photopolymerization initiator. Furthermore, the ultraviolet curable resin composition of the present disclosure is required to contain a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less as a photopolymerization initiator. By the ultraviolet curable resin composition containing a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less and performing the first step and the second step, it is possible to suppress power consumption and improve the reaction rate of the ultraviolet curable resin composition. In this specification, the maximum absorption wavelength of the photopolymerization initiator means the wavelength at which the absorbance of the photopolymerization initiator is the highest. In this specification, the maximum absorption wavelength of the photopolymerization initiator is measured in accordance with JIS K0115:2020.
[0020] Examples of the photopolymerization initiator include acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzil dimethyl ketal, benzoyl benzoate, α-acyloxime ester, and thioxanthones.
[0021] The photopolymerization initiator may be one type, or two or more types may be mixed. When two or more types of photopolymerization initiators are contained, the following embodiments (1) to (4) can be mentioned. Among these, the embodiments (3) and (4) are preferable, and the embodiment (4) is more preferable. By using the photopolymerization initiator as the embodiment (4) and performing the first step and the second step, it is possible to suppress power consumption and to easily improve the reaction rate of the ultraviolet curable resin composition. (1) An embodiment including two or more photopolymerization initiators having a maximum absorption wavelength of 250 nm or more and 300 nm or less. (2) An embodiment including a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less, and a photopolymerization initiator having a maximum absorption wavelength of less than 250 nm. (3) An embodiment including a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less, and a photopolymerization initiator having a maximum absorption wavelength of more than 300 nm. (4) An embodiment including a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less, a photopolymerization initiator having a maximum absorption wavelength of less than 250 nm, and a photopolymerization initiator having a maximum absorption wavelength of more than 300 nm.
[0022] In the above embodiment (4), when the content of the photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less is defined as W1, the content of the photopolymerization initiator having a maximum absorption wavelength of less than 250 nm is defined as W2, and the content of the photopolymerization initiator having a maximum absorption wavelength of more than 300 nm is defined as W3, it is preferable that W1 and W2, and W1 and W3 have the following mass ratio. W1:W2 is preferably 1:0.1 to 1:2, more preferably 1:0.3 to 1:1.5, and even more preferably 1:0.5 to 1:1. W1:W3 is preferably 1:0.3 to 1:3, more preferably 1:0.5 to 1:2, and even more preferably 1:0.7 to 1:1.5.
[0023] The photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less preferably has a maximum absorption wavelength of 253 nm or more and 285 nm or less, and more preferably has a maximum absorption wavelength of 255 nm or more and 270 nm or less. A photopolymerization initiator having a maximum absorption wavelength of less than 250 nm preferably has a maximum absorption wavelength of 235 nm or more and less than 250 nm, and more preferably has a maximum absorption wavelength of 240 nm or more and 248 nm or less. A photopolymerization initiator having a maximum absorption wavelength of more than 300 nm preferably has a maximum absorption wavelength of more than 300 nm and not more than 320 nm, more preferably 302 nm or more and not more than 315 nm.
[0024] The full width at half maximum of the absorbance of the photopolymerization initiator is preferably in the following range. By setting the full width at half maximum of the absorbance of the photopolymerization initiator in the following range and performing the first step and the second step, it is possible to suppress power consumption and to easily improve the reaction rate of the ultraviolet-curable resin composition. A photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less preferably has a full width at half maximum of absorbance of 10 nm or more and 50 nm or less, and more preferably 20 nm or more and 40 nm or less. In the case of a photopolymerization initiator having a maximum absorption wavelength of less than 250 nm, the full width at half maximum of absorbance is preferably 10 nm or more and 50 nm or less, and more preferably 20 nm or more and 40 nm or less. In order to facilitate curing of the ultraviolet-curable resin composition in the second step, the photopolymerization initiator having a maximum absorption wavelength of more than 300 nm preferably has a full width at half maximum of absorbance of 10 nm or more and 70 nm or less, more preferably 20 nm or more and 60 nm or less.
[0025] The full width at half maximum (nm) of absorbance of a photopolymerization initiator is represented by the following formula when "the wavelength showing the maximum absorbance of the photopolymerization initiator is λ (nm)", "among the wavelengths showing an absorbance that is 1 / 2 of the maximum value, the wavelength shorter than λ is λ' (nm)", and "among the wavelengths showing an absorbance that is 1 / 2 of the maximum value, the wavelength larger than λ is λ'' (nm)". Full width at half maximum of absorbance of photoinitiator (nm) = λ''-λ'
[0026] The content of the photopolymerization initiator is preferably 0.5 parts by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the ultraviolet-curable compound. When two or more types of photopolymerization initiators are contained, the above-mentioned content range means the total amount of the two or more types of photopolymerization initiators.
[0027] <Photopolymerization accelerator> The ultraviolet-curable resin composition may contain a photopolymerization accelerator. The photopolymerization accelerator can reduce polymerization inhibition caused by air during curing and increase the curing speed. Examples of the photopolymerization accelerator include p-dimethylaminobenzoic acid isoamyl ester and p-dimethylaminobenzoic acid ethyl ester.
[0028] <First step, second step> The method for curing the ultraviolet-curable resin composition of the present disclosure must include the following first and second steps. -First step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device.
[0029] When the ultraviolet-curable resin composition is cured in only the first step, a UV-LED irradiation device in which UV-LED chips with a central wavelength of 300 nm or less are densely integrated is required, making it impossible to reduce power consumption. When the ultraviolet-curable resin composition is cured only in the second step, the reaction rate of the ultraviolet-curable resin composition cannot be increased, and therefore the physical properties of the article containing the cured product of the ultraviolet-curable resin composition cannot be improved. The method for curing an ultraviolet-curable resin composition according to the present disclosure includes a first step and a second step, and therefore can reduce power consumption and improve the reaction rate of the ultraviolet-curable resin composition. In this specification, central wavelength refers to the wavelength that exhibits a maximum value of irradiance.
[0030] The first and second steps are preferably carried out in a nitrogen atmosphere. In this specification, a nitrogen atmosphere means an atmosphere with an oxygen concentration of 0.1% or less.
[0031] The first and second steps may be carried out simultaneously. The first and second steps can be carried out simultaneously by using a UV-LED irradiation device that includes a UV-LED chip with a central wavelength of 250 nm or more and 300 nm or less and a UV-LED chip with a central wavelength of 350 nm or more and 400 nm or less as a UV-LED irradiation device.
[0032] The first step and the second step may be carried out at different times. When the first step and the second step are carried out at different times, the interval between the first step and the second step is preferably 300 seconds or less, more preferably 180 seconds or less, more preferably 120 seconds or less, and more preferably 60 seconds or less, in order to improve the reaction rate of the ultraviolet-curable resin composition. The interval between the first step and the second step means the interval between the end of ultraviolet irradiation in one step and the start of ultraviolet irradiation in the other step.
[0033] When the first step and the second step are carried out at different times, the second step may be carried out after the first step, or the second step may be carried out after the first step. Carrying out the second step after the first step tends to improve the reaction rate of the ultraviolet-curable resin composition. When the first step and the second step are performed at different times, it is preferable to use a first UV-LED irradiation device including a UV-LED chip having a central wavelength of 250 nm or more and 300 nm or less, and a second UV-LED irradiation device including a UV-LED chip having a central wavelength of 350 nm or more and 400 nm or less, as the UV-LED irradiation device.
[0034] The cumulative dose of ultraviolet light in the first step is 1 mJ / cm 2 More than 500mJ / cm 2 Preferably, it is 5 mJ / cm or less. 2 More than 400mJ / cm 2 More preferably, it is 11 mJ / cm or less. 2 More than 300mJ / cm 2 It is even more preferable that: The cumulative dose of ultraviolet light in the first step is 1 mJ / cm 2 By setting the amount of ultraviolet light in the first step to 500 mJ / cm or more, the reaction rate of the ultraviolet-curable resin composition can be easily improved. 2 By setting the following, it becomes easier to suppress power consumption.
[0035] The cumulative amount of ultraviolet light in the second step is 50 mJ / cm 2 More than 3000mJ / cm 2 Preferably, it is 75 mJ / cm or less. 2 More than 2000mJ / cm 2 More preferably, it is 100 mJ / cm or less. 2 More than 1500mJ / cm 2 It is even more preferable that: The cumulative UV light intensity in the second step is 50 mJ / cm 2 By setting the amount of ultraviolet light in the second step to 3000 mJ / cm or more, the reaction rate of the ultraviolet-curable resin composition can be easily improved. 2By setting the following, it becomes easier to suppress power consumption.
[0036] The cumulative amount of ultraviolet light in the first step is X [mJ / cm 2 ], the cumulative amount of ultraviolet light in the second step is Y [mJ / cm 2 When X / Y is defined as: X / Y is preferably 0.0003 or more and 10 or less, more preferably 0.003 or more and 5 or less, and further preferably 0.007 or more and 3 or less. If X / Y is too large, the reaction rate is easily improved, but the power consumption tends to increase. If X / Y is too small, the power consumption is easily reduced, but the reaction rate is easily reduced. Therefore, by setting X / Y in the above range, it is easy to achieve a good balance between the power consumption and the reaction rate of the ultraviolet curable resin composition.
[0037] The integrated amount of ultraviolet light can be adjusted by the arrangement density of the UV-LED chips, the irradiation time of ultraviolet light, etc. In order to suppress variation in the integrated amount of ultraviolet light within the surface, it is preferable to narrow the intervals between the individual UV-LED chips.
[0038] In the first step, the full width at half maximum of the ultraviolet light in the first wavelength range irradiated from the UV-LED irradiation device is preferably 5 nm or more and 30 nm or less, more preferably 7 nm or more and 25 nm or less, and even more preferably 10 nm or more and 20 nm or less. By setting the full width at half maximum of the ultraviolet light in the first wavelength region to 5 nm or more, it is possible to match the absorbance curves of multiple photopolymerization initiators and facilitate reaction. By setting the full width at half maximum of the ultraviolet light in the first wavelength region to 30 nm or less, it is possible to increase the peak irradiance and facilitate reaction.
[0039] The full width at half maximum of ultraviolet light in the first wavelength region is expressed by the following formula when "the wavelength exhibiting the maximum irradiance in the first wavelength region is defined as λ (nm)," "among the wavelengths exhibiting 1 / 2 the maximum irradiance, the wavelength shorter than λ is defined as λ' (nm)," and "among the wavelengths exhibiting 1 / 2 the maximum irradiance, the wavelength larger than λ is defined as λ'' (nm)." "The wavelength exhibiting the maximum irradiance in the first wavelength region" means "the central wavelength of the first wavelength region." Full width at half maximum of ultraviolet light in the first wavelength range (nm) = λ''-λ'
[0040] In the second step, the full width at half maximum of the ultraviolet light in the second wavelength range irradiated from the UV-LED irradiation device is preferably 7 nm or more and 50 nm or less, more preferably 10 nm or more and 40 nm or less, and even more preferably 12 nm or more and 30 nm or less. By setting the full width at half maximum of the ultraviolet light in the second wavelength region to 7 nm or more, when a photopolymerization initiator with a maximum absorption wavelength of more than 300 nm is included, the absorbance curve can be matched, making it easier to react. By setting the full width at half maximum of the ultraviolet light in the second wavelength region to 50 nm or less, the peak irradiance can be increased, making it easier to react.
[0041] The full width at half maximum of ultraviolet light in the second wavelength region is expressed by the following formula when "the wavelength exhibiting the maximum irradiance in the second wavelength region is defined as λ (nm)", "among the wavelengths exhibiting 1 / 2 the maximum irradiance, the wavelength shorter than λ is defined as λ' (nm)", and "among the wavelengths exhibiting 1 / 2 the maximum irradiance, the wavelength larger than λ is defined as λ'' (nm)". "The wavelength exhibiting the maximum irradiance in the second wavelength region" means "the central wavelength of the second wavelength region". Full width at half maximum of ultraviolet light in the second wavelength range (nm) = λ''-λ'
[0042] In the curing method of the ultraviolet curable resin composition of the present disclosure, it is preferable to carry out the first and second steps in a state where a coating film containing the ultraviolet curable resin composition is formed on a substrate. By carrying out the first and second steps in the above-mentioned state, the ultraviolet curable resin composition can be stably cured.
[0043] <Base material> Examples of the substrate include a paper substrate, a fiber substrate, a glass substrate, and a resin substrate. Among these, a resin substrate is preferable. The substrate may be a single layer or a laminate.
[0044] Examples of the resin substrate include substrates containing one or more of resins such as polyester, triacetyl cellulose (TAC), cellulose diacetate, cellulose acetate butyrate, polyamide, polyimide, polyethersulfone, polysulfone, polypropylene, polymethylpentene, polyvinyl chloride, polyvinyl acetal, polyether ketone, polymethyl methacrylate, polycarbonate, polyurethane, and amorphous olefin (Cyclo-Olefin-Polymer: COP).
[0045] In order to improve the adhesion to the ultraviolet-curable resin composition, one or both sides of the substrate may be subjected to a surface treatment such as a physical surface treatment, such as an oxidation method or a roughening method, or a chemical surface treatment.
[0046] The thickness of the substrate may be appropriately selected depending on the desired performance. In order to ensure mechanical properties and improve handling, the thickness of the substrate is usually 10 μm to 200 μm, preferably 20 μm to 150 μm, and more preferably 30 μm to 120 μm. In addition, when a paper substrate is used as the substrate, the basis weight is usually 20 g / m2 to improve handling. 2 More than 150g / m 2 Less than 30 g / m 2 More than 100g / m 2 The following is the result.
[0047] The substrate is preferably a roll-shaped sheet so that it can be fed to a conveying line and processed continuously.
[0048] The coating film containing the ultraviolet-curable resin composition can be formed, for example, by applying an ink for a functional layer, which contains an ultraviolet-curable resin composition containing an ultraviolet-curable compound and a photopolymerization initiator, onto a substrate. A general-purpose coating method can be used to apply the ink.
[0049] The ink for the functional layer may contain a dilution solvent. When the ink contains a solvent, it is preferable to carry out a drying step for drying the solvent before irradiating with ultraviolet light. The ink for the functional layer may contain additives such as a matting agent, a pigment, a dye, a refractive index adjuster, a leveling agent, an antioxidant, and a light stabilizer.
[0050] When the first step and the second step are performed in a state where a coating film containing an ultraviolet-curable resin composition is formed on a substrate, it is preferable to start the first step and / or the second step with the surface temperature of the coating film set to 55° C. or less. That is, it is preferable to adjust the surface temperature of the coating film to 55° C. or less before performing the first step and / or the second step. In the first and second steps, heat is generated by irradiation with ultraviolet rays, which may damage or deform the substrate. For this reason, by setting the surface temperature of the coating film to 55° C. or less, damage to the substrate can be easily suppressed. In order to more easily suppress damage to the substrate, it is preferable to set the surface temperature of the coating film to 55° C. or less in the first and second steps. On the other hand, if the surface temperature of the coating film is too low, the reaction rate of the ultraviolet-curable resin composition tends to be low. Therefore, it is preferable to perform the first step and / or the second step with the surface temperature of the coating film set to 15° C. or higher. In order to more easily suppress the decrease in the reaction rate of the ultraviolet-curable resin composition, it is preferable to set the surface temperature of the coating film to 15° C. or higher in the first step and the second step. In the first step and / or the second step, the surface temperature of the coating film is more preferably 15°C or higher and 55°C or lower, and further preferably 20°C or higher and 50°C or lower.
[0051] The surface temperature of the coating film can be adjusted, for example, by increasing or decreasing the temperature of the transport roll.
[0052] [Method of manufacturing laminate] The method for producing a laminate according to the present disclosure includes: A coating step of coating a functional layer ink containing an ultraviolet-curable resin composition containing an ultraviolet-curable compound and a photopolymerization initiator on a substrate to form a coating film containing the ultraviolet-curable resin composition; and a curing step of irradiating the coating film with ultraviolet light to cure the ultraviolet-curable resin composition to form a functional layer, As the photopolymerization initiator, a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less is used, The curing step includes the following first and second steps. -First step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device.
[0053] The means for applying the ink for the functional layer onto the substrate can be a general-purpose coating means. When the ink for the functional layer contains a dilution solvent, it is preferable to carry out a drying step for drying off the solvent between the coating step and the curing step. The ink for the functional layer may contain additives such as a matting agent, a pigment, a dye, a refractive index adjuster, a leveling agent, an antioxidant, and a light stabilizer.
[0054] Examples of the functional layer include a hard coat layer, an antiglare layer, a low reflection layer, an antistatic layer, and an antifouling layer. The thickness of the functional layer is not particularly limited, but is preferably from 0.05 μm to 100 μm, and more preferably from 0.1 μm to 50 μm.
[0055] In the method for producing a laminate according to the present disclosure, embodiments of the substrate, the ultraviolet-curable compound, the photopolymerization initiator, the ultraviolet-curable resin composition, the ink, the first step, the second step, and the like may be similar to those of the above-described method for curing an ultraviolet-curable resin composition according to the present disclosure. For example, in the method for producing a laminate of the present disclosure, examples of the substrate include a paper substrate, a fiber substrate, a glass substrate, a resin substrate, and the like, and among these, a resin substrate is preferred. In the method for producing a laminate according to the present disclosure, the integrated amount of ultraviolet light in the first step is X [mJ / cm 2 ], the cumulative amount of ultraviolet light in the second step is Y [mJ / cm 2 When X / Y is defined as: X / Y is preferably 0.0003 or more and 10 or less, more preferably 0.003 or more and 5 or less, and further preferably 0.007 or more and 3 or less.
[0056] In the method for producing a laminate of the present disclosure, the laminate may have another layer other than the substrate and the functional layer. The other layer may be located between the substrate and the functional layer, or may be located on the opposite side of the functional layer from the substrate. The other layer may be a layer containing a cured product of an ultraviolet-curable resin composition.
[0057] This disclosure includes the following [1] to
[13] . [1] A method for curing an ultraviolet-curable resin composition containing an ultraviolet-curable compound and a photopolymerization initiator by irradiating the composition with ultraviolet light, comprising the steps of: The photopolymerization initiator includes a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less, A method for curing an ultraviolet-curable resin composition, comprising the following first and second steps: -First step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device. [2] The method for curing an ultraviolet-curable resin composition according to [1], wherein the first step and the second step are carried out simultaneously. [3] The method for curing an ultraviolet-curable resin composition according to [1], wherein the first step and the second step are carried out at different times. [4] The method for curing an ultraviolet-curable resin composition according to [3], wherein the second step is carried out after the first step. [5] The method for curing an ultraviolet-curable resin composition according to [3] or [4], wherein an interval between the first step and the second step is 300 seconds or less. [6] The integrated amount of ultraviolet light in the first step is 1 mJ / cm 2 More than 500mJ / cm 2 The method for curing an ultraviolet-curable resin composition according to any one of [1] to [5] below. [7] The cumulative amount of ultraviolet light in the second step is 50 mJ / cm 2 More than 3000mJ / cm 2 The method for curing an ultraviolet-curable resin composition according to any one of [1] to [6] below. [8] The cumulative amount of ultraviolet light in the first step is X [mJ / cm 2 ], the integrated amount of ultraviolet light in the second step is Y [mJ / cm 2 [8] The method for curing an ultraviolet ray curable resin composition according to any one of [1] to [7], wherein X / Y is 0.0003 or more and 10 or less when X / Y is defined as [9] The method for curing an ultraviolet-curable resin composition according to any one of [1] to [8], wherein in the first step, a full width at half maximum of the ultraviolet light in the first wavelength region irradiated from the UV-LED irradiation device is 5 nm or more and 30 nm or less.
[10] The method for curing an ultraviolet-curable resin composition according to any one of [1] to [9], wherein in the second step, a full width at half maximum of the ultraviolet light in the second wavelength region irradiated from the UV-LED irradiation device is 7 nm or more and 50 nm or less.
[11] The method for curing an ultraviolet-curable resin composition according to any one of [1] to
[10] , wherein the first step and the second step are carried out in a state in which a coating film containing the ultraviolet-curable resin composition is formed on a substrate.
[12] The method for curing an ultraviolet-curable resin composition according to
[11] , wherein the surface temperature of the coating film is set to 55° C. or lower before starting the first step and / or the second step.
[13] A coating step of coating a functional layer ink containing an ultraviolet-curable resin composition containing an ultraviolet-curable compound and a photopolymerization initiator on a substrate to form a coating film containing the ultraviolet-curable resin composition; and a curing step of irradiating the coating film with ultraviolet light to cure the ultraviolet-curable resin composition to form a functional layer, As the photopolymerization initiator, a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less is used, A method for producing a laminate, wherein the curing step includes the following first and second steps: -First step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device. EXAMPLES
[0058] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to these examples in any way.
[0059] 1. Measurement and Evaluation The following measurements and evaluations were carried out for the curing methods of the ultraviolet-curable resin compositions and the manufacturing methods of the laminates of the Examples and Comparative Examples. Unless otherwise specified, the atmosphere during each measurement and evaluation was a temperature of 23±5°C and a relative humidity of 40% to 65%. Before starting each measurement and evaluation, the target sample was exposed to the above atmosphere for 30 minutes to 60 minutes, and then the measurement and evaluation were performed.
[0060] 1-1. Response rate For the surface of the functional layer side of the laminates obtained in the examples and comparative examples, 820 to 800 cm corresponding to the C=C stretching vibration of the unsaturated hydrocarbon group in the polymerizable group was measured. -1 The peak intensity was measured before and after ultraviolet irradiation (=peak intensity after completion of the first and second steps). The reaction rate was calculated as follows. A reaction rate of 30% or more is acceptable, preferably 35% or more, and more preferably 40% or more. <Calculation of reaction rate> Regarding the ultraviolet-curable resin composition after ultraviolet irradiation, the 820 to 800 cm corresponding to the C=C stretching vibration of the unsaturated hydrocarbon group in the polymerizable group -1 The peak intensity of X is 1780 to 1650 cm corresponding to the C=O stretching vibration of the ester group in the polymerizable group. -1 The peak intensity of the ultraviolet-curable resin composition before ultraviolet irradiation is defined as Y. The peak intensity of the ultraviolet-curable resin composition before ultraviolet irradiation is defined as Y. -1 The peak intensity of X* is the peak intensity of 1780 to 1650 cm corresponding to the C=O stretching vibration of the ester group in the polymerizable group. -1 The peak intensity of is Y*. Under these conditions, the reaction rate can be calculated using the following formula: Reaction rate (%)=(1-(X / Y) / (X* / Y*))×100
[0061] 1-2.Power consumption The power consumption due to ultraviolet light irradiation was evaluated according to the following criteria. A:Using a UV-LED irradiation device, power consumption is less than 2,800 watts. B: Using a UV-LED irradiation device, power consumption is more than 2,800 watts and less than 3,400 watts. C: Using a UV-LED irradiation device, power consumption is over 3,400 watts. D: Uses ultra-high pressure mercury lamps, consuming more than 6,000 watts of power.
[0062] 1-3.Pencil hardness The laminates obtained in the examples and comparative examples were cut into samples measuring 5 cm x 10 cm. Unless otherwise noted, the pencil hardness of the functional layer side of the samples was measured in accordance with JIS K5600-5-4:1999. The load during measurement was 500 g, and the speed was 1.4 mm / sec. A pencil hardness tester (product number: NP-type pencil scratch coating hardness tester) manufactured by Toyo Seiki Seisakusho was used for the measurement. Both ends of the cut sample were attached to the base of the pencil hardness tester using mending tape (3M, product number "810-3-18"). Five pencil hardness tests were performed, and the hardness at which no appearance abnormality such as scratches was observed four or more times was taken as the pencil hardness value of each sample. For example, five tests were performed using a 2H pencil, and if no appearance abnormality occurred four times, the pencil hardness of the antiglare laminate was 2H. Appearance abnormalities were checked for scratches and dents, not including discoloration. A pencil hardness of 2H or more was the pass level.
[0063] 2. Curing of UV-curable resin composition and production of laminate [Example 1] A triacetyl cellulose resin film (manufactured by Fujifilm Corporation, product name: TD80UL) having a thickness of 80 μm was used as a substrate. The following ultraviolet-curable resin composition was applied onto the substrate to form a coating film containing the ultraviolet-curable resin composition. The coating film was then dried at 70° C. for 1 minute. Next, the first step was carried out as the first UV irradiation from the coating film side. The temperature of the coating film surface at the start of the first step was 25°C. 60 seconds after the UV irradiation in the first step was completed, the second step was carried out as the second UV irradiation. The temperature of the coating film surface at the start of the second step was 25°C. The UV-curable resin composition in the coating film formed on the substrate was cured by the first and second steps to obtain a functional layer having a functional layer on the substrate. The thickness of the functional layer was 5 μm. <First step> A process in which ultraviolet light is irradiated for 3 seconds using a first UV-LED irradiation device (central wavelength 280 nm, full width at half maximum 15 nm). The cumulative amount of ultraviolet light in the first process is 200 mJ / cm 2 . <Second step> A process in which ultraviolet light is irradiated for 3 seconds using a second UV-LED irradiation device (central wavelength 365 nm, full width at half maximum 20 nm). The cumulative amount of ultraviolet light in the second process is 500 mJ / cm 2 .
[0064] <Ultraviolet curable resin composition> Urethane acrylate 60 parts by weight (Product name: UV1700B, manufactured by Mitsubishi Chemical Corporation, 10 functional groups) Pentaerythritol triacrylate 40 parts by weight ·Organic particles 3 parts by mass (Spherical polyacrylic-styrene copolymer, average particle size 2.0 μm, refractive index 1.55) Silica particles 1 part by weight (Fumed silica, manufactured by Nippon Aerosil Co., Ltd., average primary particle size: 12 nm) Photopolymerization initiator 2 parts by weight (ESACUREONE, Lamberti, maximum absorption wavelength: 260 nm, full width at half maximum of absorbance: 32 nm) Photopolymerization initiator 1 part by weight (Product name "Omnirad184", IGM Resins BV, maximum absorption wavelength: 245 nm, full width at half maximum of absorbance: 25 nm) Photopolymerization initiator 1.5 parts by weight (Product name "Omnirad907", IGM Resins BV, maximum absorption wavelength: 305 nm, full width at half maximum of absorbance: 42 nm) Silicone leveling agent 0.1 parts (Product name: TSF4460, Momentive Performance Materials, Inc.) Toluene 100 parts by weight 30 parts by weight of isopropyl alcohol Cyclohexanone 15 parts by weight
[0065] [Examples 2 to 8 and Comparative Examples 1 to 3] The curing method of the ultraviolet-curable resin composition and the manufacturing method of the laminate of Examples 2 to 8 and Comparative Examples 1 to 3 were carried out in the same manner as in Example 1, except that the ultraviolet irradiation conditions were changed to those in Table 1.
[0066] [Table 1]
[0067] From the results in Table 1, it can be confirmed that the method for curing the ultraviolet-curable resin composition and the method for producing the laminate of the examples can reduce power consumption and improve the reaction rate of the ultraviolet-curable resin composition. [Explanation of symbols]
[0068] 10: Base material 20: Functional layer 100: Laminate 200: Coating device 301:UV-LED irradiation device 302:UV-LED irradiation device
Claims
1. A method for curing an ultraviolet-curable resin composition containing an ultraviolet-curable compound and a photopolymerization initiator by irradiating the composition with ultraviolet light, comprising the steps of: The photopolymerization initiator includes a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less, A method for curing an ultraviolet-curable resin composition, comprising the following first and second steps: --First step-- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device.
2. The method for curing an ultraviolet ray curable resin composition according to claim 1 , wherein the first step and the second step are carried out simultaneously.
3. The method for curing an ultraviolet ray curable resin composition according to claim 1 , wherein the first step and the second step are carried out at different times.
4. The method for curing an ultraviolet-curable resin composition according to claim 3 , wherein the second step is carried out after the first step.
5. 5. The method for curing an ultraviolet ray curable resin composition according to claim 3, wherein an interval between the first step and the second step is 300 seconds or less.
6. The integrated amount of ultraviolet light in the first step is 1 mJ / cm 2 More than 500mJ / cm 2 2. A method for curing the ultraviolet-curable resin composition according to claim 1, wherein the ultraviolet-curable resin composition is:
7. The integrated amount of ultraviolet light in the second step is 50 mJ / cm 2 More than 3000mJ / cm 2 2. A method for curing the ultraviolet-curable resin composition according to claim 1, wherein the ultraviolet-curable resin composition is:
8. The integrated amount of ultraviolet light in the first step is X [mJ / cm 2 ], the integrated amount of ultraviolet light in the second step is Y [mJ / cm 2 2. The method for curing an ultraviolet ray curable resin composition according to claim 1, wherein X / Y is 0.0003 or more and 10 or less when X / Y is defined as the sum of X / Y and Y / Y.
9. 2. The method for curing an ultraviolet ray curable resin composition according to claim 1, wherein in the first step, a full width at half maximum of the ultraviolet ray in the first wavelength region irradiated from the UV-LED irradiation device is 5 nm or more and 30 nm or less.
10. 2. The method for curing an ultraviolet ray curable resin composition according to claim 1, wherein in the second step, the full width at half maximum of the ultraviolet ray in the second wavelength region irradiated from the UV-LED irradiation device is 7 nm or more and 50 nm or less.
11. 2. The method for curing an ultraviolet-curable resin composition according to claim 1, wherein the first step and the second step are performed in a state where a coating film containing the ultraviolet-curable resin composition is formed on a substrate.
12. The method for curing an ultraviolet ray curable resin composition according to claim 11, wherein the first step and / or the second step is started with the surface temperature of the coating film being set to 55°C or less.
13. A coating step of coating a functional layer ink containing an ultraviolet curable resin composition containing an ultraviolet curable compound and a photopolymerization initiator on a substrate to form a coating film containing the ultraviolet curable resin composition; and a curing step of irradiating the coating film with ultraviolet light to cure the ultraviolet-curable resin composition to form a functional layer, As the photopolymerization initiator, a photopolymerization initiator having a maximum absorption wavelength of 250 nm or more and 300 nm or less is used, A method for producing a laminate, wherein the curing step includes the following first and second steps: --First step-- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a first wavelength range having a center wavelength of 250 nm or more and 300 nm or less by a UV-LED irradiation device. -Second step- A step of irradiating the ultraviolet-curable resin composition with ultraviolet light in a second wavelength range having a center wavelength of 350 nm or more and 400 nm or less by a UV-LED irradiation device.
Citation Information
Patent Citations
Method for producing optical film, optical film production device, optical film and liquid crystal display
JP2010112986A
Ultra violet radiation apparatus and method of manufacturing optical film
JP2015166770A
Cited By
Method for curing UV-curable resin compositions and UV irradiation apparatus for curing UV-curable resin compositions
JP2026130789A