Phenol resin formed with mesopore, and carbonized material formed with mesopore
A carbonized material with mesopores is produced using a specific heating and carbonization process, addressing the issue of platinum nanoparticle aggregation in fuel cells, thereby enhancing catalytic performance and extending catalyst life.
Patent Information
- Application Number
- JP2023062773
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing carbon carriers for platinum catalysts in fuel cells have low platinum utilization efficiency due to insufficient mesopore formation, leading to aggregation and sintering of platinum nanoparticles, which reduces catalytic performance.
A method for producing a carbonized material with mesopores by heating a mixture of phenol compound, formaldehyde, alkali metal hydroxide or ammonia, organic amine, quaternary organic ammonium salt, and nonionic surfactant under specific temperature conditions, followed by drying and carbonization, to create a carbon carrier that supports platinum nanoparticles effectively.
The method enhances platinum nanoparticle support and distribution, preventing aggregation, increasing catalytic activity and extending catalyst life by facilitating high-speed transport of reactants and products.
Smart Images

Figure 2024149098000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbonized material having mesopores and a phenolic resin having mesopores. [Background technology]
[0002] As part of recent research and development aimed at realizing a carbon-neutral society, there is currently development in the automotive field to replace automobiles equipped with engines that use fossil fuels with electric vehicles that use secondary batteries such as lithium-ion secondary batteries as their energy device, and fuel cell vehicles that use fuel cells as their energy device.
[0003] Due to the improvement of the charging capacity and the fall of the price of lithium-ion secondary batteries, passenger cars have rapidly become popular in recent years, and as a result, electric vehicles are being replaced. On the other hand, trucks and buses have a longer driving distance per charge than passenger cars, so a single charge of secondary batteries such as lithium-ion secondary batteries is not enough to cover the required driving distance, and it is not realistic to increase the number of batteries installed due to the weight and cost of the batteries. For this reason, fuel cell vehicles are considered to be the likely replacements for trucks and buses.
[0004] The fuel cell used in fuel cell-equipped vehicles is a polymer electrolyte fuel cell (PEFC) consisting of an anode catalyst layer, a polymer electrolyte membrane, and a cathode catalyst layer. The cathode, which is the air electrode of the fuel cell, uses a catalyst in which platinum or a platinum alloy is supported on a carbon support.
[0005] Platinum is expensive and there is a need to reduce its use because of the scarcity of platinum reserves worldwide. Therefore, in order to reduce the amount of platinum used as a cathode catalyst in fuel cells, attempts have been made to reduce the amount of platinum used by making it into small particles and supporting it on a carbon support.
[0006] However, when small platinum particles are repeatedly used as a catalyst for a cell reaction, they tend to aggregate and sinter to become larger particles. When the particles become larger, their performance as a catalyst for a cell reaction decreases, so simply supporting small platinum particles results in a high rate of deterioration in the performance of the fuel cell.
[0007] Therefore, platinum nanoparticles have been supported in the mesopores of a carbon support in which mesopores are formed, thereby preventing the platinum nanoparticles from agglomerating and sintering due to repeated use in battery reactions. Patent Document 1 discloses a platinum-supported metal catalyst in which a platinum catalyst is supported on mesoporous carbon nanodendrites (MCND).
[0008] However, in the platinum-supported metal catalyst described in Patent Document 1, uniform mesopores are not formed in the support, and platinum particles supported in the deep mesopores are unable to contribute to the catalytic reaction, resulting in low utilization efficiency of the platinum catalyst.
[0009] For this reason, Patent Document 2 discloses a supported metal catalyst for improving the utilization efficiency of a platinum catalyst supported on a carbon support, the supported metal catalyst comprising a support which is an aggregate of conductive particles, and active metal particles dispersed and supported on the conductive particles, the conductive particles including a plurality of pores, the pores having an average inlet pore diameter of 1 to 20 nm, a standard deviation of the average inlet pore diameter being 50% or less of the average inlet pore diameter, the number fraction of the active metal particles supported on the surface region of the conductive particles being 50% or more, and the surface region being a region on the surface of the conductive particle, or a region within the pores within a depth of 15 nm from the surface. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2018-10806 A [Patent Document 2] International Publication No. 2021 / 161929 Summary of the Invention [Problem to be solved by the invention]
[0011] In the supported metal catalyst of Patent Document 2, the framework of the carbon support on which the metal particles are supported has a three-dimensional network structure in which spherical carbon nanoparticles are connected in a three-dimensional direction, and the framework has mesopores that can support platinum nanoparticles within the pores. This three-dimensional network structure contributes to high-speed transport of products and reactants, for example, by making it easier for water vapor generated by the cell reaction at the cathode to escape from the electrode.
[0012] However, in the carbon support of Patent Document 2, the gaps between the skeletons of the three-dimensional mesh structure are too large, resulting in a problem that the skeleton parts capable of supporting platinum nanoparticles are reduced, resulting in a low amount of platinum nanoparticles supported per cell.
[0013] Therefore, an object of the present invention is to provide a carbon support in which mesopores capable of supporting platinum nanoparticles are formed within the pores, which has a structure suitable for high-speed transport of substances, such as by making it easier for water vapor generated by the battery reaction at the cathode to escape from the electrode, and which can increase the amount of platinum nanoparticles supported per cell. [Means for solving the problem]
[0014] The above problems are solved by the present invention described below. That is, the present invention provides (1) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 83° C. or higher and 88° C. or lower to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 58° C. or higher and 67° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; A phenolic resin having mesopores formed therein, which is obtained by carrying out the steps of: (2) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 78°C or higher and lower than 83°C to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 63° C. or higher and 72° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; A phenolic resin having mesopores formed therein, which is obtained by carrying out the steps of: (3) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 73° C. or higher and lower than 78° C. to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 67° C. or higher and 72° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; A phenolic resin having mesopores formed therein, which is obtained by carrying out the steps of: (4) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water at 50° C. or more and 58° C. or less to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 73° C. or higher and 78° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; A phenolic resin having mesopores formed therein, which is obtained by carrying out the steps of: (5) A carbonized material having mesopores, characterized in that it is obtained by a carbonization step in which a phenolic resin having mesopores formed therein is heat-treated at 300° C. or more and 450° C. or less in an inert gas atmosphere, the heat-treated product is then calcined at 450° C. or more and 800° C. or less in an inert gas atmosphere, and the calcined product is then carbonized at 800° C. or more and 2000° C. or less in an inert gas atmosphere to obtain a carbonized material having mesopores. This provides: Effect of the Invention
[0015] According to the present invention, it is possible to provide a carbon support having mesopores formed therein that can support platinum nanoparticles, the carbon support having a structure suitable for high-speed transport of substances, such as by facilitating the escape of water vapor generated by a battery reaction at the cathode from the electrode, and capable of supporting a large amount of platinum nanoparticles per cell. [Brief description of the drawings]
[0016] [Figure 1] 1 is a STEM image of the phenol resin obtained in Example 1. [Diagram 2] 1 is a STEM image of the phenol resin obtained in Example 2. [Diagram 3] 1 is a STEM image of the phenol resin obtained in Example 3. [Figure 4] 1 is a STEM image of the phenol resin obtained in Example 4. [Diagram 5] 1 is a STEM image of the phenol resin obtained in Example 5. [Figure 6] 1 is a STEM image of the phenol resin obtained in Example 6. [Figure 7] 1 is a STEM image of the phenol resin obtained in Example 7. [Figure 8] 1 is a STEM image of the phenol resin obtained in Example 8. [Figure 9] 1 is a STEM image of the phenol resin obtained in Comparative Example 1. [Figure 10] 1 is a STEM image of the phenol resin obtained in Comparative Example 2. [Figure 11] 1 is a STEM image of the phenol resin obtained in Comparative Example 3. [Figure 12] 1 is a STEM image of the phenol resin obtained in Comparative Example 4. [Figure 13] 1 is a STEM image of the phenol resin obtained in Comparative Example 5. [Figure 14] 1 is a STEM image of the phenol resin obtained in Comparative Example 6. [Figure 15] 1 is a STEM image of the phenol resin obtained in Comparative Example 7. [Figure 16] 1 is a STEM image of the phenol resin obtained in Comparative Example 8. [Figure 17] 1 is a STEM image of the phenolic resin obtained in Comparative Example 9. [Figure 18] 1 is a STEM image of the phenol resin obtained in Comparative Example 10. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings as appropriate. The detailed description of the present invention below is an example of an embodiment, and the present invention is not to be construed as being limited to this embodiment.
[0018] The phenolic resin having mesopores formed therein according to the first embodiment of the present invention is a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at 83° C. or higher and 88° C. or lower to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 58° C. or higher and 67° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; The present invention is characterized in that the above-mentioned is obtained by carrying out the above steps.
[0019] The phenolic resin having mesopores formed therein according to the second embodiment of the present invention is a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 78°C or higher and lower than 83°C to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 63° C. or higher and 72° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; The present invention is characterized in that the above-mentioned is obtained by carrying out the above steps.
[0020] The phenolic resin having mesopores formed therein according to the third embodiment of the present invention is A first process for obtaining a first treated product by heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 73° C. or higher and lower than 78° C.; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 67° C. or higher and 72° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; The present invention is characterized in that the above-mentioned is obtained by carrying out the above steps.
[0021] The phenolic resin having mesopores according to the fourth embodiment of the present invention is a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 50° C. or higher and 58° C. or lower to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 73° C. or higher and 78° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; The present invention is characterized in that the above-mentioned is obtained by carrying out the above steps.
[0022] The phenolic resins in which mesopores are formed according to the first to fourth embodiments of the present invention have some similarities, although the heating conditions in the first and second steps are different. Therefore, the different parts will be explained separately, and the similar parts will be explained by collectively describing the phenolic resins in which mesopores are formed according to the first to fourth embodiments of the present invention as the phenolic resins in which mesopores are formed of the present invention.
[0023] The first step for producing the phenolic resin having mesopores of the present invention is a step of heating a mixture of a phenolic compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product.
[0024] The phenolic compound used in the first step of the present invention for the phenolic resin having mesopores is not particularly limited as long as it is a compound having a phenolic skeleton, and examples thereof include phenol (C6H5OH), substituted phenols in which an aromatic ring is substituted with one or more alkyl groups, specifically C6H4(OH)CH3 (any one or a combination of two or more of 2-methylphenol, 3-methylphenol, and 4-methylphenol), C6H3(OH)(CH3)2 (any one or a combination of two or more of 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, and 3,5-dimethylphenol), resorcinol (C6H4(OH)2), pyrocatechol (C6H4(OH)2), etc. Among these, phenolic compounds are preferably phenol (C6H5OH).
[0025] The formaldehyde used in the first step for the mesopore-formed phenolic resin of the present invention is usually added as an aqueous formaldehyde solution to water for preparing the mixed solution. The concentration of the aqueous formaldehyde solution is not particularly limited, and is usually 10.0% by mass or more and 40.0% by mass or less.
[0026] The alkali metal hydroxide used in the first step for the phenolic resin having mesopores of the present invention is not particularly limited, but from the viewpoint of preferentially proceeding with the addition reaction of phenol, sodium hydroxide, potassium hydroxide and lithium hydroxide are preferred, and sodium hydroxide is particularly preferred.
[0027] In the first step of the present invention for the phenolic resin having mesopores, ammonia, an organic amine such as ethanolamine, or a quaternary organic ammonium salt such as tetramethylammonium hydroxide can be used instead of an alkali metal hydroxide. By using an alkali metal hydroxide, ammonia, an organic amine, or a quaternary ammonium salt in the first step of the present invention, a reaction for producing a resol resin can be carried out under basic conditions.
[0028] Examples of the organic amine used in the first step include ethanolamine, propanolamine, alkylamine, and cyclic amine. Examples of the ethanolamine include monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, N-ethylethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, and aminoethoxyethanol. Examples of the propanolamine include 1-amino-2-propanol, 2-amino-2-methyl-1-propanol, and 2-amino-2-methyl-1,3-propanediol. Examples of the alkylamine include monomethylamine, dimethylamine, trimethylamine, ethyleneamine, ethylenediamine, diethylenetriamine, triethylenetetramine, hexamethylenetetramine, and tetraethylenepentamine. Examples of the cyclic amine include choline and morpholine.
[0029] Examples of the quaternary organic ammonium salt used in the first step include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, N,N,N-triethyl-N-(2-hydroxyethyl)ammonium hydroxide, and N,N-diethyl-N,N-di(2-hydroxyethyl)ammonium hydroxide.
[0030] The organic amine or quaternary organic ammonium salt used in the first step is preferably one having strong basicity, more preferably a quaternary ammonium salt, and particularly preferably tetramethylammonium hydroxide, tetraethylammonium hydroxide, or the like.
[0031] Nonionic surfactants used in the first step for the phenolic resin having mesopores of the present invention include polyoxyethylene alkyl ethers and polyoxyethylene alkyl phenyl ethers, and more specifically, copolymers of polyethylene oxide (PEO) and polypropylene oxide (PPO), particularly those in which the molar mass of PPO is from 3,000 to 4,000 and the intramolecular proportion of PEO is from 30% to 90%.
[0032] The water used in the first step for the phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the first step for the phenolic resin having mesopores of the present invention preferably contains fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.
[0033] In the mixture used in the first step for the phenolic resin having mesopores of the present invention, the molar ratio of formaldehyde to the phenolic compound (formaldehyde / phenolic compound) is 2.6 or more and 5.0 or less, the molar ratio of alkali metal hydroxide to the phenolic compound (alkali metal hydroxide / phenolic compound) is 0.24 or more and 0.48 or less, the molar ratio of ammonia to the phenolic compound (ammonia / phenolic compound) is 0.24 or more and 0.96 or less, the molar ratio of organic amine to the phenolic compound (organic amine / phenolic compound) is 0.24 or more and 0.96 or less, and the molar ratio of quaternary organic ammonium salt to the phenolic compound (quaternary organic ammonium salt / phenolic compound) is 0.24 or more and 0.48 or less.
[0034] In the first step relating to the phenolic resin having mesopores of the present invention, the amount of nonionic surfactant mixed is an amount such that the mass ratio of the nonionic surfactant to the phenolic compound in the first processed product (nonionic surfactant / phenolic compound) is 1.5 or more and 2.3 or less.
[0035] The amount of water to be mixed in the first step for the phenolic resin having mesopores of the present invention is an amount that results in a nonionic surfactant concentration of 21 mg / mL or more and 45 mg / mL or less relative to the total amount of the first processed product.
[0036] The method for preparing the mixture used in the first step for the phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include a method in which predetermined amounts of a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, and a nonionic surfactant are added to a predetermined amount of water and mixed. The formaldehyde, the alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, and the nonionic surfactant may be added in the form of an aqueous solution.
[0037] In the first step for the phenolic resin having mesopores of the first embodiment of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 83° C. or higher and 88° C. or lower to obtain a first treated product. In the first step for the phenolic resin having mesopores of the first embodiment of the present invention, the heating time for heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is 1 hour or higher and 6 hours or lower.
[0038] In the first step for the phenolic resin having mesopores of the second embodiment of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 78° C. or more and less than 83° C. to obtain a first treated product. In the first step for the phenolic resin having mesopores of the second embodiment of the present invention, the heating time for heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is 1 hour or more and 6 hours or less.
[0039] In the first step for the phenolic resin having mesopores of the third embodiment of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 73° C. or more and less than 78° C. to obtain a first treated product. In the first step for the phenolic resin having mesopores of the third embodiment of the present invention, the heating time for heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is 1 hour or more and 6 hours or less.
[0040] In the first step relating to the phenolic resin having mesopores of the fourth embodiment of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 50° C. or more and 58° C. or less to obtain a first treated product. In the first step relating to the phenolic resin having mesopores of the fourth embodiment of the present invention, the heating time when the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated is 1 hour or more and 6 hours or less.
[0041] The second step relating to the mesopore-formed phenolic resin of the present invention is a step of mixing water with the first treated product obtained by carrying out the first step and heating the resulting mixture to obtain a sol liquid.
[0042] The water used in the second step for the phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the second step for the phenolic resin having mesopores of the present invention preferably contains fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.
[0043] In the second step relating to the phenolic resin having mesopores of the present invention, the amount of water to be mixed with the first treated product is an amount such that the concentration of the nonionic surfactant in the mixture obtained after mixing the first treated product with water is 9 mg / mL or more and 20 mg / mL or less.
[0044] In the second step relating to the phenolic resin having mesopores of the present invention, the method for mixing water with the first treated product is not particularly limited, and examples thereof include a method in which a predetermined amount of water is added to a predetermined amount of the first treated product and mixed.
[0045] In the second step for the phenolic resin having mesopores of the first embodiment of the present invention, the mixture obtained by mixing water with the first treated product is heated at 58° C. to 67° C. to obtain a sol. In the second step for the phenolic resin having mesopores of the first embodiment of the present invention, the heating time for heating the mixture obtained by mixing water with the first treated product is 12 hours to 24 hours.
[0046] In the second step for the phenolic resin having mesopores of the second embodiment of the present invention, the mixture obtained by mixing water with the first treated product is heated at 63° C. to 72° C. to obtain a sol. In the second step for the phenolic resin having mesopores of the second embodiment of the present invention, the heating time for heating the mixture obtained by mixing water with the first treated product is 12 hours to 24 hours.
[0047] In the second step for the phenolic resin having mesopores of the third embodiment of the present invention, the mixture obtained by mixing water with the first treated product is heated at 67° C. to 72° C. to obtain a sol. In the second step for the phenolic resin having mesopores of the third embodiment of the present invention, the heating time for heating the mixture obtained by mixing water with the first treated product is 12 hours to 24 hours.
[0048] In the second step relating to the phenolic resin having mesopores of the fourth embodiment of the present invention, the mixture obtained by mixing water with the first treated product is heated at 73° C. to 78° C. to obtain a sol. In the second step relating to the phenolic resin having mesopores of the fourth embodiment of the present invention, the heating time for heating the mixture obtained by mixing water with the first treated product is 12 hours to 24 hours.
[0049] The sol liquid obtained by carrying out the second step related to the phenolic resin having mesopores of the present invention may be used as it is in the gelation step. Alternatively, after carrying out the second step related to the phenolic resin having mesopores of the present invention, the sol liquid obtained by carrying out the second step may be filtered before carrying out the gelation step, and the obtained filtrate may be used as the sol liquid in the gelation step.
[0050] The gelation step for the phenolic resin having mesopores of the present invention is a step of mixing water with the sol liquid obtained by carrying out the second step for the phenolic resin having mesopores of the first, second, third or fourth embodiment of the present invention, and heating the resulting mixture under pressure to obtain a wet gel.
[0051] The water used in the gelation step for the phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the gelation step for the phenolic resin having mesopores of the present invention preferably contains fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.
[0052] In the gelation step of the present invention for the phenolic resin having mesopores, the amount of water mixed in the sol liquid is 1.5 to 6.0 times the mass of the first processed product.
[0053] In the gelation step of the present invention involving the phenolic resin having mesopores, the method for mixing water with the sol liquid is not particularly limited, and examples thereof include a method in which a predetermined amount of water is added to a predetermined amount of sol liquid and mixed.
[0054] In the gelation process for the phenolic resin having mesopores of the present invention, a mixture obtained by mixing water with a sol liquid is heated under pressure at 120°C to 140°C to obtain a wet gel. In the gelation process for the phenolic resin having mesopores of the present invention, the pressure (absolute pressure) when the mixture obtained by mixing water with a sol liquid is heated is 0.34 MPa to 0.51 MPa. In the gelation process for the phenolic resin having mesopores of the present invention, the heating time when the mixture obtained by mixing water with a sol liquid is heated is 6 hours to 48 hours.
[0055] The wet gel obtained by carrying out the gelling step for the phenolic resin having mesopores of the present invention may be dried directly in the drying step. Alternatively, after carrying out the gelling step for the phenolic resin having mesopores of the present invention, the wet gel obtained by carrying out the gelling step may be washed one or more times before carrying out the drying step, and the obtained wet gel may be dried in the drying step.
[0056] The drying step for the phenolic resin having mesopores of the present invention is a step of drying the wet gel obtained by the gelling step to obtain a phenolic resin having mesopores.
[0057] In the drying step for the phenolic resin having mesopores of the present invention, the method for drying the wet gel is not particularly limited, and examples thereof include: (i) a method in which the wet gel is added to water, dispersed in water, the obtained wet gel dispersion is freeze-granulated by spraying it into liquid nitrogen using a spray-freeze granulator, and then the obtained frozen granules are vacuum-dried to dry the wet gel; (ii) a method in which the wet gel is added to water, dispersed in water, and the obtained wet gel dispersion is sprayed into hot air using a spray dryer to heat-dry; and (iii) a method in which the wet gel is heat-dried by treatment with microwaves.
[0058] The phenolic resin obtained by carrying out the drying step for the phenolic resin having mesopores of the present invention is the phenolic resin having mesopores of the present invention.
[0059] The carbonized material having mesopores of the present invention is characterized in that it is obtained by carrying out a carbonization step in which a phenolic resin having mesopores of the present invention, i.e., a phenolic resin having mesopores of the first, second, third or fourth embodiment of the present invention, is heat-treated at 300°C or more and 450°C or less in an inert gas atmosphere, the obtained heat-treated product is then calcined at 450°C or more and 800°C or less in an inert gas atmosphere, and the obtained calcined product is carbonized at 800°C or more and 2000°C or less in an inert gas atmosphere to obtain a carbonized material having mesopores.
[0060] In the carbonization process for the carbonized product of the present invention having mesopores formed therein, the heat treatment temperature for the heat treatment of the phenolic resin of the present invention having mesopores formed therein is 300°C or more and 450°C or less. In the carbonization process for the present invention, by heat treating the phenolic resin of the present invention having mesopores formed therein within the above temperature range, it becomes possible to remove the surfactant remaining in the phenolic resin of the present invention having mesopores formed therein and maintain the mesopore structure. In the carbonization process for the carbonized product of the present invention having mesopores formed therein, the heat treatment time for the heat treatment of the phenolic resin of the present invention having mesopores formed therein is 30 minutes or more and 6 hours or less. In the carbonization process for the carbonized product of the present invention having mesopores formed therein, the heat treatment atmosphere for the heat treatment of the phenolic resin of the present invention having mesopores formed therein is an inert gas atmosphere such as nitrogen gas, helium gas, argon gas, etc.
[0061] In the carbonization process for the carbonized product of the present invention having mesopores formed, the firing temperature when firing the heat-treated product of the present invention of the phenolic resin having mesopores formed is 450° C. or more and 800° C. or less. In the carbonization process for the carbonized product of the present invention having mesopores formed, the firing time when firing the heat-treated product of the present invention of the phenolic resin having mesopores formed is 30 minutes or more and 6 hours or less. In the carbonization process for the carbonized product of the present invention having mesopores formed, the firing atmosphere when firing the heat-treated product of the present invention of the phenolic resin having mesopores formed is an inert gas atmosphere such as nitrogen gas, helium gas, argon gas, etc.
[0062] In the carbonization process for the carbonized product of the present invention having mesopores formed, the carbonization temperature when the burned product of the present invention of the phenolic resin having mesopores formed is carbonized is 800° C. or more and 2000° C. or less. In the carbonization process for the carbonized product of the present invention having mesopores formed, the carbonization time when the burned product of the present invention of the phenolic resin having mesopores formed is carbonized is 30 minutes or more and 6 hours or less. In the carbonization process for the carbonized product of the present invention having mesopores formed, the burning atmosphere when the burned product of the present invention of the phenolic resin having mesopores formed is carbonized is an inert gas atmosphere such as nitrogen gas, helium gas, argon gas, etc.
[0063] The carbonized product obtained by carrying out the carbonization step relating to the carbonized product having mesopores of the present invention is the carbonized product having mesopores of the present invention.
[0064] In the carbonized material of the present invention in which mesopores are formed, the diameter of the skeleton is 18 nm or more and 72 nm or less. In the present invention, the method for measuring the diameter of the skeleton of the carbonized material in which mesopores are formed is as follows. First, a sample is prepared by dispersing a wet gel in ethanol, dropping it onto a grid for transmission electron microscope observation, and drying it, and the sample is observed with a scanning transmission electron microscope (STEM: HD-2700 (manufactured by Hitachi High-Technologies Corporation), accelerating voltage 200 kV) to obtain a STEM image. Next, 100 circles circumscribed on the skeleton image of the obtained STEM image are arranged, and the average of their diameters is taken as the diameter of the skeleton.
[0065] The structure of the carbonized material of the present invention in which mesopores are formed differs from the structure of the carbon support on which the metal catalyst is supported (hereinafter referred to as the carbon support of Patent Document 2) in the supported metal catalyst of Patent Document 2. The difference between the structure of the carbon support of Patent Document 2 and the carbonized material of the present invention in which mesopores are formed will be described below.
[0066] The skeleton of the carbon support in Patent Document 2 has a three-dimensional network structure formed by spherical carbon nanoparticles linked in a three-dimensional direction. Therefore, in the skeleton of the carbon support in Patent Document 2, the largest diameter part of the linked spherical carbon nanoparticles becomes the part of the skeleton with a large diameter, and the connecting part of adjacent carbon nanoparticles becomes the part of the skeleton with a small diameter, and protrusions and constrictions derived from the spherical carbon nanoparticles are observed on the wall surface of the skeleton.
[0067] In contrast, the skeleton of the carbonized material of the present invention in which mesopores are formed has a three-dimensional mesh structure connected in the three-dimensional direction, but the difference in diameter due to the difference in the skeleton position is smaller than that of the carbon support of Patent Document 2.
[0068] Furthermore, the three-dimensional network structure of the carbonized material of the present invention in which mesopores are formed has a higher skeleton density and smaller gaps between skeletons than the carbon support of Patent Document 2.
[0069] In the carbonized material of the present invention in which mesopores are formed, the difference in diameter due to differences in the position of the skeleton is small, the density of the skeleton is high, and the gaps between the skeletons are small, so that the specific surface area of the skeleton is larger than that of the carbon support of Patent Document 2. Therefore, in the carbonized material of the present invention in which mesopores are formed, the amount of mesopores supporting platinum nanoparticles formed per cell is increased, so that the carbonized material of the present invention in which mesopores are formed can support a large amount of platinum nanoparticles per cell.
[0070] In the three-dimensional network structure of the carbonized material of the present invention having mesopores formed therein, the gaps between the frameworks are smaller than those in the carbon support of Patent Document 2, but the gaps are large enough to allow water vapor generated by the cell reaction at the cathode to easily escape from the electrode. Therefore, in the carbonized material of the present invention having mesopores formed therein, water vapor generated by the cell reaction at the cathode can easily escape from the electrode.
[0071] The framework of the carbonized material having mesopores of the present invention has mesopores of 2 nm to 9 nm formed uniformly and at a high density, and therefore the carbonized material having mesopores of the present invention can fix a large number of platinum nanoparticles having a small particle size and a large specific surface area effective for catalytic reactions, thereby increasing catalytic activity, and inhibiting sintering of the platinum nanoparticles by fixing them in the mesopores, thereby extending the catalyst life.
[0072] In the present invention, whether or not the phenolic resin has uniform and dense mesopores formed therein can be confirmed by the following procedure. First, a small portion of the wet gel is dispersed in ethanol, dropped onto a grid for transmission electron microscope observation, and dried to prepare a sample, which is then observed with a scanning transmission electron microscope (STEM: HD-2700 (Hitachi High-Technologies Corporation), accelerating voltage 200 kV) to observe the surface pore structure at a magnification of 500,000 times. Next, a circle with a diameter of 30 to 40 nm is drawn at any point in the skeleton of the obtained STEM image where a clear mesopore is obtained as an image, and the number of mesopores with a diameter of 2 to 9 nm present in the circle is counted and divided by the circle area to obtain the mesopore density at each point. This measurement of the mesopore density at each point is performed at any 50 points in the skeleton, and the average value is taken as the mesopore density. Then, when the mesopore density of the phenolic resin in which the mesopores are formed is found to be 0.0040 pores / nm 2 More than 0.0088 pieces / nm 2 When the mesopore density is 0.0040 / nm or less, it is judged that the mesopores are formed uniformly and densely. However, since the pores may not be visible in the STEM image depending on the observation conditions, unclear areas are excluded. In other words, in the phenolic resin of the present invention in which mesopores are formed, the mesopore density is 0.0040 / nm 2 More than 0.0088 pieces / nm 2 The following is the result.
[0073] The phenolic resin having mesopores of the present invention is preferably a phenolic resin having ordered mesopores. A phenolic resin having ordered mesopores is a phenolic resin having a mesopore density of 0.0040 pores / nm 2 More than 0.0088 pieces / nm 2The term "phenolic resin" refers to a phenolic resin in which mesopores with a circular diameter of 2 nm to 9 nm are formed in a 2D hexagonal structure or an arrangement equivalent thereto. Note that in the phenolic resin in which mesopores are formed as described in the examples of the present invention, the mesopore density is 0.0041 pores / nm 2 More than 0.0053 pieces / nm 2 The following is the result.
[0074] The phenolic resin having mesopores of the present invention is a precursor to the carbonized product having mesopores of the present invention before carbonization. Although the carbonized product having mesopores of the present invention shrinks overall upon carbonization compared to the phenolic resin having mesopores of the present invention, the three-dimensional network structure of the carbonized product having mesopores of the present invention is similar to the three-dimensional network structure of the phenolic resin having mesopores of the present invention.
[0075] The carbonized material having mesopores of the present invention is suitable for use as a carbon support for a platinum catalyst used as a cathode catalyst in a polymer electrolyte fuel cell. That is, by supporting platinum nanoparticles on the carbonized material having mesopores of the present invention, more specifically, by supporting platinum nanoparticles in the mesopores of the carbonized material having mesopores of the present invention, a cathode catalyst for a polymer electrolyte fuel cell can be produced.
[0076] The method for producing a phenolic resin having mesopores according to the first embodiment of the present invention comprises the steps of: a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 83° C. or higher and 88° C. or lower to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 58° C. or higher and 67° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; The present invention is characterized by having the following.
[0077] The method for producing a phenolic resin having mesopores according to the second embodiment of the present invention comprises the steps of: a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 78°C or higher and lower than 83°C to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 63° C. or higher and 72° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; The present invention is characterized by having the following.
[0078] A method for producing a phenolic resin having mesopores according to a third embodiment of the present invention comprises the steps of: a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at 73° C. or higher and lower than 78° C. to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 67° C. or higher and 72° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; The present invention is characterized by having the following.
[0079] A method for producing a phenolic resin having mesopores according to a fourth embodiment of the present invention comprises the steps of: a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 50° C. or higher and 58° C. or lower to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 73° C. or higher and 78° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; The present invention is characterized by having the following.
[0080] The methods for producing a phenolic resin having mesopores according to the first to fourth embodiments of the present invention have some similarities, although the heating conditions in the first and second steps are different. Therefore, the different parts will be explained separately, and the similar parts will be explained by collectively referring to the methods for producing a phenolic resin having mesopores according to the first to fourth embodiments of the present invention as the method for producing a phenolic resin having mesopores according to the present invention.
[0081] The first step in the method for producing a phenolic resin having mesopores of the present invention is a step of heating a mixture of a phenolic compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product.
[0082] The phenolic compound used in the first step of the method for producing a phenolic resin having mesopores of the present invention is not particularly limited as long as it is a compound having a phenolic skeleton, and examples thereof include phenol (C6H5OH), substituted phenols in which an aromatic ring is substituted with one or more alkyl groups, specifically C6H4(OH)CH3 (any one or a combination of two or more of 2-methylphenol, 3-methylphenol, and 4-methylphenol), C6H3(OH)(CH3)2 (any one or a combination of two or more of 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, and 3,5-dimethylphenol), resorcinol (C6H4(OH)2), pyrocatechol (C6H4(OH)2), etc. Among these, phenolic compounds are preferably phenol (C6H5OH).
[0083] The formaldehyde used in the first step of the method for producing a phenolic resin having mesopores according to the present invention is usually added as an aqueous formaldehyde solution to water for preparing a mixed solution. The concentration of the aqueous formaldehyde solution is not particularly limited, and is usually 10.0% by mass or more and 40.0% by mass or less.
[0084] The alkali metal hydroxide used in the first step of the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, but from the viewpoint of preferentially proceeding with the addition reaction of phenol, sodium hydroxide, potassium hydroxide and lithium hydroxide are preferred, and sodium hydroxide is particularly preferred.
[0085] In the first step of the method for producing a phenolic resin having mesopores according to the present invention, ammonia, an organic amine such as ethanolamine, or a quaternary organic ammonium salt such as tetramethylammonium hydroxide can be used instead of an alkali metal hydroxide. By using an alkali metal hydroxide, ammonia, an organic amine, or a quaternary ammonium salt in the first step of the present invention, a reaction for producing a resol resin can be carried out under basic conditions.
[0086] Examples of the organic amine used in the first step include ethanolamine, propanolamine, alkylamine, and cyclic amine. Examples of the ethanolamine include monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, N-ethylethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, and aminoethoxyethanol. Examples of the propanolamine include 1-amino-2-propanol, 2-amino-2-methyl-1-propanol, and 2-amino-2-methyl-1,3-propanediol. Examples of the alkylamine include monomethylamine, dimethylamine, trimethylamine, ethyleneamine, ethylenediamine, diethylenetriamine, triethylenetetramine, hexamethylenetetramine, and tetraethylenepentamine. Examples of the cyclic amine include choline and morpholine.
[0087] Examples of the quaternary organic ammonium salt used in the first step include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, N,N,N-triethyl-N-(2-hydroxyethyl)ammonium hydroxide, and N,N-diethyl-N,N-di(2-hydroxyethyl)ammonium hydroxide.
[0088] The organic amine or quaternary organic ammonium salt used in the first step is preferably one having strong basicity, more preferably a quaternary ammonium salt, and particularly preferably tetramethylammonium hydroxide, tetraethylammonium hydroxide, or the like.
[0089] Examples of the nonionic surfactant used in the first step of the method for producing a phenolic resin having mesopores of the present invention include polyoxyethylene alkyl ethers and polyoxyethylene alkyl phenyl ethers. More specifically, examples of such surfactants include copolymers of polyethylene oxide (PEO) and polypropylene oxide (PPO), in particular copolymers of PPO having a molar mass of 3,000 or more and 4,000 or less and a PEO ratio in the molecule of 30% or more and 90% or less.
[0090] The water used in the first step of the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the first step of the method for producing a phenolic resin having mesopores of the present invention preferably contains fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.
[0091] In the mixture used in the first step of the method for producing a phenolic resin having mesopores of the present invention, the molar ratio of formaldehyde to the phenolic compound (formaldehyde / phenolic compound) is 2.6 or more and 5.0 or less, and from the viewpoint of promoting addition polymerization, is preferably 3.2 or more and 4.4 or less, the molar ratio of alkali metal hydroxide to the phenolic compound (alkali metal hydroxide / phenolic compound) is 0.24 or more and 0.48 or less, the molar ratio of ammonia to the phenolic compound (ammonia / phenolic compound) is 0.24 or more and 0.96 or less, the molar ratio of organic amine to the phenolic compound (organic amine / phenolic compound) is 0.24 or more and 0.96 or less, and the molar ratio of quaternary organic ammonium salt to the phenolic compound (quaternary organic ammonium salt / phenolic compound) is 0.24 or more and 0.48 or less.
[0092] In the first step of the method for producing a phenolic resin having mesopores of the present invention, the amount of nonionic surfactant mixed is an amount such that the mass ratio of the nonionic surfactant to the phenolic compounds in the first process product (nonionic surfactant / phenolic compounds) is 1.5 or more and 2.3 or less, and from the viewpoint of increasing the conversion rate of phenol to resin, the amount is preferably 1.6 or more and 2.1 or less.
[0093] The amount of water to be mixed in the first step for the phenolic resin having mesopores of the present invention is preferably an amount such that the concentration of the nonionic surfactant relative to the total amount of the first processed product is 21 mg / mL or more and 45 mg / mL or less.
[0094] The method for preparing the mixture used in the first step of the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include a method in which predetermined amounts of a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, and a nonionic surfactant are added to a predetermined amount of water and mixed. The formaldehyde, the alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, and the nonionic surfactant may be added in the form of an aqueous solution.
[0095] In the first step of the method for producing a phenolic resin having mesopores according to the first embodiment of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 83°C to 88°C to obtain a first treated product. When the heating temperature of the mixture in the first step is within the above range, a carbonized product having a structure specific to the carbonized product having mesopores according to the present invention and a phenolic resin serving as a precursor thereof can be obtained. In the first step of the phenolic resin having mesopores according to the first embodiment of the present invention, the heating temperature when heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is preferably 84°C to 86°C from the viewpoint of promoting the development of a network structure. In the first step of the method for producing a phenolic resin having mesopores according to the first embodiment of the present invention, the heating time for heating a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is from 1 hour to 6 hours, preferably from 2 hours to 4 hours.
[0096] In the first step of the method for producing a phenolic resin having mesopores according to the second embodiment of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 78°C or higher and lower than 83°C to obtain a first treated product. By heating the mixture in the first step within the above range, it is possible to obtain a carbonized product having a structure specific to the carbonized product having mesopores according to the present invention described above and a phenolic resin serving as a precursor thereof. In the first step of the method for producing a phenolic resin having mesopores according to the second embodiment of the present invention, the heating temperature when heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is preferably 79°C or higher and 81°C or lower from the viewpoint of promoting the development of a network structure. In the first step of the method for producing a phenolic resin having mesopores according to the second embodiment of the present invention, the heating time for heating a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is from 1 hour to 6 hours, preferably from 2 hours to 4 hours.
[0097] In the first step of the method for producing a phenolic resin having mesopores according to the third embodiment of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 73°C or higher and lower than 78°C to obtain a first treated product. By heating the mixture in the first step within the above range, it is possible to obtain a carbonized product having a structure specific to the carbonized product having mesopores according to the present invention described above and a phenolic resin serving as a precursor thereof. In the first step of the method for producing a phenolic resin having mesopores according to the third embodiment of the present invention, the heating temperature when heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is preferably 74°C or higher and 76°C or lower from the viewpoint of promoting the development of a network structure. In the first step of the method for producing a phenolic resin having mesopores according to the third embodiment of the present invention, the heating time for heating a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is from 1 hour to 6 hours, preferably from 2 hours to 4 hours.
[0098] In the first step of the method for producing a phenolic resin having mesopores according to the fourth embodiment of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 50°C to 58°C to obtain a first treated product. By heating the mixture in the first step within the above range, it is possible to obtain a carbonized product having a structure specific to the carbonized product having mesopores according to the present invention and a phenolic resin serving as a precursor thereof. In the first step of the method for producing a phenolic resin having mesopores according to the fourth embodiment of the present invention, the heating temperature when heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is preferably 53°C to 56°C from the viewpoint of promoting the development of a network structure. In the first step of the method for producing a phenolic resin having mesopores according to the fourth embodiment of the present invention, the heating time for heating a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is from 1 hour to 6 hours, preferably from 2 hours to 4 hours.
[0099] The second step in the method for producing a phenolic resin having mesopores of the present invention is a step of mixing water with the first treated product obtained by carrying out the first step and heating the resulting mixture to obtain a sol liquid.
[0100] The water used in the second step in the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the second step in the production of a phenolic resin having mesopores of the present invention preferably contains fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.
[0101] In the second step relating to the mesopore-formed phenolic resin of the present invention, the amount of water to be mixed with the first treated product is preferably an amount such that the concentration of the nonionic surfactant in the mixture obtained after mixing the first treated product with water is 9 mg / mL or more and 20 mg / mL or less, more preferably 10 mg / mL or more and 16 mg / mL or less.
[0102] In the second step of the method for producing a phenolic resin having mesopores of the present invention, the method for mixing water with the first treated product is not particularly limited, and examples thereof include a method in which a predetermined amount of water is added to a predetermined amount of the first treated product and mixed.
[0103] In the second step of the method for producing a phenolic resin having mesopores according to the first embodiment of the present invention, the mixture obtained by mixing the first treated product with water is heated at 58°C to 67°C to obtain a sol. The heating temperature of the mixture in the second step is within the above range, so that it is possible to obtain a carbonized product having a structure specific to the carbonized product having mesopores according to the present invention and a phenolic resin serving as a precursor thereof. In the second step of the method for producing a phenolic resin having mesopores according to the first embodiment of the present invention, the heating temperature when the mixture obtained by mixing the first treated product with water is heated is preferably 59°C to 65°C from the viewpoint of promoting the development of a network structure. In the second step of the method for producing a phenolic resin having mesopores according to the first embodiment of the present invention, the heating time when the mixture obtained by mixing the first treated product with water is heated is 12 hours to 24 hours, preferably 15 hours to 20 hours.
[0104] In the second step of the method for producing a phenolic resin having mesopores according to the second embodiment of the present invention, the mixture obtained by mixing the first treated product with water is heated at 63°C to 72°C to obtain a sol. When the heating temperature of the mixture in the second step is within the above range, it is possible to obtain a carbonized product having a structure specific to the carbonized product having mesopores according to the present invention and a phenolic resin serving as a precursor thereof. In the second step of the method for producing a phenolic resin having mesopores according to the second embodiment of the present invention, the heating temperature when the mixture obtained by mixing the first treated product with water is heated is preferably 64°C to 70°C from the viewpoint of promoting the development of a network structure. In the second step of the method for producing a phenolic resin having mesopores according to the second embodiment of the present invention, the heating time when the mixture obtained by mixing the first treated product with water is heated is 12 hours to 24 hours, preferably 15 hours to 20 hours.
[0105] In the second step of the method for producing a phenolic resin having mesopores according to the third embodiment of the present invention, the mixture obtained by mixing the first treated product with water is heated at 67°C to 72°C to obtain a sol. When the heating temperature of the mixture in the second step is within the above range, it is possible to obtain a carbonized product having a structure specific to the carbonized product having mesopores according to the present invention and a phenolic resin serving as a precursor thereof. In the second step of the method for producing a phenolic resin having mesopores according to the third embodiment of the present invention, the heating temperature when the mixture obtained by mixing the first treated product with water is heated is preferably 68°C to 70°C from the viewpoint of promoting the development of a network structure. In the second step of the method for producing a phenolic resin having mesopores according to the third embodiment of the present invention, the heating time when the mixture obtained by mixing the first treated product with water is heated is 12 hours to 24 hours, preferably 15 hours to 20 hours.
[0106] In the second step of the method for producing a phenolic resin having mesopores according to the fourth embodiment of the present invention, the mixture obtained by mixing the first treated product with water is heated at 73°C to 78°C to obtain a sol. When the heating temperature of the mixture in the second step is within the above range, it is possible to obtain a carbonized product having a structure specific to the carbonized product having mesopores according to the present invention and a phenolic resin serving as a precursor thereof. In the second step of the method for producing a phenolic resin having mesopores according to the fourth embodiment of the present invention, the heating temperature when the mixture obtained by mixing the first treated product with water is heated is preferably 74°C to 76°C from the viewpoint of promoting the development of a network structure. In the second step of the method for producing a phenolic resin having mesopores according to the fourth embodiment of the present invention, the heating time when the mixture obtained by mixing the first treated product with water is heated is 12 hours to 24 hours, preferably 15 hours to 20 hours.
[0107] The sol liquid obtained by carrying out the second step in the method for producing a phenolic resin having mesopores of the present invention may be used as it is in the gelation step. Alternatively, after carrying out the second step in the method for producing a phenolic resin having mesopores of the present invention, the sol liquid obtained by carrying out the second step and before carrying out the gelation step may be filtered, and the filtrate obtained may be used as the sol liquid in the gelation step.
[0108] The gelation step in the method for producing a phenolic resin having mesopores of the present invention is a step of mixing water with the sol liquid obtained by carrying out the second step in the method for producing a phenolic resin having mesopores of the first, second, third or fourth embodiment of the present invention, and heating the resulting mixture under pressure to obtain a wet gel.
[0109] The water used in the gelation step in the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the gelation step in the method for producing a phenolic resin having mesopores of the present invention preferably has fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.
[0110] In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, the amount of water mixed into the sol liquid is 1.5 to 6.0 times the mass of the first processed product, and preferably 2.5 to 6.0 times the mass of the first processed product.
[0111] In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, the method for mixing water with the sol liquid is not particularly limited, and examples thereof include a method in which a predetermined amount of water is added to a predetermined amount of sol liquid and mixed.
[0112] In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, a mixture obtained by mixing water with a sol liquid is heated under pressure at 120°C to 140°C to obtain a wet gel. When the heating temperature of the mixture in the gelation step is within the above range, it is possible to obtain a carbonized product having a structure specific to the carbonized product having mesopores of the present invention and a phenolic resin that serves as a precursor thereof. In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, the heating temperature when the mixture obtained by mixing water with a sol liquid is heated is preferably 125°C to 135°C from the viewpoint of promoting the formation of a gel skeleton. In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, the pressure (absolute pressure) when the mixture obtained by mixing water with a sol liquid is heated is 0.34 MPa to 0.51 MPa, preferably 0.38 MPa to 0.46 MPa. In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, the heating time when the mixture obtained by mixing water with a sol liquid is heated is 6 hours to 48 hours, preferably 20 hours to 48 hours.
[0113] The wet gel obtained by carrying out the gelling step according to the method for producing a phenolic resin having mesopores of the present invention may be dried directly in a drying step. Alternatively, after carrying out the gelling step according to the method for producing a phenolic resin having mesopores of the present invention, the wet gel obtained by carrying out the gelling step may be washed one or more times before carrying out the drying step, and the obtained wet gel may be dried in a drying step.
[0114] The drying step in the method for producing a phenolic resin having mesopores of the present invention is a step of drying the wet gel obtained by the gelling step to obtain a phenolic resin having mesopores.
[0115] In the drying step in the method for producing a phenolic resin having mesopores of the present invention, the method for drying the wet gel is not particularly limited, and examples thereof include: (i) a method in which the wet gel is added to water, dispersed in water, the obtained wet gel dispersion is freeze-granulated by spraying it into liquid nitrogen using a spray-freeze granulator, and then the obtained frozen granules are vacuum-dried to dry the wet gel; (ii) a method in which the wet gel is added to water, dispersed in water, and the obtained wet gel dispersion is sprayed into hot air using a spray dryer to heat-dry; and (iii) a method in which the wet gel is heat-dried by treatment with microwaves.
[0116] Then, a drying step according to the method for producing a phenolic resin having mesopores of the present invention is carried out to obtain a phenolic resin having mesopores.
[0117] The method for producing a carbonized material having mesopores of the present invention is characterized by comprising a carbonization step of heat-treating a phenolic resin having mesopores obtained by carrying out the method for producing a phenolic resin having mesopores of the present invention, i.e., the first, second, third or fourth embodiment of the present invention, in an inert gas atmosphere at 300°C or more and 450°C or less, calcining the resulting heat-treated product in an inert gas atmosphere at 450°C or more and 800°C or less, and carbonizing the resulting calcined product in an inert gas atmosphere at 800°C or more and 2000°C or less, thereby obtaining a carbonized material having mesopores.
[0118] In the carbonization step according to the method for producing a carbonized product having mesopores of the present invention, the heat treatment temperature for heat treating the phenolic resin having mesopores of the present invention is 300°C or higher and 450°C or lower. In the carbonization step according to the present invention, by heat treating the phenolic resin having mesopores in the above temperature range, it is possible to remove the surfactant remaining in the phenolic resin having mesopores and maintain the mesopore structure. In the carbonization step according to the method for producing a carbonized product having mesopores of the present invention, the heat treatment time for heat treating the phenolic resin having mesopores of the present invention is 30 minutes or longer and 6 hours or shorter, preferably 1 hour or longer and 3 hours or shorter. In the carbonization step according to the method for producing a carbonized product having mesopores of the present invention, the heat treatment atmosphere for heat treating the phenolic resin having mesopores of the present invention is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.
[0119] In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the firing temperature when firing the heat-treated phenolic resin having mesopores is 450°C or more and 800°C or less, and from the viewpoint of suitably removing organic-containing gas generated during carbonization of the phenolic resin, is preferably 500°C or more and 800°C or less. In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the firing time when firing the heat-treated phenolic resin having mesopores is 30 minutes or more and 6 hours or less, preferably 1 hour or more and 3 hours or less. In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the firing atmosphere when firing the heat-treated phenolic resin having mesopores is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.
[0120] In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the carbonization temperature when the burned product of the phenolic resin having mesopores is carbonized is 800°C or more and 2000°C or less, and from the viewpoint of balancing the crystallinity of the carbonized material and the economic efficiency of the production step, it is preferably 900°C or more and 1600°C or less, more preferably 1000°C or more and 1300°C or less. In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the carbonization time when the burned product of the phenolic resin having mesopores is carbonized is 30 minutes or more and 6 hours or less, preferably 1 hour or more and 3 hours or less. In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the burning atmosphere when the burned product of the phenolic resin having mesopores is carbonized is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.
[0121] Then, by carrying out the carbonization step relating to the carbonized material having mesopores of the present invention, a carbonized material having mesopores is obtained.
[0122] In the carbonized material having mesopores obtained by carrying out the method for producing a carbonized material having mesopores of the present invention, the diameter of the skeleton is 18 nm or more and 72 nm or less.
[0123] Although the skeleton of the carbonized product having mesopores formed therein obtained by carrying out the method for producing a carbonized product having mesopores formed therein of the present invention has a three-dimensional network structure connected in the three-dimensional direction, the difference in diameter due to the difference in the position of the skeleton is smaller than that of the carbon support of Patent Document 2. In addition, the three-dimensional network structure of the carbonized product having mesopores formed therein obtained by carrying out the method for producing a carbonized product having mesopores formed therein of the present invention has a higher skeleton density and smaller gaps between the skeletons than that of the carbon support of Patent Document 2. In addition, in the carbonized product having mesopores formed therein obtained by carrying out the method for producing a carbonized product having mesopores formed therein of the present invention, the difference in diameter due to the difference in the position of the skeleton is small, the skeleton density is high, and the gaps between the skeletons are small, so that the specific surface area of the skeleton is larger than that of the carbon support of Patent Document 2. Therefore, the carbonized product having mesopores formed therein obtained by carrying out the method for producing a carbonized product having mesopores formed therein of the present invention has a larger amount of mesopores per cell that support platinum nanoparticles, so that the carbonized product having mesopores formed therein obtained by carrying out the method for producing a carbonized product having mesopores formed therein of the present invention can support a larger amount of platinum nanoparticles per cell. Furthermore, the three-dimensional network structure of a carbonized material having mesopores obtained by carrying out the method for producing a carbonized material having mesopores of the present invention has gaps large enough to allow water vapor generated by a cell reaction at the cathode to easily escape from the electrode. Therefore, in the carbonized material having mesopores obtained by carrying out the method for producing a carbonized material having mesopores of the present invention, water vapor generated by a cell reaction at the cathode can easily escape from the electrode.
[0124] According to the method for producing a carbonized material having mesopores of the present invention, it is possible to produce a carbonized material in which mesopores are formed with small difference in diameter due to difference in the position of the skeleton, high skeleton density, and small gaps between the skeletons. Therefore, the method for producing a carbonized material having mesopores of the present invention can increase the specific surface area of the skeleton of the carbonized material that serves as a carrier for platinum nanoparticles, thereby increasing the amount of mesopores formed per cell that support platinum nanoparticles and increasing the amount of platinum nanoparticles supported per cell.
[0125] The skeleton of a carbonized material having mesopores obtained by carrying out the method for producing a carbonized material having mesopores of the present invention has mesopores formed therein, which are uniformly and densely distributed. Therefore, the carbonized material having mesopores obtained by carrying out the method for producing a carbonized material having mesopores of the present invention can support highly active catalytic metal nanoparticles at a high density on a support surface that is easily accessible, thereby increasing the catalytic activity per mass of the supported catalyst.
[0126] The present invention will be described using the following examples. However, the following examples are merely examples of the present invention and are not intended to be limiting.
[0127] Example 1 (1) First step In 60 g of pure water, 3.84 g of a nonionic surfactant (polyethylene oxide (PEO) and polypropylene oxide (PPO) copolymer (trade name Pluronic (registered trademark) F127, structural formula: PEO m -PPO n -PEO m An aqueous solution of 2.42 g of phenol, 8.40 g of formaldehyde solution (formaldehyde concentration: 35% by mass), and 60.65 g of 0.1 mol / L aqueous sodium hydroxide solution was placed in a flask and stirred at 200 rpm with a stirrer at an internal temperature (heating temperature) of 85°C for 120 minutes to obtain a first processed product.
[0128] (2)Second process Next, 200 g of pure water was added to the first treated product obtained in (1) in a flask, the internal temperature (heating temperature) was adjusted to 65° C., and the mixture was stirred for 20 hours to obtain a sol liquid.
[0129] (3) Gelling process The sol prepared in (2) was filtered through a 5 μm membrane filter, and the filtrate was collected. 700 g of pure water was added to 280 g of this filtrate (the total amount of the sol considering the evaporation was 300 mL), and the mixture was placed in a stainless steel sealed container and subjected to hydrothermal treatment at 130°C for 20 hours to obtain a wet gel. The gel was collected by filtration through a 5 μm membrane filter, and then redispersed in 200 g of pure water and filtered through a membrane filter again. This process was repeated three times to obtain a wet gel from which unreacted substances had been removed.
[0130] <Structure confirmation> A small portion of the wet gel was dispersed in ethanol, dropped onto a grid for transmission electron microscope observation, and dried to prepare a sample. The sample was then observed with a scanning transmission electron microscope (STEM: HD-2700 (Hitachi High-Technologies Corporation), accelerating voltage 200 kV) to observe the pore structure. The obtained STEM image is shown in Figure 1. Two STEM images at different magnifications obtained from the example and comparative example are shown in one figure. Next, to determine the diameter of the skeleton, 100 circles were circumscribed on the skeleton depiction of the obtained STEM image, and the average of these diameters was taken as the diameter of the skeleton. The results are shown in Table 1. In addition, the diameter of the spherical particles forming the skeleton was measured in Comparative Examples 6 to 10. The particle diameter of the spherical particles was determined as the average value of the diameter of the circle circumscribing 50 arbitrarily selected spherical particle images. In addition, a circle with a diameter of 30 to 40 nm was drawn at any point in the skeleton of the obtained STEM image, and the number of mesopores with a diameter of 2 to 9 nm present in the circle was counted and divided by the area of the circle to obtain the mesopore density at each point. This mesopore density measurement was performed at 50 random points in the skeleton, and the average value was taken as the mesopore density. When the mesopore density was 0.0040 pores / nm 2 More than 0.0088 pieces / nm 2When the mesopores were equal to or smaller than the above, it was judged that the mesopores were formed uniformly and densely. However, since the pores may not be visible in the STEM image depending on the observation conditions, unclear areas were excluded.
[0131] (4) Drying process The entire amount of the wet gel obtained in (3) was placed in 160 g of pure water, stirred with a high-speed stirrer at 2,000 rpm for 5 minutes, and further treated for 5 to 10 minutes in an ultrasonic cleaner with an output of 70 W to prepare a dispersion. This dispersion was freeze-granulated by spraying it into liquid nitrogen with a spray-freeze granulator, then placed in a dedicated glass container cooled with liquid nitrogen, attached to a vacuum dryer, and subjected to vacuum drying treatment at approximately -40°C for 60 hours to obtain a granulated dry gel (phenolic resin with mesopores formed). <Calculation of gel yield> Gel yield (mg / mL) = final yield of dried gel (mg) / hydrothermally treated sol (mL)
[0132] (5) Carbonization process The dried gel obtained in (4) was placed in a calcination furnace, heated to 350°C at a heating rate of 1°C / min under nitrogen gas flow, maintained at that temperature for 2 hours, then heated again to 600°C at a heating rate of 1°C / min, maintained at that temperature for 2 hours, and cooled to room temperature. Next, the gel was placed in a carbonization furnace, heated to 1000°C at a heating rate of 1°C / min under a pressurized nitrogen gas atmosphere, maintained at that temperature for 2 hours, and cooled to room temperature to obtain a carbonized material.
[0133] Example 2 The same procedure as in Example 1 was carried out except that the heating temperature in the second step was changed to 60° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0134] Example 3 The same procedure as in Example 1 was carried out except that the heating temperature in the first step was changed to 80° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0135] Example 4 The same procedure as in Example 1 was carried out, except that the heating temperature in the first step was changed to 75° C. and the heating temperature in the second step was changed to 70° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0136] Example 5 The same procedure as in Example 1 was carried out, except that the heating temperature in the first step was changed to 55° C. and the heating temperature in the second step was changed to 75° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0137] Example 6 The same procedure as in Example 1 was carried out except that in the first step, the amount of phenol was changed to 1.85 g, the amount of formaldehyde liquid (formaldehyde concentration: 35% by mass) to 6.41 g, and the heating temperature was changed to 80° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0138] Example 7 The same procedure as in Example 6 was carried out except that the heating temperature in the first step was changed to 85° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0139] Example 8 The same procedure as in Example 6 was repeated, except that the heating temperature in the first step was changed to 75° C., and the heating temperature in the second step was changed to 70° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0140] Comparative Example 1 The same procedure as in Example 1 was carried out except that the heating temperature in the second step was changed to 70° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0141] Comparative Example 2 The same procedure as in Example 1 was carried out except that the heating temperature in the first step was changed to 90° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0142] Comparative Example 3 The same procedure as in Example 1 was carried out, except that the heating temperature in the first step was changed to 90° C. and the heating temperature in the second step was changed to 55° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0143] Comparative Example 4 The same procedure as in Example 1 was carried out, except that the heating temperature in the first step was changed to 70° C., and the heating temperature in the second step was changed to 70° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0144] Comparative Example 5 The same procedure as in Example 1 was carried out, except that the heating temperature in the first step was changed to 55° C. and the heating temperature in the second step was changed to 70° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0145] Comparative Example 6 The same procedure as in Example 1 was carried out except that the heating temperature in the second step was changed to 55° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0146] Comparative Example 7 The same procedure as in Example 1 was carried out, except that the heating temperature in the first step was changed to 80° C. and the heating temperature in the second step was changed to 60° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0147] Comparative Example 8 The same procedure as in Example 1 was carried out except that the heating temperature in the first step was changed to 75° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0148] Comparative Example 9 The same procedure as in Example 1 was carried out except that the heating temperature in the first step was changed to 70° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0149] Comparative Example 10 The same procedure as in Example 1 was carried out except that the heating temperature in the first step was changed to 60° C. The pore structure of the wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in FIG.
[0150] Scanning transmission electron microscope observation confirmed that the phenolic resins in Examples 1 to 8 and Comparative Examples 6 to 10 had uniform and high-density ordered mesopores of 2 to 9 nm. On the other hand, no mesopores were observed in the phenolic resins in Comparative Examples 1 and 2, and non-uniform mesopores were observed in the phenolic resins in Comparative Examples 3 to 5.
[0151] In addition, as a result of observation with a scanning transmission electron microscope, it was confirmed that the phenolic resins in Examples 1 to 8 had a three-dimensional network structure in which the skeletal density was high and the gaps between the skeletal parts were small, whereas the phenolic resins in Comparative Examples 6 to 10 had a structure in which the skeletal density and gaps between the skeletal parts were larger than those in the Examples.
[0152] [Table 1]
[0153] [Table 2]
[0154] [Table 3]
[0155] [Table 4]
[0156] In the table, the surfactant / phenol mass ratio refers to the mass ratio of the nonionic surfactant to the phenol compound in the first process product (nonionic surfactant / phenol compound).
[0157] As a result of observation with a scanning transmission electron microscope, ordered mesopores of 2 to 9 nm were formed uniformly and at a high density in the carbonized materials obtained by carrying out the carbonization step in Examples 1 to 8 and Comparative Examples 6 to 10. On the other hand, no mesopores were confirmed in the carbonized materials obtained by carrying out the carbonization step in Comparative Examples 1 and 2, and non-uniform mesopores were formed in the carbonized materials obtained by carrying out the carbonization step in Comparative Examples 3 to 5.
[0158] Furthermore, as a result of observation with a scanning transmission electron microscope, a three-dimensional mesh structure with a high skeletal density and small gaps between skeletal parts was formed in the carbonized materials obtained by carrying out the carbonization step in Examples 1 to 8. On the other hand, in the carbonized materials obtained by carrying out the carbonization step in Comparative Examples 6 to 10, a structure with a large skeletal density and large gaps between the skeletal parts was formed compared to the examples.
Claims
1. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 83° C. or higher and 88° C. or lower to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 58° C. or higher and 67° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; A phenolic resin having mesopores formed therein, which is obtained by carrying out the steps of:
2. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 78° C. or higher and lower than 83° C. to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 63° C. or higher and 72° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; A phenolic resin having mesopores formed therein, which is obtained by carrying out the steps of:
3. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 73° C. or higher and lower than 78° C. to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 67° C. or higher and 72° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; A phenolic resin having mesopores formed therein, which is obtained by carrying out the steps of:
4. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 50° C. or higher and 58° C. or lower to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 73° C. or higher and 78° C. or lower to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower under pressure to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; A phenolic resin having mesopores formed therein, which is obtained by carrying out the steps of:
5. 5. A carbonized material having mesopores, comprising: a phenolic resin having mesopores according to claim 1 , heat-treated at 300° C. or more and 450° C. or less in an inert gas atmosphere; calcining the heat-treated product at 450° C. or more and 800° C. or less in an inert gas atmosphere; and carbonizing the calcined product at 800° C. or more and 2000° C. or less in an inert gas atmosphere to obtain a carbonized material having mesopores.
Citation Information
Patent Citations
Catalyst layer for fuel cell, carbon material for catalyst carrier, and method for manufacturing carbon material for catalyst carrier
JP2018010806A
Supported metal catalyst, method for producing same, and method for producing carrier
WO2021161929A1