High-strength steel pipe for fitting with superior moldability
A high-strength steel pipe with a tailored hardness distribution and chemical composition addresses the challenge of stable diameter reduction and seismic resistance, enhancing the formability and earthquake resistance of overhead line columns.
Patent Information
- Application Number
- JP2023063220
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
Existing high-strength steel pipes used in overhead line columns face challenges in achieving both high seismic resistance and stable diameter reduction due to increased processing loads, which can exceed the capacity of molding machines, especially when transitioning to 590 MPa class or higher strengths.
A high-strength fitting steel pipe with a specific hardness distribution, ranging from 150Hv to 185Hv in certain sections, and a controlled chemical composition to ensure both formability and strength, allowing for stable diameter reduction without requiring jigs.
The solution enables stable diameter reduction processing even at high strengths, ensuring excellent earthquake resistance and formability, thereby maintaining the integrity and functionality of the steel pipes.
Smart Images

Figure 2024150015000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength steel pipe for fitting, which has excellent formability and is provided with a reduced length portion for fitting and is used, for example, as a high-strength overhead line pole for railways, etc. [Background technology]
[0002] Steel pipes used for overhead poles (for example, with an outer diameter of 200 to 500 mm and a wall thickness of 6.0 to 16.0 mm) are required to be earthquake-resistant due to the effects of recent major earthquakes. One of the ways to meet this demand is the overhead pole with an interlocking structure, which is a composite pole with an interlocking structure and has excellent earthquake resistance for two reasons: the upper pipe can be made lighter and resonance can be suppressed. In the case of an interlocking structure, the lower pipe, which is subjected to a moment at the ground level, determines the earthquake resistance, and although pipes up to 540 MPa in strength have been used up to now, a strength level of 590 MPa or higher has been required to further improve earthquake resistance. The interlocking structure requires the diameter of the mating part to be reduced, but there was a problem that as the strength increases, the processing load increases and molding becomes unstable, or the molding load exceeds the capacity of the molding machine, making molding impossible.
[0003] Patent Document 1, which is a conventional technique, describes composite columns of steel pipes in terms of their composition, dimensions, plating, etc., but does not describe aspects of improving formability or the hardness distribution of steel pipes. Patent Document 2 describes high-strength electric resistance welded steel pipes in terms of their composition, dimensions, strength, etc., and also describes fitting steel pipes together using a jig. However, there is no description of a fitting structure that fits without a jig, or of the diameter reduction process required for this. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5858816 [Patent Document 2] Patent No. 6841392 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention provides a high-strength steel pipe for fitting, which has excellent formability and enables easy diameter reduction of the mating portion of a fitting structure. [Means for solving the problem]
[0006] In order to solve this problem, the inventors clarified the relationship between hardness and forming load, and by providing an appropriate hardness distribution to the tapered portion that serves as the fitting portion, it became possible to achieve both formability and strength. (1) A steel pipe using a steel containing, in mass%, C: 0.05-0.20%, Si: 0.03-0.40%, Mn: 1.00-2.00%, P: 0.000-0.030%, S: 0.000-0.010%, Al: 0.005-0.500%, Nb: 0.010-0.060%, N: 0.0003-0.0060%, the remainder being Fe and unavoidable impurities, and wherein, when the length of a first taper portion that becomes a fitting portion is taken as 100%, before diameter reduction processing, This high-strength fitting steel pipe has excellent formability and a tensile strength of 500 MPa or more, characterized in that the hardness is 150 Hv to 185 Hv at least in the range of 0% to 36% from the pipe end, the hardness is 185 Hv or more in the range of 100% to 120% from the pipe end, and the difference in average hardness between the base material and the welded part is less than 20 Hv in the range of 0% to 120% from the pipe end. (2) In (1), further comprising, by mass%, Ti: 0.000 to 0.200%, B: 0.0000 to 0.0050%, Cu: more than 0.00% and not more than 1.00%, Ni: more than 0.00% and not more than 1.00%, Cr: more than 0.00% and not more than 1.00%, Mo: more than 0.00% and not more than 0.50%, V: more than 0.00% and not more than 0.20%, W: more than 0.00% and not more than 0.10%. The present invention relates to a high-strength steel pipe for fitting, which has excellent formability and a tensile strength of 500 MPa or more, and is characterized in that it uses steel containing one or more of the following: Ca: more than 0.0000% and not more than 0.0200%, Mg: more than 0.0000% and not more than 0.0200%, Zr: more than 0.0000% and not more than 0.0200%, and REM: more than 0.0000% and not more than 0.0200%. Effect of the Invention
[0007] According to the present invention, it is possible to stably reduce the diameter even when the steel pipe has high strength, and it is possible to provide a high-strength steel pipe for fitting that has excellent earthquake resistance. [Brief description of the drawings]
[0008] [Figure 1] This is a schematic diagram of two fitting steel pipes being fitted together to attach to an overhead line pole. [Diagram 2] FIG. 2 is a diagram showing an outline of a first tapered portion and a second tapered portion. [Diagram 3] FIG. 13 is a diagram showing the relationship between the range of a portion to be softened and a molding load. [Figure 4] FIG. 1 is a diagram showing the relationship between hardness at 0 to 36% position and molding load. [Diagram 5] FIG. 4 is a diagram showing the relationship between heat treatment temperature and hardness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] First, in explaining the present invention, the fitting steel pipe will be briefly explained. FIG. 1 shows a schematic diagram of a case where a plurality of fitting steel pipes (for example, two fittings) are fitted to an overhead pole. The characteristic part of the present invention is the diameter-reduced part of the upper tube end of the fitting lower pipe (the fitting side), and the other expanded upper pipe is placed over the upper tube end of the fitting lower pipe, so that they are fitted together by friction. At this time, the diameter-reduced part of the fitting lower pipe has a first taper part with a gentle taper rate and a second taper part with a steeper taper rate than the first taper part. The first taper part that fits with the upper pipe is particularly important in terms of the characteristics of the present invention, and it is necessary to reduce the diameter significantly from the original diameter. Here, as shown in FIG. 2, the length of the fitting part according to the present invention varies depending on the size of the overhead pole, etc., so for convenience, the length of the first taper part is defined as 100%.
[0010] In order to solve the problem, the inventors have identified the parts that are heavily loaded during diameter reduction by analysis, and have considered softening the parts to improve workability. Furthermore, in consideration of the amount of work hardening due to strain caused by diameter reduction, the inventors aimed to reduce the hardness difference between the base material and the welded parts over the entire length corresponding to the processed parts so that the strength level of 590 MPa or more required for the final product is ensured in all parts and the diameter reduction can be performed stably without buckling. Since the actual amount of work hardening is expected to be 90 MPa or more in the reduced diameter part, the strength of 500 MPa or more is required before the diameter reduction by softening it through heat treatment. In order to achieve these requirements, the inventors have invented a method for obtaining a high-strength steel pipe for a fitting overhead line pole that satisfies all of the above conditions by changing the heat treatment conditions in the longitudinal direction.
[0011] The inventors performed a diameter reduction analysis using FEM, and as a result of thorough investigation, they found that the load during diameter reduction increases with the displacement of the diameter reduction device (hereinafter referred to as the stroke) and reaches its maximum load at the final stroke (when the final displacement is reached), but that the area causing the large load is near the end of the tube where the contact surface pressure with the die is high, specifically in the range of 0% to 36% from the end of the tube. Figure 3 shows the relationship between the softening range and the forming load. Therefore, softening the area at least in the range of 36% or less from the end of the tube is particularly effective for formability.
[0012] Furthermore, in the relationship between hardness and forming load in Figure 4, if the hardness is less than 150Hv, although work hardening occurs during diameter reduction, the target strength of 590MPa will not be achieved. On the other hand, if the hardness is more than 185Hv, the material is too hard and a high forming load is applied during diameter reduction, which exceeds the capacity of the testing machine and may damage the drive unit or die, making it unsuitable for diameter reduction. Therefore, the hardness range suitable for diameter reduction is 150Hv to 185Hv.
[0013] In addition, if the hardness is less than 185Hv in the range of 100% to 120% from the tube end as shown in Figure 2, the second taper portion which is the same as this portion or overlaps with this portion is not a portion where sufficient work hardening can be obtained during diameter reduction, so the hardness after diameter reduction will also be less than 185Hv, and the target strength of 590MPa will not be achieved. Therefore, in the range of 100% to 120% from the tube end, a hardness of 185Hv or more is required.
[0014] Furthermore, if the difference in average hardness between the base material and the welded part is 20 Hv or more in the range of 0% to 120% from the tube end, strain will concentrate at the boundary between the base material and the welded part during diameter reduction, causing buckling and making the forming unstable, so it is preferable that the difference be less than 20 Hv.
[0015] From the above, the high-strength steel pipe of the present invention has a hardness of 150Hv to 185Hv at least in the range of 0% to 36% from the pipe end before diameter reduction, and a hardness of 185Hv or more in the range of 100% to 120% from the pipe end. The part from 36% to less than 100% from the pipe end may be softened as long as the hardness is in the range of 150Hv to 185Hv. The wider this range is, the lower the forming load is, and the more advantageous the formability is. However, the part 100% or more from the pipe end (the range of 100% to 120% from the pipe end) must have a hardness of 185Hv or more from the viewpoint of ensuring strength as described above.
[0016] <Hardness measurement method> Here, the average hardness was measured at least at the 0%, 36%, 100%, and 120% positions, which are the ends of the first taper portion, using a micro Vickers hardness tester on samples that were cut at 90° from the base material of the heat-treated steel pipe, and then the C-section (the cross section of the steel pipe when cut into rings) was embedded and polished. The measurement was performed at the center of the plate thickness with a load of 500 gf, and 10 points were measured at 0.3 mm pitch in the circumferential direction of the steel pipe, and the average value was taken as the average hardness.
[0017] <Ingredients> The chemical composition of the base metal part of the high-strength fitting steel pipe of the present invention (hereinafter also referred to as "chemical composition of the present invention") will be described below. The steel used may be that used in the manufacture of ordinary steel pipes of 590MPa to 800MPa class, and may have, for example, approximately 0.10% by mass of C, 0.2% by mass of Si, 1.5% by mass of Mn, 0.04% by mass of Nb, and 0.015% by mass of Al. However, in order to stably obtain a strength of 590MPa or more, the following range of mass% components is preferable.
[0018] C: 0.05-0.20%, To provide the necessary strength for overhead line poles, the C content should be at least 0.05%, but if it exceeds 0.20%, the strength becomes too high, making it difficult to reduce the diameter.
[0019] Si: 0.03 to 0.40%, Silicon is an element used for deoxidation. If the silicon content is less than 0.03%, deoxidation is insufficient and coarse oxides may be generated. Therefore, the silicon content is preferably 0.03% or more. On the other hand, if the silicon content exceeds 0.40%, it may lead to the generation of inclusions such as SiO2, which may easily cause microvoids during molding. Therefore, the silicon content is preferably 0.40% or less.
[0020] Mn: 1.00-2.00%, Mn is an element that improves hardenability, and in manufacturing the high-strength steel of the present invention, the Mn content is preferably 1.00% or more. On the other hand, if it exceeds 2.00%, coarse MnS is generated, which may deteriorate the formability, so the Mn content is preferably 2.00% or less.
[0021] P: 0.000~0.030%, P is an element that may be contained as an impurity in steel. If the P content exceeds 0.030%, it is likely to concentrate at grain boundaries, which may deteriorate formability. Therefore, the P content is preferably 0.030% or less. On the other hand, in the present invention, the P content may be 0.000% since it is substantially an impurity.
[0022] S: 0.000~0.010%, S is an element that may be contained as an impurity in steel. If the S content exceeds 0.010%, coarse MnS is generated, which may deteriorate formability. Therefore, the S content is preferably 0.010% or less. On the other hand, in the present invention, the S content may be 0.000% since it is substantially an impurity.
[0023] Al: 0.005 to 0.500%, Al is an element that produces AlN and contributes to the refinement of austenite grains through the pinning effect, and as a result, contributes to strength. If the Al content is less than 0.005%, no contribution to strength can be expected. Therefore, the Al content is preferably 0.005% or more. On the other hand, if the Al content exceeds 0.500%, coarse AlN may precipitate, deteriorating formability. Therefore, the Al content is preferably 0.500% or less.
[0024] Nb: 0.010~0.060%, Nb is an element that produces NbC and contributes to the refinement of austenite grains through the pinning effect, and as a result contributes to strength. If the Nb content is less than 0.010%, no contribution to strength can be expected. Therefore, the Nb content is preferably 0.010% or more. On the other hand, if the Nb content exceeds 0.060%, coarse NbC precipitates, which may deteriorate formability. Therefore, the Nb content is preferably 0.060% or less.
[0025] N: 0.0003~0.0060%, N is an element that generates AlN and contributes to the refinement of austenite grains through the pinning effect, and as a result, contributes to strength. Although 0 is acceptable, the lower limit is set to 0.0003 from the viewpoint of cost and productivity. On the other hand, if the N content exceeds 0.0060%, coarse AlN may precipitate, which may deteriorate formability. Therefore, the N content is preferably 0.0060% or less.
[0026] Furthermore, one or more of the following elements that affect strength may be contained as optional elements.
[0027] Ti: 0.000~0.200%, Ti is an optional element and does not have to be contained. That is, the Ti content may be 0.00%. If Ti is contained, it must be more than 0.00%. Ti is an element that forms precipitates and contributes to strength. However, if added in excess, coarse TiN is formed, which may deteriorate formability, so 0.200% or less is preferable.
[0028] B: 0.0000~0.0050%, B is an optional element and does not have to be contained. That is, the B content may be 0.00%. When B is contained, it is more than 0.00%. B is an element that improves hardenability and contributes to strength. On the other hand, if it exceeds 0.0050%, coarse precipitates of B may occur and formability may deteriorate, so 0.0050% or less is preferable.
[0029] Cu: more than 0.00% and less than 1.00%, Cu is an optional element and may not be contained. That is, the Cu content may be 0.00%. If it is contained, it is more than 0.00%. Cu is an element that affects the strength of steel. On the other hand, if Cu is contained in excess, the effect becomes saturated and the cost may increase. Therefore, it is preferable that the content be 1.00% or less.
[0030] Ni: more than 0.00% and less than 1.00%, Ni is an optional element and may not be contained. That is, the Ni content may be 0.00%. If Ni is contained, it must be more than 0.00%. Ni is an element that affects the strength of steel. On the other hand, if Ni is contained in excess, the effect may saturate and the cost may increase. Therefore, it is preferable that Ni content is 1.00% or less.
[0031] Cr: more than 0.00% and less than 1.00%, Cr is an optional element and may not be contained. That is, the Cr content may be 0.00%. If Cr is contained, it must be more than 0.00%. Cr is an element that contributes to the strength of steel. On the other hand, if Cr is contained in excess, the effect may saturate and the cost may increase. Therefore, 1.00% or less is preferable.
[0032] Mo: more than 0.00% and less than 0.50%, Mo is an optional element and may not be contained. That is, the Mo content may be 0.00%. When Mo is contained, it is more than 0.00%. Mo is an element that contributes to the strength of steel. On the other hand, if Mo is contained in excess, the effect becomes saturated and the cost may increase. Therefore, 0.50% or less is preferable.
[0033] V: more than 0.00% and less than 0.20%, V is an optional element and may not be contained. That is, the V content may be 0.00%. When V is contained, it is more than 0.00%. V is an element that contributes to the strength of steel. On the other hand, if V is contained in excess, the effect becomes saturated and the cost may increase. Therefore, 0.20% or less is preferable.
[0034] W: more than 0.00% and less than 0.10%, W is an optional element and may not be contained. That is, the W content may be 0.00%. When W is contained, it is more than 0.00%. W is an element that contributes to the strength of steel. On the other hand, if W is contained in excess, the effect becomes saturated and the cost may increase. Therefore, 0.10% or less is preferable.
[0035] Ca: more than 0.0000% and less than 0.0200%, Ca is an optional element and may not be contained. That is, the Ca content may be 0.0000%. When Ca is contained, it is more than 0.0000%. Ca has the effect of controlling inclusions, further improving formability, and affecting strength. On the other hand, if Ca is contained in excess, coarse inclusions may be generated, and formability may deteriorate. Therefore, 0.0200% or less is preferable.
[0036] Mg: more than 0.0000% and less than 0.0200%, Mg is an optional element and may not be contained. That is, the Mg content may be 0.0000%. If Mg is contained, it is more than 0.0000%. Mg has the effect of controlling inclusions, further improving formability, and affecting strength. On the other hand, excessive Mg content may cause coarse inclusions and deteriorate formability. Therefore, 0.0200% or less is preferable.
[0037] Zr: more than 0.0000% and less than 0.0200%, Zr is an optional element and may not be contained. That is, the Zr content may be 0.0000%. If it is contained, it is more than 0.0000%. Zr has the effect of controlling inclusions, further improving formability, and affecting strength. On the other hand, if Zr is contained in excess, coarse inclusions may occur and formability may deteriorate. Therefore, 0.0200% or less is preferable.
[0038] REM: more than 0.0000% and less than 0.0200%, REM is an optional element and may not be contained. That is, the REM content may be 0.0000%. When contained, it is more than 0.0000%. Here, "REM" refers to rare earth elements, that is, at least one element selected from the group consisting of Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. REM has the effect of controlling inclusions, further improving formability, and affecting strength. On the other hand, if REM is contained excessively, coarse inclusions may occur, and formability may deteriorate. Therefore, 0.0200% or less is preferable.
[0039] <Production method> The manufacturing process is in the order of steel making ⇒ hot rolling ⇒ pipe making ⇒ heat treatment. The hardness is controlled in the heat treatment process as mentioned above, and formability is improved. Up to this point in the pipe making process, no special controls or manufacturing methods are required, and the product is manufactured under general conditions equivalent to those used for other products.
[0040] Regarding the manufacturing conditions, if the temperature during heat treatment is less than 780°C in at least the range of 0% to 36% from the tube end of the first tapered portion, the softening effect is insufficient and the hardness exceeds 185Hv. Also, if the temperature exceeds 900°C, the softening is excessive and the hardness is less than 150Hv. Figure 5 shows the relationship between heat treatment temperature and hardness. If the heat treatment time is less than 1 minute after reaching 780°C or higher, the heat is not sufficiently transferred to the member, so the softening effect is not sufficiently obtained. If it exceeds 60 minutes, the effect is already saturated, so further heat treatment is not appropriate because it deteriorates productivity and increases costs, so the heat treatment time is preferably 1 minute or more and 60 minutes or less after reaching 780°C or higher.
[0041] If the temperature during heat treatment is less than 600°C in the range of 100-120% from the tube end, the effect of softening the welded part is insufficient, and the difference in average hardness between the base material and the welded part will exceed 20Hv. Also, if the time is less than 1 minute, the heat is not sufficiently transferred to the parts, so the softening effect is not fully achieved. If the time exceeds 60 minutes, the effect is already saturated, so further heat treatment is not appropriate because it will reduce productivity and increase costs.
[0042] To simultaneously perform the heat treatment under the two conditions above, it is necessary to devise a furnace structure. Specifically, partitions can be installed in the furnace to change the set temperature in each zone, or the heater burners in the furnace can be arranged in a way that more burners are placed in the zone with a higher set temperature to create a temperature deviation, or the seal at the furnace entrance can be adjusted to allow a moderate amount of air to flow into the furnace, thereby keeping the temperature on the furnace entrance side low. Any of these methods are acceptable for the present invention, and as long as the thermometers placed in each zone are within the temperature range of the present invention, a high-strength steel pipe for overhead line poles with excellent formability can be obtained. EXAMPLES
[0043] Steel with the composition shown in Table 1 was used to manufacture high-strength steel pipes for fitting overhead line poles with dimensions of φ400 x t10.0 mm under the conditions shown in Table 2, through the processes of steelmaking ⇒ hot rolling ⇒ pipe making ⇒ heat treatment. The pipes were manufactured under standard conditions, and the furnace temperatures of the first and second taper sections were set using three heating methods during heat treatment, A to C, and the heat treatment was performed simultaneously. To evaluate formability, a diameter reduction process was performed so that the outer diameter of the tip of the first taper section was φ350 mm, and the load during diameter reduction and the hardness of the product after diameter reduction were investigated. The investigation results are shown in Table 2.
[0044] [Table 1]
[0045] [Table 2]
[0046] It is clear that all of the examples that meet the requirements of the present invention are excellent in hardness and moldability.
Claims
1. A steel pipe using a steel containing, in mass %, C: 0.05-0.20%, Si: 0.03-0.40%, Mn: 1.00-2.00%, P: 0.000-0.030%, S: 0.000-0.010%, Al: 0.005-0.500%, Nb: 0.010-0.060%, N: 0.0003-0.0060%, with the remainder being Fe and unavoidable impurities, When the length of the first taper portion, which is the fitting portion, is 100%, before the diameter reduction process, Hardness of 150Hv to 185Hv in the range of 0% to 36% from at least the tube end; In the range of 100% to 120% from the tube end, the hardness is 185Hv or more. The difference in average hardness between the base material and the welded part is less than 20Hv in the range of 0% to 120% from the pipe end. A high-strength steel pipe for fitting, having excellent formability and a tensile strength of 500 MPa or more, characterized in that
2. In claim 1, further in mass %, Ti: 0.000 to 0.200%, B: 0.0000 to 0.0050%, Cu: more than 0.00% and 1.00% or less, Ni: 0.
00. % more than 1.00%, Cr: more than 0.00% and less than 1.00%, Mo: more than 0.00% and less than 0.50%, V: more than 0.00% and less than 0.20%, W: more than 0.00% and less than 0.10% and a high-strength steel pipe for fitting having excellent formability and a tensile strength of 500 MPa or more, characterized in that the steel used contains one or more of the following: Ca: more than 0.0000% and not more than 0.0200%, Mg: more than 0.0000% and not more than 0.0200%, Zr: more than 0.0000% and not more than 0.0200%, and REM: more than 0.0000% and not more than 0.0200%.
Citation Information
Patent Citations
Cable protecting cover
JP1983058816A
Methods for using high-strength electric resistance welded steel pipes and high-strength electric resistance welded steel pipes for ground stabilization work
JP6841392B2