Aluminum member, aluminum resin composite and method for manufacturing aluminum resin composite

By forming nano-order protrusions with amorphous alumina and α-alumina on the aluminum surface, the bonding strength and acid resistance of aluminum resin composites are enhanced, addressing the issue of resin separation in conventional composites.

JP2024150293AActive Publication Date: 2024-10-23PRIME PLANET ENERGY & SOLUTIONS INC +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023063640
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Conventional aluminum resin composites experience separation of the resin member from the aluminum member due to decomposition of the oxide film by hydrogen fluoride or hydrogen chloride, resulting in insufficient bonding strength, especially when immersed in non-aqueous electrolytes containing lithium hexafluorophosphate or hydrochloric acid.

Method used

The surface of the aluminum member is treated with a pulsed laser to form nano-order protrusions with amorphous alumina and α-alumina, enhancing the anchor effect and chemical stability, thereby improving the bonding strength and resistance to acids.

Benefits of technology

The treatment results in improved bonding strength and resistance to hydrofluoric acid and hydrochloric acid, reducing the likelihood of resin separation in non-aqueous electrolytes, thus enhancing the durability of the aluminum resin composite.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150293000001_ABST
    Figure 2024150293000001_ABST
Patent Text Reader

Abstract

To provide an aluminum member excellent in bonding strength, an aluminum resin composite, and a method for manufacturing the aluminum resin composite.SOLUTION: Projection parts (a lid upper surface projection part layer F11, a lid lower surface projection part layer F21, a terminal side projection part layer F31 and a terminal lower surface projection part layer F41) having a diameter and height of less than 1 μm in nano order are densely arranged on the surface of a member body (a lid member 30 and a positive electrode terminal member 50) made of metal aluminum. Base ends connected to a member surface in the projection parts include amorphous alumina and α-alumina .SELECTED DRAWING: Figure 14
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technical field disclosed in this specification relates to an aluminum member, an aluminum resin composite, and a method for manufacturing an aluminum resin composite. [Background technology]

[0002] An aluminum resin composite in which an aluminum member and a resin member are bonded is known. In order to increase the bonding strength between the aluminum member and the resin member, the surface of the aluminum member is roughened in advance. For example, Patent Document 1 is an example of a related prior art.

[0003] In Patent Document 1, in order to obtain an aluminum resin composite, first, the surface of the aluminum member is roughened by immersing the aluminum member in an etching agent. As a result of the roughening treatment, a fine uneven shape is formed on the surface of the aluminum member. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-164989 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when a conventional aluminum resin composite is immersed in a liquid in which water is added to a nonaqueous electrolyte containing lithium hexafluorophosphate, the resin member may separate from the aluminum member. The reason for this is explained below. Generally, a very thin oxide film is formed on the surface of the aluminum member. Therefore, in the aluminum resin composite, the resin member is bonded to the aluminum member via this oxide film. And hydrogen fluoride is generated in the liquid. Therefore, when the aluminum resin composite is immersed in the liquid, the oxide film is decomposed by the hydrogen fluoride in the liquid. As a result, the resin member separates from the aluminum member. Similarly, when the aluminum resin composite is immersed in hydrochloric acid, the oxide film is decomposed by the hydrogen chloride in the liquid, and the resin member separates from the aluminum member.

[0006] Thus, it is considered that the conventional aluminum resin composite does not have high resistance to acid or hydrofluoric acid. In other words, when an aluminum member is joined to a resin member, the joint strength of the joint is insufficient. Therefore, it has been desired to further increase the joint strength of the joint.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and its object is to provide an aluminum member, an aluminum resin composite, and a method for manufacturing an aluminum resin composite that have excellent bonding strength at the joint when joined to a resin member. [Means for solving the problem]

[0008] The metal member made for the purpose of solving the above-mentioned problems is: The surface of the component body made of metallic aluminum is densely lined with nano-order protrusions with diameters and heights of less than 1 μm. The protrusions include a base end portion connected to the surface of the member, which base end portion contains amorphous alumina and α-alumina.

[0009] According to the aluminum member of the present invention, nano-order protrusions each having a diameter and height of less than 1 μm are densely arranged on the surface of the member, and therefore, due to the anchor effect, the bonding strength of the bonding portion when the aluminum member is bonded to a resin member is improved. Furthermore, the base end of the protrusions connected to the surface of the member contains not only amorphous alumina but also α-alumina, which has excellent chemical stability, and therefore, the acid resistance and hydrofluoric acid resistance of the bonding portion are improved, and further, the difficulty of separation of the resin member when immersed in a nonaqueous electrolyte solution containing hydrochloric acid or lithium hexafluorophosphate to which water has been added is improved. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view of a battery according to an embodiment. [Diagram 2] 2 is a cross-sectional view taken along line AA in FIG. 1. [Diagram 3] FIG. [Figure 4] FIG. 2 is a perspective view of a unit member extracted from the battery of FIG. 1. [Diagram 5] 4A is a cross-sectional view taken along line BB in FIG. 4, and FIG. 4B is a cross-sectional view taken along line CC in FIG. [Figure 6] FIG. 1A is an explanatory diagram illustrating the bonding area between the upper surface of the lid member and the positive electrode resin member, and the area on the upper surface of the lid member that has been roughened; FIG. 1B is an explanatory diagram illustrating the bonding area between the lower surface of the lid member and the positive electrode resin member, and the area on the lower surface of the lid member that has been roughened. [Figure 7] FIG. 1A is an explanatory diagram illustrating a joint region between a side surface of a positive electrode terminal member and a positive electrode resin member, and a region on the side surface of the positive electrode terminal member that has been roughened; FIG. 1B is an explanatory diagram illustrating a joint region between an underside of a long straight portion of a positive electrode terminal member and a positive electrode resin member, and a region on the underside of a long straight portion of a positive electrode terminal member that has been roughened. [Figure 8]This is an image showing how a pulsed laser was irradiated onto the surface of an aluminum component under the same conditions as for the pulsed laser irradiation of the roughened area, resulting in the formation of numerous nano-order protrusions on the surface of the component, which are arranged in a dense network-like pattern. [Figure 9] (A) is an enlarged projection image of a cross-sectional sample obtained by TEM-EELS, (B-1) is a mapping image (result of chemical state analysis) showing chemical state A, (B-2) is a mapping image (result of chemical state analysis) showing chemical state B, and (B-3) is a mapping image (result of chemical state analysis) showing chemical state C. [Figure 10] This is a graph showing the EELS spectrum of an Al-related compound obtained from an analysis company and the EELS spectrum obtained from the cross-sectional sample. [Figure 11] 2 is a flowchart of a method for manufacturing a battery according to an embodiment. [Figure 12] 1A is a schematic diagram showing the roughening treatment performed on the roughened region on the underside of the lid, and FIG. 1B is a schematic diagram showing the roughening treatment performed on the roughened region on the side of the terminal. [Figure 13] 1A to 1C are diagrams illustrating an insert molding process. [Figure 14] 1A is a table showing the results of an acid resistance test, and FIG. 1B is a table showing the results of a hydrofluoric acid resistance test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The battery 1 constituting the aluminum resin composite according to the present invention is an example of an electricity storage device, specifically, a rectangular sealed lithium ion secondary battery mounted on vehicles such as hybrid cars, plug-in hybrid cars, and electric cars. In the following, the symbols X, Y, and Z relating to the directions in the drawings represent the left-right direction, the front-rear direction, and the up-down direction as specifying the direction. In addition, the symbols U, D, L, R, F, and B written at the end of the arrows relating to each direction represent the upper side, lower side, left side, right side, front side, and rear side as specifying the position. However, these directions and positions are specified for the convenience of explanation. Therefore, the direction in which the battery 1 is installed is not limited in any way.

[0012] [Battery configuration] Fig. 1 is a perspective view of a battery 1. Fig. 2 is a cross-sectional view taken along line AA in Fig. 1. As shown in Figs. 1 and 2, the battery 1 has a case 10 that seals the inside, an electrode assembly 40 housed in the case 10, an electrolyte 3 and an insulating holder 5, and a positive electrode terminal member 50 and a negative electrode terminal member 60 connected to the electrode assembly 40.

[0013] Case 10 has an overall flat rectangular parallelepiped shape with a bottom. Case 10 is composed of a body member 20 and a cover member 30. In this embodiment, case 10 is made of aluminum. However, the material of case 10 may be an aluminum-based metal other than aluminum, such as an aluminum alloy. Furthermore, the material of case 10 may be a metal other than aluminum-based metal, such as an iron-based metal.

[0014] The main body member 20 has a bottomed rectangular tube shape. The main body member 20 also has an opening 21. In other words, the main body member 20 has a rectangular plate-shaped bottom 12, a pair of front side parts 13 and rear side parts 14 that are vertically erected from the edge of the front side F and the edge of the rear side B of the bottom 12, and a pair of left side parts 15 and right side parts 16 that are vertically erected from the end of the left side L and the end of the right side R of the bottom 12. The shape of the opening 21 is a rectangle with the left-right direction X as the long side direction and the front-rear direction Y as the short side direction. The shape of the bottom 12 is a rectangular plate with the left-right direction X as the long side direction and the front-rear direction Y as the short side direction. The shape of the front side part 13 and the rear side part 14 is a rectangular plate with the left-right direction X as the long side direction and the up-down direction Z as the short side direction. The shape of the left side part 15 and the right side part 16 is a rectangular plate with the up-down direction Z as the long side direction and the up-down direction Y as the short side direction.

[0015] The height (length in the vertical direction Z) of the front portion 13 and the rear portion 14 is the same as the height (length in the vertical direction Z) of the left portion 15 and the right portion 16. Furthermore, the height (length in the vertical direction Z) of the front portion 13, etc. and the length in the horizontal direction X of the front portion 13 and the rear portion 14 are significantly longer than the length in the front-to-back direction Y of the left portion 15 and the right portion 16. Therefore, hereinafter, with regard to the case 10, the main body member 20 and the cover member 30, the horizontal direction X may be referred to as the "length direction", the front-to-back direction Y as the "width direction", and the vertical direction as the "height direction".

[0016] The lid member 30 closes the opening 21 of the main body member 20. In detail, the peripheral portion of the lid member 30 is laser welded over the entire circumference to the tip portions of the upper sides U of the front side portion 13, the rear side portion 14, the left side portion 15, and the right side portion 16. Note that at the boundary portion between the tip portion of the main body member 20 and the peripheral portion of the lid member 30, a melted and solidified portion 18 is formed over the entire circumference where the main body member 20 and the lid member 30 are melted and solidified by the laser.

[0017] A safety valve 19 is provided slightly to the left L of the center of the lid member 30 in the left-right direction X. The safety valve 19 breaks and opens when the internal pressure of the case 10 exceeds a valve opening pressure. A liquid inlet hole 30k that penetrates the lid member 30 in the up-down direction Z is formed slightly to the right R of the center of the lid member 30 in the left-right direction X. An aluminum sealing member 39 is fitted into the liquid inlet hole 30k from an upper side U, thereby airtightly sealing the liquid inlet hole 30k.

[0018] A positive electrode insertion hole 33h is formed near the end of the cover member 30 on one side in the left-right direction X (left side L in Figs. 1 and 2), penetrating the cover member 30 in the up-down direction Z. A negative electrode insertion hole 34h is formed near the end of the cover member 30 on the other side in the left-right direction X (right side R in Figs. 1 and 2), penetrating the cover member 30 in the up-down direction Z. The positive electrode insertion hole 33h and the negative electrode insertion hole 34h are formed in a rectangular shape with the left-right direction X as the long side direction and the front-rear direction Y as the short side direction. A positive electrode terminal member 50 having an overall vertically elongated shape (extending in one direction) is inserted from the upper side U along the length direction into the positive electrode insertion hole 33h. A negative electrode terminal member 60 having an overall vertically elongated shape (extending in one direction) is inserted from the upper side U along the length direction into the negative electrode insertion hole 34h.

[0019] The positive electrode terminal member 50 is fixed to the lid member 30 in a state insulated from the lid member 30 via the positive electrode resin member 70. Therefore, the positive electrode terminal member 50 is supported by the lid member 30 via the positive electrode resin member 70. In this embodiment, the positive electrode terminal member 50 is made of aluminum. However, the material of the positive electrode terminal member 50 can be appropriately set within a range that allows electrical connection with a positive electrode current collecting portion 41r of the electrode body 40 described later.

[0020] The negative electrode terminal member 60 is fixed to the lid member 30 in a state insulated from the lid member 30 via the negative electrode resin member 80. Therefore, the negative electrode terminal member 60 is supported by the lid member 30 via the negative electrode resin member 80. In this embodiment, the negative electrode terminal member 60 is made of copper. However, the material of the negative electrode terminal member 60 can be appropriately selected within a range that allows electrical connection with the negative electrode current collecting part 42r of the electrode body 40 described later.

[0021] The electrode body 40 is a so-called "wound type" electrode body. In the electrode body 40, a strip-shaped positive electrode plate 41 and a strip-shaped negative electrode plate 42 are wound in a predetermined winding direction with a strip-shaped separator 43 sandwiched therebetween. As a result, the electrode body 40 is formed in a flat shape having horizontally elongated rectangular side surfaces extending in the vertical direction Z and the horizontal direction X on the front side F and the rear side B as a whole.

[0022] The positive electrode plate 41 has a positive electrode current collecting foil (not shown) and a positive electrode active material layer (not shown) supported on the current collecting foil. The positive electrode current collecting foil is made of aluminum. However, the material of the positive electrode current collecting foil can be appropriately set within a range in which it can function as a positive electrode of a lithium ion secondary battery. On the other hand, the negative electrode plate 42 has a negative electrode current collecting foil (not shown) and a negative electrode active material layer (not shown) supported on the current collecting foil. The negative electrode current collecting foil is made of copper. However, the material of the negative electrode current collecting foil can be appropriately set within a range in which it can function as a negative electrode of a lithium ion secondary battery.

[0023] In addition, a positive electrode current collecting portion 41r is formed on the electrode body 40. The positive electrode current collecting portion 41r is a portion where the positive electrode current collecting foil is exposed. A positive electrode terminal lower portion 52 of the positive electrode terminal member 50 is bonded to the positive electrode current collecting portion 41r. Similarly, a negative electrode current collecting portion 42r is formed on the electrode body 40. The negative electrode current collecting portion 42r is a portion where the negative electrode current collecting foil is exposed. A negative electrode terminal lower portion 62 of the negative electrode terminal member 60 is bonded to the negative electrode current collecting portion 42r. Therefore, the electrode body 40 is supported by the cover member 30 via the positive electrode terminal member 50 and the negative electrode terminal member 60.

[0024] Although detailed illustration is omitted, the positive electrode current collecting portion 41r is a portion that protrudes beyond the negative electrode plate 42 and the separator 43 in the axial direction of the electrode body 40 and is wound with only the positive electrode current collecting foil. Similarly, the negative electrode current collecting portion 42r is a portion that protrudes beyond the positive electrode plate 41 and the separator 43 in the axial direction of the electrode body 40 and is wound with only the negative electrode current collecting foil. In this embodiment, the positive electrode current collecting portion 41r is formed at the end of the left side L of the electrode body 40. On the other hand, the negative electrode current collecting portion 42r is formed at the end of the right side R of the electrode body 40.

[0025] The electrode body 40 is spaced apart from the bottom 12, front side 13, rear side 14, left side 15, right side 16, and cover member 30 of the main body member 20 by a certain distance. An insulating holder 5 is disposed between the electrode body 40 and the main body member 20 to reliably maintain insulation. The shape and material of the insulating holder 5 can be appropriately set as long as it can be disposed between the electrode body 40 and the main body member 20 and can insulate the electrode body 40 from the main body member 20. In this embodiment, the insulating holder 5 is made of a strip-shaped film of polypropylene (PP), which is a synthetic resin. The insulating holder 5 is formed in a bag shape. The bag-shaped insulating holder 5 encases the electrode body 40 with the upper side U open. That is, the insulating holder 5 insulates the inner surfaces of the bottom 12 , front side 13 , rear side 14 , left side 15 and right side 16 of the body member 20 from the outer surface of the electrode body 40 facing the body member 20 .

[0026] The positive electrode resin member 70 is made of a thermoplastic resin, specifically polyphenylene sulfide (PPS). The positive electrode resin member 70 is bonded to the cover member 30 and the positive electrode terminal member 50. The cover member 30, the positive electrode terminal member 50, and the positive electrode resin member 70 are integrated by bonding the positive electrode resin member 70 to the cover member 30 and the positive electrode terminal member 50, so that the battery 1 including the integrated member constitutes a composite body of aluminum and resin. The positive electrode resin member 70 also hermetically seals the cover member 30 and the positive electrode terminal member 50 while insulating them from each other. That is, the positive electrode resin member 70 functions as an insulating member and a sealing member between the cover member 30 and the positive electrode terminal member 50. The material of the positive electrode resin member 70 can be appropriately selected as long as it can hermetically seal the lid member 30 and the positive electrode terminal member 50 while insulating them from each other, and can also be other types of resin such as other types of thermoplastic resins or thermosetting resins.

[0027] The negative electrode resin member 80 is made of a thermoplastic resin, specifically polyphenylene sulfide (PPS). The negative electrode resin member 80 is bonded to the lid member 30 and the negative electrode terminal member 60. The lid member 30, the negative electrode terminal member 60, and the negative electrode resin member 80 are integrated by bonding the negative electrode resin member 80 to the lid member 30 and the negative electrode terminal member 60, so that the battery 1 including the integrated member constitutes a composite body of metal and resin. The negative electrode resin member 80 also provides insulation between the lid member 30 and the negative electrode terminal member 60 while hermetically sealing them. That is, the negative electrode resin member 80 functions as an insulating member and a sealing member between the lid member 30 and the negative electrode terminal member 60. The material of the negative electrode resin member 80 can be appropriately selected as long as it can hermetically seal the lid member 30 and the negative electrode terminal member 60 while insulating them from each other, and can also be other types of resin such as other types of thermoplastic resins or thermosetting resins.

[0028] Next, the shape of the positive electrode terminal member 50 will be described. Fig. 3 is a perspective view of the positive electrode terminal member 50. As shown in Fig. 3, the positive electrode terminal member 50 has a positive electrode terminal upper part 51, a positive electrode terminal lower part 52, and a positive electrode terminal intermediate part 53. In the battery 1, the positive electrode terminal upper part 51 is disposed relatively on the upper side U. The positive electrode terminal lower part 52 is disposed relatively on the lower side D.

[0029] The positive terminal upper part 51 has a constant L-shaped cross-sectional shape in one direction. In detail, one straight line portion of the L-shape is longer than the other straight line portion of the L-shape. Therefore, the rectangular plate-shaped portion of the positive terminal upper part 51 that corresponds to the longer straight line portion of the L-shaped cross-sectional shape is referred to as the "long straight line portion 51a," and the portion extending perpendicularly from one edge of the long straight line portion 51a is referred to as the "short straight line portion 51b."

[0030] In the following description of the positive electrode terminal member 50, for convenience, the symbols O, P, and Q shown in FIG. 3 are used to specify directions. The symbols O, P, and Q represent "the direction in which the L-shaped cross-sectional shape of the positive electrode terminal upper part 51 extends at a constant rate," "the direction along the straight line of the long straight portion 51a," and "the direction along the straight line of the short straight portion 51b," respectively. In addition, in the following description of the positive electrode terminal member 50, the side in the third direction Q where the positive electrode terminal upper part 51 is located may be referred to as the "upper side," and the side in the third direction Q where the positive electrode terminal lower part 52 is located may be referred to as the "lower side."

[0031] The positive terminal lower portion 52 is formed perpendicular to the long straight portion 51a as a whole. The positive terminal lower portion 52 is shaped like a rectangular plate with its long side in the third direction Q and its short side in the second direction P. In addition, in the first direction O, a part of the positive terminal lower portion 52 fits inside the positive terminal upper portion 51, and another part protrudes outside the positive terminal upper portion 51. In addition, in the second direction P, a part of the positive terminal lower portion 52 fits inside the positive terminal upper portion 51, and another part protrudes outside the positive terminal upper portion 51.

[0032] The positive terminal intermediate portion 53 has an overall crank shape, and connects the positive terminal upper portion 51 and the positive terminal lower portion 52. When viewed from the second direction P, the positive terminal intermediate portion 53 has a rectangular shape with its longer side in the first direction O and its shorter side in the third direction. The length of the positive terminal intermediate portion 53 in the first direction O is longer than the length of the positive terminal lower portion 52 in the first direction O. The side surface of the positive terminal lower portion 52 that protrudes outward from the positive terminal upper portion 51 in the first direction O is continuous with the side surface of the positive terminal intermediate portion 53 on the same side in the first direction O.

[0033] In addition, both surfaces of the positive terminal intermediate portion 53 perpendicular to the second direction P near the connection to the short straight portion 51b are formed on the same plane as both surfaces of the short straight portion 51b perpendicular to the second direction P. Hereinafter, the portion of the positive terminal intermediate portion 53 formed on the same plane as both surfaces of the short straight portion 51b perpendicular to the second direction P is referred to as the "upper connection portion 53a". The surface of the positive terminal upper portion 51 including the short straight portion 51b on the side where the positive terminal lower portion 52 is located in the second direction P is flush with the surface of the upper connection portion 53a on the same side. In addition, on the opposite side of the short straight portion 51b in the third direction Q of the upper connection portion 53a, a bent portion 53b is formed that is bent in a crank shape toward the outside of the positive terminal upper portion 51 along the second direction P.

[0034] In this embodiment, the shape of the negative electrode terminal member 60 is the same as that of the positive electrode terminal member 50. Therefore, a description using a perspective view of the negative electrode terminal member 60 will be omitted, but the negative electrode terminal member 60 has a negative electrode terminal upper portion 61, a negative electrode terminal lower portion 62, and a negative electrode terminal intermediate portion 63 corresponding to the positive electrode terminal upper portion 51, the positive electrode terminal lower portion 52, and the positive electrode terminal intermediate portion 53, similar to the positive electrode terminal member 50.

[0035] Next, the joint structure between the positive electrode resin member 70 and the lid member 30 and the positive electrode terminal member 50, and the roughening treatment of the lid member 30 and the positive electrode terminal member 50 will be described. FIG. 4 is a perspective view of a unit member 1A consisting of the lid member 30, the positive electrode terminal member 50, the positive electrode resin member 70, the negative electrode terminal member 60, and the negative electrode resin member 80, which are integrated and form a part of the battery 1 shown in FIG. 1 and FIG. 2. FIG. 5(A) is a BB cross-sectional view of FIG. 4, and FIG. 5(B) is a CC cross-sectional view of FIG. 4. FIG. 6 is an explanatory diagram for explaining the joint region between the lid member 30 and the positive electrode resin member 70, and the region of the lid member 30 that has been roughened. FIG. 7 is an explanatory diagram for explaining the joint region between the positive electrode terminal member 50 and the positive electrode resin member 70, and the region of the positive electrode terminal member 50 that has been roughened.

[0036] The positive electrode terminal member 50 is fixed to the lid member 30 via the positive electrode resin member 70 with the first direction O parallel to the left-right direction X and the positive electrode terminal lower portion 52 disposed on the rear side B. On the other hand, the negative electrode terminal member 60 is fixed to the lid member 30 via the negative electrode resin member 80 with the first direction O parallel to the left-right direction X and the negative electrode terminal lower portion 62 disposed on the front side F.

[0037] The top surface of the long straight portion 51a is exposed to the upper side U. In addition, the top surface of the cover member 30 and the bottom surface of the long straight portion 51a are disposed at substantially the same position in the vertical direction Z. Furthermore, the bottom surface of the short straight portion 51b is disposed at a position slightly lower than the bottom surface of the cover member 30 in the vertical direction Z. In a plan view (a line of sight from the upper side U to the lower side D), the long straight portion 51a of the positive electrode terminal member 50 inserted into the positive electrode insertion hole 33h is completely contained within the positive electrode insertion hole 33h. In the left-right direction X and the front-rear direction Y, the long straight portion 51a is disposed at substantially the center of the positive electrode insertion hole 33h.

[0038] The positive electrode resin member 70 is formed in the vertical direction Z from the upper end of the positive electrode terminal upper part 51 to a position slightly above the lower end of the upper connection part 53a. The positive electrode resin member 70 hermetically seals the gap between the cover member 30 and the positive electrode terminal member 50. As described later, in this embodiment, the positive electrode resin member 70 is integrally formed by insert molding. For convenience, the portion of the positive electrode resin member 70 above the upper surface of the cover member 30 is referred to as the "positive electrode resin upper part 71", the portion below the lower surface of the cover member 30 is referred to as the "positive electrode resin lower part 72", and the portion between the upper and lower surfaces of the cover member 30, in other words, the portion filled in the positive electrode insertion hole 33h, is referred to as the "positive electrode resin middle part 73".

[0039] The positive electrode resin upper portion 71 has a positive electrode resin upper frame portion 71a that surrounds the entire periphery of the long straight portion 51a, and a positive electrode resin upper protrusion portion 71b that is connected to the positive electrode resin upper frame portion 71a.

[0040] The positive resin upper frame portion 71a is formed in a rectangular frame shape. The first width W1, which is the distance from the inner edge to the outer edge of each straight portion of the positive resin upper frame portion 71a, is approximately the same. The positive resin upper protrusion portion 71b is formed to protrude toward the right side R from a part of the range of approximately the center of the straight portion formed on the right side R of the positive resin upper frame portion 71a. The shape of the positive resin upper protrusion portion 71b is a rectangular plate shape with the left-right direction X as the long side direction and the front-rear direction Y as the short side direction. The length of the positive resin upper protrusion portion 71b in the left-right direction X and the length of the front-rear direction Y are longer than the first width W1. The positive resin upper protrusion portion 71b is a portion where a gate member GT (see FIG. 13) into which molten resin is injected during the insert molding is placed.

[0041] The positive electrode resin upper frame portion 71a is joined to the entire outer surface of the long straight portion 51a and to a rectangular annular lid upper frame joining region E11 that surrounds the entire edge of the positive electrode insertion hole 33h on the upper surface of the lid member 30. A second width W2, which is the distance from the inner edge to the outer edge of each straight portion of the lid upper frame joining region E11, is approximately the same. The positive electrode resin upper protrusion 71b is joined to the upper surface of the lid member 30 over the entire bottom surface.

[0042] In the following, the region on the upper surface of the lid member 30 that is joined to the positive electrode resin upper protrusion 71b is referred to as the "lid upper surface rectangular joining region E12". The lid upper surface rectangular joining region E12 is formed by protruding toward the right side R from a part of the range of approximately the center of the straight part on the right side R of the lid upper surface frame-shaped joining region E11. That is, the lid upper surface frame-shaped joining region E11 and the lid upper surface rectangular joining region E12 are connected to each other and constitute a joining region with the positive electrode resin member 70 on the upper surface of the lid member 30. Therefore, the lid upper surface frame-shaped joining region E11 and the lid upper surface rectangular joining region E12 are collectively referred to as the "lid upper surface joining region E1".

[0043] The positive electrode resin lower portion 72 is generally formed in a rectangular plate shape with its long sides in the left-right direction X and its short sides in the front-rear direction Y. The overlapping portions of the positive electrode terminal member 50 in the up-down direction Z are completely embedded inside the positive electrode resin lower portion 72. Therefore, the positive electrode resin lower portion 72 is joined to the entire outer surfaces of the overlapping portions of the short straight portion 51b and the upper connection portion 53a of the positive electrode terminal member 50 in the up-down direction Z.

[0044] The positive electrode resin lower portion 72 is joined to a rectangular annular lid underside joining region E2 that completely surrounds the edge of the positive electrode insertion hole 33h on the underside of the lid member 30. The distances from the inner edge to the outer edge of each straight portion of the lid underside joining region E2 are substantially the same on the front side F and the rear side B and are substantially the same on the left side L and the right side R. A fourth width W4, which is the distance from the inner edge to the outer edge of the straight portion on the left side L and the right side R, is wider than a third width W3, which is the distance from the inner edge to the outer edge of the straight portion on the front side F and the rear side B.

[0045] The positive electrode resin intermediate portion 73 is connected to the positive electrode resin upper portion 71 and the positive electrode resin lower portion 72. The positive electrode resin intermediate portion 73 is filled in the positive electrode insertion hole 33h. Therefore, the positive electrode resin intermediate portion 73 is joined to the inner surface of the positive electrode insertion hole 33h of the cover member 30 over the entire circumference. Furthermore, the portion of the short straight portion 51b of the positive electrode terminal member 50 that overlaps in the vertical direction Z is completely embedded inside the positive electrode resin intermediate portion 73. Therefore, the positive electrode resin intermediate portion 73 is joined to the entire outer surface of the portion of the short straight portion 51b of the positive electrode terminal member 50 that overlaps in the vertical direction Z.

[0046] The entire outer surface of the long straight portion 51a of the positive terminal member 50 is joined to the positive resin upper frame portion 71a. The entire outer surface of the short straight portion 51b of the positive terminal member 50 overlapping with the positive resin intermediate portion 73 and the positive resin lower portion 72 in the vertical direction Z is joined to the positive resin intermediate portion 73 and the positive resin lower portion 72. The entire outer surface of the upper connection portion 53a of the positive terminal member 50 overlapping with the positive resin lower portion 72 in the vertical direction Z is joined to the positive resin intermediate portion 73 and the positive resin lower portion 72. Therefore, the region of the side surface of the positive terminal member 50 that is flush across the positive terminal upper portion 51 and the upper connection portion 53a and that is joined to the positive resin member 70 is referred to as the "terminal side surface joining region E3." In addition, the area that is joined to the positive electrode resin member 70, which is the entire lower surface of the long straight portion 51a on the side of the positive electrode terminal member 50 in the third direction Q on which the positive electrode terminal lower portion 52 is formed, is referred to as the "terminal lower surface joining area E4."

[0047] Thus, the cover member 30 and the positive electrode terminal member 50 have a plurality of bonding regions with the positive electrode resin member 70. Then, in order to improve the sealing performance, specific regions of the cover member 30 and the positive electrode terminal member 50, including the bonding regions with the positive electrode resin member 70, are subjected to a roughening treatment by pulse laser irradiation. The roughening treatment will now be described.

[0048] Roughening treatment is applied to a lid upper surface roughened region F1 that completely surrounds and contains inside the lid upper surface joining region E1 on the upper surface of the lid member 30, and a lid lower surface roughened region F2 that completely surrounds and contains inside the lid lower surface joining region E2 on the lower surface of the lid member 30. Furthermore, roughening treatment is applied to a terminal side surface roughened region F3 that completely surrounds and contains inside the terminal side surface joining region E3 by the entire side surface that is flush across the positive terminal upper portion 51 and the upper connection portion 53a of the positive terminal member 50, and a terminal lower surface roughened region F4 which is the terminal lower surface joining region E4 itself.

[0049] Although detailed conditions will be described later, the roughening treatment of the roughened lid upper surface region F1, the roughened lid lower surface region F2, the roughened terminal side surface region F3, and the roughened terminal lower surface region F4 is performed by pulsed laser irradiation. In the roughened lid upper surface region F1, the roughened lid lower surface region F2, the roughened terminal side surface region F3, and the roughened terminal lower surface region F4, numerous protrusions are arranged in a dense mesh-like pattern overall.

[0050] "A large number of protrusions are densely arranged in a mesh-like state" means that the protrusions formed by pulsed laser irradiation are arranged (standing tall) at a distance between adjacent protrusions in a planar view at least equal to or less than the overall average diameter of the protrusions, and the gaps between the protrusions are also two-dimensionally expanded and connected in an approximately lattice shape. The approximately lattice shape here includes planar shapes other than a rectangle, such as a rhombus, and is not particularly limited. In addition, the approximately lattice shape may be uniform overall, or may not be uniform.

[0051] The protrusions formed in the roughened lid upper surface region F1 and the roughened lid lower surface region F2 are formed by debris particles generated by irradiating the surface of the lid member 30 with a pulsed laser, which are linked together in a string of beads and extend generally in the height direction. Similarly, the protrusions formed in the roughened terminal side surface region F3 and the roughened terminal lower surface region F4 are formed by debris particles generated by irradiating the surface of the positive terminal member 50 with a pulsed laser, which are linked together in a string of beads and extend generally in the height direction.

[0052] Debris particles are particles with a diameter of 100 nm or less that are formed when the surface of a metal component is irradiated with a pulsed laser, causing part of the surface to explosively evaporate, and then condense compounds produced by reactions between metal vapor or metal atoms and atmospheric gas. These particles then fall onto the surface near the position where the pulsed laser is irradiated.

[0053] The numerous protrusions in the roughened lid upper surface region F1 are collectively referred to as the "lid upper surface protrusion layer F11." Similarly, the numerous protrusions in the roughened lid lower surface region F2, the roughened terminal side surface region F3, and the roughened terminal lower surface region F4 are collectively referred to as the "lid lower surface protrusion layer F21," "terminal side surface protrusion layer F31," and "terminal lower surface protrusion layer F41."

[0054] The diameter of the numerous protrusions included in each of the protrusion layers F11 to F41 is 5 nm to 20 nm. The overall average diameter (average diameter) of the numerous protrusions included in each of the protrusion layers F11 to F41 is on the nano order of less than 1 μm. "Nano order of less than 1 μm" means on the "nm" level, in other words, several nm to several hundred nm.

[0055] The following method is one example of a method for calculating the average diameter of the multiple protrusions included in each of the protrusion layers F11 to F41. First, a cross-sectional sample of the joint portion between the cover member 30 or the positive electrode terminal member 50 and the positive electrode resin member 70 is prepared using a predetermined cross-sectional sample preparation device (for example, a Cross Section Polisher (registered trademark): manufactured by JEOL Ltd.). Next, the cross-sectional sample is observed using a field emission scanning electron microscope (FE-SEM). Then, the ridge lines of the protrusions of the cover member 30 or the positive electrode terminal member 50 in the cross-sectional sample are identified. Finally, the average diameter of the multiple protrusions in the cross-sectional sample is measured based on the identified ridge lines.

[0056] The height of the multiple protrusions included in each of the protrusion layers F11 to F41 is 10 nm to 1000 nm. The overall average height (average height) of the multiple protrusions included in each of the protrusion layers F11 to F41 is on the nano order of less than 1 μm. However, the average height of the multiple protrusions included in each of the protrusion layers F11 to F41 is preferably 84 nm to 1000 nm.

[0057] The following method is one example of a method for calculating the average height of a large number of protrusions included in each of the protrusion layers F11 to F41. In this calculation method, first, a plate-shaped aluminum member is prepared as a test piece. This aluminum member test piece is referred to as the "average height test piece." Then, one entire plane of the average height test piece is irradiated with a pulse laser under the same conditions as the pulse laser irradiation for each of the roughened regions F1 to F4.

[0058] Next, a cross-sectional sample including the flat portion irradiated with the pulsed laser is prepared from the test piece for average height using a predetermined cross-sectional sample preparation device (for example, Cross Section Polisher (registered trademark): manufactured by JEOL Ltd.). The cross-sectional sample is parallel to the thickness direction of the test piece for average height. Next, a cross-sectional image of the cross-sectional sample is obtained using a scanning electron microscope (JEM ARM 200F Dual-X: manufactured by JEOL Ltd.). The magnification of this cross-sectional image is 150,000 times.

[0059] Next, the cross-sectional area and base length of the protrusions in the cross-sectional image are measured using the image processing software "ImageJ". Then, the average height of the protrusions is calculated using the following formula 1. [Formula 1] TIFF2024150293000002.tif9159

[0060] Here, an image is shown in Fig. 8, which shows how a surface of an aluminum member is actually irradiated with a pulsed laser under the same conditions as those for the pulsed laser irradiation of the roughened regions F1 to F4, and how numerous protrusions of nano-order level are formed on the member surface and arranged in a dense mesh-like state. As shown in Fig. 8, numerous protrusions with diameters and heights of nano-order level are arranged in a dense mesh-like state. Note that one interval of the scale written in the lower right corner of the lower image in Fig. 8 represents 30 nm.

[0061] Each of the protrusion layers F11 to F41 as a whole contains metallic aluminum, amorphous alumina, and α-alumina. Furthermore, at least the base end portion of each of the protrusion layers F11 to F41, in other words, the range from the base of the protrusion to a height of 20 nm, contains amorphous alumina and α-alumina.

[0062] The presence of metallic aluminum, amorphous alumina and α-alumina in the protrusions could be confirmed by element mapping. Specifically, first, a cross-sectional sample was prepared by FIB (Focused Ion Beam) method from the surface of the aluminum member irradiated with a pulsed laser under the same conditions as the pulsed laser irradiation for the roughened regions F1 to F4. The cross-sectional sample included the boundaries between the aluminum member and the numerous protrusions. Next, an enlarged projection image of the cross-sectional sample and the results of chemical state analysis were obtained by TEM-EELS (Transmission Electron Microscopy-Electron Energy Loss Spectroscopy).

[0063] Fig. 9(A) is an enlarged projection image of a cross-sectional sample obtained by TEM-EELS. Fig. 9(B-1) to Fig. 9(B-3) are mapping images of the chemical states contained in the cross-sectional sample obtained by TEM-EELS. In detail, Fig. 9(B-1) is a mapping image (chemical state analysis result) showing chemical state A, Fig. 9(B-2) is a mapping image (chemical state analysis result) showing chemical state B, and Fig. 9(B-3) is a mapping image (chemical state analysis result) showing chemical state C.

[0064] It is believed that chemical state A is metallic aluminum, chemical state B is α-alumina, and chemical state C is amorphous alumina. This is based on a comparison of the EELS spectrum of Al-related compounds previously obtained from an analysis company (Toray Research Center, Inc.) with the EELS spectrum obtained from this cross-sectional sample. For reference, each spectrum is shown in Figure 10.

[0065] The following can be inferred from Figures 9(B-1) to 9(B-3). (1) Metallic aluminum and aluminum oxide (amorphous alumina and α-alumina) are present throughout the protrusion. (2) Amorphous alumina and α-alumina are mixed at the base end of the protrusion, in other words, the area of ​​α-alumina / area of ​​amorphous alumina is >0.01. (3) At the base end of the protrusion (within 20 nm from the base), the area of ​​α-alumina is larger than the area of ​​amorphous alumina; in other words, there is more α-alumina than amorphous alumina. (4) Although the amount is small compared to amorphous alumina and α-alumina, metallic aluminum is included in the base end portion of the protrusion. The area of ​​aluminum oxide (amorphous alumina + α-alumina) / area of ​​metallic aluminum + area of ​​aluminum oxide is > 90%.

[0066] The resin (polyphenylene sulfide) of the positive electrode resin member 70 is impregnated up to the base ends (roots) of the protrusions. In other words, the positive electrode resin member 70 is joined to the cover member 30 and the positive electrode terminal member 50 at the base ends (roots) of the protrusions. The fact that the positive electrode resin member 70 is joined to the cover member 30 and the positive electrode terminal member 50 at the base ends (roots) of the protrusions means that the positive electrode resin member 70 is joined to the cover member 30 and the positive electrode terminal member 50 even at the tip ends of the protrusions.

[0067] The joint structure between the negative electrode resin member 80 and the lid member 30 and the negative electrode terminal member 60 is configured similarly to the joint structure between the positive electrode resin member 70 and the lid member 30 and the positive electrode terminal member 50 described above with reference to Figures 5 to 7. The roughening treatment of the joint region between the lid member 30 and the negative electrode resin member 80 and the joint region between the negative electrode terminal member 60 and the negative electrode resin member 80 is configured similarly to the roughening treatment of the lid member 30 and the positive electrode terminal member 50 described above with reference to Figures 5 to 7.

[0068] [Battery manufacturing] Next, a manufacturing method of the battery 1 will be described with reference to the flowchart of Fig. 11. The manufacturing method of the battery 1 includes a member preparation step S1, a protrusion formation step S2, an insert molding step S3, a lid assembly completion step S4, a closing step S5, a welding step S6, a liquid injection / sealing step S7, and an initial charging / aging step S8.

[0069] In the member preparation step S1, the cover member 30, the positive electrode terminal member 50, and the negative electrode terminal member 60 are prepared. Specifically, the liquid injection hole 30k, the positive electrode insertion hole 33h, the negative electrode insertion hole 34h, and the safety valve 19 are formed in an aluminum plate by a conventional general processing method to obtain the cover member 30. In addition, the positive electrode terminal member 50 having the shape shown in FIG. 3 is obtained from the aluminum plate by a conventional general processing method. Furthermore, the negative electrode terminal member 60 having the same shape as the positive electrode terminal member 50 is obtained from a copper plate by a conventional general processing method.

[0070] Following the member preparation step S1, a protrusion formation step S2 is performed. In the protrusion formation step S2, a pulsed laser is irradiated onto the surface of the lid member 30 that may become the lid upper surface roughened region F1 and the lid lower surface roughened region F2 in a state where no protrusions are formed, thereby forming the lid upper surface roughened region F1 and the lid lower surface roughened region F2. Similarly, in the protrusion formation step S2, a terminal side surface roughened region F3 and a terminal lower surface roughened region F4 are formed on the surface of the positive electrode terminal member 50 that may become the terminal side surface roughened region F3 and the terminal lower surface roughened region F4 in a state where no protrusions are formed.

[0071] As an example of the irradiation conditions of the pulsed laser irradiation in the protrusion forming step S2, the energy density of one pulse of the laser irradiation is 24 J / cm for aluminum. 2 , and 32 J / cm for copper. 2 For example, for aluminum, the wavelength is set to 1060 nm, the average power to 25 W, the pulse period to 40 μs, the pulse width to 50 ns, the spot diameter to 63 μm, the feed rate to 1450 mm / s, and the line pitch to 0.059 mm. Fig. 12 is a schematic diagram showing the trajectory of pulse laser irradiation when the pulse laser is irradiated to the lid undersurface roughened region F2 and the terminal side surface roughened region F3 in the protrusion forming process S2.

[0072] As shown in FIG. 12(A), the lid underside roughened region F2 is irradiated with a pulsed laser at the tip (the side marked "start point" in FIG. 12(A)) of one side (the left side L in FIG. 12(A)) along the left-right direction X in the lid underside roughened region F2, proceeding to one side in the front-rear direction Y (the rear side B in FIG. 12(A)). Next, the pulsed laser is irradiated by shifting the other side in the front-rear direction Y (the front side F in FIG. 12(A)) by the set line pitch (0.059 mm). Then, the pulsed laser is irradiated by shifting the other side in the front-rear direction X (the right side R in FIG. 12(A)) by the set line pitch (0.059 mm) and proceeding again (the rear side B in FIG. 12(A)). Thereafter, the pulsed laser irradiation is repeated to travel to one side or the other side in the front-to-back direction Y until it reaches the tip (the side marked "end point" in FIG. 12(A)) of the other side (the right side R in FIG. 12(A)) along the left-right direction X in the lid underside roughened region F2.

[0073] By irradiating the lid undersurface roughened region F2 with a pulsed laser under the above conditions, protrusions containing aluminum metal, amorphous alumina and α-alumina and having diameters and heights on the nano-order level are formed in a dense network pattern on the surface of the lid member 30 made of aluminum metal.

[0074] The position where pulsed laser irradiation starts for the roughened lid undersurface region F2 (the side marked "start point" in FIG. 12(A)) is not limited to FIG. 12(A), and the side marked "end point" in FIG. 12(A) may be the position where pulsed laser irradiation starts. Pulsed laser irradiation for the roughened lid upper surface region F1 is also performed in the same manner as the pulsed laser irradiation for the roughened lid lower surface region F2 shown in FIG. 12(A). However, pulsed laser irradiation for the roughened lid upper surface region F1 and pulsed laser irradiation for the roughened lid lower surface region F2 may be performed in different manners.

[0075] As shown in FIG. 12B, the terminal side roughened region F3 is irradiated with a pulsed laser beam traveling in one of the second directions P of the positive terminal member 50 at the tip of one side of the terminal side roughened region F3 along the third direction Q of the positive terminal member 50 (the side marked "start point" in FIG. 12B). Next, the pulsed laser beam is shifted to the other side of the positive terminal member 50 along the third direction Q by the set line pitch (0.059 mm) and travels in the other of the second directions P. Then, the pulsed laser beam is shifted to the other side of the positive terminal member 50 along the third direction Q by the set line pitch (0.059 mm) and travels in one of the second directions P again. Thereafter, the pulsed laser beam irradiation traveling in one or the other of the second directions P is repeated until the pulsed laser beam irradiation traveling in one or the other of the second directions P reaches the tip of the other side of the terminal side roughened region F3 along the third direction Q (the side marked "end point" in FIG. 12B).

[0076] By irradiating the terminal side roughened region F3 with a pulsed laser under the above conditions in this manner, protrusions containing metallic aluminum, amorphous alumina, and α-alumina and having diameters and heights on the nano-order level are formed in a dense, mesh-like pattern on the surface of the positive electrode terminal member 50 made of metallic aluminum.

[0077] The position where the pulsed laser irradiation is started for the rough terminal side surface region F3 (the side marked "start point" in FIG. 12(B)) is not limited to FIG. 12(B), and the side marked "end point" in FIG. 12(B) may be the position where the pulsed laser irradiation is started. The pulsed laser irradiation for the rough terminal lower surface region F4 is also performed in the same manner as the pulsed laser irradiation for the rough terminal side surface region F3 shown in FIG. 12(B). However, in this case, the direction in which the pulsed laser irradiation proceeds is the same as the laser irradiation for the rough terminal side surface region F3, but the start position and end position of the pulsed laser irradiation are the tip on one side and the tip on the other side of the rough terminal lower surface region F4 along the second direction P of the positive electrode terminal member 50. Furthermore, the direction in which the pulsed laser irradiation is shifted by the set line pitch (0.059 mm) is one of the second directions P of the positive electrode terminal member 50.

[0078] In the protrusion forming process S2, the joining region of the lid member 30 around the negative electrode insertion hole 34h with the negative electrode resin member 80 is irradiated with a pulse laser in substantially the same manner as the lid upper surface roughened region F1 and the lid lower surface roughened region F2, except for the energy density. Similarly, the joining region of the negative electrode terminal member 60 with the negative electrode resin member 80 is irradiated with a pulse laser in substantially the same manner as the terminal side surface roughened region F3 and the terminal lower surface roughened region F4, except for the energy density. Here, "substantially the same manner" refers to the region to be irradiated with the pulse laser and the conditions for the pulse laser irradiation.

[0079] After the protrusion forming step S2, the insert molding step S3 is performed. In the insert molding step S3, a positive electrode resin member 70 and a negative electrode resin member 80 are formed, and the positive electrode resin member 70 is joined to the lid member 30 and the positive electrode terminal member 50 to be integrated, and the negative electrode resin member 80 is joined to the lid member 30 and the negative electrode terminal member 60 to be integrated. That is, the unit member 1A, which is an aluminum resin composite, is manufactured. FIG. 13 is an explanatory diagram that shows a schematic representation of the insert molding step S3 on the positive electrode terminal member 50 side.

[0080] In the insert molding step S3, a mold DE is used. The mold DE has a lower mold DE1 arranged on the lower side and an upper mold DE2 arranged on the upper side. First, the lower mold DE1 and the upper mold DE2 are set to place the cover member 30, the positive electrode terminal member 50, and the negative electrode terminal member 60 in predetermined positions. At this time, the positive electrode terminal member 50 inserted in the positive electrode insertion hole 33h, the negative electrode terminal member 60 inserted in the negative electrode insertion hole 34h, and the cover member 30 are integrally supported by the mold DE. In addition, a space corresponding to the positive electrode resin member 70 and the negative electrode resin member 80 is formed by the set lower mold DE1 and upper mold DE2.

[0081] In the insert molding process S3, first, a filling process S31 is performed, and then a solidification process S32 is performed. In the filling process S31, as shown in Fig. 13, the molten resin MR, which is the material of the positive electrode resin member 70 and the negative electrode resin member 80, is injected from the gate member GT through the upper mold DE2 into the space formed by the lower mold DE1 and the upper mold DE2. At this time, for example, the molten resin MR fills the gaps between the many protrusions until it reaches the bases of the protrusions.

[0082] The material of the positive electrode resin member 70 and the negative electrode resin member 80 is mainly composed of polyphenylene sulfide. The material of the positive electrode resin member 70 and the negative electrode resin member 80 contains a glass filler. The linear expansion coefficient of the material of the positive electrode resin member 70 and the negative electrode resin member 80 is set between the linear expansion coefficient of copper (1.65) and the linear expansion coefficient of aluminum (2.31).

[0083] After the injection of the molten resin MR is completed, the molten resin MR is appropriately cooled in the solidification step S32 to form the positive electrode resin member 70 and the negative electrode resin member 80. In detail, for example, the molten resin MR filled in the gaps between the many protrusions included in the roughened regions F1 to F4 until it reaches the base of the protrusions in the filling step S31 is solidified to form the positive electrode resin member 70 bonded to the bonding regions E1 to E4 including the roughened regions F1 to F4. Similarly, the negative electrode resin member 80 is also formed. Then, the upper mold DE2 is moved upward, and the unit member 1A consisting of the integrated lid member 30, the positive electrode resin member 70, the positive electrode terminal member 50, the negative electrode resin member 80, and the negative electrode terminal member 60 is taken out from the lower mold DE1.

[0084] After the insert molding step S3, a lid assembly completion step S4 is performed. In the lid assembly completion step S4, the lid assembly is completed. Specifically, the electrode body 40 is prepared, and the positive electrode terminal lower part 52 and the negative electrode terminal lower part 62 of the unit member 1A generated in the insert molding step S3 are welded and connected to the positive electrode current collecting part 41r and the negative electrode current collecting part 42r of the electrode body 40, respectively. Thereafter, the electrode body 40 in this state is wrapped in a bag-shaped insulating holder 5. As a result, a lid assembly consisting of the lid member 30, the positive electrode terminal member 50, the negative electrode terminal member 60, the positive electrode resin member 70, the negative electrode resin member 80, the electrode body 40, and the insulating holder 5 is completed.

[0085] Following the lid assembly completion step S4, a closing step S5 is performed. In the closing step S5, a main body member 20 is prepared, and the portion of the lid assembly completed in the lid assembly completion step S4 below the lid member 30, including the electrode body 40 and the insulating holder 5, is inserted into the main body member 20, and the opening 21 of the main body member 20 is closed with the lid member 30.

[0086] Following the closing step S5, a welding step S6 is performed. In the welding step S6, the leading ends of the front side portion 13, the rear side portion 14, the left side portion 15, and the right side portion 16 of the main body member 20 are laser-welded to the peripheral edge portion of the cover member 30 along the entire periphery, thereby hermetically sealing the opening 21.

[0087] Following the welding step S6, a liquid injection / sealing step S7 is performed. In the liquid injection / sealing step S7, the electrolyte 3 is injected into the case 10 through the liquid injection hole 30k, and the electrolyte 3 is impregnated into the electrode body 40. Thereafter, the sealing member 39 is fitted into the liquid injection hole 30k from the upper side U, and the sealing member 39 is welded to the lid member 30 around its entire periphery to hermetically seal the gap between the sealing member 39 and the lid member 30.

[0088] Following the liquid injection and sealing step S7, a charging and aging step S8 is performed. In the charging and aging step S8, a charging device (not shown) is connected to the battery 1 to initially charge the battery 1. The initially charged battery 1 is then left for a predetermined period of time to age the battery 1. In this manner, the battery 1 is completed.

[0089] Next, an experiment for verifying the acid resistance and hydrofluoric acid resistance of the joint between the aluminum member and the resin member will be described. The experiment was conducted by the applicant. The experiment is also referred to as the "joint durability verification experiment." The joint durability verification experiment is composed of the following three steps (1) to (3). (1) Production of test specimens (2) Acid resistance test (3) Hydrofluoric acid resistance test

[0090] First, (1) the production of the test specimen will be described. The test specimen is a specimen for a joint durability verification experiment. The test specimen is formed by joining a plate-shaped aluminum member and a resin member. The resin member is made of polyphenylene sulfide (PPS). The plate-shaped aluminum member is made of metallic aluminum. The plate-shaped aluminum members include one whose surface is irradiated with a pulsed laser under the irradiation conditions related to the protrusion formation step S2 described above, and one whose surface is not irradiated with a pulsed laser.

[0091] In the following, the aluminum components irradiated with the pulsed laser are referred to as “irradiated aluminum components,” and the aluminum components not irradiated with the pulsed laser are referred to as “non-irradiated aluminum components.” In the joint durability verification experiment, three irradiated aluminum components and three non-irradiated aluminum components were prepared for the acid resistance test, and three irradiated aluminum components and three non-irradiated aluminum components were prepared for the hydrofluoric acid resistance test.

[0092] Each aluminum member is generally formed into a square in plan view, with each side of the square measuring 50 mm, and the thickness of the metal member being 0.5 mm.

[0093] Furthermore, a roughened region is formed on the surface of each irradiated aluminum member on the side to be joined with the resin member by irradiating with a pulsed laser under the irradiation conditions for the protrusion forming step S2 described above. The shape of the roughened region is a circle with a diameter of 20 mm. The center of the roughened region approximately coincides with the center of the irradiated aluminum member. In the roughened region, a large number of protrusions with diameters and heights on the nano-order level are formed in a dense mesh-like arrangement, similar to the above-mentioned roughened regions F1 to F4.

[0094] A resin member is joined to each aluminum member by insert molding. The resin member is in the shape of a circular plate. The diameter of the resin member is 16 mm, and the height of the resin member is 3 mm. The center of the resin member is approximately the same as the center of the aluminum member. In this experiment, the resin member is joined to the irradiated aluminum member within the roughened region.

[0095] Next, (2) the acid resistance test will be described. In the acid resistance test, the irradiated aluminum member and the non-irradiated aluminum member were each immersed in 0.1 mol / L hydrochloric acid. Then, 1, 5, and 24 hours after immersion, each of the irradiated aluminum member and the non-irradiated aluminum member was removed. Then, for each immersion time, the presence or absence of peeling of the resin member from the aluminum member was confirmed 1 hour after removal.

[0096] Finally, (3) Hydrofluoric Acid Resistance Test will be described. In the hydrofluoric acid resistance test, the irradiated aluminum member and the non-irradiated aluminum member were each immersed in an electrolyte solution of EC / DEC=1:1 containing 1M LiPF6 with 1200 ppm of water added. Next, after 1, 5, and 24 hours of immersion, the irradiated aluminum member and the non-irradiated aluminum member were each taken out one by one. Then, for each immersion time, the presence or absence of peeling of the resin member from the aluminum member was confirmed one hour after removal.

[0097] Fig. 14(A) is a table showing the results of the (2) acid resistance test, and Fig. 14(B) is a table showing the results of the (3) hydrofluoric acid resistance test. The tables in Fig. 14(A) and Fig. 14(B) show the relationship between the elapsed time after the aluminum component was removed and the presence or absence of peeling for each aluminum component.

[0098] As shown in FIG. 14(A), as a result of the (2) acid resistance test, the irradiated aluminum member did not peel off, and the non-irradiated aluminum member peeled off 24 hours after removal. Also, as shown in FIG. 14(B), as a result of the (3) hydrofluoric acid resistance test, the irradiated aluminum member did not peel off, and the non-irradiated aluminum member peeled off 24 hours after removal. Therefore, it is considered that the acid resistance and hydrofluoric acid resistance of the joint with the resin member are higher in the irradiated aluminum member than in the non-irradiated aluminum member. Although a detailed explanation is omitted, element mapping was performed by the above-mentioned FIB method and TEM-EELS for each irradiated aluminum member. As a result, the presence of α-alumina was confirmed in each irradiated aluminum member. Also, it is considered that an oxide film was formed on the surface of the non-irradiated aluminum member, and α-alumina was not present. Therefore, the acid resistance and hydrofluoric acid resistance of the joint with the resin member are higher in the case where the protrusions contain α-alumina than in the case where the protrusions do not contain α-alumina.

[0099] As described above, since a large number of nano-order protrusions each having a diameter and height of less than 1 μm are densely arranged on the surface of the lid member 30 and the positive electrode terminal member 50 made of metal aluminum, the anchor effect improves the bonding strength of the bonding portion when the lid member 30 and the positive electrode terminal member 50 are bonded to the positive electrode resin member 70. Furthermore, the base end of the protrusions connected to the member surface contains not only amorphous alumina but also α-alumina, which has excellent chemical stability, so that the acid resistance and hydrofluoric acid resistance of the bonding portion, and further the difficulty of peeling off the positive electrode resin member 70 when immersed in a nonaqueous electrolyte solution containing hydrochloric acid or lithium hexafluorophosphate to which water has been added, are improved. Furthermore, the base end of the large number of protrusions contains more α-alumina than amorphous alumina. Therefore, the acid resistance and hydrofluoric acid resistance of the joint portion, and therefore the resistance to separation of the positive electrode resin member 70 when immersed in a nonaqueous electrolyte solution containing hydrochloric acid or lithium hexafluorophosphate and water, are further improved.

[0100] Furthermore, since the positive electrode resin member 70 fills the gaps between the numerous protrusions formed in the roughened regions F1 to F4, the aluminum resin composite has improved bonding strength at the bonded portion between the aluminum member and the resin member, and further improves the acid resistance and hydrofluoric acid resistance of the bonded portion, as well as the resistance of the positive electrode resin member 70 to separation when immersed in a nonaqueous electrolyte solution containing hydrochloric acid or lithium hexafluorophosphate to which water has been added.

[0101] Furthermore, the above-mentioned protrusion forming step S2 forms protrusions that contain α-alumina and have a diameter and height on the nano-order level in a dense mesh-like state, and the above-mentioned insert molding step S3 allows the positive electrode resin member 70 to fill the gaps between the numerous protrusions. This improves the bonding strength of the bonding portions between the cover member 30 and the positive electrode terminal member 50 and the positive electrode resin member 70, and also improves the acid resistance and hydrofluoric acid resistance of the bonding portions, and further improves the resistance of the positive electrode resin member 70 to separation when immersed in a nonaqueous electrolyte solution containing hydrochloric acid or lithium hexafluorophosphate to which water has been added.

[0102] It should be noted that the present embodiment is merely an example and does not limit the present invention in any way. Naturally, the present invention can be improved and modified in various ways without departing from the spirit and scope of the present invention. The following describes improvements and modifications of the present embodiment.

[0103] In this embodiment, the flat wound electrode body 40 is exemplified as the electrode body housed in the case 10, but the electrode body may be a laminated electrode body. In addition, although one electrode body is housed in the case 10 in this embodiment, multiple electrode bodies may be housed in the case 10.

[0104] In this embodiment, the case 10 has a generally flat rectangular parallelepiped shape with a bottom, but the shape of the case 10 can also be appropriately changed and may have other shapes such as a cylindrical shape. In addition, the shape of one or both of the positive electrode terminal member 50 and the negative electrode terminal member 60 may be appropriately changed. Similarly, the shape of one or both of the positive electrode resin member 70 and the negative electrode resin member 80 may be appropriately changed. Furthermore, in this embodiment, the shape of the positive electrode terminal member 50 and the shape of the negative electrode terminal member 60 are the same, but they may be different. Similarly, in this embodiment, the shape of the positive electrode resin member 70 and the shape of the negative electrode resin member 80 are the same, but they may be different.

[0105] In this embodiment, a battery 1 in which a cover member 30 and a positive electrode terminal member 50 each made of metallic aluminum are joined to a positive electrode resin member 70 is included in the aluminum resin composite of the present invention, and the unit member 1A constituting the battery 1 is also included in the aluminum resin composite of the present invention.

[0106] In this embodiment, the present invention is applied to a lithium ion battery, but it can be applied to any general power storage device, such as a nickel-metal hydride battery or a nickel-cadmium battery. The use of the present invention is not limited to batteries, and it can be widely applied to composites that bond aluminum members and resin members.

[0107] In this embodiment, the irradiation conditions of the pulsed laser irradiation in the protrusion forming step S2, in other words, the irradiation conditions of the pulsed laser irradiation for forming protrusions containing metallic aluminum, amorphous alumina and α-alumina and having nano-order diameters and heights arranged in a dense mesh-like state, are set to a wavelength of 1060 nm, but may be appropriately changed within a range of 1060 to 1080 nm. Similarly, the spot diameter may be appropriately set within a range of 10 to 200 μm. More preferably, the spot diameter may be appropriately set within a range of 50 to 100 μm. Furthermore, the interval of the laser irradiation may be set to ±10% of the spot diameter.

[0108] Also, according to Fig. 9(B-2) and Fig. 9(B-3), at the base end of the protrusion (within a range of 20 nm from the base), the area of ​​α-alumina is larger than the area of ​​amorphous alumina, in other words, it is presumed that more α-alumina is contained than amorphous alumina, but the content ratio of amorphous alumina and the content ratio of α-alumina may be approximately the same. Alternatively, the amount of amorphous alumina may be greater than the amount of α-alumina. However, from the viewpoint of acid resistance and hydrofluoric acid resistance, it is preferable that the amount of α-alumina is greater than that of amorphous alumina.

[0109] In this embodiment, the positive electrode resin member 70 reaches the base ends (roots) of the numerous protrusions that make up the roughened regions F1 to F4. However, for example, the positive electrode resin member 70 may fill the gaps between the numerous protrusions in a state where it reaches, as a whole, the tips of the protrusions, the part between the tips and the middle, or the part approximately in the middle or between the middle and the base end.

[0110] In this embodiment, the roughened regions F1 and F2 are formed over the entire bonding regions E1 and E2, but the roughened regions F1 and F2 may be formed in parts of the bonding regions E1 and E2. In this case, however, it is preferable that the roughened regions F1 and F2 are formed in an annular shape surrounding the positive electrode insertion hole 33h in the bonding regions E1 and E2. In addition, the roughened regions F3 and F4 are formed over the entire bonding regions E3 and E4, but the roughened regions F3 and F4 may be formed in parts of the bonding regions E3 and E4. In this case, however, it is preferable that the roughened region F3 is formed over the entire portion of the positive electrode terminal intermediate portion 53 in the bonding region E3. In addition, it is preferable that the roughened region F4 is formed in an annular shape along the peripheral portion of the bonding region E4. [Explanation of symbols]

[0111] 1... battery, 10... case, 20... main body member, 30... cover member, 33h: positive electrode insertion hole, 34h: negative electrode insertion hole, 50: Positive electrode terminal member, 60: Negative electrode terminal member, 70: Positive electrode resin member, 80: Negative electrode resin member, 30a, 50a...protrusion, E1... upper lid surface contact area, E2... lower lid surface contact area, E3...Terminal side surface bonding area, E4...Terminal bottom surface bonding area, F1... Roughened area on the upper surface of the lid, F2... Roughened area on the lower surface of the lid, F3...Roughened area on the side surface of the terminal, F4...Roughened area on the bottom surface of the terminal

Claims

1. A member body made of metal aluminum has a surface on which nano-order protrusions each having a diameter and height of less than 1 μm are densely arranged, The aluminum member has protruding portions, the base ends of which are connected to the surface of the member and which contain amorphous alumina and α-alumina.

2. The aluminum member according to claim 1, The base end of the protrusion is an aluminum member containing more α-alumina than amorphous alumina.

3. 3. An aluminum resin composite body comprising the aluminum member according to claim 1 or 2 and a resin member bonded thereto.

4. The method for producing the aluminum resin composite according to claim 3, a protrusion forming step of irradiating a laser onto the surface of the member before the protrusion is formed, to form the protrusion on the surface of the member; A method for manufacturing an aluminum resin composite, comprising: an insert molding process for forming the resin member on the surface of the member by insert molding after the protrusion forming process.

Citation Information

Patent Citations

  • Composite member

    JP1979054926A

  • Semiconductor device and manufacture thereof

    JP1991154343A

  • Surface coated cutting tool

    JP2010137315A

  • Metal member, method for producing metal member, metal-resin joined body and method for producing metal-resin joined body

    US20200070477A1

  • Metal member, method for producing metal member, metal-resin bonded body and method for producing metal-resin bonded body

    WO2019097624A1