Method for producing phenol resin formed with mesopore, and method for producing carbonized material formed with mesopore

A method for producing phenolic resin and carbonized products with homogeneous mesopores addresses yield and cost issues, enhancing platinum catalyst utilization and fuel cell performance by forming carbon carriers with optimized conditions.

JP2024149099APending Publication Date: 2024-10-18TOKAI CARBON CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023062774
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing methods for producing carbon carriers with homogeneous mesopores for platinum catalyst support in fuel cells are limited by low yield and high manufacturing costs due to the small amount produced per reaction vessel, and there is a need to enhance the utilization efficiency of platinum catalysts by reducing by-product generation.

Method used

A method involving specific temperature and concentration conditions for mixing phenol, formaldehyde, alkali metal hydroxide, and a nonionic surfactant to form a phenolic resin, followed by carbonization, to create a carbonized product with homogeneous mesopores, increasing yield and reducing by-products.

Benefits of technology

The method enhances the yield of carbon carriers with homogeneous mesopores, reducing manufacturing costs and improving platinum catalyst utilization efficiency by preventing aggregation and sintering, thus optimizing fuel cell performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149099000001_ABST
    Figure 2024149099000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a phenol resin formed with mesopores and a method for producing a carbonized material formed with mesopores which have homogeneous mesopores formed therein and can enhance a yield and produce less by-products.SOLUTION: A method for producing a phenol resin formed with mesopores includes: a first step of heating a mixture of a phenol compound, formaldehyde, alkali metal hydroxide, ammonia, organic amine or a quaternary organic ammonium salt, a non-ionic surface active agent, and water at 63°C or higher and lower than 78°C to obtain a first treated substance; a second step of mixing water with the first treated substance, and heating the obtained mixture at 58°C or higher and lower than 67°C to obtain a sol solution; a gelation step of mixing water with the sol solution, and heating the obtained mixture at 120°C or higher and 140°C or lower to obtain a wet gel; and a drying step of drying the wet gel to obtain a phenol resin formed with mesopores, in which a mass ratio of the non-ionic surface active agent to the phenol compound is 1.7 or more and 3.0 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a phenolic resin having mesopores and a method for producing a carbonized material having mesopores. [Background technology]

[0002] As part of recent research and development aimed at realizing a carbon-neutral society, there is currently development in the automotive field to replace automobiles equipped with engines that use fossil fuels with electric vehicles that use secondary batteries such as lithium-ion secondary batteries as their energy device, and fuel cell vehicles that use fuel cells as their energy device.

[0003] Due to the improvement of the charging capacity and the fall of the price of lithium-ion secondary batteries, passenger cars have rapidly become popular in recent years, and as a result, electric vehicles are being replaced. On the other hand, trucks and buses have a longer driving distance per charge than passenger cars, so a single charge of secondary batteries such as lithium-ion secondary batteries is not enough to cover the required driving distance, and it is not realistic to increase the number of batteries installed due to the weight and cost of the batteries. For this reason, fuel cell vehicles are considered to be the likely replacements for trucks and buses.

[0004] The fuel cell used in fuel cell-equipped vehicles is a polymer electrolyte fuel cell (PEFC) consisting of an anode catalyst layer, a polymer electrolyte membrane, and a cathode catalyst layer. The cathode, which is the air electrode of the fuel cell, uses a platinum catalyst in which platinum or a platinum alloy is supported on a carbon support.

[0005] Platinum is expensive and there is a need to reduce its use because of the scarcity of platinum reserves worldwide. Therefore, in order to reduce the amount of platinum used as a cathode catalyst in fuel cells, attempts have been made to reduce the amount of platinum used by making it into small particles and supporting it on a carbon support.

[0006] However, when small platinum particles are repeatedly used as a catalyst for a cell reaction, they tend to aggregate and sinter to become larger particles. When the particles become larger, their performance as a catalyst for a cell reaction decreases, so simply supporting small platinum particles results in a high rate of deterioration in the performance of the fuel cell.

[0007] Therefore, platinum nanoparticles have been supported in the mesopores of a carbon support in which mesopores are formed, thereby preventing the platinum nanoparticles from agglomerating and sintering due to repeated use in battery reactions. Patent Document 1 discloses a platinum-supported metal catalyst in which a platinum catalyst is supported on mesoporous carbon nanodendrites (MCND).

[0008] However, in the platinum-supported metal catalyst described in Patent Document 1, uniform mesopores are not formed in the support, and platinum particles supported in the deep mesopores are unable to contribute to the catalytic reaction, resulting in low utilization efficiency of the platinum catalyst.

[0009] For this reason, Patent Document 2 discloses a supported metal catalyst for improving the utilization efficiency of a platinum catalyst supported on a carbon support, the supported metal catalyst comprising a support which is an aggregate of conductive particles, and active metal particles dispersed and supported on the conductive particles, the conductive particles including a plurality of pores, the pores having an average inlet pore diameter of 1 to 20 nm, a standard deviation of the average inlet pore diameter being 50% or less of the average inlet pore diameter, the number fraction of the active metal particles supported on the surface region of the conductive particles being 50% or more, and the surface region being a region on the surface of the conductive particle, or a region within the pores within a depth of 15 nm from the surface. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2018-10806 A [Patent Document 2] International Publication No. 2021 / 161929 Summary of the Invention [Problem to be solved by the invention]

[0011] In the supported metal catalyst of Patent Document 2, the framework of the carbon support on which the metal particles are supported has a three-dimensional network structure in which spherical carbon nanoparticles are connected in a three-dimensional direction, and the framework has mesopores formed therein that can support platinum nanoparticles within the pores.

[0012] The mesopores formed in the carbon support of the supported metal catalyst in Patent Document 2 are homogeneous pores. In addition, a supported metal catalyst in which platinum nanoparticles are supported in the mesopores of a carbon support in which homogeneous mesopores are formed is expected to have a high utilization efficiency of the platinum catalyst.

[0013] Therefore, from the viewpoint of reducing the manufacturing cost, it is desired to increase the yield of the carbon support in which uniform mesopores are formed. However, since the carbon support of Patent Document 2 is a nanoparticle that is generated in a dilute aqueous solution, the amount of the carbon support generated per volume of the synthesis reaction vessel is small, which causes a problem of high manufacturing costs. In order to reduce the manufacturing cost, it is necessary to increase the amount of the carbon support generated per reaction vessel, and it is necessary to find the optimal reaction conditions that increase the gel conversion rate of the raw material phenol.

[0014] Therefore, an object of the present invention is to provide a method for producing a phenolic resin having homogeneous mesopores and a carbonized product thereof, which can achieve a high yield and reduce the production of by-products. [Means for solving the problem]

[0015] The above problems are solved by the present invention described below. That is, the present invention provides (1) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 63° C. or higher and lower than 78° C. to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 58° C. or higher but lower than 67° C. to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; having A method for producing a phenolic resin having mesopores, wherein a mass ratio of the nonionic surfactant to the phenolic compound is 1.7 or more and 3.0 or less. (2) The method for producing a phenolic resin having mesopores according to (1), wherein the amount of water to be mixed in the first step is an amount that results in a concentration of the nonionic surfactant of 21 mg / mL or more and 45 mg / mL or less relative to the total amount of the first processed product. (3) The method for producing a phenolic resin having mesopores according to (1), wherein the heating temperature in the first step is 68°C or higher and lower than 78°C. (4) The method for producing a phenolic resin having mesopores according to (1), wherein the heating temperature in the second step is 63° C. or higher and lower than 67° C. (5) A method for producing a carbonized material having mesopores, comprising a carbonization step of heat-treating a phenolic resin having mesopores produced by the method for producing a phenolic resin having mesopores described in any one of (1) to (4) in an inert gas atmosphere at 300° C. or more and 450° C. or less, calcining the heat-treated product in an inert gas atmosphere at 450° C. or more and 800° C. or less, and carbonizing the calcined product in an inert gas atmosphere at 800° C. or more and 2000° C. or less to obtain a carbonized product. This provides: Effect of the Invention

[0016] According to the present invention, there can be provided a method for producing a phenolic resin having homogeneous mesopores and a carbonized product thereof, which can achieve a high yield and reduce the production of by-products, and a method for producing a phenolic resin having mesopores and a carbonized product thereof. [Brief description of the drawings]

[0017] [Figure 1] 1 is a STEM image of the phenol resin obtained in Example 1. [Diagram 2] 1 is a STEM image of the phenol resin obtained in Example 2. [Diagram 3] 1 is a STEM image of the phenol resin obtained in Example 3. [Figure 4] 1 is a STEM image of the phenol resin obtained in Example 4. [Diagram 5] 1 is a STEM image of the phenol resin obtained in Example 5. [Figure 6] 1 is a STEM image of the phenol resin obtained in Example 6. [Figure 7] 1 is a STEM image of the phenol resin obtained in Example 7. [Figure 8] 1 is a STEM image of the phenol resin obtained in Example 8. [Figure 9] 1 is a STEM image of the phenol resin obtained in Example 9. [Figure 10] 1 is a STEM image of the phenol resin obtained in Comparative Example 1. [Figure 11] 1 is a STEM image of the phenol resin obtained in Comparative Example 2. [Figure 12] 1 is a STEM image of the phenol resin obtained in Comparative Example 3. [Figure 13] 1 is a STEM image of the phenol resin obtained in Comparative Example 4. [Figure 14] 1 is a STEM image of the phenol resin obtained in Comparative Example 5. [Figure 15] 1 is a STEM image of the phenol resin obtained in Comparative Example 6. [Figure 16] 1 is a STEM image of the phenol resin obtained in Comparative Example 7. [Figure 17] 1 is a STEM image of the phenol resin obtained in Comparative Example 8. [Figure 18] 1 is a STEM image showing an example of a by-product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings as appropriate. The detailed description of the present invention below is an example of an embodiment, and the present invention is not to be construed as being limited to this embodiment.

[0019] The method for producing a phenolic resin having mesopores of the present invention comprises the steps of: A first process for obtaining a first treated product by heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 63° C. or higher and lower than 78° C.; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 58° C. or higher but lower than 67° C. to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; having The mass ratio of the nonionic surfactant to the phenol compound is 1.7 or more and 3.0 or less.

[0020] The first step in the method for producing a phenolic resin having mesopores of the present invention is a step of heating a mixture of a phenolic compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product.

[0021] The phenol compound used in the first step of the method for producing a phenolic resin having mesopores according to the present invention is not particularly limited as long as it is a compound having a phenol skeleton. 6 H 5 OH), substituted phenols in which the aromatic ring is substituted with one or more alkyl groups, specifically C 6 H 4 (OH)CH 3 (2-methylphenol, 3-methylphenol, and 4-methylphenol, any one or a combination of two or more of them), C 6 H 3 (OH)(CH 3 ) 2 (2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, and 3,5-dimethylphenol), resorcinol (C 6 H 4 (OH) 2 ), pyrocatechol (C 6 H 4 (OH) 2 Among these, phenolic compounds include phenol (C 6 H 5 OH) is preferred.

[0022] The formaldehyde used in the first step of the method for producing a phenolic resin having mesopores according to the present invention is usually added as an aqueous formaldehyde solution to water for preparing a mixed solution. The concentration of the aqueous formaldehyde solution is not particularly limited, and is usually 10.0% by mass or more and 40.0% by mass or less.

[0023] The alkali metal hydroxide used in the first step of the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, but from the viewpoint of preferentially proceeding with the addition reaction of phenol, sodium hydroxide, potassium hydroxide and lithium hydroxide are preferred, and sodium hydroxide is particularly preferred.

[0024] In the first step of the method for producing a phenolic resin having mesopores according to the present invention, ammonia, an organic amine such as ethanolamine, or a quaternary organic ammonium salt such as tetramethylammonium hydroxide can be used instead of an alkali metal hydroxide. By using an alkali metal hydroxide, ammonia, an organic amine, or a quaternary ammonium salt in the first step of the present invention, a reaction for producing a resol resin can be carried out under basic conditions.

[0025] Examples of the organic amine used in the first step include ethanolamine, propanolamine, alkylamine, and cyclic amine. Examples of the ethanolamine include monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, N-ethylethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, and aminoethoxyethanol. Examples of the propanolamine include 1-amino-2-propanol, 2-amino-2-methyl-1-propanol, and 2-amino-2-methyl-1,3-propanediol. Examples of the alkylamine include monomethylamine, dimethylamine, trimethylamine, ethyleneamine, ethylenediamine, diethylenetriamine, triethylenetetramine, hexamethylenetetramine, and tetraethylenepentamine. Examples of the cyclic amine include choline and morpholine.

[0026] Examples of the quaternary organic ammonium salt used in the first step include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, N,N,N-triethyl-N-(2-hydroxyethyl)ammonium hydroxide, and N,N-diethyl-N,N-di(2-hydroxyethyl)ammonium hydroxide.

[0027] The organic amine or quaternary organic ammonium salt used in the first step is preferably one having strong basicity, more preferably a quaternary organic ammonium salt, and particularly preferably tetramethylammonium hydroxide, tetraethylammonium hydroxide, or the like.

[0028] Examples of the nonionic surfactant used in the first step of the method for producing a phenolic resin having mesopores of the present invention include polyoxyethylene alkyl ethers and polyoxyethylene alkyl phenyl ethers. More specifically, examples of such surfactants include copolymers of polyethylene oxide (PEO) and polypropylene oxide (PPO), in particular copolymers of PPO having a molar mass of 3,000 or more and 4,000 or less and a PEO ratio in the molecule of 30% or more and 90% or less.

[0029] The water used in the first step of the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the first step of the method for producing a phenolic resin having mesopores of the present invention preferably contains fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.

[0030] In the first step of the method for producing a phenolic resin having mesopores of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated.

[0031] In the mixture used in the first step of the method for producing a phenolic resin having mesopores of the present invention, the molar ratio of formaldehyde to the phenolic compound (formaldehyde / phenolic compound) is 2.6 or more and 5.0 or less, and from the viewpoint of promoting addition polymerization, is preferably 3.2 or more and 4.4 or less, the molar ratio of alkali metal hydroxide to the phenolic compound (alkali metal hydroxide / phenolic compound) is 0.24 or more and 0.48 or less, the molar ratio of ammonia to the phenolic compound (ammonia / phenolic compound) is 0.24 or more and 0.96 or less, the molar ratio of organic amine to the phenolic compound (organic amine / phenolic compound) is 0.24 or more and 0.96 or less, and the molar ratio of quaternary organic ammonium salt to the phenolic compound (quaternary organic ammonium salt / phenolic compound) is 0.24 or more and 0.48 or less.

[0032] The method for preparing the mixture used in the first step in the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include a method in which predetermined amounts of a phenolic compound, formaldehyde, and an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, and a nonionic surfactant are added to a predetermined amount of water and mixed. The formaldehyde, and the alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, and a nonionic surfactant may be added in the form of an aqueous solution.

[0033] In the first step of the method for producing a phenolic resin having mesopores according to the present invention, the amount of the nonionic surfactant mixed when mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is an amount such that the mass ratio of the nonionic surfactant to the phenolic compound in the first treated product (nonionic surfactant / phenolic compound) is 1.7 to 3.0, preferably 1.8 to 2.5, and more preferably 1.8 to 2.3. By setting the mass ratio of the nonionic surfactant to the phenolic compound within the above range, the conversion rate of the phenolic compound to a phenolic resin having mesopores (phenol conversion rate) can be increased, and the production of by-products can be reduced.

[0034] The amount of water to be mixed in the first step of the method for producing a phenolic resin having mesopores of the present invention is preferably an amount that results in a concentration of the nonionic surfactant of 21 mg / mL or more and 45 mg / mL or less relative to the total amount of the first processed product, and is preferably 25 mg / mL or more and 45 mg / mL or less in terms of increasing the effect of increasing the phenol conversion rate from the phenol compound to a phenolic resin having mesopores and increasing the effect of reducing the production of by-products.

[0035] In the first step of the method for producing a phenolic resin having mesopores of the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated at 63°C or more and less than 78°C to obtain a first treated product. By heating the mixture in the first step within the above range, a carbonized material having mesopores and a phenolic resin having mesopores, which is a precursor of the carbonized material, can be obtained. In the first step of the method for producing a phenolic resin having mesopores of the present invention, the heating temperature when heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is preferably 68°C or more and less than 78°C from the viewpoint of promoting the development of a network structure. In the first step of the method for producing a phenolic resin having mesopores of the present invention, the heating time for heating the mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is from 1 hour to 6 hours, preferably from 2 hours to 4 hours.

[0036] The second step in the method for producing a phenolic resin having mesopores of the present invention is a step of mixing water with the first treated product obtained by carrying out the first step and heating the resulting mixture to obtain a sol liquid.

[0037] The water used in the second step in the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the second step in the method for producing a phenolic resin having mesopores of the present invention preferably contains fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.

[0038] In the second step of the method for producing a phenolic resin having mesopores of the present invention, the amount of water to be mixed with the first treated product is preferably an amount such that the concentration of the nonionic surfactant in the mixture obtained after mixing the first treated product with water is 9 mg / mL or more and 20 mg / mL or less, more preferably 10 mg / mL or more and 16 mg / mL or less.

[0039] In the second step of the method for producing a phenolic resin having mesopores of the present invention, the method for mixing water with the first treated product is not particularly limited, and examples thereof include a method in which a predetermined amount of water is added to a predetermined amount of the first treated product and mixed.

[0040] In the second step of the method for producing a phenolic resin having mesopores of the present invention, the mixture obtained by mixing the first treated product with water is heated at 58°C or more and less than 67°C to obtain a sol. By heating the mixture in the second step within the above range, it is possible to obtain a carbonized material having mesopores and a phenolic resin having mesopores as its precursor. In the second step of the method for producing a phenolic resin having mesopores of the present invention, the heating temperature when the mixture obtained by mixing the first treated product with water is heated is preferably 63°C or more and less than 67°C from the viewpoint of promoting the development of a network structure. In the second step of the method for producing a phenolic resin having mesopores of the present invention, the heating time when the mixture obtained by mixing the first treated product with water is heated is 12 hours or more and 24 hours or less, preferably 15 hours or more and 20 hours or less.

[0041] The sol liquid obtained by carrying out the second step in the method for producing a phenolic resin having mesopores of the present invention may be used as it is in the gelation step. Alternatively, after carrying out the second step in the method for producing a phenolic resin having mesopores of the present invention, the sol liquid obtained by carrying out the second step and before carrying out the gelation step may be filtered, and the filtrate obtained may be used as the sol liquid in the gelation step.

[0042] The gelation step in the method for producing a phenolic resin having mesopores of the present invention is a step of mixing water with the sol liquid obtained by carrying out the second step in the method for producing a phenolic resin having mesopores of the present invention, and heating the resulting mixture to obtain a wet gel.

[0043] The water used in the gelation step in the method for producing a phenolic resin having mesopores of the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the gelation step in the method for producing a phenolic resin having mesopores of the present invention preferably has fewer impurities in order to prevent inhibition of the addition polymerization reaction by impurities.

[0044] In the gelation step in the method for producing a phenolic resin having mesopores of the present invention, the amount of water mixed into the sol liquid is preferably 1.5 to 6.0 times, and more preferably 2.5 to 6.0 times, the mass of the first processed product.

[0045] In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, the method for mixing water with the sol liquid is not particularly limited, and examples thereof include a method in which a predetermined amount of water is added to a predetermined amount of sol liquid and mixed.

[0046] In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, a mixture obtained by mixing water with a sol liquid is heated at 120°C or more and 140°C or less to obtain a wet gel. When the heating temperature of the mixture in the gelation step is within the above range, a carbonized material having mesopores and a phenolic resin having mesopores as a precursor thereof can be obtained. In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, the pressure (absolute pressure) when the mixture obtained by mixing water with a sol liquid is heated is 0.34 MPa or more and 0.51 MPa or less, preferably 0.38 MPa or more and 0.46 MPa or less. In the gelation step according to the method for producing a phenolic resin having mesopores of the present invention, the heating time when the mixture obtained by mixing water with a sol liquid is heated is 6 hours or more and 48 hours or less, preferably 20 hours or more and 48 hours or less.

[0047] The wet gel obtained by carrying out the gelling step according to the method for producing a phenolic resin having mesopores of the present invention may be dried directly in a drying step. Alternatively, after carrying out the gelling step according to the method for producing a phenolic resin having mesopores of the present invention, the wet gel obtained by carrying out the gelling step may be washed one or more times before carrying out the drying step, and the obtained wet gel may be dried in a drying step.

[0048] The drying step in the method for producing a phenolic resin having mesopores of the present invention is a step of drying the wet gel obtained by the gelling step to obtain a phenolic resin having mesopores.

[0049] In the drying step in the method for producing a phenolic resin having mesopores of the present invention, the method for drying the wet gel is not particularly limited, and examples thereof include: (i) a method in which the wet gel is added to water, dispersed in water, the obtained wet gel dispersion is freeze-granulated by spraying it into liquid nitrogen using a spray-freeze granulator, and then the obtained frozen granules are vacuum-dried to dry the wet gel; (ii) a method in which the wet gel is added to water, dispersed in water, and the obtained wet gel dispersion is sprayed into hot air using a spray dryer to heat-dry; and (iii) a method in which the wet gel is heat-dried by treatment with microwaves.

[0050] The phenolic resin obtained by carrying out the drying step according to the method for producing a phenolic resin having mesopores of the present invention is the phenolic resin having mesopores of the present invention.

[0051] The method for producing a carbonized material having mesopores of the present invention is characterized by comprising a carbonization step of heat-treating a phenolic resin having mesopores, obtained by carrying out the method for producing a phenolic resin having mesopores of the present invention, in an inert gas atmosphere at 300°C or more and 450°C or less, then calcining the resulting heat-treated product in an inert gas atmosphere at 450°C or more and 800°C or less, and then carbonizing the resulting calcined product in an inert gas atmosphere at 800°C or more and 2000°C or less, to obtain a carbonized material having mesopores.

[0052] In the carbonization step according to the method for producing a carbonized product having mesopores of the present invention, the heat treatment temperature for heat treating the phenolic resin having mesopores of the present invention is 300°C or higher and 450°C or lower. In the carbonization step according to the present invention, by heat treating the phenolic resin having mesopores in the above temperature range, it is possible to remove the surfactant remaining in the phenolic resin having mesopores and maintain the mesopore structure. In the carbonization step according to the method for producing a carbonized product having mesopores of the present invention, the heat treatment time for heat treating the phenolic resin having mesopores of the present invention is 30 minutes or longer and 6 hours or shorter, preferably 1 hour or longer and 3 hours or shorter. In the carbonization step according to the method for producing a carbonized product having mesopores of the present invention, the heat treatment atmosphere for heat treating the phenolic resin having mesopores of the present invention is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.

[0053] In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the firing temperature when firing the heat-treated phenolic resin having mesopores is 450°C or more and 800°C or less, and from the viewpoint of suitably removing organic-containing gas generated during carbonization of the phenolic resin, is preferably 500°C or more and 800°C or less. In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the firing time when firing the heat-treated phenolic resin having mesopores is 30 minutes or more and 6 hours or less, preferably 1 hour or more and 3 hours or less. In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the firing atmosphere when firing the heat-treated phenolic resin having mesopores is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.

[0054] In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the carbonization temperature when the burned product of the phenolic resin having mesopores is carbonized is 800°C or more and 2000°C or less, and from the viewpoint of balancing the crystallinity of the carbonized material and the economic efficiency of the production step, it is preferably 900°C or more and 1600°C or less, more preferably 1000°C or more and 1300°C or less. In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the carbonization time when the burned product of the phenolic resin having mesopores is carbonized is 30 minutes or more and 6 hours or less, preferably 1 hour or more and 3 hours or less. In the carbonization step according to the method for producing a carbonized material having mesopores of the present invention, the burning atmosphere when the burned product of the phenolic resin having mesopores is carbonized is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.

[0055] The carbonized product obtained by the method for producing a carbonized product having mesopores of the present invention has homogeneous mesopores. Examples of such carbonized products include spherical carbon nanoparticles having homogeneous mesopores (hereinafter also referred to as carbon support (1)), the carbon support on which the metal catalyst is supported in the supported metal catalyst of Patent Document 2, i.e., a carbon support in which a large number of spherical carbon nanoparticles having homogeneous mesopores are connected to form a three-dimensional network structure (hereinafter also referred to as carbon support (2)), and a carbon support in which the skeleton of the carbonized product having mesopores has a three-dimensional network structure connected in the three-dimensional direction and in which the difference in diameter due to the difference in the position of the skeleton is small (hereinafter also referred to as carbon support (3)).

[0056] In the present invention, the term "homogeneous mesopores" means that, when the surface pore structure of a phenolic resin in which mesopores are formed is observed at a magnification of 500,000 times in a scanning transmission electron microscope image, mesopores having a circular diameter of 2 to 9 nm are evenly spaced on the skeleton surface at a density of 0.0040 pores / nm. 2 More than 0.0088 pieces / nm 2This means that the pores are arranged at a surface density of 0.0047 pores / nm2 or less, and that the arrangement of the pores is formed in a 2D hexagonal structure or an arrangement equivalent thereto. In the present invention, homogeneous mesopores can also be referred to as ordered mesopores, and the phenolic resin of the present invention in which mesopores are formed is preferably a phenolic resin in which ordered mesopores are formed. In the phenolic resin in which mesopores are formed described in the examples of the present invention, the mesopore density is 0.0047 pores / nm2 or less. 2 More than 0.0054 pieces / nm 2 The following is the result.

[0057] The carbon support (1) is a carbonized material and has homogeneous mesopores. The structure of the carbon support (1) is a structure in which a single spherical carbon nanoparticle having homogeneous mesopores is present or a plurality of spherical carbon nanoparticles having homogeneous mesopores are connected. The structure in which a plurality of spherical carbon nanoparticles are connected in the carbon support (1) is not a three-dimensional mesh structure like that of the carbon support (2), but rather a structure in which the spherical particles do not form a partial integral structure (neck structure) with other particles but exist alone or the particles simply aggregate together and do not form a three-dimensional mesh structure.

[0058] The carbon support (2) is a carbonized material, and has homogeneous mesopores formed in the skeleton. The structure of this carbon support (2) has a three-dimensional network structure formed by spherical carbon nanoparticles that form the skeleton and are connected in a three-dimensional direction. Therefore, in the skeleton of the carbon support (2), the largest diameter part of the connected spherical carbon nanoparticles becomes the part of the skeleton with a large diameter, and the connection part of adjacent carbon nanoparticles becomes the part of the skeleton with a small diameter, and protrusions and constrictions originating from the spherical carbon nanoparticles are observed on the wall surface of the skeleton. The carbon support (2) has gaps large enough to allow water vapor generated by the cell reaction at the cathode to easily escape from the electrode.

[0059] The carbon support (3) is a carbonized material, and has homogeneous mesopores formed in the skeleton. The structure of the carbon support (3) has a three-dimensional mesh structure in which the skeleton is connected in a three-dimensional direction, and the difference in diameter due to the difference in the position of the skeleton is smaller than that of the skeleton of the carbon support (2). Furthermore, the carbon support (3) has a higher density of the skeleton and smaller gaps between the skeletons than the carbon support (2). Furthermore, the carbon support (3) has a smaller difference in diameter due to the difference in the position of the skeleton, a higher density of the skeleton, and smaller gaps between the skeletons, so that the specific surface area of ​​the skeleton is larger than that of the carbon support (2). Therefore, the carbon support (3) has a larger amount of mesopores per cell that support platinum nanoparticles, and can support a larger amount of platinum nanoparticles per cell.

[0060] Although the gaps between the skeletons of the carbon support (3) are smaller than those between the skeletons of the carbon support (2), the gaps are large enough to allow water vapor generated by the cell reaction at the cathode to easily escape from the electrode. Therefore, the carbon support (3) allows water vapor generated by the cell reaction at the cathode to easily escape from the electrode.

[0061] The phenolic resin obtained by the method for producing a phenolic resin having mesopores of the present invention is a pre-carbonized product, that is, a precursor of the carbonized product obtained by the method for producing a carbonized product having mesopores of the present invention. Although the carbonized product obtained by the method for producing a carbonized product having mesopores of the present invention shrinks overall upon carbonization compared to the phenolic resin obtained by the method for producing a phenolic resin having mesopores of the present invention, the structure of the carbonized product obtained by the method for producing a carbonized product having mesopores of the present invention is similar to the structure of the phenolic resin obtained by the method for producing a phenolic resin having mesopores of the present invention.

[0062] The method for producing a phenolic resin having mesopores of the present invention has a high conversion rate (phenol conversion rate) at which the raw material phenol compound is converted into a phenolic resin having mesopores, and produces very little by-products. In other words, the method for producing a phenolic resin having mesopores and the method for producing a carbonized product having mesopores of the present invention can increase the yields of the phenolic resin having mesopores and the carbonized product.

[0063] The carbonized material obtained by the method for producing a carbonized material having mesopores of the present invention is suitable for use as a carbon support for a platinum catalyst used as a cathode catalyst in a polymer electrolyte fuel cell. That is, by supporting platinum nanoparticles on the carbonized material having mesopores of the present invention, more specifically, by supporting platinum nanoparticles in the mesopores of the carbonized material having mesopores of the present invention, a cathode catalyst for a polymer electrolyte fuel cell can be produced. EXAMPLES

[0064] The present invention will be described using the following examples. However, the following examples are merely examples of the present invention and are not intended to be limiting.

[0065] Example 1 (1) First step In 60 g of pure water, 3.84 g of a nonionic surfactant (polyethylene oxide (PEO) and polypropylene oxide (PPO) copolymer (trade name Pluronic (registered trademark) F127, structural formula: PEO m -PPO n -PEO m An aqueous solution of 1.85 g of phenol, 6.41 g of formaldehyde solution (formaldehyde concentration: 35 mass%), and 60.65 g of 0.1 mol / L aqueous sodium hydroxide solution was placed in a flask and stirred at 200 rpm with a stirrer at an internal temperature (heating temperature) of 75°C for 120 minutes to obtain a first processed product.

[0066] (2)Second process Next, 200 g of pure water was added to the first treated product obtained in (1) in a flask, the internal temperature (heating temperature) was adjusted to 65° C., and the mixture was stirred for 20 hours to obtain a sol liquid.

[0067] (3) Gelling process The sol prepared in (2) was filtered through a 5 μm membrane filter, and the filtrate was collected. 700 g of pure water was added to 280 g of this filtrate (the total amount of the sol considering the evaporation was 300 mL), and the mixture was placed in a stainless steel sealed container and subjected to hydrothermal treatment at 130°C for 20 hours to obtain a wet gel. The gel was collected by filtration through a 5 μm membrane filter, and then redispersed in 200 g of pure water and filtered through a membrane filter again. This process was repeated three times to obtain a wet gel from which unreacted substances had been removed.

[0068] <Structure confirmation> A small portion of the wet gel was dispersed in ethanol, dropped onto a grid for transmission electron microscope observation, and dried to prepare a sample. The sample was then observed with a scanning transmission electron microscope (STEM: HD-2700 (Hitachi High-Technologies Corporation), accelerating voltage 200 kV) to observe the surface pore structure. Low-magnification and high-magnification images of the obtained STEM images are shown in Figure 1. The particle diameter of the spherical particles was determined as the average value of the diameter of circles circumscribed on 50 arbitrarily selected spherical particle images. Regarding by-products, particles that are 5 times larger than the average particle diameter present in any 10 μm × 10 μm field of view of the STEM image are defined as by-products (large particles), and the number of particles per 100 μm is defined as 10 particles (large particles). 2 If the number was more than this, it was judged as "many," if the number was less than this, it was judged as "present," and if no particles were observed at all, it was judged as "absent." Figure 18 shows an example of a STEM image obtained by observing by-product 1 in the wet gel. In addition, a circle with a diameter of 30 nm to 40 nm was drawn at any point in the skeleton of the obtained STEM image, and the number of mesopores with a diameter of 2 nm to 9 nm present in the circle was counted and divided by the area of ​​the circle to determine the mesopore density at each point. This mesopore density measurement was performed at 50 random points in the skeleton, and the average value was taken as the mesopore density. When the mesopore density was 0.0040 pores / nm 2 More than 0.0088 pieces / nm2 It was determined that homogeneous mesopores had formed when the mesopores were equal to or smaller than the above. However, since pores may not be visible in STEM images depending on the observation conditions, unclear areas were excluded.

[0069] (4) Drying process The entire amount of the wet gel obtained in (3) was placed in 160 g of pure water, stirred with a high-speed stirrer at 2,000 rpm for 5 minutes, and further treated in an ultrasonic cleaner with an output of 70 W for 5 to 10 minutes to prepare a dispersion. This dispersion was freeze-granulated by spraying it into liquid nitrogen with a spray-freeze granulator, then placed in a dedicated glass container cooled with liquid nitrogen, attached to a vacuum dryer, and subjected to vacuum drying treatment at approximately -40°C for 60 hours to obtain a granulated dry gel (phenolic resin with mesopores formed).

[0070] <Calculation of gel yield> Gel yield (mg / mL) = final yield of dried gel (mg) / hydrothermally treated sol (mL)

[0071] <Calculation of phenol conversion rate> If the weight loss at around 330-360°C in thermogravimetric analysis (TG) in nitrogen gas is considered to be the decomposition of the surfactant, the amount of surfactant in the dried gel is estimated to be 47%. Therefore, the amount of phenolic resin in the obtained dried gel is 53%. Furthermore, based on the stoichiometric ratio of phenol to formaldehyde, the amount of phenol in the phenolic resin is 87.7%. Therefore, if the amount of the recovered dried gel is A (mg / mL), the amount of phenol in the gel, B (mg / mL), is: B = A x 0.53 x 0.877 (mg / mL) Since the total amount of the sol obtained in the second step of (2) is 300 mL, if the amount of phenol added in the first step of (1) is C, the phenol conversion rate can be calculated by the following formula. Phenol conversion rate (%) = (B x 300 / C) x 100

[0072] (5) Carbonization process The dried gel obtained in (4) was placed in a calcination furnace, heated to 350°C at a heating rate of 1°C / min under nitrogen gas flow, maintained for 2 hours, then heated again to 600°C at a heating rate of 1°C / min, maintained for 2 hours, and cooled to room temperature. Next, it was placed in a carbonization furnace, heated to 1000°C at a heating rate of 1°C / min under a pressurized nitrogen gas atmosphere, maintained for 2 hours, and cooled to room temperature to obtain a carbonized material.

[0073] (Examples 2 to 9, Comparative Examples 1 to 8) The same procedure as in Example 1 was carried out except that the blend amounts and temperature conditions were as shown in Tables 1 to 3. The surface pore structure of each wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in Figures 2 to 17.

[0074] As a result of observation with a scanning transmission electron microscope, it was confirmed that the phenol resins had homogeneous mesopores formed in Examples 1 to 9 and Comparative Examples 1 to 3 and 7 to 8. In Comparative Examples 4 to 6, the formation of homogeneous mesopores was insufficient or no mesopores were formed.

[0075] In Comparative Examples 1 to 3, it was confirmed that the phenolic resin had homogeneous mesopores, but the yield (gel yield) was lower than that in Examples 1 to 9. In Comparative Examples 3, 7 to 8, it was confirmed that the phenolic resin had homogeneous mesopores, but the by-products were 10 / 100 μm. 2 The above occurred.

[0076] [Table 1]

[0077] [Table 2]

[0078] [Table 3]

[0079] In the table, the surfactant / phenol mass ratio refers to the mass ratio of the nonionic surfactant to the phenol compound in the first processed product (nonionic surfactant / phenol compound). The first process temperature refers to the internal temperature (heating temperature) of the first process, the second process temperature refers to the internal temperature (heating temperature) of the second process, and the gelation process temperature refers to the hydrothermal treatment temperature of the gelation process.

[0080] In addition, when the carbonized materials obtained by carrying out the carbonization step in the examples and comparative examples were observed with a scanning transmission electron microscope, uniform mesopores were formed in Examples 1 to 9 and Comparative Examples 1 to 3 and 7 to 8. On the other hand, in Comparative Examples 4 to 6, the formation of mesopores was insufficient or no mesopores were formed. [Explanation of symbols]

[0081] 1 By-products

Claims

1. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, a quaternary organic ammonium salt, a nonionic surfactant, and water at a temperature of 63° C. or higher and lower than 78° C. to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture at a temperature of 58° C. or higher but lower than 67° C. to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having mesopores; having A method for producing a phenolic resin having mesopores, wherein a mass ratio of the nonionic surfactant to the phenolic compound is 1.7 or more and 3.0 or less.

2. 2. The method for producing a phenolic resin having mesopores according to claim 1, wherein an amount of water to be mixed in the first step is an amount such that a concentration of the nonionic surfactant relative to a total amount of the first processed product is 21 mg / mL or more and 45 mg / mL or less.

3. 2. The method for producing a phenolic resin having mesopores according to claim 1, wherein the heating temperature in the first step is 68° C. or higher and lower than 78° C.

4. 2. The method for producing a phenolic resin having mesopores according to claim 1, wherein the heating temperature in the second step is 63° C. or higher and lower than 67° C.

5. 5. A method for producing a carbonized material having mesopores, comprising the steps of: heat-treating a phenolic resin having mesopores produced by the method for producing a phenolic resin having mesopores according to any one of claims 1 to 4 in an inert gas atmosphere at 300°C or more and 450°C or less; calcining the resulting heat-treated product in an inert gas atmosphere at 450°C or more and 800°C or less; and carbonizing the resulting calcined product in an inert gas atmosphere at 800°C or more and 2000°C or less to obtain a carbonized product.

Citation Information

Patent Citations

  • Catalyst layer for fuel cell, carbon material for catalyst carrier, and method for manufacturing carbon material for catalyst carrier

    JP2018010806A

  • Supported metal catalyst, method for producing same, and method for producing carrier

    WO2021161929A1