Method for producing phenol resin having three-dimensional network structure formed with mesopore, and method for producing carbonized material having three-dimensional network structure formed with mesopore

JP2024149154APending Publication Date: 2024-10-18TOKAI CARBON CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023062860
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18

AI Technical Summary

Benefits of technology

【0017】 本発明によれば、均質なメソ孔が形成されている三次元網目構造を有するフェノール樹脂及び炭素化物の製造方法であり、収率を高くすることができる、メソ孔が形成されている三次元網目構造を有するフェノール樹脂の製造方法及びメソ孔が形成されている三次元網目構造を有する炭素化物の製造方法を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149154000001_ABST
    Figure 2024149154000001_ABST
Patent Text Reader

Abstract

To provide methods for producing a phenol resin and a carbonized material which have three-dimensional network structures that have homogeneous mesopores and can enhance a yield.SOLUTION: A method for producing a phenol resin having a three-dimensional network structure formed with mesopores includes: a first step of heating a mixture of a phenol compound, formaldehyde, alkali metal hydroxide, ammonia, organic amine or a quaternary organic ammonium salt, a non-ionic surface active agent, and water to obtain a first treated substance; a second step of heating a mixture of the first treated substance and water to obtaining a sol solution; a step of mixing water with the sol solution, and heating the mixture at 120°C to 140°C to obtain a wet gal; and a step of drying the wet gel to obtain a phenol resin having a three-dimensional network structure having mesopores, in which a mass ratio of a surface active agent to the phenol compound is 1.4 to 1.7, and a heating temperature at the first step and a heating temperature at the second step satisfy a specific formula.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a phenolic resin having a three-dimensional network structure and formed with mesopores, and a method for producing a carbonized material having a three-dimensional network structure and formed with mesopores. [Background technology]

[0002] As part of recent research and development aimed at realizing a carbon-neutral society, there is currently development in the automotive field to replace automobiles equipped with engines that use fossil fuels with electric vehicles that use secondary batteries such as lithium-ion secondary batteries as their energy device, and fuel cell vehicles that use fuel cells as their energy device.

[0003] Due to the improvement of the charging capacity and the fall of the price of lithium-ion secondary batteries, passenger cars have rapidly become popular in recent years, and as a result, electric vehicles are being replaced. On the other hand, trucks and buses have a longer driving distance per charge than passenger cars, so a single charge of secondary batteries such as lithium-ion secondary batteries is not enough to cover the required driving distance, and it is not realistic to increase the number of batteries installed due to the weight and cost of the batteries. For this reason, fuel cell vehicles are considered to be the likely replacements for trucks and buses.

[0004] The fuel cell used in fuel cell-equipped vehicles is a polymer electrolyte fuel cell (PEFC) consisting of an anode catalyst layer, a polymer electrolyte membrane, and a cathode catalyst layer. The cathode, which is the air electrode of the fuel cell, uses a platinum catalyst in which platinum or a platinum alloy is supported on a carbon support.

[0005] Platinum is expensive and there is a need to reduce its use because of the scarcity of platinum reserves worldwide. Therefore, in order to reduce the amount of platinum used as a cathode catalyst in fuel cells, attempts have been made to reduce the amount of platinum used by making it into small particles and supporting it on a carbon support.

[0006] However, when small platinum particles are repeatedly used as a catalyst for a cell reaction, they tend to aggregate and sinter to become larger particles. When the particles become larger, their performance as a catalyst for a cell reaction decreases, so simply supporting small platinum particles results in a high rate of deterioration in the performance of the fuel cell.

[0007] Therefore, platinum nanoparticles have been supported in the mesopores of a carbon support in which mesopores are formed, thereby preventing the platinum nanoparticles from agglomerating and sintering due to repeated use in battery reactions. Patent Document 1 discloses a platinum-supported metal catalyst in which a platinum catalyst is supported on mesoporous carbon nanodendrites (MCND).

[0008] However, in the platinum-supported metal catalyst described in Patent Document 1, uniform mesopores are not formed in the support, and platinum particles supported in the deep mesopores are unable to contribute to the catalytic reaction, resulting in low utilization efficiency of the platinum catalyst.

[0009] For this reason, Patent Document 2 discloses a supported metal catalyst for improving the utilization efficiency of a platinum catalyst supported on a carbon support, the supported metal catalyst comprising a support which is an aggregate of conductive particles, and active metal particles dispersed and supported on the conductive particles, the conductive particles including a plurality of pores, the pores having an average inlet pore diameter of 1 to 20 nm, a standard deviation of the average inlet pore diameter being 50% or less of the average inlet pore diameter, the number fraction of the active metal particles supported on the surface region of the conductive particles being 50% or more, and the surface region being a region on the surface of the conductive particle, or a region within the pores within a depth of 15 nm from the surface. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2018-10806 A [Patent Document 2] International Publication No. 2021 / 161929 Summary of the Invention [Problem to be solved by the invention]

[0011] In the supported metal catalyst of Patent Document 2, the framework of the carbon support on which the metal particles are supported has a three-dimensional network structure in which spherical carbon nanoparticles are connected in a three-dimensional direction, and the framework has mesopores formed therein that can support platinum nanoparticles within the pores.

[0012] The mesopores formed in the carbon support of the supported metal catalyst in Patent Document 2 are homogeneous pores. In addition, a supported metal catalyst in which platinum nanoparticles are supported in the mesopores of a carbon support in which homogeneous mesopores are formed is expected to have a high utilization efficiency of the platinum catalyst.

[0013] Furthermore, the carbon support of the supported metal catalyst in Patent Document 2 has a three-dimensional network structure formed by spherical carbon nanoparticles forming the framework, which are connected in a three-dimensional direction, and has gaps large enough to allow water vapor generated by the cell reaction at the cathode to easily escape from the electrode. This leads to a reduction in material transport resistance, and is expected to lead to higher output of fuel cells that can handle high current densities.

[0014] Therefore, from the viewpoint of reducing the manufacturing cost, it is desired to increase the yield of the carbon support in which uniform mesopores are formed. However, since the carbon support of Patent Document 2 is a nanoparticle that is generated in a dilute aqueous solution, the amount of the carbon support generated per volume of the synthesis reaction vessel is small, which causes a problem of high manufacturing costs. In order to reduce the manufacturing cost, it is necessary to increase the amount of the carbon support generated per reaction vessel, and it is necessary to find the optimal reaction conditions that increase the gel conversion rate of the raw material phenol.

[0015] Therefore, the present invention is a method for producing a phenolic resin having a three-dimensional network structure in which homogeneous mesopores are formed, and a carbonized product thereof, which is capable of increasing yields, and an object of the present invention is to provide a method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, and a carbonized product having a three-dimensional network structure in which mesopores are formed. [Means for solving the problem]

[0016] The above problems are solved by the present invention described below. That is, the present invention provides (1) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; The heating temperature in the first step and the heating temperature in the second step are expressed by the following formulas (1), (2), and (3): 136≦X+Y≦144 (1) 76≦X≦89 (2) 51≦Y≦64 (3) (In the formula, X represents the heating temperature (°C) in the first step, and Y represents the heating temperature (°C) in the second step.) Both of the above must be satisfied. A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, characterized by: (2) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (i) the heating temperature in the first step is 78°C or more and less than 81°C, and the heating temperature in the second step is 58°C or more and 62°C or less; A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, characterized by: (3) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (ii) the heating temperature in the first step is 81°C or more and less than 83°C, and the heating temperature in the second step is 56°C or more and 58°C or less; A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, characterized by: (4) a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (iii) the heating temperature in the first step is 83°C or higher and 88°C or lower, and the heating temperature in the second step is 52°C or higher and 56°C or lower; A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, characterized by: (5) The method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to (1), wherein an amount of water to be mixed in the first step is an amount that causes a concentration of the nonionic surfactant to be 21 mg / mL or more and 45 mg / mL or less relative to the total amount of the first processed product. (6) A method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed, comprising a carbonization step of heat-treating a phenolic resin having a three-dimensional network structure in which mesopores are formed, produced by the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to any one of (1) to (5), in an inert gas atmosphere at 300°C or more and 450°C or less, calcining the resulting heat-treated product in an inert gas atmosphere at 450°C or more and 800°C or less, and carbonizing the resulting calcined product in an inert gas atmosphere at 800°C or more and 2000°C or less, thereby obtaining a carbonized material having a three-dimensional network structure in which mesopores are formed. This provides: Effect of the Invention

[0017] According to the present invention, there can be provided a method for producing a phenolic resin having a three-dimensional network structure in which homogeneous mesopores are formed, and a carbonized product thereof, which can increase yields. [Brief description of the drawings]

[0018] [Figure 1] 1 is a STEM image of the phenol resin obtained in Example 1. [Diagram 2] 1 is a STEM image of the phenol resin obtained in Example 2. [Diagram 3] 1 is a STEM image of the phenol resin obtained in Example 3. [Figure 4] 1 is a STEM image of the phenol resin obtained in Comparative Example 1. [Diagram 5] 1 is a STEM image of the phenol resin obtained in Comparative Example 2. [Figure 6] 1 is a STEM image of the phenol resin obtained in Comparative Example 3. [Figure 7] 1 is a STEM image of the phenol resin obtained in Comparative Example 4. [Figure 8] 1 is a STEM image of the phenol resin obtained in Comparative Example 5. [Figure 9] 1 is a STEM image of the phenol resin obtained in Comparative Example 6. [Figure 10] 1 is a STEM image of the phenol resin obtained in Comparative Example 7. [Figure 11] 1 is a STEM image of the phenol resin obtained in Comparative Example 8. [Figure 12] 1 is a STEM image of the phenolic resin obtained in Comparative Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings as appropriate. The detailed description of the present invention below is an example of an embodiment, and the present invention is not to be construed as being limited to this embodiment.

[0020] The method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the first embodiment of the present invention comprises the steps of: a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; The heating temperature in the first step and the heating temperature in the second step are expressed by the following formulas (1), (2), and (3): 136≦X+Y≦144 (1) 76≦X≦89 (2) 51≦Y≦64 (3) (In the formula, X indicates the heating temperature (°C) in the first step, and Y indicates the heating temperature (°C) in the second step.) The present invention is characterized by satisfying all of the above.

[0021] The second aspect of the present invention provides a method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, comprising the steps of: a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (i) The heating temperature in the first step is 78°C or more and less than 81°C, and the heating temperature in the second step is 58°C or more and 62°C or less.

[0022] A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to a third aspect of the present invention comprises the steps of: a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (ii) The heating temperature in the first step is 81° C. or more and less than 83° C., and the heating temperature in the second step is 56° C. or more and 58° C. or less.

[0023] A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to a fourth embodiment of the present invention comprises the steps of: a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (iii) The heating temperature in the first step is 83° C. or higher and 88° C. or lower, and the heating temperature in the second step is 52° C. or higher and 56° C. or lower.

[0024] The first embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the second embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the third embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, and the fourth embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed are similar to each other except that the heating temperatures in the first step and the second step are different. Therefore, the points common to the first embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the second embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the third embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, and the fourth embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed will be collectively referred to as the "method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention" and described below.

[0025] The first step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention is a step of heating a mixture of a phenolic compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product.

[0026] The phenolic compound used in the first step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is not particularly limited as long as it is a compound having a phenolic skeleton, and examples thereof include phenol (C6H5OH), substituted phenols in which an aromatic ring is substituted with one or more alkyl groups, specifically C6H4(OH)CH3 (any one or a combination of two or more of 2-methylphenol, 3-methylphenol, and 4-methylphenol), C6H3(OH)(CH3)2 (any one or a combination of two or more of 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 2,6-dimethylphenol, 3,4-dimethylphenol, and 3,5-dimethylphenol), resorcinol (C6H4(OH)2), pyrocatechol (C6H4(OH)2), etc. Among these, phenolic compounds are preferably phenol (C6H5OH).

[0027] The formaldehyde used in the first step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is usually added as an aqueous formaldehyde solution to water for preparing a mixed liquid. The concentration of the aqueous formaldehyde solution is not particularly limited, and is usually 10.0% by mass or more and 40.0% by mass or less.

[0028] The alkali metal hydroxide used in the first step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is not particularly limited. From the viewpoint of preferentially progressing the addition reaction of phenol, however, sodium hydroxide, potassium hydroxide and lithium hydroxide are preferred, and sodium hydroxide is particularly preferred.

[0029] In the first step of the present invention for the phenolic resin having a three-dimensional network structure in which mesopores are formed, ammonia, an organic amine such as ethanolamine, or a quaternary organic ammonium salt such as tetramethylammonium hydroxide can be used instead of an alkali metal hydroxide. By using an alkali metal hydroxide, ammonia, an organic amine, or a quaternary ammonium salt in the first step of the present invention, a reaction for producing a resol resin can be carried out under basic conditions.

[0030] Examples of the organic amine used in the first step include ethanolamine, propanolamine, alkylamine, and cyclic amine. Examples of the ethanolamine include monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, N-ethylethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, and aminoethoxyethanol. Examples of the propanolamine include 1-amino-2-propanol, 2-amino-2-methyl-1-propanol, and 2-amino-2-methyl-1,3-propanediol. Examples of the alkylamine include monomethylamine, dimethylamine, trimethylamine, ethyleneamine, ethylenediamine, diethylenetriamine, triethylenetetramine, hexamethylenetetramine, and tetraethylenepentamine. Examples of the cyclic amine include choline and morpholine.

[0031] Examples of the quaternary organic ammonium salt used in the first step include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, N,N,N-triethyl-N-(2-hydroxyethyl)ammonium hydroxide, and N,N-diethyl-N,N-di(2-hydroxyethyl)ammonium hydroxide.

[0032] The organic amine or quaternary organic ammonium salt used in the first step is preferably one having strong basicity, more preferably a quaternary organic ammonium salt, and particularly preferably tetramethylammonium hydroxide, tetraethylammonium hydroxide, or the like.

[0033] Examples of the nonionic surfactant used in the first step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention include polyoxyethylene alkyl ethers and polyoxyethylene alkyl phenyl ethers, and more specifically, copolymers of polyethylene oxide (PEO) and polypropylene oxide (PPO), in particular copolymers in which the molar mass of PPO is from 3,000 to 4,000 and the proportion of PEO in the molecule is from 30% to 90%.

[0034] The water used in the first step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the first step in the production of a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention preferably contains fewer impurities in order to prevent impurities from interfering with the addition polymerization reaction.

[0035] In the first step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention, a mixture obtained by mixing a phenolic compound, formaldehyde, an alkali metal hydroxide, ammonia, an organic amine, or a quaternary organic ammonium salt, a nonionic surfactant, and water is heated.

[0036] In the mixture used in the first step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention, the molar ratio of formaldehyde to the phenolic compound (formaldehyde / phenolic compound) is 2.6 or more and 5.0 or less, and from the viewpoint of promoting addition polymerization, is preferably 3.2 or more and 4.4 or less, the molar ratio of alkali metal hydroxide to the phenolic compound (alkali metal hydroxide / phenolic compound) is 0.24 or more and 0.48 or less, the molar ratio of ammonia to the phenolic compound (ammonia / phenolic compound) is 0.24 or more and 0.96 or less, the molar ratio of organic amine to the phenolic compound (organic amine / phenolic compound) is 0.24 or more and 0.96 or less, and the molar ratio of quaternary organic ammonium salt to the phenolic compound (quaternary organic ammonium salt / phenolic compound) is 0.24 or more and 0.48 or less.

[0037] The method for preparing the mixture used in the first step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is not particularly limited, and examples thereof include a method in which predetermined amounts of a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, and a nonionic surfactant are added to a predetermined amount of water and mixed. The formaldehyde, the alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, and the nonionic surfactant may be added in the form of an aqueous solution.

[0038] In the first step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the amount of the nonionic surfactant mixed when mixing a phenolic compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water is an amount in which the mass ratio of the nonionic surfactant to the phenolic compound in the first treated product (nonionic surfactant / phenolic compound) is 1.4 or more and less than 1.7, preferably 1.5 or more and less than 1.7, and more preferably 1.6 or more and less than 1.7. By setting the mass ratio of the nonionic surfactant to the phenolic compound within the above range, the conversion rate of the phenolic compound to a phenolic resin in which mesopores are formed (phenol conversion rate) can be increased.

[0039] The amount of water to be mixed in the first step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is preferably an amount that results in a concentration of the nonionic surfactant of 21 mg / mL or more and 45 mg / mL or less relative to the total amount of the first processed product, and is preferably 25 mg / mL or more and 45 mg / mL or less in terms of increasing the phenol conversion rate from the phenol compound to the phenolic resin in which mesopores are formed.

[0040] The second step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is a step of mixing water with the first treated product obtained by carrying out the first step, and heating the resulting mixture to obtain a sol liquid.

[0041] The water used in the second step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the second step in the production of a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention preferably contains fewer impurities in order to suppress inhibition of the addition polymerization reaction by impurities.

[0042] In the second step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention, the amount of water to be mixed with the first treated product is preferably an amount such that the concentration of the nonionic surfactant in the mixture obtained after mixing the first treated product with water is 9 mg / mL or more and 20 mg / mL or less, more preferably 10 mg / mL or more and 16 mg / mL or less.

[0043] In the second step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention, the method for mixing water with the first treated product is not particularly limited, and examples thereof include a method in which a predetermined amount of water is added to a predetermined amount of the first treated product and mixed.

[0044] In the first embodiment of the present invention, the heating temperatures in the first step and the second step are determined based on the following formulas (1), (2), and (3): 136≦X+Y≦144 (1) 76≦X≦89 (2) 51≦Y≦64 (3) (In the formula, X represents the heating temperature (°C) in the first step, and Y represents the heating temperature (°C) in the second step.) Meet the following. The lower limit of formula (1) is preferably 137 or more (137≦X+Y), more preferably 138 or more (138≦X+Y), and the upper limit of formula (1) is preferably 143 or less (X+Y≦143), more preferably 142 or less (X+Y≦142). The lower limit of formula (2) is preferably 77 or more (77≦X), more preferably 78 or more (78≦X), and the upper limit of formula (2) is preferably 88 or less (X≦88), more preferably 87 or less (X≦87). The lower limit of formula (3) is preferably 52 or more (52≦Y), more preferably 53 or more (53≦Y), and the upper limit of formula (3) is preferably 63 or less (Y≦63), more preferably 62 or less (Y≦62). When the heating temperature in the first step and the heating temperature in the second step satisfy all of the above formulae (1), (2), and (3), the yield of the carbonized material having a three-dimensional network structure in which mesopores are formed and the yield of the phenolic resin having a three-dimensional network structure in which mesopores are formed, which is the precursor of the carbonized material, are increased. On the other hand, when the heating temperature in the first step and the heating temperature in the second step do not satisfy one or more of the above formulae (1), (2), and (3), single-cell nanoparticles or aggregates (aggregates) thereof without a three-dimensional network structure, or fibrous structures or irregular mesopore structures are formed, or nanoparticles having a three-dimensional network structure with a low gel yield are formed. In the first embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time in the first step is preferably 1 hour or more and 6 hours or less, more preferably 2 hours or more and 4 hours or less. In the first embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time in the second step is preferably 12 hours or more and 24 hours or less, more preferably 15 hours or more and 20 hours or less.

[0045] In the second embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, (i) the heating temperature in the first step is 78°C or more and less than 81°C, and the heating temperature in the second step is 58°C or more and 62°C or less. By setting the heating temperatures in the first step and the second step within the above ranges, the yield of the carbonized material having a three-dimensional network structure in which mesopores are formed and the phenolic resin having a three-dimensional network structure in which mesopores are formed, which is the precursor of the carbonized material, is increased. In the second embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time in the first step is preferably 1 hour or more and 6 hours or less, more preferably 2 hours or more and 4 hours or less. In the second embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time in the second step is preferably 12 hours or more and 24 hours or less, more preferably 15 hours or more and 20 hours or less.

[0046] In the third embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, (ii) the heating temperature in the first step is 81° C. or more and less than 83° C., and the heating temperature in the second step is 56° C. or more and 58° C. or less. By setting the heating temperatures in the first step and the second step within the above ranges, the yield of the carbonized material having a three-dimensional network structure in which mesopores are formed and the phenolic resin having a three-dimensional network structure in which mesopores are formed, which is the precursor of the carbonized material, is increased. In the third embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time in the first step is preferably 1 hour or more and 6 hours or less, more preferably 2 hours or more and 4 hours or less. In the third embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time in the second step is preferably 12 hours or more and 24 hours or less, more preferably 15 hours or more and 20 hours or less.

[0047] In the fourth embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, (iii) the heating temperature in the first step is 83° C. or more and 88° C. or less, and the heating temperature in the second step is 52° C. or more and 56° C. or less. By setting the heating temperatures in the first step and the second step within the above ranges, the yield of the carbonized material having a three-dimensional network structure in which mesopores are formed and the phenolic resin having a three-dimensional network structure in which mesopores are formed, which is the precursor of the carbonized material, is increased. In the fourth embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time in the first step is preferably 1 hour or more and 6 hours or less, more preferably 2 hours or more and 4 hours or less. In the fourth embodiment of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time in the second step is preferably 12 hours or more and 24 hours or less, more preferably 15 hours or more and 20 hours or less.

[0048] In the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention, the sol liquid obtained by carrying out the second step according to the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention may be used as the sol liquid to be used in the gelling step as it is. Alternatively, after carrying out the second step according to the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention, the sol liquid obtained by carrying out the second step and before carrying out the gelling step may be filtered, and the obtained filtrate may be used as the sol liquid to be used in the gelling step.

[0049] The gelation step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention is a step of mixing water with the sol liquid obtained by carrying out the second step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention, and heating the resulting mixture to obtain a wet gel.

[0050] The water used in the gelation step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is not particularly limited, and examples thereof include distilled water, ion-exchanged water, industrial water, etc. The water used in the gelation step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention preferably contains fewer impurities in order to prevent impurities from interfering with the addition polymerization reaction.

[0051] In the gelation step of the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention, the amount of water mixed into the sol liquid is preferably 1.5 to 6.0 times, and more preferably 2.5 to 6.0 times, the mass of the first processed product.

[0052] In the gelation step according to the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the method for mixing water with the sol liquid is not particularly limited, and examples thereof include a method in which a predetermined amount of water is added to a predetermined amount of sol liquid and mixed.

[0053] In the gelation step according to the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, a mixture obtained by mixing water with a sol liquid is heated at 120°C to 140°C to obtain a wet gel. By heating the mixture in the gelation step within the above range, a carbonized material having a three-dimensional network structure in which mesopores are formed and a phenolic resin having a three-dimensional network structure in which mesopores are formed, which is a precursor of the carbonized material, can be obtained. In the gelation step according to the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the pressure (absolute pressure) when heating the mixture obtained by mixing water with a sol liquid is 0.34 MPa to 0.51 MPa, preferably 0.38 MPa to 0.46 MPa. In the gelation step according to the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the heating time when heating the mixture obtained by mixing water with a sol liquid is 6 hours to 48 hours, preferably 20 hours to 48 hours.

[0054] The wet gel obtained by carrying out the gelling step according to the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention may be dried as it is in the drying step. Alternatively, after carrying out the gelling step according to the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention, the wet gel obtained by carrying out the gelling step may be washed one or more times before carrying out the drying step, and the obtained wet gel may be dried in the drying step.

[0055] The drying step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention is a step of drying the wet gel obtained by the gelling step to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed.

[0056] In the drying step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to the present invention, the method for drying the wet gel is not particularly limited, and examples thereof include: (i) a method in which the wet gel is added to water, dispersed in water, the obtained wet gel dispersion is freeze-granulated by spraying it into liquid nitrogen using a spray-freeze granulator, and then the obtained frozen granules are vacuum-dried to dry the wet gel; (ii) a method in which the wet gel is added to water, dispersed in water, and the obtained wet gel dispersion is sprayed into hot air using a spray dryer to heat-dry; and (iii) a method in which the wet gel is heat-dried by treatment with microwaves.

[0057] The phenolic resin obtained by carrying out the drying step in the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention is the phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention.

[0058] The phenolic resin obtained by the method of the present invention for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed has homogeneous mesopores formed therein, and has a three-dimensional network structure in which a large number of spherical phenolic resin particles in which homogeneous mesopores are formed are connected to one another.

[0059] In the method of the present invention for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, the yield of the phenolic resin having a three-dimensional network structure in which mesopores are formed can be increased by setting the mass ratio of the nonionic surfactant to the phenolic compound used in the first step within a predetermined range and controlling the heating temperatures in the first step and the second step within predetermined ranges.

[0060] The method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed of the present invention is characterized by comprising a carbonization step of heat-treating a phenolic resin having a three-dimensional network structure in which mesopores are formed, obtained by carrying out the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention, in an inert gas atmosphere at 300°C or more and 450°C or less, then calcining the resulting heat-treated product in an inert gas atmosphere at 450°C or more and 800°C or less, and then carbonizing the resulting calcined product in an inert gas atmosphere at 800°C or more and 2000°C or less, to obtain a carbonized material having a three-dimensional network structure in which mesopores are formed.

[0061] In the carbonization step according to the method for producing a carbonized product having a three-dimensional network structure in which mesopores are formed of the present invention, the heat treatment temperature when the phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention is heat treated is 300°C or more and 450°C or less. In the carbonization step according to the present invention, by heat treating the phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention in the above temperature range, it is possible to remove the surfactant remaining in the phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention and maintain the mesopore structure. In the carbonization step according to the method for producing a carbonized product having a three-dimensional network structure in which mesopores are formed of the present invention, the heat treatment time when the phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention is 30 minutes or more and 6 hours or less, preferably 1 hour or more and 3 hours or less. In the carbonization step according to the method for producing a carbonized product having a three-dimensional network structure in which mesopores are formed of the present invention, the heat treatment atmosphere when the phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.

[0062] In the carbonization step according to the method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed of the present invention, the firing temperature when firing the heat-treated phenolic resin having a three-dimensional network structure in which mesopores are formed is 450°C or more and 800°C or less, and preferably 500°C or more and 800°C or less from the viewpoint of suitably removing the organic content-containing gas generated with the carbonization of the phenolic resin. In the carbonization step according to the method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed of the present invention, the firing time when firing the heat-treated phenolic resin having a three-dimensional network structure in which mesopores are formed of is 30 minutes or more and 6 hours or less, preferably 1 hour or more and 3 hours or less. In the carbonization step according to the method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed of the present invention, the firing atmosphere when firing the heat-treated phenolic resin having a three-dimensional network structure in which mesopores are formed of is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.

[0063] In the carbonization step according to the method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed of the present invention, the carbonization temperature when carbonizing the burned product of the phenolic resin having a three-dimensional network structure in which mesopores are formed is 800°C or more and 2000°C or less, and from the viewpoint of balancing the crystallinity of the carbonized material and the economic efficiency of the production process, it is preferably 900°C or more and 1600°C or less, more preferably 1000°C or more and 1300°C or less. In the carbonization step according to the method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed of the present invention, the carbonization time when carbonizing the burned product of the phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention is 30 minutes or more and 6 hours or less, preferably 1 hour or more and 3 hours or less. In the carbonization step according to the method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed of the present invention, the burning atmosphere when carbonizing the burned product of the phenolic resin having a three-dimensional network structure in which mesopores are formed of is an inert gas atmosphere such as nitrogen gas, helium gas, or argon gas.

[0064] In the carbonized material obtained by the method of the present invention for producing a carbonized material having a three-dimensional network structure in which mesopores are formed, homogeneous mesopores are formed, and the carbonized material has a three-dimensional network structure in which a large number of spherical carbon nanoparticles in which homogeneous mesopores are formed are connected, similar to the carbon support on which the metal catalyst is supported in the supported metal catalyst of Patent Document 2.

[0065] In the present invention, the term "homogeneous mesopores" means that, when the surface pore structure of a phenolic resin in which mesopores are formed is observed at a magnification of 500,000 times in a scanning transmission electron microscope image, mesopores with a circular diameter of 2 nm to 9 nm are evenly spaced at 0.0040 pores / nm on the skeleton surface. 2 More than 0.0088 pieces / nm 2 This means that the pores are arranged at a surface density of 0.0052 pores / nm2 or less, and that the arrangement of the pores is formed in a 2D hexagonal structure or an arrangement equivalent thereto. In the present invention, homogeneous mesopores can also be referred to as ordered mesopores, and the phenolic resin of the present invention in which mesopores are formed is preferably a phenolic resin in which ordered mesopores are formed. In the phenolic resin in which mesopores are formed described in the examples of the present invention, the mesopore density is 0.0052 pores / nm2 or less. 2 More than 0.0053 pieces / nm 2 The following is the result.

[0066] In the carbonized product (carbonized product of the present invention) obtained by the method for producing a carbonized product having a three-dimensional network structure in which mesopores are formed according to the present invention, homogeneous mesopores are formed in the skeleton. The structure of the carbonized product of the present invention has a three-dimensional network structure formed by spherical carbon nanoparticles forming the skeleton being connected in a three-dimensional direction. Therefore, in the skeleton of the carbonized product of the present invention, the largest diameter part of the connected spherical carbon nanoparticles becomes the part of the skeleton with a large diameter, and the connection part of adjacent carbon nanoparticles becomes the part of the skeleton with a small diameter, and convex parts and constrictions derived from the spherical carbon nanoparticles are observed on the wall surface of the skeleton. The carbonized product of the present invention has gaps large enough to allow water vapor generated by the battery reaction at the cathode to easily escape from the electrode.

[0067] The phenolic resin obtained by the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention is a precursor of the carbonized product obtained by the method for producing a carbonized product having a three-dimensional network structure in which mesopores are formed of the present invention before carbonization. Although the carbonized product obtained by the method for producing a carbonized product having a three-dimensional network structure in which mesopores are formed of the present invention shrinks overall upon carbonization compared to the phenolic resin obtained by the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention, the structure of the carbonized product obtained by the method for producing a carbonized product having a three-dimensional network structure in which mesopores are formed of the present invention is similar to the structure of the phenolic resin obtained by the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed of the present invention.

[0068] The method of the present invention for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed has a high conversion rate (phenol conversion rate) at which the raw material phenol compound is converted into a phenolic resin having mesopores formed. In other words, the method of the present invention for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed and the method of the present invention for producing a carbonized material having a three-dimensional network structure in which mesopores are formed can increase the yield of the phenolic resin and carbonized material having a three-dimensional network structure in which mesopores are formed.

[0069] The carbonized material obtained by the method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed according to the present invention is suitable for use as a carbon support for a platinum catalyst used as a cathode catalyst in a polymer electrolyte fuel cell. That is, by supporting platinum nanoparticles on the carbonized material having a three-dimensional network structure in which mesopores are formed according to the present invention, more specifically, by supporting platinum nanoparticles in the mesopores of the carbonized material having a three-dimensional network structure in which mesopores are formed according to the present invention, a cathode catalyst for a polymer electrolyte fuel cell can be produced. EXAMPLES

[0070] The present invention will be described using the following examples. However, the following examples are merely examples of the present invention and are not intended to be limiting.

[0071] Example 1 (1) First step In 60 g of pure water, 3.84 g of a nonionic surfactant (polyethylene oxide (PEO) and polypropylene oxide (PPO) copolymer (trade name Pluronic (registered trademark) F127, structural formula: PEO m -PPO n -PEO m An aqueous solution of 2.42 g of phenol, 8.40 g of formaldehyde solution (formaldehyde concentration: 35% by mass), and 60.65 g of 0.1 mol / L aqueous sodium hydroxide solution was placed in a flask and stirred at 200 rpm with a stirrer at an internal temperature (heating temperature) of 85°C for 120 minutes to obtain a first processed product.

[0072] (2)Second process Next, 200 g of pure water was added to the treated material obtained in (1) in a flask, the internal temperature (heating temperature) was adjusted to 55° C., and the mixture was stirred for 20 hours to obtain a sol liquid.

[0073] (3) Gelling process The sol prepared in (2) was filtered through a 5 μm membrane filter, and the filtrate was collected. 700 g of pure water was added to 280 g of this filtrate (the total amount of the sol considering the evaporation was 300 mL), and the mixture was placed in a stainless steel sealed container and subjected to hydrothermal treatment at 130°C for 20 hours to obtain a wet gel. The gel was collected by filtration through a 5 μm membrane filter, and then redispersed in 200 g of pure water and filtered through a membrane filter again. This process was repeated three times to obtain a wet gel from which unreacted substances had been removed.

[0074] <Structure confirmation> A small portion of the wet gel was dispersed in ethanol, dropped onto a grid for transmission electron microscope observation, and dried to prepare a sample. The sample was then observed with a scanning transmission electron microscope (STEM: HD-2700 (Hitachi High-Technologies Corporation), accelerating voltage 200 kV) to observe the surface pore structure. Low-magnification and high-magnification images of the obtained STEM images are shown in Figure 1. The particle diameter of the spherical particles was determined as the average value of the diameter of circles circumscribed on 50 arbitrarily selected spherical particle images. In addition, a circle with a diameter of 30 nm to 40 nm was drawn at any point in the skeleton of the obtained STEM image, and the number of mesopores with a diameter of 2 nm to 9 nm present in the circle was counted and divided by the area of ​​the circle to determine the mesopore density at each point. This mesopore density measurement was performed at 50 random points in the skeleton, and the average value was taken as the mesopore density. When the mesopore density was 0.0040 pores / nm 2 More than 0.0088 pieces / nm 2 It was determined that homogeneous mesopores had formed when the mesopores were equal to or smaller than the above. However, since pores may not be visible in STEM images depending on the observation conditions, unclear areas were excluded.

[0075] (4) Drying process The entire amount of the wet gel obtained in (3) was placed in 160 g of pure water, stirred with a high-speed stirrer at 2,000 rpm for 5 minutes, and further treated in an ultrasonic cleaner with an output of 70 W for 5 to 10 minutes to prepare a dispersion. This dispersion was freeze-granulated by spraying it into liquid nitrogen with a spray-freeze granulator, then placed in a dedicated glass container cooled with liquid nitrogen, attached to a vacuum dryer, and subjected to vacuum drying treatment at approximately -40°C for 60 hours to obtain a granulated dry gel (phenolic resin having a three-dimensional network structure in which mesopores are formed).

[0076] <Calculation of gel yield> Gel yield (mg / mL) = final yield of dried gel (mg) / hydrothermally treated sol (mL)

[0077] <Calculation of phenol conversion rate> If the weight loss at around 330-360°C in thermogravimetric analysis (TG) in nitrogen gas is considered to be the decomposition of the surfactant, the amount of surfactant in the dried gel is estimated to be 47%. Therefore, the amount of phenolic resin in the obtained dried gel is 53%. Furthermore, based on the stoichiometric ratio of phenol to formaldehyde, the amount of phenol in the phenolic resin is 87.7%. Therefore, if the amount of the recovered dried gel is A (mg / mL), the amount of phenol in the gel, B (mg / mL), is: B = A x 0.53 x 0.877 (mg / mL) Since the total amount of the sol obtained in the second step of (2) is 300 mL, if the amount of phenol added in the first step of (1) is C, the phenol conversion rate can be calculated by the following formula. Phenol conversion rate (%) = (B x 300 / C) x 100

[0078] (5) Carbonization process The dried gel obtained in (4) was placed in a calcination furnace, heated to 350°C at a heating rate of 1°C / min under nitrogen gas flow, maintained for 2 hours, then heated again to 600°C at a heating rate of 1°C / min, maintained for 2 hours, and cooled to room temperature. Next, it was placed in a carbonization furnace, heated to 1000°C at a heating rate of 1°C / min under a pressurized nitrogen gas atmosphere, maintained for 2 hours, and cooled to room temperature to obtain a carbonized material.

[0079] (Examples 2 to 3, Comparative Examples 1 to 9) The same procedure as in Example 1 was carried out except that the blend amounts and temperature conditions were as shown in Tables 1 and 2. The surface pore structure of each wet gel was observed, and low-magnification and high-magnification STEM images obtained are shown in Figs.

[0080] As a result of observation with a scanning transmission electron microscope, it was confirmed that the phenol resins had homogeneous mesopores and a three-dimensional network structure in Examples 1 to 3 and Comparative Examples 1, 3, 5, and 9. On the other hand, it was confirmed that the phenol resins had homogeneous mesopores but no three-dimensional network structure in Comparative Examples 6 to 7. In Comparative Examples 2, 4, and 8, the formation of homogeneous mesopores was insufficient or no mesopores were formed.

[0081] In Comparative Examples 1, 3, 5, and 9, phenol resins having a three-dimensional network structure in which uniform mesopores were formed were confirmed, but the yields (gel yields and phenol conversion rates) were lower than those in Examples 1 to 3.

[0082] [Table 1]

[0083] [Table 2]

[0084] In the table, the surfactant / phenol mass ratio refers to the mass ratio of the nonionic surfactant to the phenol compound in the first processed product (nonionic surfactant / phenol compound). The first process temperature refers to the internal temperature (heating temperature) of the first process, the second process temperature refers to the internal temperature (heating temperature) of the second process, and the gelation process temperature refers to the hydrothermal treatment temperature of the gelation process.

[0085] In addition, when the carbonized materials obtained by carrying out the carbonization step in the Examples and Comparative Examples were observed with a scanning transmission electron microscope, it was confirmed that the carbonized materials had homogeneous mesopores and a three-dimensional network structure in Examples 1 to 3 and Comparative Examples 1, 3, 5, and 9. On the other hand, it was confirmed that the carbonized materials had homogeneous mesopores but no three-dimensional network structure in Comparative Examples 6 to 7. In Comparative Examples 2, 4, and 8, the formation of homogeneous mesopores was insufficient or no mesopores were formed.

Claims

1. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; The heating temperature in the first step and the heating temperature in the second step satisfy the following formulas (1), (2), and (3): 136≦X+Y≦144 (1) 76≦X≦89 (2) 51≦Y≦64 (3) (In the formula, X represents the heating temperature (°C) in the first step, and Y represents the heating temperature (°C) in the second step.) Both of the above must be satisfied. A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, characterized by:

2. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (i) the heating temperature in the first step is 78° C. or more and less than 81° C., and the heating temperature in the second step is 58° C. or more and 62° C. or less; A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, characterized by:

3. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (ii) the heating temperature in the first step is 81° C. or more and less than 83° C., and the heating temperature in the second step is 56° C. or more and 58° C. or less; A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, characterized by:

4. a first step of heating a mixture of a phenol compound, formaldehyde, an alkali metal hydroxide or ammonia or an organic amine or a quaternary organic ammonium salt, a nonionic surfactant, and water to obtain a first treated product; a second step of mixing the first treated product with water and heating the resulting mixture to obtain a sol; a gelation step of mixing the sol with water and heating the resulting mixture at 120° C. or higher and 140° C. or lower to obtain a wet gel; a drying step of drying the wet gel to obtain a phenolic resin having a three-dimensional network structure in which mesopores are formed; having a mass ratio of the nonionic surfactant to the phenol compound is 1.4 or more and less than 1.7; (iii) the heating temperature in the first step is 83° C. or more and 88° C. or less, and the heating temperature in the second step is 52° C. or more and 56° C. or less; A method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed, characterized by:

5. 2. The method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to claim 1, wherein an amount of water to be mixed in the first step is an amount such that a concentration of the nonionic surfactant relative to a total amount of the first processed product is 21 mg / mL or more and 45 mg / mL or less.

6. 6. A method for producing a carbonized material having a three-dimensional network structure in which mesopores are formed, comprising the steps of: heat-treating a phenolic resin having a three-dimensional network structure in which mesopores are formed, produced by the method for producing a phenolic resin having a three-dimensional network structure in which mesopores are formed according to any one of claims 1 to 5, in an inert gas atmosphere at 300°C or more and 450°C or less; calcining the resulting heat-treated product at 450°C or more and 800°C or less in an inert gas atmosphere; and carbonizing the resulting calcined product at 800°C or more and 2000°C or less in an inert gas atmosphere to obtain a carbonized material having a three-dimensional network structure in which mesopores are formed.

Citation Information

Patent Citations

  • Catalyst layer for fuel cell, carbon material for catalyst carrier, and method for manufacturing carbon material for catalyst carrier

    JP2018010806A

  • Supported metal catalyst, method for producing same, and method for producing carrier