Method for producing titanic acid aggregate

The use of a titanyl sulfate and ammonium sulfate hydrolysis process addresses chloride-related corrosion and contamination issues, enabling the production of titanic acid aggregates with uniform particle size and narrow distribution, suitable for titanium oxide and composite oxides.

JP2024150302APending Publication Date: 2024-10-23SAKAI CHEM IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023063655
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Existing methods for producing titanic acid aggregates with uniform particle size face challenges due to equipment corrosion and contamination risks from chloride salts, and difficulty in achieving narrow particle size distribution using commercially available titanium oxide precursors.

Method used

A hydrolysis process using titanyl sulfate and ammonium sulfate is employed to produce titanic acid aggregates with uniform particle size, avoiding chloride salts and minimizing equipment corrosion, with specific conditions for ammonium sulfate usage and reaction parameters.

Benefits of technology

The method enables the production of titanic acid aggregates with uniform particle size and narrow distribution, suitable as precursors for titanium oxide and composite oxides, without equipment damage or contamination, and enhances their suitability for applications like electronic materials and catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150302000006
    Figure 2024150302000006
  • Figure 2024150302000007
    Figure 2024150302000007
  • Figure 2024150302000008
    Figure 2024150302000008
Patent Text Reader

Abstract

To provide a method for producing titanic acid aggregate with a uniform particle size without damaging a production facility.SOLUTION: A method for producing titanic acid aggregate includes a hydrolysis step in which a solution containing titanyl sulfate and ammonium sulfate are mixed and hydrolyzed.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a titanic acid aggregate. [Background technology]

[0002] Titanium composite oxides such as lithium titanate, barium titanate, and potassium titanate are synthesized by a dry process or a wet process using titanium oxide, metatitanic acid, or titanic acid as a precursor, and lithium salt, barium salt, or potassium salt. Here, elements such as lithium and potassium promote grain growth as flux agents, so if the precursor is a highly reactive fine particle, it becomes difficult to control the size and grain size of the titanium composite oxide. For this reason, when synthesizing a titanium composite oxide having a particle size of 1 micron or more, there is a problem that the grain size distribution tends to become wide when a precursor of submicron or less is used. On the other hand, if the primary particle size of the precursor is large, the reactivity is poor and the reaction does not progress to the inside of the particle. In this way, the particle shape and grain size of the precursor are factors that greatly affect the particle shape and grain size of the target product.

[0003] Among the above precursors, titanium oxide (TiO2) is produced by calcining metatitanic acid (TiO(OH)2) or titanic acid (Ti(OH)4), and by adjusting the calcination temperature or promoting particle growth by additives in the calcination process, titanium oxide with a desired particle size can be obtained. However, it is difficult to produce titanium oxide with a particle size of 1 μm or more by this method, and titanium oxide distributed on the market as an industrial product is limited to a size of several nanometers to submicron. For this reason, it is not easy to produce titanium oxide and composite oxides with other elements having a particle size of 1 μm or more with a narrow particle size distribution using commercially available titanium oxide as a raw material. In contrast, by making the precursor (I) an aggregated particle consisting of fine primary particles, (II) having a secondary particle size on the order of microns, and further (III) having a narrow particle size distribution, it is possible to produce titanium oxide and composite oxides with other elements having a particle size of 1 μm or more with a narrow particle size distribution. Regarding such a precursor, Patent Document 1 discloses that metatitanic acid aggregates with a uniform particle size are formed by adding a chloride salt in the hydrolysis process of titanyl sulfate. Other methods for producing titanium compounds have been disclosed, including a method for producing spherical hydrous titanium dioxide in which titanyl sulfate is hydrolyzed at a temperature of 170°C or higher and at a pressure equal to or higher than the saturated water vapor pressure at said temperature (see Patent Document 2), and a method for producing anatase-type titanium dioxide fine particles in which an acidic aqueous solution of titanyl sulfate or titanium sulfate, the concentration of which has been adjusted so that the acid concentration at the end of the reaction is in the strong acidic range of 3.0 to 8.0 N, is heated and hydrolyzed (see Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-154527 A [Patent Document 2] Japanese Patent Application Publication No. 5-163022 [Patent Document 3] Japanese Patent Application Publication No. 5-178617 Summary of the Invention [Problem to be solved by the invention]

[0005] As described above, a method for producing titanic acid aggregates with uniform particle size by adding a chloride salt in the hydrolysis process of titanyl sulfate has been disclosed. However, when a chloride salt is used, corrosive hydrogen chloride and hydrochloric acid are generated in the hydrolysis process (e.g., NaCl+H2SO4→HCl+NaHSO4), which may cause corrosion of the production equipment. In addition, if Cl is mixed into the precursor, chlorine gas and hydrogen chloride gas are generated in the subsequent firing process, which may cause corrosion of the firing furnace. In addition, when a chloride salt is added in this way, the possibility of equipment corrosion increases, and there is an associated risk of contamination. For this reason, a method for producing titanic acid aggregates with uniform particle size in a reaction system that does not use chlorides is required.

[0006] In view of the above-mentioned current situation, an object of the present invention is to provide a method for producing titanic acid aggregates having a uniform particle size in a reaction system that does not use chlorides. [Means for solving the problem]

[0007] The inventors investigated a method for producing titanic acid aggregates with uniform particle size without using chlorides, and discovered that by mixing a solution containing titanyl sulfate with ammonium sulfate and performing a hydrolysis process, titanic acid aggregates with uniform particle size can be produced in a reaction system that does not use chlorides, thereby completing the present invention.

[0008] That is, the present invention is as follows. [1] A method for producing a titanic acid aggregate, comprising a hydrolysis step of mixing a solution containing titanyl sulfate with ammonium sulfate and hydrolyzing the mixture.

[0009] [2] The method for producing a titanic acid aggregate according to [1], wherein ammonium sulfate is used in an amount of 0.30 to 3.0 molar equivalents relative to titanyl sulfate in the hydrolysis step.

[0010] [3] The method for producing a titanic acid aggregate according to [1] or [2], characterized in that in the hydrolysis step, the concentration of ammonium sulfate in the solution containing titanyl sulfate and ammonium sulfate is 0.20 to 1.80 mol / L.

[0011] [4] The method for producing a titanic acid aggregate according to any one of [1] to [3], characterized in that the hydrolysis step is carried out by heating a solution containing titanyl sulfate and ammonium sulfate to 90 to 120°C. Effect of the Invention

[0012] The method for producing a titanic acid aggregate of the present invention can produce a titanic acid aggregate with a uniform particle size without damaging the production equipment. The obtained titanic acid aggregate can be suitably used as a precursor for producing titanium oxide having a particle size of 1 μm or more with a narrow particle size distribution and a composite oxide with other elements. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 1. [Diagram 2] FIG. 2 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 2. [Diagram 3] FIG. 2 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 3. [Figure 4] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 4. [Diagram 5] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 5. [Figure 6] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 6. [Figure 7]FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 7. [Figure 8] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 8. [Figure 9] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 9. [Figure 10] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 10. [Figure 11] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, 10,000x) of the titanic acid aggregate obtained in Example 11. [Figure 12] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 12. [Figure 13] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 13. [Figure 14] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 14. [Figure 15] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 15. [Figure 16] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 16. [Figure 17] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 17. [Figure 18] FIG. 1 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Example 18. [Figure 19]FIG. 2 shows the results of electron microscope observation (magnifications: 200x, 2000x, and 10,000x) of the titanic acid aggregate obtained in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] A preferred embodiment of the present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified and applied as appropriate within the scope that does not change the gist of the present invention.

[0015] Method for producing titanic acid aggregates The method for producing a titanic acid aggregate of the present invention is characterized by including a hydrolysis step of mixing a solution containing titanyl sulfate with ammonium sulfate and hydrolyzing the mixture. As described above, when a chloride salt is used in the hydrolysis process of titanyl sulfate, titanic acid aggregates with a uniform particle size can be obtained, but the manufacturing equipment may be corroded. In addition, if Cl is mixed into the precursor, the firing furnace may be corroded. In contrast, by using ammonium sulfate, among sulfates, instead of chloride salts, it is possible to produce titanic acid aggregates with a uniform particle size without damaging the manufacturing equipment. Although titanic acid includes metatitanic acid (TiO(OH)2) and orthotitanic acid (Ti(OH)4), the titanic acid aggregate obtained by the manufacturing method of the present invention is composed mainly of metatitanic acid.

[0016] In the above hydrolysis step, it is preferable to use 0.30 to 3.0 molar equivalents of ammonium sulfate relative to the titanium contained in titanyl sulfate. When sulfate is used in the hydrolysis of titanyl sulfate, the sulfate and titanyl sulfate may form a double salt, which may complicate the hydrolysis reaction. In contrast, by using 0.30 to 3.0 molar equivalents of ammonium sulfate relative to titanyl sulfate, the formation of double salts is suppressed to prevent the hydrolysis reaction from becoming complicated, and as a result, titanic acid is precipitated in the reaction system at a constant hydrolysis rate, and titanic acid aggregates with a more uniform particle size distribution can be obtained. The amount of ammonium sulfate used is more preferably 0.35 to 1.70 molar equivalents relative to the titanium contained in titanyl sulfate, and even more preferably 0.40 to 1.60 molar equivalents.

[0017] In the above hydrolysis step, ammonium sulfate may be added to a solution containing titanyl sulfate and then mixed, or the solution containing titanyl sulfate may be added to ammonium sulfate and then mixed. In the above hydrolysis step, in either case of adding ammonium sulfate to a solution containing titanyl sulfate or adding a solution containing titanyl sulfate to ammonium sulfate, the method of addition is not particularly limited, and may be a lump addition, a divided addition, or a continuous addition.

[0018] In the hydrolysis step, the concentration of titanyl sulfate in the solution containing titanyl sulfate is not particularly limited, but considering the yield of titanic acid aggregate and production efficiency, the concentration is preferably 0.10 to 3.5 mol / L, more preferably 0.50 to 2.5 mol / L, and even more preferably 0.70 to 2.0 mol / L.

[0019] In the above hydrolysis step, the concentration of ammonium sulfate in the solution containing titanyl sulfate and ammonium sulfate is preferably 0.20 to 1.80 mol / L. In this way, the titanic acid aggregate can be produced with high production efficiency by proceeding with the hydrolysis step while taking into consideration the solubility of each raw material used in the hydrolysis and the viscosity of the solution and preventing the amount of the reaction solution from becoming too large. The concentration of ammonium sulfate in the solution containing titanyl sulfate and ammonium sulfate is more preferably 0.30 to 1.56 mol / L, and even more preferably 0.50 to 1.10 mol / L.

[0020] The hydrolysis step is preferably carried out with the addition of an acid in order to sufficiently promote hydrolysis. The acid to be added is not particularly limited, but a mineral acid is preferred, and sulfuric acid is more preferred.

[0021] The hydrolysis step is preferably carried out by heating the solution containing titanyl sulfate and ammonium sulfate to 90 to 120°C. By heating to such a temperature, the hydrolysis reaction can be more sufficiently progressed, and titanic acid aggregates can be obtained in a higher yield. The temperature of the solution containing titanyl sulfate and ammonium sulfate in the hydrolysis step is more preferably 95 to 115°C, and further preferably 103 to 110°C.

[0022] The time for carrying out the hydrolysis step is not particularly limited, but in consideration of obtaining titanic acid aggregates in a high yield and production efficiency, the hydrolysis step is preferably carried out for 30 to 720 minutes, more preferably 45 to 360 minutes, and even more preferably 60 to 240 minutes.

[0023] The method for producing a titanic acid aggregate of the present invention preferably includes a step of neutralizing the hydrolyzate obtained in the hydrolysis step. This makes it possible to more efficiently remove sulfate ions remaining in the titanic acid aggregate. The neutralization step can be carried out by adding a basic compound to the hydrolyzate. The basic compound used for neutralization is not particularly limited, and ammonia, sodium hydroxide, sodium carbonate, sodium hydrogen carbonate, potassium hydroxide, etc. can be used. Among these, ammonia, sodium hydroxide, sodium carbonate, and sodium hydrogen carbonate are preferred because the basic compound itself and the salt generated by neutralization are water-soluble. Ammonia is more preferred. These may be added in a solid or gas state, but are usually added as an aqueous solution.

[0024] In the neutralization step, it is preferable to add a basic compound until the pH of the repulp slurry obtained by repulping the hydrolyzate in water in an amount 10 times the mass of the hydrolyzate becomes 7 to 10. This allows the compound consisting of sulfate ions to form a salt and improves water solubility, so that sulfate ions can be removed more efficiently. It is more preferable to add a basic compound until the pH of the repulp slurry becomes 8 to 9.

[0025] In the method for producing a titanic acid aggregate of the present invention, it is preferable to carry out a step of filtering and washing the hydrolyzate obtained after the hydrolysis step before subjecting it to the neutralization step. The washing of the hydrolyzate is preferably carried out until the electrical conductivity of the water used for washing becomes 1000 μS / cm or less, which allows the unnecessary ammonium sulfate contained in the hydrolyzate to be sufficiently removed.

[0026] In the method for producing a titanic acid aggregate of the present invention, it is preferable to carry out a process of filtering and washing the solid matter obtained after the neutralization process. This makes it possible to remove salts generated in the neutralization process and increase the purity of the titanic acid aggregate. The neutralized product is preferably washed with water until the electrical conductivity of the water used for washing is 1000 μS / cm or less, which makes it possible to sufficiently remove salts generated in the neutralization process. It is more preferable to wash the neutralized product with water until the electrical conductivity is 500 μS / cm or less, and even more preferable to wash the neutralized product with water until the electrical conductivity is 1000 μS / cm or less.

[0027] After the neutralization step (if a step of filtering and washing the obtained neutralized product is performed after the neutralization step), a step of drying the obtained titanic acid aggregate is preferably performed. The method for drying the titanic acid aggregate is not particularly limited, but is preferably performed by heating. The heating temperature is preferably 80 to 200°C, and more preferably 100 to 150°C. The drying time is not limited, but is preferably 1 to 48 hours, and more preferably 2 to 24 hours. Drying at the above temperature for the above time allows for sufficient drying while preventing excessive sintering between particles.

[0028] The method for producing the titanic acid aggregate may include other steps in addition to the steps described above. Examples of the other steps include a step of crushing the titanic acid aggregate after drying and a step of classifying the aggregate.

[0029] By using the method for producing titanic acid aggregates of the present invention, it is possible to produce titanic acid aggregates suitable as precursors for producing titanium oxides having a narrow particle size distribution and a particle size of 1 μm or more, and composite oxides with other elements having a particle size of 1 μm or more, without using chlorides. 90 / D 10 Titanate aggregates having a molecular weight of less than 3.5 can be produced. Since the primary particle diameter of titanic acid is generally about 3 to 10 nm, when the (secondary particle diameter / primary particle diameter) is 300 or more, the secondary particle diameter is 900 to 1200 nm or more. 1) In this case, most of the primary particles are adjacent to the primary particles in the same secondary particle, and only a few primary particles are adjacent to the primary particles on the surface of other secondary particles. 2) Furthermore, since each primary particle in the secondary particle is attracted to each other by van der Waals force, they are easily sintered during firing. 3) On the other hand, since there is no particular attractive force between secondary particles of 900 to 1200 nm or more, the distance between the particles is far, and the reactivity between the secondary particles is poor. Due to these factors 1) to 3), in titanic acid aggregates with a (secondary particle diameter / primary particle diameter) of 300 or more, sintering between primary particles in the secondary particle occurs preferentially to sintering between secondary particles during firing, and sintering between aggregates is suppressed. and D of titanate aggregates 90 / D 10 When the particle size distribution of the titanate aggregates is less than 3.5, the particle size distribution of the titanate aggregates is uniform, and by using these as precursors for producing titanium oxide and composite oxides with other elements, the powder properties such as the particle size distribution and particle diameter of the titanate aggregates can be reflected in the target product. Therefore, the titanate aggregates obtained by the titanate aggregate manufacturing method of the present invention can be suitably used as precursors for producing titanium oxides having particle sizes of 1 μm or more and a narrow particle size distribution, and composite oxides with other elements. Furthermore, the resulting titanium oxide or titanium composite oxide has an excellent particle size distribution and can be suitably used for applications such as electronic materials, fillers, catalysts, and pigments. EXAMPLES

[0030] In order to explain the present invention in detail, specific examples are given below, but the present invention is not limited to these examples. Unless otherwise specified, "%" and "wt%" mean "weight % (mass %)". The measurement methods for each physical property are as follows.

[0031] <Specific surface area> Using a fully automatic specific surface area measuring device (Macsorb, manufactured by Microtrac), the sample was degassed at 200° C. for 30 minutes and preheated at 200° C. for 5 minutes, after which the specific surface area was measured by adsorption / desorption measurement. <Primary particle size> From the results of the specific surface area measurement, the primary particle size was calculated by the following formula. Primary particle diameter (μm)=6 / (r S)×1000 r: Theoretical density (g / cm 3 ), S: Specific surface area (m 2 / g) In each of the examples and comparative examples, the main crystal phase was anatase type, so the theoretical density was 3.90 g / cm 3 It was decided. <Secondary particle size, particle size distribution> Using a laser diffraction / scattering type particle size distribution analyzer (LA-950, HORIBA), 0.025% hexametaphosphoric acid aqueous solution was used as the dispersion medium, and the particle size distribution was measured for the sample that had been dispersed for 1 minute using an ultrasonic homogenizer (US-600, Nippon Seiki Co., Ltd.). The median diameter (D 50 ), 10% diameter by volume (D 10 ), volumetric 90% diameter (D 90 ) was measured. D 10 and D. 90 From the numerical value of (D 90 / D 10 ) was calculated. <Electron microscope observation> SEM images were taken using a field emission scanning electron microscope (JSM-7000, manufactured by JEOL).

[0032] Example 1 1200 mL of pure water and 240 g of titanyl sulfate n-hydrate (19.9 wt% as Ti) were placed in a separable flask, and 33.04 g of ammonium sulfate (0.5 molar equivalent to titanyl sulfate), 140 mL of pure water, and 20 mL of sulfuric acid were added thereto and mixed. The mixed solution was heated and stirred at 200 rpm and refluxed for 3 hours. The obtained slurry was added to a Buchner funnel and subjected to suction filtration, and washed with pure water until the electrical conductivity of the filtrate was 100 μS / cm or less. The washed solid content was repulped in pure water of about 10 times the mass of the solid content, and an aqueous ammonia solution was added until the pH of the repulped slurry was about 8-9. The pH-adjusted slurry was filtered again and washed with water so that the electrical conductivity of the filtrate was 100 μS / cm or less. The washed solid content was dried at 100 ° C. and sieved through a 150 μm sieve to produce the titanic acid aggregate of Example 1. Since no chlorides are used, there was no damage to the manufacturing equipment due to the generation of hydrogen chloride or hydrochloric acid. The specific surface area, secondary particle size, degree of aggregation, and particle size distribution (D 90 / D 10 The results are shown in Table 1.

[0033] Examples 2 to 5 Titanic acid aggregates of Examples 2 to 5 were produced in the same manner as in Example 1, except that titanyl sulfate, ammonium sulfate, pure water, and sulfuric acid were added in amounts as shown in Table 1. The concentration of ammonium sulfate in the table means the amount of ammonium sulfate (mol) relative to the amount of solution (L) obtained by adding sulfuric acid to pure water. The same applies to the following tables. The specific surface area, secondary particle size, degree of aggregation, and particle size distribution (D 90 / D 10 The results are shown in Table 1.

[0034] [Table 1]

[0035] Examples 6 to 10 The titanic acid aggregates of Examples 6 to 10 were produced in the same manner as Example 1, except that the molar ratio of ammonium sulfate to titanyl sulfate was adjusted to 1.0 and the amounts of titanyl sulfate, ammonium sulfate, pure water, and sulfuric acid were added as shown in Table 2. The specific surface area, secondary particle size, degree of aggregation, and particle size distribution (D 90 / D 10 The results are shown in Table 2.

[0036] [Table 2]

[0037] Examples 11 to 15 The titanic acid aggregates of Examples 11 to 15 were produced in the same manner as Example 1, except that the molar ratio of ammonium sulfate to titanyl sulfate was adjusted to 1.5 and the amounts of titanyl sulfate, ammonium sulfate, pure water, and sulfuric acid were added as shown in Table 3. The specific surface area, secondary particle size, degree of aggregation, and particle size distribution (D 90 / D 10 The results are shown in Table 3.

[0038] [Table 3]

[0039] Examples 16 to 18 The titanic acid aggregates of Examples 16 to 18 were produced in the same manner as Example 1, except that the molar ratio of ammonium sulfate to titanyl sulfate was adjusted to 3.0 and the amounts of titanyl sulfate, ammonium sulfate, pure water, and sulfuric acid were added as shown in Table 4. The specific surface area, secondary particle size, degree of aggregation, and particle size distribution (D 90 / D 10 The results are shown in Table 4.

[0040] [Table 4]

[0041] Comparative Example 1 The titanic acid aggregate of Comparative Example 1 was produced in the same manner as in Example 1, except that sodium sulfate was used instead of ammonium sulfate, the molar ratio of sodium sulfate to titanyl sulfate was adjusted to 1.0, the sodium sulfate concentration in the reaction solution was adjusted to 0.80 mol / L, and the amounts of titanyl sulfate, sodium sulfate, pure water, and sulfuric acid were added as shown in Table 5. The specific surface area, secondary particle size, degree of aggregation, and particle size distribution (D 90 / D 10 The results are shown in Table 5.

[0042] Comparative Example 2 The titanic acid aggregate of Comparative Example 2 was produced in the same manner as in Example 1, except that sodium carbonate was used instead of ammonium sulfate, the molar ratio of sodium carbonate to titanyl sulfate was adjusted to 1.0, the sodium carbonate concentration in the reaction solution was adjusted to 0.80 mol / L, and the amounts of titanyl sulfate, sodium carbonate, pure water, and sulfuric acid were added as shown in Table 5. The specific surface area, secondary particle size, degree of aggregation, and particle size distribution (D 90 / D 10 The results are shown in Table 5.

[0043] Comparative Example 3 A titanic acid aggregate of Comparative Example 3 was produced in the same manner as in Example 1, except that ammonium sulfate was not added and the amounts of titanyl sulfate, pure water, and sulfuric acid were changed as shown in Table 5. The specific surface area, secondary particle size, degree of aggregation, and particle size distribution (D 90 / D 10 The results are shown in Table 5.

[0044] [Table 5]

[0045] By synthesizing using the method shown in the examples, the ratio of (secondary particle diameter / primary particle diameter) is 300 or more, and D 90 / D 10 It was possible to produce titanic acid aggregates having a σ of less than 3.5. On the other hand, the titanic acid aggregates synthesized by the method shown in Comparative Example 1 90 / D 10 is D in the embodiment 90 / D 10 In Comparative Example 1, it is considered that sodium sulfate and titanyl sulfate formed a double salt in the reaction system, which complicated the hydrolysis reaction and made the precipitation rate of titanic acid not constant, resulting in a broader particle size distribution than when ammonium sulfate was used. Furthermore, the titanic acid aggregate D 90 / D 10 is D in the examples and comparative example 1 90 / D 10 The sodium carbonate aqueous solution is basic, and therefore, unlike the examples and Comparative Example 1, in the reaction system of Comparative Example 2, the hydrolysis reaction of titanyl sulfate by the base proceeds. Therefore, rapid precipitation of titanic acid occurs in the reaction system, and uniform secondary particle growth does not occur, resulting in a large amount of D 90 / D 10 is thought to be a very large figure. In addition, the titanic acid aggregate D 90 / D 10 Also, D in the Example and Comparative Example 1 90 / D 10 This is thought to be because, since no salts that contribute to the formation of aggregates were included, titanic acid was highly dispersed in water after the reaction was completed, and during the drying process, titanic acid randomly aggregated. 90 / D 10 is thought to be a very large figure. From the results of the Examples and Comparative Examples, it was confirmed that by using the method for producing a metatitanic acid aggregate of the present invention, a metatitanic acid aggregate with a uniform particle size can be produced in a reaction system that does not use chlorides. In addition, from the comparison with Comparative Examples 1 to 3, it was confirmed that it is important to add ammonium sulfate during the hydrolysis of titanyl sulfate.

Claims

1. A method for producing a titanic acid aggregate, comprising a hydrolysis step of mixing a solution containing titanyl sulfate with ammonium sulfate and hydrolyzing the mixture.

2. 2. The method for producing a titanic acid aggregate according to claim 1, wherein ammonium sulfate is used in an amount of 0.30 to 3.0 molar equivalents relative to titanyl sulfate in the hydrolysis step.

3. 2. The method for producing a titanic acid aggregate according to claim 1, wherein in the hydrolysis step, the concentration of ammonium sulfate in the solution containing titanyl sulfate and ammonium sulfate is 0.20 to 1.80 mol / L.

4. 2. The method for producing a titanic acid aggregate according to claim 1, wherein the hydrolysis step is carried out by heating a solution containing titanyl sulfate and ammonium sulfate to 90 to 120°C.

Citation Information

Patent Citations

  • Spherical anatase titanium oxide and its production

    JP1993163022A

  • Production of spherical particulate made of titanate and spherical particulate obtained by the same

    JP1993178617A