Auxiliary burner of flash smelting furnace
The auxiliary burner's design with a larger dispersion cone diameter and tungsten carbide protective layers addresses wear issues, maintaining efficient raw material mixing and copper quality in flash smelting furnaces.
Patent Information
- Application Number
- JP2023063260
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
The dispersion cone of the auxiliary burner in flash smelting furnaces experiences rapid wear due to high-temperature and oxidizing conditions, leading to poor mixing of smelting raw materials with reaction gas and increased copper loss in molten metal.
The auxiliary burner features a dispersion cone with a larger upper end diameter and a hardened protective layer, comprising a first and second layer made of tungsten carbide alloy, to protect the cone from wear and maintain mixing efficiency.
The hardened protective layer effectively prevents wear and damage to the dispersion cone, ensuring long-term maintenance of smelting raw material dispersibility and improving copper quality in the molten metal.
Smart Images

Figure 2024150037000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an auxiliary burner for a flash smelting furnace, and more particularly to an improvement in an auxiliary burner in which the wear resistance of a dispersion cone, which is a component of the auxiliary burner, is improved. [Background technology]
[0002] A flash smelting furnace is used for smelting non-ferrous metal sulfides such as copper sulfide and nickel sulfide, etc. The flash smelting furnace is equipped with a concentrate burner that supplies the smelting material and reactive gas into the furnace.
[0003] In operating a flash smelting furnace, it is necessary to control the melting and smelting reaction in the furnace and perform stable operation. The melting and smelting reaction is an oxidation reaction of metal sulfides contained in the smelting raw materials. This oxidation reaction occurs when the smelting raw materials come into contact with the reactive gas. Therefore, the more thoroughly the smelting raw materials and the reactive gas are mixed, the easier it is for the oxidation reaction to proceed. For this reason, premixing is performed in the concentrate burner, where the smelting raw materials and the reactive gas are mixed together.
[0004] An auxiliary burner is provided at the center of the concentrate burner. A roughly truncated cone-shaped dispersion cone is provided at the lower end of the auxiliary burner, and a nozzle hole for spraying gas (e.g., oxygen) is provided above the dispersion cone (see Patent Document 1). The smelting raw material is appropriately dispersed by the action of the inclined surface of the dispersion cone and the gas sprayed from the nozzle hole, and is mixed with the reaction gas. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2000-97411 A Summary of the Invention [Problem to be solved by the invention]
[0006] Incidentally, the dispersion cone of the auxiliary burner is a component that is directly impacted by the raw material, and therefore is subject to a large degree of wear. In Patent Document 1, it is said that the gas ejected from the ejection holes covers the inclined surface of the dispersion cone, which reduces the impact of the raw material and reduces the wear of the dispersion cone (see paragraph 0017 of Patent Document 1). However, the reduction effect is not sufficient, and the wear of the dispersion cone progresses at a high speed.
[0007] As the wear of the dispersion cone progresses, the dispersion of the raw materials deteriorates, which causes insufficient mixing with the reaction gas, resulting in an increase in copper loss in the molten metal (kalami), and a deterioration in the grade. Here, kalami refers to molten metal that contains almost no copper components, such as FeO·SiO2, and is discharged outside the system.
[0008] As described above, the dispersion cone, which is a component of the auxiliary burner, is susceptible to wear and damage because it comes into contact with the smelting raw material in a harsh environment of high temperature and a highly oxidizing atmosphere.
[0009] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide an auxiliary burner having an improved wear resistance of a dispersion cone. [Means for solving the problem]
[0010] That is, the first invention according to the present invention is: An auxiliary burner provided for a concentrate burner of a flash smelting furnace, comprising: a blowing pipe having a plurality of nozzles formed on a lower peripheral surface of a pipe body into which gas is supplied, for spraying the gas from the inside to the outside; A dispersion cone having a generally truncated cone shape provided at a lower end of the blowing pipe; a hardened protective layer that protects the dispersion cone from wear; Equipped with The outer diameter of the upper end of the dispersion cone is set to be larger than the outer diameter of the lower end of the blowing pipe, The hardened protective layer is characterized by having a first hardened protective layer provided at a step between the upper end of the dispersion cone and the lower end of the blowing pipe, and a second hardened protective layer that is flush with the surface of the first hardened protective layer and covers the inclined surface of the dispersion cone, The second invention is In the auxiliary burner of the flash smelting furnace according to the first aspect of the present invention, The first hardened protective layer is provided so as to fill an imaginary ring-shaped space having an approximately triangular cross-section formed by the surface of the blowing pipe and the extended surface portion of the inclined surface of the dispersion cone when the inclined surface of the dispersion cone is extended from its upper edge toward the surface of the blowing pipe below the outlet hole.
[0011] Next, the third invention according to the present invention is In the auxiliary burner for the flash smelting furnace according to the first or second invention, The upper end of the hardened protective layer is set at a position directly below the nozzle of the blowing pipe, The fourth invention is In the auxiliary burner for the flash smelting furnace according to the first or second invention, The first hardened protective layer and the second hardened protective layer are characterized in that they are made of an alloy containing 50% or more of tungsten carbide.
[0012] The fifth aspect of the present invention is In the auxiliary burner for a flash smelting furnace according to the fourth aspect of the present invention, The first hardened protective layer and the second hardened protective layer are formed as hardened layers by overlay welding, The sixth invention is In the auxiliary burner of the flash smelting furnace according to the fifth aspect of the present invention, The hardfacing layer is characterized in that the number of layers is two or less.
[0013] Furthermore, the seventh invention is In the auxiliary burner for the flash smelting furnace according to the first or second invention, The outer diameter of the upper end of the dispersion cone is set to be larger than the outer diameter of the lower end of the blowing pipe by at least twice the wall thickness of the blowing pipe, The eighth invention is In the auxiliary burner of the flash smelting furnace according to the fifth aspect of the present invention, A groove is provided at the lower end of the blow pipe, and the first hardened protective layer formed of a hardened build-up layer is provided so as to fill the ring-shaped space including the groove portion. Effect of the Invention
[0014] The dispersion cone of the auxiliary burner according to the present invention comprises: The outer diameter of the upper end of the dispersion cone is set to be larger than the outer diameter of the lower end of the blowing pipe, and a hardened protective layer that protects the dispersion cone from wear; The hardened protective layer has a first hardened protective layer provided at the step between the upper end of the dispersion cone and the lower end of the blowing tube, and a second hardened protective layer that is flush with the surface of the first hardened protective layer and covers the inclined surface of the dispersion cone.
[0015] Therefore, even if the dispersion cone comes into contact with the smelting raw material under harsh conditions such as high temperature and a highly oxidizing atmosphere, the step portion and inclined surface of the dispersion cone are protected by the hardened protective layer, making it possible to prevent wear and damage to the dispersion cone.
[0016] In particular, by providing the first hardened protective layer so as to fill the virtual ring-shaped space formed by the surface of the blowing pipe and the extended portion of the inclined surface of the dispersion cone, a first hardened protective layer of sufficient thickness is formed while maintaining the inclined surface shape of the inclined surface of the dispersion cone, so that it is possible to maintain the dispersion function of the smelting raw materials for a long period of time while preventing wear and damage to the dispersion cone. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a vertical cross-sectional view showing the configuration of a flash smelting furnace. [Diagram 2] FIG. 2 is a vertical cross-sectional view showing the configuration of a concentrate burner. [Diagram 3] FIG. [Figure 4] FIG. 1 is a vertical cross-sectional view showing the configuration of a conventional auxiliary burner. [Diagram 5] FIG. 2 is a front view of an auxiliary burner according to the present invention in the process of being manufactured, showing a step between the upper end of the dispersion cone and the lower end of the blowing tube. [Figure 6] FIG. 1 is a vertical cross-sectional view showing one embodiment of an auxiliary burner according to the present invention. [Figure 7] FIG. 13 is a front view of an auxiliary burner according to the present invention in the process of being manufactured, showing a state in which a first hardened protective layer is provided in a manner that fills an imaginary ring-shaped space formed by the blowing pipe surface and the extended surface portion of the dispersion cone inclined surface. [Figure 8] FIG. 8 is a vertical cross-sectional view of the auxiliary burner according to the present invention in the process of being manufactured, showing a state in which a first hardened protective layer is provided in a manner that fills the ring-shaped space in FIG. 7. [Figure 9] FIG. 13 is a longitudinal sectional view of the auxiliary burner according to the present invention in the process of being manufactured, showing a state in which a groove is provided at the lower end of the blow pipe. [Figure 10] 10 is a longitudinal sectional view of the auxiliary burner according to the present invention in the process of being manufactured, showing a state in which a first hardened protective layer is provided in a manner that fills a ring-shaped space including the groove portion in FIG. 9. [Figure 11] FIG. 4 is a vertical cross-sectional view showing another embodiment of the auxiliary burner according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Next, an embodiment of the present invention will be described in detail with reference to the drawings.
[0019] 1. Self-melting smelting furnace First, the overall configuration of the flash smelting furnace FF will be described.
[0020] As shown in Fig. 1, the flash smelting furnace FF is equipped with a settler 11. A reaction tower 12 is provided on the upper surface of one end of the settler 11. A flue gas duct 13 is provided on the upper surface of the other end of the settler 11. A concentrate burner 20 is provided on the upper end of the reaction tower 12. A slag removal port 14 is provided at the height of the slag, and a slag removal port 15 is provided at the height of the slag on the side wall of the settler 11, separated from each other.
[0021] Copper smelting operations using a flash smelting furnace (FF) are carried out as follows:
[0022] Powdered smelting raw materials and a reaction gas (e.g., oxygen-enriched air) are blown into the reaction tower 12 from the concentrate burner 20. The smelting raw materials contain at least copper sulfide concentrate (e.g., CuFeS2: hereinafter simply referred to as "copper concentrate") and flux. The flux is added to produce high-quality smelting powder, and is, for example, silica sand. The smelting raw materials also contain cooling materials and the like as necessary.
[0023] The smelting raw materials blown into the reactor 12 are heated by the heat of the auxiliary burners and the radiant heat from the furnace walls of the reactor 12, and melt as the sulfur and iron in the copper concentrate burn. The molten smelting raw materials are stored in the settler 11. In the settler 11, the molten material is gravity separated into a slag (as mentioned above, a molten material that contains almost no copper components, such as FeO·SiO2) and a molten material (a molten material that contains copper components, such as Cu2S·FeS).
[0024] The slag at the top of the molten metal is discharged from the slag removal port 14 and treated in an electric smelting furnace. The appropriate amount of the slag at the bottom of the molten metal is discharged from the slag removal port 15 according to the requirements of the converter in the next process. The smelting gas generated in the reaction tower 12 and the settler 11 is discharged from the flash smelting furnace FF through the flue gas 13, and the heat is recovered in the waste heat boiler.
[0025] 2. Concentrate Burner Next, the configuration of the concentrate burner 20 will be described.
[0026] As shown in Fig. 2, the concentrate burner 20 is equipped with a wind box 21 into which the reaction gas is introduced. The lower part of the wind box 21 is formed into a cone shape tapered downward, and a cylindrical burner cone 22 is connected to the lower end of the wind box 21. The burner cone 22 is erected at the upper end of the reaction tower 12. In addition, an inspection hatch 23 is provided in the burner cone 22.
[0027] The concentrate burner 20 is equipped with an auxiliary burner 30. The auxiliary burner 30 is disposed vertically, penetrating the inside of the wind box 21 and the burner cone 22. The auxiliary burner 30 is disposed at the center of the burner cone 22. The lower end of the auxiliary burner 30, from which the flame is ejected, is located near the lower end of the burner cone 22.
[0028] The concentrate chute 24 is provided so as to surround the outer periphery of the auxiliary burner 30. The concentrate chute 24 is a cylindrical member coaxial with the auxiliary burner 30. The concentrate chute 24 is disposed in the wind box 21 and can move up and down within the wind box 21. The smelting raw material is supplied into the flash smelting furnace FF through the concentrate chute 24.
[0029] A wind speed regulator 25 is provided so as to surround the outer periphery of the concentrate chute 24. The wind speed regulator 25 is disposed in the wind box 21 and can be raised and lowered within the wind box 21 independently of the concentrate chute 24. By raising and lowering the wind speed regulator 25, the flow path width of the reaction gas supplied from the wind box 21 to the burner cone 22 can be adjusted. This makes it possible to adjust the flow rate of the reaction gas.
[0030] 3. Auxiliary Burner (1) Conventional auxiliary burner Next, the conventional auxiliary burner 30 will be described.
[0031] As shown in Fig. 3, the auxiliary burner 30 has an injection pipe 31. The injection pipe 31 is a hollow pipe arranged vertically, and a plurality of injection holes 32 for injecting gas from the inside to the outside are formed on the lower peripheral surface of the pipe body into which gas is supplied.
[0032] A dispersion cone 33 is provided at the lower end of the blowing pipe 31. The dispersion cone 33 is a member having a generally truncated cone shape that extends downward and has a through hole at the center.
[0033] As shown in Fig. 4, an inner pipe 34 is provided inside the blowing pipe 31. The inner pipe 34 is a hollow pipe with a smaller diameter than the blowing pipe 31. The blowing pipe 31 and the inner pipe 34 are arranged coaxially with the blowing pipe 31 on the outside. The dispersion cone 33 is fixed to the lower end of the blowing pipe 31 and the lower end of the inner pipe 34.
[0034] A heavy oil burner 35 is disposed inside the inner pipe 34. A nozzle 35a of the heavy oil burner 35 is disposed near the lower end of the inner pipe 34.
[0035] There is a gap between the blowing pipe 31 and the inner pipe 34, which serves as a gas flow path. The blowing pipe 31 is provided with a first supply port 36 that communicates with this flow path. Gas is supplied to the inside of the blowing pipe 31 through the first supply port 36. The gas supplied to the inside of the blowing pipe 31 passes through the flow path between the blowing pipe 31 and the inner pipe 34 and is ejected from the ejection hole 32. At this time, the gas passes through the ejection hole 32 and is ejected from the inside of the blowing pipe 31 to the outside. The gas supplied to the blowing pipe 31 is not particularly limited, but high-pressure oxygen or oxygen-enriched air is preferred.
[0036] The inner pipe 34 is provided with a second supply port 37 that communicates with its interior. Oxygen or oxygen-enriched air is supplied to the inside of the inner pipe 34 through the second supply port 37. The oxygen or oxygen-enriched air supplied to the inside of the inner pipe 34 passes through the inside of the inner pipe 34 and is discharged from the lower end. At this time, the oxygen or oxygen-enriched air is used to ignite and burn the heavy oil sprayed from the nozzle 35a of the heavy oil burner 35.
[0037] The raw material falls through the concentrate chute 24 (see FIG. 2). The falling raw material is dispersed by the inclined surface of the dispersion cone 33. The raw material is also dispersed by the gas ejected from the ejection hole 32. This causes the raw material to be mixed with the reactive gas.
[0038] As described in Patent Document 1, the gas ejected from the ejection holes 32 covers the inclined surface of the dispersion cone 33, mitigating the collision of the smelting raw materials and reducing wear of the dispersion cone 33. However, this effect is not sufficient, and wear of the dispersion cone 33 progresses at a high speed.
[0039] As described above, in the conventional auxiliary burner 30, the wear of the dispersion cone 33 progresses at a high speed, which causes a problem that the dispersion of the smelting raw material deteriorates and the mixing with the reaction gas becomes insufficient.
[0040] (2) Auxiliary burner according to the present invention The auxiliary burner according to the present invention has a unique structure that solves the above problems, and thereby improves the wear resistance of the auxiliary burner, particularly the wear resistance of the dispersion cone.
[0041] 5 and 6, the dispersion cone 43 of the auxiliary burner 40 is formed of a generally truncated cone-shaped member with a through hole in the center, as in the conventional case, but the outer diameter of the upper end side of the dispersion cone 43 (hereinafter also referred to as the upper end outer diameter) is set larger than the outer diameter of the lower end side of the blowing pipe 41 (hereinafter also referred to as the lower end outer diameter), and the inclined surface of the dispersion cone 43 is provided with a hardened protective layer described below that protects the dispersion cone 43 from wear. In addition, in FIG. 6, the members with the same reference numerals as those in FIG. 4 are the same as those in FIG. 4.
[0042] Here, it is preferable that the outer diameter of the upper end of the dispersion cone 43 is set to be larger than the outer diameter of the lower end of the blowing pipe 41 by at least twice the thickness of the blowing pipe 41. This makes it possible to enjoy a higher wear resistance effect, as will be described in detail later.
[0043] The cured protective layer will now be described.
[0044] 4. hardened protective layer As shown in Fig. 6, the hardened protective layer 45 for protecting the dispersion cone 43 from wear includes a first hardened protective layer 45a provided on a step portion 44 (see Fig. 5) between the upper end of the dispersion cone 43 and the lower end of the blowing pipe 41, and a second hardened protective layer 45b that is flush with the surface of the first hardened protective layer 45a and covers the inclined surface of the dispersion cone 43. Of these, the first hardened protective layer 45a is provided in a manner that connects from the upper end of the dispersion cone 43 to the lower end surface of the blowing pipe 41, as shown in Fig. 6.
[0045] For reasons that will be described later, the first hardened protective layer 45a is desirably provided in a manner that fills an imaginary ring-shaped space 46 shown in FIGS.
[0046] In other words, when the inclined surface of the dispersion cone 43 is extended from its upper edge toward the surface below the outlet hole 42 of the blowing pipe 41, it is desirable that the first hardened protective layer 45a is provided in such a manner that it fills an imaginary ring-shaped space 46 having an approximately triangular cross-section formed by the surface 41a of the blowing pipe 41 and the extended surface portion 43a of the inclined surface of the dispersion cone 43.
[0047] (1) 1st hardened protective layer The region where the ring-shaped space 46 shown in Figs. 7 and 8 is formed is a region where the smelting raw material repeatedly hits with high frequency, and therefore wear is particularly likely to progress.
[0048] Therefore, in the auxiliary burner according to the present invention, the outer diameter of the upper end of the dispersion cone 43 is set larger than the outer diameter of the lower end of the blowing pipe 41 as described above, and the first hardened protective layer 45a is provided in such a manner as to fill the virtual ring-shaped space 46 having a substantially triangular cross section formed by the surface 41a of the blowing pipe 41 and the extended surface portion 43a of the inclined surface of the dispersion cone 43, thereby making it possible to give the first hardened protective layer 45a a sufficient thickness (i.e., the thickness in the normal direction of the inclined surface of the dispersion cone 43) while almost maintaining the inclined surface shape of the inclined surface of the dispersion cone 43. However, since the virtual ring-shaped space 46 has a substantially triangular cross section, the thickness of the edge region of the first hardened protective layer 45a on the side connected to the surface of the blowing pipe 41 and the edge region of the first hardened protective layer 45a on the side connected to the dispersion cone 43 are not limited to this.
[0049] In other words, in the auxiliary burner of the present invention, the first hardened protective layer 45a is arranged in a manner that fills the ring-shaped space 46, which makes it possible to avoid the inconvenience of forming convex portions (convex portions due to the surface shape of the first hardened protective layer 45a that is arranged in a manner that does not fill the ring-shaped space 46) that have an adverse effect on the dispersion of the smelting raw material in the area where the ring-shaped space 46 is formed, while still making it possible to provide the first hardened protective layer 45a with a sufficient thickness.
[0050] Therefore, the auxiliary burner of the present invention can effectively avoid the inconvenience of wear caused by repeated collisions of the smelting raw materials while maintaining good dispersion of the smelting raw materials.
[0051] Furthermore, as described above, by setting the outer diameter of the upper end of the dispersion cone 43 to be larger than the outer diameter of the lower end of the blowing pipe 41 by more than twice the thickness of the blowing pipe 41, it becomes easier to form the thickness of the first hardened protective layer 45a to be greater than or equal to the thickness of the blowing pipe 41, so that a higher wear resistance effect can be expected.
[0052] [Materials of the first cured protective layer] The first hardened protective layer is not particularly limited as long as it is made of a material having sufficient hardness. For example, it is preferable to form the first hardened protective layer using an alloy material containing 50% or more of tungsten carbide and the remainder containing 30% or more of carbon and iron in total, since this makes it easy to obtain a high hardness of 900HV or more.
[0053] Examples of the above-mentioned material include welding rods containing 50% or more of tungsten carbide. Specifically, examples include tungsten carbide flux-cored wire (manufactured by ING: "UW-O tungsten carbide build-up wire") containing approximately 60% tungsten carbide particles and approximately 40% carbon and iron, and tungsten carbide special surface-hardened welding rods (manufactured by Belgium's SOUDOMETAL: "DIADUR-2000-gas rod" and "ING-DIAMIG-wire") containing approximately 65% tungsten carbide and approximately 35% Ni-Cr-B-Si matrix.
[0054] Using such a welding rod for overlay welding makes construction easier, and is particularly preferable when creating an auxiliary burner by assembling a divided blow pipe and a dispersion cone as shown in this embodiment, because the rod can also be used as a joining material for joining the dispersion cone to the blow pipe.
[0055] In this case, a groove 41b is provided at the lower end of the blow pipe 41 as shown in Figure 9, and the ring-shaped space 46 shown in Figures 9 and 10, which includes this groove 41b, is filled with a first hardened protective layer 45a made of a weld metal (hardened buildup layer) of the above composition, thereby making it possible to further increase the thickness of the hardened protective layer.
[0056] (2) 2nd hardened protective layer The hardened protective layer 45, which protects the dispersion cone 43 from wear, has, as described above, a first hardened protective layer 45a and a second hardened protective layer 45b that is flush with the surface of the first hardened protective layer 45a and covers the inclined surface of the dispersion cone 43.
[0057] The second hardened protective layer 45b is provided over the entire area from the lower edge of the inclined surface of the dispersion cone 43 to the connection position where the first hardened protective layer 45a connects to the blowing pipe 41, as shown in Figures 6 and 11.
[0058] In addition, when the auxiliary burner is made by assembling the divided blowing pipe and the dispersion cone, the first hardened protective layer is provided when the blowing pipe and the dispersion cone are joined as described above, and therefore, after the first hardened protective layer is provided, the second hardened protective layer is provided, which is flush with the surface of the first hardened protective layer and covers the inclined surface of the dispersion cone. However, when the blowing pipe and the dispersion cone are integrated in advance, a method of providing the second hardened protective layer first may be adopted. That is, a method of first providing the second hardened protective layer so as to cover the inclined surface from the lower edge of the inclined surface of the dispersion cone, and then providing the first hardened protective layer, which is flush with the surface of the second hardened protective layer, at the step portion between the upper end of the dispersion cone and the lower end of the blowing pipe.
[0059] [Materials of the second cured protective layer] The second hardened protective layer 45b can be formed, for example, by using a welding rod similar to the welding rod for forming the first hardened protective layer 45a. Specifically, the second hardened protective layer 45b may be formed as a hardened layer by build-up welding. In this case, if the welding rod is further moved in the circumferential direction and the weld metal (hardened layer) is built up without leaving any gap in the radial direction, the thickness of the weld metal (hardened layer) can be easily controlled.
[0060] In addition, the number of layers of the weld metal (hardfacing layer), i.e., the number of layers of the weld metal (hardfacing layer) in the normal direction of the inclined surface of the dispersion cone, is preferably up to 2 layers. When the smelting raw material adheres to the inclined surface of the dispersion cone, a "thrust rod" for poking and removing the adhesion may be inserted through the inspection hole 23 (see FIG. 2) of the burner cone 22 to push down the adhesion. Even in such a case, the internal stress caused by welding can be suppressed by limiting the number of layers of the weld metal (hardfacing layer) to 2 layers or less, so that the inconvenience of cracks occurring and progressing in the weld metal (hardfacing layer) due to the impact of poking, and the inconvenience of peeling off can be effectively avoided.
[0061] (3) Top edge position of hardened protective layer Incidentally, the present inventor has found that when the auxiliary burner 40 is used for a certain period of time, the members below the ejection hole 42 are locally worn. This is believed to be due to the following reason. A strong vortex is formed below the ejection hole 42 due to the flow of the reaction gas outside the blowing pipe 41 and the flow of the gas ejected from the ejection hole 42. The smelting raw material caught in this vortex collides with it, causing localized wear of the members below the ejection hole 42.
[0062] When the members around the nozzle hole 42 are worn, the nozzle hole 42 may expand or deform. This changes the direction and flow rate of the gas ejected from the nozzle hole 42, causing the raw material to be dispersed unevenly. This in turn causes the density of the gas covering the inclined surface of the dispersion cone to become uneven, which in turn causes the wear of the dispersion cone to progress further, and the efficiency of the flash smelting furnace to decrease.
[0063] Therefore, in the auxiliary burner of the present invention, the position of the ejection hole 42 and the outer diameter of the upper end of the dispersion cone 43 are optimized to match the inclination angle of the inclined surface of the dispersion cone 43 so that the side edge of the hardened protective layer 45 connected to the blowing pipe 41 (i.e., the upper end of the hardened protective layer 45) is directly below the ejection hole 42, as shown in Figure 11, and therefore localized wear of the ejection hole 42 is less likely to occur.
[0064] In this way, the auxiliary burner of the present invention can prevent wear and damage to the dispersion cone and effectively suppress the enlargement and deformation of the nozzle holes, thereby making it possible to further extend the life of the dispersion cone. EXAMPLES
[0065] Next, examples of the present invention will be specifically described with reference to comparative examples.
[0066] [Example 1] An auxiliary burner according to Example 1 shown in FIG. 11 was produced in which a dispersion cone was joined to the lower end of an injection pipe having a plurality of nozzle holes on the lower peripheral surface of the pipe body, and a hardened protective layer was provided to protect the dispersion cone from wear.
[0067] Here, the hardened protective layer has a first hardened protective layer provided to fill the ring-shaped space 46 shown in Figure 9, and a second hardened protective layer that is flush with the surface of the first hardened protective layer and covers the inclined surface of the dispersion cone, and is formed by build-up welding using a tungsten carbide welding rod (ING: ``UW-O tungsten carbide build-up wire'') containing approximately 60% tungsten carbide particles and approximately 40% carbon and iron, and the number of layers of the hardened protective layer (second hardened protective layer) was two, and the upper end of the hardened protective layer was set to be directly below the nozzle hole in the blowing pipe.
[0068] In addition, in order to prevent cracking of the hardened layer, the blow pipe and the dispersion cone were preheated (preheating temperature: 400°C) when welding the blow pipe and the dispersion cone and when overlay welding the hardened layer. The hardness of the formed protective hardened layer was about 950HV and its thickness was about 5mm.
[0069] The auxiliary burner according to Example 1 thus manufactured was incorporated into a concentrate burner, and the flash smelting furnace was operated for 4 weeks to process 200 t / h to 250 t / h of raw materials for smelting. After that, the auxiliary burner was removed, and the wear state of the dispersion cone was visually observed.
[0070] As a result, almost no wear was found on the entire dispersion cone, including the upper end of the dispersion cone, which had previously been subject to significant wear.
[0071] [Comparative Example 1] The conventional auxiliary burner shown in Figures 3 and 4 (i.e., an auxiliary burner in which the outer diameter of the upper end of the dispersion cone and the outer diameter of the lower end of the blowing pipe are set to be approximately the same, and which does not have a hardened protective layer that protects the dispersion cone from wear) was installed in a concentrate burner, and a flash smelting furnace that processes 200 t / h to 250 t / h of smelting raw materials was operated for 4 weeks. After that, the auxiliary burner according to Comparative Example 1 was removed, and the wear state of the dispersion cone was visually observed.
[0072] The researchers found that the top end of the dispersion cone was particularly worn, and furthermore that the entire inclined surface of the dispersion cone was also worn. The wear was 2 to 8 mm in the thickness direction.
[0073] When the copper content of the molten metal (karami) obtained on the final day of operation was checked, it was estimated that the melting and smelting reaction in the furnace had deteriorated due to a deterioration in the dispersion of the smelting raw materials, and the copper content was approximately 20% worse than that of the molten metal (karami) in Example 1 (i.e., the amount of copper lost in the karami increased by approximately 20%).
[0074] [confirmation] Comparison with Comparative Example 1 confirmed that the auxiliary burner of Example 1 can improve the wear resistance, particularly the wear resistance of the dispersion cone, and can prevent deterioration of the copper grade in the slag over a long period of time. [Industrial Applicability]
[0075] The auxiliary burner according to the present invention can maintain the function of dispersing the smelting raw materials for a long period of time while preventing wear and damage to the dispersion cone, and therefore has industrial applicability for use as an auxiliary burner in a flash smelting furnace. [Explanation of symbols]
[0076] FF Self-melting smelting furnace 11 Settler 12 Reaction tower 13 Flue flue 14. Slit opening 15. River drain 20 Concentrate Burner 21 Windbox 22 Burner Cone 23 Inspection hatch 24 Concentrate Chute 25 Wind speed regulator 30 Auxiliary Burner 31 Blowing pipe 32 Spout hole 33 Dispersion Cone 34 Inner tube 35 Heavy Oil Burner 35a Nozzle 36 1st supply port 37 2nd supply port 40 Auxiliary Burner 41 Blowing pipe 41a surface 41b Bevel 42 Spout hole 43 Dispersion Cone 43a Extension surface part 44 Step part 45 Hardened protective layer 45a 1st hardened protective layer 45b 2nd hardened protective layer 46 Ring-shaped space
Claims
1. An auxiliary burner provided for a concentrate burner of a flash smelting furnace, comprising: a blowing pipe having a plurality of nozzles formed on a lower peripheral surface of a pipe body into which gas is supplied, for spraying the gas from the inside to the outside; A dispersion cone having a generally truncated cone shape provided at a lower end of the blowing pipe; a hardened protective layer that protects the dispersion cone from wear; Equipped with The outer diameter of the upper end of the dispersion cone is set to be larger than the outer diameter of the lower end of the blowing pipe, 1. An auxiliary burner for a flash smelting furnace, comprising: a first hardened protective layer provided at a step between an upper end of the dispersion cone and a lower end of the blowing pipe; and a second hardened protective layer that is flush with the surface of the first hardened protective layer and covers the inclined surface of the dispersion cone.
2. 2. The auxiliary burner for a flash smelting furnace according to claim 1, wherein the first hardened protective layer is provided so as to fill an imaginary ring-shaped space having a substantially triangular cross section formed by the surface of the blow pipe and the extended surface portion of the inclined surface of the dispersion cone when the inclined surface of the dispersion cone is extended from its upper end edge toward the surface of the blow pipe below the nozzle hole.
3. 3. The auxiliary burner for a flash smelting furnace according to claim 1, wherein an upper end of said hardened protective layer is set at a position directly below the nozzle hole of said blow pipe.
4. 3. The auxiliary burner for a flash smelting furnace according to claim 1, wherein the first hardened protective layer and the second hardened protective layer are made of an alloy containing 50% or more of tungsten carbide.
5. 5. The auxiliary burner for a flash smelting furnace according to claim 4, wherein the first hardened protective layer and the second hardened protective layer are formed as hardening layers by overlay welding.
6. 6. The auxiliary burner for a flash smelting furnace according to claim 5, wherein the number of layers of the hardfacing layer is two or less.
7. 3. An auxiliary burner for a flash smelting furnace as claimed in claim 1, wherein the outer diameter of the upper end of the dispersion cone is set to be at least twice as large as the outer diameter of the lower end of the blowing pipe and the thickness of the blowing pipe.
8. The auxiliary burner for a flash smelting furnace according to claim 5, characterized in that a groove is provided at the lower end of the blowing pipe, and the first hardened protective layer formed of a hardening layer is provided so as to fill the ring-shaped space including the groove portion.
Citation Information
Patent Citations
Jet nozzle of concentrate
CN104388695A
Auxiliary burner of flash smelting furnace and method for manufacturing the same
JP2021032431A
Burner cone liner and method for producing the same
JP2021191888A
Method and arrangement for controlling a burner of a suspension smelting furnace
US20200080784A1
Raw material supply device, flash furnace, and operation method of flash furnace
WO2019139079A1