Rubber composition and tire

A rubber composition with a rosin compound and filler, designed to change reversibly with water, addresses the lack of such properties in existing compositions, improving tire grip and abrasion resistance.

JP2024149371APending Publication Date: 2024-10-18SUMITOMO RUBBER INDUSTRIES LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023221492
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-06
Filing Date
2023-12-27
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing rubber compositions do not exhibit reversible changes in physical properties when exposed to water, which is crucial for improving grip performance and abrasion resistance in tires.

Method used

A rubber composition containing a rubber component, filler, and a rosin compound, formulated to satisfy the conditions tanδ when wet with water/tanδ when dry > 1.00 and E* when wet with water/E* when dry < 1.00, achieved through the use of rosin metal salts that aggregate and dissociate with water, altering the glass transition temperature and mobility of the rubber.

Benefits of technology

The composition exhibits reversible changes in physical properties with water, enhancing wet grip performance and abrasion resistance in tires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149371000003
    Figure 2024149371000003
  • Figure 2024149371000001
    Figure 2024149371000001
  • Figure 2024149371000002
    Figure 2024149371000002
Patent Text Reader

Abstract

To provide a rubber composition that exhibits reversible changes in physical properties due to exposure to water, and to provide a tire.SOLUTION: A rubber composition contains a rubber component, a filler and a rosin compound, while fulfilling the formulae (1)-(2): (1) tanδ in water-moist conditions / tan δ in dry conditions>1.00 and (2) E* in water-moist conditions / E* in dry conditions<1.00. (In the formulae (1) and (2), tanδ and E* denote a loss tangent and a complex modulus measured under conditions of 30°C temperature, 10% initial strain, 1% dynamic strain, 10 Hz frequency, and elongation mode).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition and a tire. [Background technology]

[0002] For products such as tires, various performances are being imparted by using various materials, and improvements in performance are being desired. Conventionally, there has been a demand for technologies aimed at improving grip performance and abrasion resistance (Patent Document 1, etc.). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-285524 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to solve the above problems and to provide a rubber composition and a tire that exhibit reversible changes in physical properties due to water. [Means for solving the problem]

[0005] The present invention relates to a rubber composition which contains a rubber component, a filler, and a rosin compound and satisfies the following formulas (1) and (2). (1) Tangent delta when wet / tangent delta when dry > 1.00 (2) E* when wet / E* when dry < 1.00 (In the formulas (1) and (2), tan δ and E* are the loss tangent and complex modulus measured under the conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, a frequency of 10 Hz, and an elongation mode.) Effect of the Invention

[0006] The present invention provides a rubber composition that contains a rubber component, a filler, and a rosin compound and satisfies the above formulas (1) and (2), and therefore can provide a rubber composition that exhibits reversible changes in physical properties due to water. [Brief description of the drawings]

[0007] [Figure 1] IR spectra of gum rosin, gum rosin Na, and gum rosin Zn. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] <Rubber composition> The present invention relates to a rubber composition that contains a rubber component, a rosin compound, and a filler, and satisfies the following formulas (1) and (2). (1) Tangent delta when wet / tangent delta when dry > 1.00 (2) E* when wet / E* when dry < 1.00 (In the formulas (1) and (2), tan δ and E* are the loss tangent and complex modulus measured under the conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, a frequency of 10 Hz, and an elongation mode.)

[0009] The reason why the above-mentioned effect is obtained is not entirely clear, but it is presumed to be due to the following mechanism. It is believed that when a rosin compound such as a rosin metal salt is blended into a rubber composition, the rubber composition aggregates due to strong ionic bonds and other bonds when it is dried, raising the glass transition temperature Tg and making it difficult for the rubber mixed with the rosin compound to move. On the other hand, when the rubber composition is wetted with water, it is believed that bonds such as ionic bonds are dissociated, Tg is lowered, and the rubber mixed with the rosin compound becomes more mobile. Therefore, it is presumed that by compounding a rosin compound such as a rosin metal salt, a rubber composition that satisfies the above formulas (1) and (2) is obtained, and that the rubber composition exhibits reversible changes in physical properties due to water.

[0010] In this way, the present invention solves the problem (objective) of exhibiting reversible changes in physical properties due to water by configuring a rubber composition that contains a rubber component, a rosin compound, and a filler, and satisfies the formula (1) "tan δ when wet with water / tan δ when dry>1.00" and the formula (2) "E* when wet with water / E* when dry<1.00". In other words, the parameters of formulas (1) and (2) do not define the problem (objective), and the object of the present invention is to exhibit reversible changes in physical properties due to water, and a configuration that satisfies the above parameters is used as a means to achieve this.

[0011] In this specification, the tan δ and E* of a rubber composition means the tan δ and E* of the rubber composition after crosslinking when the rubber composition is crosslinkable, for example, in the case of a crosslinkable rubber composition containing a diene rubber, sulfur, etc., the tan δ and E* of the rubber composition after vulcanization (crosslinking) are meant. Also, the tan δ and E* are values ​​obtained by carrying out a viscoelasticity test on the rubber composition (rubber composition after crosslinking).

[0012] The rubber composition exhibits reversible changes in physical properties due to the action of water. For example, the loss tangent (tan δ) and the complex modulus of elasticity (E*) are reversibly changed by the action of water. Here, in this specification, the loss tangent (tan δ) and complex modulus (E*) change reversibly due to water means that the tan δ and E* of the rubber composition (after vulcanization) reversibly increase or decrease due to the presence of water. For example, when changing from dry to wet to dry, it is sufficient that the tan δ and E* change reversibly, and the tan δ and E* do not have to be the same at the first drying time and the second drying time, and the tan δ and E* may be the same at the first drying time and the second drying time.

[0013] In this specification, tan δ and E* when dry means the tan δ and E* of a rubber composition in a dry state, specifically, the tan δ and E* of a rubber composition dried by the method described in the examples. In this specification, tan δ, E* when wet with water means the tan δ, E* of a rubber composition in a state wetted with water, specifically, the tan δ, E* of a rubber composition wetted with water by the method described in the examples.

[0014] In this specification, tan δ, E* of a rubber composition is a tan δ, E* measured under conditions of a temperature of 30° C., an initial strain of 10%, a dynamic strain of 1%, a frequency of 10 Hz, and an elongation mode.

[0015] The rubber composition satisfies the following formula (1). (1) Tangent delta when wet / tangent delta when dry > 1.00 (In formula (1), tan δ is the loss tangent measured under the conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, a frequency of 10 Hz, and an elongation mode.) Tan δ when wet with water / tan δ when dry is preferably 1.04 or more, preferably more than 1.06, more preferably more than 1.07, even more preferably more than 1.07, even more preferably more than 1.09, even more preferably more than 1.14, particularly preferably more than 1.19, and particularly preferably more than 1.20. The upper limit of tan δ when wet with water / tan δ when dry is not particularly limited, but is preferably 1.80 or less, more preferably 1.70 or less, even more preferably 1.65 or less, and particularly preferably 1.60 or less. Within the above range, the effect can be obtained favorably.

[0016] The rubber composition has a tan δ when wet with water of preferably 0.15 or more, more preferably 0.20 or more, even more preferably 0.22 or more, particularly preferably 0.24 or more, and especially preferably 0.28 or more. The upper limit of tan δ when wet with water is preferably 0.50 or less, more preferably 0.37 or less, even more preferably 0.31 or less, and especially preferably 0.30 or less. Within the above range, the effect can be suitably obtained.

[0017] The rubber composition satisfies the following formula (2). (2) E* when wet / E* when dry < 1.00 (In formula (2), E* is the complex modulus measured under the conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, a frequency of 10 Hz, and an elongation mode.) The ratio of E* when wet with water / E* when dry is preferably 0.98 or less, more preferably 0.97 or less, even more preferably less than 0.97, even more preferably less than 0.96, even more preferably less than 0.93, particularly preferably 0.92 or less, and especially preferably 0.91 or less. The lower limit of the ratio of E* when wet with water / E* when dry is preferably 0.80 or more, more preferably 0.83 or more, even more preferably 0.85 or more, and particularly preferably 0.87 or more. When it is within the above range, the effect can be obtained favorably.

[0018] The rubber composition has an E* value when wet with water of preferably 12.10 MPa or less, more preferably 9.33 MPa or less, even more preferably 8.40 MPa or less, even more preferably 8.20 MPa or less, especially preferably 5.00 MPa or less, and particularly preferably 4.82 MPa or less. The lower limit of E* when wet with water is preferably 3.00 MPa or more, more preferably 3.50 MPa or more, and even more preferably 4.00 MPa or more. When it is within the above range, the effect can be preferably obtained.

[0019] The reversible changes in tan δ and E* of the rubber composition due to water, as represented by the above formulas (1) and (2), can be achieved, for example, by compounding a rosin compound such as a rosin metal salt. Specifically, for example, when a rosin compound such as a rosin metal salt is compounded, the rubber composition aggregates due to strong ionic bonds when it is dried, increasing the glass transition temperature Tg, and the rubber mixed with the rosin compound becomes less mobile, whereas when the rubber composition is wet with water, the ionic bonds are dissociated, decreasing Tg, and the rubber mixed with the rosin compound becomes more mobile. As a result, it is believed that this can be achieved by an increase in tan δ and a decrease in E* when it is wet with water, and a decrease in tan δ and an increase in E* when it is dried.

[0020] The dry tan δ can be adjusted by the type and amount of chemicals (particularly rubber components, fillers, plasticizers, sulfur, vulcanization accelerators, and silane coupling agents) compounded in the rubber composition. For example, the dry tan δ tends to increase when a plasticizer (such as various resins) that is poorly compatible with the rubber component is used, when a non-modified polymer is used, when the amount of filler is increased, when the amount of plasticizer is increased, when the amount of sulfur is decreased, when the amount of vulcanization accelerator is decreased, or when the amount of silane coupling agent is decreased.

[0021] The dry E* can be adjusted by the types and amounts of chemicals (especially rubber components, fillers, and plasticizers) compounded in the rubber composition. For example, the dry E* tends to increase by reducing the amount of plasticizer or increasing the amount of filler.

[0022] For example, when a rosin compound such as a rosin metal salt is blended, ionic bonds dissociate when the rubber is wet, making it easier for the rubber to move. As a result, tan δ and E* tend to increase and E* decrease compared to when the rubber is dry. In addition, tan δ and E* when wet can be adjusted by the type and amount of chemicals blended into the rubber composition. For example, by using a method similar to the above-mentioned method for adjusting E* when dry and tan δ when dry, similar trends can be obtained for tan δ and E* when wet.

[0023] It is desirable that the rubber composition has the following formulas in which tan δ when wet / tan δ when dry (hereinafter also referred to as index 1) and E* when wet / E* when dry (hereinafter also referred to as index 2): Indicator 1 / Indicator 2>1.05 Index 1 / index 2 ((tan δ when wet / tan δ when dry) / (E* when wet / E* when dry)) is preferably 1.06 or more, more preferably greater than 1.10, even more preferably 1.11 or more, even more preferably 1.20 or more, especially more preferably greater than 1.20, especially more preferably 1.22 or more, particularly preferably greater than 1.28, and especially more preferably 1.30 or more. The upper limit of index 1 / index 2 is preferably 1.50 or less, more preferably 1.40 or less, and even more preferably 1.38 or less. Within the above range, the effect can be suitably obtained.

[0024] It is not clear why a greater effect is obtained by adjusting index 1 / index 2 > 1.05, but it is thought that when index 1 / index 2 shows a large value, the rubber tends to be less mobile when the rubber composition is dry and more mobile when wet with water, and as a result, reversible changes in physical properties are significantly exhibited by water.

[0025] Incidentally, index 1 (tan δ when wet with water / tan δ when dry) and index 2 (E* when wet with water / E* when dry) can be appropriately adjusted by adjusting tan δ when dry, E* when dry, tan δ when wet with water, and E* when wet with water using the method described above.

[0026] The rubber composition includes a rubber component. Here, the rubber component is a component that contributes to crosslinking, and generally corresponds to a polymer component that is not extracted with acetone and has a weight average molecular weight (Mw) of 10,000 or more. The rubber component is in a solid state at room temperature (25°C).

[0027] The weight average molecular weight of the rubber component is preferably 50,000 or more, more preferably 150,000 or more, even more preferably 200,000 or more, and particularly preferably 270,000 or more, and is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. Within the above ranges, the effect tends to be better obtained.

[0028] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) can be determined by standard polystyrene conversion based on the measured values ​​obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation).

[0029] The rubber component usable in the rubber composition may be either a non-modified rubber or a modified rubber. The modified rubber may be a rubber having a functional group that interacts with a filler such as silica. For example, the modified rubber may be a terminal modified rubber (terminal modified rubber having the functional group at the terminal) in which at least one terminal of the rubber is modified with a compound (modifier) ​​having the functional group, a main chain modified rubber having the functional group at the main chain, a main chain terminal modified rubber having the functional group at the main chain and terminal (for example, a main chain terminal modified rubber having the functional group at the main chain and at least one terminal modified with the modifier), or a terminal modified rubber modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or an epoxy group introduced therein.

[0030] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.

[0031] The rubber component may, for example, be a diene rubber. Examples of diene rubbers include isoprene rubber, butadiene rubber (BR), styrene butadiene rubber (SBR), styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR). Examples of rubber components include butyl rubber and fluororubber. These may be used alone or in combination of two or more. These rubber components may be modified or hydrogenated, and extended rubber extended with oil, resin, liquid rubber component, or the like may be used. Among these, it is preferable to include at least one of NR, BR, and SBR, more preferably to include at least two of NR, BR, and SBR, and even more preferably to include NR, BR, and SBR. It is nice.

[0032] Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubber industry-standard rubbers. Examples of IR include IR2200 and other rubber industry-standard rubbers. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more.

[0033] In the rubber composition, the content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less. Within the above ranges, the effect tends to be better obtained.

[0034] The BR is not particularly limited, and for example, high cis BR with a high cis content, BR containing syndiotactic polybutadiene crystals, BR synthesized using a rare earth catalyst (rare earth BR), etc. can be used. These may be used alone or in combination of two or more. In particular, the BR preferably contains high cis BR with a cis content of 90% by mass or more. The cis content is more preferably 95% by mass or more. The cis content can be measured by infrared absorption spectroscopy.

[0035] The cis amount of BR means the cis amount of the BR when there is one type of BR, and means the average cis amount when there are multiple types of BR. The average cis content of BR can be calculated by {Σ(content of each BR × cis content of each BR)} / total content of all BRs. For example, when 100% by mass of the rubber component contains 20% by mass of BR with a cis content of 90% by mass and 10% by mass of BR with a cis content of 40% by mass, the average cis content of BR is 73.3% by mass (=(20×90+10×40) / (20+10)).

[0036] In addition, either unmodified or modified BR can be used as the BR. Modified BR includes modified BR in which the same functional group as that of modified rubber is introduced. In addition, hydrogenated butadiene polymer (hydrogenated BR) can also be used as the BR.

[0037] As the BR, for example, products from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc. can be used.

[0038] In the rubber composition, the BR content in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less. Within the above ranges, the effect tends to be better obtained.

[0039] There are no particular limitations on the SBR, and examples of the SBR that can be used include emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. These may be used alone or in combination of two or more.

[0040] The styrene content of SBR is preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more. The styrene content is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. Within the above range, the effect tends to be better obtained. In this specification, the styrene content is 1 It can be measured by H-NMR measurement.

[0041] The styrene amount of SBR means the styrene amount of the SBR when there is one type of SBR, and means the average styrene amount when there are multiple types of SBR. The average styrene amount of SBR can be calculated by {Σ(content of each SBR × styrene amount of each SBR)} / total content of all SBRs. For example, when 100% by mass of the rubber component contains 85% by mass of SBR with a styrene amount of 40% by mass and 5% by mass of SBR with a styrene amount of 25% by mass, the average styrene amount of the SBR is 39.2% by mass (=(85×40+5×25) / (85+5)).

[0042] The vinyl bond content of SBR is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 41% by mass or more. The vinyl bond content is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. When it is within the above range, the effect tends to be better obtained. In this specification, the vinyl bond amount (1,2-bonded butadiene unit amount) can be measured by infrared absorption spectroscopy.

[0043] The vinyl content of SBR (amount of 1,2-bonded butadiene units) is the proportion of vinyl bonds when the total mass of the butadiene parts in SBR is taken as 100 (unit: mass%), and is calculated as vinyl content [mass%] + cis content [mass%] + trans content [mass%] = 100 [mass%]. When there is one type of SBR, it means the vinyl content of that SBR, and when there are multiple types, it means the average vinyl content. The average vinyl content of SBR can be calculated by Σ{content of each SBR × (100 [mass%] - styrene content of each SBR [mass%]) × vinyl content of each SBR [mass%]} / Σ{content of each SBR × (100 [mass%] - styrene content of each SBR [mass%])}. For example, in 100 parts by mass of the rubber component, there are 75 parts by mass of SBR with a styrene content of 40 mass% and a vinyl content of 30 mass%, 25 parts by mass of styrene, and 10 parts by mass of vinyl. In the case where SBR with a vinyl content of 20 mass% is 15 parts by mass and the remaining 10 parts by mass is a component other than SBR, the average vinyl content of the SBR is 28 mass% (={75 × (100 [mass%] - 40 [mass%]) × 30 [mass%] + 15 × (100 [mass%] - 25 [mass%]) × 20 [mass%])} / {75 × (100 [mass%] - 40 [mass%]) + 15 × (100 [mass%] - 25 [mass%])}.

[0044] Both unmodified and modified SBR can be used. Modified SBR includes modified SBR with the same functional groups as modified rubber. Hydrogenated styrene-butadiene copolymer (hydrogenated SBR) can also be used as SBR.

[0045] As the SBR, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc. can be used. In addition, SBR synthesized by a known method can also be used.

[0046] In the rubber composition, the content of SBR in 100% by mass of the rubber component is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, and is preferably 80% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. Within the above ranges, the effect tends to be better obtained.

[0047] The above rubber composition contains a filler. From the viewpoint of obtaining more effects, it is desirable that the content Fc (total amount of fillers such as carbon black and silica, parts by mass) of the filler with respect to 100 parts by mass of the rubber component satisfies the following formula. 40 < Fc < 90 The lower limit of Fc is preferably more than 42 parts by mass, more preferably more than 44 parts by mass, still more preferably 51 parts by mass or more. The upper limit of Fc is preferably 86 parts by mass or less, more preferably less than 85 parts by mass, still more preferably less than 80 parts by mass, and even more preferably less than 75 parts by mass. When within the above range, there is a tendency to obtain better effects.

[0048] When 40 < Fc < 90, the reason for obtaining more effects is not clear, but in the case of a rubber composition containing an appropriate amount of filler, the rubber is less likely to move during drying of the rubber composition, and the effect of making the rubber more likely to move when water-wetted is significantly obtained. As a result, it is considered that a reversible physical property change is significantly exhibited by water.

[0049] The above filler is not particularly limited, and materials known in the rubber field can be used. For example, inorganic fillers such as carbon black, silica, calcium carbonate, talc, alumina, clay, aluminum hydroxide, aluminum oxide, mica, biochar (BIO CHAR); poorly dispersible fillers, etc. can be mentioned. Among them, from the viewpoint of obtaining more effects, carbon-derived fillers (carbon-containing fillers) such as carbon black and silica are preferred. The filler may be used alone or in combination of two or more.

[0050] In the rubber composition, usable carbon black is not particularly limited, but examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin-Nichika Carbon Co., Ltd., and Columbia Carbon Co., Ltd. These may be used alone or in combination of two or more. In addition to conventional carbon black made from mineral oils, carbon black made from biomass materials such as lignin may be used. In addition, recycled carbon black obtained by decomposing rubber products and plastic products containing carbon black, such as tires, may be appropriately substituted for the above carbon black in an equal amount.

[0051] The nitrogen adsorption specific surface area (N2SA) of carbon black is 50m 2 / g or more is preferable, and 80m 2 / g or more is more preferable, and 100m 2 / g or more is more preferable, and 114m 2 / g or more is particularly preferable. 2 / g or less is preferable, and 130m 2 / g or less is more preferable, and 120m 2 Within the above range, there is a tendency that the effect is better obtained. The nitrogen adsorption specific surface area of ​​carbon black can be determined in accordance with JIS K6217-2:2001.

[0052] The dibutyl phthalate oil absorption (DBP) of the carbon black is preferably 40 ml / 100 g or more, more preferably 60 ml / 100 g or more, and even more preferably 70 ml / 100 g or more. In addition, when the DBP is within the above range of preferably 200 ml / 100 g or less, more preferably 150 ml / 100 g or less, and even more preferably 100 ml / 100 g or less, the effect tends to be better. The DBP of carbon black is determined by the measurement method of JIS K6217-4:2001.

[0053] In the rubber composition, the content of carbon black is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 6 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0054] In the rubber composition, examples of silica that can be used include dry process silica (anhydrous silica) and wet process silica (hydrated silica). Among them, wet process silica is preferred because it has a large number of silanol groups. Commercially available products include those from Degussa, Rhodia, Tosoh Silica, Solvay Japan, and Tokuyama. These may be used alone or in combination of two or more.

[0055] As the silica, plant-derived silica can also be suitably used. Examples of plant-derived silica include silica derived from plants containing silica. Examples of plants containing silica include rice, corn, sugarcane, horsetail, wheat, barley, rye, pearl barley, millet, foxtail millet, Japanese barnyard millet, and Erianthus. In addition, the saccharification residue of the above-mentioned plants containing silica can also be used. Among them, rice husks and straws with high silica content are preferred, and rice husks are more preferred. In addition, the plants containing silica may be those that have been burned to ash or those that have been carbonized.

[0056] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 50 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 / g or more, particularly preferably 175m 2The upper limit of the N2SA of silica is not particularly limited, but is preferably 350 m 2 / g or less, more preferably 300m 2 / g or less, more preferably 250m 2 Within the above range, there is a tendency for the effect to be better obtained. The N2SA of silica is a value measured by the BET method in accordance with ASTM D3037-93.

[0057] In the rubber composition, the content of silica is preferably 30 parts by mass or more, more preferably 40 parts by mass or more, and even more preferably 45 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 100 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 80 parts by mass or less. Within the above range, the effect tends to be better obtained. The content of the plant-derived silica and the content of the rice husk silica are also desirably in the same range.

[0058] Examples of the poorly dispersible filler include microfibrillated vegetable fibers, short fiber cellulose, gel compounds, etc. Among these, microfibrillated vegetable fibers are preferred.

[0059] The microfibrillated plant fiber is preferably cellulose microfibril, since it has good reinforcing properties. The cellulose microfibril is not particularly limited as long as it is derived from a natural product, and examples thereof include those derived from resource biomass such as fruits, grains, and root vegetables, wood, bamboo, hemp, jute, and kenaf, and pulp, paper, cloth, agricultural waste, waste biomass such as food waste and sewage sludge obtained from these as raw materials, unused biomass such as rice straw, wheat straw, and thinned wood, as well as cellulose produced by sea squirts, acetic acid bacteria, etc. These microfibrillated plant fibers may be used alone or in combination of two or more.

[0060] In this specification, cellulose microfibrils typically refer to cellulose fibers having an average fiber diameter of 10 μm or less, more typically cellulose fibers having a microstructure formed by the aggregation of cellulose molecules and an average fiber diameter of 500 nm or less. Typical cellulose microfibrils are formed, for example, as an aggregate of cellulose fibers having the above-mentioned average fiber diameter.

[0061] When the rubber composition contains a poorly dispersible filler, the content of the poorly dispersible filler is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit of the content is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less. Within the above range, the effect tends to be better obtained.

[0062] In the rubber composition, the silica content in the filler (100% by mass) is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more. The upper limit is not particularly limited and may be 100% by mass, but is preferably 95% by mass or less, more preferably 93% by mass or less, and even more preferably 90% by mass or less. Within the above range, the effect tends to be better obtained.

[0063] When the rubber composition contains silica, it is preferable that the rubber composition further contains a silane coupling agent. The silane coupling agent is not particularly limited, and those known in the rubber field can be used. For example, bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl-N, Examples of such silylsilanes include sulfide-based silylsilanes such as N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silylsilanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based silylsilanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silylsilanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silylsilanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silylsilanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based silylsilanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those manufactured by Degussa, Momentive, Shin-Etsu Silicones, Tokyo Chemical Industry, Azumax, and Dow Corning Toray Co., Ltd. These may be used alone or in combination of two or more.

[0064] In the rubber composition, the content of the silane coupling agent is preferably 0.1 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, particularly preferably 7 parts by mass or more, and particularly preferably 8 parts by mass or more, based on 100 parts by mass of silica. The upper limit of the content is preferably 50 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 15 parts by mass or less, and particularly preferably 10 parts by mass or less. Within the above range, the effect tends to be better obtained.

[0065] The rubber composition contains a rosin compound as a plasticizer. In this specification, the rosin compound means rosin, a rosin derivative derived from rosin, or a rosin metal salt (a rosin acid metal salt). The rosin compounds may be used alone or in combination of two or more kinds.

[0066] The glass transition temperature (Tg) of the rosin compound is preferably 20° C. or higher, more preferably 50° C. or higher, even more preferably 70° C. or higher, and particularly preferably 80° C. or higher. There is no particular upper limit, and the upper limit may be, for example, 1000° C. or lower, 800° C. or lower, or 700° C. or lower. Within the above range, better tire performance such as wet grip performance tends to be obtained. In this specification, the glass transition temperature (Tg) of raw materials such as a rosin compound can be measured by differential scanning calorimetry (DSC) at a temperature rise rate of 10° C. / min in accordance with JIS K 7121-1987.

[0067] In the rubber composition, the content of the rosin compound (total amount of rosin metal salt, rosin, etc.) is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, per 100 parts by mass of the rubber component. The upper limit is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less. Within the above range, the effect tends to be better obtained.

[0068] The rosin is a refined resin acid contained in pine, and can be classified into gum rosin, wood rosin, and tall oil rosin. The main components of the rosin are rosin acids such as abietic acid, neoabietic acid, levopimaric acid, hydroabietic acid, and dextropimaric acid.

[0069] Examples of the rosin derivative include disproportionated rosin, hydrogenated rosin, dehydrogenated rosin, polymerized rosin, rosin alcohol, rosin amine, unsaturated acid-modified rosin, and rosin esters thereof.

[0070] Among the above rosin compounds, rosin metal salts (rosin acid metal salts) are preferred from the viewpoint of obtaining a greater effect.

[0071] The rosin metal salt is, for example, a salt of rosin acid and a metal, such as a salt composed of rosin acid and a monovalent, divalent, trivalent, or tetravalent polyvalent metal. Specific examples include Na salt, K salt, Ca salt, Ba salt, Sr salt, Al salt, Zn salt, Cu salt, and Mg salt of rosin (rosin acid); reaction products of rosin and other metal compounds, and the like. Among these, sodium rosinate, zinc rosinate, and potassium rosinate are preferable from the viewpoint of obtaining a greater effect.

[0072] The reason why metal rosin salts such as sodium rosinate, zinc rosinate, and potassium rosinate are more effective is not clear, but it is thought that when metal rosin salts are used, the rubber tends to be less mobile when the rubber composition is dry and more mobile when wet with water, and as a result, reversible changes in physical properties are significantly exhibited by water.

[0073] The rosin metal salt can be synthesized, for example, by reacting rosin with a metal compound by a known method.

[0074] The glass transition temperature (Tg) of the rosin metal salt is preferably 20° C. or higher, more preferably 50° C. or higher, even more preferably 70° C. or higher, and particularly preferably 80° C. or higher. There is no particular upper limit, and the temperature may be, for example, 1000° C. or lower, 800° C. or lower, or 700° C. or lower. Within the above range, better tire performance such as wet grip performance tends to be obtained.

[0075] In the rubber composition, the content of the rosin metal salt is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less. Within the above range, the effect tends to be better obtained.

[0076] The rubber composition may contain a plasticizer other than the rosin compound. In this specification, the plasticizer is a material that imparts plasticity to the rubber component, and may be liquid or solid at room temperature (25° C.) These may be used alone or in combination of two or more kinds.

[0077] The plasticizer may be an oil, a liquid polymer, a resin, etc. These may be used alone or in combination of two or more kinds.

[0078] The oil is not particularly limited, and may be any conventionally known oil, such as paraffinic process oil, aromatic process oil, naphthenic process oil, low PCA (polycyclic aromatic) process oil such as TDAE and MES, vegetable-derived oil, and mixtures thereof. These may be used alone or in combination of two or more. From the viewpoint of life cycle analysis, lubricating oil or waste edible oil after use in a rubber mixing mixer or automobile engine may be used as appropriate.

[0079] Examples of the plant-derived oils (also called vegetable oils) include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil.

[0080] As the above oil, for example, products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mills Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., Nisshin Oillio Group Co., Ltd., etc. can be used.

[0081] Examples of the liquid polymer include liquid diene polymers (liquid rubber) and liquid farnesene polymers at 25°C. Examples of liquid rubber include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), and liquid styrene isoprene styrene block copolymers (liquid SIS block polymers). The ends or main chains of these may be modified with polar groups. Hydrogenated products of these may also be used.

[0082] The liquid diene polymer has a weight average molecular weight (Mw) of 1.0×10 in terms of polystyrene measured by gel permeation chromatography (GPC). 3 ~5.0×10 4 Preferably, it is 3.0×10 3 ~1.5×10 4 The lower or upper limit of Mw of the liquid diene polymer may be 4,500 or 8,500. In this specification, the Mw of the liquid diene-based polymer is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0083] As the liquid diene polymer, for example, products available from Sartomer Co., Ltd., Kuraray Co., Ltd., etc. can be used.

[0084] The resin may be a resin that is commonly used as a tire compound, and may be liquid or solid at room temperature (25°C). Examples of the resin include aromatic vinyl polymers, coumarone-indene resins, coumarone resins, indene resins, phenolic resins, petroleum resins, terpene resins, and acrylic resins. The resin may also be a hydrogenated resin (hydrogenated resin). These may be used alone or in combination of two or more. The resin itself may also be a copolymer of monomer components of multiple origins. Among these, aromatic vinyl polymers, petroleum resins, terpene resins, and hydrogenated resins thereof are preferable.

[0085] When a resin that is solid at room temperature is used, the softening point of the resin is preferably 50° C. or higher, more preferably 55° C. or higher, even more preferably 60° C. or higher, and particularly preferably 85° C. or higher. Also, the softening point is preferably 160° C. or lower, more preferably 150° C. or lower, even more preferably 140° C. or lower, and particularly preferably 100° C. or lower. Within the above range, the effect tends to be better obtained. When the resin is liquid at room temperature, the softening point is preferably 20° C. or lower, more preferably 10° C. or lower, and even more preferably 0° C. or lower. In the case of hydrogenated resins, it is desirable for the softening point to be similar to that mentioned above. The softening point of the resin is the temperature at which the ball drops when the softening point specified in JIS K6220-1:2001 is measured using a ring and ball softening point tester.

[0086] The aromatic vinyl polymer is a polymer containing an aromatic vinyl monomer as a structural unit. For example, it can be a resin obtained by polymerizing α-methylstyrene and / or styrene, and specifically, it can be a homopolymer of styrene (styrene resin), a homopolymer of α-methylstyrene (α-methylstyrene resin), a copolymer of α-methylstyrene and styrene, a copolymer of styrene and another monomer, etc.

[0087] The coumarone-indene resin is a resin containing coumarone and indene as main monomer components constituting the resin skeleton (main chain). Other monomer components contained in the skeleton besides coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc.

[0088] The coumarone resin is a resin containing coumarone as a main monomer component constituting the skeleton (main chain) of the resin.

[0089] The indene resin is a resin containing indene as a main monomer component constituting the skeleton (main chain) of the resin.

[0090] The phenolic resin may be a known polymer obtained by reacting phenol with an aldehyde such as formaldehyde, acetaldehyde, or furfural in the presence of an acid or alkali catalyst. Among these, those obtained by reacting with an acid catalyst (such as novolac-type phenolic resin) are preferred.

[0091] Examples of the petroleum resin include C5 resin, C9 resin, C5 / C9 resin, dicyclopentadiene (DCPD) resin, C9 / DCPD resin, and hydrogenated versions of these resins. Among these, DCPD resin, hydrogenated DCPD resin, C9 / DCPD resin, and C9 / hydrogenated DCPD resin are preferred.

[0092] The terpene resin is a polymer containing terpene as a constituent unit. For example, polyterpene resin obtained by polymerizing a terpene compound, aromatic modified terpene resin obtained by polymerizing a terpene compound and an aromatic compound, etc. can be mentioned. As the aromatic modified terpene resin, terpene phenol resin made from terpene compounds and phenolic compounds, terpene styrene resin made from terpene compounds and styrene compounds, and terpene phenol styrene resin made from terpene compounds, phenolic compounds, and styrene compounds can also be used. In addition, examples of the terpene compound include α-pinene, β-pinene, etc., examples of the phenolic compound include phenol, bisphenol A, etc., and examples of the aromatic compound include styrene compounds (styrene, α-methylstyrene, etc.). Among them, aromatic modified terpene resin is preferable.

[0093] The acrylic resin is a polymer containing an acrylic monomer as a constituent unit. For example, a styrene-acrylic resin having a carboxyl group and obtained by copolymerizing an aromatic vinyl monomer component and an acrylic monomer component, such as a styrene-acrylic resin, can be used. Among them, a solventless carboxyl group-containing styrene-acrylic resin can be preferably used.

[0094] Examples of the resins that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Exxon Mobil Corporation, KRATON, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., ENEOS Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.

[0095] From the viewpoint of sustainability, it is desirable to use, as the plasticizer, a plant-derived plasticizer such as the plant-derived oil or farnesene-based polymer.

[0096] Farnesene polymers are polymers obtained by polymerizing farnesene and have structural units based on farnesene. Farnesene has isomers such as α-farnesene ((3E,7E)-3,7,11-trimethyl-1,3,6,10-dodecatetraene) and β-farnesene (7,11-dimethyl-3-methylene-1,6,10-dodecatriene), but (E)-β-farnesene, which has the following structure, is preferred. [ka]

[0097] The farnesene-based polymer may be a homopolymer of farnesene (farnesene homopolymer) or a copolymer of farnesene and a vinyl monomer (farnesene-vinyl monomer copolymer). These may be used alone or in combination of two or more. Among them, a copolymer of farnesene and a vinyl monomer is preferred.

[0098] Examples of vinyl monomers include aromatic vinyl compounds such as styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, 5-t-butyl-2-methylstyrene, vinylethylbenzene, divinylbenzene, trivinylbenzene, divinylnaphthalene, tert-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethylether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-t-butylstyrene, 3-t-butylstyrene, 4-t-butylstyrene, vinylxylene, vinylnaphthalene, vinyltoluene, vinylpyridine, diphenylethylene, and tertiary amino group-containing diphenylethylene, as well as conjugated diene compounds such as butadiene and isoprene. These may be used alone or in combination of two or more. Among these, butadiene is preferred. That is, the farnesene-vinyl monomer copolymer is preferably a copolymer of farnesene and butadiene (farnesene-butadiene copolymer).

[0099] In the farnesene-vinyl monomer copolymer, the copolymerization ratio by mass of farnesene and vinyl monomer (farnesene / vinyl monomer) is preferably 40 / 60 to 90 / 10.

[0100] The farnesene-based polymer preferably has a weight average molecular weight (Mw) of 3000 or more and 300,000 or less. The Mw of the farnesene-based polymer is preferably 8000 or more, more preferably 10,000 or more, and is preferably 100,000 or less, more preferably 60,000 or less, and even more preferably 50,000 or less. Within the above ranges, the effect tends to be more preferably obtained.

[0101] The farnesene-based polymer may be either a liquid or solid polymer at room temperature (25° C.), and is preferably a liquid farnesene-based polymer that is a liquid at room temperature (25° C.).

[0102] In the rubber composition, the content of the plasticizer (total amount of the rosin compound and the plasticizer other than the rosin compound) is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, even more preferably 25 parts by mass or more, and even more preferably 35 parts by mass or more, per 100 parts by mass of the rubber component. The upper limit is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 45 parts by mass or less. Within the above range, the effect tends to be better obtained. The plasticizer content includes the amount of oil and resin contained in the oil-extended rubber and resin-extended rubber.

[0103] In the rubber composition, the content of the solid plasticizer in a solid state at room temperature (25°C) is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less. Within the above range, the effect tends to be better obtained. The content of the above resin in a solid state at room temperature (25° C.) is also desirably in the same range.

[0104] In the rubber composition, the content of the liquid plasticizer in a liquid state at room temperature (25°C) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less. Within the above range, the effect tends to be better obtained. The liquid plasticizer content includes the amount of oil contained in the oil-extended rubber and the amount of liquid resin in the resin-extended rubber that has been extended with the liquid resin. A similar range is also desirable for the oil content that is liquid at room temperature (25°C).

[0105] From the viewpoints of crack resistance, ozone resistance, and the like, the rubber composition preferably contains an antioxidant.

[0106] The antiaging agent is not particularly limited, and examples thereof include naphthylamine-based antiaging agents such as phenyl-α-naphthylamine; diphenylamine-based antiaging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, Examples of the antioxidant include p-phenylenediamine antioxidants such as amines; quinoline antioxidants such as polymerized 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Among these, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and polymerized 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. Commercially available products include, for example, products from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd.

[0107] In the rubber composition, the content of the antioxidant is preferably 1.0 part by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 4.0 parts by mass or more, based on 100 parts by mass of the rubber component. The content is preferably 7.0 parts by mass or less, and more preferably 5.0 parts by mass or less.

[0108] The rubber composition preferably contains stearic acid. In the above rubber composition, the content of stearic acid is preferably 0.5 parts by mass or more, more preferably 2.0 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, based on 100 parts by mass of the rubber component.

[0109] As the stearic acid, any conventionally known product can be used, for example, products available from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.

[0110] The rubber composition preferably contains zinc oxide. In the above rubber composition, the content of zinc oxide is preferably 0.5 parts by mass or more, more preferably 1.7 parts by mass or more, and preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, based on 100 parts by mass of the rubber component.

[0111] As the zinc oxide, any known zinc oxide can be used, for example, products available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc.

[0112] The rubber composition may contain wax. In the above rubber composition, the wax content per 100 parts by mass of the rubber component is preferably 1.0 part by mass or more, more preferably 2.0 parts by mass or more, and preferably 10.0 parts by mass or less, more preferably 7.0 parts by mass or less.

[0113] The wax is not particularly limited, and examples thereof include petroleum waxes, natural waxes, etc. Also, synthetic waxes obtained by refining or chemically treating multiple waxes can be used. These waxes may be used alone or in combination of two or more kinds.

[0114] Examples of petroleum waxes include paraffin wax and microcrystalline wax. Examples of natural waxes are not particularly limited as long as they are derived from resources other than petroleum, and include, for example, vegetable waxes such as candelilla wax, carnauba wax, Japan wax, rice wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; and refined products thereof. Examples of commercially available products include products from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., and Seiko Chemical Co., Ltd.

[0115] It is preferable to compound sulfur into the rubber composition in order to form an appropriate amount of crosslinked chains in the polymer chains and impart good performance.

[0116] In the rubber composition, the amount of sulfur is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, and even more preferably 1.0 part by mass or more, based on 100 parts by mass of the rubber component. The amount is preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, and even more preferably 2.0 parts by mass or less.

[0117] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0118] The rubber composition preferably contains a vulcanization accelerator. In the rubber composition, the content of the vulcanization accelerator is not particularly limited and may be freely determined according to the desired vulcanization speed and crosslink density, but is preferably 1.0 part by mass or more, more preferably 3.0 parts by mass or more, and even more preferably 4.4 parts by mass or more, based on 100 parts by mass of the rubber component. The upper limit is preferably 8.0 parts by mass or less, more preferably 7.0 parts by mass or less, and even more preferably 6.0 parts by mass or less.

[0119] The type of vulcanization accelerator is not particularly limited, and commonly used ones can be used. Examples of the vulcanization accelerator include benzothiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazyl sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolylguanidine, and orthotolylbiguanidine. As commercially available products, products of Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Industry Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. Among them, sulfenamide-based, guanidine-based, and benzothiazole-based vulcanization accelerators are preferred.

[0120] In addition to the above-mentioned components, the rubber composition may contain compounding agents generally used in the tire industry, such as materials such as a mold release agent.

[0121] The rubber composition can be produced, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.

[0122] As for the kneading conditions, in the base kneading step in which additives other than the crosslinking agent (vulcanizing agent) and the vulcanization accelerator are kneaded, the kneading temperature is preferably 100°C or higher, more preferably 120°C or higher, and also preferably 180°C or lower, more preferably 170°C. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is preferably 70°C or higher, more preferably 80°C or higher, and also preferably 120°C or lower, more preferably 110°C or lower. In addition, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is preferably 140°C or higher, more preferably 150°C or higher, and also preferably 190°C or lower, more preferably 185°C or lower.

[0123] The rubber composition can be used for tires, shoe soles, flooring materials, vibration-proof materials, seismic isolation materials, butyl frames, belts, hoses, packings, drug stoppers, and other rubber industrial products, etc. In particular, it is preferable to use the rubber composition as a tire rubber composition since it has excellent tire performance such as wet grip performance.

[0124] The tire components to which the rubber composition is applied are not particularly limited, and include any tire components such as cap tread, sidewall, base tread, bead apex, clinch apex, inner liner, under tread, breaker topping, bright topping, etc. Among them, the rubber composition is preferably applied to the cap tread because of its excellent wet grip performance.

[0125] <Tires> The rubber composition can be suitably used for tires. Examples of tires include pneumatic tires and non-pneumatic tires, and among these, pneumatic tires are preferred. In particular, the rubber composition can be suitably used as summer tires (summer tires), winter tires (studless tires, snow tires, studded tires, etc.), all-season tires, etc. Tires can be used as passenger car tires, large passenger car tires, large SUV tires, heavy load tires such as trucks and buses, light truck tires, two-wheeled automobile tires, racing tires (high performance tires), etc. Among these, the rubber composition can be suitably used for passenger car tires and light truck tires.

[0126] The tire is manufactured by a normal method using the rubber composition. For example, the rubber composition containing various materials is extruded in an unvulcanized state to match the shape of a tire component such as a cap tread, and molded together with other tire components in a tire building machine by a normal method to form an unvulcanized tire, and then heated and pressurized in a vulcanizer to manufacture the tire. EXAMPLES

[0127] In the following, examples (embodiments) that are considered to be preferable for carrying out the present invention will be shown, but the scope of the present invention is not limited to the examples.

[0128] (Synthesis of modified resin A (sodium rosinate)) Gum rosin is added to 10% by mass NaOH and stirred for 3 hours at 90 to 95° C. Water is then removed to obtain modified resin A (gum rosin Na).

[0129] (Synthesis of modified resin B (sodium rosinate)) The polymerized rosin is added to 10% by mass NaOH, and the mixture is stirred for 3 hours at 90 to 95° C. Water is then removed to obtain modified resin B (polymerized rosin Na).

[0130] (Synthesis of modified resin C (zinc rosinate)) Modified resin C (gum rosin Zn) is obtained by adding a ZnSO4 aqueous solution to the gum rosin Na aqueous solution produced in the synthesis of modified resin A and drying the precipitate.

[0131] The materials used in the synthesis of modified resins A to C are as follows: The glass transition temperature (Tg) of the rosin compound is measured by the following method. Gum rosin: Fujifilm Wako Pure Chemical Industries, Ltd. (Tg 40℃) Polymerized rosin: Synthomer (Tg90℃) NaOH: Fujifilm Wako Pure Chemical Industries, Ltd. ZnSO4: Fujifilm Wako Pure Chemical Industries, Ltd.

[0132] <Glass transition temperature (Tg)> The Tg of the rosin compound is determined as the glass transition onset temperature by measuring at a temperature increase rate of 10° C. / min using a differential scanning calorimeter (Q200) manufactured by TA Instruments Japan in accordance with JIS K 7121-1987.

[0133] Figure 1 shows the IR spectra of gum rosin, modified resin A (gum rosin Na), and modified resin C (gum rosin Zn) in the synthesis of modified resins A and C. The IR spectra show that gum rosin Na and gum rosin Zn were synthesized.

[0134] The various chemicals used in the manufacture of tires are described below. If necessary, the chemicals are refined according to standard methods.

[0135] NR: Nomura Trading Co., Ltd. SVR-L SBR: HPR840 manufactured by JSR Corporation (modified SBR, styrene content: 10% by mass, vinyl bond content: 41% by mass) BR: BR730 manufactured by JSR Corporation Carbon black: Diablack I (N220, N2SA114m) manufactured by Mitsubishi Chemical Corporation 2 / g) Silica: Ultrasil VN3 (N2SA175m) from Evonik Degussa2 / g) Silane coupling agent: EVONIK's Si266 (bis(3-triethoxysilylpropyl) disulfide) Oil: Diana Process NH-70S (aromatic process oil) manufactured by Idemitsu Kosan Co., Ltd. Aromatic vinyl polymer: SYLVARES SA85 (copolymer of α-methylstyrene and styrene, softening point: 85°C) manufactured by Arizona Chemical Co. Resin: Gum rosin (Tg 40℃) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Modified resin A: The above modified resin A (sodium rosinate) Modified resin B: The above modified resin B (sodium rosinate) Modified resin C: The above modified resin C (zinc rosinate) Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Antioxidant 1: Nocrac 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Antioxidant 2: Nocrac RD (poly(2,2,4-trimethyl-1,2-dihydroquinoline)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Stearic acid: NOF Corporation's "Tsubaki" stearic acid Sulfur: Powdered sulfur (containing 5% oil) manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator 1: Noccelaer D (diphenyl guanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0136] <Production of test tires> According to the formulation in Table 1, materials other than sulfur and vulcanization accelerator are kneaded to obtain a kneaded mixture. To the above kneaded material, sulfur and a vulcanization accelerator are added according to the formulation in Table 1, and the mixture is kneaded at 70° C. for 8 minutes to obtain an unvulcanized rubber composition. The unvulcanized rubber composition is extruded into a cap tread shape, and is laminated together with other tire components on a tire building machine to form an unvulcanized tire. The unvulcanized tire is press-vulcanized at 170°C for 20 minutes to obtain a test tire (size 195 / 65R15, specifications: Table 1).

[0137] The results of calculations based on the following evaluation method were shown in Table 1, assuming test tires obtained from rubber compositions whose formulations and specifications were changed according to Table 1. The reference comparative examples are as follows. Reference Comparative Example: Comparative Example 1

[0138] <Viscoelasticity test> A viscoelasticity measurement sample of 40 mm in length, 3 mm in width, and 0.5 mm in thickness is taken from inside the rubber layer of the cap tread of each test tire so that the long side is in the tire circumferential direction, and tan δ and E* are measured using a TA Instruments RSA series under the conditions of temperature 30°C, initial strain 10%, dynamic strain 1%, frequency 10 Hz, elongation mode, and measurement time 10 minutes, and the measured value is obtained 10 minutes after the start of measurement. The thickness direction of the sample is the tire radial direction.

[0139] <E* and tan δ when dry> The viscoelasticity measurement sample (length 40 mm × width 3 mm × thickness 0.5 mm) is dried under normal temperature and pressure conditions until it reaches a constant weight, to obtain a dry vulcanized rubber composition. The complex elastic modulus E* and loss tangent tanδ of the dried vulcanized rubber composition (rubber piece) are measured by the above-mentioned method, and these are defined as E* and tanδ when dried.

[0140] <E* and tan δ when wet with water> The above viscoelasticity measurement sample (length 40 mm x width 3 mm x thickness 0.5 mm) is immersed in 100 ml of water at 23°C for 2 hours to obtain a vulcanized rubber composition when wet with water. The complex elastic modulus E* and loss tangent tanδ of the vulcanized rubber composition (rubber piece) when wet with water are measured in water by the above-mentioned method using an RSA immersion measurement tool, and these are defined as E* and tanδ when wet with water. The water temperature is set to 30°C.

[0141] <Wet grip performance> Each test tire is fitted to all wheels of a vehicle (domestic FF 2000cc) and driven around a course on wet roads for 10 laps. 20 test drivers evaluate the braking performance on wet roads on a 5-point scale from 1 to 5. The higher the score, the better the performance. The scores of the 20 drivers are added together and the total score of the standard comparative example is set to 100 to create an index. The higher the index, the better the wet grip performance.

[0142] [Table 1]

[0143] The present invention (1) is a rubber composition that contains a rubber component, a filler, and a rosin compound and satisfies the following formulas (1) and (2). (1) Tangent delta when wet / tangent delta when dry > 1.00 (2) E* when wet / E* when dry < 1.00 (In the formulas (1) and (2), tan δ and E* are the loss tangent and complex modulus measured under the conditions of a temperature of 30°C, an initial strain of 10%, a dynamic strain of 1%, a frequency of 10 Hz, and an elongation mode.)

[0144] The present invention (2) is the rubber composition according to the present invention (1), wherein the content Fc (parts by mass) of the filler relative to 100 parts by mass of the rubber component satisfies the following formula: 40 <Fc<90

[0145] The present invention (3) is the rubber composition according to the present invention (1) or (2), in which the rosin compound contains a rosin metal salt.

[0146] The present invention (4) is a rubber composition in any combination with any of the present inventions (1) to (3), in which the rosin compound is at least one selected from the group consisting of sodium rosinate and zinc rosinate.

[0147] The present disclosure (5) is a rubber composition in any combination with any of the present inventions (1) to (4), wherein the rubber component contains at least one of natural rubber, butadiene rubber, and styrene-butadiene rubber.

[0148] The present disclosure (6) is a rubber composition in any combination with any of the present inventions (1) to (5), in which the content of natural rubber in 100% by mass of the rubber component is 30 to 70% by mass.

[0149] The present disclosure (7) is a rubber composition in any combination with any of the present inventions (1) to (6), in which the content of the butadiene rubber in 100% by mass of the rubber component is 5 to 50% by mass.

[0150] The present disclosure (8) is a rubber composition in any combination with any of the present inventions (1) to (7), in which the content of the styrene-butadiene rubber in 100% by mass of the rubber component is 20 to 80% by mass.

[0151] The present disclosure (9) is a rubber composition in any combination with any of the present inventions (5) to (8), in which the styrene content of the styrene-butadiene rubber is 5 to 50 mass %.

[0152] The present disclosure (10) is a rubber composition in any combination with any of the present inventions (5) to (9), in which the vinyl bond amount of the styrene-butadiene rubber is 10 to 70 mass %.

[0153] The present disclosure (11) is directed to a method for manufacturing a filler comprising the steps of: 2 The rubber composition is any combination of the rubber composition of the present invention (1) to (10) in which the total weight of the rubber component is 1000 g / g.

[0154] The present disclosure (12) is a rubber composition in any combination with any of the present inventions (1) to (11), in which the carbon black content per 100 parts by mass of the rubber component is 1 to 50 parts by mass.

[0155] The present disclosure (13) is a rubber composition in any combination with any of the present inventions (1) to (12), in which the content of silica per 100 parts by mass of the rubber component is 40 to 80 parts by mass.

[0156] The present disclosure (14) is a rubber composition in any combination with any of the present inventions (1) to (13), in which the content of the rosin compound per 100 parts by mass of the rubber component is 5 to 50 parts by mass.

[0157] The present invention (15) is a rubber composition in any combination with any of the present inventions (1) to (14), which satisfies the following formula, when the water-wet tan δ / dry tan δ is index 1 and the water-wet E* / dry E* is index 2: Indicator 1 / Indicator 2>1.05

[0158] The present invention (16) is the rubber composition according to the present invention (15), which satisfies the following formula: Indicator 1 / Indicator 2>1.10

[0159] The present invention (17) is a rubber composition in any combination with any of the present inventions (1) to (16) which satisfies the following formula: Tan δ when wet / tan δ when dry>1.07

[0160] The present invention (18) is a rubber composition in any combination with any of the present inventions (1) to (17) which satisfies the following formula: E* when wet / E* when dry<0.97

[0161] The present invention (19) is a tire having a cap tread constituted of a rubber composition in any combination with any of the present inventions (1) to (18).

Claims

1. A rubber composition comprising a rubber component, a filler, and a rosin compound, and satisfying the following formulas (1) and (2): (1) tan δ when wet with water / tan δ when dry > 1.00 (2) E* when wet / E* when dry < 1.00 (In the formulas (1) and (2), tan δ and E* are the loss tangent and complex modulus measured under the conditions of a temperature of 30° C., an initial strain of 10%, a dynamic strain of 1%, a frequency of 10 Hz, and an elongation mode.)

2. The rubber composition according to claim 1 , wherein a content Fc (parts by mass) of the filler relative to 100 parts by mass of the rubber component satisfies the following formula: 40<Fc<90

3. The rubber composition according to claim 1 or 2, wherein the rosin compound comprises a rosin metal salt.

4. 3. The rubber composition according to claim 1, wherein the rosin compound is at least one selected from the group consisting of sodium rosinate and zinc rosinate.

5. The rubber composition according to claim 1 or 2, wherein the rubber component comprises at least one of natural rubber, butadiene rubber, and styrene-butadiene rubber.

6. 3. The rubber composition according to claim 1, wherein the content of the natural rubber in 100% by mass of the rubber component is 30 to 70% by mass.

7. 3. The rubber composition according to claim 1, wherein the content of the butadiene rubber in 100% by mass of the rubber component is 5 to 50% by mass.

8. The rubber composition according to claim 1 or 2, wherein the content of the styrene-butadiene rubber in 100% by mass of the rubber component is 20 to 80% by mass.

9. The rubber composition according to claim 5, wherein the styrene-butadiene rubber has a styrene content of 5 to 50 mass %.

10. The rubber composition according to claim 5, wherein the styrene-butadiene rubber has a vinyl bond content of 10 to 70 mass %.

11. The filler contains carbon black, and N of the carbon black 2 SA is 50-150m 2 The rubber composition according to claim 1 or 2, wherein the elastic modulus is 1 / g.

12. 3. The rubber composition according to claim 1, wherein the amount of carbon black per 100 parts by mass of the rubber component is 1 to 50 parts by mass.

13. The rubber composition according to claim 1 or 2, wherein the content of silica per 100 parts by mass of the rubber component is 40 to 80 parts by mass.

14. The rubber composition according to claim 1 or 2, wherein the content of the rosin compound per 100 parts by mass of the rubber component is 5 to 50 parts by mass.

15. The rubber composition according to claim 1 or 2, wherein the ratio of tan δ when wetted with water / tan δ when dry is index 1 and the ratio of E* when wetted with water / E* when dry is index 2, satisfies the following formula: Indicator 1 / Indicator 2 > 1.05

16. The rubber composition according to claim 15, which satisfies the following formula: Indicator 1 / Indicator 2 > 1.10

17. The rubber composition according to claim 1 or 2, which satisfies the following formula: Tan δ when wet with water / tan δ when dry>1.07

18. The rubber composition according to claim 1 or 2, which satisfies the following formula: E* when wet / E* when dry < 0.97

19. A tire having a cap tread made of the rubber composition according to claim 1 or 2.

Citation Information

Patent Citations