Composite membrane for gas separation and gas separation system using the same

The composite membrane with a porous support, functional, and coating layer addresses the challenge of simultaneous high permeability and selectivity for small and large molecular gases, enhancing gas separation efficiency by optimizing structural and compositional parameters.

JP2024150418APending Publication Date: 2024-10-23TORAY INDUSTRIES INC +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024059554
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-04-02
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Conventional gas separation technologies struggle to achieve high selective separation of gases with small molecular diameters such as hydrogen, helium, water vapor, and ammonia, while simultaneously suppressing the permeation of gases with larger molecular diameters like oxygen, nitrogen, and methane.

Method used

A composite membrane for gas separation is designed with a porous support layer, a separation functional layer, and a coating layer, optimized for high permeability and selectivity through specific structural and compositional parameters, including contact angles, pore sizes, and materials like crosslinked aromatic polyamide, which reduces permeation through large pores and defects.

Benefits of technology

The composite membrane exhibits enhanced selective separation properties for gases with small molecular diameters while significantly reducing the permeation of gases with larger molecular diameters, achieving improved gas separation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150418000001_ABST
    Figure 2024150418000001_ABST
Patent Text Reader

Abstract

To provide a composite membrane for gas separation having high permeation of gas having a small molecular diameter and high selection separability of other kind of gas, and a composite module for gas separation and a gas separation system which use the same.SOLUTION: There are provided a composite membrane for gas separation which has at least a porous support layer, a separation function layer and a coating layer in this order, wherein when nano-perm porometry analysis is performed using non-condensable gas as He and condensable gas as H2O under the condition of a temperature of 40°C, He permeability at relative humidity of 90% is 60% or more and 100% or less of He permeability at relative humidity of 10%, a contact angle of the surface of the coating layer and pure water in air measured in accordance with ISO 19403-1 (2017) is 50° or more and 130° or less; and a composite module for gas separation and a gas separation system which use the same.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite membrane for gas separation capable of selectively separating at least one component in a gas mixture, and a gas separation system using the same. [Background technology]

[0002] In recent years, hydrogen has been attracting attention as a clean energy source. Hydrogen is obtained by reforming and gasifying fossil fuels such as natural gas and coal, and removing unnecessary gases from the mixed gas containing hydrogen and carbon dioxide as main components. It can also be obtained by decomposing water using electricity or photocatalysis, and extracting only hydrogen from the mixed gas containing hydrogen, oxygen, and water vapor. Hydrogen is also used in the Haber-Bosch process to synthesize ammonia. This is a method of synthesizing ammonia by reacting hydrogen and nitrogen at high temperature and pressure, but a process is required to separate and recover unreacted hydrogen and nitrogen at the production plant.

[0003] Membrane separation, which utilizes differences in the gas permeability of materials to selectively allow the target gas to pass through, has attracted attention as a low-cost method for concentrating a specific gas from a mixed gas.

[0004] Patent Document 1 proposes a method of improving the selective separation of gases by attaching a surfactant to a single-layer hollow fiber membrane. Non-Patent Document 1 describes a technology for improving the selective separation of helium and carbon dioxide by coating the surface of a polyamide composite membrane with polyphenylene oxide. Non-Patent Document 2 describes a method for improving the selective separation of methane and other gases by coating the surface of an RO membrane with polydimethylsiloxane. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 3-186327 [Non-patent literature]

[0006] [Non-Patent Document 1] Seung-Hak Choi and 2 others, 'Journal of Membrane Science', 553, 2018, p.180-188 [Non-Patent Document 2] Jaesung Park, 3 others, 'Journal of Membrane Science', 604, 2020, 118009 Summary of the Invention [Problem to be solved by the invention]

[0007] However, conventional techniques cannot efficiently increase the permeation resistance of other gases such as oxygen, nitrogen, and methane, and therefore have the problem that they cannot simultaneously achieve high permeability to gases with small molecular diameters such as hydrogen, helium, water vapor, and ammonia, and high selective separation ability for other gases such as oxygen, nitrogen, and methane.

[0008] The present invention has been made in consideration of the above-mentioned conventional situation, and aims to provide a composite membrane for gas separation that has high permeability to gases with small molecular diameters, such as hydrogen, helium, water vapor, and ammonia, and high selective separation ability from other gases, such as oxygen, nitrogen, and methane, as well as a composite module for gas separation, a gas separation system, and a method for purifying He or H2 that use the same. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems, and as a result have significantly improved the performance, particularly the selectivity, of composite membranes for gas separation.

[0010] (1) A composite membrane for gas separation having at least a porous support layer, a separation functional layer, and a coating layer in this order, When nanoperm porometry analysis was performed under conditions of a non-condensable gas being He and a condensable gas being H2O, and a temperature of 40°C, the He permeability at a relative humidity of 90% was 60% to 100% of the He permeability at a relative humidity of 10%, A composite membrane for gas separation, in which the contact angle between the surface of the coating layer and pure water in air, as measured in accordance with ISO 19403-1 (2017), is 50° or more and 130° or less. (2) The composite membrane for gas separation according to (1), wherein a contact angle X 1 second after a drop of pure water lands on the surface of the coating layer and a contact angle Y 30 seconds after the drop of pure water lands on the surface of the coating layer satisfy formula 1.

number

[0011] According to the present invention, it is possible to provide a composite membrane for gas separation having high selectivity for separating gases with small molecular diameters such as hydrogen, helium, water vapor, and ammonia, a spiral-type composite membrane module for gas separation, and a gas separation system using the same. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view of a composite membrane for gas separation according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a partially exploded perspective view of a spiral-type composite membrane module for gas separation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] 1. Composite membranes for gas separation The composite membrane for gas separation of the present invention is a composite membrane for gas separation having at least a porous support layer, a separation functional layer, and a coating layer in this order, and when nanoperm porometry analysis is performed under conditions of a temperature of 40° C., with He as a non-condensable gas and H2O as a condensable gas, the He permeability at a relative humidity of 90% is 60% to 100% of the He permeability at a relative humidity of 10%. The composite membrane for gas separation of the present invention will be described in detail below.

[0014] As shown in Fig. 1, the gas separation composite membrane (51) of this embodiment includes at least a porous support layer (52), a separation functional layer (53), and a coating layer (54) in this order. It may also include a substrate (55). Furthermore, this gas separation composite membrane is a gas separation composite membrane in which the contact angle between the surface of the coating layer and pure water in air is 50° or more and 130° or less, as measured in accordance with ISO 19403-1 (2017).

[0015] (base material) The composite membrane for gas separation of the present invention may have a substrate. The substrate does not need to have a selective gas separation capability, but only needs to support the separation functional layer and provide strength to the entire composite membrane for gas separation.

[0016] The resin constituting the substrate is not particularly limited, and examples thereof include polyester polymers, polyamide polymers, polyolefin polymers, polysulfide polymers, and mixtures or copolymers thereof. Among these, polyester polymers and polysulfide polymers, which have high mechanical strength and thermal stability, are particularly preferred as the resin constituting the substrate.

[0017] The form of the substrate is not particularly limited, but nonwoven fabrics or woven / knitted fabrics such as long fiber nonwoven fabrics and short fiber nonwoven fabrics are preferred, and it is particularly preferred to use long fiber nonwoven fabrics. Here, the long fiber nonwoven fabric refers to a nonwoven fabric with an average fiber length of 300 mm or more and an average fiber diameter of 3 to 30 μm. By using a long fiber nonwoven fabric, the polymer solution that will become the porous support layer can be sufficiently impregnated, so that the adhesion to the substrate can be improved and the physical stability of the porous support membrane can be increased. In addition, by sufficiently impregnating the substrate with the polymer solution, the replacement rate with the nonsolvent increases during phase separation to form the porous support layer. As a result, the generation of macrovoids can be suppressed, which contributes to improving the selectivity of gas permeation.

[0018] (porous support layer) The composite membrane for gas separation of the present invention has a porous support layer. The porous support layer may be any layer that can permeate hydrogen or helium. The porous support layer may or may not have a selective gas separation permeability, and may provide strength to the entire composite membrane for gas separation by supporting the separation functional layer.

[0019] The size and distribution of the pores in the porous support layer are not particularly limited, but for example, the pore size may be uniform throughout the entire porous support layer, or may gradually increase from the surface of the porous support layer that contacts the separation functional layer to the other surface.

[0020] The material of the porous support layer is not particularly limited, and examples thereof include homopolymers or copolymers of polysulfone, polyethersulfone, polyamide, polyaramid, polyester, cellulose polymer, vinyl polymer, polyphenylene sulfide, polyphenylene sulfide sulfone, polyphenylene sulfone, polyphenylene oxide, etc., which can be used alone or in combination. Examples of cellulose polymers include cellulose acetate and cellulose nitrate, and examples of vinyl polymers include polyethylene, polypropylene, polyvinyl chloride, polyacrylonitrile, etc.

[0021] Among these, the material of the porous support layer is preferably a homopolymer or copolymer of polysulfone, polyamide, polyester, cellulose acetate, cellulose nitrate, polyvinyl chloride, polyacrylonitrile, polyphenylene sulfide, polyphenylene sulfide sulfone, etc. Cellulose acetate, polysulfone, polyphenylene sulfide sulfone, or polyphenylene sulfone is more preferable because of its high chemical, mechanical, and thermal stability, and polysulfone and cellulose acetate are particularly preferable.

[0022] The thicknesses of the substrate and the porous support layer affect the strength of the composite semipermeable membrane and the packing density when it is made into an element. From the viewpoint of obtaining good mechanical strength and packing density, the total thickness of the substrate and the porous support layer is preferably 30 to 300 μm, more preferably 100 to 220 μm. The thickness of the porous support layer is preferably 20 to 100 μm, more preferably 23 μm to 50 μm, and even more preferably 27 μm to 40 μm. The thicknesses of the substrate and the porous support layer can be calculated by calculating the average value of the thicknesses at 20 points measured at 20 μm intervals in a direction perpendicular to the thickness direction (plane direction of the membrane) by cross-sectional observation.

[0023] (separation functional layer) The material of the separation functional layer in the composite membrane for gas separation of the present invention is not particularly limited, but it is preferable to use cellulose, polyimide, polyamide, etc., and a composite membrane having a separation functional layer containing polyamide is preferable. When the separation functional layer is mainly composed of polyamide, it can be formed by performing interfacial polycondensation of a polyfunctional amine and a polyfunctional acid halide on a porous support layer.

[0024] "Polyamide is the main component" means that polyamide accounts for 50% by weight or more of the separation functional layer (100% by weight), and the amount of polyamide in 100% by weight of the separation functional layer is preferably 80% by weight or more, and more preferably 90% by weight or more and 100% by weight or less.

[0025] The polyamide in the separation functional layer may be a wholly aromatic polyamide, a wholly aliphatic polyamide, or a polyamide having both aromatic and aliphatic portions, but in order to achieve higher performance, it is preferable that it is wholly aromatic.

[0026] Specifically, the polyfunctional amine is a polyfunctional aromatic amine or a polyfunctional aliphatic amine. The polyfunctional aromatic amine means an aromatic amine having two or more amino groups selected from a primary amino group and a secondary amino group in one molecule, at least one of the amino groups being a primary amino group. The polyfunctional aliphatic amine means an aliphatic amine having two or more amino groups selected from a primary amino group and a secondary amino group in one molecule.

[0027] Examples of polyfunctional aromatic amines include polyfunctional aromatic amines in which two amino groups are bonded to an aromatic ring at the ortho, meta, or para positions, such as o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, o-xylylenediamine, m-xylylenediamine, p-xylylenediamine, o-diaminopyridine, m-diaminopyridine, and p-diaminopyridine.

[0028] Examples of polyfunctional aliphatic amines include ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, piperazine, 2-methylpiperazine, 2,4-dimethylpiperazine, 2,5-dimethylpiperazine, 2,6-dimethylpiperazine, etc. These polyfunctional amines may be used alone or in combination of two or more kinds.

[0029] The polyfunctional acid halide specifically means a polyfunctional aromatic acid halide or a polyfunctional aliphatic acid halide.

[0030] The polyfunctional acid halide refers to an acid halide having at least two halogenated carbonyl groups in one molecule. For example, a trifunctional acid halide may be trimesic acid chloride, and a bifunctional acid halide may be biphenyldicarboxylic acid dichloride, azobenzenedicarboxylic acid dichloride, terephthalic acid chloride, isophthalic acid chloride, and the like.

[0031] In consideration of the reactivity with polyfunctional amines, the polyfunctional acid halide is preferably a polyfunctional acid chloride, and in consideration of the selectivity and heat resistance of the gas separation composite membrane, the polyfunctional acid chloride is preferably a polyfunctional acid chloride having 2 to 4 carbonyl chloride groups in one molecule.

[0032] Among them, trimesoyl chloride is more preferable from the viewpoints of availability and ease of handling. These polyfunctional acid halides may be used alone or in combination of two or more kinds.

[0033] The polycondensation reaction is specifically interfacial polycondensation.

[0034] In order to achieve higher performance, the separation functional layer of the present invention is preferably composed mainly of a crosslinked aromatic polyamide. The crosslinked aromatic polyamide can be formed by performing interfacial polycondensation between a polyfunctional aromatic amine and a polyfunctional aromatic acid halide.

[0035] In the separation functional layer, the thin film may have a pleated structure having concave and convex portions. When the thin film has a pleated structure, the surface area having the separation function of the membrane is increased relative to the membrane area, thereby increasing the gas permeability.

[0036] (covering layer) The composite membrane for gas separation of the present invention has a coating layer on a separation functional layer. The separation functional layer has a small number of regions with extremely high gas permeability due to coarse pores, defects, etc. In such regions, the contribution of separation by molecular sieves is small, and the selective separation property for gases with small molecular diameters such as hydrogen, helium, water vapor, and ammonia is low. Reducing the contribution of regions with low selective separation property due to coarse pores, defects, etc. is important for improving the selective separation property of the entire membrane.

[0037] By forming a coating layer on the separation functional layer, it is possible to suppress gas permeation through large pores and defects. The permeation of oxygen, nitrogen, methane, etc. is greatly suppressed, but the effect on the permeation of light gases such as hydrogen and helium is small, so the selective separation can be greatly improved.

[0038] The coating layer does not necessarily need to cover the entire surface of the separation functional layer. There may be cases where the coating layer is partially missing due to uneven coating when forming the coating layer, or where the coating layer is formed only on surfaces that have particularly large pores or defects.

[0039] The coating layer can penetrate into the separation functional layer and the support layer. When the coating layer components penetrate into the support layer, they block the gas permeation path, so the permeability tends to decrease. On the other hand, the adhesive strength between the functional layer and the support layer, or between the support layer and the substrate, may be reduced, or the support layer structure may be destroyed, causing the gas to leak through the gaps and reducing the selectivity. Therefore, it is preferable that the coating layer penetrates into the support layer as little as possible. The penetration depth of the coating layer into the support layer depends on the structure of the coating layer and the support layer, but it is possible to perform element mapping of only the support layer and only the coating layer using TEM-EDX (transmission electron microscope-energy dispersive X-ray spectroscopy), or to perform component analysis in the depth direction using TOF-SIMS (time-of-flight secondary ion mass spectrometry). When the support layer is polysulfone and the coating layer is silicone, the S contained in the polysulfone and the Si contained in the coating layer are mapped using TEM-EDX, and the penetration depth is determined within the overlapping range. In this case, the overlap of Si and S, that is, the penetration depth, is preferably 0 to 150 nm, more preferably 0 to 130 nm, and further preferably 0 to 100 nm.

[0040] When the composite membrane for gas separation of the present invention is subjected to nanoperm porometry analysis under conditions of a temperature of 40° C., with He as a non-condensable gas and H2O as a condensable gas, the He permeability at a relative humidity of 90% is 60% to 100% of the He permeability at a relative humidity of 10%, more preferably 70% to 100%, and even more preferably 90% to 100%.

[0041] Nanoperm porometry is an analytical technique that can measure the pore size distribution of 0.5 nm to 50 nm from the relationship with the capillary condensation diameter by supplying a mixture of condensable and non-condensable gases to a measurement sample, changing the relative pressure of the condensable gas, and measuring the change in the amount of non-condensable gas that permeates from the sample. The capillary condensation diameter is 0.9 nm at a temperature of 40 ° C and a relative humidity of 10%, and the capillary condensation diameter is 20 nm at a temperature of 40 ° C and a relative humidity of 90%. When the He permeability at a relative humidity of 90% is 60% or more compared to the He permeability at a relative humidity of 10%, the contribution of the capillary condensation diameter of about 0.9 nm to about 20 nm to the He permeability is 40% or less, which means that there are few coarse pores of nano size or larger. The smaller the permeation contribution of the coarse pores, the less undesirable permeation of other gases such as oxygen, nitrogen, and methane caused by the coarse pores occurs, and high separation performance can be exhibited.

[0042] In the composite membrane for gas separation of the present invention, the contact angle between the surface of the coating layer and pure water in air is preferably 50° or more and 130° or less. A contact angle of 50° or more can suppress gas permeation through the coarse pores, and can significantly suppress the permeation of oxygen, nitrogen, methane, etc. A contact angle of 130° or less can suppress the decrease in the permeability of light gases such as hydrogen and helium, and can exhibit high selective separation properties. A contact angle of 80° or more and 130° or less is more preferable, and a contact angle of 100° or more and 130° or less is particularly preferable.

[0043] The contact angle here refers to the static contact angle, and in accordance with ISO 19403-1 (2017), 3.0 μL of distilled water was dropped onto the coating layer side of the composite membrane for gas separation, and the contact angle (the angle between the tangent of the droplet and the solid surface) was measured 1 second after the water droplet was dropped. When pure water is dropped onto the surface of the coating layer, the following equation 2, known as the "Young's equation," holds true.

[0044]

number

[0045] Here, γ S is the surface tension of the coating layer, γ Lis the surface tension of pure water, γ SL is the interfacial tension between the coating layer and pure water. When this formula is satisfied, the angle θ between the tangent to the pure water and the coating layer surface is called the contact angle. Contact angles can be measured using a wide variety of commercially available devices, for example, a Contact Angle Meter (manufactured by Kyowa Interface Science Co., Ltd.).

[0046] The contact angle gradually decreases over time. In the present invention, when the contact angle 1 second after a drop of pure water is applied to the surface of the coating layer is defined as X and the contact angle 30 seconds after is defined as Y, the following formula 1 is satisfied.

[0047]

number

[0048] Y / X is preferably 0.8 or more and 1 or less, more preferably 0.9 or more and 1 or less, and particularly preferably 0.95 or more and 1 or less. When Y / X is in this range, it is possible to promote the permeation of light gases such as hydrogen and helium, and to suppress the permeation of gases such as oxygen and nitrogen, thereby achieving high selective separation properties.

[0049] The average pore diameter Rc [nm] of the coating layer formed by the positron beam method is preferably 0.6 nm to 1.2 nm, more preferably 0.7 nm to 1.0 nm, and even more preferably 0.75 nm to 0.85 nm. By making the average pore diameter Rc [nm] of the coating layer 0.6 nm or more, it is possible to maintain the permeability of gases with small molecular diameters such as hydrogen, helium, water vapor, and ammonia as large as possible, and by making it 1.0 nm or less, it is possible to effectively suppress the permeation of oxygen, nitrogen, methane, etc. caused by coarse pores and defects in the functional layer.

[0050] The positron beam method is one of the positron annihilation lifetime measurement methods, which measures the time from when a positron enters a sample until it annihilates, and is a method for non-destructively evaluating information on the size, number density, and distribution of vacancies of approximately 0.1 to 10 nm from the annihilation time. 22 This method differs from the usual positron annihilation method in that it uses a positron beam instead of Na), making it possible to measure thin films with a thickness of several hundred nm. The average vacancy diameter Rc [nm] of the coating layer can be calculated from the positron annihilation lifetime τ when a positron is bombarded with 1 keV energy from the surface with the coating layer.

[0051] The average vacancy diameter Rc [nm] of the coating layer is calculated based on the above-mentioned positron annihilation lifetime τ from the following formula 3. Formula 3 shows the relationship when it is assumed that orthopositronium (o-Ps) exists in the vacancy of average vacancy diameter Rc in the electron layer of thickness ΔR, and ΔR is empirically calculated to be 0.166 nm (details are described in Nakanishi et al., Journal of Polymer Science, Part B: Polymer Physics, Vol. 27, p. 1419, John Wiley & Sons, Inc. (1989)).

[0052]

number

[0053] The material for forming the coating layer may be an organic material such as silicone resin, polyolefin resin, polyvinyl alcohol, or polyurethane, or a metal-organic framework such as MOF (Metal Organic Frameworks), or a metal-based material using palladium or a palladium alloy as a hydrogen permeable material. Polysiloxane is particularly preferable from the viewpoints of availability, ease of handling, and the fact that the average pore diameter Rc [nm] of the material satisfies the above-mentioned range.

[0054] The thickness of the coating layer is preferably 0.2 μm to 2.0 μm, more preferably 0.5 μm to 1.5 μm, and even more preferably 0.7 μm to 1.2 μm. By making it 0.2 μm or more, it is possible to prevent defects in the coating layer caused by unevenness in the separation functional layer or uneven thickness of the coating. By making it 2.0 μm or less, it is possible to reduce the reduction in gas permeability caused by the coating layer and maintain a high gas permeability.

[0055] The coating layer thickness can be determined by observing the cross section of the composite gas separation membrane using a scanning electron microscope and analyzing the cross section image obtained. The freeze fracturing method is used to prepare the observation sample. Specifically, the sample is frozen using a refrigerant such as liquid nitrogen, and the cross section is exposed using a razor or microtome. Image analysis software such as ImageJ and Mac-View can be used for image analysis.

[0056] Si in a region of 0 to 50 nm depth from the surface of the coating layer side detected by time-of-flight secondary ion mass spectrometry (TOF-SIMS) - The peak is preferably 10,000 counts or more and 100,000 counts or less, more preferably 15,000 counts or more and 100,000 counts or less, and even more preferably 20,000 counts or more and 100,000 counts or less. By having a Si-peak of 10,000 counts or more, a coating layer of sufficient thickness can be formed to suppress permeation through the coarse pores of the separation functional layer.

[0057] (Gas permeability of composite membranes for gas separation) It is essential that the He permeability is 1.10 times or more and 1.65 times or less of the H2 permeability, more preferably 1.20 times or more and 1.60 times or less, and further preferably 1.30 times or more and 1.50 times or less.

[0058] The kinetic molecular diameter (also called kinetic molecular diameter) of He is 0.260 nm, and that of H2 is 0.289 nm, with He being slightly smaller than H2. The greater the difference between the He permeability and the H2 permeability, the more small pores are distributed in the gas separation composite membrane, and the greater the difference in permeability according to the kinetic molecular diameter of the gas, and the higher the selective separation ability for oxygen, nitrogen, and methane.

[0059] When the He permeability is 1.10 times or more the H2 permeability, selective separation from gases with large molecular diameters can be achieved by screening according to the molecular diameter of the gas, and when it is 1.65 times or less, it is possible to prevent a decrease in H2 permeability due to excessively small pores and inhibition of H2 permeation due to low H2 solubility.

[0060] In addition, the H2 permeability at 25℃ is 1nmol / m 2 / s / Pa or more 100nmol / m 2 / s / Pa or less is preferable, and 5 nmol / m 2 / s / Pa or more 60nmol / m 2 / s / Pa or less is more preferable, and 10 nmol / m 2 / s / Pa or more 40nmol / m 2 / s / Pa or less is more preferable. 2 / s / Pa or more, the membrane area required for hydrogen separation can be reduced, and the 2 / s / Pa or less, it is possible to suppress the membrane surface polarization during hydrogen permeation under high pressure conditions, and prevent a decrease in separation performance.

[0061] (Rf and d NKP Relationship The average pore radius Rf [nm] of the separation functional layer determined by a positron beam method and the pore diameter d of the gas separation composite membrane determined by Equation 4 NKP It is preferable that [nm] satisfies formula 5.

[0062]

number

[0063]

number

[0064] Here, "i" is either H2, N2, or CH4, and "Pi" is the permeability of gas i at 25°C [nmol / m 2 / s / Pa], and P He is the permeability of He gas at 25°C [nmol / m 2 / s / Pa], Mi is the molecular weight of gas i, M He is the molecular weight of He gas, and d k,i is the kinetic diameter of gas i [nm], and d k,He is the kinetic molecular diameter of He gas [nm].

[0065] The average pore radius Rf [nm] of the separation functional layer can be calculated from a pore size analysis of the separation functional layer observed by a positron beam method or a scanning transmission electron microscope (hereinafter, "STEM"). The positron beam method is one of the positron annihilation lifetime measurement methods, which measures the time from when a positron enters a sample until it annihilates, and is a method for non-destructively evaluating information on the size, number density, and distribution of vacancies of approximately 0.1 to 10 nm from the annihilation time. 22 This method differs from the usual positron annihilation method in that it uses a positron beam instead of Na, making it possible to measure thin films with a thickness of several hundred nm. The average pore radius Rf [nm] of the separation functional layer can be calculated from the positron annihilation lifetime τ when a positron is implanted with an energy of 1 keV from the surface having the separation functional layer.

[0066] The average pore radius Rf [nm] of the separation functional layer of the gas separation composite membrane of the present invention is calculated based on the above-mentioned positron annihilation lifetime τ from the following formula 6. Formula 6 shows the relationship when it is assumed that orthopositronium (o-Ps) is present in the pores of average pore radius Rf of the separation functional layer in the electronic layer of thickness ΔR, and ΔR has been empirically calculated to be 0.166 nm (details are described in Nakanishi et al., Journal of Polymer Science, Part B: Polymer Physics, Vol. 27, p. 1419, John Wiley & Sons, Inc. (1989)).

[0067]

number

[0068] When analyzing by STEM, the sample with the substrate and support layer removed is transferred to a grid for TEM observation and measured using scanning electron microscopy (SEM) with a STEM and a secondary electron detector attached to the STEM device. The acquired STEM image is deconvoluted with DeConvHAADF (HREM research inc.) to highlight the pores and polyamide structure. Next, binarization is performed using ImageJ, and particle size analysis is performed to quantitatively analyze the number of pores and pore size in each region. From this analysis, the pore size and area for each pore can be calculated as the number of pixels in the image. The average pore radius Rf [nm] of the separation functional layer is preferably 0.2 nm to 0.4 nm, more preferably 0.22 nm to 0.35 nm, and even more preferably 0.24 nm to 0.30 nm. When the average pore radius Rf [nm] of the separation functional layer is 0.2 nm or more, the permeability of the gas to be permeated through the membrane can be increased, and when it is 0.4 nm or less, selective separation according to the molecular diameter of the gas can be expressed.

[0069] pore diameter d NKP[nm] is calculated from the following formula 4 based on the NKP (Normalized-Knudsen-based Permeance) method. The NKP method measures the membrane permeation flow rate of many types of non-condensable gases with different molecular diameters, plots the dynamic molecular diameter of the gas on the horizontal axis and the membrane permeation flow rate on the vertical axis, and calculates the pore diameter d by curve fitting using formula 4. NKP In this specification, four types of gases, He, H2, N2, and CH4, are used as non-condensable gases (Lie Meng et al., Journal of Membrane Science, Vol. 496, p. 211-218, Department of Chemical Engineering, Graduate School of Engineering, Hiroshima University (2015) for details).

[0070]

number

[0071] In general, the separation functional layer of a composite membrane for gas separation has a pore size distribution. Ideally, it should have only appropriate pores with appropriate pore sizes that provide excellent selective separation of the target gas. However, in reality, it often has coarse pores with low selective separation, and in order to improve selective separation, it is important to reduce the contribution of coarse pores.

[0072] In a membrane in which the contribution of the coarse pores in the separation functional layer is reduced, the pore diameter d calculated by the NKP method is the pore diameter (2Rf) calculated from the average pore radius Rf [nm] of the separation functional layer. NKP [nm] becomes smaller. The pore diameter d calculated by the NKP method NKP It is preferable that the pore diameter d [nm] is 0.60 times or more and 0.90 times or less of the pore diameter (2Rf) calculated from the average pore radius Rf [nm] of the separation functional layer, that is, it satisfies the formula 5, it is more preferable that it is 0.65 times or more and 0.85 times or less, and it is even more preferable that it is 0.70 times or more and 0.80 times or less. NKPBy making the "pore diameter (2Rf)" 0.60 times or more, the permeation of gases with small molecular diameters such as hydrogen, helium, water vapor, and ammonia can be increased, and the "pore diameter d NKP By setting the "pore size (2Rf)" to 0.90 or less, the selective separation can be increased.

[0073] Methods for reducing the contribution of coarse pores in the separation functional layer, that is, methods for satisfying formula 5, include coating the surface of the separation functional layer, adsorption of different substances to the functional layer and / or the porous support layer, densifying the support membrane by improving the manufacturing method, consolidating the porous support layer by applying pressure, etc. Providing gas permeation resistance to places other than the separation functional layer by these methods is important for reducing the contribution of coarse pores.

[0074] Coarse pores have a low gas permeation resistance and therefore a significantly high gas permeability. On the other hand, proper pores have a much higher gas permeation resistance and a lower gas permeability than coarse pores. When gas permeation resistance is provided to a portion other than the separation functional layer using the above-mentioned method, gas permeation from the coarse pores is significantly suppressed, but the effect on gas permeation through proper pores is small, so that it is possible to reduce the contribution of gas permeation from the coarse pores and improve the selective separation property of the entire membrane.

[0075] 2. Manufacturing method of composite membrane for gas separation Next, the method for producing the above-mentioned composite membrane for gas separation will be described with reference to an example.

[0076] (Formation of the support film) The laminate of the substrate and the porous support layer is called a support membrane, and this case will be described. In the example given below, the method of forming the support membrane includes a step of preparing a polymer solution by dissolving a polymer, which is a component of the porous support layer, in a good solvent for the polymer, a step of applying the polymer solution to the substrate, and a step of wet-coagulating the polymer by immersing the polymer solution in a coagulation bath. The coagulated polymer corresponds to the porous support layer.

[0077] When at least one of polysulfone and polyethersulfone is used as the polymer, a polymer solution is obtained by dissolving it in N,N-dimethylformamide (DMF). Water is preferably used as the coagulation bath.

[0078] Aramid, an example of a polymer, can be obtained by solution polymerization or interfacial polymerization using acid chlorides and diamines as monomers. In solution polymerization, aprotic organic polar solvents such as N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethylacetamide (DMAc) can be used as the solvent. When acid chlorides and diamines are used as monomers to produce polyamides, hydrogen chloride is produced as a by-product. To neutralize hydrogen chloride, inorganic neutralizing agents such as calcium hydroxide, calcium carbonate, and lithium carbonate, as well as organic neutralizing agents such as ethylene oxide, propylene oxide, ammonia, triethylamine, triethanolamine, and diethanolamine are used.

[0079] (Formation of separation functional layer) Next, the process of forming the separation functional layer will be described. In the following description, a separation functional layer made of polyamide, which is one example of the separation functional layer, will be described. The separation functional layer made of polyamide is formed by forming polyamide on the support membrane through interfacial polycondensation of a polyfunctional amine and a polyfunctional acid halide.

[0080] More specifically, the process for forming the separation functional layer includes the following steps. (a) applying an aqueous solution containing a polyfunctional amine onto a porous support layer; (b) after step (a), applying to the porous support layer an organic solvent solution containing a polyfunctional acid halide.

[0081] In step (a), the concentration of the polyfunctional amine in the aqueous polyfunctional amine solution is preferably in the range of 0.1% by weight to 20% by weight, more preferably in the range of 0.5% by weight to 15% by weight. When the concentration of the polyfunctional amine is in this range, sufficient selective separation property and gas permeability can be obtained.

[0082] The polyfunctional amine aqueous solution may contain a surfactant, an organic solvent, an alkaline compound, an antioxidant, etc., as long as it does not interfere with the reaction between the polyfunctional amine and the polyfunctional acid halide. The surfactant has the effect of improving the wettability of the support membrane surface and reducing the interfacial tension between the polyfunctional amine aqueous solution and the nonpolar solvent.

[0083] The application of the polyfunctional amine aqueous solution to the porous support layer is preferably performed uniformly and continuously on the porous support layer. The application means contacting the polyfunctional amine aqueous solution with the porous support layer, specifically, coating the surface of the porous support layer with the polyfunctional amine aqueous solution, or immersing the support film in the polyfunctional amine aqueous solution. Examples of the coating method include dripping, spraying, and roller application.

[0084] The time from when the aqueous polyfunctional amine solution is applied onto the porous support layer until the solution is drained or when the polyfunctional acid halide is applied (i.e., the contact time between the porous support layer and the aqueous polyfunctional amine solution) is preferably from 1 second to 10 minutes, and more preferably from 10 seconds to 3 minutes.

[0085] After the aqueous solution of the polyfunctional amine is applied to the porous support layer, the solution is drained so that no droplets remain on the porous support layer. Areas where droplets remain can become membrane defects and reduce separation performance, but draining the solution can prevent this. Methods that can be used include holding the support membrane after application of the aqueous solution of the polyfunctional amine vertically to allow excess aqueous solution to flow naturally, or blowing an air current such as nitrogen from an air nozzle to forcibly drain the solution.

[0086] In step (b), the concentration of the polyfunctional acid halide in the organic solvent solution is preferably in the range of 0.01% by weight to 10% by weight, more preferably in the range of 0.02% by weight to 2.0% by weight, because a sufficient reaction rate can be obtained by making it 0.01% by weight or more, and the occurrence of side reactions can be suppressed by making it 10% by weight or less.

[0087] The organic solvent is preferably one that is immiscible with water, dissolves the polyfunctional acid halide, and does not destroy the support film, and is inactive against the polyfunctional amine compound and the polyfunctional acid halide. Preferred examples include hydrocarbon compounds such as n-hexane, n-octane, n-nonane, n-decane, n-undecane, n-dodecane, n-tridecane, isooctane, isodecane, and isododecane, or mixtures thereof.

[0088] The method of applying the polyfunctional acid halide solution to the porous support layer may be the same as the method of applying the polyfunctional amine aqueous solution to the porous support layer, except that the polyfunctional acid halide solution is preferably applied to only one side of the porous support layer, and therefore is preferably applied by coating rather than immersion.

[0089] At this time, the porous support layer contacted with the organic solvent solution of the polyfunctional acid halide may be heated. The temperature for the heat treatment is 50°C or more and 180°C or less, preferably 60°C or more and 160°C or less. By heating at 60°C or more, the decrease in reactivity due to the consumption of monomers in the interfacial polymerization reaction can be compensated for by the heat-induced reaction promotion effect. By heating at 160°C or less, the solvent can be prevented from completely volatilizing, which would cause a significant decrease in reaction efficiency. In addition, the heat treatment time for each time is preferably 5 seconds or more and 600 seconds or less. By setting it to 5 seconds or more, the reaction promotion effect can be obtained, and by setting it to 600 seconds or less, the solvent can be prevented from completely volatilizing.

[0090] Furthermore, a polyfunctional halide may be added during the interfacial polycondensation reaction to promote consumption of the polyfunctional amine.

[0091] (Formation of coating layer) Next, the process of forming the coating layer will be described. The coating layer is preferably formed by contacting the separation functional layer with a solution or emulsion containing a substance that forms a coating layer. The contact method is not particularly limited, but it is preferable to coat the separation functional layer with a solution or emulsion containing a substance that forms a coating layer, since it is easy to control the thickness of the coating layer. Other contact methods include application from the porous support layer side and immersion of the membrane in a solution.

[0092] The coating method is not particularly limited, but microgravure, bar coating, spin coating, and the like, which are suitable for thin film coating, are preferred.

[0093] Examples of the solvent for the solution or emulsion containing the substance that forms the coating layer include water, alcohols such as ethanol, 2-butanol, and isopropanol, pentane, benzene, hexane, toluene, and chloroform, and water, ethanol, and hexane are preferred in that they cause less deterioration of the separation functional layer and the porous support layer. When water is used as the solvent, the pH of the aqueous solution is preferably in the range of 3 to 11 in order to minimize deterioration of the composite membrane for gas separation.

[0094] The material forming the coating layer is not particularly limited, but as described above, organic materials such as silicone resin, polyolefin resin, polyvinyl alcohol, polyurethane, etc., as well as metal-organic frameworks (MOFs), hydrogen permeable materials such as palladium or palladium alloys, etc., can be used. From the viewpoints of availability, ease of handling, and the material being capable of satisfying the above-mentioned range of contact angle between the coating layer surface and pure water in air, it is preferable to use polysiloxane as the main component. The polysiloxane may be brought into contact with the separation functional layer, or the polysiloxane may be formed after contact. Examples of such reagents include methyl ethyl ketoxime, methyl tris (methyl ethyl ketoxime) silane, vinyl tris (methyl ethyl ketoxime) silane, amino ethyl amino propyl trimethoxy silane, γ-amino propyl triethoxy silane, octamethyl cyclotetrasiloxane, cyclic siloxane ester, polydimethyl siloxane, etc. Furthermore, among these, a polymer obtained by polymerizing one type of monomer, a polymer obtained by polymerizing two or more types of monomers, or a solution containing a commercially available mixture may be brought into contact. For example, the TSE series manufactured by Momentive Performance Materials, Inc., silicone resin, silicone oligomer, and silicone emulsion manufactured by Shin-Etsu Silicones Co., Ltd. may be used.

[0095] 3. Spiral-type composite membrane module for gas separation (overview) When the composite membrane for gas separation of the present invention has a flat membrane shape, it can be applied to a spiral-type module or a stack-type module, and when it has a hollow fiber shape, it can be applied to a hollow fiber type module, but the following description will focus on a spiral-type module.

[0096] The spiral-type composite membrane module for gas separation of the present invention is a composite membrane module for gas separation in which the above-mentioned composite membrane for gas separation of the present invention, a feed-side flow path material, and a permeation-side flow path material are wound around a central tube that accumulates the permeating gas, and will be described in detail below.

[0097] 2 is a partially exploded perspective view of the spiral-type composite membrane module for gas separation (50). As shown in Fig. 2, the spiral-type composite membrane module for gas separation (50) includes a central tube (56), a composite membrane for gas separation (51), a feed-side flow path material (57), and a permeate-side flow path material (58).

[0098] (central canal) The central tube (56) is a hollow cylindrical member with a through hole formed on the side. The material of the central tube (56) may be any material that does not deteriorate depending on the pressure, temperature, or type of gas on the supply side when the module is used. In Fig. 2, G1 indicates the mixed gas, G2 indicates the permeated gas, and G3 indicates the concentrated gas.

[0099] (Composite membrane for gas separation) The gas separation composite membrane (51) is as described above. The gas separation composite membrane (51) is overlapped with a feed-side passage material (57) and a permeate-side passage material (58) and is spirally wound around a central tube (56).

[0100] One spiral-wound module can include a plurality of composite membranes for gas separation (51). By including these wound components, the spiral-wound composite membrane module for gas separation (50) has a generally cylindrical appearance with its major axis aligned along the longitudinal direction of the central tube (56).

[0101] The composite membranes for gas separation (51) are stacked so that the surfaces of the coating layers (supply side) face each other and the surfaces of the porous support layers or substrates (permeation side) face each other.

[0102] A feed-side passage material (57) is inserted between the surfaces of the gas separation composite membrane (51) on the coating layer side, and a permeate-side passage material (58) is inserted between the surfaces of the gas separation composite membrane (51) on the permeate side.

[0103] The supply-side flow passage is open at both longitudinal ends of the central tube (56). That is, a supply-side inlet is provided at one end of the spiral-type composite gas separation membrane module (50), and a supply-side outlet is provided at the other end. On the other hand, the supply-side flow passage is sealed at the end on the inner side in the winding direction, i.e., the end on the central tube side. The sealing is formed by folding the composite gas separation membrane, bonding the composite gas separation membrane with a hot melt or chemical adhesive, or fusing the composite gas separation membranes together using a laser or the like.

[0104] (channel material) The feed-side channel material (57) and the permeate-side channel material (58) are spacers that secure a channel between the gas separation composite membranes. The permeate-side channel material and the feed-side channel material may be the same material or different materials. Hereinafter, the permeate-side channel material and the feed-side channel material are collectively referred to as "channel material."

[0105] Examples of the flow path material include porous sheets such as nets, nonwoven fabrics, woven fabrics, knitted fabrics, and films. One or both sides of the sheet may be provided with protrusions made of resin or the like. Alternatively, protrusions may be directly fixed to the composite membrane for gas separation, and the protrusions may be used as the flow path material.

[0106] When the flow path material has a sheet and protrusions, the shape of the protrusions may be dots, curved or straight. If the protrusions are curved or straight, the gas flow can be controlled along the shape. The composition of the protrusions may be any composition that does not deteriorate depending on the pressure, temperature or type of gas on the supply side during use.

[0107] The flow path material is preferably made of a thermoplastic resin. From the viewpoint of suppressing damage to the gas separation composite membrane, the thermoplastic resin is preferably polyester, nylon, polyphenylene sulfide, polyethylene, polypropylene, polysulfone, polyethersulfone, ABS (acrylonitrile-butadiene-styrene) resin, or a UV-curable resin.

[0108] At least one of the feed-side flow passage material and the permeation-side flow passage material, and preferably both, has a thickness of 1000 μm or less, more preferably 700 μm or less, and particularly preferably 400 μm or less. By thinning the flow passage material in this way, the rigidity against bending is reduced, and it becomes less likely to break. In addition, by thinning the flow passage material, the area of ​​the composite membrane for gas separation that can be filled can be increased while maintaining the volume of the composite membrane module for gas separation.

[0109] 4.Gas Separation System The above-mentioned composite membrane for gas separation is capable of selectively permeating gases having small molecular diameters, such as hydrogen, helium, water vapor, and ammonia, and is applied to a gas separation system.

[0110] The gas separation system according to this embodiment includes the following steps. (1) A step of supplying a mixed gas containing gas A, which is a permeable component, and gas B, which is a non-permeable component, to one side of a composite membrane for gas separation. (2) A step of obtaining a gas having a molar ratio of gas A / gas B greater than that of the mixed gas from the other surface of the composite gas separation membrane.

[0111] In other words, according to this separation system, by taking advantage of the difference in the permeability of the gas separation composite membrane between gas A and gas B, which is an unwanted component, a permeable gas with a reduced concentration of gas B can be obtained from a mixture of gas A and gas B.

[0112] Although the gas B is not limited to a specific type, it is preferable that the mixed gas contains at least one gas selected from the group consisting of oxygen, nitrogen, and methane as the gas B. This is because the composite membrane for gas separation can efficiently separate gases with small molecular diameters, such as hydrogen, helium, water vapor, and ammonia, due to a large difference between the permeability of gases with small molecular diameters, such as hydrogen, helium, water vapor, and ammonia, and the permeability of oxygen, nitrogen, and methane.

[0113] The mixed gas may also contain water vapor. Water vapor adheres to the membrane and causes a decrease in the selective separation of light gases, but the composite membrane for gas separation exhibits excellent selective separation of gases even when the feed gas contains water vapor.

[0114] In the gas separation system of the present invention, the above-mentioned spiral-type composite membrane module for gas separation can be used. In addition, in the gas separation system of the present invention, the pressure vessels can be connected in series and / or parallel and housed in the pressure vessel for use.

[0115] In step (1), the feed gas may be pressurized by a compressor and then fed to the composite membrane for gas separation (its element), or the pressure on the permeate side of the composite membrane for gas separation may be reduced by a pump.

[0116] In addition, multiple elements may be connected in series. When multiple elements are used, either the permeate gas or the non-permeate gas of the upstream element may be supplied to the downstream element. In addition, the permeate gas or non-permeate gas of the downstream element may be mixed with the supply gas of the upstream element. The permeate gas or non-permeate gas may be supplied to the subsequent element, which may be pressurized by a compressor.

[0117] The gas supply pressure is not particularly limited, but is preferably 0.1 MPa to 10 MPa. By setting it to 0.1 MPa or more, the gas permeation rate increases, and by setting it to 10 MPa or less, pressure deformation of the gas separation composite membrane and its element members can be prevented. The value of "supply side pressure / permeation side pressure" is also not particularly limited, but is preferably 1.01 to 100,000, more preferably 1.10 to 1,000, and particularly preferably 1.50 to 100. By setting the value of "supply side pressure / permeation side pressure" to 1.01 or more, the gas permeation rate can be increased, and by setting it to 100,000 or less, the power costs for increasing the pressure on the supply side and reducing the pressure on the permeation side can be suppressed.

[0118] The gas supply temperature is not particularly limited, but is preferably 0°C to 200°C, and more preferably 15°C to 180°C. A temperature of 15°C or higher provides good gas permeability, while a temperature of 180°C or lower can prevent thermal deformation of the members constituting the gas separation composite membrane element. By using the above-mentioned gas separation composite membrane, it is possible to supply gas at a temperature of 80°C or higher, 90°C or higher, or 100°C or higher.

[0119] 5.Applications The composite membrane for gas separation of the present invention has excellent separation performance and can be suitably used for, for example, separating hydrogen gas from a mixed gas containing hydrogen and nitrogen, etc., separating hydrogen gas from a mixed gas containing hydrogen and oxygen, nitrogen, ammonia, etc., separating helium from a mixed gas containing helium and oxygen, nitrogen, etc., purifying He and H2, etc. EXAMPLES

[0120] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0121] A. Preparation of porous support membrane Unless otherwise specified, the temperature conditions are room temperature (25°C). The base material is a polyester nonwoven fabric made of long fibers (air permeability 2.0cc / cm 2 A 16 wt% dimethylformamide (DMF) solution of polysulfone (PSf) was cast onto the substrate (1000 nm / sec) at 25°C to a thickness of 200 µm, and the substrate was immediately immersed in pure water and left for 5 minutes to form a porous support layer. In this way, a porous support membrane having a substrate and a porous support layer was produced.

[0122] B. Preparation of separation functional layer (Composite separation membrane P) The porous support membrane obtained in A was immersed in a 0.2 wt % piperazine aqueous solution for 2 minutes. The porous support membrane was slowly pulled up vertically, and excess aqueous solution was removed from the surface of the porous support layer by blowing nitrogen from an air nozzle.

[0123] Next, an n-undecane solution containing 0.17% by weight of trimesoyl chloride (TMC) was applied so that the surface of the porous support layer was completely wet, and the layer was left to stand for 60 seconds at 25° C. After that, in order to remove excess solution from the separation membrane, the separation membrane was vertically held to allow the solution to flow, and then a blower was used to blow air at 25° C. onto the membrane to dry it, thereby draining the solution.

[0124] (Composite separation membrane Q) The porous support membrane obtained in A was immersed in a 0.2 wt % piperazine aqueous solution for 2 minutes. The porous support membrane was slowly pulled up vertically, and excess aqueous solution was removed from the surface of the porous support layer by blowing nitrogen from an air nozzle.

[0125] Next, in a booth kept at 45° C., an n-undecane solution containing 0.17% by weight of trimesoyl chloride (TMC) was applied so that the surface of the porous support layer was completely wet, and then dried for 60 seconds at 60° C. After that, in order to remove excess solution from the separation membrane, the separation membrane was vertically placed to allow the solution to flow, and further, air at 25° C. was blown onto the membrane using a blower to dry it, thereby draining the solution.

[0126] (Composite separation membrane R) The porous support membrane obtained in A was immersed in an aqueous solution of 4.0% by weight of m-phenylenediamine for 1 minute. The porous support membrane was slowly pulled up vertically, and excess aqueous solution was removed from the surface of the porous support layer by blowing nitrogen from an air nozzle.

[0127] Next, in a booth kept at 45° C., an n-undecane solution containing 0.20% by weight of trimesoyl chloride (TMC) was applied so that the surface of the porous support layer was completely wet, and then dried for 60 seconds in an oven at 100° C. After that, in order to remove excess solution from the separation membrane, the separation membrane was vertically placed to allow the solution to flow, and then a blower was used to blow air at 25° C. to dry the membrane, thereby draining the solution.

[0128] (Composite separation membrane S) The porous support membrane obtained in A was immersed in a 6.0 wt% m-phenylenediamine aqueous solution for 60 seconds. The porous support membrane was slowly pulled up vertically, and excess aqueous solution was removed from the surface of the porous support layer by blowing nitrogen from an air nozzle.

[0129] Next, in a booth kept at 45°C, an n-decane solution containing 0.17% by weight of trimesoyl chloride (TMC) was applied so that the surface of the porous support layer was completely wet, and the membrane was placed in an oven at 140°C and dried for 30 seconds while supplying water vapor at 100°C from a nozzle provided on the back side of the membrane. After that, in order to remove excess solution from the separation membrane, the separation membrane was turned vertically to make the solution flow, and then a blower was used to blow air at 25°C to dry it, thereby draining the liquid.

[0130] C. Gas permeability measurements (hydrogen, nitrogen permeability and selectivity) A separation membrane was held between the supply cell and the permeation cell of a test cell having a supply cell and a permeation cell. Hydrogen and nitrogen were used as measurement gases, and the pressure change of the permeation side per unit time of hydrogen and nitrogen was measured at a measurement temperature of 25°C in accordance with the pressure sensor method of ISO 15105-1 (2007). Here, the supply side was set to 100 kPa, the permeation side was set to 0 kPa, and the pressure difference between the supply side and the permeation side was set to 100 kPa. Next, the permeation rate Q of the permeated gas was calculated by the following formula, and the gas permeability was determined by the arithmetic mean when five arbitrary points were taken and measured for the same membrane. Then, the selectivity was calculated as the ratio of the permeation rates of the gases of each component. Incidentally, STP means standard conditions. Q = [Gas permeation flow rate (m 3 ·STP)] / [Membrane area (m 2 ) × time (s) × pressure difference (Pa)

[0131] D. Nanoperm Porometry Analysis A separation membrane was held between the supply cell and the permeation cell of a test cell having a supply cell and a permeation cell. Using H2O as a condensable gas and He as a non-condensable gas, the helium permeation rate was measured at a total of 21 points when the relative humidity was set at approximately 5% intervals from 0% to 95% at a measurement temperature of 40°C. In the measurement results, the value closer to 10% of the two points sandwiching a relative humidity of 10% was taken as the helium permeation rate at 10%, and the value closer to 90% of the two points sandwiching 90% was taken as the helium permeation rate at 90%. Here, the supply side was set to 190 kPa and the permeation side to 100 kPa, the flow rate was measured using a flow meter, and the He permeability was calculated. (Details of the measurement apparatus are given in Toshinori Tsuru et al., Journal of Membrane Science, Vol. 186, p. 257-265, Department of Chemical Engineering, Hiroshima University (2001).) The He permeability at each humidity was determined by the arithmetic average of measurements taken at three random points on the same membrane.

[0132] E. Contact angle measurement The contact angle was measured according to ISO 19403-1 (2017) by dropping 3.0 μL of distilled water onto the separation functional layer side of the composite membrane for gas separation, and measuring the contact angle (angle between the tangent of the droplet and the solid surface) 1 second after the water droplet was dropped. The contact angle 1 second after the pure water landed on the surface of the coating layer was defined as X, and the contact angle 30 seconds after was defined as Y, and the value was calculated as Y / X.

[0133] F. Measurement of the average pore radius Rf [nm] of the separation functional layer using the positron beam method The positron annihilation lifetime measurement of the separation functional layer in each example was carried out using a positron beam method as follows. That is, the separation functional layer was dried at room temperature under reduced pressure and cut into 1.5 cm x 1.5 cm squares to prepare test samples. The test samples were measured with a barium difluoride scintillation counter using a photomultiplier tube at a total count of 5 million at room temperature under vacuum using a thin film positron annihilation lifetime measurement device equipped with a positron beam generator (this device is described in detail in, for example, Radiation Physics and Chemistry, 58, 603, Pergamon (2000)). The test samples were measured with a total count of 5 million using a barium difluoride scintillation counter using a photomultiplier tube at a beam intensity of 1 keV, room temperature, and vacuum, and analyzed using POSITRONFIT. From the average positron annihilation lifetime τ of the fourth component obtained by the analysis, Rf [nm] was calculated using Equation 6. Rf was determined by the arithmetic mean of measurements taken at three arbitrary points on the same film.

[0134] G. TOF-SIMS peak intensity The separation membrane was dried at room temperature under vacuum, and time-of-flight secondary ion mass spectrometry was performed using a TOF SIMS 5 (ION TOF) device (secondary ion polarity: negative, mass range (m / z) = 0-2500, raster size: 300 μm, scan number: 1 scan / cycle, pixel number (per side): 128 pixels, measurement vacuum level (before sample introduction): 4 × 10 -7 Pa or less, charge neutralization: yes, post-acceleration: 9.5 kV, primary ion species: Bi3 ++ , Primary ion acceleration voltage: 30 kV, Pulse width: 14.1 ns, Bunching: Yes, Edging ion: Ar-GCIV, Edging ion acceleration voltage: 5 kV). Si in the separation membrane - The peak intensity of Si in the region from the surface of the coating layer to a depth of 0 to 50 nm was measured at intervals of 2.5 nm or less. - The average of the peak intensities was calculated. The Si was calculated by arithmetic average of five arbitrary points on the same film. - Peaks were determined.

[0135] H. Coating thickness measurement After freezing the composite membrane for gas separation with liquid nitrogen, the cross section was exposed with a razor. The cross section of the exposed composite membrane for gas separation was observed at a magnification of 10,000 times using a scanning electron microscope (Hitachi High-Technologies S-5500 type). At this time, the area observed was the range from the surface layer of the composite membrane for gas separation to the porous support layer. Before observing with the SEM, the membrane was coated with platinum-palladium. The obtained cross-sectional image was binarized with ImageJ and analyzed by image analysis. Specifically, thresholding was performed on the cross-sectional image with ImageJ, and the black layer that was continuous from the surface of the composite membrane for gas separation was taken as the coating layer. The coating layer thickness was measured at three points, the center, the right end, and the left end of the image, and the coating layer thickness in the cross-sectional image obtained was calculated by the arithmetic mean of the three points. The same operation was performed on five slice samples, and three fields of view were observed for each sample, and the coating layer thickness was determined by the arithmetic mean of a total of 15 data.

[0136] I. Measurement of the penetration thickness of the coating layer into the support film When the main component of the support layer was polysulfone and the main component of the coating layer was silicone, the following measurements were made using TEM-EDX.

[0137] The specimens were sliced ​​in the cross-sectional direction by the focused ion beam (FIB) method and observed using an analytical electron microscope (JEM-F200, manufactured by JEOL). Element mapping was performed at an acceleration voltage of 200 kV using an energy dispersive X-ray spectroscopy (EDX) detector (JED2300T 100 mm2 silicon drift (SDD) type, manufactured by JEOL). For the obtained 1 μm square image, the mapping image of Si in the coating layer and the mapping image of S in the support layer were superimposed. Next, the overlap of Si and S was measured at 10 points in the width direction, and the penetration thickness of the coating layer in the obtained cross-sectional image was calculated by the arithmetic mean of the 10 points. The same operation was performed in two fields of view, and the arithmetic mean value of the two fields of view was taken as the penetration thickness of the coating layer.

[0138] When the main component of the support layer was other than polysulfone, or the main component of the coating layer was other than silicone, SEM cross-sectional images were obtained as described above in H, and the thickness of the coating layer penetrating into the support layer was determined in the same manner as in calculating the thickness of the coating layer.

[0139] J. Support layer thickness measurement Since the functional layer thickness of the gas separation composite membrane is very thin, the support layer thickness was calculated by subtracting the coating layer thickness obtained in H above and the thickness of the substrate alone from the thickness of the gas separation composite membrane after the coating layer was formed. First, the thickness of the gas separation composite membrane was measured using a PEACOCK digital thickness gauge manufactured by Ozaki Seisakusho Co., Ltd. 20 points were measured in the width direction, and the average value was calculated. Next, the coating layer, functional layer, and support layer of the gas separation composite membrane were peeled off from the substrate, and the thickness of the substrate was measured in the same manner. Support layer thickness (μm) = composite membrane thickness for gas separation (μm) - substrate thickness (μm) - coating layer thickness (μm) K. Measurement of the average pore radius Rf [nm] of the separation functional layer by STEM When it was difficult to peel off the coating layer and the separation functional layer and Rf could not be calculated by the method E above, the support layer was dissolved to separate the separation functional layer and the support layer, a sample consisting of only the separation functional layer and the coating layer was formed, and Rf was obtained by STEM observation of the separation functional layer side. When the main component of the support layer was polysulfone and the main component of the coating layer was silicone, the substrate was physically peeled off and the polysulfone was dissolved with dichloromethane to obtain a sample consisting of only the separation functional layer and the coating layer. The sample was transferred to a grid for TEM observation, and the sample was prepared so that the separation functional layer could be observed from the side that was in contact with the support layer. The prepared sample was photographed using a field emission transmission electron microscope (Hitachi High-Tech HF5000) at an accelerating voltage of 200 kV, and a STEM image with a magnification of 100,000 was obtained. The obtained image was then analyzed using image processing software to calculate the pore size.

[0140] Example 1 The composite separation membrane P obtained in B has a membrane area of ​​25 cm 2The membrane was cut into a circular shape. Polymethylpentene (Momentive Performance Materials) was dissolved in hexane (Fujifilm Wako Pure Chemical Industries, Ltd.) to prepare a 4 wt% polymethylpentene solution. 1 mL of the solution was dropped onto the surface of the separation functional layer, and spin-coated at a speed of 500 rpm for 60 seconds to form a coating layer. Finally, the membrane was dried in a vacuum at 40°C for 12 hours or more to obtain a composite membrane for gas separation. The obtained composite membrane for gas separation was evaluated, and the results are shown in Table 1.

[0141] Example 2 A composite membrane for gas separation was produced by forming a coating layer of poly(1-trimethylsilyl-1-propyne) by carrying out the same treatment as in Example 1, except that poly(1-trimethylsilyl-1-propyne) was used instead of polymethylpentene. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 1.

[0142] Example 3 A composite membrane for gas separation was produced by forming a coating layer of polydimethylsiloxane by carrying out the same process as in Example 1, except that TSE389 (manufactured by Momentive Performance Materials, Inc.) was used instead of polymethylpentene. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 1.

[0143] Example 4 A composite membrane for gas separation was produced by forming a coating layer of polymethylpentene by carrying out the same treatment as in Example 1, except that the composite separation membrane was Q. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 1.

[0144] Example 5 A composite membrane for gas separation was produced by forming a coating layer of polydimethylsiloxane by carrying out the same treatment as in Example 3, except that the composite separation membrane was Q. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 1.

[0145] [Table 1]

[0146] Example 6 A composite membrane for gas separation was produced by forming a coating layer of polymethylpentene by carrying out the same treatment as in Example 1, except that the composite separation membrane was R. The obtained composite membrane for gas separation was evaluated, and the results are shown in Table 2.

[0147] Example 7 A composite membrane for gas separation was produced by forming a coating layer of poly(1-trimethylsilyl-1-propyne) by carrying out the same treatment as in Example 2, except that the composite separation membrane was R. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 2.

[0148] Example 8 A composite membrane for gas separation was produced by forming a coating layer of polydimethylsiloxane by carrying out the same treatment as in Example 3, except that the composite separation membrane was R. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 2.

[0149] Example 9 A composite membrane for gas separation was produced by forming a coating layer of polydimethylsiloxane by carrying out the same treatment as in Example 3, except that the composite separation membrane was S. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 2.

[0150] Example 10 A composite membrane for gas separation was produced by forming a coating layer of polydimethylsiloxane by carrying out the same treatment as in Example 9, except that the amount of TSE389 was 2.0 wt %. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 2.

[0151] Example 11 A composite membrane for gas separation was produced by forming a coating layer of polydimethylsiloxane by carrying out the same treatment as in Example 9, except that the amount of TSE389 was 12.0 wt %. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 2.

[0152] [Table 2]

[0153] Comparative Example 1 Composite separation membrane P was evaluated as a composite membrane for gas separation without forming a coating layer, and the results are shown in Table 3. Because it had no coating layer, it was hydrophilic with a contact angle of 29 degrees, and furthermore, the contribution of permeation from the coarse pores was large, so the ratio of He permeability at a relative humidity of 90% to that at a relative humidity of 10% was extremely low at 0.45, and selectivity could not be sufficiently improved.

[0154] Comparative Example 2 When the composite separation membrane Q was evaluated as it is as a composite membrane for gas separation without forming a coating layer, the results are shown in Table 3. Because it had no coating layer, it was hydrophilic with a contact angle of 22 degrees, and furthermore, because the contribution of permeation from the coarse pores was large, the ratio of He permeability at a relative humidity of 90% to that at a relative humidity of 10% was extremely low at 0.47, and selectivity could not be sufficiently improved.

[0155] Comparative Example 3 When the composite separation membrane R was evaluated as it is as a composite membrane for gas separation without forming a coating layer, the results are shown in Table 3. Because it did not have a coating layer, the contact angle was hydrophilic at 38 degrees, and furthermore, the contribution of permeation from the coarse pores was large, so the ratio of He permeability at a relative humidity of 90% to that at a relative humidity of 10% was low at 0.55, and selectivity could not be sufficiently improved.

[0156] Comparative Example 4 When the composite separation membrane S was evaluated as it was for gas separation without forming a coating layer, the results are shown in Table 3. Because it had no coating layer, it was hydrophilic with a contact angle of 41 degrees, and furthermore, because the contribution of permeation from the coarse pores was large, the ratio of He permeability at a relative humidity of 90% to that at a relative humidity of 10% was low at 0.57, and selectivity could not be sufficiently improved.

[0157] Comparative Example 5 A composite membrane for gas separation was produced by forming a coating layer of polymethylpentene by carrying out the same process as in Example 1, except that the amount of polymethylpentene was 1.0 wt %. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 3. Although the membrane had a coating layer, the coating layer was not sufficiently formed, so that the permeation contribution from the coarse pores was large, and the ratio of the He permeability at a relative humidity of 90% to that at a relative humidity of 10% was large at 0.61, while the contact angle was 48 degrees, which was hydrophilic, and the selectivity could not be sufficiently improved.

[0158] Comparative Example 6 A composite membrane for gas separation was produced by forming a polydimethylsiloxane coating layer by carrying out the same process as in Example 9, except that the amount of TSE389 was 0.5 wt%. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 3. Although the membrane had a coating layer and was hydrophobic with a contact angle of 122 degrees, the coating layer was not sufficiently formed, which increased the contribution of permeation from the coarse pores. As a result, the ratio of the He permeability at a relative humidity of 90% to that at a relative humidity of 10% was low at 0.58, and the selectivity could not be sufficiently improved.

[0159] Comparative Example 7 A composite membrane for gas separation was prepared in the same manner as in Example 9, except that the amount of perfluoropentanoic acid chloride was 0.2% by weight. The composite membrane for gas separation thus obtained was evaluated, and the results are shown in Table 3. Although no coating layer was formed and the contact angle was 139 degrees, which was hydrophobic, the selectivity could not be sufficiently improved due to a significant decrease in light gas permeability.

[0160] [Table 3]

[0161] (Reference example 1) The composite membrane for gas separation described in Non-Patent Document 1, in which the surface of a polyamide composite membrane is coated with polyphenylene oxide, is as shown in Table 4.

[0162] (Reference example 2) The composite membrane for gas separation described in Non-Patent Document 2, in which the surface of a polyamide composite membrane is coated with polydimethylsiloxane, is as shown in Table 4.

[0163] [Table 4] [Industrial Applicability]

[0164] The composite membrane for gas separation of the present invention is suitably used for separating and purifying a specific gas from a mixed gas. [Explanation of symbols]

[0165] 50: Spiral-type composite membrane module for gas separation 51: Composite membranes for gas separation 52: Porous support layer 53: Separation functional layer 54: Covering layer 55: Base material 56: Central tube 57: Supply side channel material 58: Permeate side channel material G1: Mixed gas G2: Permeable gas G3: Concentrated gas

Claims

1. A composite membrane for gas separation having at least a porous support layer, a separation functional layer, and a coating layer in this order, The non-condensable gas is He, and the condensable gas is H 2 When nanoperm porometry analysis was performed under conditions of 0 and a temperature of 40° C., the He permeability at a relative humidity of 90% was 60% to 100% of the He permeability at a relative humidity of 10%, A composite membrane for gas separation, in which the contact angle between the coating layer surface and pure water in air measured in accordance with ISO 19403-1 (2017) is 50° or more and 130° or less.

2. 2. The composite membrane for gas separation according to claim 1, wherein a contact angle X 1 second after a drop of pure water lands on the surface of the coating layer and a contact angle Y 30 seconds after the drop of pure water lands on the surface of the coating layer satisfy formula 1. [0010]

3. 2. The composite membrane for gas separation according to claim 1, wherein the average pore radius Rf [nm] of the separation functional layer determined by a positron beam spectroscopy is 0.2 nm or more and 0.4 nm or less.

4. A coating layer is provided on the separation functional layer, and Si in a region of 0 to 50 nm deep from the surface of the coating layer side is detected by time-of-flight secondary ion mass spectrometry (TOF-SIMS). - 2. The composite membrane for gas separation according to claim 1, wherein the peak is from 10,000 counts to 100,000 counts.

5. 2. The composite membrane for gas separation according to claim 1, wherein the main component of the separating functional layer is a crosslinked aromatic polyamide.

6. H at 25°C 2 Permeability is 1 nmol / m 2 / s / Pa or more 100nmol / m 2 2. The composite membrane for gas separation according to claim 1, wherein the viscosity is 1 / s / Pa or less.

7. 7. A spiral-type composite membrane module for gas separation, comprising the composite membrane for gas separation according to claim 1, a feed-side flow path material, and a permeate-side flow path material wound around a central tube.

8. A gas separation system comprising the spiral-type composite membrane module for gas separation according to claim 7.

9. He or H using the gas separation system according to claim 8. 2 A method for refining.

Citation Information

Patent Citations