Heat storage and release material
The oriented grain structure in heat storage/dissipation titanium oxide aggregates reduces phase transition energy, enhancing the efficiency and practicality of heat storage and radiation materials.
Patent Information
- Application Number
- JP2023063219
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing heat storage and radiation materials using titanium oxide face challenges in efficiently dissipating heat due to high phase transition pressures, especially when using micron-sized particles, which hinders practical application.
A heat storage and radiation material composed of an aggregate of heat storage/dissipation titanium oxide crystal grains with an oriented grain structure, where fine crystals are aligned in a specific direction, facilitating efficient pressure propagation and reducing phase transition energy.
The oriented grain structure allows for lower energy phase transitions, enabling efficient heat storage and release, making the material more practical and cost-effective for heat exchange applications.
Smart Images

Figure 2024150014000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat storage and release material containing heat storage and release titanium oxide. [Background technology]
[0002] Heat-storing and releasing titanium oxide, a ceramic-based heat-storing material, is known as a heat-storing and releasing material that repeatedly stores and releases heat. Heat-storing and releasing titanium oxide is a trititanium pentoxide (i.e., Ti3O5)-based material that undergoes a phase transition between λ phase and β phase (see, for example, Non-Patent Documents 1 to 4), and has the property of potentially storing heat with the phase transition from β phase to λ phase, and releasing the stored heat with the phase transition from λ phase to β phase. Heat-storing and releasing materials containing heat-storing and releasing titanium oxide are easy to handle because they utilize the phase transition from solid phase to solid phase, and can efficiently store thermal energy such as exhaust heat from systems, so they are expected to be applied to heat exchange parts of various systems.
[0003] When the heat-storing and releasing titanium oxide is heated in the β phase, it undergoes a phase transition directly to the λ phase or via the α phase to the λ phase, and after the phase transition to the λ phase, it maintains that state unless it is subjected to an external stimulus such as pressure or light. It is known that such a heat-storing and releasing titanium oxide in the λ phase can be produced, for example, by using nano-sized particles of titanium dioxide (i.e., TiO2) as a raw material and reducing and firing it under a hydrogen atmosphere. In addition, Patent Document 1 proposes improving the heat-absorbing properties by adjusting the particle size of the titanium pentoxide particles containing the β phase to an appropriate median diameter D50 of 3 μm or more. Specifically, it is disclosed that the phase transition temperature and heat absorption and heat-absorbing properties according to the particle size can be obtained by crushing the lump-shaped titanium pentoxide synthesized by a chemical reaction or the like to obtain titanium pentoxide particles with a desired particle size distribution, and that, for example, when the median diameter D50 is 15 μm or more, the heat-absorbing properties are more stable. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-8390 [Non-patent literature]
[0005] [Non-Patent Document 1] “Synthesis of a metal oxide with a room-temperature photoreversible phase transition” Nature Chemistry, vol.2, p.539-545 (2010) [Non-Patent Document 2] “External stimulation-controllable heat-storage ceramics” Nature Communications vol.6,7037 (2015) [Non-Patent Document 3] “Ultrafast dynamics of photoinduced semiconductor-to-metal transition in the optical switching nano-oxide Ti3O5” Physical Review B 90, 014303(2014) [Non-Patent Document 4] “Electronic structure and correlation in β-Ti3O5 and λ-Ti3O5studied by hard x-ray photoelectron spectroscopy” Physical Review B 95, 085133(2017) Summary of the Invention [Problem to be solved by the invention]
[0006] When applying a heat storage and release material to a heat storage and release device, it is required to utilize the properties of heat storage and release titanium oxide to absorb and store the surrounding heat, and to efficiently release the stored heat by applying an external stimulus such as pressure at any timing. However, although there have been proposals focusing on the heat absorption properties, such as Patent Document 1, the heat release properties of heat storage and release titanium oxide have not necessarily been fully studied. In addition, using micron-sized raw material particles larger than nano-sized particles is advantageous for reducing manufacturing costs, but the pressure required for the phase transition of the obtained heat storage and release titanium oxide is relatively high, and it is desired to enable the phase transition at a lower pressure when it is put into practical use.
[0007] The present invention has been made in consideration of these problems, and aims to provide a heat storage and release material that can reduce the phase transition energy required for causing a phase transition of heat storage and release titanium oxide from the λ phase to the β phase, and that can efficiently extract the heat stored in the heat storage and release titanium oxide. [Means for solving the problem]
[0008] One aspect of the present invention is A heat storage and release material comprising an aggregate (1) of crystal grains (2) of heat storage and release titanium oxide, The heat-storing and dissipating titanium oxide is a titanium pentoxide-based material that stores or dissipates heat as it undergoes a phase transition between a lambda phase and a beta phase, The crystal grains are in a heat storage and release material having an oriented grain structure in which the fine crystal grains (20) of the heat storage and release titanium oxide are aggregated with an orientation. Effect of the Invention
[0009] The heat storage and release material is composed of an aggregate of crystal grains of heat storage and release titanium oxide, which is a trititanium pentoxide-based material, and when an external stimulus such as pressure is applied while the material is in a heat storage state, it undergoes a phase transition from the lambda phase to the beta phase and releases heat. At this time, the crystal grains that make up the aggregate have an oriented grain structure, and the fine crystals within the crystal grains are gathered so that their orientation is aligned, so pressure is efficiently transmitted and the phase transition is easily promoted. It is presumed that this makes it possible to reduce the energy required for the phase transition.
[0010] As described above, according to the above-mentioned embodiment, it is possible to reduce the phase transition energy required for the heat-storing and dissipating titanium oxide to undergo a phase transition from the λ phase to the β phase, and it is possible to provide a heat storage and dissipation material that can efficiently extract the heat stored in the heat-storing and dissipating titanium oxide. In addition, the symbols in parentheses described in the claims and the means for solving the problems indicate a correspondence with the specific means described in the embodiments described below, and do not limit the technical scope of the present invention. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a schematic diagram showing an example of the aggregate state of crystal grains constituting the heat storage and release material in the first embodiment and the orientation state of the crystal grains in a partial cross section thereof. [Diagram 2] 2 is a schematic diagram showing an example of the appearance of an aggregate of crystal grains and the aggregated state of the crystal grains in a partial cross section thereof in the first embodiment. FIG. [Diagram 3] FIG. 2 is a schematic diagram showing an example of the structure of a crystal grain of heat storing and releasing titanium oxide in the first embodiment. [Figure 4] FIG. 2 is a schematic diagram for explaining the mechanism of phase transition of the heat storing and releasing titanium oxide in the first embodiment. [Diagram 5] FIG. 2 is a schematic diagram for explaining the production process of the heat storing and releasing titanium oxide and the crystal grain growth process in the first embodiment. [Figure 6] FIG. 2 is a schematic diagram showing an example of the structure of crystal grains of heat storing and releasing titanium oxide in Comparative Example 1. [Figure 7] FIG. 2 is a schematic diagram for explaining the mechanism of phase transition of heat storing and releasing titanium oxide in Comparative Example 1. [Figure 8] FIG. 1 is a schematic diagram showing an example of the configuration of a production apparatus for a heat storage and release material in a first embodiment. [Figure 9] 3 is an image observed by a scanning electron microscope, showing the crystal aggregation state of the agglomerated particles and crystal grains containing the heat storing and releasing titanium oxide crystal grains in Example 1. [Figure 10] FIG. 2 is a crystal orientation map of the heat storage and release material in Example 1, obtained by electron backscatter diffraction. [Figure 11] FIG. 2 is a diagram showing a comparison of the crystal grain structures and phase transition characteristics of heat storage and release materials in Examples 1 and 2 and Comparative Examples 1 and 2. [Figure 12] 1 shows crystal orientation maps in Examples 1 and 2 and Comparative Examples 1 and 2, and an image observed by a scanning electron microscope showing the crystal assembly state of the heat storing and releasing titanium oxide in Comparative Example 3. [Figure 13] FIG. 4 is a graph showing the relationship between the average grain size of crystal grains of a heat storage and release material and the phase transition pressure in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (Embodiment 1) A first embodiment of the heat storage and release material will be described with reference to the drawings. In this embodiment, the heat storage and release material is a powder material containing crystals of heat storage and release titanium oxide, and can store or release thermal energy. The heat storage and release titanium oxide is a titanium trioxide-based material known as a type of reduced titanium oxide, and has the property of storing or releasing heat as it undergoes a phase transition between the λ phase and the β phase. The titanium trioxide-based material contains titanium trioxide having a composition of Ti3O5 as a main component, and may be a material containing substituted titanium trioxide in which part of the Ti in titanium trioxide is replaced with another element. Such titanium trioxide-based material can be used as a heat storage and release body for heat exchange and other applications.
[0013] As shown diagrammatically in Figures 1 and 2, the heat storage and release material is made up of an aggregate 1 of heat storage and release titanium oxide crystal grains 2. As shown in an enlarged view in the figure, each crystal grain 2 has an oriented grain structure in which fine crystals 20 of heat storage and release titanium oxide are aggregated with an orientation. Here, "oriented grain structure" refers to a structure in which the fine crystals 20 constituting the crystal grains 2 are arranged so that they are aligned in a specific direction.
[0014] It is preferable that each crystal grain 2 has a structure oriented in one or two specific directions. When the assembly 1 is composed of crystal grains 2 having such an "oriented grain structure", it is possible to reduce the phase transition energy from the β phase to the λ phase of the heat storing and releasing titanium oxide, compared to a crystal assembly having no orientation.
[0015] Preferably, the aggregate 1 includes crystal grains 2 with a twin structure. Specifically, the crystal grains 2 constituting the aggregate 1 are composed of single crystals or polycrystals, and include a crystallite 3 consisting of a single crystal as a minimum unit. Each crystal grain 2 may include a single or multiple crystallites 3, and when multiple crystallites 3 are included, it is desirable that the crystal grain 2 has a twin structure, that is, has orientation in two specific directions. The crystal grain 2 with a twin structure (hereinafter, appropriately referred to as a twin grain 2A) includes multiple paired crystallites 3, and is configured by arranging these crystallites 3 in layers with a crystal interface 31 between them.
[0016] Here, a "twin" refers to a combination of multiple crystals of the same structure, and a crystal grain 2 of a twin structure includes two or more identical crystals that share a specific crystal plane or crystal axis. In the example shown in Fig. 1, a pair of crystal planes 3A and 3B appearing in the cross section of the crystal grain 2 corresponds to multiple paired crystallites 3, and the crystal planes 3A and 3B are alternately arranged with the crystal interface 31 as the common crystal plane to form multiple layers that are roughly parallel to each other.
[0017] At this time, the aggregate 1 has a structure in which oriented grains having orientation in one or two specific directions are assembled by including a crystal grain 2 consisting of a single crystallite 3 or a twin grain 2A consisting of a pair of crystallites 3. It can be confirmed, for example, by observing the crystal orientation using an electron microscope that the crystal grains 2 have orientation and a twin structure.
[0018] Here, the "crystal orientation" refers to the direction of the crystal plane appearing in the cross section of the crystal grain 2, and can generally be determined by crystal orientation analysis using electron backscatter diffraction pattern (hereinafter abbreviated as EBSD) method. In this case, "having orientation" means that the "crystal orientation" of the fine crystals 20 contained in the crystal grain 2 is almost uniform.
[0019] Preferably, the crystal grains 2 constituting the aggregate 1 have a connected grain shape in which the fine crystals 20 are connected with orientation. The fine crystals 20 grow by connecting with each other while being oriented in a specific direction, so that the individual crystallites 3 and even the crystal grains 2 become larger, and it becomes possible to further reduce the phase transition energy. The structure of the crystal grains 2 and the mechanism of the phase transition are considered as follows.
[0020] As shown in Fig. 3, which is a schematic diagram of a portion of the structure of a twin grain 2A, the crystal grain 2 includes a plurality of fine crystals 20 that are granular masses, and adjacent fine crystals 20 may include a connection portion 21 that is a slightly narrow portion between them. The adjacent fine crystals 20 are connected to each other so as to maintain the crystal orientation, and here, a plurality of crystallites 3 having specific crystal faces 3A, 3B are alternately arranged to form a twin. In the case of a crystal grain 2 that does not include a twin, the entire grain is composed of a single crystallite 3.
[0021] In the crystal grains 2 including the twin grains 2A, the individual shapes and number of connections of the fine crystals 20 are arbitrary, and the crystal grains 2 have an irregular connected shape in which a plurality of fine crystals 20 are irregularly connected. It is preferable that a larger number of fine crystals 20 are connected with orientation, which tends to result in oriented grains containing larger crystallites 3. In this case, the crystal grains 2 become larger, thereby reducing the surface energy of the crystal grains 2, and the internal energy is efficiently transmitted, making it possible to reduce the energy required for phase transition.
[0022] In the case of a twin crystal structure, as shown in Fig. 4, a plurality of paired crystallites 3 are arranged in layers with a crystal interface 31 in between, and the pressure applied for phase transition is uniformly and efficiently propagated in the stacking direction via the crystal interface 31, which is a common crystal face. Therefore, it is presumed that the pressure is not dispersed inside the crystal grain 2, and the phase transition proceeds quickly, making it possible to perform the phase transition at a lower pressure.
[0023] 5, the heat-storing and releasing titanium oxide crystal grains 2 are formed, for example, by a reduction reaction of heat-storing and releasing titanium oxide raw material particles 4, in which heat-storing and releasing titanium oxide seed crystals 40 are generated, which grow and further connect to each other. During this process, the heat-storing and releasing titanium oxide crystals generated by the reduction of the raw material particles 4 generate fine crystal grains 20 that are aggregated with orientation, and as the grains grow, they connect to each other to maintain the orientation, thereby generating the crystal grains 2.
[0024] At this time, by adjusting the conditions of the reduction reaction, it is possible to control the generation and orientation of the fine crystals 20, and it is presumed that, for example, the growth of a specific crystal plane is promoted, which makes it easier for twins to be generated during the grain growth process. It is considered that the twins generated under such controlled conditions further grow and connect to each other while maintaining the twin structure, thereby becoming, for example, larger twin grains 2A having specific crystal planes 3A and 3B. The manufacturing method of the heat storage and release material including such crystal grains 2 will be described in detail later.
[0025] In contrast, as shown in FIG. 6 as a comparative embodiment 1, when the conditions of the reduction reaction are not adjusted, the crystal grains 2 have a connected grain shape that does not have orientation. The granular crystals 2 have a configuration in which, for example, a plurality of fine crystals 20 with different crystal orientations are connected in an indefinite manner. Therefore, the orientation is not maintained in the connecting portion 21, and the crystal grains 2 include a plurality of crystallites 3 with different crystal orientations corresponding to each of the plurality of fine crystals 20. In that case, as shown in FIG. 7 as a schematic diagram, it is presumed that the energy required for the phase transition is greater than that of the crystal grains 2 with an oriented grain structure because the pressure applied for the phase transition is easily dispersed in the connecting portion 21 of the granular crystals 2.
[0026] The crystal structure of titanium pentoxide has polymorphism including β-phase, λ-phase, and α-phase. In the temperature range below 460K (i.e., about 187°C), it is in the monoclinic crystal phase (i.e., λ-phase) in which it maintains the state of a paramagnetic metal, and can maintain this state unless it receives an external stimulus. When an external stimulus such as pressure is applied to titanium pentoxide in the λ-phase, it releases the heat that it had stored latent, and undergoes a phase transition to the monoclinic crystal phase (i.e., β-phase) that has the properties of a nonmagnetic semiconductor. When titanium pentoxide is in the β-phase and the temperature is increased, it undergoes a phase transition to the orthorhombic crystal phase (i.e., α-phase) in which it maintains the state of a paramagnetic metal in the temperature range above 460K, and then undergoes a phase transition from the α-phase to the λ-phase when the temperature drops below 460K.
[0027] λ-phase titanium dioxide stores energy as bond energy, and can release it as heat energy when an external stimulus causes a phase transition to the β-phase by breaking and recombining Ti-O bonds. When external energy is applied while the titanium dioxide is in the β-phase, it undergoes a direct phase transition to the λ-phase, or a phase transition to the λ-phase via the α-phase. The λ-phase and α-phase have metallic properties and exhibit lower electrical resistivity than the β-phase, which has semiconductor properties. The external energy is, for example, at least one of electrical energy, thermal energy, and light energy, and the external stimulus is at least one of pressure, light, and electric current.
[0028] The heat storage and release material and its manufacturing method will be described in detail below. In Fig. 2, the powder material that serves as the heat storage and release material is composed of an aggregate 1 of crystal grains 2 that contain a large number of heat storage and release titanium oxide crystals, and each crystal grain 2 has an oriented grain structure. In general, the crystal grains 2, which are primary particles, aggregate to form agglomerated particles 100, which are secondary particles, and the agglomerated particles 100 further aggregate to form the powder material. The crystal grains 2 are amorphous particles made of single crystals or polycrystals, and contain, as the smallest unit, crystallites 3 made of single crystals of heat storage and release titanium oxide.
[0029] The cross section of the aggregate 1 shown enlarged in FIG. 2 shows the aggregated state of the crystal grains 2 inside the aggregate particle 100. The multiple crystal grains 2 contained in the aggregate 1 may each be oriented grains having orientation in one or two specific directions, and the orientation directions of the crystal grains 2 may be the same or different. The crystallites 3 constituting the crystal grains 2 may be single or multiple, and if multiple, they are preferably twin grains 2A containing twin crystals. In that case, a layered structure is observed in which the crystallites 3 corresponding to the two crystal orientations forming the twin crystals are alternately arranged.
[0030] The shape and aggregation state of the crystal grains 2 in the aggregate 1 are based on the results of cross-sectional observation of a powder sample containing agglomerated particles 100 of heat storing and releasing titanium oxide, using a scanning electron microscope (hereinafter, referred to as SEM, as appropriate). Here, in the cross-section of the aggregate 1, which is the observation surface, the space portion 11 where no crystals are observed and the crystal portion are divided by dashed lines, and further, based on the crystal orientation within the crystal portion, each region that becomes a single crystal grain 2 is divided by dashed lines. Also, the regions that contain twins and the regions that do not contain twins are shown with different patterns.
[0031] Specifically, regions where the crystal orientation difference between multiple measurement points measured by the above-mentioned EBSD method is within a predetermined angle (for example, within 5 degrees) can be regarded as having the same crystal orientation, and the grain boundaries and crystal interfaces 31 of the crystal grains 2 can be identified. Furthermore, regions that can be regarded as the same crystal with the same crystal orientation can be regarded as a single crystallite 3, and the orientation state of the crystal grains 2 and the presence or absence of twin formation can be identified. A region containing twins is a layered region where the same crystal orientation appears alternately, and the crystal interfaces 31 that are twin boundaries are indicated by dotted lines.
[0032] The shapes of the crystal grains 2 and twin grains 2A shown in Fig. 2 are merely examples, and any shape can be adopted according to the state of crystal assembly during the growth of the oriented grains. The proportion of twin grains 2A in the crystal grains 2 constituting the aggregate 1 is not particularly limited, but the size of the crystal grains 2 tends to be large under conditions that make it easy for twins to form, and it is preferable that the crystal grains 2 with a twin structure are contained in almost the entire area of the aggregated particle 100 including the aggregate 1.
[0033] When the crystal grain 2 is a twin grain 2A, it has a layered structure in which a plurality of paired crystallites 3 are arranged alternately. The twin grain 2A may have a multi-layer structure containing twins throughout, as long as it contains twins in at least a part of it. In the plurality of twin grains 2A contained in the aggregate 1, the crystal orientations of the paired crystallites 3 may be the same or different. Here, as examples of the paired crystallites 3, a pair of crystal faces 3A, 3B and a pair of crystal faces 3C, 3D that appear on the observation surface are shown separately. The other twin grains 2A also have paired crystal faces, and are integrally bonded via a common crystal face that becomes the crystal interface 31.
[0034] In the twin grain 2A, a pair of crystal faces 3A, 3B are, for example, a region sandwiched between a pair of crystal interfaces 31, each having an anisotropic belt-like or rectangular shape, and are formed alternately and generally parallel to each other. The width of the crystal faces 3A, 3B is arbitrary and may be an appropriate width depending on the manufacturing conditions, etc. The direction in which the crystal faces 3A, 3B are arranged, i.e., the width direction, is also arbitrary and may be different from that of adjacent or nearby other twin grains 2A.
[0035] As shown in FIG. 1, a cross section of a twin grain 2A is enlarged, and specifically, a crystal grain 2 is formed by connecting a large number of fine crystals 20 to each other so that their crystal orientations match. That is, a single crystallite 3 is formed by integrally connecting fine crystals 20 having the same crystal orientation while maintaining the crystal orientation. Alternatively, a plurality of adjacent fine crystals 20 are connected to each other so that the crystal orientations of the adjacent fine crystals 20 are in a twin relationship, and a plurality of paired crystallites 3 are formed across a crystal interface 31. It is preferable that the crystal orientation difference between the paired crystallites 3 is in the range of 90 degrees or more and 180 degrees or less. When it is in this range, a structure in which stress is easily propagated at the contact surface of the plurality of crystallites 3 is formed, which is advantageous for reducing phase transition energy.
[0036] In this case, the shape and size of the crystallite 3 are not particularly limited, and depend on the shape and number of connections of the fine crystals 20 constituting the crystallite 3. It is preferable that the size of the crystal grain 2 including the crystallite 3 is larger, which is advantageous for reducing the phase transition energy. For example, the more connections of the fine crystals 20, the larger the size of each crystallite 3 and the larger the size of the crystal grain 2. In the case of the twin grain 2A, the more the number of crystallites 3 arranged in a layered form, the larger the size of the crystal grain 2 including the twin.
[0037] Preferably, the crystallites 3 constituting the crystal grains 2 have a porous connected shape in which a large number of fine crystals 20 are irregularly connected with voids 10. As described above, it is presumed that the heat storing and releasing titanium oxide seed crystals 40 are bonded to maintain orientation while growing as grains, so that the fine crystals 20 are three-dimensionally bonded via the connecting parts 21 to form oriented grains having a porous shape and including a large number of voids 10. Here, the shape and size of each fine crystal 20 are not particularly limited, and the boundaries between adjacent fine crystals 20 and the shape of the connecting parts 21 do not necessarily have to be clear.
[0038] In addition, it is desirable that the entire crystal grains 2 consisting of oriented grains having a porous shape have a smooth surface. Specifically, a large number of fine crystals 20 and connecting parts 21 are connected by a smooth curved or flat surface, and a crystallite 3 having a porous connected shape is formed. In general, it is considered that the surface of the crystal grains 2 becomes smooth as the production of heat-storing and releasing titanium oxide progresses due to the reduction reaction of the raw material particles 4, and the smoothness allows pressure to be transmitted evenly and is less likely to cause destruction due to stress, making it possible to efficiently carry out the phase transition of the heat-storing and releasing titanium oxide.
[0039] In the twin grain 2A shown in Fig. 1, the arrangement of the paired crystal faces 3A, 3B and the shape of the corresponding crystallite 3 are merely examples, and each crystallite 3 may have a connected shape formed by an arbitrary number of fine crystals 20 connected in an arbitrary direction. Here, a large number of fine crystals 20 are connected via connecting parts 21 in the direction along the crystal interface 31, so that belt-like crystal faces 3A, 3B are formed between adjacent crystal interfaces 31. In addition, by arranging the fine crystals 20 including twins along the crystal interface 31, these crystal faces 3A, 3B are also connected in the width direction, resulting in a porous shape having orientation in specific two directions as a whole.
[0040] The same is true for crystal grains 2 that do not include twins, and have a similar connected shape, except that fine crystals 20 of the same crystal orientation form a single crystallite 3 and layered crystallites 3 are not formed. The individual fine crystals 20 are, for example, flake-like, scale-like, thin plate-like, etc., and when they are connected in roughly one direction, they become connected shapes such as leaf-like, string-like, column-like, etc. In addition, when the fine crystals 20 are further connected in a direction different from the connecting direction, for example, so as to branch out from multiple places, the area with the same crystal orientation spreads. As a result, connected granular crystallites 3 such as dendrites and nets are formed, and the size of the crystallites 3 becomes larger.
[0041] As described above, the multiple fine crystals 20 each have an appropriate shape and size formed by grain growth of the seed crystals 40 of the heat storing and releasing titanium oxide. Not only are such fine crystals 20 connected with an orientation, but they also form twins, resulting in a larger oriented grain structure. It is presumed that by forming an aggregate 1 of crystal grains 2 including such twin grains 2A, it becomes possible to efficiently transmit the energy required for the phase transition of the heat storing and releasing titanium oxide.
[0042] For example, the presence or absence of orientation and the mechanism of phase transition in the shape examples shown in Figs. 3 and 5 are considered as follows. Specifically, the twin grain 2A shown in Fig. 3 has a connected shape including a plurality of fine crystals 20, which is mainly composed of crystal faces 3A, and a plurality of crystal faces 3B are arranged so as to penetrate a plurality of places (e.g., three places) in the center where a plurality of (e.g., six) fine crystals 20 are gathered. The plurality of crystal faces 3B are, for example, substantially parallel belt-like shapes extending in the main connection direction of the plurality of fine crystals 20 as the longitudinal direction. When a plurality of fine crystals 20 adjacent to each other in the longitudinal direction are included, the plurality of crystal faces 3B may be formed so as to be continuous in the longitudinal direction across the plurality of fine crystals 20. In the peripheral portion of the connected grain including a plurality of fine crystals 20, the crystal faces 3A surrounded by the crystal interface 31 and the grain boundaries of the granular crystals 2 are irregular in shape along the substantially arc-shaped fine crystals 20.
[0043] As shown by the arrows in Fig. 4, when pressure for phase transition is applied to the crystal grain 2 having the structure shown in Fig. 3, the pressure propagates through the inside of the crystal grain 2 and the phase transition progresses. At this time, the crystal grain 2 is a twin grain 2A, and contains paired crystallites 3, which facilitates pressure propagation. That is, in the twin grain 2A, when some crystallites 3 subjected to pressure undergo phase transition, the pressure propagates to the adjacent crystallites 3 one after another. At this time, the phase transition is accompanied by a volume change, so that stress is propagated uniformly through the multiple parallel crystal interfaces 31.
[0044] As a result, the pressure is not dispersed inside the crystal grains 2, but is quickly propagated. In addition, since the interfacial energy of the crystal interface 31, which is the contact surface of the twin crystals, is relatively small, the stress is efficiently propagated, and the phase transition progresses. As a result, it is presumed that it is possible to cause the phase transition of the entire crystal grains 2 at a lower pressure. Furthermore, since the crystal grains 2 including such twin grains 2A are aggregated to form the orientation region 10, it is possible to reduce the phase transition pressure, which is the energy required for the phase transition of the aggregate 1.
[0045] On the other hand, as shown in FIG. 6 as Comparative Form 1, when the crystal grains 2 of the heat storage and release titanium oxide are connected grains without crystal orientation, for example, a plurality of fine crystals 20 each become crystallites 3, forming a randomly bonded polycrystal. That is, the crystal grains 2 are randomly oriented connected grains including a plurality of crystallites 3 with different crystal orientations, and the orientation is not maintained at the connection portion 21 with the adjacent fine crystals 20. In that case, large crystallites 3 or twin crystals with aligned crystal orientations are not formed, and a plurality of crystal interfaces 31 are formed between the adjacent crystallites 3. Therefore, the number of crystallites 3 is large compared to the size of the crystal grains 2, and each crystallite 3 tends to be small.
[0046] At this time, as shown by the arrows in Fig. 7, when pressure for phase transition is applied to the crystal grains 2, after the part receiving the pressure undergoes phase transition, the pressure tends to disperse at the crystal interfaces 31 with the adjacent crystallites 3. Therefore, it is presumed that the pressure does not propagate quickly inside the granular crystals 2, making it difficult for the phase transition to proceed. Due to such differences in crystal structure, when the crystal grains 2 are included, the energy required for phase transition is greater than that of the aggregate 1 including the crystal grains 2 with an oriented grain structure.
[0047] Here, the "phase transition pressure" refers to the pressure for causing a phase transition of heat-storing and releasing titanium oxide from the λ phase to the β phase, and is expressed as the pressure required for the phase transition from the λ phase to the β phase when, for example, a heat storage and release material containing heat-storing and releasing titanium oxide is placed in a pressurizable container and pressure is applied using a uniaxial press or the like. When pressure is used as the energy for the phase transition, the configuration of the heat storage body using the heat storage and release material and the configuration of the device for the phase transition of the heat storage body can be made relatively simple.
[0048] The heat storage and release material containing the heat storage and release titanium oxide obtained in this way can be used as a heat storage body that absorbs and stores thermal energy such as exhaust heat from a system, and releases the heat at the desired timing, enabling efficient heat exchange. In addition, since heat storage and release titanium oxide utilizes a phase transition between solids, it has the advantages of being easy to handle as a heat storage body, having good controllability during heat storage and release, being capable of long-term storage at low temperatures, and being able to be manufactured from inexpensive raw materials.
[0049] Preferably, the heat storage and release titanium oxide contained in the heat storage and release material is 90% or more by mass. If the proportion of crystal phases other than the heat storage and release titanium oxide trititanium pentoxide-based material increases in the crystal grains 2, this may affect the propagation of pressure within the crystal grains 2. More preferably, the heat storage and release titanium oxide should be 95% or more by mass, which facilitates pressure propagation and is advantageous for reducing phase transition pressure.
[0050] In addition, the size of the crystal grains 2 is preferably 50 μm or more in terms of the area-based average grain size based on the crystal orientation analysis by the EBSD method. The area-based average grain size is the 50% value of the grain size distribution based on the area when the crystal grains 2 are regarded as circles, and as described later, the grain boundaries of the crystal grains 2 having an oriented grain structure are specified from the results of the crystal orientation analysis, and the measurement results of the area can be calculated as a value converted into a circle. When the average grain size of the crystal grains 2 having the oriented grain structure is 50 μm or more, pressure propagation easily progresses, and the phase transition to the β phase is possible at a lower pressure than before. From the viewpoint of reducing the phase transition pressure, the average grain size of the crystal grains 2 including the twin grains 2A is larger, and for example, 100 μm or more is more preferable. From the viewpoint of reducing the cost and time required for manufacturing, for example, the average grain size is preferably about 140 μm or less.
[0051] Next, a method for producing a heat storage and release material containing heat storage and release titanium oxide will be described. In FIG. 5, the heat storage and release material including crystal grains 2 of heat storage and release titanium oxide can be manufactured by firing raw material particles 4 including titanium dioxide in a reducing atmosphere to generate fine crystal grains 40 of a titanium pentoxide-based material, and then allowing the grains to grow. The manufacturing process includes (1) a raw material preparation process, (2) a reduction and firing process, and (3) a cooling process, and the heat storage and release material is obtained through the manufacturing process. Preferably, in the reduction and firing process (2), the raw material particles 4 are rocked so that a sufficient amount of reducing gas including hydrogen is supplied around each raw material particle 4, as shown by the arrows in the figure. This allows the raw material particles 4 to come into contact with a sufficient amount of reducing gas while suppressing agglomeration of the raw material particles 4, and makes it possible to promote the growth of the crystal grains 2 including the twin grains 2.
[0052] Specifically, in the (1) raw material preparation step, a powder material containing titanium dioxide is prepared as the raw material for the heat-storing and releasing titanium oxide. In general, titanium dioxide is known to have a rutile or anatase crystal structure, and titanium dioxide powder containing either of these or a mixture thereof can be used as the raw material powder. Preferably, titanium dioxide powder having a rutile crystal structure is used. When the heat-storing and releasing titanium oxide to be produced contains substituted trititanium pentoxide, titanium dioxide powder to which a material containing a substitution element has been added can be used as the raw material powder.
[0053] The size of the titanium dioxide powder to be the raw material particles 4 is not necessarily limited, but is preferably within the range of 50% particle size (D 50 ) is preferably 0.5 μm or more. In that case, it is possible to promote the reduction reaction of the titanium dioxide as the raw material while suppressing the raw material cost. Preferably, the average particle size is 1.0 μm or more. From the viewpoint of uniformly promoting the reduction reaction of titanium dioxide throughout the entire powder material including the raw material particles 4, the average particle size is preferably 5 μm or less. Preferably, the average particle size is 4 μm or less.
[0054] (2) In the reduction firing step, raw material powder including titanium dioxide raw material particles 4 is heated and brought into contact with a reducing gas including hydrogen while being contained in a container not shown in the figure, thereby causing a reduction reaction. Preferably, the contained raw material powder is brought into contact with the reducing gas introduced into the movable container while being rocked using a firing device equipped with a rocking device. For example, the raw material particles 4 can be rocked or vibrated by rocking the movable container.
[0055] 8, specifically, a manufacturing apparatus 200 can be used in which a movable container 201 is cylindrical, a gas inlet 301 and a gas outlet 302 are provided at both ends, and the movable container 201 is rotatable about its axis. In this case, by arranging a heating unit 203 around the container, the raw material powder inside is heated evenly, and by constantly rocking the container, the reducing gas passing through the inside of the movable container 201 can be evenly supplied around each raw material particle 4.
[0056] The reducing gas may be hydrogen gas or a mixed gas obtained by mixing hydrogen gas with an inert gas such as nitrogen gas. The hydrogen concentration in the reducing gas may be suitably selected within a range of 75% by volume or more and 100% by volume or less, and the reduction reaction of the raw material powder by hydrogen may proceed suitably. The hydrogen concentration is preferably 80% by volume or more. The supply of the reducing gas is preferably adjusted so that the reduction gas flow rate in the internal space of the movable container 201 is usually 1 L / min or more. This allows the supply of hydrogen necessary for the progress of the reduction reaction to the periphery of the raw material powder, and preferably, the gas flow rate is 2 L / min or more from the viewpoint of supplying sufficient hydrogen. In addition, from the viewpoint of suppressing the supply of excessive hydrogen, the gas flow rate is preferably 4 L / min or less.
[0057] The firing temperature is preferably 1250°C or higher in order to facilitate the hydrogen reduction reaction of the raw material powder. Preferably, the firing temperature is 1300°C or higher in order to enhance the orientation of the crystals produced. In addition, from the viewpoint of the heat resistance of the manufacturing apparatus 200, the firing temperature is preferably 1600°C or lower, preferably 1500°C or lower. The holding time at the firing temperature can be, for example, 0.5 hours or more, and is appropriately selected depending on the firing temperature. If the holding time is less than 0.5 hours, there is a risk of insufficient reduction, and preferably, it can be 2 hours or more. Specifically, the higher the firing temperature or the longer the holding time, the more the connection of the fine crystals 20 progresses, and the size of the crystal grains 2 tends to become larger. However, if the firing temperature is high or the holding time is long, there is a risk of excessive reduction, and it is desirable to appropriately adjust the holding time depending on the firing temperature, for example, within a range of 10 hours or less, preferably 5 hours or less.
[0058] Here, the movement of the movable container 201 may be any movement capable of imparting a "rocking" motion in which the raw material particles 4 rock in any direction. The "rocking" includes "vibration" in a specific direction or periodically. Specifically, the movement of the movable container may include a rotational motion, a pivoting motion, a reciprocating motion in a specific direction, a rocking motion in any direction, and other movements. As a result, the raw material particles 4 do not remain in a fixed position in the internal space 202 of the movable container 201 but rock arbitrarily, so that aggregation of the raw material particles 4 is suppressed, the opportunities for contact with the reducing gas are increased, and the reduction reaction is promoted.
[0059] The movable container 201 containing the raw material powder may be configured to be displaceable by an attached drive unit and to be rotated, turned, vibrated, or the like. This allows the raw material powder contained therein to be "rocked" so that it moves while swinging in any direction, or "vibrated" so that it periodically swings in a specific direction, while the reducing gas is circulated around it. The movable container 201 is preferably a heat-resistant container into which the reducing gas can be introduced and discharged, and is configured to be equipped with a heater or the like serving as the heating unit 203 so that the raw material powder inside can be heated to a predetermined temperature.
[0060] Specifically, (2) the reduction firing process includes a gas supply process for supplying a reducing gas to the movable container 201, a temperature raising process for raising the temperature of the movable container 201, a rotation driving process for rotating the movable container 201, a raw material introduction process for introducing raw material powder into the movable container 201, and a temperature maintaining process for maintaining the movable container 201 at a predetermined temperature for a predetermined time. By carrying out these processes in this order, the temperature can be raised quickly while the individual raw material particles 4 are swung to increase the opportunity for contact with hydrogen, thereby accelerating the reduction reaction of titanium dioxide.
[0061] As a result, as shown in step (2-1), a reduction reaction of titanium dioxide produces microcrystalline grains 40 of trititanium pentoxide. At this time, a sufficient amount of reducing gas is supplied to the entire surface of each raw material particle 4 while suppressing aggregation of the raw material powder, which facilitates the production of microcrystalline grains 40 made of single crystals or polycrystals including twin crystals. It is presumed that these microcrystalline grains 40 then gather together while maintaining the crystal orientation and grow to produce crystal grains 2 including twin grains 2A, as shown in step (2-2).
[0062] At that time, it is presumed that a difference in reactivity with hydrogen occurs depending on the crystal face exposed on the surface of the raw material particle 4, making it easier for twins to form, and that the highly reactive parts grow into grains and tend to become amorphous, flaky crystals. It is considered that, as hydrogen is continuously supplied to such flaky fine crystal grains 40 containing twins, the highly reactive parts grow further into grains, and that the multiple crystals 40 connect to maintain the twins and grow into larger twin grains 2A.
[0063] Also, the movable container 201 can be tilted to oscillate the supplied raw material powder and to be movable in the tilted direction (i.e., the axial direction X). It is preferable to make the direction of movement of the raw material powder and the direction of gas introduction opposite. In this way, the raw material particles 4 are subjected to a force in the tilted or rotating direction and move gradually while being moderately oscillated, so that aggregation between particles is suppressed and a sufficient amount of reducing gas is stably supplied around each particle. In this case, the raw material powder comes into sufficient contact with the reducing gas at a high temperature, the reduction reaction of titanium dioxide progresses, and the growth of the crystallites 3 of the resulting titanium pentoxide is promoted, resulting in crystal grains 2 having a relatively large grain size and orientation.
[0064] The movable container 201 may be of a continuous type, in which a raw material powder supply port 204 is provided at the end on the gas outlet 302 side, and raw material powder is continuously charged and passed through the internal space 202, or of a batch type, in which a predetermined amount of raw material powder is charged and taken out after a predetermined holding time has elapsed. In the former case, the inclination angle of the movable container 201 and the like are adjusted so that the raw material powder reaches the outlet 205 provided at the end on the gas inlet 301 side after a predetermined holding time. The main body of the movable container 201, except for both ends, is accommodated inside the housing 300 together with the heating unit 203, and is rotatably supported by a bearing unit fixed to the outside of the housing 300. The rotation speed of the movable container 201 is controlled by a rotation drive unit 303 attached to the bearing unit so that the raw material powder in the internal space 202 is in an appropriate oscillating state.
[0065] By going through each of these steps (1) raw material preparation step and (2) reduction and firing step, a heat storage and release material containing crystal grains 2 of heat storage and release titanium oxide can be produced. Then, in (3) cooling step, the heat storage and release material obtained in (2) reduction and firing step is taken out and allowed to cool to room temperature in a cooling section. The configuration for taking out and cooling is not particularly limited, and for example, a space section that is continuous with the outlet 205 and extends in the vertical direction can be used as the cooling section, and the material can be air-cooled or naturally cooled while falling under its own weight. EXAMPLES
[0066] Example 1 Based on the above-mentioned manufacturing process, a heat storage and release material was manufactured by the following method. First, in a raw material preparation process, titanium dioxide powder was prepared as the raw material for the heat storage and release titanium oxide. Next, in a reduction and firing process using a manufacturing apparatus 200 shown in FIG. 8, a reduction treatment was carried out at a predetermined firing temperature to obtain a powder material that would become an aggregate 1 of crystal grains 2 of titanium pentoxide. The titanium dioxide powder used as the raw material had a cumulative 50% particle size (D 50 ) having an average particle size of 2.5 μm was used.
[0067] In the manufacturing apparatus 200, hydrogen gas was introduced into a cylindrical furnace serving as a movable container 201 from an inlet 301 at one end toward an outlet 302 at the other end, replacing the internal space 202 with a hydrogen gas atmosphere. The movable container 201 was heated and heated by a heating unit 203, and the movable container 201 was rotated and driven by a driving unit 304. In this state, raw material powder was fed from a supply port 204 at the other end of the movable container 201, and reduction firing was performed in the internal space 202 at a predetermined firing temperature and for a predetermined holding time. The conditions in the reduction firing process were as follows: Reducing gas: Hydrogen gas (100% by volume) Gas flow rate: 2L / min Firing temperature: 1300℃ Retention time: 3 hours
[0068] Thereafter, the generated heat-storing and releasing titanium oxide powder was taken out from the outlet 205 of the movable container 201, and was allowed to cool to room temperature in a cooling process. The obtained heat-storing and releasing titanium oxide powder sample was subjected to shape observation using an electron microscope. Figure 9 shows SEM observation images (magnifications x600, x5000) showing the appearance of the obtained powder sample and the state of crystal aggregation in a part of it.
[0069] As shown in the left diagram of Fig. 9, the obtained powder contains agglomerated particles 100 in which crystals of heat storage and release titanium oxide are aggregated, and each agglomerated particle 100 has a generally spherical or cylindrical shape with rounded edges. Also, as shown in the right diagram of Fig. 9, the agglomerated particles 100 are formed by assembling a large number of fine crystals 20 so as to be three-dimensionally irregularly connected, and have a porous shape in which a large number of voids 10 are formed between adjacent or nearby fine crystals 20 via narrow connecting parts 21. It was confirmed that each of the large number of fine crystals 20 has a smoothly curved or planar surface, and the entire surface including the connecting parts 21 formed between adjacent fine crystals 20 is formed with a smooth curved surface.
[0070] In addition, the crystal orientation of the obtained powder was measured and analyzed using the EBSD method with a SEM. First, the obtained powder was embedded in resin to prepare a sample for the measurement. The surface was mechanically polished using an automatic polishing machine, then finish polished by vibration polishing, and the polished surface to be measured was carbon sputtered to create a measurement sample.
[0071] For this measurement sample, analysis was performed based on the EBSD pattern obtained when irradiating it with an electron beam under the following conditions: The electron beam was moved across the measurement surface in a specified step width, the diffraction pattern generated was detected, information on the crystal orientation at each measurement point was obtained, and an IPF (Inverse Pole Figure) map shown in Figure 10 was created. Acceleration voltage: 15 kV Irradiation current: 5nA Sample tilt: 70deg. Acquisition rate: 31.19Hz
[0072] In Fig. 10, the IPF map is color-coded based on a predetermined inverse pole figure color scale, and is shown here in black and white shading for convenience. Also, by regarding the points where the orientation difference between adjacent measurement points exceeds a predetermined angle (here, 5 degrees) as crystal grain boundaries, the grain boundaries of crystal grains 2 are specified and shown by white dotted lines in the figure. The black parts in the figure are parts without crystals, and it can be seen that each crystal grain 2 is formed by connecting or aggregating many tiny granular crystals, and has an overall amorphous shape.
[0073] It was also confirmed that the multiple crystal grains 2 have a layered structure, with layers of two types of crystal orientations arranged alternately inside. It was confirmed that these two types of crystal orientations form twin grains 2A including crystallites 3 that form twins at 110 degrees to 130 degrees in all of the crystal grains 2. The multiple crystallites 3 in the twin grains 2A are made up of a series of minute granular crystals, and have a rough band-like or rectangular shape as a whole, with the structure being stacked approximately parallel to one another in the width direction of the crystallites 3.
[0074] Thus, each crystal grain 2 gathered on the measurement surface has an oriented grain structure with a uniform crystal orientation. Therefore, crystal orientation analysis was performed on any measurement surface using the EBSD method, and each identified crystal grain 2 was considered to be a circle, and the crystal grain size was calculated by converting the area measurement results into a circle value. From the distribution of the calculated crystal grain size and area ratio, the value at which the integrated value was 50% was taken as the average grain size. The area-based average grain size calculated by this method was 121 μm.
[0075] In addition, the crystal phase of the obtained powder was identified by X-ray diffraction (hereinafter, appropriately referred to as XRD). To identify the crystal phase, a powder X-ray diffraction device (device name: smartLAB) manufactured by Rigaku Corporation was used, and the obtained XRD pattern confirmed that a heat-storing and releasing titanium oxide including a λ-phase peak (i.e., 2θ=32.17°) and a β-phase peak (i.e., 2θ=28.35°) had been produced. Note that no products other than the heat-storing and releasing titanium oxide, trititanium pentoxide, were confirmed.
[0076] Next, the following heat storage and release test was performed using the obtained heat storage and release material, and the phase transition pressure was calculated. First, the heat storage and release titanium oxide powder was placed in a crucible and heated in an electric furnace at 350°C for 2 hours to cause a phase transition to the λ phase. Then, the heat storage and release titanium oxide powder was filled into a specified mold and pressed using an autograph to perform a heat release test in which the phase transition was from the λ phase to the β phase, and the phase transition pressure was calculated. Specifically, the applied pressure was calculated from the mold area on the pressing surface and the pressure applied by the autograph, and the λ phase ratio in the heat storage and release titanium oxide before and after pressing was measured using the above-mentioned XRD device.
[0077] The λ phase ratio is calculated by measuring the peak intensity of the λ phase and the peak intensity of the β phase from the obtained XRD pattern, and using the known formula 1 below. Based on this, the applied pressure at which the phase transition to the λ phase was confirmed was taken as the phase transition pressure (unit: MPa). Formula 1: λ phase ratio = {(λ phase peak intensity) × 28.2) / [(λ phase peak intensity) × 28.2) + (β phase peak intensity) × 31.0)]} × 100 At this time, the applied pressure at which the phase transition to the β phase is confirmed from the change in the λ phase ratio can be taken as the phase transition pressure (unit: MPa). The phase transition pressure measured by this method was 40 MPa.
[0078] Example 2 A heat storage and release material was produced and evaluated in the same manner as in Example 1. A powder containing heat storage and release titanium oxide was produced in the same manner, except that titanium dioxide powder was used as the raw material and the firing temperature and firing time in the reduction firing step were changed as follows. Reducing gas: Hydrogen gas (100% by volume) Gas flow rate: 2L / min Firing temperature: 1300℃ Retention time: 0.5 hours
[0079] For the obtained heat storage and release material, crystal orientation analysis based on the EBSD pattern was performed in the same manner as in Example 1 to examine the structure and orientation of the crystal grains 2. In addition, the production rate of trititanium pentoxide, which is the heat storage and release titanium oxide (i.e., the Ti3O5 rate), was calculated based on the XRD pattern, and a heat storage and release test was performed to calculate the phase transition pressure. The table in FIG. 11 shows the calculation results and a mapping image of the IPF based on the crystal orientation analysis of the crystal grains 2, together with the results of Example 1.
[0080] (Comparative Examples 1 and 2) For comparison, a heat storage and release material was produced and evaluated under the following production conditions, which were different from those of Example 1. In Comparative Example 1, the same raw materials as those of Example 1 were used, and in the production apparatus 200 used in the reduction and firing step, the cylindrical furnace to which the titanium dioxide powder was supplied was not operated, but the powder was reduced by contacting the powder with a reducing gas to produce a powder containing heat storage and release titanium oxide. Reducing gas: Hydrogen gas (100% by volume) Gas flow rate: 2L / min Firing temperature: 1300℃ Hold time: 2 hours
[0081] In Comparative Example 2, the same raw materials as in Example 1 were used, and a powder containing heat-storing and -releasing titanium oxide was produced in the same manner, except that the firing temperature and firing time in the reduction firing step were changed as follows. Reducing gas: Hydrogen gas (100% by volume) Gas flow rate: 2L / min Firing temperature: 1400℃ Retention time: 5 hours
[0082] For the heat storage and release materials obtained in Comparative Examples 1 and 2, crystal orientation analysis based on the EBSD pattern was performed in the same manner as in Example 1 to examine the structure and orientation of the crystal grains 2. In addition, the Ti3O5 ratio was calculated based on the XRD pattern, and a heat storage and release test was performed to calculate the phase transition pressure. The table in FIG. 11 shows the calculation results and a mapping image of the IPF based on the crystal orientation analysis of the crystal grains 2. The mapping image of the IPF is shown separately in FIG. 12. The area-based average grain size of Example 2 was 67 μm, and the area-based average grain size of Comparative Examples 1 and 2 was 2.4 μm and 157 μm, respectively.
[0083] In the IPF mapping image of Fig. 12, the crystal grain 2 of Example 1 has an oriented grain structure in which twin crystals of paired crystal orientations are observed throughout the region where the granular crystals are gathered. In contrast, the crystal grain 2 of Comparative Example 1 has a grain structure in which many crystal orientations are observed and the orientation of the granular crystals is random, resulting in an overall grain structure that has no orientation. Therefore, the phase transition pressure of Comparative Example 1 is high at 70 MPa, while the phase transition pressure of Example 1 is significantly reduced to 40 MPa.
[0084] In addition, it was confirmed that the crystal grains 2 of Example 2 have an oriented grain structure, including a region in which adjacent or nearby granular crystals are aligned throughout. As a result, the phase transition pressure is 60 MPa, which is higher than that of Example 1, but lower than that of Comparative Example 1, and is effective in reducing the phase transition pressure. Note that, although granular crystals including twins are partially observed in the crystal grains 2 of Example 2, twin grains 2A of a twin structure in which paired crystallites 3 are clearly formed were not observed.
[0085] On the other hand, in the crystal grains 2 of Comparative Example 2, granular crystals with the same crystal orientation were connected and a structure in which paired crystallites 3 were formed in layers was observed, but the Ti3O5 ratio was 85%. At this time, the phase transition pressure of Comparative Example 2 was 90 MPa, which was higher than that of Comparative Example 1, and it is presumed that the longer the firing time, the larger the average grain size was, but the more likely it was to become over-reduced, and the increase in compositions other than Ti3O5 made the phase transition more difficult.
[0086] As shown in FIG. 12, an SEM observation image (magnification x 10,000) is shown as Comparative Example 3. When the supply of reducing gas is insufficient or the firing temperature or firing time is insufficient, the reduction is insufficient and the surface crystal grains 2 tend to have a rough surface. In other words, the surface does not become smooth. In that case, pressure is less likely to be applied uniformly compared to a smooth surface, and there is a risk that the surface may become the starting point of stress-induced destruction. In contrast, it is believed that pressure is more likely to be applied uniformly to crystal grains 2 having a smooth surface, and the bias of the applied pressure is suppressed, thereby suppressing the variation in the phase transition pressure of the particles.
[0087] Furthermore, as shown in Fig. 13, heat-storing and -releasing titanium oxide powders having various average particle sizes were produced by changing the firing temperature and firing time in the reduction firing step in the same manner as in Example 1. The obtained heat-storing and -releasing titanium oxide powders were subjected to a heat storage and release test similar to that in Example 1 to investigate the relationship between the average particle size and the phase transition pressure. The results are shown in Fig. 13 together with Examples 1 and 2 and Comparative Examples 1 and 2.
[0088] Specifically, by adjusting the firing temperature to 1300°C to 1400°C and the firing time to 0.5 to 5 hours, a heat storage and release material containing crystal grains 2 with an area-based average grain size of about 50 μm to about 140 μm was obtained. It was confirmed that all of these crystal grains 2 had a Ti3O5 ratio of 100 mass% and had an oriented grain structure. From the results in FIG. 13, it can be seen that, preferably, by adjusting the average grain size of the crystal grains 2 to be in the range of 50 μm to 140 μm, it is possible to improve the phase transition pressure while suppressing over-reduction.
[0089] From the above results, it is possible to efficiently carry out a phase transition from the λ phase to the β phase and reduce the phase transition energy by having an oriented grain structure containing fine crystals 20 of heat storage and release titanium oxide in the crystal grains 2 constituting the heat storage and release material aggregate 1. Such a heat storage and release material can be obtained by supplying a sufficient amount of reducing gas containing hydrogen around the raw material particles 4 and growing the fine crystals 20 so that they are oriented and connected, and can be manufactured, for example, by using a firing device equipped with a rocking device.
[0090] The present invention is not limited to the above-mentioned embodiments, and can be applied to various embodiments without departing from the gist of the present invention. In addition, the manufacturing method and manufacturing device of the heat storage and release material are only examples, and are not limited to the methods and devices described in the embodiments. In addition, the heat storage and release material is applied to the heat exchanger of various systems as a material for a heat storage body, but is not particularly limited and can be used for any purpose. [Explanation of symbols]
[0091] 1 aggregate 2. Grains 20 Fine crystal 21 Connecting part 2A Twin grain 3. Crystallites 3A, 3B crystal plane 10 void 11 Space section 100 Agglomerated particles
Claims
1. A heat storage and release material comprising an aggregate (1) of crystal grains (2) of heat storage and release titanium oxide, The heat-storing and dissipating titanium oxide is a titanium pentoxide-based material that stores or dissipates heat as it undergoes a phase transition between a lambda phase and a beta phase, The heat storage and release material has an oriented grain structure in which the crystal grains are an aggregate of fine crystal grains (20) of the heat storage and release titanium oxide having an orientation.
2. The heat storage and release material according to claim 1 , wherein the crystal grains have an orientation in one or two specific directions.
3. The heat storage and release material according to claim 2 , wherein the aggregate includes the crystal grains having a twin crystal structure.
4. The heat storage and release material according to claim 3, wherein the crystal grains of the twin structure are constituted by a plurality of paired crystallites (3) arranged in a layered manner.
5. The heat storage and release material according to claim 1 or 2, wherein the crystal grains have a connected grain shape in which the fine crystals are connected together with an orientation.
6. The heat storage and dissipation material according to claim 5 , wherein the fine crystals have a smooth surface.
7. 3. The heat storage and release material according to claim 1, wherein the crystal grains have an area-based average grain size of 50 μm or more based on crystal orientation analysis by electron backscatter diffraction pattern analysis.
8. 3. The heat storage and release material according to claim 1, wherein the content of the heat storage and release titanium oxide in the aggregate is 90 mass % or more.
Citation Information
Patent Citations
Titanium oxide material, heat storage / radiation device, and method for producing titanium oxide material
JP2021008390A