Laminated film
The laminated film with a propylene homopolymer and petroleum resin intermediate layer, and ethylene/propylene resin seal layer addresses stretching unevenness and lubricity issues, enhancing processing stability and sealing strength for food packaging.
Patent Information
- Application Number
- JP2023062540
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing laminated films face issues with stretching unevenness in the Machine Direction (MD) and lack of sufficient lubricity, making them difficult to process, as highlighted in Patent Document 1.
A laminated film structure comprising a base layer made of propylene homopolymer, an intermediate layer with a specific weight percent concentration of propylene homopolymer (65 wt% to 99.5 wt%) and petroleum resin (0.5 wt% to 35 wt%), and a seal layer with ethylene resin (80 wt% to 99.5 wt%) and propylene resin (0.5 wt% to 20 wt%) to ensure lubricity and prevent stretching unevenness and adhesion to stretching rolls.
The film achieves reduced stretching unevenness and improved lubricity, ensuring stable processing and heat sealing strength, while maintaining low gas permeability for food preservation.
Smart Images

Figure 2024148942000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated film. [Background technology]
[0002] Japanese Patent Laid-Open Publication No. 9-99525 (Patent Document 1) discloses a thermally adhesive laminated polyolefin film, which includes a layer made of a crystalline polypropylene resin and a layer made of a copolymer of ethylene and a vinyl compound (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 9-99525 Summary of the Invention [Problem to be solved by the invention]
[0004] The manufacturing process of a laminated film may include a stretching step in the MD (Machine Direction). Stretching in the MD is performed, for example, to impart stiffness to the laminated film. For example, in a laminated film that has been subjected to a stretching step in the MD, streaks (uneven stretching) extending in the TD (Transverse Direction) may occur. Furthermore, if a certain degree of lubricity is not ensured in the laminated film, it becomes difficult to process the laminated film. The above-mentioned Patent Document 1 does not disclose a means for solving such problems.
[0005] The present invention has been made to solve such problems, and its object is to provide a laminated film that has a certain degree of lubricity and is less likely to suffer from stretching unevenness during the MD stretching process. [Means for solving the problem]
[0006] The laminated film according to the present invention comprises a base layer, an intermediate layer, and a seal layer. The base layer is made of a propylene homopolymer. The intermediate layer is made of a propylene homopolymer and a petroleum resin. In the intermediate layer, the weight percent concentration of the propylene homopolymer is 65 wt% or more and 99.5 wt% or less, and the weight percent concentration of the petroleum resin is 0.5 wt% or more and 35 wt% or less.
[0007] The inventors have found that when the weight percent concentration of the propylene homopolymer is 65wt% or more and 99.5wt% or less and the weight percent concentration of the petroleum resin is 0.5wt% or more and 35wt% or less in the intermediate layer of the laminated film, the laminated film can have a certain degree of lubricity and can suppress the occurrence of stretching unevenness in the MD. In the intermediate layer of the laminated film according to the present invention, the weight percent concentration of the propylene homopolymer is 65wt% or more and 99.5wt% or less and the weight percent concentration of the petroleum resin is 0.5wt% or more and 35wt% or less. Therefore, this laminated film can suppress the occurrence of stretching unevenness while ensuring a certain degree of lubricity.
[0008] In the above laminated film, the sealing layer may be composed of an ethylene-based resin and a propylene-based resin, and in the sealing layer, the weight percentage concentration of the ethylene-based resin may be 80 wt% or more and 99.5 wt% or less, and the weight percentage concentration of the propylene-based resin may be 0.5 wt% or more and 20 wt% or less.
[0009] The inventors have found that when the weight percent concentration of the ethylene-based resin in the seal layer is 80wt% or more and 99.5wt% or less, and the weight percent concentration of the propylene-based resin in the seal layer is 0.5wt% or more and 20wt% or less, the heat seal strength of the laminated film is ensured to a certain degree and adhesion of the seal layer to the stretching roll is suppressed. In the seal layer of the laminated film according to the present invention, the weight percent concentration of the ethylene-based resin is 80wt% or more and 99.5wt% or less, and the weight percent concentration of the propylene-based resin is 0.5wt% or more and 20wt% or less. Therefore, with this laminated film, it is possible to suppress adhesion of the seal layer to the stretching roll while ensuring a certain degree of heat seal strength.
[0010] In the intermediate layer included in the laminate film, the weight percent concentration of the petroleum resin may be 3.5 wt % or more and 10 wt % or less.
[0011] The inventors have found that if the weight percent concentration of the petroleum resin in the intermediate layer is 3.5 wt% or more and 10 wt% or less, the lubricity is ensured to a certain extent and the occurrence of stretching unevenness is suppressed. In the intermediate layer of the laminated film according to the present invention, the weight percent concentration of the petroleum resin is 3.5 wt% or more and 10 wt% or less. Therefore, with this laminated film, it is possible to ensure the lubricity and suppress the occurrence of stretching unevenness while suppressing the content of the petroleum resin in the intermediate layer. Effect of the Invention
[0012] According to the present invention, it is possible to provide a laminated film which ensures a certain degree of lubricity and is less susceptible to uneven stretching during the stretching step. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram showing a cross section of a packaging container using a laminated film. [Diagram 2] FIG. 2 is a diagram illustrating a cross section of a laminated film. [Diagram 3]FIG. 13 is a diagram for explaining a problem that may occur if the intermediate layer does not contain petroleum resin. [Figure 4] FIG. 2 is a diagram showing a schematic configuration of a laminated film manufacturing apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment according to one aspect of the present invention (hereinafter also referred to as "the present embodiment") will be described in detail with reference to the drawings. Note that the same or corresponding parts in the drawings are given the same reference numerals and their description will not be repeated. Also, each drawing is drawn in a schematic manner with objects appropriately omitted or exaggerated for ease of understanding.
[0015] [1. Overview] FIG. 1 is a schematic diagram showing a cross section of a packaging container 5 using a laminated film 10 according to the present embodiment. As shown in FIG. 1, the packaging container 5 includes a container body 7 and a laminated film 10. The container body 7 is, for example, a paper cup having a circular shape in a plan view. The inner surface of the container body 7 is, for example, laminated with polyethylene. The edge portion of the container body 7 is warped outward. Since the edge portion is warped outward, the surface (inner surface) of the edge portion of the container body 7 that is laminated with polyethylene faces upward.
[0016] For example, food F1 is contained within the container body 7. One example of the food F1 is a fermented food such as natto. With the food F1 contained within the container body 7, the opening of the container body 7 is covered with a laminated film 10. The laminated film 10 contacts the container body 7 along the entire periphery of the edge portion of the container body 7. The laminated film 10 is heat-sealed to the polyethylene-laminated surface along the entire periphery of the edge portion of the container body 7. In this way, the food F1 is contained within the packaging container 5.
[0017] In this way, the laminated film 10 is used, for example, to package food F1. If the gas permeability of the laminated film 10 is high, the freshness of the food F1 contained in the packaging container 5 will not be adequately maintained. As will be described in detail later, the gas permeability of the laminated film 10 is suppressed to a level sufficient for packaging the food F1. Furthermore, the laminated film 10 has a degree of lubricity that allows sufficient processability. Also, in the stretching process included in the manufacturing process of the laminated film 10, stretching unevenness is unlikely to occur. The laminated film 10 will be described in detail below.
[0018] [2. Structure of laminated film] FIG. 2 is a diagram showing a cross section of the laminated film 10. As shown in FIG. 2, the laminated film 10 includes a base layer 100, an intermediate layer 110, and a seal layer 120. The thickness of the laminated film 10 is, for example, 25 μm or more and 35 μm or less. The thickness of the base layer 100 is, for example, 1.5 μm or more and 2.5 μm or less. The thickness of the intermediate layer 110 is, for example, 21 μm or more and 29 μm or less. The thickness of the seal layer 120 is, for example, 2.5 μm or more and 3.5 μm or less. In the laminated film 10, the intermediate layer 110 is laminated on the base layer 100, and the seal layer 120 is laminated on the intermediate layer 110. That is, in the laminated film 10, the base layer 100 is formed on one side, and the seal layer 120 is formed on the other side. The surface of the laminated film 10 on which the seal layer 120 is formed is heat-sealed to the edge of the container body 7. The intermediate layer 110 is located between the base layer 100 and the seal layer 120 in the thickness direction of the laminated film 10.
[0019] The base layer 100 is composed of, for example, a homopolymer of propylene. The base layer 100 does not necessarily have to be composed of only a homopolymer of propylene, and may contain other components. In the base layer 100, the content of the homopolymer of propylene is 50 wt% or more, preferably 70 wt% or more, more preferably 80 wt% or more, and even more preferably 90 wt% or more. In the base layer 100, the content of the homopolymer of propylene may be 100 wt%. An example of a commercially available product of the homopolymer of propylene is PC412A (manufactured by SunAllomer Co., Ltd.).
[0020] The intermediate layer 110 is composed of, for example, a propylene homopolymer and a petroleum resin. The intermediate layer 110 does not necessarily have to be composed of only a propylene homopolymer and a petroleum resin, and may contain other components. The propylene homopolymer used may be the same as the propylene homopolymer contained in the base layer 100, or may be different.
[0021] Petroleum resins refer to resins made from the C4-C5 fraction (mainly the C5 fraction) or C5-C9 fraction (mainly the C9 fraction) remaining after pyrolysis of naphtha to remove compounds such as ethylene, propylene, and butadiene, and hydrogenated compounds thereof. Examples of such resins include aromatic petroleum resins, aliphatic petroleum resins, aromatic hydrocarbon resin-based petroleum resins, alicyclic saturated hydrocarbon resin-based petroleum resins, copolymers of the above-mentioned petroleum resins, and hydrogenated products of these petroleum resins. Examples of commercially available petroleum resins include Imave (manufactured by Idemitsu Kosan Co., Ltd.), Alcon (manufactured by Arakawa Chemical Industries Co., Ltd.), and Regalite (manufactured by Eastman Co., Ltd.).
[0022] In the intermediate layer 110, the weight percent concentration of the propylene homopolymer is 65 wt% or more and 99.5 wt% or less, and the weight percent concentration of the petroleum resin is 0.5 wt% or more and 35 wt% or less. The weight percent concentration of the petroleum resin in the intermediate layer 110 is preferably 3.5 wt% or more and 10 wt% or less. The reason why the petroleum resin is contained in the intermediate layer 110 will be explained in detail later.
[0023] The seal layer 120 is made of, for example, an ethylene-based resin and a propylene-based resin. Note that the seal layer 120 does not necessarily have to be made of only an ethylene-based resin and a propylene-based resin, and may contain other components.
[0024] Examples of ethylene-based resins include linear low-density polyethylene, branched low-density polyethylene, ethylene-vinyl acetate copolymer, ionomer resin, and mixtures thereof. Furthermore, copolymers of ethylene and α-olefins are also examples of ethylene-based resins. Examples of α-olefins include, but are not limited to, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and the like. The copolymers may be random copolymers or block copolymers. Examples of commercially available ethylene-based resins include EVOLUE (manufactured by Prime Polymer Co., Ltd.), UMERIT (manufactured by Ube Maruzen Polyethylene Co., Ltd.), NOVATEC (manufactured by Japan Polyethylene Co., Ltd.), SUMIKASEN (manufactured by Sumitomo Chemical Co., Ltd.), and NOVATEC (manufactured by Japan Polyethylene Co., Ltd.).
[0025] Examples of the propylene-based resin include propylene copolymers, long-chain branched polypropylenes, and propylene-based elastomers. The seal layer 120 may contain one of these, or may contain two or more of them. The propylene copolymer may be a binary or ternary random copolymer having propylene as the main component and an α-olefin as the copolymerization component. The propylene-based resin may also be a mixture of different propylene-α-olefin random copolymers. As described above, the α-olefin is not particularly limited, but examples thereof include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene. An example of a commercially available propylene-based resin is Waymax (manufactured by Japan Polypropylene Corporation).
[0026] In the seal layer 120, the weight percent concentration of the ethylene-based resin is 80 wt% or more and 99.5 wt% or less, and the weight percent concentration of the propylene-based resin is 0.5 wt% or more and 20 wt% or less. The reason why the propylene-based resin is contained in the seal layer 120 will be explained in detail later. The weight percent concentrations of the ethylene-based resin and the propylene-based resin in the seal layer 120 do not necessarily have to be within this numerical range. In addition, the seal layer 120 does not necessarily have to contain both the ethylene-based resin and the propylene-based resin. For example, the seal layer 120 does not necessarily have to contain the propylene-based resin.
[0027] In the laminated film 10, oxygen (O 2 ) has a gas permeability of, for example, 1860 cm 3 / (m 2 ·24h·atm) and 1700cm 3 / (m 2 24h atm) or less, and 1500cm 3 / (m 2 24h atm) or less, and 1400cm 3 / (m 2 It is even more preferable that the temperature is less than 24h atm.
[0028] In addition, in the laminated film 10, carbon dioxide (CO 2 ) has a gas permeability of, for example, 5260 cm 3 / (m 2 ·24h·atm) and 5000cm 3 / (m 2 24h atm) or less, and 4000cm 3 / (m 2 24h atm) or less, and 3300cm 3 / (m 2 1.24h·atm) or less is even more preferable. In laminated film 10, since intermediate layer 110 contains petroleum resin, the gas permeability of each of oxygen and carbon dioxide is low. Since laminated film 10 has low gas permeability, for example, even when prepared food using vegetables or the like is contained in packaging container 5 (FIG. 1), the freshness of the prepared food is sufficiently maintained.
[0029] Furthermore, regarding the lubricity of the laminate film 10, the dynamic friction coefficient measured when the base layers 100 are brought into contact with each other in accordance with the American Society for Testing and Materials (ASTM) standard D-1894 is 0.6 or less, preferably 0.5 or less, and more preferably 0.4 or less. By satisfying such a standard, the processability of the laminate film 10 during the manufacturing process of the laminate film 10 is sufficiently guaranteed.
[0030] [3. Suppression of uneven stretching] As described above, in the laminate film 10, the petroleum resin is contained in the intermediate layer 110. The reason why the petroleum resin is contained in the intermediate layer 110 will be explained next.
[0031] FIG. 3 is a diagram for explaining a problem that may occur if the intermediate layer 110 does not contain petroleum resin. The manufacturing process of the laminated film 10 will be described in detail later, but the manufacturing process of the laminated film 10 may include a stretching process in MD (Machine Direction). In this figure, the laminated film 10A conveyed downstream from the longitudinal stretching machine 240 is shown from above. The laminated film 10A includes a base layer, an intermediate layer, and a seal layer. The intermediate layer of the laminated film 10A is composed only of a homopolymer of propylene, and does not contain petroleum resin. That is, the laminated film 10A is different from the laminated film 10 according to the present embodiment. Below, the characteristics of the laminated film 10 will be explained by comparing it with the laminated film 10A.
[0032] 3, the laminated film 10 is stretched in the MD by a longitudinal stretching machine 240. The longitudinal stretching machine 240 includes a plurality of stretching rolls 241. The plurality of stretching rolls 241 are lined up in the MD. In the longitudinal stretching machine 240, the downstream stretching roll 241 rotates at a higher speed than the upstream stretching roll 241. This causes the laminated film 10A to be stretched in the MD.
[0033] After the stretching process in the longitudinal stretching machine 240, streaks extending in the TD (transverse direction) may occur in the laminated film 10A. That is, after the stretching process in the longitudinal stretching machine 240, stretching unevenness may occur in the laminated film 10A.
[0034] The present inventor(s) found that the occurrence of stretching unevenness after the MD stretching step can be suppressed by adding a petroleum resin to the intermediate layer 110 of the laminated film 10. This is believed to be because the melting point of petroleum resin is lower than that of a propylene homopolymer, and petroleum resin has the property of being more easily stretched than a propylene homopolymer.
[0035] Furthermore, the inventor(s) found that when the weight percent concentration of the propylene homopolymer is 65 wt% or more and 99.5 wt% or less and the weight percent concentration of the petroleum resin is 0.5 wt% or more and 35 wt% or less in the intermediate layer 110 of the laminated film 10, the laminated film 10 can ensure a certain degree of slippage and can suppress the occurrence of stretching unevenness in the MD. In the intermediate layer 110 of the laminated film 10 according to the present embodiment, the weight percent concentration of the propylene homopolymer is 65 wt% or more and 99.5 wt% or less and the weight percent concentration of the petroleum resin is 0.5 wt% or more and 35 wt% or less. Therefore, according to the laminated film 10, it is possible to suppress the occurrence of stretching unevenness while ensuring a certain degree of slippage.
[0036] In addition, the seal layer of the laminated film 10A is composed only of an ethylene-based resin, and does not contain a propylene-based resin. When the laminated film 10A is stretched in the longitudinal stretching machine 240, the seal layer may adhere to the stretching roll 241.
[0037] The present inventor(s) found that by adding a propylene-based resin to the seal layer 120 of the laminated film 10, adhesion of the seal layer 120 to the stretching roll 241 is suppressed. This is believed to be because the melting point of the propylene-based resin is higher than the melting point of the ethylene-based resin.
[0038] Furthermore, the inventor(s) found that when the weight percent concentration of the ethylene-based resin in the seal layer 120 is 80 wt% or more and 99.5 wt% or less and the weight percent concentration of the propylene-based resin in the seal layer 120 is 0.5 wt% or more and 20 wt% or less, the heat seal strength of the laminated film 10 is ensured to a certain degree and adhesion of the seal layer 120 to the stretching roll 241 is suppressed. In the seal layer 120 of the laminated film 10 according to the present embodiment, the weight percent concentration of the ethylene-based resin is 80 wt% or more and 99.5 wt% or less and the weight percent concentration of the propylene-based resin is 0.5 wt% or more and 20 wt% or less. Therefore, according to the laminated film 10, adhesion of the seal layer 120 to the stretching roll 241 can be suppressed while ensuring a certain degree of heat seal strength.
[0039] [4. Manufacturing method of laminated film] 4 is a diagram showing a schematic configuration of a manufacturing apparatus 20 for the laminated film 10 according to the present embodiment. The laminated film 10 is manufactured by the manufacturing apparatus 20. As shown in FIG. 4, the manufacturing apparatus 20 includes a T-die 200, cast rolls 210 and 220, a longitudinal stretching machine 240, and a transverse stretching machine 250.
[0040] The T-die 200 includes a T-die body 201 and raw material input sections 230, 231, and 232. Raw material for forming the base layer 100 is input into the raw material input section 230. For example, a resin made of a homopolymer of propylene is input into the raw material input section 230. Raw material for forming the intermediate layer 110 is input into the raw material input section 231. For example, a resin made of a homopolymer of propylene and a petroleum resin are input into the raw material input section 231. Raw material for forming the seal layer 120 is input into the raw material input section 232. For example, an ethylene-based resin and a propylene-based resin are input into the raw material input section 232. For example, at least a part of an antiblocking agent, an antistatic agent, and an antioxidant may be further input into each of the raw material input sections 230 and 232. In addition, for example, an antioxidant may be further input into the raw material input section 231.
[0041] The T-die body 201 is configured to co-extrude the raw materials fed through the raw material feed sections 230, 231, and 232, thereby fusing the molten materials fed into each raw material feed section to form a single integrated film (molten material). The cast rolls 210 and 220 are configured to cool the extruded molten material and send it downstream. The longitudinal stretching machine 240 stretches the molten material cooled by the cast rolls 210 and 220 in MD. The transverse stretching machine 250 stretches the laminated film 10 stretched in MD in TD.
[0042] The laminated film 10 that has been subjected to various stretching processes is wound up by a winding roll (not shown) located downstream. Through the manufacturing process in the manufacturing apparatus 20, a roll of the laminated film 10 is manufactured.
[0043] [5. Features] As described above, in the laminated film 10 according to the present embodiment, the weight percent concentration of the propylene homopolymer in the intermediate layer is 65 wt% to 99.5 wt%, and the weight percent concentration of the petroleum resin is 0.5 wt% to 35 wt%. Therefore, the laminated film 10 can suppress the occurrence of uneven stretching while ensuring a certain degree of lubricity.
[0044] The above describes the embodiments of the present invention by way of example. That is, the detailed description and the accompanying drawings are disclosed for the purpose of illustrative description. Therefore, some components described in the detailed description and the accompanying drawings may be non-essential components for solving the problem. Therefore, just because the non-essential components are described in the detailed description and the accompanying drawings, it should not be immediately determined that the non-essential components are essential.
[0045] Furthermore, the above-described embodiment is merely an example of the present invention in every respect. The above-described embodiment can be improved or modified in various ways within the scope of the present invention. In other words, in implementing the present invention, specific configurations can be appropriately adopted according to the embodiment. EXAMPLES
[0046] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0047] [1. Examples and Comparative Examples] The laminated films of Examples 1-11 and Comparative Examples 1-2 were manufactured by the following method. The raw material composition constituting each layer was put into an extruder with a barrel temperature of 160 to 240°C, extruded from a multilayer die at 240°C into a three-layered sheet, and cooled and solidified by a take-up roll at 50°C. Next, the film was roll-drawn 4 times in MD at 90°C, and then stretched 10 times in TD in a tenter at 165°C, and then heat-set at 167°C to obtain a three-layer polypropylene-based laminated film. The total thickness of each of the obtained laminated films was 30 μm. In each laminated film, the thickness of each layer was 25 μm for the intermediate layer, 2 μm for the base layer, and 3 μm for the seal layer.
[0048] In each of the laminated films of Examples 1-5, the sealing layer was made of EVA (Ethylene-Vinyl Acetate), and the base layer was made of a propylene homopolymer. The intermediate layer was made of a propylene homopolymer and a petroleum resin. In each of the laminated films of Examples 1-5, only the weight percent concentration of the petroleum resin in the intermediate layer was different. In each of the laminated films of Examples 1-5, the weight percent concentrations of the petroleum resin in the intermediate layer were 0.5 wt%, 10 wt%, 20 wt%, 30 wt%, and 35 wt%, respectively.
[0049] In each laminate film of Examples 6-11, the sealing layer was composed of EVA and polypropylene-based resin, and the base layer was composed of propylene homopolymer. The intermediate layer was composed of propylene homopolymer and petroleum resin. In each laminate film of Examples 6-11, the weight percent concentration of the petroleum resin in the intermediate layer and the weight percent concentration of the propylene-based resin in the sealing layer were different. In each laminate film of Examples 6-11, the weight percent concentrations of the petroleum resin in the intermediate layer were 30wt%, 2wt%, 3.5wt%, 5wt%, 30wt%, and 30wt%, respectively. In each laminate film of Examples 6-11, the weight percent concentrations of the propylene-based resin in the sealing layer were 0.5wt%, 10wt%, 10wt%, 10wt%, 20wt%, and 25wt%, respectively.
[0050] In the laminated film of Comparative Example 1, the sealing layer was made of EVA, and the base layer was made of a homopolymer of propylene. Also, the intermediate layer was made of a homopolymer of propylene. In the laminated film of Comparative Example 2, the sealing layer was made of EVA, and the base layer was made of a homopolymer of propylene. Also, the intermediate layer was made of a homopolymer of propylene and a petroleum resin. In the laminated film of Comparative Example 2, the weight percent concentration of the petroleum resin in the intermediate layer was 40wt%. The compositions of the laminated films of Examples 1-11 and Comparative Examples 1-2 are shown in Table 1 below.
[0051] [Table 1]
[0052] [2. Various measurements] <2-1. Uneven stretching> The sheet-like film (laminated film) after stretching in MD was visually observed. If the film was produced stably without any streaks in TD, it was rated as "A". If 1 to 3 streaks extending in TD occurred per 1 m of MD, it was rated as "B". If 4 or more streaks extending in TD occurred per 1 m of MD, it was rated as "C".
[0053] <2-2. Contamination of the stretching roll> The sheet-like film was stretched in MD, and if the seal layer did not adhere to the stretching roll in MD and a film was produced stably, it was rated as "A". If the seal layer adhered to the stretching roll in MD to some extent but the film was produced without any problems, it was rated as "B". If the seal layer adhered to the stretching roll in MD or the film was wrapped around the stretching roll in MD, it was rated as "C".
[0054] <2-3. Smoothness> In accordance with the American Society for Testing and Materials (ASTM) standard D-1894, the dynamic friction coefficient was measured with a surface property tester (14FW, manufactured by Shinto Scientific Co., Ltd.) while the base layers of each laminated film were in contact with each other.
[0055] <2-4. Gas permeability> Each laminate film was cut into a 10 cm square to prepare a measurement sample. The oxygen permeability and carbon dioxide permeability of each measurement sample were measured by the differential pressure method using a differential pressure gas permeability measuring device (manufactured by Toyo Seiki Seisakusho Co., Ltd.) under conditions of a set pressure of 101.3 kPa and a set temperature of 23.0°C.
[0056] <2-5. Haze> Four samples of 50 mm x 100 mm were cut out from each laminate film. The haze (%) of each sample was measured using a haze meter (NDH5000, manufactured by Nippon Denshoku Industries Co., Ltd.) according to a method conforming to JIS K-7136. The average value of the four samples for each laminate film was calculated, and the calculated average value was regarded as the haze of each laminate film.
[0057] <2-6. Heat seal strength> The paper material with the polyethylene-treated surface and the laminated film sample were combined and heated for 0.5 seconds under a pressure of 0.26 MPa to fuse the laminated film sample to the paper material. The sealing temperature was 135°C. A heat sealer (HG-100-2, manufactured by Toyo Seiki Seisakusho) was used for the sealing and fusing. The fusion width was TD10mm x MD10mm, and the sample width was TD50mm x MD10mm. One end of the unfused laminated film sample was spread out at 180°, and the strength was measured by peeling the sample at a pulling speed of 200mm / min toward the TD at room temperature using a peel strength tester (HEIDON TYPE:17, manufactured by Shinto Scientific Co., Ltd.). The heat seal strength was calculated by multiplying the obtained result by 1.5.
[0058] [3. Measurement results] The measurement results are shown in Table 2 below.
[0059] [Table 2] As shown in Table 2, the occurrence of stretching unevenness was suppressed in each of the laminate films of Examples 1-11, compared to the laminate film of Comparative Example 1. Furthermore, in each of the laminate films of Examples 1-11, better results were obtained in terms of lubricity, compared to the laminate film of Comparative Example 2. That is, in the intermediate layer, when the weight percent concentration of the propylene homopolymer was 65 wt% or more and 99.5 wt% or less, and the weight percent concentration of the petroleum resin was 0.5 wt% or more and 35 wt% or less, good results were obtained in terms of stretching unevenness and lubricity.
[0060] Furthermore, in each of the laminate films of Examples 6-10, better results were obtained with respect to stretch roll staining compared to Examples 1-5, and better results were obtained with respect to heat seal strength compared to the laminate film of Example 11. That is, in the seal layer, when the weight percent concentration of the ethylene-based resin was 80 wt% or more and 99.5 wt% or less, and the weight percent concentration of the propylene-based resin was 0.5 wt% or more and 20 wt% or less, good results were obtained with respect to stretch roll staining and heat seal strength. [Explanation of symbols]
[0061] 5 packaging container, 7 container body, 10, 10A laminated film, 20 manufacturing apparatus, 100 base layer, 110 intermediate layer, 120 sealing layer, 200 T-die, 201 T-die body, 210, 220 casting roll, 230, 231, 232 raw material input section, 240 longitudinal stretching machine, 241 stretching roll, 250 transverse stretching machine, F1 food, U1 stretching unevenness.
Claims
1. A base layer, an intermediate layer, and a seal layer are provided, The base layer is composed of a propylene homopolymer, the intermediate layer is composed of the propylene homopolymer and a petroleum resin, A laminated film, wherein in the intermediate layer, the weight percent concentration of the propylene homopolymer is 65 wt % or more and 99.5 wt % or less, and the weight percent concentration of the petroleum resin is 0.5 wt % or more and 35 wt % or less.
2. The sealing layer is composed of an ethylene-based resin and a propylene-based resin, 2. The laminated film according to claim 1, wherein in the sealing layer, the weight percent concentration of the ethylene-based resin is 80 wt % or more and 99.5 wt % or less, and the weight percent concentration of the propylene-based resin is 0.5 wt % or more and 20 wt % or less.
3. 3. The laminated film according to claim 1, wherein the weight percent concentration of the petroleum resin in the intermediate layer is 3.5 wt % or more and 10 wt % or less.
Citation Information
Patent Citations
Ptp multilayered polypropylene sheet
JP1995186346A
Polypropylene-based film
JP2001171056A
Thermal adhesive laminated polyolefinic film
JP1997099525A