Silicone composition

A silicone composition with α-aluminum oxide and zinc oxide enhances thermal conductivity and fluidity, addressing heat dissipation and reliability issues in electronic components, particularly CPUs, by using a specific blend of components to reduce thermal resistance and maintain durability.

JP2024148978AActive Publication Date: 2024-10-18SHIN ETSU CHEMICAL CO LTD
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2023062586
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

Existing thermally conductive silicone compositions fail to provide adequate heat dissipation, durability, and reliability under high temperature and humidity conditions, especially when used with integrated circuit elements like CPUs, due to insufficient thermal conductivity, fluidity, and insulation properties.

Method used

A silicone composition containing α-aluminum oxide with a defined polyhedral shape and specific particle size, combined with zinc oxide and organopolysiloxanes, maintains fluidity and thermal conductivity while ensuring insulation and reliability, using a blend of components that include α-aluminum oxide, zinc oxide, and organopolysiloxanes to enhance thermal conductivity and reduce contact thermal resistance.

Benefits of technology

The composition achieves efficient heat dissipation, maintains fluidity, and ensures durability and reliability under high temperature and humidity conditions, effectively reducing thermal resistance and improving the stability and life of heat-generating electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148978000001
    Figure 2024148978000001
  • Figure 2024148978000002
    Figure 2024148978000002
  • Figure 2024148978000003
    Figure 2024148978000003
Patent Text Reader

Abstract

To provide a silicone composition that retains fluidity, is excellent in treatment, is excellent in heat dissipation, further excellent in durability / reliability under high temperature or high temperature and high humidity condition even when a thermally conductive filler is highly filled in order to impart excellent insulation and thermal conductivity.SOLUTION: A silicone composition comprises (A) Organopolysiloxane represented by the following general formula (1): 50-100 pts.mass, (B) Organopolysiloxane represented by the following average composition formula (2) R3cSiO(4-c) / 2 (2): 0-50 pts.mass, (C) α-aluminum oxide powder having a hexagonal close-packed lattice crystal structure composed of polyhedra having 8 or more faces, and (D) a silicone composition containing zinc oxide powder having an average particle diameter of 0.01 μm or more and less than 3 μm, where the thermal conductivity is 4.0 W / m K or more and less than 7.0 W / m K in the hot disk method according to ISO 22007-2, and the viscosity is 5-800 Pa s when the rotation speed is measured at 10 rpm by a spiral viscometer at 25°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicone composition. [Background technology]

[0002] Many electronic components generate heat during use, and in order to ensure that they function properly, it is necessary to remove the heat from the electronic components. In particular, integrated circuit elements such as CPUs used in personal computers are generating more heat due to faster operating frequencies, making heat countermeasures a major issue.

[0003] Many methods have been proposed as a means of removing this heat. In particular, for electronic components that generate a large amount of heat, a method has been proposed in which a thermally conductive material such as a thermally conductive grease composition or a thermally conductive sheet is placed between the electronic component and a member such as a heat sink to release the heat, but this method is not satisfactory for dissipating heat, especially in areas where the specified thickness differs greatly (see Patent Document 1).

[0004] As such a thermally conductive material, a heat dissipating grease composition based on silicone oil and containing zinc oxide or alumina powder has been proposed, but its heat resistance at 200°C is unsatisfactory (see Patent Documents 2 and 3).

[0005] In order to improve thermal conductivity, the above Patent Document 1 proposes a thixotropic thermal conductive material consisting of at least one selected from a liquid organosilicone carrier, silica fiber, dendritic zinc oxide, flaky aluminum nitride, and flaky boron nitride as a thermal conductive material using aluminum nitride powder. Patent Document 4 proposes a silicone grease composition obtained by blending a specific organopolysiloxane with a spherical hexagonal aluminum nitride powder having a certain particle size range. Patent Document 5 proposes a thermally conductive silicone grease composition combining an aluminum nitride powder having a fine particle size and an aluminum nitride powder having a coarse particle size. Patent Document 6 proposes a thermally conductive silicone grease composition combining an aluminum nitride powder and a zinc oxide powder. Patent Document 7 proposes a thermally conductive grease composition using an aluminum nitride powder surface-treated with an organosilane, but both are unsatisfactory in terms of durability and reliability. Patent Document 8 proposes a thermally conductive silicone composition containing a silicone resin, diamond, zinc oxide, and a dispersant, but the properties after heat resistance are particularly unsatisfactory.

[0006] In addition, metals are materials with high thermal conductivity and can be used in places where insulation of electronic components is not required. Patent Document 9 proposes a thermally conductive grease composition obtained by mixing metallic aluminum powder with a base oil such as silicone oil, but it is unsatisfactory because it does not have insulating properties. Recently, all thermally conductive materials and thermally conductive grease compositions have become insufficient for the heat generation of integrated circuit elements such as CPUs.

[0007] As can be seen from the theoretical formulas of Maxwell and Bruggeman, the thermal conductivity of a material obtained by blending a thermally conductive filler with silicone oil is almost independent of the thermal conductivity of the thermally conductive filler when the volume fraction of the thermally conductive filler is 0.6 or less. The effect of the thermally conductive filler on the thermal conductivity begins to appear only when the volume fraction exceeds 0.6. In other words, in order to increase the thermal conductivity of a thermally conductive grease composition, it is important to first highly fill the thermally conductive filler and to use a filler with high thermal conductivity. However, there is a problem that the fluidity of the thermally conductive grease composition decreases due to high filling, which deteriorates workability such as applicability (dispensability, screen printability), making it impossible to use in practice. Furthermore, there is a problem that the fluidity decreases and the composition cannot follow the fine unevenness of the surfaces of electronic components and heat sinks, resulting in increased contact thermal resistance.

[0008] To date, in order to achieve high loading and obtain a thermally conductive material with good fluidity, there have been studies on compounding alkoxy-containing organopolysiloxanes, which treat the surface of thermally conductive fillers to greatly improve dispersibility, with thermally conductive materials (see Patent Documents 10 and 11). However, these treatments have the drawback of being altered by hydrolysis or the like under high temperature and humidity conditions, which induces a deterioration in the performance of the thermally conductive material.

[0009] In response, thermally conductive silicone grease compositions have been proposed that suppress the deterioration of the performance of thermally conductive materials even under high temperature and high humidity conditions. However, although there are regulations regarding the average particle size of the thermally conductive filler, there are no regulations regarding the shape, hydroxyl group content, or coarse particle size of the thermally conductive filler, and these compositions are not satisfactory, particularly for applications requiring electrical insulation (Patent Document 12).

[0010] In Japanese Patent No. 5755977 (Patent Document 13), a highly thermally conductive resin composition is proposed in which a spherical aluminum oxide powder having a specific average sphericity, a specific hydroxyl group content, and an average particle size of 10 to 50 μm is blended with an aluminum oxide powder having an average particle size of 0.3 to 1 μm, and the blending ratio and volume ratio of each aluminum oxide is specified. Although it is stated that the average particle size of the spherical aluminum oxide powder is a maximum of 50 μm, there is no specification regarding the range of coarse particle size or the content, and when an attempt is made to apply the highly thermally conductive resin composition to a thin film of 50 μm or less, there is a problem that the thermal resistance is insufficient.

[0011] In addition, in republished 2002-092693 (Patent Document 14), a thermally conductive silicone composition using an alumina powder with an average particle size of 0.1 to 100 μm is proposed, but no specific thermal conductivity or viscosity is specified. Furthermore, a mixture of a spherical alumina powder with an average particle size of 5 to 50 μm (but not including 5 μm) and a spherical or irregular alumina powder with an average particle size of 0.1 to 5 μm may be used, and a thermally conductive silicone composition with a specified blending ratio and weight ratio of each aluminum oxide is proposed, but there is no specification for the average sphericity or amount of hydroxyl groups of the spherical alumina with a large average particle size, and further no specification for the range or content of coarse particle size, and this also has the same problem of insufficient thermal resistance as Patent Document 14.

[0012] In Patent Publication No. 6866877 (Patent Document 15), it was discovered that a silicone composition containing α-aluminum oxide powder having a hexagonal close-packed lattice crystal structure consisting of polyhedrons with a specified average particle size and coarse particle content could reduce the contact thermal resistance and improve thermal resistance, but there was a demand for even higher thermal conductivity. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Japanese Patent Application Publication No. 56-28264 [Patent Document 2] Special Publication No. 52-33272 [Patent Document 3] Special Publication No. 59-52195 [Patent Document 4] Japanese Patent Application Publication No. 2-153995 [Patent Document 5] Japanese Patent Application Publication No. 3-14873 [Patent Document 6] Japanese Patent Application Publication No. 10-110179 [Patent Document 7] JP 2000-63872 A [Patent Document 8] JP 2002-30217 A [Patent Document 9] JP 2000-63873 A [Patent Document 10] JP 2004-262972 A [Patent Document 11] JP 2005-162975 A [Patent Document 12] Patent No. 4933094 [Patent Document 13] Patent No. 5755977 [Patent Document 14] Republished Publication No. 2002-092693 [Patent Document 15] Patent No. 6866877 Summary of the Invention [Problem to be solved by the invention]

[0014] The present invention has been made in view of the above circumstances, and has as its object to provide a silicone composition which maintains fluidity, is easy to handle, and has excellent heat dissipation performance, even when highly filled with a thermally conductive filler in order to impart excellent insulating properties and thermal conductivity, as well as excellent durability and reliability under high temperature or high temperature / high humidity conditions. [Means for solving the problem]

[0015] As a result of intensive research by the present inventors in order to achieve the above-mentioned object, they have discovered that a silicone composition containing α-aluminum oxide having a polyhedral shape with a defined average particle size and coarse particle content has excellent insulating properties and thermal conductivity, and also has good fluidity and therefore easy to handle, and further conforms to fine irregularities and reduces thermal contact resistance, thereby obtaining a silicone composition with excellent heat dissipation performance and low thermal resistance, and further has excellent durability under high temperature or high temperature and high humidity conditions, and can improve reliability during mounting, which has led to the completion of the present invention.

[0016] Accordingly, the present invention provides a silicone composition as follows: 1. (A) The following general formula (1): [ka] (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon radicals; R 2 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group, a is an integer of 5 to 100, and b is an integer of 1 to 3. The kinematic viscosity at 25°C is 10 to 10,000 mm 2 / s organopolysiloxane: 50 to 100 parts by mass, (B) The following average composition formula (2): R 3 c SiO (4-c) / 2 (2) (In the formula, R 3 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and c is a number from 1.8 to 2.2. The kinetic viscosity at 25°C is 10 to 100,000 mm 2 / s organopolysiloxane: 0 to 50 parts by mass (However, the total amount of components (A) and (B) is 100 parts by mass.) (C) An α-aluminum oxide powder having a hexagonal close-packed lattice crystal structure consisting of polyhedrons with 8 or more faces, in which, when the maximum particle diameter parallel to the hexagonal lattice planes of the hexagonal close-packed lattice is D and the particle diameter perpendicular to the hexagonal lattice planes is H, the α-aluminum oxide powder has a particle shape in which the D / H ratio is 0.3 to 30, the average particle diameter is 7 to 30 μm, and the proportion of coarse particles having a diameter of 50 μm or more in a laser diffraction particle size distribution is 1 mass% or less of the total, and the purity is 99% or more. (D) zinc oxide powder having an average particle size of 0.01 μm or more and less than 3 μm, and the proportion of coarse particles having a size of 10 μm or more in a laser diffraction particle size distribution is 1 mass % or less of the total mass of component (D); (However, the blending ratio of components (C) and (D) is 5:5 to 9.5:0.5 by mass, and the total blending amount of components (C) and (D) is 75 to 85% by volume.) The silicone composition has a thermal conductivity of 4.0 W / m K or more and less than 7.0 W / m K when measured by the hot disk method in accordance with ISO 22007-2, and a viscosity at 25°C of 5 to 800 Pa s when measured at a rotation speed of 10 rpm with a spiral viscometer. 2. Thermal resistance at 25℃ measured by the laser flash method is 11mm 2 2. The silicone composition according to claim 1, wherein the silicone composition has a molecular weight of 0.4 or less. 3. After leaving the product in an atmosphere of 130℃ / 85%RH for 96 hours, the thermal resistance at 25℃ measured by the laser flash method was 11mm 2 3. The silicone composition according to 1 or 2, wherein the silicone composition has a molecular weight of 0.8 kg / W or less. 4. The silicone composition according to any one of 1 to 3, which has a viscosity of 1,000 Pa s or less at 25°C after thermal aging at 200°C for 100 hours, when measured with a spiral viscometer at a rotation speed of 10 rpm. 5. The silicone composition according to any one of 1 to 4, further comprising (E) a volatile solvent capable of dispersing or dissolving the components (A) and (B): 100 parts by mass or less per 100 parts by mass of the combined amount of the components (A) and (B). 6. Furthermore, (F) a compound represented by the following general formula (3): R 4 d R5 e Si(OR 6 ) 4-d-e (3) (In the formula, R 4 are each independently an alkyl group having 9 to 15 carbon atoms; R 5 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 8 carbon atoms, R 6 each independently represents an alkyl group having 1 to 6 carbon atoms, d is an integer of 1 to 3, and e is an integer of 0 to 2, with the proviso that d+e is an integer of 1 to 3. The silicone composition according to any one of 1 to 5, wherein the alkoxysilane represented by the formula (I) is contained in an amount of 0.1 to 50 parts by mass per 100 parts by mass of the total amount of the components (A) and (B), and the components (C) and (D) have been surface-treated with the component (F). 7. Volume resistivity is 1 x 10 9 7. The silicone composition according to any one of 1 to 6, having a resistivity of Ω·cm or more. Effect of the Invention

[0017] The silicone composition of the present invention has good thermal conductivity while having insulating properties, and is excellent in workability due to maintaining good fluidity. In addition, it has excellent adhesion to heat-generating electronic components and heat-dissipating components, so that the contact thermal resistance can be reduced and low thermal resistance can be achieved. That is, by interposing the silicone composition of the present invention between a heat-generating electronic component and a heat-dissipating component, the heat generated from the heat-generating electronic component can be efficiently dissipated to the heat-dissipating component. Furthermore, the silicone composition of the present invention has excellent durability under high temperature or high temperature and high humidity conditions, and can provide very good reliability when used, for example, for dissipating heat from general power sources, electronic devices, and the like, and for dissipating heat from integrated circuit elements such as LSIs and CPUs used in electronic devices such as personal computers and digital video disk drives. Therefore, the low thermal resistance silicone composition of the present invention can significantly improve the stability and life of heat-generating electronic components and electronic devices using them. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described in detail below. [Component (A)] The component (A) is represented by the following general formula (1): [ka] (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon radicals; R 2 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group, a is an integer of 5 to 100, and b is an integer of 1 to 3. The kinematic viscosity at 25°C is 10 to 10,000 mm 2 and the organopolysiloxane may be used alone or in combination of two or more.

[0019] Component (A) maintains the fluidity of the composition and imparts good handleability to the composition, even when the composition is highly filled with the thermally conductive fillers of components (C) and (D) in order to obtain a thermally conductive silicone composition.

[0020] Above R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups, and the number of carbon atoms is preferably 1 to 18, more preferably 1 to 10. Specific examples include linear alkyl groups, branched alkyl groups, cyclic alkyl groups, alkenyl groups, aryl groups, aralkyl groups, and halogenated alkyl groups. Examples of linear alkyl groups include methyl groups, ethyl groups, propyl groups, hexyl groups, and octyl groups. Examples of branched alkyl groups include isopropyl groups, isobutyl groups, tert-butyl groups, and 2-ethylhexyl groups. Examples of cyclic alkyl groups include cyclopentyl groups and cyclohexyl groups. Examples of alkenyl groups include vinyl groups and allyl groups. Examples of aryl groups include phenyl groups and tolyl groups. Examples of aralkyl groups include 2-phenylethyl groups and 2-methyl-2-phenylethyl groups. Examples of halogenated alkyl groups include a 3,3,3-trifluoropropyl group, a 2-(nonafluorobutyl)ethyl group, and a 2-(heptadecafluorooctyl)ethyl group.1 is preferably a methyl group or a phenyl group.

[0021] Above, R 2 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group. The number of carbon atoms is preferably 1 to 18, and more preferably 1 to 10. Examples of the alkyl group include R 1 Examples of the alkenyl group include the linear alkyl group, branched alkyl group, and cyclic alkyl group as exemplified for R 1 Examples of the alkoxyalkyl group include a methoxyethyl group and a methoxypropyl group. Examples of the acyl group include an acetyl group and an octanoyl group. R 2 is preferably an alkyl group, and particularly preferably a methyl group or an ethyl group.

[0022] a is an integer of 5 to 100, preferably an integer of 5 to 50, and more preferably an integer of 5 to 30. b is an integer of 1 to 3, and preferably 3.

[0023] The kinetic viscosity of component (A) at 25°C is 10 to 10,000 mm 2 / s, 10 to 5,000 mm 2 / s is preferable. 2 If the kinematic viscosity is less than 10,000 mm / s, oil bleeding will occur from the resulting silicone composition. 2 If the viscosity exceeds 1 / s, the fluidity of the resulting silicone composition will be poor. Note that in the present invention, the kinematic viscosity of component (A) is the value measured at 25°C using an Ostwald viscometer.

[0024] The blending amount of the (A) component is in the range of 50 to 100 parts by mass, preferably 55 to 95 parts by mass. However, the total amount of the (A) component and the (B) component described later is 100 parts by mass. When the blending amount is within this range, the silicone composition is likely to maintain good fluidity and workability. In addition, it is easy to highly fill the silicone composition with the thermally conductive fillers of the (C) and (D) components described later. Note that, if the (A) component is less than 50 parts by mass, the composition cannot be highly filled with the thermally conductive fillers of the (C) and (D) components.

[0025] Specific examples of suitable components (A) include the following: [ka]

[0026] [(B) Component] The component (B) of the present invention is represented by the following average composition formula (2): R 3 c SiO (4-c) / 2 (2) (In the formula, R 3 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and c is a number from 1.8 to 2.2. The kinetic viscosity at 25°C is 10 to 100,000 mm 2 and the like. Component (B) is an organopolysiloxane having a molecular weight of 1 to 200, and can be used alone or in combination of two or more. Component (B) is used for the purpose of imparting properties such as viscosity modifier and tackifier to the silicone composition of the present invention.

[0027] Above R 3 R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms. 3Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; and halogenated hydrocarbon groups such as 3,3,3-trifluoropropyl, 2-(perfluorobutyl)ethyl, 2-(perfluorooctyl)ethyl, and p-chlorophenyl. Among these, methyl, phenyl, and alkyl groups having 6 to 18 carbon atoms are preferred, and methyl and phenyl groups are more preferred.

[0028] From the viewpoint of the viscosity required for the composition of the present invention as a silicone composition having low thermal resistance, the above c is a number from 1.8 to 2.2, and preferably a number from 1.9 to 2.1.

[0029] The kinetic viscosity of component (B) at 25°C is 10 to 100,000 mm 2 / s, 10 to 10,000 mm 2 It is preferable that the kinematic viscosity is 10 mm / s. 2 If the kinematic viscosity is less than 100,000 mm / s, liquid separation and oil bleeding will occur from the resulting silicone composition. 2 If it exceeds 1 / s, the fluidity of the resulting silicone composition will be poor, resulting in problems with poor workability. The kinetic viscosity of component (B) is also a value measured at 25°C using an Ostwald viscometer.

[0030] Specific examples of the component (B) include the following: [ka]

[0031] The blending amount of component (B) is 0 to 50 parts by mass, and more preferably 5 to 45 parts by mass (however, the total amount of components (A) and (B) described above should be 100 parts by mass). Component (B) may not be blended. When the blending amount is within this range, the silicone composition tends to maintain good fluidity and workability, and it is also easy to highly fill the composition with the thermally conductive fillers of components (C) and (D), which will be described later. On the other hand, when the blending amount of component (B) exceeds 50 parts by mass, it becomes impossible to highly fill the silicone composition with the thermally conductive fillers of components (C) and (D).

[0032] [(C) component] The component (C) of the present invention is an α-aluminum oxide powder having a hexagonal close-packed lattice crystal structure consisting of polyhedrons with 8 or more faces, in which, when the maximum particle diameter parallel to the hexagonal lattice planes of the hexagonal close-packed lattice is D and the particle diameter perpendicular to the hexagonal lattice planes is H, the powder has a particle shape in which the D / H ratio is 0.3 to 30, the average particle diameter is 7 to 30 μm, the proportion of coarse particles having a diameter of 50 μm or more in a laser diffraction particle size distribution is 1 mass% or less of the total, and the α-aluminum oxide powder has a purity of 99% or more, and may be used alone or in combination of two or more types.

[0033] The aluminum oxide of component (C) has a hexagonal close-packed lattice crystal structure consisting of a polyhedron with eight or more faces, but is preferably an octahedron to icosahedron, and is preferably α-aluminum oxide having a crystal structure substantially composed of eight and / or 16 faces. The crystal structure can be confirmed by the following image diffractometer.

[0034] The particle shape of the component (C) in the present invention is such that the D / H ratio is in the range of 0.3 to 30, where D is the maximum particle diameter parallel to the hexagonal lattice plane of the α-aluminum oxide powder having a hexagonal close-packed lattice structure, and H is the particle diameter perpendicular to the hexagonal lattice plane. The D / H ratio can be measured as follows by importing a particle image taken with a scanning electron microscope into an image analyzer, for example, a JEOL product under the trade name "JSM-7500F". That is, the maximum particle diameter of the particle parallel to the hexagonal lattice plane is measured from the photograph as D, and the particle diameter perpendicular to the hexagonal lattice plane is measured as H. The D / H ratio of 10 arbitrary particles thus obtained is calculated, and the average value is taken as D / H. In the present invention, the D / H ratio is preferably in the range of 0.3 to 5. If the D / H ratio is less than 0.3, the filling property in the resin is deteriorated, the contact between the particles is reduced, and the thermal resistance is increased due to the increase in the interparticle contact thermal resistance. Furthermore, if the D / H ratio of component (C) exceeds 30, there will be significant contact between particles, resulting in greater irregularities on the surface of the silicone composition, increasing the interfacial heat resistance and therefore the thermal resistance.

[0035] The average particle size (primary particle size and / or secondary particle size) of component (C) is 7 to 30 μm, preferably 10 to 25 μm, on a volume basis. If the average particle size is within this range, the bulk density of component (C) is likely to be large and the specific surface area is likely to be small, making it easy to highly pack component (C) into the silicone composition of the present invention. If the average particle size is less than 7 μm, it becomes difficult to achieve the desired thermal conductivity of the present invention. On the other hand, if the average particle size exceeds 30 μm, oil separation may easily proceed, resulting in a deterioration of thermal resistance over time.

[0036] If the content of coarse particles of 50 μm or more in the laser diffraction particle size distribution is 1 mass% or less of the total of component (C), the desired thermal resistance and high thermal conductivity can be achieved at the same time. On the other hand, if the content of coarse particles of 50 μm or more exceeds 1 mass% of the total of component (C), the thickness may not be 60 μm or less, and the desired thermal resistance tends not to be achieved. The content of such coarse particles is preferably 0.5 mass% or less of the total of component (C).

[0037] The volume-based average particle size of component (C) in the present invention can be measured, for example, using Shimadzu's "Laser Diffraction Particle Size Distribution Measuring Instrument SALD-2300". For the evaluation sample, 50 mL of pure water and 5 g of the thermally conductive powder to be measured are added to a glass beaker, stirred with a spatula, and then dispersed in an ultrasonic cleaner for 10 minutes. The solution of the dispersed thermally conductive material powder is added drop by drop to the sampler section of the instrument with a dropper, and the absorbance is allowed to stabilize until it can be measured. When the absorbance stabilizes in this way, measurement is performed. In the laser diffraction particle size distribution measuring instrument, the particle size distribution is calculated from the data of the light intensity distribution of the diffracted / scattered light by the particles detected by the sensor. The average particle size is calculated by multiplying the measured particle size value by the relative particle amount (difference %) and dividing by the total relative particle amount (100%). The average particle size is the average diameter of the particles. For example, the content ratio of coarse particles of component (C) of 50 μm or more can be easily confirmed from the overall particle size distribution. Two or more types of particles having different average particle sizes may be used in combination as long as the effects of the present invention are not impaired.

[0038] The purity of component (C) is 99% or more, and preferably 99.5% or more. If the purity is less than this, the thermal resistance tends to be high. In the present invention, the purity of component (C) is a value measured by atomic absorption spectroscopy based on JIS K 1410. The blending ratio of component (C) is as described below.

[0039] [(D) component] Component (D) is a zinc oxide powder having an average particle size of 0.01 μm or more and less than 3 μm, and the content of coarse particles of 10 μm or more in a laser diffraction particle size distribution is 1 mass % or less of the total. The zinc oxide powder of component (D) functions as a thermally conductive filler in the silicone composition of the present invention. Component (D) may be used alone or in combination of two or more types.

[0040] The average particle size of component (D) is 0.01 μm or more and less than 3 μm on a volume basis, preferably 0.01 to 2 μm, more preferably 0.01 to 1 μm, and even more preferably 0.01 to 0.5 μm. If the average particle size is within this range, the bulk density of component (D) tends to be large and the specific surface area tends to be small, making it easy to highly pack component (D) into the silicone composition of the present invention. If the average particle size is less than 0.01 μm, the packing ability into the resin is poor and the viscosity becomes significantly high. On the other hand, if the average particle size exceeds 3 μm, oil separation easily proceeds.

[0041] In component (D), the content of coarse particles of 10 μm or more in a laser diffraction particle size distribution is 1% by mass or less of the total component (D), and preferably 0.2% by mass or less. By setting it in this range, desired thermal resistance and high thermal conductivity can be achieved at the same time. On the other hand, if the content of coarse particles of 10 μm or more exceeds 1% by mass of the total, the thickness may not be 20 μm or less, and the desired thermal resistance may not be achieved. The method for measuring the average particle size and coarse particle content of component (D) is the same as that for component (C).

[0042] The shape of component (D) may be either spherical or irregular, or may be a mixture of these. In the component (D) of the present invention, the irregular shape is anything other than spherical, and may be, for example, rod-like, needle-like, or disk-like, without any particular limitation, as long as it does not impair the effects of the present invention. Component (D) may be spherical or irregular, or may be a combination of these. Incidentally, component (D) being spherical means that the average sphericity is preferably 0.8 or more, more preferably 0.9 or more.

[0043] The average sphericity of component (D) can be measured by importing particle images taken with a scanning electron microscope into an image analyzer, such as a JEOL product called "JSM-7500F," and proceeding as follows. That is, the projected area (X) and perimeter (Z) of the particle are measured from the photograph. If the area of ​​a perfect circle corresponding to the perimeter (Z) is taken as (Y), the sphericity of the particle can be expressed as X / Y. Assuming a perfect circle with the same perimeter as the perimeter (Z) of the sample particle, then Z=2πr and Y=πr 2(r is the radius.) Therefore, Y = π × (Z / 2π) 2 The sphericity of each particle is given by: Sphericity = X / Y = X × 4π / Z 2 The sphericity of 100 randomly selected particles thus obtained was determined, and the average value was taken as the average sphericity.

[0044] The purity of component (D) is preferably 99.5% or more, and more preferably 99.8% or more in view of impurities such as Pb, Cd, etc. The method for measuring the purity is the same as that described for component (C).

[0045] The blending ratio of component (C) to component (D) in component (D) is 5:5 to 9.5:0.5 by mass, preferably 6:4 to 9:1. If the ratio of component (C) is less than 5 by mass, the filling property of the filler is poor. Conversely, if the ratio of component (C) is more than 9.5 by mass, the filler is difficult to fill densely, and the thermal conductivity is reduced.

[0046] The total amount of (C) and (D) in the silicone composition of the present invention, i.e., the total content of the thermally conductive filler, is 75 to 85 volume % of the entire composition, and preferably 76 to 84 volume %. If the total amount of (C) and (D) is less than 75 volume %, the thermal conductivity of the silicone composition becomes insufficient, and if it exceeds 85 volume %, it becomes difficult to fill the thermally conductive filler. In the present invention, even if the total amount of (C) and (D) is high, the desired effect can be obtained.

[0047] [(E) component] The composition of the present invention may further contain, as component (E), a volatile solvent capable of dispersing or dissolving components (A) and (B). When the present invention further contains component (F) described below in addition to components (A) and (B), the volatile solvent is preferably capable of dispersing or dissolving component (F). There are no particular limitations on component (E) as long as it can dissolve or disperse components (A) and (B), and optionally component (F). Component (E) may be used alone or in combination of two or more.

[0048] The thermal conductivity of the thermally conductive silicone composition is basically correlated with the filling rate of the thermally conductive filler, so the more the thermally conductive filler is filled, the more the thermal conductivity is improved.However, it is natural that the filling amount of the thermally conductive filler is increased, and the dilatancy of the composition when shearing is applied is also likely to increase.In particular, in screen printing, when the thermally conductive silicone composition is squeezed, if the dilatancy is strongly expressed in the thermally conductive silicone composition, the fluidity of the thermally conductive silicone composition is temporarily strongly suppressed, so that the thermally conductive silicone composition cannot pass through the screen mask and the screen mesh, and the application property may be extremely deteriorated.As such, in the past, it was difficult to easily and uniformly install a high thermally conductive silicone composition that is highly filled with a thermally conductive filler on a heat sink or the like by screen printing in a thin layer. Even if the silicone composition of the present invention contains the thermally conductive fillers (C) and (D) at a high filling rate, if it contains the volatile solvent (E), the viscosity is likely to drop sharply and dilatancy is unlikely to occur, so that the applicability is likely to be good and it can be easily applied to a heat sink or the like by screen printing. After application, it is easy to volatilize the contained component (E) at room temperature or by actively heating it. Therefore, in the present invention, a silicone composition with low thermal resistance that is highly filled with thermally conductive fillers can be easily and uniformly applied thinly to a heat sink or the like by screen printing.

[0049] The boiling point of component (E) is preferably within the range of 80 to 260°C. When the boiling point is within this range, it is easy to prevent component (E) from volatilizing suddenly from the silicone composition during the application of the obtained silicone composition, so it is easy to suppress an increase in the viscosity of the silicone composition and it is easy to ensure sufficient application properties of the silicone composition. In addition, since component (E) is unlikely to remain in the silicone composition after the application of the silicone composition, heat dissipation properties are likely to be improved.

[0050] Specific examples of the (E) component include toluene, xylene, acetone, methyl ethyl ketone, cyclohexane, n-hexane, n-heptane, butanol, isopropanol (IPA), isoparaffin-based solvents, and the like. Among these, from the standpoints of safety, health, and workability, isoparaffin-based solvents are preferred, and isoparaffin-based solvents having a boiling point of 80 to 260°C are particularly preferred.

[0051] When component (E) is added to the composition of the present invention, the amount of component (E) is preferably 100 parts by mass or less, more preferably 75 parts by mass or less, relative to 100 parts by mass of the total of components (A) and (B). When the amount is within this range, rapid precipitation of components (C) and (D) is easily suppressed, which tends to improve the storage stability of the silicone composition. There is no particular lower limit for the amount of component (E), but from the viewpoint of the coatability of the silicone composition of the present invention, it is preferably 1 part by mass or more, more preferably 5 parts by mass or more.

[0052] [Component (F)] The composition of the present invention may further contain an alkoxysilane (F). The component (F) is represented by the following general formula (3): R 4 d R 5 e Si(OR 6 ) 4-d-e (3) (In the formula, R 4 are each independently an alkyl group having 9 to 15 carbon atoms; R 5 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 8 carbon atoms; R 6 are each independently an alkyl group having 1 to 6 carbon atoms, d is an integer of 1 to 3, and e is an integer of 0 to 2, with the proviso that d+e is an integer of 1 to 3. The component (F) can be used alone or in combination of two or more different compounds.

[0053] The component (F) is a wetter component and also an additive that prevents the deterioration of the component (A) under high temperature and high humidity. By treating the surfaces of the thermally conductive fillers (C) and (D) with the component (F), the wettability of the component (A) to the components (C) and (D) can be further improved. As a result, the component (F) assists in high loading of the components (C) and (D). In addition, the component (F) acts to suppress contact between the water vapor and the component (A) under high temperature and high humidity conditions when used in combination with the component (A). As a result, the component (F) prevents the performance of the silicone composition of the present invention from deteriorating due to the deterioration of the component (A) caused by hydrolysis or the like under high temperature and high humidity conditions. The component (F) may be used alone or in combination of two or more types.

[0054] Above R 4 are each independently an alkyl group having 9 to 15 carbon atoms, specific examples of which include a nonyl group, a decyl group, a dodecyl group, a tetradecyl group, a pentadecyl group, etc. If the number of carbon atoms is less than 9, the wettability with the thermally conductive filler (component (C) and component (D)) is likely to be insufficient, and if it is more than 15, component (F) is likely to solidify at room temperature, making handling thereof inconvenient, and the heat resistance and flame retardancy of the obtained composition may be easily reduced.

[0055] Above R 5 are each independently an unsubstituted or substituted, saturated or unsaturated monovalent hydrocarbon group having 1 to 8 carbon atoms, and specific examples thereof include alkyl groups such as methyl, ethyl, propyl, hexyl, and octyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; and halogenated hydrocarbon groups such as 3,3,3-trifluoropropyl, 2-(nonafluorobutyl)ethyl, and p-chlorophenyl, with methyl and ethyl being particularly preferred.

[0056] Above R 6are each independently an alkyl group having 1 to 6 carbon atoms, specific examples of which include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, with a methyl group and an ethyl group being particularly preferred.

[0057] The above d is an integer of 1 to 3, and is preferably 1. The above e is an integer of 0 to 2, with the proviso that d+e is an integer of 1 to 3.

[0058] Specific examples of the component (F) include the following: C 10 H 21 Si(OCH 3 ) 3 , C 10 H 21 Si(OC 2 H 5 ) 3 , C 12 H 25 Si(OCH 3 ) 3 , C 12 H 25 Si(OC 2 H 5 ) 3 , C 10 H 21 Si(CH 3 )(OCH 3 ) 2 , C 10 H 21 Si(C 6 H 5 )(OCH 3 ) 2 , C 10 H 21 Si(CH 3 )(OC 2 H 5 ) 2 , C 10 H 21 Si(CH=CH 2 )(OCH 3 ) 2 , C 10 H21 Si(CH 2 CH 2 CF 3 )(OCH 3 ) 2

[0059] When the (F) component is blended, the blending amount is usually preferably 0.1 to 50 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the total of the (A) and (B) components. When the blending amount is within this range, the wetter effect and the high temperature and high humidity resistance effect tend to increase according to the blending amount, which is economical. On the other hand, since the (F) component is somewhat volatile, if a silicone composition containing the (F) component is left in an open system, the (F) component may evaporate from the silicone composition, causing the composition to gradually harden. When the blending amount of the (F) component is within this range, such a phenomenon is easily prevented.

[0060] The surface treatment of components (C) and (D) with component (F) can be carried out by a spraying method using a fluid nozzle, a stirring method with shear force, a dry method using a ball mill or mixer, or a wet method using an aqueous or organic solvent. It is important that the stirring is carried out at a temperature that does not destroy the spherical aluminum oxide powder. The temperature in the system or the drying temperature after treatment in the dry method is appropriately determined according to the type of surface treatment agent so long as the surface treatment agent does not volatilize or decompose, and is 80 to 180°C. Alternatively, a method can be adopted in which components (C) and (D) are heated and mixed together with components (A) and (B), then cooled, and component (F) is added and mixed.

[0061] [Other additives] To the silicone composition of the present invention, additives, fillers, etc. that are usually used may be further added as optional components within a range that does not impair the effects of the present invention. Specifically, fluorine-modified silicone surfactants; colorants such as carbon black, titanium dioxide, red iron oxide, etc.; flame retardant imparting agents such as platinum catalysts, metal oxides such as iron oxide, titanium oxide, and cerium oxide; metal hydroxides, etc. may be added. Furthermore, as an agent for preventing the thermally conductive filler from settling at high temperatures, precipitated silica, fine powder silica such as calcined silica, thixotropy improvers, etc. may be added as desired. The amounts of these ingredients are appropriately selected within the usual range and within a range that does not impair the effects of the present invention.

[0062] [Preparation of Composition] The silicone composition of the present invention is prepared by mixing the above-mentioned components using a mixing device such as a dough mixer (kneader), a gate mixer, a planetary mixer, etc. The silicone composition thus obtained has a significantly improved thermal conductivity and good workability, durability, and reliability.

[0063] [Thermal Conductivity] The thermal conductivity of the silicone composition of the present invention at 25°C is preferably 4.0 W / m·K or more, more preferably 4.0 W / m·K or more and less than 7.0 W / m·K, and even more preferably 4.5 to 6.5 W / m·K, as measured by the hot disk method in accordance with ISO 22007-2. By setting the thermal conductivity to less than 7 W / m·K, the coatability of the silicone composition is further improved. The thermal conductivity of the composition of the present invention can be measured using a thermal conductivity measuring device, for example, a product name "TPS 2500 S" manufactured by Kyoto Electronics Co., Ltd.

[0064] [viscosity] The viscosity of the silicone composition of the present invention at 25°C is 5 to 800 Pa·s, preferably 5 to 750 Pa·s, and more preferably 5 to 500 Pa·s, when measured with a spiral viscometer at a rotation speed of 10 rpm. When the viscosity is within this range, the resulting silicone composition is likely to have good fluidity, which tends to improve workability such as dispensability and screen printability, and tends to make it easier to apply the composition thinly to a substrate. The viscosity of the silicone composition of the present invention can be measured using a spiral viscometer, for example, a product name "Type PC-10AA" manufactured by Malcom Co., Ltd.

[0065] The silicone composition of the present invention preferably has a viscosity of 1,000 Pa s or less, more preferably 700 Pa s or less, and even more preferably 500 Pa s or less, measured at 25°C in the same manner as above after thermal degradation in a dryer at 200°C for 100 hours. Being a non-curable type and having thixotropy, it is possible to ensure the reliability of heat-generating electronic components.

[0066] [Thermal resistance] The heat resistance of the silicone composition of the present invention at 25°C measured by the laser flash method was 11 mm 2 ·K / W or less is preferable, 10mm 2 With the configuration of the present invention, such a low heat resistance silicone composition can be obtained.

[0067] The silicone composition of the present invention has a thermal resistance of 11 mm at 25°C as measured by the laser flash method after being left for 96 hours in an atmosphere of 130°C / 85% RH. 2 ·K / W or less is preferable, 10mm 2 It is more preferable that the thermal resistivity is less than 1.0 K / W. When the silicone composition of the present invention is applied to a heat generating body with a large heat generation amount, the composition can efficiently dissipate the heat generated by the heat generating body to a heat dissipating component if the thermal resistivity is within this range. The measurement of thermal resistance by the laser flash method can be carried out in accordance with ASTM E 1461.

[0068] [Volume resistivity] The silicone composition of the present invention has a volume resistivity of 1×10 9 It is preferable that the resistivity is Ω·cm or more, and more preferably 1×10 10 Within this range, the silicone composition of the present invention can better ensure its insulating properties.

[0069] [Uses of silicone compositions] The silicone composition of the present invention is applied to a heat generating body or a heat sink. Examples of the heat generating body include general power sources; electronic devices such as power transistors for power sources, power modules, thermistors, thermocouples, and temperature sensors; and heat generating electronic components such as integrated circuit elements such as LSIs and CPUs. Examples of the heat sink include heat dissipation components such as heat spreaders and heat sinks; heat pipes, heat sinks, and the like. The application can be performed, for example, by screen printing. Screen printing can be performed, for example, using a metal mask or a screen mesh. By applying the composition of the present invention between a heat generating body and a heat sink, heat can be efficiently conducted from the heat generating body to the heat sink, and heat can be effectively removed from the heat generating body. EXAMPLES

[0070] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0071] [Examples 1 to 5, Comparative Examples 1 to 4] The following components were prepared to prepare the silicone composition of the present invention. The kinematic viscosity was measured at 25° C. using an Ostwald viscometer. Component (A) A-1: Represented by the following formula, specific gravity (25°C) is 0.97, kinetic viscosity is 30mm 2 / s organopolysiloxane [ka]

[0072] (B) Component B-1: Organopolysiloxane B-1: Organopolysiloxane represented by the following formula (2) where c = 2.0, specific gravity (25°C) is 0.97, kinetic viscosity is 500 mm 2 / s organopolysiloxane [ka]

[0073] (C) Aluminum oxide powder (specific gravity 3.98) [Table 1]

[0074] The average particle size shown here is a volume-based value calculated from the entire particle size distribution obtained by the laser diffraction particle size distribution, measured using a Shimadzu Laser Diffraction Particle Size Distribution Analyzer SALD-2300. The coarse particle content is the percentage of coarse particles of 50 μm or more in the entire particle size distribution obtained by the laser diffraction particle size distribution.

[0075] (D) Zinc oxide powder (D-1) Irregular zinc oxide powder (average particle size 0.27 μm, coarse particle content of 10 μm or more is 0.1 mass%, specific gravity is 5.67) The average particle size shown here is a volume-based value calculated from the entire particle size distribution obtained by the laser diffraction particle size distribution, measured using a Shimadzu SALD-2300 laser diffraction particle size distribution analyzer. The coarse particle content is the content ratio of 10 μm coarse particles to the entire particle size distribution obtained by the laser diffraction particle size distribution.

[0076] (E) A volatile solvent (specific gravity 0.79) capable of dispersing or dissolving the components (A-1), (B-1), and (F-1). E-1: Isoparaffin solvent, boiling point 210-254°C: Isozole (registered trademark) 400 (product name, manufactured by ENEOS Corporation)

[0077] (F) Alkoxysilane F-1: Alkoxysilane represented by the following formula (specific gravity is 0.90) C 10 H 21 Si(OCH 3 ) 3

[0078] [Manufacturing method] Components (A) to (D), and further components (E) and (F) as necessary, were mixed as follows to obtain compositions of Examples 1 to 5 and Comparative Examples 1 to 4. That is, components (A) to (D) were weighed out in a 5-liter planetary mixer (manufactured by Inoue Seisakusho Co., Ltd.) in the composition ratios (parts by mass) shown in Tables 2 and 3, and mixed under reduced pressure of 30 mmHg or less at 150°C for 1 hour. The resulting mixture was then cooled to room temperature and mixed. When components (E) and (F) were added, components (E) and (F) were added to the cooled mixture in the amounts shown in Table 2 and mixed uniformly.

[0079] [Test Method] The properties of the resulting silicone composition were measured using the following test methods, and the results are shown in Tables 2 and 3.

[0080] 〔viscosity〕 The resulting silicone composition was allowed to stand in a thermostatic chamber at 25° C. for 24 hours, and then its viscosity was measured at 10 rpm using a viscometer (product name: Spiral Viscometer PC-10AA, manufactured by Malcom Co., Ltd.).

[0081] [Viscosity after thermal degradation] The resulting silicone composition was thermally aged in a dryer at 200° C. for 100 hours, and then left to stand in a thermostatic chamber at 25° C. for 24 hours, after which measurements were taken in the same manner as above.

[0082] [Thermal Conductivity] The test was performed based on the hot disk method in accordance with ISO 22007-2. The obtained silicone composition was wrapped in kitchen wrap to prevent bubbles and the like from getting in, and two samples were prepared. The samples were then sandwiched between the sensors of a thermal conductivity meter (product name: TPS-2500S) manufactured by Kyoto Electronics Manufacturing Co., Ltd., and the thermal conductivity of the composition at 25°C was measured.

[0083] [Volume resistivity] Based on JIS K 6911, a test piece was prepared so that the sample thickness was 1 mm in order to measure by the double ring electrode method, 500 V was applied between the electrodes, and the volume resistivity was measured after 1 minute.

[0084] [Preparation of test pieces for measuring thickness and thermal resistance] A 40 μm thick composition was sandwiched between two circular aluminum plates with a diameter of 12.6 mm and a thickness of 1 mm, and a pressure of 0.15 MPa was applied at 25° C. for 60 minutes to prepare a test piece.

[0085] [Thickness measurement] The thickness of the test piece was measured with a micrometer (manufactured by Mitutoyo Corporation), and the thickness of the composition was calculated by subtracting the thicknesses of the two aluminum plates that had been measured in advance.

[0086] [Measurement of thermal resistance] Using the above test piece, the thermal resistance (unit: mm 2 ·K / W) was measured at 25°C using a thermal resistance measuring device based on the laser flash method (Netsch xenon flash analyzer; LFA447 NanoFlash).

[0087] [Measurement of thermal resistance after exposure to high temperature and humidity] After the thermal resistance measurement, the test piece was left in an atmosphere of 130°C / 85% RH for 96 hours, and then the thermal resistance (unit: mm 2 ·K / W) was measured using the same thermal resistance measuring instrument.

[0088] [Table 2]

[0089]

Table 3

Claims

1. (A) a compound represented by the following general formula (1): 【Chemistry 1】 (In the formula, R 1 are independently unsubstituted or substituted monovalent hydrocarbon groups; R 2 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group, a is an integer from 5 to 100, and b is an integer from 1 to 3. and the kinetic viscosity at 25°C is 10 to 10,000 mm 2 / s organopolysiloxane: 50 to 100 parts by mass, (B) The following average composition formula (2): R 3 c SiO (4-c) / 2 (2) (In the formula, R 3 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and c is a number from 1.8 to 2.

2. The kinetic viscosity at 25°C represented by 2 / s organopolysiloxane: 0 to 50 parts by mass (However, the total amount of components (A) and (B) is 100 parts by mass.) (C) An α-aluminum oxide powder having a hexagonal close-packed lattice crystal structure consisting of polyhedrons with 8 or more faces, in which, when the maximum particle diameter parallel to the hexagonal lattice planes of the hexagonal close-packed lattice is D and the particle diameter perpendicular to the hexagonal lattice planes is H, the α-aluminum oxide powder has a particle shape in which the D / H ratio is 0.3 or more and 30 or less, the average particle diameter is 7 to 30 μm, and the proportion of coarse particles having a diameter of 50 μm or more in a laser diffraction particle size distribution is 1 mass% or less of the total, and the purity is 99% or more. (D) zinc oxide powder having an average particle size of 0.01 μm or more and less than 3 μm, and a ratio of coarse particles having a size of 10 μm or more in a laser diffraction particle size distribution is 1 mass % or less of the total amount of component (D); (However, the blending ratio of components (C) and (D) is 5:5 to 9.5:0.5 by mass, and the total blending amount of components (C) and (D) is 75 to 85% by volume.) The silicone composition has a thermal conductivity of 4.0 W / m K or more and less than 7.0 W / m K when measured by a hot disk method in accordance with ISO 22007-2, and a viscosity at 25°C of 5 to 800 Pa s when measured at a rotation speed of 10 rpm using a spiral viscometer.

2. Thermal resistance at 25°C measured by the laser flash method is 11 mm 2 2. The silicone composition according to claim 1, wherein the viscosity is less than or equal to 1.0 K / W.

3. After leaving it in an atmosphere of 130°C / 85% RH for 96 hours, the thermal resistance at 25°C measured by the laser flash method was 11 mm 2 2. The silicone composition according to claim 1, wherein the viscosity is less than or equal to 1.0 K / W.

4. 2. The silicone composition according to claim 1, which after thermal aging at 200° C. for 100 hours has a viscosity at 25° C. of 1,000 Pa·s or less when measured with a spiral viscometer at a rotation speed of 10 rpm.

5. 2. The silicone composition according to claim 1, further comprising: (E) a volatile solvent capable of dispersing or dissolving the components (A) and (B): 100 parts by mass or less per 100 parts by mass of the combined amount of the component (A) and the component (B).

6. Furthermore, (F) a compound represented by the following general formula (3): R 4 d R 5 e Si(OR 6 ) 4-d-e (3) (In the formula, R 4 are each independently an alkyl group having 9 to 15 carbon atoms; R 5 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 8 carbon atoms; R 6 are each independently an alkyl group having 1 to 6 carbon atoms, d is an integer of 1 to 3, and e is an integer of 0 to 2, with the proviso that d+e is an integer of 1 to 3. The silicone composition according to claim 1, wherein the silicone composition contains an alkoxysilane represented by the formula:

7. Volume resistivity is 1×10 9 The silicone composition according to any one of claims 1 to 6, which has a viscosity of at least Ω·cm.

Citation Information

Patent Citations

  • Heat conductive silicone composition

    JP1999049958A

  • Heat conductive silicone grease composition

    JP2012052137A

  • Thermal conductive silicone composition, cured article and composite sheet

    JP2018053260A

  • Low thermal resistance silicone composition

    JP2019210305A

  • Thermally conductive silicone composition and thermally conductive silicone material

    WO2021171970A1