Optical film

By using a crystalline polymer resin film treated with a solvent and dried to adjust birefringence, the optical film achieves reduced thickness-direction birefringence, improving display quality and enabling controlled optical properties in stretched films.

JP2024149703AInactive Publication Date: 2024-10-18ZEON CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024129817
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional optical films with anisotropic refractive indices face challenges in achieving a balanced birefringence in the thickness and in-plane directions, particularly in reducing birefringence in the thickness direction to improve display quality, such as viewing angle and contrast, which is difficult with polymers having positive intrinsic birefringence.

Method used

A method involving a resin film made of a crystalline polymer with positive intrinsic birefringence, where the film is contacted with a solvent to adjust birefringence in the thickness direction, followed by drying to achieve a specific birefringence range, enabling the production of an optical film with a negative birefringence in the thickness direction and a negative NZ coefficient.

Benefits of technology

The method allows for the production of an optical film with reduced birefringence in the thickness direction, enhancing display quality by improving viewing angle and contrast, and facilitating the production of stretched films with controlled optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149703000001
    Figure 2024149703000001
Patent Text Reader

Abstract

To provide an optical film which is formed of resin including a crystalline polymer with a positive intrinsic birefringence and has a small birefringence in a thickness direction.SOLUTION: An optical film is formed of resin including a crystalline polymer with a positive intrinsic birefringence. A birefringence Rth / d in a thickness direction of the optical film is -14.0×10-3 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical film, a method for producing the same, and a method for producing a stretched film using the optical film. [Background technology]

[0002] 2. Description of the Related Art Conventionally, techniques for producing films using resins have been proposed (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2020 / 066899 [Patent Document 2] International Publication No. 2017 / 065222 Summary of the Invention [Problem to be solved by the invention]

[0004] Resins may be used to manufacture optical films having anisotropy in refractive index. Such optical films having anisotropy in refractive index may have birefringence. Optical films having birefringence may be provided in display devices as films such as anti-reflection films and viewing angle compensation films.

[0005] When an optical film is provided in a display device, it is required to appropriately adjust the balance between the birefringence in the thickness direction and the birefringence in the in-plane direction perpendicular to the thickness direction. The balance between the birefringence in the thickness direction and the birefringence in the in-plane direction can be expressed by the NZ coefficient of the optical film. For example, if an optical film with an NZ coefficient of less than 1.0 is obtained, the optical film can improve the display quality of the display device, such as the viewing angle, contrast, and image quality.

[0006] When trying to make an optical film with an NZ coefficient of less than 1.0 thinner, it is desirable to reduce the birefringence in the thickness direction of the optical film. In particular, it is desirable to make the birefringence in the thickness direction a negative value and to increase the absolute value. However, it is difficult to reduce the birefringence in the thickness direction in an optical film manufactured using a polymer with positive intrinsic birefringence. For this reason, it is desirable to use a polymer with positive intrinsic birefringence and to reduce the birefringence in the thickness direction by -11.5×10 -3 It has not yet been possible to obtain an optical film having the following birefringence in the thickness direction:

[0007] The present invention has been devised in view of the above-mentioned problems, and aims to provide an optical film and a method for producing the same, which are formed from a resin containing a crystalline polymer having positive intrinsic birefringence and have small birefringence in the thickness direction; and a method for producing a stretched film using the optical film. [Means for solving the problem]

[0008] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a method including a step of contacting a resin film formed from a resin containing a crystalline polymer having positive intrinsic birefringence with a solvent to change the birefringence in the thickness direction, and have completed the present invention. That is, the present invention includes the following.

[0009] [1] An optical film formed of a resin containing a crystalline polymer having positive intrinsic birefringence, The birefringence Rth / d in the thickness direction of the optical film is −11.5×10 -3 The following is an optical film. [2] The optical film according to [1], wherein the crystalline polymer contains an alicyclic structure. [3] The optical film according to [1] or [2], wherein the crystallinity of the crystalline polymer measured by X-ray diffraction is 10% or more. [4] A method for producing the optical film according to any one of [1] to [3], (i) preparing a resin film formed of a resin containing a crystalline polymer having positive intrinsic birefringence; and (ii) contacting the resin film with a solvent to change the birefringence in the thickness direction. [5] The method for producing an optical film according to [4], further comprising the step (iii) of drying the resin film after the step (ii) to change the birefringence in the thickness direction. [6] A method for producing a stretched film, comprising stretching the optical film according to any one of [1] to [3]. [7] The method for producing a stretched film according to [6], wherein the thickness of the stretched film is 20 μm or less. [8] The method for producing a stretched film according to [6] or [7], wherein the stretched film has an NZ coefficient of 0.0 or more and less than 1.0. Effect of the Invention

[0010] According to the present invention, there can be provided an optical film formed of a resin containing a crystalline polymer having positive intrinsic birefringence and having small birefringence in the thickness direction, and a method for producing the same; and a method for producing a stretched film using the optical film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0012] In the following description, the in-plane retardation Re of the film is a value expressed by Re = (nx - ny) x d unless otherwise specified. The birefringence in the in-plane direction of the film is a value expressed by (nx - ny) unless otherwise specified, and is therefore expressed by Re / d. The retardation Rth in the thickness direction of the film is a value expressed by Rth = [{(nx + ny) / 2} - nz] x d unless otherwise specified. The birefringence in the thickness direction of the film is a value expressed by [{(nx + ny) / 2} - nz] unless otherwise specified, and is therefore expressed by Rth / d. The NZ coefficient of the film is a value expressed by (nx - nz) / (nx - ny) unless otherwise specified. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the film (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in the in-plane direction of the film and perpendicular to the direction of nx. nz represents the refractive index in the thickness direction of the film. d represents the thickness of the film. The measurement wavelength is 590 nm unless otherwise specified.

[0013] In the following description, unless otherwise specified, a material having positive intrinsic birefringence means a material whose refractive index in the stretching direction is greater than that in the direction perpendicular thereto. Thus, unless otherwise specified, a polymer having positive intrinsic birefringence means a polymer whose refractive index in the stretching direction is greater than that in the direction perpendicular thereto. Furthermore, unless otherwise specified, a resin having positive intrinsic birefringence means a resin whose refractive index in the stretching direction is greater than that in the direction perpendicular thereto.

[0014] In the following description, a "long" shape refers to a shape having a length 5 times or more than the width, preferably 10 times or more, specifically a film shape having a length that can be wound into a roll for storage or transportation. There is no particular upper limit on the length, but it is usually 100,000 times or less than the width.

[0015] In the following description, unless otherwise specified, the directions of elements as "parallel," "vertical," and "orthogonal" may include an error within a range that does not impair the effect of the present invention, for example, within a range of ±5°.

[0016] In the following description, unless otherwise specified, the terms "polarizing plate," "circular polarizing plate," "wave plate," and "positive C plate" include not only rigid members but also flexible members such as resin films.

[0017] [1. Overview of optical films] An optical film according to one embodiment of the present invention satisfies the following requirements (A) and (B) in combination. Requirement (A): The optical film is formed from a resin containing a crystalline polymer having positive intrinsic birefringence. Requirement (B): The birefringence Rth / d in the thickness direction of the optical film is -11.5×10 -3 The following is the result.

[0018] Although the above optical film has been difficult to produce in the past, it can be easily produced by using a specific production method described later.

[0019] [2. Resins containing crystalline polymers] The optical film according to one embodiment of the present invention is formed of a resin containing a crystalline polymer having positive intrinsic birefringence. The crystalline polymer refers to a polymer having crystallinity. The crystalline polymer refers to a polymer having a melting point Tm (i.e., the melting point Tm can be observed by a differential scanning calorimeter (DSC)). In the following description, a resin containing a crystalline polymer may be referred to as a "crystalline resin".

[0020] The crystalline polymer contained in the optical film has a positive intrinsic birefringence. Therefore, the crystalline resin containing the crystalline polymer also usually has a positive intrinsic birefringence. The crystalline resin is preferably a thermoplastic resin. The optical film preferably contains a crystalline resin, and more preferably consists of only a crystalline resin.

[0021] The crystalline polymer may be, for example, polyester such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN); polyolefin such as polyethylene (PE) or polypropylene (PP); and the like, but is not particularly limited, and preferably contains an alicyclic structure. When a crystalline polymer containing an alicyclic structure is used, the mechanical properties, heat resistance, transparency, low moisture absorption, dimensional stability, and light weight of the optical film can be improved. The polymer containing an alicyclic structure refers to a polymer having an alicyclic structure in the molecule. Such a polymer containing an alicyclic structure may be, for example, a polymer obtained by a polymerization reaction using a cyclic olefin as a monomer, or a hydrogenated product thereof.

[0022] Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure. Among these, the cycloalkane structure is preferred because it is easy to obtain an optical film having excellent properties such as thermal stability. The number of carbon atoms contained in one alicyclic structure is preferably 4 or more, more preferably 5 or more, and preferably 30 or less, more preferably 20 or less, and particularly preferably 15 or less. When the number of carbon atoms contained in one alicyclic structure is within the above range, mechanical strength, heat resistance, and moldability are highly balanced.

[0023] In the crystalline polymer containing an alicyclic structure, the ratio of the structural unit having an alicyclic structure to all structural units is preferably 30% by weight or more, more preferably 50% by weight or more, and particularly preferably 70% by weight or more. When the ratio of the structural unit having an alicyclic structure is high as described above, heat resistance can be improved. The ratio of the structural unit having an alicyclic structure to all structural units can be 100% by weight or less. In addition, in the crystalline polymer containing an alicyclic structure, the remainder other than the structural unit having an alicyclic structure is not particularly limited and can be appropriately selected according to the purpose of use.

[0024] Examples of the crystalline polymer containing an alicyclic structure include the following polymers (α) to (δ). Among these, polymer (β) is preferred because it is easy to obtain an optical film having excellent heat resistance. Polymer (α): A ring-opening polymer of a cyclic olefin monomer, which has crystallinity. Polymer (β): A hydrogenated product of polymer (α) and has crystallinity. Polymer (γ): An addition polymer of a cyclic olefin monomer, which has crystallinity. Polymer (δ): A hydrogenated polymer (γ) having crystallinity.

[0025] Specifically, the crystalline polymer containing an alicyclic structure is preferably a dicyclopentadiene ring-opening polymer having crystallinity, and a dicyclopentadiene ring-opening polymer hydrogenation product having crystallinity. Among them, a dicyclopentadiene ring-opening polymer hydrogenation product having crystallinity is particularly preferred. Here, the dicyclopentadiene ring-opening polymer refers to a polymer in which the ratio of dicyclopentadiene-derived structural units to all structural units is usually 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more, and even more preferably 100% by weight.

[0026] The hydrogenated ring-opening polymer of dicyclopentadiene preferably has a high ratio of racemo dyads. Specifically, the ratio of racemo dyads in the repeating units of the hydrogenated ring-opening polymer of dicyclopentadiene is preferably 51% or more, more preferably 70% or more, and particularly preferably 85% or more. A high ratio of racemo dyads indicates high syndiotactic stereoregularity. Therefore, the higher the ratio of racemo dyads, the higher the melting point of the hydrogenated ring-opening polymer of dicyclopentadiene tends to be. The ratio of racemo-dyads is described in the Examples below. 13 It can be determined based on C-NMR spectrum analysis.

[0027] As the polymer (α) to polymer (δ), polymers obtained by the production method disclosed in WO 2018 / 062067 can be used.

[0028] The melting point Tm of the crystalline polymer is preferably 200° C. or higher, more preferably 230° C. or higher, and preferably 290° C. or lower. When a crystalline polymer having such a melting point Tm is used, an optical film having an even better balance between moldability and heat resistance can be obtained.

[0029] Generally, a crystalline polymer has a glass transition temperature Tg. The specific glass transition temperature Tg of a crystalline polymer is not particularly limited, but is generally 85°C or higher and generally 170°C or lower.

[0030] The glass transition temperature Tg and melting point Tm of a polymer can be measured by the following method. First, the polymer is melted by heating, and the melted polymer is quenched with dry ice. Then, using this polymer as a test specimen, the glass transition temperature Tg and melting point Tm of the polymer can be measured using a differential scanning calorimeter (DSC) at a heating rate of 10° C. / min (heating mode).

[0031] The weight average molecular weight (Mw) of the crystalline polymer is preferably 1,000 or more, more preferably 2,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less. A crystalline polymer having such a weight average molecular weight has an excellent balance between moldability and heat resistance.

[0032] The molecular weight distribution (Mw / Mn) of the crystalline polymer is preferably 1.0 or more, more preferably 1.5 or more, and is preferably 4.0 or less, more preferably 3.5 or less. Here, Mn represents the number average molecular weight. A crystalline polymer having such a molecular weight distribution has excellent moldability.

[0033] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the polymer can be measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a developing solvent.

[0034] The degree of crystallinity of the crystalline polymer contained in the optical film is preferably 10% or more, more preferably 13% or more, and particularly preferably 15% or more. There is no particular upper limit, and it can be, for example, 40% or less. The degree of crystallinity of the crystalline polymer can be measured by X-ray diffraction. In general, when X-ray diffraction measurement is performed on a crystallized crystalline polymer, a peak occurs in the diffracted X-ray intensity at a specific diffraction angle 2θ. When X-ray diffraction measurement is performed on a crystalline polymer contained in an optical film, a peak can be measured at a specific diffraction angle 2θ, and the crystallinity of the crystalline polymer contained in the optical film can be measured by this peak. When X-ray diffraction measurement is performed on a crystalline polymer contained in an optical film, a broad peak can be measured at the specific diffraction angle 2θ. Therefore, the present inventor believes that the value of the degree of crystallinity of the crystalline polymer contained in the optical film may include the influence of diffraction due to factors other than the crystallization of the crystalline polymer. However, the high crystallinity of the crystalline polymer contained in the optical film indicates that the molecules of the crystalline polymer contained in the optical film have an orientation state with regularity that can at least cause X-ray diffraction. Therefore, the crystallinity is a parameter that represents the orientation state of the molecules of the crystalline polymer contained in the optical film, and is therefore considered to be related to the optical properties of the optical film according to this embodiment.

[0035] The crystalline polymer may be used alone or in combination of two or more kinds in any ratio.

[0036] The proportion of the crystalline polymer in the crystalline resin is preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 90% by weight or more. When the proportion of the crystalline polymer is equal to or more than the lower limit of the above range, the birefringence expression and heat resistance of the optical film can be improved. The upper limit of the proportion of the crystalline polymer can be 100% by weight or less.

[0037] The crystalline resin may contain optional components in addition to the crystalline polymer. Examples of the optional components include antioxidants such as phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants; light stabilizers such as hindered amine-based light stabilizers; waxes such as petroleum wax, Fischer-Tropsch wax, and polyalkylene wax; nucleating agents such as sorbitol-based compounds, metal salts of organic phosphoric acids, metal salts of organic carboxylic acids, kaolin, and talc; diaminostilbene derivatives, coumarin derivatives, and azole-based derivatives (e.g., benzoxazole derivatives, benzotriazole derivatives, and benzimide derivatives). Examples of the optional components include fluorescent brighteners such as benzothiazole derivatives, carbazole derivatives, pyridine derivatives, naphthalic acid derivatives, and imidazolone derivatives; ultraviolet absorbers such as benzophenone-based ultraviolet absorbers, salicylic acid-based ultraviolet absorbers, and benzotriazole-based ultraviolet absorbers; inorganic fillers such as talc, silica, calcium carbonate, and glass fibers; colorants; flame retardants; flame retardant assistants; antistatic agents; plasticizers; near-infrared absorbers; lubricants; fillers; and any polymer other than a crystalline polymer, such as a soft polymer. The optional components may be used alone or in combination of two or more types in any ratio. The amount of the optional components may be appropriately determined within a range that does not significantly impair the effects of the present invention. The amount of the optional components may be, for example, within a range that can maintain the total light transmittance of the optical film at 85% or more.

[0038] [3. Birefringence Rth / d in the thickness direction of optical film] The optical film according to one embodiment of the present invention has a birefringence Rth / d in a specific range in the thickness direction. Specifically, the birefringence Rth / d in the thickness direction of the optical film is usually −11.5×10 -3 Below, preferably -12.0 x 10 -3 Less than or equal to -14.0×10 -3 The following is particularly preferably -16.0 x 10 -3 The lower limit of the birefringence Rth / d in the thickness direction of the optical film is not particularly limited, but from the viewpoint of achieving short production time, it is preferably −50.0×10 -3 More preferably, -40.0×10 -3More preferably, −30.0×10 -3 That's all.

[0039] A film formed of a resin containing a polymer having positive intrinsic birefringence, such as the optical film according to the present embodiment, generally has positive birefringence characteristics. The film "has positive birefringence characteristics" means that when the film is stretched in one stretching direction, the increase in the refractive index in the stretching direction is greater than the increase in the refractive index in the direction perpendicular to the stretching direction. Since it is an increase, when the refractive index increases due to stretching, the increase in the refractive index is a positive value, and when the refractive index decreases due to stretching, the increase in the refractive index is a negative value.

[0040] Therefore, when a film formed from a crystalline resin containing a crystalline polymer having positive intrinsic birefringence is stretched in the in-plane direction, the refractive index in the thickness direction may become small. Therefore, when stretched, the birefringence in the thickness direction of the film usually becomes a positive value. Even if the birefringence in the thickness direction of the film becomes negative, the value usually only becomes close to 0. Therefore, in conventional technology, a crystalline resin containing a crystalline polymer having positive intrinsic birefringence can reduce the refractive index in the thickness direction by -11.5×10 -3 In view of the above circumstances, it is surprising for a person skilled in the art that the optical film according to the present embodiment can achieve the above-mentioned small birefringence Rth / d in the thickness direction within a specific range.

[0041] [4. Characteristics of optical films] As described above, the optical film according to one embodiment of the present invention has a small thickness direction birefringence Rth / d, and therefore can have a small thickness direction retardation. More specifically, the optical film has a negative thickness direction retardation, and the absolute value of the thickness direction retardation can be increased. The specific range of the thickness direction retardation of the optical film can be set according to the application of the optical film. For example, the thickness direction retardation of the optical film is preferably -2000 nm or more, more preferably -1000 nm or more, particularly preferably -500 nm or more, and preferably -50 nm or less, more preferably -100 nm or less.

[0042] The in-plane retardation of the optical film according to one embodiment of the present invention is not particularly limited and can be set according to the application of the optical film. For example, the specific in-plane retardation Re of the optical film can be preferably 10 nm or less, more preferably 5 nm or less, and particularly preferably 3 nm or less. When the in-plane retardation Re of the optical film is within the above-mentioned preferred range, the optical film can be used as a positive C plate. In addition, when the optical film is used as a material for a stretched film, the control of the optical properties of the stretched film obtained after stretching can be simplified.

[0043] The retardation of the film can be measured by a phase difference meter ("AxoScanOPMF-1" manufactured by AXOMETRICS).

[0044] The in-plane birefringence Re / d of the optical film according to one embodiment of the present invention is not particularly limited and can be set according to the application of the optical film. For example, the specific in-plane birefringence Re / d of the optical film is preferably 0.0 to 1.0×10 -3 , more preferably 0.0 to 0.5 × 10 -3 , and particularly preferably 0.0 to 0.1 × 10 -3When the in-plane birefringence Re / d of the optical film is within the above-mentioned preferred range, the optical film can be used as a positive C plate. In addition, when the optical film is used as a material for a stretched film, the optical properties of the stretched film obtained after stretching can be easily controlled.

[0045] As described above, the optical film according to one embodiment of the present invention has a small birefringence Rth / d in the thickness direction, and therefore can have a small NZ coefficient. More specifically, the optical film has a negative NZ coefficient, and the absolute value of the NZ coefficient can be increased. The specific range of the NZ coefficient of the optical film is not particularly limited, but is preferably -500 or more, more preferably -400 or more, particularly preferably -300 or more, and is preferably -30 or less, more preferably -40 or less, particularly preferably -50 or less.

[0046] The NZ coefficient of a film can be calculated from the in-plane retardation Re and the retardation in the thickness direction Rth of the film.

[0047] The optical film according to one embodiment of the present invention preferably has high transparency. The specific total light transmittance of the optical film is preferably 80% or more, more preferably 85% or more, and particularly preferably 88% or more. The total light transmittance of the film can be measured in the wavelength range of 400 nm to 700 nm using an ultraviolet-visible spectrometer.

[0048] The optical film according to one embodiment of the present invention preferably has a small haze. The haze of the optical film is preferably less than 1.0%, more preferably less than 0.8%, particularly preferably less than 0.5%, and ideally 0.0%. When an optical film having such a small haze is provided in a display device, the clarity of the image displayed on the display device can be increased. The haze of the film can be measured using a haze meter (for example, "NDH5000" manufactured by Nippon Denshoku Industries Co., Ltd.).

[0049] The optical film according to one embodiment of the present invention may contain a solvent. This solvent may be incorporated into the film in the step of contacting the resin film with the solvent in the manufacturing method of the optical film described below. In detail, all or a part of the solvent incorporated into the film by contacting the resin film may penetrate into the inside of the polymer. Therefore, even if drying is performed at or above the boiling point of the solvent, it is difficult to completely remove the solvent. Therefore, the optical film may contain a solvent.

[0050] The optical film according to one embodiment of the present invention may have a multi-layer structure including a plurality of layers, but preferably has a single-layer structure. The single-layer structure refers to a structure having only a single layer having the same composition, and not having a layer having a different composition from the above composition. Therefore, it is preferable that the optical film has only a layer formed of the above crystalline resin.

[0051] The optical film according to one embodiment of the present invention may be a sheet film or a long film having a long shape. When the optical film has a long shape, it is possible to continuously manufacture a polarizing plate by bonding the optical film and a long polarizing film.

[0052] The thickness of the optical film according to one embodiment of the present invention can be appropriately set depending on the application of the optical film, but it is usually desirable to have a thin thickness. The specific thickness of the optical film is preferably 3 μm or more, more preferably 5 μm or more, particularly preferably 7 μm or more, and is preferably 100 μm or less, more preferably 20 μm or less, particularly preferably 10 μm or less.

[0053] [5. Manufacturing method of optical film] The optical film according to one embodiment of the present invention is (i) preparing a resin film formed of a crystalline resin containing a crystalline polymer having positive intrinsic birefringence; (ii) contacting the resin film with a solvent to change the birefringence in the thickness direction; It can be produced by a production method including the steps of:

[0054] The present inventors speculate that the mechanism by which an optical film is obtained by the above-mentioned manufacturing method is as follows, although the technical scope of the present invention is not limited to the mechanism described below.

[0055] When a resin film formed of a crystalline resin containing a crystalline polymer is brought into contact with a solvent, the solvent penetrates into the resin film. The action of the penetrating solvent causes micro-Brownian motion in the molecules of the crystalline polymer in the film, and the molecular chains are oriented. According to the study by the present inventors, it is believed that the solvent-induced crystallization phenomenon of the crystalline polymer may progress during this orientation of the molecular chains.

[0056] The surface area of ​​the resin film is large on the front surface and the back surface, which are the main surfaces. Therefore, the penetration speed of the solvent is high in the thickness direction through the front surface or the back surface. Then, the orientation of the molecules of the crystalline polymer can proceed so that the molecules of the polymer are oriented in the thickness direction. And, by orienting the molecules of the crystalline polymer in the thickness direction in this way, the birefringence in the thickness direction changes, and a small birefringence in the thickness direction can be obtained.

[0057] The above-mentioned method for producing an optical film may further include any step in combination with the steps (i) and (ii). For example, the method for producing an optical film preferably includes a step (iii) of drying the resin film after the step (ii).

[0058] [6. Step (i) of preparing a resin film] A method for producing an optical film according to an embodiment of the present invention includes a step (i) of preparing a resin film made of a crystalline resin containing a crystalline polymer having positive intrinsic birefringence. The crystalline resin as a material of the resin film prepared in the step (i) may be the same as the crystalline resin contained in the optical film.

[0059] However, the crystallinity of the crystalline polymer contained in the resin film is preferably small. The specific crystallinity is preferably less than 10%, more preferably less than 5%, and particularly preferably less than 3%. If the crystallinity of the crystalline polymer contained in the resin film before contact with the solvent is low, many molecules of the crystalline polymer can be oriented in the thickness direction by contact with the solvent, so that the birefringence Rth / d in the thickness direction of the optical film can be adjusted in a wide range.

[0060] The resin film preferably has optical isotropy. Therefore, the resin film preferably has a small birefringence Re / d in the in-plane direction, and preferably has a small absolute value |Rth / d| of birefringence in the thickness direction. Specifically, the birefringence Re / d in the in-plane direction of the resin film is preferably 1.0×10 -3 less than 0.5×10 -3 less than 0.2×10 -3 The absolute value of birefringence in the thickness direction of the resin film |Rth / d| is preferably less than 1.0×10 -3 less than 0.5×10 -3 less than 0.2×10 -3 The optical isotropy indicates that the orientation of the crystalline polymer molecules contained in the resin film is low and substantially non-oriented. When such an optically isotropic resin film is used, precise control of the optical properties of the resin film is not required, and therefore precise control of the orientation of the crystalline polymer molecules is not required, so that the manufacturing method of the optical film can be simplified. Furthermore, when an optically isotropic resin film is used, an optical film with small haze can usually be obtained.

[0061] The resin film preferably has a small solvent content, and more preferably does not contain a solvent. The ratio of the solvent contained in the resin film to 100% by weight of the resin film (solvent content) is preferably 1% or less, more preferably 0.5% or less, particularly preferably 0.1% or less, and ideally 0.0%. Since the amount of solvent contained in the resin film before contact with the solvent is small, many crystalline polymer molecules can be oriented in the thickness direction by contact with the solvent, so that the birefringence Rth / d in the thickness direction of the optical film can be adjusted in a wide range. The solvent content of the resin film can be measured by its density.

[0062] The haze of the resin film is preferably less than 1.0%, preferably less than 0.8%, more preferably less than 0.5%, and ideally 0.0%. The smaller the haze of the resin film, the easier it is to reduce the haze of the resulting optical film.

[0063] The thickness of the resin film is preferably set according to the thickness of the optical film to be produced and the thickness of the stretched film produced by stretching the optical film. Usually, the thickness is increased by contacting with a solvent in step (ii). In addition, when the optical film is stretched to produce a stretched film, the thickness is decreased by the stretching. Therefore, the thickness of the resin film may be set in consideration of the change in thickness in the steps after step (ii) as described above.

[0064] The resin film may be a sheet-like film, but is preferably a long film. By using a long resin film, the optical film can be continuously produced by a roll-to-roll method, and the productivity of the optical film can be effectively improved.

[0065] As a method for producing the resin film, a resin molding method such as an injection molding method, an extrusion molding method, a press molding method, an inflation molding method, a blow molding method, a calendar molding method, a cast molding method, a compression molding method, etc. is preferable because a resin film containing no solvent can be obtained. Among these, an extrusion molding method including melt extrusion of a crystalline resin is preferable because the thickness can be easily controlled.

[0066] The manufacturing conditions in the extrusion molding method are preferably as follows. The cylinder temperature (molten resin temperature) is preferably Tm or higher, more preferably "Tm+20°C" or higher, and preferably "Tm+100°C" or lower, more preferably "Tm+50°C" or lower. The cooling body that the molten resin extruded into a film first comes into contact with is not particularly limited, but a cast roll is usually used. The cast roll temperature is preferably "Tg-50°C" or higher, preferably "Tg+70°C" or lower, more preferably "Tg+40°C" or lower. When a resin film is manufactured under such conditions, a resin film having a thickness of 1 μm to 1 mm can be easily manufactured. Here, "Tm" represents the melting point of the crystalline polymer, and "Tg" represents the glass transition temperature of the crystalline polymer.

[0067] [7. Step (ii) of contacting the resin film with a solvent] The method for producing an optical film according to one embodiment of the present invention includes, after step (i), step (ii) of contacting a resin film with a solvent. This step (ii) changes the birefringence of the resin film in the thickness direction, so that an optical film can be obtained as a resin film having a birefringence in the thickness direction different from that before contact with the solvent.

[0068] As the solvent, an organic solvent is usually used. Specific types of the solvent include those that can penetrate into the resin film without dissolving the crystalline polymer contained in the resin film, such as hydrocarbon solvents such as cyclohexane, toluene, limonene, and decalin; and carbon disulfide. The type of the solvent may be one type or two or more types.

[0069] The method of contacting the resin film with the solvent is not limited. Examples of the contact method include a spray method in which the resin film is sprayed with the solvent, a coating method in which the resin film is coated with the solvent, and a dipping method in which the resin film is dipped in the solvent. Among these, the dipping method is preferred because it is easy to perform continuous contact.

[0070] The temperature of the solvent brought into contact with the resin film may be any temperature within a range in which the solvent can maintain a liquid state, and therefore may be set within a range from the melting point to the boiling point of the solvent.

[0071] The contact time between the resin film and the solvent can be appropriately set within a range in which an optical film having desired optical properties can be obtained. The specific contact time is preferably 0.5 seconds or more, more preferably 1.0 seconds or more, particularly preferably 5.0 seconds or more, and preferably 24 hours or less, more preferably 12 hours or less, particularly preferably 2 hours or less. When the contact time is equal to or greater than the lower limit of the range, the birefringence in the thickness direction can be effectively changed by contact with the solvent. On the other hand, even if the immersion time is extended, the amount of change in birefringence tends not to change significantly. Therefore, when the contact time is equal to or less than the upper limit of the range, the productivity can be increased without impairing the quality of the optical film.

[0072] The refractive index of the resin film changes when it is brought into contact with a solvent. This change in refractive index usually appears as a change in birefringence Rth / d in the thickness direction. The change in birefringence Rth / d in the thickness direction caused by contact with a solvent is preferably 1.0×10 -3 More preferably, 3.0×10 -3 More preferably, 5.0×10 -3 or more, preferably 50.0×10 -3 Less than or equal to 30.0×10 -3 The following is particularly preferably 20.0×10 -3The change in the birefringence Rth / d in the thickness direction represents the absolute value of the change in the birefringence Rth / d in the thickness direction. A specific change in the birefringence Rth / d in the thickness direction is calculated by subtracting the birefringence Rth / d in the thickness direction of the resin film before contact with the solvent from the birefringence Rth / d in the thickness direction of the resin film after contact with the solvent, and then calculating the absolute value. Usually, the birefringence Rth / d in the thickness direction is reduced (i.e., changes in the negative direction) by contacting the resin film with the solvent.

[0073] The in-plane birefringence Re / d of the resin film may or may not change upon contact with a solvent. For example, when the optical film is used as a material for a stretched film, from the viewpoint of simplifying the control of the optical properties of the stretched film obtained after stretching, it is preferable that the change in the in-plane birefringence Re / d of the resin film caused by contact with a solvent is small, and it is more preferable that no change occurs. The amount of change in the in-plane birefringence Re / d of the resin film caused by contact with a solvent is preferably 0.0×10 -3 ~1.0×10 -3 , more preferably 0.0×10 -3 ~0.5×10 -3 , particularly preferably 0.0×10 -3 ~0.3×10 -3 The change in the in-plane birefringence Re / d refers to the absolute value of the change in the in-plane birefringence Re / d. A specific change in the in-plane birefringence Re / d is calculated as the absolute value by subtracting the in-plane birefringence Re / d of the resin film before contact with the solvent from the in-plane birefringence Re / d of the resin film after contact with the solvent.

[0074] In step (ii), the thickness of the resin film is usually increased by the penetration of the solvent contacted with the resin film into the resin film. The lower limit of the change rate of the thickness of the resin film at this time may be, for example, 1% or more, 10% or more, or 15% or more. The upper limit of the change rate of the thickness may be, for example, 80% or less, 50% or less, or 40% or less. The change rate of the thickness of the resin film is a ratio obtained by dividing the difference in thickness between the resin film before contact with the solvent and the resin film after contact with the solvent by the thickness of the resin film before contact with the solvent.

[0075] As described above, the birefringence Rth / d in the thickness direction of the resin film is changed by the step (ii). When a resin film having desired optical properties can be obtained by such a change in the birefringence Rth / d in the thickness direction, the resin film can be obtained as an optical film. In the method for producing an optical film according to this embodiment, the resin film after step (ii) may be subjected to an arbitrary step.

[0076] [8. Step (iii) of drying the resin film] The method for producing an optical film according to an embodiment of the present invention may include a step (iii) of drying the resin film after the step (ii). By drying, the amount of the solvent contained in the resin film can be reduced.

[0077] The drying of the resin film in step (iii) is preferably carried out so that the refractive index in the thickness direction of the resin film is changed by the drying. According to the study by the present inventor, it has been found that the birefringence Rth / d in the thickness direction of the resin film can be changed when the drying is carried out in a reduced pressure environment lower than normal pressure (1 atm). Therefore, the drying in step (iii) is preferably carried out in a reduced pressure environment.

[0078] The pressure condition in the reduced pressure environment is preferably 10,000 Pa or less, more preferably 5,000 Pa or less, and particularly preferably 1,000 Pa or less. There is no particular lower limit, and the pressure may be 0 Pa, but it is usually 100 Pa or more.

[0079] The present inventors speculate that the mechanism by which the birefringence in the thickness direction of the resin film can be changed by drying in a reduced pressure environment is as follows. By drying in a reduced pressure environment, the orientation of the molecules of the crystalline polymer contained in the resin film in the film thickness direction can be further promoted as the solvent contained in the resin film is sent out to the outside of the film. It is considered that the birefringence in the thickness direction of the resin film changes as the orientation of the molecules of the crystalline polymer having a positive intrinsic birefringence in the film thickness direction progresses. In addition, the above drying may cause the crystallization of the crystalline polymer to progress. However, the technical scope of the present invention is not limited by the above mechanism.

[0080] The drying temperature in step (iii) is not particularly limited. From the viewpoint of increasing the change in birefringence Rth / d in the thickness direction of the resin film, it is preferable to perform drying at a high temperature. Specifically, the drying temperature is preferably Tg or higher, more preferably Tg+10°C or higher, particularly preferably Tg+20°C or higher, and preferably Tg+130°C or lower, more preferably Tg+100°C or lower, particularly preferably Tg+80°C or lower. Here, "Tg" represents the glass transition temperature of the crystalline polymer.

[0081] The drying time in step (iii) is not particularly limited. From the viewpoint of increasing the degree of removal of the solvent by drying and the degree of change in birefringence in the thickness direction by drying, the drying time is preferably 10 minutes or more, more preferably 2 hours or more, particularly preferably 4 hours or more, and is preferably 24 hours or less, more preferably 12 hours or less, particularly preferably 6 hours or less.

[0082] The change in birefringence Rth / d in the thickness direction of the resin film that can occur due to drying is preferably 1.0×10 -3 More preferably, 3.0×10 -3 More preferably, 5.0×10 -3 or more, preferably 50.0×10 -3 Less than or equal to 30.0×10-3 The following is particularly preferably 20.0×10 -3 The change in the birefringence Rth / d in the thickness direction represents the absolute value of the change in the birefringence Rth / d in the thickness direction. A specific change in the birefringence Rth / d in the thickness direction is calculated by subtracting the birefringence Rth / d in the thickness direction of the resin film before drying from the birefringence Rth / d in the thickness direction of the resin film after drying, and then calculating the absolute value. Usually, the birefringence Rth / d in the thickness direction is reduced by drying (i.e., changes in the negative direction).

[0083] The birefringence Re / d in the in-plane direction of the resin film may or may not change due to drying. For example, when the optical film is used as a material for a stretched film, from the viewpoint of simplifying the control of the optical properties of the stretched film obtained after stretching, it is preferable that the change in the birefringence Re / d in the in-plane direction of the resin film caused by drying is small, and it is more preferable that no change occurs. The change in the birefringence Re / d in the in-plane direction of the resin film caused by drying is preferably 0.0×10 -3 ~1.0×10 -3 , more preferably 0.0×10 -3 ~0.5×10 -3 , particularly preferably 0.0×10 -3 ~0.3×10 -3 The change in the in-plane birefringence Re / d refers to the absolute value of the change in the in-plane birefringence Re / d. A specific change in the in-plane birefringence Re / d is calculated as the absolute value by subtracting the in-plane birefringence Re / d of the resin film before drying from the in-plane birefringence Re / d of the resin film after drying.

[0084] When a resin film having desired optical properties is obtained after drying in step (iii), the resin film can be used as an optical film.

[0085] [9. Optional process] The method for producing an optical film according to one embodiment of the present invention may further include any step in combination with the steps described above, such as a step of subjecting the resin film to a heat treatment to promote crystallization of the crystalline polymer, a step of thermally shrinking the resin film to remove residual stress in the film, etc.

[0086] According to the above-mentioned manufacturing method, a long optical film can be manufactured using a long resin film. The manufacturing method of the optical film may include a step of winding the long optical film thus manufactured into a roll. Furthermore, the manufacturing method of the optical film may include a step of cutting the long optical film into a desired shape.

[0087] [10. Method for producing stretched film] A method for producing a stretched film according to an embodiment of the present invention includes stretching the above-mentioned optical film. By stretching, the molecules of the crystalline polymer contained in the optical film can be oriented in a direction according to the stretching direction. Therefore, by this stretching, the optical properties of the optical film can be adjusted, and a stretched film having desired optical properties can be obtained as the stretched optical film.

[0088] When an optical film is stretched, the orientation direction of the molecules of the crystalline polymer contained in the optical film usually changes to approach the in-plane direction perpendicular to the thickness direction. Since the crystalline polymer has a positive intrinsic birefringence, the refractive index nz in the thickness direction of the optical film can be reduced by the change in the orientation direction of the crystalline polymer due to stretching. Therefore, the stretching can obtain a stretched film having a larger NZ coefficient than the optical film, and for example, a three-dimensional retardation film having an NZ coefficient larger than 0.0 and smaller than 1.0 can be manufactured as a stretched film. In general, it has been difficult to manufacture a thin three-dimensional retardation film. In contrast, in the manufacturing method according to this embodiment, an optical film that can have a thin thickness can be further thinned by stretching to manufacture a three-dimensional retardation film, so that it is possible to provide a three-dimensional retardation film that is thinner than conventional ones. However, the stretched film manufactured by the manufacturing method according to this embodiment is not limited to a three-dimensional retardation film.

[0089] There is no limitation on the stretching direction of the optical film, and examples thereof include the longitudinal direction, the width direction, and the oblique direction. Here, the oblique direction refers to a direction perpendicular to the thickness direction, and is neither parallel nor perpendicular to the width direction. The stretching direction may be one direction or two or more directions. Thus, examples of the stretching method include uniaxial stretching methods such as a method of uniaxially stretching a resin film in the longitudinal direction (longitudinal uniaxial stretching method) and a method of uniaxially stretching a resin film in the width direction (transverse uniaxial stretching method); biaxial stretching methods such as a simultaneous biaxial stretching method in which a resin film is stretched in the longitudinal direction and simultaneously stretched in the width direction, and a sequential biaxial stretching method in which a resin film is stretched in one of the longitudinal direction and the width direction and then stretched in the other direction; and a method of stretching a resin film in an oblique direction (oblique stretching method). Among them, the uniaxial stretching method in which stretching is performed only in one direction is preferred, and from the viewpoint of obtaining a particularly thin stretched film, free uniaxial stretching in which no restraining force is applied in a direction other than the stretching direction is more preferred.

[0090] The stretching ratio is preferably 1.1 times or more, more preferably 1.2 times or more, and preferably 20.0 times or less, more preferably 10.0 times or less, even more preferably 5.0 times or less, and particularly preferably 2.0 times or less. It is desirable to appropriately set the specific stretching ratio according to factors such as the optical properties, thickness, and mechanical strength of the stretched film to be produced. When the stretching ratio is equal to or greater than the lower limit of the above range, the birefringence of the film can be significantly changed by stretching. When the stretching ratio is equal to or less than the upper limit of the above range, the direction of the slow axis can be easily controlled and the breakage of the film can be effectively suppressed.

[0091] The stretching temperature is preferably "Tg+5°C" or higher, more preferably "Tg+10°C" or higher, and preferably "Tg+100°C" or lower, more preferably "Tg+90°C" or lower. Here, "Tg" represents the glass transition temperature of the crystalline polymer. When the stretching temperature is equal to or higher than the lower limit of the above range, the optical film can be sufficiently softened to perform uniform stretching. When the stretching temperature is equal to or lower than the upper limit of the above range, the hardening of the resin film due to the progress of crystallization of the crystalline polymer can be suppressed, so that the stretching can be performed smoothly, and large birefringence can be expressed by stretching. Furthermore, the haze of the obtained stretched film can usually be reduced to increase transparency.

[0092] The method for producing a stretched film according to one embodiment of the present invention may further include an optional step in combination with the step of stretching the optical film. Examples of the optional step include the same steps as those described in the method for producing an optical film.

[0093] The stretched film produced by the production method according to the present embodiment preferably has an NZ coefficient in an appropriate range according to its application. In particular, from the viewpoint of achieving an NZ coefficient that has been difficult to achieve in a film using a crystalline polymer having positive intrinsic birefringence and utilizing the advantages according to the present embodiment, the NZ coefficient of the stretched film is preferably 0.0 or more, more preferably greater than 0.0, even more preferably greater than 0.1, particularly preferably greater than 0.2, and also preferably less than 1.0, more preferably less than 0.9, and even more preferably less than 0.8.

[0094] The stretched film produced by the production method according to the present embodiment preferably has a birefringence Rth / d in the thickness direction within an appropriate range according to its application. Usually, the birefringence Rth / d in the thickness direction increases (i.e., changes in the positive direction) due to stretching. Therefore, the birefringence Rth / d in the thickness direction of the stretched film can be larger than the birefringence Rth / d in the thickness direction of the optical film. The specific birefringence Rth / d in the thickness direction of the stretched film is preferably −20×10 -3 More preferably, -15×10 -3 More preferably, -10×10 -3 or more, preferably 20×10 -3 Less than or equal to 15×10 -3 Below, particularly preferably 10 × 10 -3 The following is the result.

[0095] The stretched film produced by the production method according to this embodiment preferably has a thickness direction retardation Rth in an appropriate range according to its application. Usually, the thickness direction retardation Rth increases (i.e., changes in the positive direction) by stretching. Therefore, the thickness direction retardation Rth of the stretched film can be larger than the thickness direction retardation Rth of the optical film. The specific thickness direction retardation Rth of the stretched film is preferably -500 nm or more, more preferably -300 nm or more, particularly preferably -100 nm or more, and is preferably 200 nm or less, more preferably 100 nm or less, particularly preferably 10 nm or less.

[0096] The stretched film produced by the above-mentioned production method preferably has an in-plane retardation in an appropriate range depending on its application. For example, the specific in-plane retardation Re of the stretched film can be preferably 100 nm or more, more preferably 110 nm or more, particularly preferably 120 nm or more, and preferably 180 nm or less, more preferably 170 nm or less, particularly preferably 160 nm or less. In this case, the stretched film can function as a quarter-wave plate.

[0097] For example, the specific in-plane retardation Re of the stretched film may be preferably 245 nm or more, more preferably 265 nm or more, particularly preferably 270 nm or more, and may be preferably 320 nm or less, more preferably 300 nm or less, particularly preferably 295 nm or less. In this case, the optical film can function as a 1 / 2 wavelength plate.

[0098] The stretched film preferably has high transparency, for example, a total light transmittance in the same range as that of the optical film. The stretched film preferably has a small haze, for example, a haze in the same range as that of the optical film. Furthermore, the stretched film may contain a solvent, as in the optical film.

[0099] The stretched film may have a multi-layer structure, but preferably has a single-layer structure. The stretched film may be a sheet film or a long film having a long shape.

[0100] The thickness of the stretched film produced by the production method according to this embodiment is not particularly limited, but is preferably thin from the viewpoint of utilizing the advantages of the above-mentioned production method. Specifically, the thickness of the stretched film is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 8 μm or less, and particularly preferably 6 μm or less. There is no lower limit, and it can be, for example, 1 μm or more, 2 μm or more, or 3 μm or more. In particular, it is particularly difficult to achieve such a thin thickness while having an NZ coefficient in the above-mentioned range with a conventional film containing a crystalline polymer having a positive intrinsic birefringence, and its industrial value is high.

[0101] [11. Applications of optical films and stretched films] There is no limitation on the use of the optical film and stretched film described above. These films can be used alone or in combination with other members for a wide range of applications in the optical field. Examples of the use of the optical film and stretched film include a base film for forming an arbitrary layer on the base film; a polarizing plate protective film; a viewing angle compensation film for a liquid crystal display device, and a retardation film such as a quarter-wave plate provided on a circular polarizing plate; etc. EXAMPLES

[0102] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto. In the following description, the units "%" and "parts" are by weight unless otherwise specified. Furthermore, the operations described below were carried out in air at room temperature and normal pressure (23°C and 1 atm) unless otherwise specified.

[0103] [Evaluation method] (Method of measuring weight average molecular weight Mw and number average molecular weight Mn of polymer) The weight average molecular weight Mw and number average molecular weight Mn of the polymer were measured as polystyrene equivalent values ​​using a gel permeation chromatography (GPC) system (Tosoh Corporation, "HLC-8320"). In the measurement, an H-type column (Tosoh Corporation) was used as the column, and tetrahydrofuran was used as the solvent. The temperature during the measurement was 40°C.

[0104] (Method for measuring hydrogenation rate of polymer) The hydrogenation rate of the polymer was measured using orthodichlorobenzene-d4 as a solvent at 145°C. 1 Measured by H-NMR measurement.

[0105] (Method of measuring glass transition temperature Tg and melting point Tm) The glass transition temperature Tg and melting point Tm of the polymer were measured as follows. First, the polymer was melted by heating, and the melted polymer was quenched with dry ice. Then, the glass transition temperature Tg and melting point Tm of the polymer were measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min (heating mode) using the polymer as a test specimen.

[0106] (Method for measuring the ratio of racemo-dyads in polymers) The ratio of racemo-dyads in the polymer was measured as follows. The ratio of the racemo-dyads in the polymer was measured by applying the inverse-gated decoupling method at 200°C using orthodichlorobenzene-D4 as a solvent. 13 C-NMR measurements were performed. 13 In the C-NMR measurement, a signal at 43.35 ppm from the meso dyad and a signal at 43.43 ppm from the racemo dyad were identified, with the peak at 127.5 ppm from orthodichlorobenzene-d4 as the reference shift. The ratio of the racemo dyads in the polymer was calculated based on the intensity ratio of these signals.

[0107] (Method of measuring film retardation and NZ coefficient) The in-plane retardation Re, thickness direction retardation Rth, and NZ coefficient of the film were measured using a retardation meter ("AxoScanOPMF-1" manufactured by AXOMETRICS) at a wavelength of 590 nm.

[0108] (Method for measuring the crystallinity of crystalline polymers) The crystallinity of the crystalline polymer contained in the film was confirmed by X-ray diffraction in accordance with JIS K 0131. Specifically, the diffracted X-ray intensity from the crystallized portion was determined using a wide-angle X-ray diffractometer (Rigaku Corporation, "RINT2000"), and the crystallinity was calculated from the ratio to the total diffracted X-ray intensity according to the following formula (I). Xc = K·Ic / It(I) In the above formula (I), Xc represents the crystallinity of the test sample, Ic represents the diffracted X-ray intensity from the crystallized portion, It represents the total diffracted X-ray intensity, and K represents a correction term.

[0109] [Production Example 1. Production of crystalline resin] A metallic pressure-resistant reactor was thoroughly dried and then purged with nitrogen. 154.5 parts of cyclohexane, 42.8 parts of a 70% cyclohexane solution of dicyclopentadiene (endo isomer content of 99% or more) (30 parts as dicyclopentadiene), and 1.9 parts of 1-hexene were added to the metallic pressure-resistant reactor and heated to 53°C.

[0110] 0.014 parts of tetrachlorotungsten phenylimide (tetrahydrofuran) complex was dissolved in 0.70 parts of toluene to prepare a solution. 0.061 parts of a 19% diethylaluminum ethoxide / n-hexane solution was added to this solution and stirred for 10 minutes to prepare a catalyst solution. This catalyst solution was added to a pressure-resistant reactor to start a ring-opening polymerization reaction. The reaction was then continued for 4 hours while maintaining the temperature at 53°C to obtain a solution of a ring-opened polymer of dicyclopentadiene. The number-average molecular weight (Mn) and weight-average molecular weight (Mw) of the obtained ring-opened polymer of dicyclopentadiene were 8,750 and 28,100, respectively, and the molecular weight distribution (Mw / Mn) calculated from these was 3.21.

[0111] To 200 parts of the obtained solution of the ring-opened polymer of dicyclopentadiene, 0.037 parts of 1,2-ethanediol was added as a terminator, and the mixture was heated to 60°C and stirred for 1 hour to terminate the polymerization reaction. One part of a hydrotalcite-like compound (Kyowa Chemical Industry Co., Ltd.'s "Kyoward (registered trademark) 2000") was added thereto, and the mixture was heated to 60°C and stirred for 1 hour. Thereafter, 0.4 parts of a filter aid (Showa Chemical Industry Co., Ltd.'s "Radiolight (registered trademark) #1500") was added, and the mixture was filtered using a PP pleated cartridge filter (Advantec Toyo Co., Ltd.'s "TCP-HX"). The adsorbent and the solution were separated by filtration.

[0112] 100 parts of cyclohexane was added to 200 parts of the filtered ring-opening polymer solution (polymer amount 30 parts), and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium was added, and hydrogenation reaction was carried out at 180°C and hydrogen pressure of 6 MPa for 4 hours. As a result, a reaction liquid containing a hydrogenated product of the ring-opening polymer of dicyclopentadiene was obtained. The reaction liquid was a slurry solution in which the hydrogenated product was precipitated.

[0113] The hydrogenated product and the solution contained in the reaction solution were separated using a centrifuge and dried under reduced pressure at 60°C for 24 hours to obtain 28.5 parts of a hydrogenated ring-opening polymer of dicyclopentadiene as a crystalline polymer having positive intrinsic birefringence. The hydrogenation rate of this hydrogenated product was 99% or more, the glass transition temperature (Tg) was 93°C, the melting point (Tm) was 262°C, and the ratio of racemo-dyads was 89%.

[0114] 100 parts of the obtained hydrogenated ring-opening polymer of dicyclopentadiene was mixed with 1.1 parts of an antioxidant (tetrakis [methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl) propionate] methane; "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd.), and then the mixture was put into a twin-screw extruder (product name "TEM-37B", manufactured by Toshiba Machine Co., Ltd.) equipped with four die holes having an inner diameter of 3 mm. The mixture of the hydrogenated ring-opening polymer of dicyclopentadiene and the antioxidant was molded into a strand shape by hot melt extrusion molding, and then chopped with a strand cutter to obtain pellets of a crystalline resin. The operating conditions of the twin-screw extruder were as follows. Barrel temperature setting: 270~280℃ Die temperature setting = 250℃ Screw speed: 145 rpm

[0115] [Example 1] (1-1. Extrusion film formation) The crystalline resin pellets produced in Production Example 1 were melt-extruded using a hot melt extrusion film molding machine equipped with a T-die (Optical Control Systems' "Measuring Extruder Type Me-20 / 2800V3") and wound on a roll at a speed of 1.5 m / min to obtain a long resin film with a width of approximately 120 mm. The operating conditions of the film molding machine are itemized below. Barrel temperature setting: 280℃~300℃ Die temperature = 300℃ Screw speed = 30 rpm Cast roll temperature = 80℃

[0116] The thickness of the obtained resin film was 50 μm. When the retardation of the resin film was measured at a wavelength of 590 nm, the in-plane retardation Re was 4 nm and the retardation in the thickness direction Rth was 8 nm.

[0117] (1-2. Solvent Contact) The resin film was cut into a rectangle of 120 mm x 120 mm. The rectangular resin film was immersed in cyclohexane as a solvent stored in a tray for 1 hour to obtain an optical film. The optical film was removed from the solvent, and the solvent on the film surface was wiped off with a Kimtowel. The retardation of this optical film was measured, and the in-plane retardation Re was 2 nm, and the retardation in the thickness direction Rth was -762 nm. The thickness of the optical film was 61 μm.

[0118] [Example 2] An optical film was produced in the same manner as in Example 1. The optical film was placed in a vacuum dryer heated to 100°C and dried for 3 hours. The pressure in the vacuum dryer was set to 100 Pa to 500 Pa. The pressure in the vacuum dryer was the same in the following examples unless otherwise specified. The optical film was taken out of the vacuum oven, and the retardation of the optical film was measured. The in-plane retardation of the dried optical film was Re=3 nm, and the retardation in the thickness direction was Rth=-1026 nm. The thickness of the dried optical film was 63 μm.

[0119] [Example 3] An optical film was produced in the same manner as in Example 1. The optical film was placed in a vacuum dryer heated to 170°C and dried for 5 hours. The optical film was removed from the vacuum oven and the retardation of the optical film was measured. The in-plane retardation of the dried optical film was Re=5 nm, and the retardation in the thickness direction was Rth=-1347 nm. The thickness of the dried optical film was 64 μm.

[0120] [Example 4] Except for changing the line speed in step (1-1) to change the thickness of the long resin film to 6 μm, an optical film was produced in the same manner as in Example 1. This optical film was placed in a vacuum dryer heated to 170° C. and dried for 5 hours.

[0121] A batch-type biaxial stretching device (manufactured by Etoh Co., Ltd.) was prepared. This stretching device was equipped with an oven unit and a clip for stretching capable of fixing a film. By using this stretching device, it is possible to stretch the film by pulling the film with the clip in the oven.

[0122] The dried optical film was cut into a rectangle of 100 mm x 100 mm. Both ends of this rectangular optical film were held by five clips of the stretching device. The optical film was pulled by the clips and freely uniaxially stretched in the longitudinal direction of the long resin film obtained in the extrusion film formation process. The stretching temperature was 130°C and the stretching ratio was 1.1 times. A stretched film was obtained as the stretched optical film by this free uniaxial stretching. The retardation of the stretched film was measured, and the in-plane retardation Re was 144 nm and the retardation in the thickness direction Rth was -72 nm.

[0123] [Example 5] Except for changing the line speed in step (1-1) to change the thickness of the long resin film to 6 μm, an optical film was produced in the same manner as in Example 1. This optical film was placed in a vacuum dryer heated to 170° C. and dried for 5 hours.

[0124] The dried optical film was cut into a rectangle of 100 mm x 100 mm. Both ends of this rectangular optical film were held by five clips of the batch-type biaxial stretching device (manufactured by Etoh Corporation). The optical film was pulled by the clips and freely uniaxially stretched in the longitudinal direction of the long resin film obtained in the extrusion film formation process. The stretching temperature was 130°C and the stretching ratio was 1.2 times. A stretched film was obtained as the optical film after stretching by this free uniaxial stretching. The retardation of the stretched film was measured, and the in-plane retardation Re was 282 nm and the retardation in the thickness direction Rth was 3 nm.

[0125] [Example 6] An optical film was produced in the same manner as in Example 1, except that the type of solvent in step (1-2) was changed to toluene, and the immersion time of the resin film in the solvent was changed to 5 seconds. The optical film was placed in a vacuum dryer heated to 170°C and dried for 5 hours. The optical film was removed from the vacuum oven, and the retardation of the optical film was measured. The in-plane retardation of the dried optical film was Re=7 nm, and the retardation in the thickness direction was Rth=-986 nm. The thickness of the dried optical film was 66 μm.

[0126] In this Example 6, a long resin film was produced by melt extrusion under the same conditions as in Examples 1 to 3. The retardation and NZ coefficient of the resin film obtained in Example 6 were different from those in Examples 1 to 3. However, the degree of this difference was sufficiently small and within the range of normal error.

[0127] [Comparative Example 1] The line speed in step (1-1) was changed to a thickness of 20 μm for the long resin film. In addition, the type of solvent in step (1-2) was changed to toluene, and the immersion time of the resin film in the solvent was changed to 1 second. Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.

[0128] [Comparative Example 2] An optical film was produced and evaluated in the same manner as in Example 1, except that the type of solvent in step (1-2) was changed to toluene and the immersion time of the resin film in the solvent was changed to 5 seconds.

[0129] [Comparative Example 3] The line speed in step (1-1) was changed to change the thickness of the long resin film to 39 μm. In addition, the immersion time of the resin film in the solvent in step (1-2) was changed to 1 minute. Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.

[0130] [result] The results of the above-mentioned Examples and Comparative Examples are shown in the following table. In the table, the meanings of the abbreviations are as follows. Cy: Cyclohexane. Tl: toluene.

[0131] [Table 1]

[0132] [Consider] In Examples 1 to 6, −11.5 × 10 -3 The optical film having the following birefringence Rth / d in the thickness direction was obtained. Therefore, it was confirmed that the present invention can provide an optical film having a small birefringence Rth / d in the thickness direction by using a crystalline polymer having a positive intrinsic birefringence. In addition, it was confirmed that in Examples 2 to 6, the birefringence Rth / d in the thickness direction can be further reduced by drying.

Claims

1. An optical film formed of a resin containing a crystalline polymer having positive intrinsic birefringence, The birefringence Rth / d in the thickness direction of the optical film is −14.0×10 -3 The following is an optical film.

2. The optical film according to claim 1 , wherein the crystalline polymer contains an alicyclic structure.

3. 3. The optical film according to claim 1, wherein the crystallinity of the crystalline polymer measured by X-ray diffraction is 10% or more.

4. The optical film according to any one of claims 1 to 3, wherein the in-plane retardation Re of the optical film is 10 nm or less.

Citation Information

Patent Citations

  • Method for producing birefringent film and liquid crystal display device using the same

    JP1993346507A

  • Molded product of cycloolefin polymer and method for producing the same

    JP2009120755A

  • Cellulose n-substituted carbamate-containing drawn film, and polarization plate and liquid crystal display device using the same

    JP2010211058A

  • Method for producing resin film, resin film, and optical film

    JP2016026909A

  • Optical laminate film and method for manufacturing the same, polarizing plate and liquid crystal display device

    JP2017097284A