Laminate and method for manufacturing laminate

A laminate with a urethane resin anchor coat layer and hydrophilic resin barrier layer addresses the challenges of oxygen barrier, adhesion, and lamination strength, offering improved performance and environmental sustainability.

JP2024149953AActive Publication Date: 2024-10-23TOYO INK MFG CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023063147
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23
Estimated Expiration
2043-04-10

Smart Images

  • Figure 2024149953000001
    Figure 2024149953000001
  • Figure 2024149953000002
    Figure 2024149953000002
  • Figure 2024149953000003
    Figure 2024149953000003
Patent Text Reader

Abstract

To provide a laminate excellent in oxygen barrier properties after bending, adhesion, blocking resistance, and laminate strength.SOLUTION: The laminate includes a substrate, an anchor coat layer, and a barrier layer in this order. The anchor coat layer contains a urethane resin (A) having a urea bond, and the urea bond concentration of the urethane resin (A) is 0.1-1.3 mmol / g. The barrier layer contains a hydrophilic resin. The anchor coat layer contains a cured product comprising the urethane resin (A) and an isocyanate-based curing agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate and a method for producing the laminate. [Background technology]

[0002] Conventionally, aluminum foil and aluminum-deposited plastic films and papers have been widely used for materials that require oxygen barrier properties, such as food packaging materials. However, in recent years, due to environmental issues and other factors, there has been a strong demand for packaging materials to be thinner, have simpler lamination methods, and be more recyclable, and so there has been a growing movement away from aluminum.

[0003] In addition, thermoplastic resin films in which a PVDC (polyvinylidene chloride) layer is formed on a plastic film by coating exhibit high oxygen barrier properties not only under low humidity but also under high humidity conditions, and also have high barrier properties against water vapor. However, when this PVDC-coated thermoplastic resin film is incinerated during waste disposal, chlorine gas and dioxins are generated due to the chlorine in the PVDC, which may have a significant adverse effect on the environment and human body, so there is a demand for a shift to other materials.

[0004] As a chlorine-free gas barrier material, a coated film in which polyvinyl alcohol or an ethylene-vinyl alcohol copolymer is coated on a thermoplastic resin film is well known. Patent Document 1 describes a laminate having a structure of a substrate / anchor coat layer / barrier layer, in which the anchor coat layer contains polyester and polyisocyanate, and the barrier layer contains polyvinyl alcohol resin and ethylene-maleic anhydride resin. Patent Document 2 describes a laminate having a structure of a substrate / anchor coat layer / barrier layer, in which the anchor coat layer contains acrylic polyol and polyisocyanate, and the barrier layer contains polyvinyl alcohol resin. Patent Document 3 describes a laminate having a structure of a substrate / anchor coat layer / barrier layer, in which the anchor coat layer contains polyol and polyisocyanate, and the barrier layer contains polyvinyl alcohol resin. Patent Document 4 describes a laminate having a structure of a substrate / anchor coat layer / barrier layer, in which the anchor coat layer contains urethane polyol and an isocyanate compound, and the barrier layer contains silane-modified polyvinyl alcohol resin. However, in all of Patent Documents 1 to 4, the target laminates have problems in any of the properties among oxygen barrier property, substrate adhesion, blocking resistance, and laminate strength depending on the conditions of use, but no technology is disclosed for solving these problems. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-144761 A [Patent Document 2] Patent Publication No. 2021-194822 [Patent Document 3] JP 2020-196791 A [Patent Document 4] JP 2001-129915 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a laminate having excellent oxygen barrier properties, adhesion, blocking resistance and lamination strength after bending. Effect of the Invention

[0007] As a result of extensive research into the above problems, the present inventors have found that the above problems can be solved by using the laminate described below, and have thus completed the present invention.

[0008] That is, the present invention relates to the following [1] to

[11] .

[0009] [1] A laminate having a substrate, an anchor coat layer, and a barrier layer in this order, the anchor coat layer contains a urethane resin (A) having a urea bond, and the urea bond concentration of the urethane resin (A) is 0.1 to 1.3 mmol / g; The laminate, wherein the barrier layer comprises a hydrophilic resin.

[0010] [2] The laminate according to [1], wherein the anchor coat layer comprises a cured product obtained by a reaction between the urethane resin (A) and an isocyanate-based curing agent.

[0011] [3] The laminate according to [2], wherein the isocyanate-based curing agent is an aliphatic isocyanate-based curing agent.

[0012] [4] The laminate according to [3], wherein the aliphatic isocyanate-based curing agent is an adduct type aliphatic isocyanate-based curing agent.

[0013] [5] The laminate according to any one of [1] to [4], wherein the anchor coat layer further contains a vinyl chloride resin and / or a polyvinyl acetal resin.

[0014] [6] The laminate according to any one of [1] to [5], wherein the anchor coat layer further contains an inorganic pigment.

[0015] [7] The laminate according to any one of [1] to [6], wherein the hydrophilic resin is a polyvinyl alcohol-based resin.

[0016] [8] The laminate according to any one of [1] to [7], wherein the barrier layer further contains an inorganic layered filler.

[0017] [9] The laminate according to [8], wherein the inorganic layered filler is at least one selected from the group consisting of montmorillonite, mica, and kaolin.

[0018]

[10] A packaging material comprising any one of the laminates described above in [1] to [9].

[0019]

[11] A method for producing a laminate having a substrate, an anchor coat layer, and a barrier layer in this order, comprising: A step of applying an anchor coating agent onto a substrate to form an anchor coating layer; A step of applying a barrier coating agent onto the anchor coating layer to form a barrier layer, the anchor coating agent contains a urethane resin (A) having a urea bond, and the urea bond concentration of the urethane resin (A) is 0.1 to 1.3 mmol / g; The method for producing a laminate, wherein the barrier coating agent contains a hydrophilic resin.

[0020] According to the present invention, it is possible to provide a laminate having excellent oxygen barrier properties, adhesion, blocking resistance and lamination strength after bending. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The following describes in detail the embodiments of the present invention. However, the embodiments or explanations of the requirements described are merely examples of the embodiments of the present invention, and the present invention is not limited to these contents as long as they do not depart from the gist of the present invention.

[0022] [Laminate] The laminate of the present invention has a substrate, an anchor coat layer, and a barrier layer in this order, the anchor coat layer contains a urethane resin (A) having a predetermined bond concentration of urea bonds, and the barrier layer contains a hydrophilic resin. The laminate is preferably used for packaging materials.

[0023] The laminate of the present invention has an anchor coat layer, which can fill fine irregularities on the surface of the substrate, and by forming a barrier layer on the anchor coat layer, the barrier layer becomes uniform and the occurrence of pinholes can be suppressed. Furthermore, the anchor coat layer contains a urethane resin (A) having a predetermined bond concentration of urea bonds, which improves the cohesive force of the coating film and also improves adhesion to the substrate. Furthermore, the barrier layer contains a hydrophilic resin, which interacts with the urethane resin (A) having urea bonds, improving the adhesion between the anchor coat layer and the barrier layer, and the oxygen barrier properties. Due to these effects, the laminate of the present invention has excellent oxygen barrier properties, adhesion, blocking resistance, and lamination strength after bending.

[0024] From the viewpoint of improving the oxygen barrier property and adhesion after bending, the mass ratio of the anchor coat layer to the barrier layer is preferably 0.1:1 to 2:1, more preferably 0.15:1 to 1:1, and even more preferably 0.2:1 to 0.6:1.

[0025] Specific examples of the laminate configuration include, but are not limited to, the following configurations. It is essential that the laminate has a substrate 1, an anchor coat layer, and a barrier layer in this order, and it is more preferable that the laminate has a substrate 1, an anchor coat layer, a barrier layer, and a substrate 2 in this order. In the following configurations, " / " means the boundary between the layers. The adhesive layer is not limited to the adhesive used in the conventionally known dry lamination and non-sol lamination, but also includes the case of a polyolefin resin or other thermoplastic resin layer in extrusion lamination. The thermoplastic resin layer is one embodiment of the adhesive layer, and is bonded to at least one of the layers. In the following Substrate 1 / anchor coat layer / barrier layer / adhesive layer / substrate 2 Substrate 1 / anchor coat layer / barrier layer / adhesive layer / intermediate substrate layer / adhesive layer / substrate 2 Substrate 1 / anchor coat layer / barrier layer / adhesive layer / intermediate substrate layer / adhesive layer (thermoplastic resin layer) / sealant Substrate 1 / anchor coat layer / barrier layer / adhesive layer / intermediate substrate layer / adhesive layer / intermediate substrate layer 2 / adhesive layer / substrate 2 (4) Substrate 1 / anchor coat layer / barrier layer / adhesive layer (thermoplastic resin layer) (5) Substrate 1 / anchor coat layer / barrier layer / adhesive layer (thermoplastic resin layer) / substrate 2 (6) Substrate 1 / anchor coat layer / barrier layer / adhesive layer (thermoplastic resin layer) / intermediate substrate layer / adhesive layer (thermoplastic resin layer) / sealant (8) Substrate 1 / anchor coat layer / barrier layer / adhesive layer (thermoplastic resin layer) / intermediate substrate layer / adhesive layer / substrate 2 (9) Substrate 1 / anchor coat layer / barrier layer / printing layer / adhesive layer / substrate 2 However, the present invention is not limited to these forms. In the above configuration example, the substrate 1, substrate 2 and intermediate substrate layer may be the same or different, and their names are determined by their positional relationships.

[0026] The substrate may be a single layer, may be a laminate of the same or different plastic substrates, or may be laminated with a substrate different from the plastic substrate via an adhesive layer or the like. The "substrate different from the plastic substrate" may be a paper substrate or the like, and may be of any type. In addition, in the case of a laminated substrate, it may be in a form including an adhesive layer. The method of lamination is not particularly limited, and may be a conventionally known method such as coextrusion, heat fusion, or pressure bonding via an adhesive layer. Preferred embodiments of the substrate 1 and the substrate 2 are described below.

[0027] [Base material 1] The substrate 1 that can be used in the laminate of the present invention is not particularly limited, but is preferably the following embodiment. That is, for example, the paper substrate can be medium-quality paper, fine paper, impregnated paper, cardboard, or kraft paper, and the plastic substrate can be biaxially oriented polypropylene (OPP), non-oriented polypropylene (CPP), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), or other polyethylene, acid-modified polyethylene, acid-modified polypropylene, copolymerized polypropylene, polyethylene terephthalate, polycarbonate, polylactic acid, polystyrene, AS resin, ABS resin, nylon, polyamide, polyvinyl chloride, polyvinylidene chloride, cellophane, or the like, and the substrate made of the above composite material can also be used. In addition, the substrate can be subjected to deposition of inorganic compounds such as silica, alumina, or aluminum, or coating treatment with polyethylene or polyvinyl alcohol, or corona treatment. Among them, the substrate 1 is preferably a paper substrate or an oriented plastic substrate. The thickness of the substrate 1 is not particularly limited, and in consideration of the processability into packaging containers, it is preferably from 5 μm to 150 μm, more preferably from 10 μm to 70 μm.

[0028] [Base material 2] The substrate 2 is not particularly limited, but in one embodiment, a polyolefin resin, particularly one having heat sealability, can be preferably used. Examples of the substrate 2 include a corona-treated biaxially oriented polypropylene (OPP) film, a high-density polyethylene film (HDPE), a non-oriented polypropylene (CPP) film, a linear low-density polyethylene (LLDPE) film, and a polyethylene resin film formed by melt coating. The thickness of the substrate 2 is not particularly limited, but from the viewpoint of processability during production of the packaging container, it is preferably 5 to 150 μm, and more preferably 10 to 70 μm.

[0029] [Anchor coat layer] The anchor coat layer in the present invention contains a urethane resin (A) having a predetermined bond concentration of urea bonds. The anchor coat layer is located between the substrate 1 and the barrier layer, and can be formed from an anchor coat agent described below.

[0030] The mass per unit area of ​​the anchor coat layer is 0.1 to 5 g / m 2 It is preferable that the thickness is 0.15 to 3 g / m 2 More preferably, the density is 0.2 to 1 g / m 2 When the mass per unit area of ​​the anchor coat layer is within the above range, the oxygen barrier property and adhesion during bending are excellent.

[0031] <Urethane resin (A)> The urethane resin (A) has a certain bond concentration of urea bond. For example, the urethane resin (A) can be a urethane urea resin obtained by reacting a urethane prepolymer having a terminal isocyanate, which is made of a polyol and a polyisocyanate, with a chain extender such as a polyamine, and is preferably used. However, it is not limited to this embodiment.

[0032] The content of the urethane resin (A) in the total mass of the anchor coat layer is preferably 20 to 90 mass%, more preferably 40 to 85 mass%, and even more preferably 60 to 80 mass%, because this improves the oxygen barrier property after bending.

[0033] The urea bond concentration of the urethane resin (A) is preferably 0.1 to 1.3 mmol / g, more preferably 0.3 to 1.15 mmol / g, and even more preferably 0.6 to 0.9 mmol / g. The urethane bond concentration of the urethane resin (A) is preferably 0.1 to 1.3 mmol / g, more preferably 0.3 to 1.15 mmol / g, and even more preferably 0.6 to 0.9 mmol / g. When it is within the above range, the oxygen barrier property, adhesion, blocking resistance, and laminate strength after bending are excellent.

[0034] (Urethane bond concentration) The urethane bond concentration is a value represented by the following formula. In the raw materials constituting the urethane resin (A), when (number of moles of NCO / number of moles of OH)>1, it is represented by the following (Formula 1). (Formula 1) Urethane bond concentration (mmol / g) = total number of moles of hydroxyl groups (mmol) / total mass of solids (g) Here, the total number of moles of hydroxyl groups refers to the total number of moles of hydroxyl groups contained in the polyol or the like used in the reaction to form the urethane, and the total solid content refers to the total mass of the non-volatile components that become the urethane resin (A). In the above, when (number of moles of NCO / number of moles of OH)<1, it is represented by the following (Equation 2). (Formula 2) Urethane bond concentration (mmol / g) = total number of moles of isocyanate groups (mmol) / total mass of solids (g) The total number of moles of isocyanate groups herein refers to the total number of moles of isocyanate groups contained in the polyisocyanate used in the reaction to form urethane.

[0035] (urea bond concentration) The urea binding concentration is a value represented by the following formula. When a prepolymer having a terminal isocyanate group is synthesized under the above condition of (moles of NCO / moles of OH)>1 and then chain-extended with polyamine to give urethane resin (A) having an amino group at the terminal, the product is represented by the following formula 3. (Formula 3) Urea bond concentration (mmol / g) = [total number of moles of isocyanate groups (mmol) - total number of moles of hydroxyl groups (mmol)] / total mass of solids (g) When a prepolymer having a terminal isocyanate group is synthesized under the above condition of (moles of NCO / moles of OH)>1 and then chain-extended with polyamine to give a urethane resin (A) having an isocyanate group at its terminal, the product is represented by the following formula 4. (Formula 4) Urea bond concentration (mmol / g) = (total number of amino group moles (mmol)) / total mass of solids (g) The total number of moles of amino groups herein refers to the total number of moles of primary or secondary amino groups contained in the polyamine used to form urea bonds by reacting with a prepolymer having a terminal isocyanate group.

[0036] The mass average molecular weight of the urethane resin (A) is preferably 10,000 to 100,000, more preferably 20,000 to 85,000, and even more preferably 30,000 to 70,000. When the mass average molecular weight of the urethane resin (A) is within the above range, the oxygen barrier property after bending is good.

[0037] The glass transition temperature of the urethane resin (A) is preferably −80 to 20° C., more preferably −60 to 0° C., and even more preferably −40 to −5° C. When the glass transition temperature of the urethane resin (A) is within the above range, the oxygen barrier property after bending is good.

[0038] The amine value of the urethane resin (A) is preferably 0.5 to 20 mgKOH / g, more preferably 1 to 15 mgKOH / g. When the amine value of the urethane resin (A) is within the above range, the oxygen barrier property after bending is good.

[0039] The hydroxyl value of the urethane resin (A) is preferably 0.5 to 30 mgKOH / g, more preferably 1 to 20 mgKOH / g. When the hydroxyl value of the urethane resin (A) is within the above range, the oxygen barrier property after bending is good.

[0040] The urethane resin (A) preferably contains a structural unit derived from a polyester polyol, and the content thereof is preferably 5 to 80 mass%, more preferably 30 to 70 mass%, based on 100 mass% of the solid content of the urethane resin (A). When the content of the structural unit derived from a polyester polyol is within the above range, the oxygen barrier property and blocking resistance after bending are good.

[0041] The method for producing the urethane resin (A) is not particularly limited, and a known method can be used. For example, a urethane resin obtained by reacting a urethane prepolymer having a terminal isocyanate, which is composed of a polyol and a polyisocyanate, with a polyamine and, if necessary, a polymerization terminator, is preferred. For example, a known method can be used, such as a prepolymer method in which a polyol and a polyisocyanate are reacted at a temperature of 50°C to 150°C (urethanization reaction) using a solvent inactive to isocyanate groups as necessary, and further using a urethanization catalyst as necessary, to produce a prepolymer having an isocyanate group at the end, and then reacting this prepolymer with a polyamine at 10 to 60°C to obtain a urethane resin, or a one-shot method in which a high molecular weight polyol, a polyisocyanate, and a polyamine (and a polymerization terminator as necessary) are reacted in one step to obtain a urethane resin (A). Polyamine can also be used in the urethane reaction of a polyol and a polyisocyanate.

[0042] Examples of the polyol include polyester polyol, polyether polyol, polycaprolactone diol, polycarbonate polyol, polyolefin polyol, castor oil polyol, hydrogenated castor oil polyol, dimer diol, and hydrogenated dimer diol. Among them, polyester polyol is preferable.

[0043] The polyester polyol may be, for example, a condensate obtained by an esterification reaction between a dibasic acid and a diol. Examples of dibasic acids include adipic acid, phthalic anhydride, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, succinic acid, oxalic acid, malonic acid, pimelic acid, azelaic acid, sebacic acid, suberic acid, glutaric acid, 1,4-cyclohexyldicarboxylic acid, dimer acid, hydrogenated dimer acid, etc. Among these, sebacic acid and adipic acid are particularly preferred. Examples of the diol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 2,4-diethyl-1,5-pentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, 1-monoglyceride, 2-monoglyceride, 1-monoglycerin ether, 2-monoglycerin ether, dimer diol, hydrogenated dimer diol, etc. Among them, polyester polyols consisting of a diol having a branched structure and a dibasic acid are preferred. The branched structure means a diol having an alkyl side chain in which at least one hydrogen atom of the alkylene group contained in the diol is replaced by an alkyl group, and examples thereof include propylene glycol, 1,3-butanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 1,4-pentanediol, 3-methyl-1,5-pentanediol, 2,5-hexanediol, 2-methyl-1,4-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, and 2,2,4-trimethyl-1,6-hexanediol. These are particularly preferred because they improve printability, printing effect, and laminate strength. These polyester polyols can be used alone or in combination of two or more. The polyester polyols can also be used in combination with a polyol having three or more hydroxyl groups and / or a polycarboxylic acid having three or more carboxyl groups.

[0044] The number average molecular weight of the polyester polyol is preferably 500 to 10,000. The number average molecular weight is calculated by the formula 5. The acid value of the polyester polyol is preferably 1.0 mgKOH / g or less, and more preferably 0.5 mgKOH / g or less. (Formula 5) Number average molecular weight of polyol = 1000 x 56.1 x hydroxyl value / hydroxyl value

[0045] In the production of the urethane resin (A), the polyol may contain a low molecular weight diol. Such low molecular weight diols preferably have a molecular weight of 50 to 800, and include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 2,4-diethyl-1,5-pentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, 1-monoglyceride, 2-monoglyceride, 1-monoglycerin ether, 2-monoglycerin ether, dimer diol, and hydrogenated dimer diol.

[0046] Examples of the polyisocyanate include various known aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, etc., which are generally used in the production of urethane resins. Specific examples include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, etc. Examples of the polyisocyanates include cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, dimeryl diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, m-tetramethylxylylene diisocyanate, 4,4-diphenylmethane diisocyanate, bis-chloromethyl-diphenylmethane-diisocyanate, 2,6-diisocyanate-benzyl chloride, and dimer diisocyanate in which the carboxyl group of a dimer acid is converted to an isocyanate group. These may be trimers to form an isocyanurate ring structure. These polyisocyanates may be used alone or in combination of two or more. Among these, tolylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, hexamethylene diisocyanate, and isocyanurates of hexamethylene diisocyanate are preferred.

[0047] The polyamine is preferably a polyamine having a molecular weight of 500 or less, but is not limited thereto, and examples thereof include diamines and polyfunctional amines, and in addition to diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, pentamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and p-phenylenediamine, diamines having hydroxyl groups such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropyldiamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine can also be used. These polyamines can be used alone or in combination of two or more. In particular, the urethane resin (A) preferably contains a structural unit derived from a polyfunctional polyamine having three or more functional groups. Specific examples of the polyfunctional polyamine include diethylenetriamine, iminobispropylamine (IBPA, 3,3'-diaminodipropylamine), triethylenetetramine, N-(3-aminopropyl)butane-1,4-diamine (spermidine), 6,6-iminodihexylamine, 3,7-diazanonane-1,9-diamine, and N,N'-bis(3-aminopropyl)ethylenediamine. The polyfunctional polyamine preferably has three amino groups. It is further preferable to use it in combination with a diamine. Among these, isophoronediamine, hexamethylenediamine, and iminobispropylamine are preferred.

[0048] The ratio of the total molar number of amino groups in the polyamine to the molar number of isocyanate groups in the prepolymer is preferably from 1.01 to 2.00, and more preferably from 1.03 to 1.06.

[0049] In addition, a monovalent active hydrogen compound can be used as a polymerization terminator for the purpose of stopping an excessive reaction. Examples of such compounds are not particularly limited as long as they are monoamine compounds having a primary or secondary amino group, and include dialkylamines such as di-n-butylamine and amino alcohols such as 2-ethanolamine. Furthermore, when it is particularly desired to introduce a carboxyl group into the urethane resin, amino acids such as glycine and L-alanine can be used as a polymerization terminator. When using a polymerization terminator, a chain extension reaction may be carried out by using the polymerization terminator together with a chain extender (polyamine), or the polymerization may be terminated by adding the polymerization terminator alone after carrying out a certain amount of chain extension reaction with the chain extender. On the other hand, although it is possible to control the molecular weight without using a polymerization terminator, in this case, a method of adding a prepolymer to a solution containing a chain extender is preferable in terms of reaction control. As the polymerization terminator, an amino alcohol is preferable, and it is preferable to use it at a ratio of 0.01 to 2.0 mass% relative to 100 mass% of the urethane resin (A).

[0050] In producing the prepolymer, the amounts of polyol and polyisocyanate are preferably adjusted so that the NCO / OH ratio, which is the ratio of the number of moles of isocyanate groups in the polyisocyanate to the number of moles of the total hydroxyl groups in the polymer polyol, is in the range of 1.1 to 3.0, and more preferably 1.3 to 2.5.

[0051] In addition, in terms of reaction control, it is preferable to use an organic solvent for synthesizing the prepolymer. The organic solvent is preferably an organic solvent inactive to an isocyanate group, and examples thereof include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethers such as dioxane and tetrahydrofuran; and esters such as ethyl acetate, butyl acetate, and propyl acetate. These can be used alone or as a mixed solvent of two or more kinds.

[0052] Furthermore, a catalyst can be used in the synthesis of the prepolymer. Examples of the catalyst include tertiary amine catalysts such as triethylamine and dimethylaniline, and metal catalysts such as tin and zinc. These catalysts are usually used in the range of 0.001 to 1 mol % based on the polyol compound.

[0053] <Resins used in combination with urethane resin (A)> The urethane resin (A) forming the anchor coat layer preferably further contains a vinyl chloride resin and a co-used resin such as a polyvinyl acetal resin, a cellulose resin, a polyamide resin, etc. The co-used resin is preferably a vinyl chloride resin and / or a polyvinyl acetal resin, and more preferably a vinyl chloride resin. The mass ratio of the urethane resin (A) to the above-mentioned co-resin is preferably 3:7 to 9.9:0.1, more preferably 5:5 to 9.5:0.5, and further preferably 7:3 to 9:1.

[0054] <Vinyl chloride resin> The vinyl chloride resin includes a structure obtained by polymerizing a monomer having an unsaturated double bond (excluding vinyl chloride) and a vinyl chloride monomer. Suitable examples of the vinyl chloride resin include vinyl chloride-acrylic copolymer resin and vinyl chloride-vinyl acetate copolymer resin.

[0055] <Vinyl chloride-acrylic copolymer resin> The vinyl chloride-acrylic copolymer resin is mainly composed of a copolymer of vinyl chloride and an acrylic monomer, and the acrylic monomer is a monomer having an acrylic group or a methacrylic group, and preferably contains an acrylic monomer having a hydroxyl group. (Hereinafter, "acrylic or methacrylic" may be referred to as "(meth)acrylic.") The vinyl chloride-acrylic copolymer resin may be a block copolymer or random copolymer of vinyl chloride and an acrylic monomer, or a graft copolymer in which an acrylic monomer is grafted to the side chain of polyvinyl chloride.

[0056] The mass average molecular weight of the vinyl chloride-acrylic copolymer resin is preferably 10,000 to 100,000, and more preferably 30,000 to 70,000. The glass transition temperature of the vinyl chloride-acrylic copolymer resin is preferably 50 to 90°C, more preferably 55 to 85°C, and even more preferably 65 to 80°C. The hydroxyl value of the vinyl chloride-acrylic copolymer resin is preferably 10 to 120 mgKOH / g, more preferably 20 to 110 mgKOH / g, even more preferably 30 to 100 mgKOH / g, and particularly preferably 40 to 80 mgKOH / g. The content of the vinyl chloride-derived structure in the vinyl chloride-acrylic copolymer resin is preferably 70 to 95 mass% in 100 mass% of the solid content of the vinyl chloride-acrylic copolymer resin.

[0057] Examples of the (meth)acrylic monomer having a hydroxyl group include hydroxyalkyl (meth)acrylate, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate (hydroxyalkyl esters), polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and glycol mono(meth)acrylate such as 1,4-cyclohexanedimethanol mono(meth)acrylate, caprolactone-modified (meth)acrylate, and hydroxyethylacrylamide. Among these, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxypropyl (meth)acrylate are preferred. These can be used alone or in combination of two or more.

[0058] The (meth)acrylic monomer may contain an alkyl (meth)acrylate. The number of carbon atoms of the alkyl group in the alkyl (meth)acrylate is preferably 1 to 20. Examples of the alkyl acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, and octadecyl (meth)acrylate. The alkyl group may have an aromatic ring structure substituted with an aryl group or the like. These may be used alone or in combination of two or more.

[0059] As the vinyl chloride-acrylic copolymer resin, for example, commercially available products such as Solvine A Type Series (manufactured by Shin-Etsu Chemical Co., Ltd.) can be used.

[0060] <Vinyl chloride-vinyl acetate copolymer resin> The vinyl chloride-vinyl acetate copolymer resin is a resin in which at least vinyl chloride and vinyl acetate are copolymerized, and the mass average molecular weight is preferably 5,000 to 100,000, and more preferably 20,000 to 70,000. In 100% by mass of the solid content of the vinyl chloride-vinyl acetate copolymer resin, the content of the structure derived from the vinyl acetate monomer is preferably 1 to 30% by mass, and the content of the structure derived from the vinyl chloride monomer is preferably 70 to 95% by mass. In addition, the vinyl chloride-vinyl acetate copolymer resin is more preferably one containing a hydroxyl group derived from vinyl alcohol derived from a saponification reaction or copolymerization, in order to improve the solubility in an organic solvent, and the hydroxyl value is preferably 20 to 200 mgKOH / g. In addition, the glass transition temperature of the vinyl chloride-vinyl acetate copolymer resin is preferably 50°C to 90°C.

[0061] As the vinyl chloride-acrylic copolymer resin, commercially available products such as Solvine C type series (manufactured by Shin-Etsu Chemical Co., Ltd.) can be used.

[0062] <Polyvinyl acetal resin> The polyvinyl acetal resin is obtained by reacting polyvinyl alcohol with an aldehyde such as butylaldehyde to form an acetal, and preferably contains a vinyl alcohol unit, a vinyl acetate unit, and an acetal ring unit. For the acetalization reaction, a known aldehyde such as formaldehyde or acetaldehyde can be used, and two or more kinds of aldehydes can also be used. Examples of polyvinyl acetal resins include polyvinyl formal, polyvinyl acetal, and polyvinyl butyral, with polyvinyl butyral being preferred.

[0063] The content of acetal rings in the polyvinyl acetal resin is preferably 60 to 90% by mass in 100% by mass of the polyvinyl acetal resin. When the content of acetal rings is within the above range, adhesion is improved and laminate strength is good. The content of vinyl alcohol units in the polyvinyl acetal resin is preferably 5 to 30% by mass, more preferably 15 to 25% by mass in 100% by mass of the polyvinyl acetal resin. When the content of vinyl alcohol units is within the above range, adhesion is improved and laminate strength is good. The content of vinyl acetate units in the polyvinyl acetal resin is preferably 0.5 to 10% by mass, more preferably 1 to 5% by mass in 100% by mass of the polyvinyl acetal resin. When the content of vinyl acetate units is within the above range, adhesion is improved and laminate strength is good.

[0064] The mass average molecular weight of the polyvinyl acetal resin is preferably 25,000 to 200,000, more preferably 40,000 to 150,000, and even more preferably 7,0000 to 120,000. When the mass average molecular weight of the polyvinyl acetal resin is within the above range, the laminate strength is good. The glass transition temperature of the polyvinyl acetal resin is preferably 50 to 80°C, and more preferably 60 to 75°C. When the glass transition temperature of the polyvinyl acetal resin is within the above range, the laminate strength is good.

[0065] As the polyvinyl acetal resin, commercially available products such as the Mobital series (manufactured by Kuraray, polyvinyl butyral resin), the S-LEC KX series (manufactured by Sekisui Chemical Co., Ltd., polyvinyl acetal resin), and the Vinylec series (manufactured by JNC, polyvinyl formal) can be used.

[0066] <Inorganic pigments> In order to improve the oxygen barrier property after bending, the anchor coat layer preferably contains an inorganic pigment. Examples of inorganic pigments include titanium oxide, zinc oxide, zinc sulfide chromium oxide, aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, iron black, silica, barium sulfate, kaolin clay, calcium carbonate, magnesium carbonate, etc., with silica, barium sulfate, kaolin clay, calcium carbonate, and magnesium carbonate being preferred, and silica being particularly preferred.

[0067] The content of the inorganic pigment in the anchor coat layer is preferably 0.5 to 15 mass %, more preferably 1 to 10 mass %, and further preferably 3 to 7 mass %, based on 100 mass % of the anchor coat layer.

[0068] <Isocyanate-based hardener> In order to improve adhesion, lamination strength, and oxygen barrier properties after bending, the anchor coat layer preferably contains a cured product derived from an isocyanate-based curing agent, i.e., the anchor coating agent for forming the anchor coat layer preferably contains an isocyanate-based curing agent. When the anchor coating agent contains an isocyanate-based curing agent, it forms a cured product by reacting with the urethane resin (A) or the like, or by reacting with the isocyanate-based curing agent itself. The cured product is preferably a product formed by the reaction between the urethane resin (A) and the isocyanate-based curing agent, i.e., it has a structure derived from the urethane resin (A) and a structure derived from the isocyanate-based curing agent.

[0069] Examples of isocyanate-based curing agents include aromatic isocyanate-based curing agents such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-dichloro-4,4'-biphenylene diisocyanate, 1,5-naphthalene diisocyanate, 1,5-tetrahydronaphthalene diisocyanate, xylylene diisocyanate, and tetramethylxylylene diisocyanate; Aliphatic isocyanate-based curing agents such as tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, dodecamethylene diisocyanate, trimethylhexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, hydrogenated xylylene diisocyanate, lysine diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and 3,3'-dimethyl-4,4'-dicyclohexylmethane diisocyanate; alicyclic isocyanate-based curing agents such as cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, and norbornane diisocyanate; an adduct type isocyanate-based curing agent which is an adduct of the above-mentioned isocyanate-based curing agent and a polyhydric alcohol; Among these, aliphatic isocyanate-based curing agents are preferred, adduct-type aliphatic isocyanate-based curing agents are more preferred, and trifunctional adduct-type aliphatic isocyanate-based curing agents are even more preferred.

[0070] Examples of the polyhydric alcohol include 1,2-propylene glycol (dihydric), diethylene glycol (dihydric), dipropylene glycol (dihydric), 1,3-butanediol (dihydric), neopentyl glycol (dihydric), trimethylolpropane (trihydric), 2,2,4-trimethyl-1,3-pentanediol (trihydric), polyethylene glycol (polyhydric), and polypropylene glycol (polyhydric), and among these, trimethylolpropane is preferred. A trifunctional adduct type aliphatic isocyanate is obtained by reacting a trihydric alcohol with an aliphatic isocyanate-based curing agent. A suitable example of the adduct type aliphatic isocyanate-based curing agent is a reaction product of 1,6-hexamethylene diisocyanate and trimethylolpropane.

[0071] As the isocyanate-based curing agent, commercially available products can be used, and examples thereof include 24A-100, 22A-75, TPA-100, TSA-100, TSS-100, TAE-100, TKA-100, P301-75E, E402-808, E405-70B, AE700-100, D101, D201, A201H (manufactured by Asahi Kasei Corporation), Mytech Y260A (manufactured by Mitsubishi Chemical Corporation), Coronate CORONATE HX, Coronate CORONATE HL, Coronate CORONATE L (manufactured by Nippon Polyurethane Co., Ltd.), and Desmodur N75MPA / X (manufactured by Bayer AG).

[0072] In the above anchor coat layer, in the cured product consisting of the urethane resin (A) and the isocyanate-based curing agent, the mass ratio of the constituent units derived from the urethane resin (A) to the constituent units derived from the isocyanate-based curing agent is preferably 99:1 to 70:30, more preferably 98:2 to 80:20, and even more preferably 95:5 to 85:15. When a combined resin is contained in addition to the urethane resin (A), the mass ratio of the total amount of the urethane resin and the combined resin to the isocyanate compound is preferably 99:1 to 70:30, more preferably 98:2 to 80:20, and even more preferably 95:5 to 85:15. When the mass ratio of the resin to the isocyanate curing agent is within the above range, the oxygen barrier property and adhesion after bending are good.

[0073] <Additives> The anchor coat layer preferably contains known additives or structures derived from additives, such as pigment derivatives, dispersants, wetting agents, adhesion aids, leveling agents, defoamers, antistatic agents, trapping agents, antiblocking agents, waxes, silane coupling agents, water, etc.

[0074] <Anchor coating agent> The anchor coating agent for forming the anchor coating layer contains a urethane resin (A). In order to improve the handling of the anchor coating agent and the oxygen barrier properties after folding, optional components such as organic solvents, co-resins, inorganic pigments, and additives can be added to the anchor coating agent alone or in combination.

[0075] The anchor coating agent can be obtained, for example, by feeding a resin solution in which a resin is dissolved in an organic solvent and an organic solvent into a mixer equipped with a stirring blade, rotor, etc., and mixing and stirring them. There are no particular limitations on the stirring speed, and the stirring can be performed at 50 to 2000 rpm.

[0076] <Organic solvent> Examples of organic solvents that can be used in the anchor coating agent include non-aromatic organic solvents such as hydrocarbons such as methylcyclohexane and ethylcyclohexane; ketones such as acetone, methyl ethyl ketone (MEK), and methyl isobutyl ketone; esters such as ethyl acetate, n-propyl acetate, and butyl acetate; and alcohols such as methanol, ethanol, propanol, isopropanol (IPA), and butanol. The organic solvent may be appropriately selected in consideration of reducing the amount of solvent remaining in the film after printing, and one type may be used alone, or two or more types may be mixed and used. The content of the organic solvent is preferably 30 to 95 mass%, more preferably 50 to 90 mass%, and particularly preferably 70 to 85 mass% in 100 mass% of the anchor coating agent.

[0077] In one embodiment of the coating, in order to improve adhesion, it is preferable to use a glycol ether-based solvent. The glycol ether-based solvent is not particularly limited, but examples thereof include ethylene glycol ether and propylene glycol ether. Among them, propylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether are preferred, and diethylene glycol monoethyl ether is more preferred. The glycol ether-based solvent is preferably present in an amount of 5 to 25% by mass, and particularly preferably 5 to 15% by mass, based on 100% by mass of the organic solvent.

[0078] <Formation of anchor coat layer> The anchor coat layer can be formed, for example, by printing the base material 1 with an anchor coat agent and then removing the volatile components. Printing methods include conventionally known methods such as gravure printing, flexographic printing, dipping, roll coating, screen printing, and spraying, but the gravure printing method is preferred. For example, the agent is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing, and is supplied to each printing unit alone or in a mixture and applied. The coating is then fixed by drying in an oven or the like to obtain an anchor coat layer.

[0079] [Barrier layer] The barrier layer in the present application is intended to impart oxygen barrier properties to the laminate, and contains a hydrophilic resin. The barrier layer is preferably formed from a barrier coating agent described below.

[0080] The mass per unit area of ​​the barrier layer is 0.1 to 5 g / m 2 It is preferable that the thickness is 0.3 to 3 g / m 2 More preferably, the thickness is 0.5 to 1.5 g / m 2 When the mass per unit area of ​​the barrier layer is within the above range, the oxygen barrier property and adhesion after bending are excellent.

[0081] <Hydrophilic resin> The hydrophilic resin refers to a resin that is miscible with water. Examples of hydrophilic resins include polyvinyl alcohol resins (including ethylene vinyl alcohol copolymer resins), aqueous acrylic resins, aqueous styrene-acrylic resins, aqueous styrene-maleic acid resins, aqueous urethane resins, aqueous polylactic acid resins, polyvinylpyrrolidone, starch, methyl cellulose, carboxymethyl cellulose, and modified resins thereof. These hydrophilic resins can be used alone or in combination of two or more. Among the above, the hydrophilic resin preferably contains a polyvinyl alcohol resin.

[0082] The content of the hydrophilic resin in the total mass of the barrier layer is preferably 30 to 95% by mass, more preferably 55 to 90% by mass, and even more preferably 70 to 80% by mass, in order to improve the oxygen barrier property after bending.

[0083] <Polyvinyl alcohol resin> The polyvinyl alcohol resin may be any resin having a vinyl alcohol unit, and further preferably contains a structural unit derived from ethylene. Examples of polyvinyl alcohol resins include polyvinyl alcohol resins and ethylene-vinyl alcohol copolymer resins, with polyvinyl alcohol resins and / or ethylene-vinyl alcohol copolymer resins being preferred, and ethylene-vinyl alcohol copolymer resins being more preferred.

[0084] The content of ethylene-derived structural units in the ethylene-vinyl alcohol copolymer resin is preferably 1 to 40 mol%, more preferably 3 to 20 mol%, and even more preferably 5 to 15 mol%. When the content of ethylene-derived structural units is within the above range, the oxygen barrier property after bending is good. The degree of polymerization of the polyvinyl alcohol resin is preferably 100 to 3,000, and more preferably 500 to 2,400. When within the above range, the oxygen barrier property after bending is good.

[0085] The polyvinyl alcohol resin may have a modified functional group, and examples of the functional group include, but are not limited to, a carbonyl group, a silicon group, etc. Also, the polyvinyl alcohol resin may be used that has been crosslinked with a crosslinking agent, and examples of the crosslinking agent used include known crosslinking agents such as an isocyanate crosslinking agent, an epoxy crosslinking agent, a melamine crosslinking agent, an oxazoline crosslinking agent, and a silane coupling crosslinking agent, and the oxazoline crosslinking agent and the silane coupling crosslinking agent are preferred.

[0086] The degree of saponification of the polyvinyl alcohol resin is represented by the following formula (6), and is preferably 80 mol% or more, more preferably 90 mol%, and more preferably 95 mol%. When it is in the above range, the oxygen barrier property is good. (Formula 6) Saponification degree: (number of hydroxyl groups) / {(number of hydroxyl groups)+(number of acetate groups)}×100 [mol %]

[0087] As the polyvinyl alcohol-based resin, Kuraray Poval R series (polyvinyl alcohol resin, manufactured by Kuraray Co., Ltd.), Kuraray Eval L104B, F104B (ethylene-vinyl alcohol copolymer resin, manufactured by Kuraray Co., Ltd.), etc. can be used.

[0088] <Inorganic layered filler> The barrier layer preferably contains an inorganic layered filler. The inorganic layered filler referred to here is an inorganic filler in which single crystal layers are stacked to form a layered structure, and is particularly preferably one that swells and / or cleaves in a solvent. The mass ratio of the hydrophilic resin to the inorganic layered filler is preferably 4:6 to 9:1, more preferably 6:4 to 8:2, and even more preferably 8:2 to 7:3. When it is within the above range, the oxygen barrier property after bending is good.

[0089] Preferred examples of the inorganic layered filler include montmorillonite, beidellite, saponite, hectorite, sauconite, vermiculite, mica, paragonite, lepidolite, margarite, clintonite, anandite, chlorite, donbassite, sudoite, cookeite, clinochlore, chamosite, nimite, tetrasilylic mica, talc, pyrophyllite, nacrite, kaolinite, halloysite, chrysotile, sodium teniolite, xanthophyllite, antigorite, dickite, hydrotalcite, etc., and one or more selected from the group consisting of kaolin, montmorillonite, and mica are preferred, and montmorillonite is more preferred. Montmorillonite has high water absorption and high viscosity after swelling due to its layered structure, so that resin easily penetrates between the layers of the layered filler, contributing to improving the oxygen barrier property of the laminate.

[0090] These inorganic layered fillers may be naturally occurring or artificially synthesized or modified, or may be treated with an organic substance such as an onium salt.

[0091] The content of the inorganic layered filler is preferably from 1 to 40 mass %, more preferably from 10 to 35 mass %, and further preferably from 20 to 30 mass %, relative to 100 mass % of the barrier layer.

[0092] <Montmorillonite> The above montmorillonite is represented by the following formula (7): Bentonite, which contains montmorillonite as a main component and further contains minerals such as quartz and feldspar, can also be preferably used. (Formula 7) M a S 4 (Al 2-a Mg a )O 10 (OH) 2 nH 2 O (In formula 7, M represents a sodium cation, and a is 0.25 to 0.60. The number of water molecules bonded to the ion-exchangeable cations between layers can vary depending on the cation species, humidity, and other conditions. 2 It is represented by O.) Montmorillonite also includes isomorphous ion-substituted products of magnesian montmorillonite, iron montmorillonite, and iron magnesian montmorillonite, which are represented by the following formulas (8) to (10), and these may also be used. (Formula 8) M a S 4 (Al 1.67-a Mg 0.5+a )O 10 (OH) 2 nH 2 O (Formula 9) M a S 4 (Fe 2-a3 +Mg a )O 10 (OH) 2 nH 2 O (Formula 10) M a S 4 (Fe 1.67-a3 +Mg 0.5+a )O 10 (OH) 2 nH 2 O (In formulas 8 to 10, M represents a sodium cation, and a is 0.25 to 0.60.)

[0093] Montmorillonite usually has cations between its layers, but the content varies depending on the place of origin. Examples of the ions include inorganic cations such as sodium ions, calcium ions, magnesium ions, and potassium ions, and organic cations such as quaternary ammonium ions. From the viewpoint of affinity with water, inorganic cations are preferred, and sodium ions and / or calcium ions are more preferred. It is also preferred to use montmorillonite that has been purified by water treatment.

[0094] The volume-average particle thickness of montmorillonite is preferably 0.05 to 30 nm, more preferably 0.1 to 10 nm, and even more preferably 0.5 to 3 nm. The volume-average particle major axis of bentonite is preferably 0.01 to 5 μm, more preferably 0.05 to 3 μm, and even more preferably 0.1 to 1 μm. In addition, the volume-average particle aspect ratio of bentonite is preferably 10 to 2,000, more preferably 100 to 1,000, and even more preferably 300 to 700. In the present invention, the particle thickness, particle major axis, and particle aspect ratio of bentonite can be measured by an atomic force microscope (AFM).

[0095] As the montmorillonite, commercially available products such as Kunipia-F and Kunipia-G (manufactured by Kunimine Kogyo Co., Ltd.) can be used.

[0096] <Kaolin> Kaolin is a type of kaolinite (Al 2 O 3 2SiO 2 H 2 O) or halloysite Al 2 O 3 2SiO 2 2H 2 It may be a natural or synthetic product, with O as the main component. Also, depending on the manufacturing method, there are dry kaolin, wet kaolin, calcined kaolin, etc., but it is not limited to these.

[0097] From the viewpoint of oxygen barrier property, the volume-average particle size of kaolin is preferably 1 to 100 μm, more preferably 3 to 50 μm, and even more preferably 5 to 20. The volume-average aspect ratio of kaolin is preferably 10 to 1,000, more preferably 30 to 500, and even more preferably 50 to 200. In the present invention, the particle size of kaolin can be measured by a laser analysis / scattering method, and the aspect ratio can be measured by a scanning electron microscope (SEM).

[0098] As the kaolin, commercially available products such as Varisurf HX (manufactured by Imerys), NN kaolin clay, and ST kaolin clay (manufactured by Takehara Chemical Industry Co., Ltd.) can be used.

[0099] <Mica> Both natural and synthetic mica can be used. Natural mica is a scaly base material made by crushing mica ore, and the particle size and aspect ratio can be controlled by mechanical crushing, cleavage by calcination, etc. Synthetic mica is SiO 2 , MgO, Al 2 0 3 , K 2 SiF 6 , Na 2 SiF 6 It is synthesized by heating industrial raw materials such as fluorine mica, melting them at a high temperature of about 1500°C, and then cooling and crystallizing them. Compared to natural mica, it has fewer impurities and is uniform in size and thickness. 3 AlSi 3 O10F 2 ), potassium tetrasilicic mica (KMg 25 AlSi 4 O10F 2 ), sodium tetrasilicic mica (NaMg 25 AlSi 4 O 10 F 2 ), Na taeniolite (NaMg 2 LiSi 4 O10F 2 ), LiNa taeniolite (LiMg 2 LiSi 4 O 10 F 2 From the viewpoint of dispersibility, synthetic mica that is easy to cleave by intercalation is preferable.

[0100] From the viewpoints of printability and oxygen barrier property, the volume average particle size of the mica is preferably 30 μm or less, more preferably 1 to 25 μm, and even more preferably 5 to 15 μm, and the volume average aspect ratio of the mica is preferably 30 to 200, more preferably 70 to 170, and even more preferably 100 to 150. In the present invention, the particle size of mica can be measured by a laser analysis / scattering method, and the aspect ratio can be measured by a scanning electron microscope (SEM).

[0101] As the mica, commercially available products such as Mica Powder TM series, Mica Powder NCF series (manufactured by Yamaguchi Mica Co., Ltd.), L60M, L100M (manufactured by Seishin Enterprise Co., Ltd.) and the like can be used.

[0102] <Additives contained in the barrier layer> The barrier layer may contain known additives such as an isocyanate compound, a silane coupling agent, a dispersant, a stabilizer, a viscosity adjuster, a colorant, etc., within the scope of not impairing the effects of the present invention.

[0103] <Barrier coating agent> The barrier coating agent for forming the barrier coating layer preferably contains a hydrophilic resin and an aqueous solvent. In addition, each component of the inorganic layered filler can be added to the coating agent alone or in combination, and additives contained in the barrier coating layer can be added as appropriate. The barrier coating agent can be obtained by charging a resin solution in which a resin is dissolved or dispersed in an aqueous solvent, and an aqueous solvent into a mixer equipped with a stirring blade, rotor, etc., and mixing and stirring the mixture. There is no particular restriction on the stirring speed, and the mixture can be stirred at 50 to 2000 rpm. In order to improve the handling and oxygen barrier properties of the barrier coating agent, inorganic layered fillers, various additives, and aqueous solvents can also be appropriately added.

[0104] <Aqueous solvent> The barrier coating agent preferably contains an aqueous solvent. The main component of the aqueous solvent is preferably water, but a hydrophilic organic solvent can be used in addition to water. Specifically, an alcohol-based organic solvent, a glycol-based organic solvent, etc. can be contained depending on the printing conditions (speed, plate depth, design, drying temperature). In the present invention, the term "mainly water" means that the content of water is the largest in the aqueous solvent, and the term "hydrophilic organic solvent" means that the solvent is liquid at 25° C. and has a solubility of 1% by mass or more in water at 25° C.

[0105] Examples of the alcohol-based organic solvent include methanol, ethanol, propanol, isopropanol, isobutanol, normal butanol, tertiary butanol, hexanol, octanol, and decanol.

[0106] Examples of the glycol-based organic solvent include acetylene diol, ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monooctyl ether, diethylene glycol, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monopropyl ether, triethylene glycol monobutyl ether, propylene glycol, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monopropyl ether, tripropylene glycol monobutyl ether, and dibutyl glycol. These may be used alone or in combination of two or more.

[0107] <Barrier layer formation> The barrier layer can be formed, for example, by printing on the anchor coat layer using a barrier coating agent, and then removing the volatile components. Printing methods include conventionally known methods such as gravure printing, flexographic printing, dipping, roll coating, screen printing, and spraying, but gravure printing is preferred, and for example, the agent is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing, and is supplied to each printing unit alone or in a mixture, and applied. Thereafter, the coating is fixed by drying in an oven or the like to obtain a barrier coat layer.

[0108] [Print layer] The printing layer preferably contains a resin and a colorant. The printing layer may be a layer that displays any design, pattern, character, symbol, etc. for the purpose of providing decoration or aesthetics, or displaying the contents, expiration date, manufacturer or seller, etc. The printed layer may be a solid printed layer having no design, pattern, letter, symbol, etc. The method for forming the printed layer is not particularly limited, and the printed layer may be formed, for example, using a printing ink. The printed layer may have a single layer structure or a multi-layer structure, and may be printed on the surface layer. The mass per unit area of ​​the printed layer is 0.1 to 12 g / m 2 It is preferable that the thickness is 0.5 to 6 g / m 2 More preferably, it is 1 to 3 g / m 2 It is more preferable that:

[0109] <Resin contained in the printing layer> The resin contained in the printing layer is not particularly limited, and may be, for example, a known resin such as a urethane resin, a cellulose-based resin, a polyamide resin, a rosin-based resin, an ethylene-vinyl acetate copolymer resin, a vinyl acetate resin, a vinyl chloride-vinyl acetate copolymer resin, an acrylic resin, a styrene resin, a styrene-maleic acid copolymer resin, a polyester resin, etc. These resins may be used alone or in combination of two or more kinds.

[0110] <Coloring agent> The printed layer and the printing ink used to form the printed layer may contain a colorant. The colorant is preferably a pigment, and known pigments such as organic pigments, inorganic pigments, etc. may be used as the pigment. The colorant such as a pigment may be used alone or in combination of two or more kinds.

[0111] <Additives contained in the printing layer> The printed layer and the printing ink used to form the printed layer may contain known additives such as defoamers, fragrances, flame retardants, hydrocarbon waxes, thickeners, leveling agents, dispersants, curing agents, silane coupling agents, plasticizers, infrared absorbers, and ultraviolet absorbers, as necessary, and preferably contain at least one selected from the group consisting of hydrocarbon waxes and dispersants.

[0112] <Printing ink manufacturing method> The printing ink used to form the printed layer can be produced, for example, by dispersing a pigment with a resin or the like in an organic solvent using a disperser, and then mixing the resulting pigment dispersion with a resin, various additives, an organic solvent, etc. As the disperser, a commonly used one, for example, a roller mill, a ball mill, a pebble mill, an attritor, or a sand mill, can be used.

[0113] <Formation of printing layer> The printing layer can be formed, for example, by printing on a substrate using a printing ink and then removing the volatile components. The printing method is preferably a gravure printing method or a flexographic printing method, and, for example, the ink is diluted with a diluting solvent to a viscosity and concentration suitable for gravure printing, and is supplied to each printing unit alone or in a mixture and applied. The printing layer can then be obtained by fixing the coating by drying in an oven or the like. [Adhesive layer] The laminate of the present invention may include an adhesive layer for the purpose of adhering each layer. The adhesive layer is not particularly limited, and suitable examples include dry lamination adhesives such as olefin adhesives, acrylic adhesives, ethylene-vinyl acetate copolymer adhesives, reactive urethane adhesives, non-solvent lamination adhesives, imine anchor coating agents, butadiene anchor coating agents, isocyanate anchor coating agents, and thermoplastic resins used in extrusion lamination. It is preferable that the adhesive layer is a reaction product of a reactive urethane adhesive consisting of polyisocyanate and polyol.

[0114] The method for bonding (also referred to as laminating) each layer is not particularly limited, and examples thereof include conventionally known methods such as extrusion lamination, dry lamination, and non-solvent lamination.

[0115] [Intermediate substrate layer] The laminate of the present invention may have an intermediate substrate layer for the purpose of improving rigidity. A specific example of the intermediate substrate layer is preferably a plastic substrate mainly containing polyolefin resin as a raw material, similar to the substrate layer. Examples of the intermediate substrate layer include polyolefin resins such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ethylene-vinyl acetate copolymer, propylene homopolymer, and ethylene-propylene copolymer. The intermediate substrate may also be a composite substrate produced by a co-extrusion method. Furthermore, it is more preferable that the intermediate substrate is made of the same (same) material as the substrate and the sealant. Examples of the same (same) material include combinations of polypropylenes and polyethylenes.

[0116] [Sealant] The laminate of the present invention may have a sealant. The inner layer of the sealant is in direct contact with the packaged item and plays a role in protecting the packaged item. In order to make the laminate into a bag shape, it is preferable that the innermost layer of the sealant has heat sealability. Examples of materials constituting the sealant include polyolefin resins such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ethylene-vinyl acetate copolymer, propylene homopolymer, and ethylene-propylene copolymer, and one or more of these resins can be used. The sealant may be composed of a single layer or may be composed of two or more layers. In order to suppress shrinkage during heat sealing, the sealant is preferably a non-stretched film made of the above-mentioned resin.

[0117] [Packaging material] The laminate of the present invention can be suitably used to form packaging materials such as flexible packaging packages and packaging bags. The laminate of the present invention may be used alone as a packaging material, or may be used in combination with other materials. The packaging material may be a packaging container.

[0118] [Method of manufacturing laminate] The method for producing a laminate of the present invention is a method for producing a laminate having a substrate, an anchor coat layer, and a barrier layer in this order, and includes the steps of applying an anchor coat agent containing a urethane resin (A) having a urea bond onto the substrate to form an anchor coat layer, and applying a barrier coat agent containing a hydrophilic resin onto the anchor coat layer to form a barrier layer. EXAMPLES

[0119] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the present invention, parts and % represent parts by mass and % by mass unless otherwise noted.

[0120] <Hydroxyl value> The hydroxyl value is the number of milligrams of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when 1 g of a sample is acetylated, and was measured by the method described in JIS K 0070. <Acid value> The acid value is the number of milligrams of potassium hydroxide required to neutralize the free fatty acids, resin acids, etc. contained in 1 g of a sample, and was measured by the method described in JIS K 0070.

[0121] <Amine value> The amine value is the amount of potassium hydroxide in mg equivalent to the amount of hydrochloric acid required to neutralize the amino groups contained in 1 g of sample, and was measured in accordance with JIS K 0070. 0.5 to 2 g of sample was precisely weighed out (sample solid content: Sg), and 50 mL of a mixed solution of methanol / methyl ethyl ketone = 60 / 40 (mass ratio) was added to the precisely weighed sample to dissolve it. Bromophenol blue was added as an indicator to the resulting solution, and the resulting solution was titrated with a 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was set as the end point, and the titration amount (AmL) at this time was used to calculate the amine value according to the following (Equation 11). (Formula 11) Amine value = (A x f x 0.2 x 56.108) / S [mgKOH / g]

[0122] <Mass average molecular weight> The weight average molecular weight was determined by measuring the molecular weight distribution using a gel permeation chromatography (GPC) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight converted using polystyrene as a standard substance. The measurement conditions are shown below. Columns: The following columns were used in series connection: Tosoh Corporation TSKgel Super AW2500 Tosoh Corporation TSKgel Super AW3000 Tosoh Corporation TSKgel Super AW4000 Tosoh Corporation's TSK gelguard column Super AWH Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min

[0123] <Glass transition temperature (Tg)> The glass transition temperature was determined by differential scanning calorimetry (DSC). The measurement was performed using a Rigaku DSC8231 with a measurement temperature range of -70 to 250°C and a heating rate of 10°C / min. The midpoint (inflection point) of the baseline shift due to the glass transition in the DSC curve was taken as the glass transition temperature.

[0124] <Mass measurement per unit area in each layer> <Anchor coat layer> Five 10 cm square pieces were cut out from the substrate 1 / anchor coat layer component of the obtained intermediate laminate, and five 10 cm square pieces were cut out from the paper substrate. The mass of each sample was measured, and the mass per unit area of ​​the anchor coat layer was calculated using the following (Equation 12). For the substrate 1, a corona-treated biaxially oriented polypropylene (OPP) film (thickness 20 μm) was used. (Formula 12) Mass per unit area of ​​anchor coat layer (g / m 2 ) = (average mass of 5 samples of substrate 1 / anchor coat layer) - (average mass of 5 samples of substrate 1)

[0125] <Layers other than the anchor coat layer> For layers other than the anchor coat layer, the mass per unit area was calculated in the same manner as for the anchor coat layer, except that the calculation formula and the cut-out location of the sample were different. Note that a non-oriented polypropylene (CPP) film (thickness 30 μm) was used as the substrate 2. (Formula 13) Barrier layer mass per unit area (g / m 2 ) = (average mass of 5 samples of substrate 1 / anchor coat layer / barrier layer) - (average mass of 5 samples of substrate 1 / anchor coat layer) (Formula 14) Mass per unit area of ​​adhesive layer (g / m 2 )=(average mass of five samples of substrate 1 / anchor coat layer / barrier layer / adhesive layer / substrate 2)-{(average mass of five samples of substrate 1 / anchor coat layer / barrier layer)+(average mass of five samples of substrate 2)}

[0126] (Resin synthesis) <Synthesis Example 1> Urethane resin PU1 120.6 parts of ethyl acetate, 153.7 parts of a polyester polyol having a number average molecular weight of 2,000, which is a condensation product of 3-methyl-1,5-pentanediol (MPD) and adipic acid (AdA) (hereinafter "MPD / AdA 2000"), 27.9 parts of a polyester polyol having a number average molecular weight of 5,000, which is a condensation product of 3-methyl-1,5-pentanediol (MPD) and adipic acid (AdA) (hereinafter "MPD / AdA 5000"), 12.4 parts of a polypropylene glycol having a number average molecular weight of 700 (hereinafter "PPG 700"), 35.0 parts of a polypropylene glycol having a number average molecular weight of 2000 (hereinafter "PPG 2000"), and 52.3 parts of isophorone diisocyanate (hereinafter "IPDI") were mixed and reacted at 90°C for 5 hours under a nitrogen atmosphere to obtain a urethane prepolymer with a terminal isocyanate. Next, 279.6 parts of isopropanol, 299.7 parts of ethyl acetate, 2.1 parts of iminobispropylamine (hereinafter "IBPA"), and 16.6 parts of isophoronediamine (hereinafter "IPDA") were mixed with stirring, and the obtained urethane prepolymer with a terminal isocyanate was gradually added at 40° C. The mixture was reacted at 80° C. for 1 hour to obtain a solution of urethane resin PU1 with a solid content of 30% by mass, a urea bond concentration of 0.78 mmol / g, an amine value of 1.3 mgKOH / g, and a mass average molecular weight of 36,100.

[0127] <Synthesis Examples 2-5, Comparative Synthesis Examples 1 and 2> Urethane resins PU2-7 Urethane resins PU2 to PU7 were obtained in the same manner as in Synthesis Example 1, except that the raw materials and compounding ratios shown in Table 1 were used. The raw materials used are as follows. NPG / AdA 2000: A polyester polyol with a number average molecular weight of 2,000, which is a condensation product of neopentyl glycol (NPG) and adipic acid (AdA). MPO / AdA 2000: A polyester polyol with a number average molecular weight of 2,000, which is a condensation product of 2-methyl-1,3-propanediol (MPO) and adipic acid (AdA). MPO / AdA 5000: A polyester polyol with a number average molecular weight of 5,000, which is a condensation product of 2-methyl-1,3-propanediol (MPO) and adipic acid (AdA). 1,4-BD: 4-butanediol AEA: N-(2-aminoethyl)ethanolamine DBA: Dibutylamine 2EtAm: 2-aminoethanol

[0128] [Table 1]

[0129] (Manufacturing of anchor coating agents) <Production Example 1> Anchor Coating Agent AC1 47 parts of urethane resin PU1 solution, 15 parts of vinyl chloride-vinyl acetate resin PVC1 (hydroxyl value: 154 mg KOH / g, mass average molecular weight: 28,000, glass transition temperature: 78 ° C., solid content mass % = 25%), 1 part of silica particles S1 (Mizusawa Chemical Industry Co., Ltd., Mizukasil P-707, average particle size (laser scattering method): 4 μm, oil absorption: 250 ml / 100 g, solid content mass % = 100%), 1 part of chlorinated polypropylene (Nippon Paper Industries Co., Ltd., Super Chron 390S, solid content mass % = 50%), 0.5 parts of fatty acid amide solution (lauric acid amide, solid content mass % = 50%), 30.5 parts of mixed solvent (normal propyl acetate (NPAC) / isopropyl alcohol (IPA) = 7 / 3), 3 parts of propylene glycol monomethyl ether, and 2 parts of water were mixed and dispersed for 20 minutes with a bead mill to obtain a pigment dispersion. The resulting pigment dispersion was mixed with 20 parts of water with stirring to obtain anchor coating agent AC1.

[0130] <Production Examples 2 to 9, Comparative Production Examples 1 and 2> Anchor Coating Agents AC2 to 11 Anchor coating agents 2 to 11 were obtained in the same manner as in Production Example 1, except that the raw materials and compounding ratios shown in Table 2 were used. The properties of the raw materials used are as follows. Vinyl chloride-acrylic copolymer resin (PVC2): hydroxyl value: 59 mgKOH / g, weight average molecular weight: 45,000, glass transition temperature: 69°C, solid content by weight: 25% Polyvinyl butyral resin (PVAc1): Kuraray Co., Ltd., Mobital B20H, solid content by mass = 25% Polyvinyl acetal resin (PVAc2): Sekisui Chemical Co., Ltd., S-LEC KX-5, solid content by mass % = 25% Silica particles (S2): WR Grace, SYLOID ED 40, solid content by mass = 100%

[0131] [Table 2]

[0132] (hardening agent) Table 3 shows the curing agents H1 to H5 used in the examples.

[0133] [Table 3]

[0134] (Manufacturing of barrier coating agents) <Production Example 10> Barrier Coating Agent V1 6 parts of polyvinyl alcohol resin PVA1 (Kuraray Co., Ltd., Exeval AQ-4104, ethylene vinyl alcohol resin, ethylene content: 6 mol%, solid mass%=100%) and 92 parts of mixed solvent (water / IPA=8 / 2) were heated with stirring, and the heating and stirring were continued at 95°C for 1 hour, after which the heating was stopped and the stirring was continued until the temperature returned to normal, to obtain an aqueous solution of polyvinyl alcohol resin PVA1. 2 parts of montmorillonite (swelling, particle aspect ratio: 500, particle thickness: 1 μm, particle spread: 500 nm, solid mass%=100%) were added to the aqueous solution of polyvinyl alcohol resin PVA1, and the mixture was mixed and stirred to obtain a barrier coating agent V1. <Production Examples 11 to 17, Comparative Production Example 3> Barrier Coating Agents V2 to V10 Barrier coating agents V2 to 10 were obtained in the same manner as in Production Example 10, except that the raw materials and compounding ratios shown in Table 4 were used. The properties of the raw materials used are as follows. Polyvinyl alcohol resin PVA2: Kuraray Co., Ltd., Kuraray Poval 28-98, polyvinyl alcohol, solid content by mass = 100% Polyvinyl alcohol resin PVA3: Sekisui Chemical Co., Ltd., ULTILOC5003, amine-modified polyvinyl alcohol, solid content mass% = 100% Acrylic resin A1: Nippon Shokubai Co., Ltd., AQUALIC HL415, weight average molecular weight 10,000, solid content weight% = 45% Bentonite: BYK, CLOISITE-Na+, Mica: non-swelling, aspect ratio 130, average particle size (laser scattering method): 11 μm, oil absorption: 42 g / 100 g, solid content by mass % = 100% Kaolin: Hayashi Kasei Co., Ltd., Hydrite SB100, average particle size (laser scattering method): 1.2 μm, solid content by mass % = 100%

[0135] [Table 4]

[0136] (Manufacture of laminates) <Example 1> Intermediate laminate p1, laminate P1 100 parts of anchor coating agent AC1 was diluted with a mixed solvent (isopropyl alcohol / ethyl acetate) to a Zahn cup #3 (Rigo Co., Ltd.) 15 seconds (25°C), and then 3 parts of hardener H1 was added and mixed. 100 parts of barrier coating agent V1 was diluted with a mixed solvent (isopropyl alcohol / water) to a Zahn cup #3 (Rigo Co., Ltd.) 16 seconds (25°C). Thereafter, the entire surface of the corona-treated surface of a corona-treated biaxially oriented polypropylene (OPP) film (thickness 20 μm) was printed with a diluted anchor coating agent AC1 to which a curing agent H1 had been added using a gravure printing machine equipped with a gravure plate having a plate depth of 30 μm at a printing speed of 50 m / min and an in-line oven temperature of 60°C to form an anchor coating layer, and the diluted barrier coating agent V1 was printed three times on the anchor coating layer using a gravure printing machine equipped with a gravure plate having a plate depth of 60 μm and having a non-image area on one half of the plate at a printing speed of 50 m / min and an in-line oven temperature of 60°C to form a barrier layer, thereby obtaining an intermediate laminate p1 having a configuration of OPP (substrate 1) / anchor coat layer / barrier layer. Next, a polyether-based reactive urethane adhesive ("TM-340V / CAT-29B" manufactured by Toyo-Morton) was applied onto the barrier layer of the intermediate laminate p1 using a dry laminator, and the solvent was dried in an oven to form an adhesive layer. After that, a non-oriented polypropylene (CPP) film (thickness 30 μm) was laminated onto the adhesive layer at a line speed of 40 m / min and kept at 40°C for one day to obtain a laminate P1 having a structure of OPP (substrate 1) / anchor coat layer / barrier layer / adhesive layer / CPP (substrate 2). The mass per unit area of ​​the anchor coat layer of the laminate P1 was 0.4 g / m 2 , the mass per unit area of ​​the barrier layer is 1.0 g / m 2 , the mass per unit area of ​​the adhesive layer is 2.5 g / m 2 It was.

[0137] <Examples 2 to 22 and Comparative Examples 1 to 6> Intermediate laminates p2 to 28, laminates P2 to 28 Intermediate laminates p2 to 28 and laminates P2 to 28 were obtained in the same manner as in Example 1, except that the raw materials shown in Tables 5 and 6 were used and the mass per unit area was adjusted.

[0138] (evaluation) The laminates obtained in the above Examples and Comparative Examples were subjected to the following evaluations. The results are shown in Tables 5 and 6. <Adhesion> A 15 mm wide × 200 mm cellophane tape was attached to the obtained intermediate laminate, and the state of the barrier layer when it was quickly peeled off was evaluated according to the following criteria, where 3 to 5 is in the range where no problem occurs in practical use. Evaluation Criteria 5: 100% of the barrier layer remained. 4: 80% or more and less than 100% of the barrier layer remained. 3: 50% or more and less than 80% of the barrier layer remained. 2: 30% or more and less than 50% by area of ​​the barrier layer remained. 1: Less than 30% of the barrier layer remained.

[0139] <Blocking resistance> The obtained intermediate laminate was cut into two pieces of 40 mm square, and the substrate surface of one laminate piece was completely overlapped with the barrier layer surface of the other laminate piece, and the laminate was then subjected to a temperature of 40°C, a humidity of 80% RH, and a load of 100 N / cm 2 After leaving it for 24 hours, the two overlapping packaging materials were peeled off, and the peeling state of the printed layer was visually observed and evaluated according to the following criteria, with 3 to 5 being in the range where no problem occurs in practical use. Evaluation Criteria 5: The amount of the barrier layer transferred to one surface of the substrate is less than 5% by area. 4: The amount of the barrier layer transferred to one surface of the substrate is 5 area % or more and less than 10 area %. 3: The amount of the barrier layer transferred to one surface of the substrate is 10% by area or more and less than 25% by area. 2: The amount of the barrier layer transferred to one surface of the substrate is 25% by area or more and less than 50% by area. 1: The amount of the barrier layer transferred to one surface of the substrate is 50% or more by area.

[0140] <Lamination strength> The obtained laminate was cut into a piece of 150 mm in length and 15 mm in width, and the laminate strength in the 90° direction was measured using a tensile tester and evaluated according to the following criteria, with 3 to 5 being in the range where no practical problems exist. Evaluation Criteria 5: 1.5N / 15mm or more 4: 1.0N / 15mm or more, less than 1.5N / 15mm 3: 0.8N / 15mm or more, less than 1.0N / 15mm 2: 0.5N / 15mm or more, less than 0.8N / 15mm 1: Less than 0.5N / 15mm

[0141] <Oxygen barrier properties after bending> The obtained laminate was cut into a 100 mm square, folded so that the two substrate surfaces overlapped each other, and a pressure of 1 kg / m was applied to the folded portion. 2 The load was applied for 5 seconds. The folded portion was cut into 3 mm squares, and the oxygen permeability was measured according to a method in accordance with JIS K 7126-2:2006 and evaluated according to the following criteria. A range of 3 to 5 is acceptable for practical use. Evaluation Criteria 5: Oxygen permeability is 100g / m 2 Less than 24 hours. 4: Oxygen permeability is 100g / m 2 ·More than 24 hours, 1000g / m 2 Less than 24 hours. 3: Oxygen permeability is 1000g / m 2 ·Over 24 hours, 1500g / m 2 Less than 24 hours. 2: Oxygen permeability is 1500g / m 2 ·24h or more, 2000g / m 2 Less than 24 hours. 1: Oxygen permeability is 2000g / m 2 -24 hours or more.

[0142] From the above results, Comparative Example 1 did not have an anchor coat layer, and therefore the oxygen barrier property, adhesion, blocking resistance, and laminate strength after folding were poor. Comparative Example 2 did not have a barrier layer, and therefore the oxygen barrier property after folding was poor. Comparative Example 3 did not have an oxygen barrier property and blocking resistance after folding, and therefore the anchor coat layer did not contain a urethane resin (A) having a urea bond. Comparative Example 4 had poor oxygen barrier property, adhesion, blocking resistance, and laminate strength after folding, and therefore the urea bond concentration of the urethane resin (A) was less than 0.1 mmol / g. Comparative Example 5 had poor oxygen barrier property, adhesion, and laminate strength after folding, and therefore the urea bond concentration of the urethane resin (A) was more than 1.3 mmol / g. Comparative Example 6 had poor oxygen barrier property, adhesion, blocking resistance, and laminate strength after folding, and therefore the barrier layer did not contain a hydrophilic resin. On the other hand, the examples had an anchor coat layer and a barrier layer, the anchor coat layer contained a urethane resin (A) having a urea bond concentration of 0.1 to 1.3 mmol / g, and the barrier layer contained a hydrophilic resin, so that the oxygen barrier properties, adhesion, blocking resistance, and laminate strength after bending were good.

[0143] [Table 5]

[0144] [Table 5]

[0145] [Table 6]

Claims

1. A laminate having a substrate, an anchor coat layer, and a barrier layer in this order, the anchor coat layer contains a urethane resin (A) having a urea bond, and the urea bond concentration of the urethane resin (A) is 0.1 to 1.3 mmol / g; The laminate, wherein the barrier layer comprises a hydrophilic resin.

2. The laminate according to claim 1 , wherein the anchor coat layer comprises a cured product obtained by a reaction between the urethane resin (A) and an isocyanate-based curing agent.

3. The laminate according to claim 2 , wherein the isocyanate-based curing agent is an aliphatic isocyanate-based curing agent.

4. The laminate according to claim 3 , wherein the aliphatic isocyanate-based curing agent is an adduct-type aliphatic isocyanate-based curing agent.

5. The laminate according to claim 1 or 2, wherein the anchor coat layer further comprises a vinyl chloride resin and / or a polyvinyl acetal resin.

6. The laminate according to claim 1 or 2, wherein the anchor coat layer further comprises an inorganic pigment.

7. 3. The laminate according to claim 1, wherein the hydrophilic resin is a polyvinyl alcohol-based resin.

8. The laminate according to claim 1 or 2, wherein the barrier layer further comprises an inorganic layered filler.

9. 9. The laminate according to claim 8, wherein the inorganic layered filler is at least one selected from the group consisting of montmorillonite, mica, and kaolin.

10. A packaging material comprising the laminate according to claim 1 or 2.

11. A method for producing a laminate having a substrate, an anchor coat layer, and a barrier layer in this order, comprising: A step of applying an anchor coating agent onto a substrate to form an anchor coating layer; A step of applying a barrier coating agent onto the anchor coating layer to form a barrier layer, the anchor coating agent contains a urethane resin (A) having a urea bond, and the urea bond concentration of the urethane resin (A) is 0.1 to 1.3 mmol / g; The method for producing a laminate, wherein the barrier coating agent contains a hydrophilic resin.

Citation Information

Patent Citations

  • Barrier laminated film

    JP2002067214A

  • Gas barrier film

    JP2002307601A

  • Gas-barrier laminated film

    JP2002316381A

  • Gas barrier film laminate

    JP2003191364A

  • Laminate ink composition for soft packaging

    JP2017039836A