Cordierite-indialite-pseudobrookite-structured ceramic body, batch compositional mixture, and method for producing ceramic body therefrom

Ceramic bodies with a cordierite-indialite-pseudobrookite crystalline structure address the challenges of high porosity, narrow pore size, and low thermal expansion in exhaust gas treatment, enhancing filtration efficiency and thermal stability for diesel and gasoline engines.

JP2024150619AActive Publication Date: 2024-10-23CORNING INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024116762
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-08-31
Filing Date
2024-07-22
Publication Date
2024-10-23
Estimated Expiration
2039-08-29

AI Technical Summary

Technical Problem

Existing ceramic honeycombs used in exhaust gas treatment applications face challenges in achieving high porosity, narrow pore size distribution, and low thermal expansion coefficients, which affect their performance and durability in extreme temperature fluctuations.

Method used

Development of ceramic bodies with a cordierite-indialite-pseudobrookite crystalline structure, specifically formulated with compositions that include 85-92% cordierite and indialite, up to 10% pseudobrookite, and controlled porosity and pore size distribution, along with low thermal expansion, to enhance filtration efficiency and thermal stability.

Benefits of technology

The ceramic bodies exhibit high porosity, narrow pore size distribution, and low thermal expansion, resulting in improved filtration efficiency, reduced backpressure, and enhanced thermal shock resistance, making them suitable for diesel and gasoline engine exhaust gas filtration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150619000001_ABST
    Figure 2024150619000001_ABST
Patent Text Reader

Abstract

To provide a ceramic body having a high porosity, a relatively large median pore diameter, a narrow pore size distribution, and a relatively low CTE, and a method for producing the ceramic body.SOLUTION: In a ceramic body, %P≥50% (where %P is an average bulk volume porosity) and df≤0.36 (where df is (d50-d10) / d50). The ceramic body contains a crystalline phase containing a total weight percentage of at least 85 wt.% of cordierite and indialite, and contains a crystalline phase containing up to 10 wt.% of a pseudobrookite structure. The ceramic body comprises, when expressed as a weight percentage based on oxides: 1 wt.% to 11 wt.% of titania, and 89 wt.% to 99 wt.% of MgO, Al2O3, and SiO2.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

Priority

[0001] This application claims priority under 35 U.S.C. § 119 of U.S. Provisional Patent Application No. 62 / 725,591, filed August 31, 2018, the contents of which are incorporated herein by reference in their entirety. This application is also a divisional application of Japanese Patent Application No. 2021-511643, filed August 29, 2019. [Technical field]

[0002] Exemplary embodiments of the present disclosure relate to cordierite and pseudobrookite structured ceramic bodies, and more particularly to porous cordierite and pseudobrookite structured honeycomb bodies useful for engine exhaust aftertreatment and other filtration applications. [Background technology]

[0003] Cordierite-based honeycombs and aluminum titanate-based honeycombs have been widely used in a variety of exhaust gas abatement / treatment applications, for example, in catalytic converters and in particulate filters for the control of emissions in diesel and gasoline engines.

[0004] Diesel particulate filters (DPF) and gasoline particulate filters (GPF) can be manufactured from a porous ceramic honeycomb body by plugging some of the channels in a pattern to form a plugged honeycomb body.

[0005] Exhaust gas flows through the porous walls of the plugged ceramic honeycomb body. Along its flow path through the porous walls, particulates from the exhaust gas can be deposited in the pores, on the surfaces of the porous walls, or on a soot layer deposited or formed on the surfaces of the porous walls, thereby providing filtration of the particulates from the exhaust gas. The soot layer that forms can be periodically combusted in a regeneration cycle, allowing the DPF / GPF to have a design life comparable to the life of a vehicle. Summary of the Invention

[0006] Exemplary embodiments of the present disclosure provide a ceramic body having a cordierite-indialite-pseudobrookite crystalline structure.

[0007] Exemplary embodiments of the present disclosure also provide a ceramic honeycomb body with porous walls comprising a cordierite-indialite-pseudobrookite crystalline structure.

[0008] Exemplary embodiments of the present disclosure also provide batch composition mixtures useful for producing cordierite-indialite-pseudobrookite crystalline structures.

[0009] One or more exemplary embodiments of the present disclosure also provide a method of making a ceramic body having a cordierite-indialite-pseudobrookite crystalline structure.

[0010] Additional features of the disclosure will be set forth in the description that follows, and in part will be obvious from the description, or may be learned by the practice of the embodiments disclosed herein.

[0011] In one aspect, an embodiment of the present disclosure is one in which: %P≧50% (where %P is the average bulk volume porosity); df≦0.36 (where df is (d 50 -d 10 ) / d 50 and a crystalline phase comprising cordierite and indialite having a combined weight percentage of at least 85 wt.%; and a crystalline phase comprising a pseudobrookite structure having a maximum of 10 wt.%; the ceramic body having a combined weight percentage of at least 85 wt.%; and a crystalline phase comprising a pseudobrookite structure having a combined weight percentage of at least ... 1 wt% to 11 wt% titania, and 89 wt% to 99 wt% MgO, Al2O3, and SiO2 (wherein the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4); or 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al2O3, and SiO2 (where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3). Contains:

[0012] Another exemplary embodiment discloses a ceramic body comprising a crystalline phase comprising cordierite and indialite with a combined weight percentage between 85 wt.% and 92 wt.% and a second crystalline phase of pseudobrookite structure comprising armalcolite with a maximum weight percentage of 10 wt.%, the ceramic body contains, expressed in weight percent on an oxide basis, 1 wt.% to 11 wt.% titania, and 89 wt.% to 99 wt.% MgO, Al2O3, and SiO2, where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4; 55% ≤ %P ≤ 72%; 8μm≦d 50 ≦20μm (where d 50 is the median pore size; 0.16≦df≦0.32 (where df is (d 50 -d 10 ) / d 50 (That is.)

[0013] Another exemplary embodiment discloses a ceramic body comprising a crystalline phase comprising cordierite and indialite with a combined weight percentage between 85 wt.% and 92 wt.% and a second crystalline phase of pseudobrookite structure comprising armalcolite with a maximum weight percentage of 10 wt.%, the ceramic body contains, expressed in weight percent on an oxide basis, 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al2O3, and SiO2, wherein the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3; 55% ≤ %P ≤ 72%; 8μm≦d 50 ≦20μm (where d 50 is the median pore size; 0.16≦df≦0.32 (where df is (d 50 -d 10 ) / d 50 (That is.)

[0014] In another exemplary embodiment, a batch composition mixture is disclosed, the batch composition mixture comprising, expressed as weight percent on an oxide basis: 1 wt.% to 11 wt.% titania, and 89 wt.% to 99 wt.% MgO, Al2O3, and SiO2, where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4; or 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al2O3, and SiO2 (where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3). The magnesia source, the alumina source, the silica source, and the titania source.

[0015] Yet another exemplary embodiment discloses a method of making a ceramic body, the method comprising: 20% to 42% by weight of a magnesia source; 25% to 40% by weight of an alumina source; 15% to 30% by weight of a silica source, and 1 wt. % to 10 wt. % of a titania source; wherein all of said weight percentages of each of said magnesia source, said alumina source, said silica source, and said titania source are based on 100% total weight of minerals present; mixing the inorganic components with an organic binder, 26 wt. % SA to 56 wt. % SA of a pore-forming agent, and a liquid vehicle to form a batch composition mixture, where wt. % SA is the weight percent of the add-on based on 100% total weight of the inorganics; forming the batch composition mixture into a green body; and firing the green body under conditions effective to convert the green body into a ceramic body having a combined weight percentage of at least 85% by weight of a crystalline phase containing cordierite and indialite, and up to 10% by weight of a crystalline phase containing a pseudobrookite structure. Includes.

[0016] It should be understood that both the foregoing Summary of the Invention and the following Detailed Description of the Invention provide a number of examples and are intended to provide a further understanding of the present disclosure.

[0017] The accompanying drawings are included to provide a further understanding of the present disclosure, are incorporated in and constitute a part of this specification, illustrate example embodiments, and together with the description, serve to explain the principles of the present disclosure. The drawings are not necessarily to scale. Like reference numerals are used to refer to the same or substantially similar parts. [Brief description of the drawings]

[0018] [Figure 1A] FIG. 1 is a perspective view of a ceramic body embodied as a honeycomb body comprising cordierite, indialite, and pseudobrookite crystalline structure ceramic according to an embodiment of the present disclosure; [Figure 1B]FIG. 1B is an enlarged end view of a portion of the ceramic honeycomb body of FIG. 1A according to an embodiment of the present disclosure. [Figure 1C] FIG. 1 is a perspective view of a ceramic body embodied as a plugged honeycomb body comprising cordierite, indialite, and pseudobrookite crystalline structure ceramic according to an embodiment of the present disclosure; [Diagram 2] FIG. 1 is a partial cross-sectional view of an extruder shown extruding a green honeycomb body according to an embodiment of the present disclosure. [Diagram 3] 1 is a ternary graph of the relative weight ratios of MgO:Al2O3:SiO2 within a field (based on a total of 100% MgO, Al2O3, and SiO2), according to an embodiment of the present disclosure. [Figure 4A] Representative photomicrographs of polished cross-sections of porous walls of exemplary ceramic bodies (e.g., Example E9) comprising cordierite, indialite, and pseudobrookite crystalline structure ceramics according to embodiments of the present disclosure. [Figure 4B] FIG. 1 is a representative photomicrograph of a polished cross section of a porous wall of an exemplary ceramic body (e.g., Example E7C) comprising cordierite, indialite, and pseudobrookite crystalline structure ceramic according to an embodiment of the present disclosure. [Figure 4C] Representative photomicrographs of polished cross-sections of porous walls of exemplary ceramic bodies (e.g., Example E20) including cordierite, indialite, and pseudobrookite crystalline structure ceramics according to embodiments of the present disclosure. [Diagram 5] Methods for Producing Ceramic Bodies Comprising Cordierite, Indialite, and Pseudobrookite Crystalline Structure Ceramic According to Embodiments of the Present Disclosure DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present disclosure will now be more fully described with reference to the accompanying drawings, which show exemplary embodiments. The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. In the drawings, the size and relative size of features and components may be exaggerated for clarity and therefore may not be drawn to scale. Like reference numbers in the drawings may refer to like elements.

[0020] When an element is said to be "on," "connected to," or "coupled to" another element, it should be understood that the element may be directly on or directly connected to the other element, or there may be intervening or interconnecting elements. In contrast, when an element is said to be "directly on," or "directly connected to," another element, there are no intervening elements present.

[0021] Various de-NOx or diesel oxidation catalysts (DOC), or three-way catalysts (TWC) or selective catalyst reduction (SCR) catalysts can be incorporated into the plugged honeycomb filter body. Relatively high catalyst efficiency can be achieved by utilizing high catalyst loadings. Washcoat loadings of 100 g / l are currently common, with future loadings potentially exceeding 150 g / l. In various embodiments, high catalyst loadings at low back pressures can be provided by honeycomb filter bodies made from ceramic honeycomb structures with extremely high porosity and relatively large pore sizes.

[0022] Porous cordierite and aluminum titanate-feldspar composite honeycomb ceramic articles can exhibit low coefficient of thermal expansion, relatively high porosity, low Young's modulus, and high strength for high performance automotive catalytic converters and diesel particulate filters. For example, as disclosed in U.S. Pat. No. 8,394,167, the contents of which are incorporated herein by reference in their entirety, cordierite-mullite-aluminum titanate (CMAT) composites are provided that exhibit improved strength compared to aluminum titanate-feldspar composites and better volumetric heat capacity compared to cordierite due to the phase assembly and microstructure of CMAT ceramic materials. The combination of these two advantages makes CMAT materials particularly suitable for applications requiring high porosity, such as in ceramic honeycomb filter bodies, such as TWC and SCR applications. The pseudobrookite structure phase in these CMAT composites can be stabilized by magnesium in solid solution, making it more thermodynamically stable than the aluminum titanate phase found in aluminum titanate feldspar (AT) composites, and better able to withstand thermal decomposition and accelerated decomposition at high temperatures when exposed to glass formers such as copper, manganese, cobalt, bismuth, etc. and their compounds. However, various embodiments herein provide various combinations of high porosity, relatively large median pore size, narrow pore size distribution, and relatively low CTE.

[0023] Exemplary ceramic body embodiments disclose cordierite, indialite, and pseudobrookite structures in compositional ranges that provide unexpectedly superior performance over prior art AT, cordierite, and cordierite-mullite-aluminum titanate (CMAT) materials. More specifically, the disclosure provides: relatively high average bulk volume porosity (e.g., %P≧50%); relatively narrow pore size distribution (e.g., df≦0.36, where df is (d 50 -d 10 ) / d 50a relatively high combined weight percentage (e.g., at least 85 wt.%) of crystalline phases including cordierite and indialite; and up to 10 wt.% of a crystalline pseudobrookite-structured phase (e.g., armalcolite).

[0024] In particular, the ceramic body comprises, expressed as weight percent on an oxide basis: 1 wt.% to 11 wt.% titania, and 89 wt.% to 99 wt.% MgO, Al2O3, and SiO2, where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4; or 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al2O3, and SiO2 (where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3). Contains:

[0025] definition Cordierite - (Mg,Fe)2Al3(Si5AlO 18 )~(Fe,Mg)2Al3(Si5AlO 18 Magnesium aluminum cyclosilicate having the series formula: Iron and nickel may be present in small amounts, i.e., less than 4% by weight. Cordierite crystals can be used to obtain very low thermal expansion along one axis.

[0026] A high-temperature polymorphic aluminosilicate phase that is the hexagonal dimorph of indialite-cordierite, which is isostructural with beryl, (Si,Al)O 18It has a random distribution of Al in the rings. It is compositionally similar to cordierite and has a negative thermal expansion along one crystallographic axis. The transformation of indialite to cordierite occurs slowly, and indialite is metastable below about 1250°C. Iron and nickel may be present in small amounts, i.e., less than 4 wt%.

[0027] Spinel - a hard, crystalline phase material occurring as octahedral crystals and composed of magnesium oxide and aluminum oxide.

[0028] Enstatite - MgSiO3 is an orthorhombic material of the pyroxene group consisting of magnesium silicate.

[0029] Rutile – A ceramic material composed primarily of titanium dioxide (TiO2).

[0030] Pseudobrookite structural phase - Tialite (Al2TiO5), pseudobrookite (Fe2TiO5), armalcolite (Mg,Fe 2+ )Ti2O5, and kaluiite (MgTi2O5).

[0031] Crystalbolite - a high temperature polymorph of silica, which means that it has the same chemical formula as quartz (SiO2) but a separate crystal structure.

[0032] Amorphous Phase - a glass containing primarily silica with lesser amounts of alumina, magnesia, titania, and oxide impurities of sodium, calcium, iron, and nickel.

[0033] Further embodiments of the present disclosure will now be described with reference to the tables and Figures 1A-5 disclosed and described herein. In some embodiments, the ceramic body 100 can be embodied as a honeycomb body as shown in Figures 1A and 1B. The ceramic body 100 embodied as a honeycomb body can comprise a matrix of interconnected porous walls 102 that form a honeycomb of a plurality of channels 104 extending along the axial length of the ceramic body 100 from a first end 103 (e.g., an inlet end) to a second end 105 (e.g., an outlet end). The channels 104 can be parallel to one another. The shape of the channels in cross-section, as outlined by the walls 102, can be square as shown in Figures 1A and 1B. However, alternatively, the cross-sectional channel shape can be rectangular (not square), triangular, octagonal, hexagonal, diamond, circular, other polygonal, combinations thereof, etc., and may have rounded corners, chamfered corners, square corners, or combinations thereof.

[0034] When configured as a honeycomb body, the ceramic body 100 can have a configuration having a lateral wall thickness, tw, of the walls 102 of between 0.002 inches and 0.016 inches (0.05 mm and 0.41 mm, see FIG. 1B), and even in some embodiments, between 0.004 and 0.012 inches (0.10 mm and 0.30 mm). Further, the interconnected porous walls 102 can have a generally constant thickness across the honeycomb body, or can have a varying thickness. For example, the wall thickness, tw, of the interconnected porous walls 102 can be greater near the skin 106 of the ceramic body 100, thereby providing a relatively thicker wall in the shape of a ring near the skin 106.

[0035] The ceramic body 100, when configured as the honeycomb body of FIG. 1A or the plugged honeycomb body of FIG. 1C, has a cell density of, for example, 15.5 cells / cm. 2 ~77.5 cells / cm 2(100 cpsi to 500 cpsi) average cell density. Other cell densities may be used. An exemplary geometry for the ceramic body 100 is 400 cpsi (62 cells / cm), defined herein as a 400 / 8 honeycomb body. 2 ) and a lateral wall thickness of about 8 mils (0.20 mm), or 400 cpsi (62 cells / cm), defined herein as a 400 / 6 honeycomb body. 2 (0.15 mm)。 Other geometries for the ceramic body 100 include, for example, average cell density / lateral wall thickness combinations of 100 / 17, 200 / 12, 200 / 19, 270 / 19, 300 / 8, 200 / 8, and 350 / 12. Other suitable combinations of cell density and lateral wall thickness may also be used.

[0036] In some honeycomb bodies, when the ceramic body 100 is embodied as a plugged ceramic honeycomb body 100P, certain of the channels 104 can be plugged. For example, as shown in FIG. 1C, a plugged ceramic honeycomb body 100P is shown that can be included in a particulate filter for diesel or gasoline engine applications. In the embodiment shown in FIG. 1C, some of the channels 104L can have a larger hydraulic area than other relatively small channels 104S, as described, for example, in U.S. Pat. Nos. 6,843,822; 6,696,132; 7,247,184; and 7,601,194. In other embodiments, the plugged ceramic honeycomb body 100P can include inlet and outlet channels of the same size, as described, for example, in U.S. Pat. Nos. 4,329,162; 6,849,181; 8512,433; and 8236,083. Other filter plugging patterns are possible, for example, as disclosed in U.S. Pat. Nos. 9,757,675; 8,673,064; 4,417,908; and 8,844,752.

[0037] The outermost cross-sectional shape of the ceramic body 100 (and plugged honeycomb body 100P) may be any desired outer cross-sectional shape, such as a circle (as shown in FIGS. 1A and 1C), an oval, an ellipse, a triangle or trilobe, a racetrack-shaped, square, or a rectangular cross-sectional profile. However, the honeycomb body 100 and plugged honeycomb bodies are not limited to these cross-sectional shapes. Other cross-sectional shapes may be used. As used herein, ceramic body 100 includes, but is not limited to, honeycomb bodies and plugged honeycomb bodies 100P.

[0038] Exemplary embodiments of the ceramic body 100 of the present disclosure can have a relatively high level of total bulk porosity, which is open and connected porosity. For example, a ceramic body 100 of the composition described herein can have an average bulk porosity %P, where %P≧50%, %P≧55%, %P≧60%, or even %P≧65%, as determined by mercury intrusion porosimetry. In some embodiments, the average bulk porosity %P can be 50%≦%P≦72%, 55%≦%P≦72%, 60%≦%P≦72%, or even 65%≦%P≦72%. Such a range of porosity for the ceramic body 100 of the present disclosure can provide low back pressure while providing sufficient overall strength and thermal shock resistance when used as a plugged honeycomb body 100P for particulate filters.

[0039] In addition to a relatively high total porosity, the ceramic body 100 of the present disclosure can also have a relatively narrow pore size distribution. This narrow pore size distribution can be evidenced by a minimal percentage of relatively fine pore sizes or relatively large pore sizes, or in some embodiments, a minimal percentage of both relatively fine pore sizes and relatively large pore sizes. Such a narrow pore size distribution has the advantage of providing low back pressure, even when coated with a catalyst-containing washcoat. Furthermore, a narrow pore size distribution can be beneficial to provide low soot load pressure drop and excellent soot capture efficiency when the ceramic body 100 is utilized in diesel and / or gas engine exhaust gas filtration applications.

[0040] For this purpose, the relative pore size distribution is determined by mercury intrusion porosimetry using the Washburn equation. For example, the quantity d 50 represents the median pore size (MPS) based on the pore volume (measured in micrometers). Thus, d 50 is the pore diameter at which mercury penetrates 50% of the open porosity of the ceramic body 100. 90 is 90% of the pore volume is d 90 The pore diameter is composed of pores having a diameter smaller than the value of d 90is also equal to the pore diameter at which mercury penetrates 10% by volume of the open porosity of the ceramic. 10 is 10% of the pore volume d 10 The pore diameter is composed of pores having a diameter smaller than the value of d 10 is equal to the pore diameter at which mercury penetrates 90% by volume of the open porosity of the ceramic. d 10 and d 90 The value is also expressed in micrometers.

[0041] d 50 According to certain aspects of the present disclosure, the porous walls 102 of the fired ceramic body 100 have a thickness of d 50 ≧10.0μm, d 50 ≧12.0μm, d 50 ≧13.0μm, d 50 ≧15.0 μm, and in some embodiments, 50 Pore ​​median diameter (d 50 Furthermore, the porous walls 102 of the fired ceramic body 100 may have a pore size within the range of 7 μm≦d50≦20 μm, 10 μm≦d 50 ≦20μm, 12μm≦d 50 ≦20 μm, and even in some embodiments ≦15 μm 50 Pore ​​median diameter (d 50 ).

[0042] df The relatively small pore fraction (d 50 The narrowness of the gap (df) can be characterized by the d factor (df), where df = {(d 50 -d 10 ) / d 50}. In exemplary embodiments of the ceramic body 100, df may be df≦0.36, df≦0.32; df≦0.30, df≦0.25, or even df≦0.22. Ultra-narrow pore size distribution embodiments described herein may exhibit d-factors where df≦0.20, df≦0.18, or even df≦0.17. In some embodiments, the porous walls 102 of the fired ceramic body 100 may have df where 0.16≦df≦0.32, 0.16≦df≦0.30, 0.16≦df≦0.25, 0.16≦df≦0.22, or even 0.16≦df≦0.20.

[0043] dB The relatively large pore fraction (d 10 From d 90 A relative measure of narrowness, including the narrowness of the pore size distribution (dB) of the open connected porosity of the ceramic body 100, can be characterized by the d-width (dB) of the pore size distribution of the open connected porosity of the ceramic body 100. For example, the d-width (dB) of the pore size distribution of the open connected porosity of the ceramic body 100 can be dB≦1.1, dB≦0.85, dB≦0.80, dB≦0.70, or even in some embodiments dB≦0.60, where dB={d 90 -d 10 ) / d 50 In some embodiments, the porous walls 102 of the fired ceramic body 100 can have a dB that is 0.45≦dB≦1.1, 0.45≦dB≦0.85, 0.45≦dB≦0.70, 0.45≦dB≦0.60, or even 0.45≦dB≦0.55.

[0044] CTE It has been discovered that the coefficient of thermal expansion (CTE) of the ceramic body 100, including the ceramic, is extremely low. According to an exemplary embodiment, it has been discovered that the ceramic material of the present invention exhibits a low coefficient of thermal expansion, which results in excellent thermal shock resistance (TSR). As will be appreciated by those skilled in the art, TSR is inversely proportional to the coefficient of thermal expansion (CTE). That is, a ceramic body 100 with a low coefficient of thermal expansion can also have a relatively high thermal shock resistance, and therefore can withstand the wide temperature fluctuations encountered in engine exhaust gas filtration applications.

[0045] Thus, in an exemplary embodiment, the ceramic body 100 of the present disclosure, including the ceramic phases described herein, can exhibit a relatively low coefficient of thermal expansion (CTE) in at least one direction, as measured by dilamptry. In particular, CTE≦14×10 -7 / ℃, CTE≦12×10 -7 / ℃, CTE≦10×10 -7 / ℃, and CTE≦9×10 -7 / °C, all measured over a temperature range of 25°C to 800°C. In some embodiments, the CTE over the temperature range of 25°C to 800°C is 7×10 -7 / ℃≦CTE≦14×10 -7 / ℃;7×10 -7 / ℃≦CTE≦12×10 -7 / ℃; and even 7×10 -7 / ℃≦CTE≦10×10 -7 In a further embodiment, the CTE over the temperature range of 25° C. to 800° C. can be 3×10 -7 / ℃≦CTE≦14×10 -7 / ℃, 3×10 -7 / ℃≦CTE≦12×10 -7 / ℃, and even 3×10 -7 / ℃≦CTE≦10×10 -7 / °C. The ceramic body 100 may have a microcrack index Nb of 0.10 or greater. 3In some embodiments, the microcrack index Nb 3 is 0.10≦Nb 3 It may be ≦0.43.

[0046] combination The average bulk porosity (%P), median pore diameter (d 50 ), low df and / or low dB, and low CTE (RT~800°C) can provide low clean and soot load pressure drops while maintaining useful filtration efficiency and improved thermal shock resistance when the ceramic body 100 of the present disclosure is used in diesel or gasoline exhaust filtration applications.

[0047] Particularly effective examples of ceramic bodies 100 can include the ceramic compositions described herein and further include an average bulk porosity (%P) of the interconnected porous walls 102, where P%≧50%, d 50 The median pore diameter (d 50 ) (where d 50 is the pore median diameter), df≦0.36 (where df={(d 50 -d 10 ) / d 50}), and CTE≦14×10 when measured at room temperature (25°C to 800°C) -7 In some embodiments, the ceramic body 100 can include a ceramic composition described herein and further have an average bulk porosity (%P) of the interconnected porous walls 102 that is 50%≦P%≦72%, 7.0 μm≦d 50 The median pore diameter (d 50 ), 0.16≦df≦0.36, and 3×10 -7 / K≦CTE≦14×10 -7 / °C.

[0048] Certain other exemplary embodiments of the present disclosure may include the ceramic compositions described herein and further include: 55%≦%P≦72%; 8 μm≦d 50≦20μm; 0.16≦df≦0.32; and 3×10 when measured at 25℃~800℃ -7 / ℃≦CTE≦14×10 -7 / °C. Additionally, certain other exemplary embodiments can achieve: 60%≦%P≦72%; 10 μm≦d 50 ≦20μm; 0.16≦df≦0.25; and 3×10 when measured at 25℃~800℃ -7 / ℃≦CTE≦13×10 -7 / ℃ can be achieved.

[0049] Of note, some exemplary embodiments are: 60%≦%P≦72%; 12 μm≦d 50 ≦20μm; 0.16≦df≦0.20; and 3×10 when measured at 25℃~800℃ -7 / ℃≦CTE≦12×10 -7 / °C. Further exemplary embodiments are: 60%≦%P≦72%; 13 μm≦d 50 ≦20μm; 0.16≦df≦0.18; and 3×10 when measured at 25℃~800℃ -7 / ℃≦CTE≦12×10 -7 / ° C. Such properties are extremely useful for use in particulate filter applications.

[0050] As previously outlined, exemplary embodiments of the present disclosure provide a ceramic body 100 that includes a ceramic composite containing a primary crystalline phase consisting of a combination of cordierite and indialite and a secondary crystalline phase comprising a solid solution with a pseudobrookite structure phase. In particular, ceramic body 100 includes at least 85% by weight of a composite crystalline phase containing cordierite and indialite and up to 10% by weight of a secondary crystalline phase comprising a solid solution pseudobrookite structure phase. Other phases may also be present.

[0051] The cordierite and indialite crystalline phases together (when added together) can be 85% to 92% by weight based on 100% by weight of the minerals present. For example, in one or more embodiments, the cordierite crystalline phase can be 53% to 78% by weight based on 100% by weight of the minerals present. The indialite crystalline phase can be 15% to 35% by weight based on 100% by weight of the minerals present. In some embodiments, the pseudobrookite structured phase in the ceramic body 100 can be 2% to 8% by weight based on 100% by weight of the minerals present. The pseudobrookite structured phase can include an armalcolite crystalline phase.

[0052] Additionally, the ceramic body 100 may include an additional mullite crystalline phase, which may be between 1.5% and 3% by weight based on 100% by weight of the minerals present. The ceramic body 100 should be substantially free of rutile crystalline phase. For example, the rutile crystalline phase may be in an amount of less than 1.0% by weight based on 100% by weight of the minerals present in the ceramic body 100. Some embodiments may include enstatite or cristobalite crystalline phases, such as in an amount of less than 2.0% by weight based on 100% by weight of the minerals present. In some embodiments, the ceramic body 100 may include less than 7% by weight of an amorphous phase based on 100% by weight of the minerals present.

[0053] The weight percentages described herein, and the identification of the various phases present, were arrived at by the Rietveld technique and are expressed as a percentage of the total weight of minerals present in the ceramic body 100, 100% by weight.

[0054] Additionally, the ceramic body 100 comprises, expressed as weight percent on an oxide basis: 1 wt. % to 11 wt. % titania, and 90 wt. % to 99 wt. % MgO (magnesium oxide), Al2O3 (alumina), and SiO2 (silica) combined, as best illustrated in region 340 of FIG. 3 (wherein the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4); or 2.5 wt% to 11 wt% titania, and 89 wt% to 97.5 wt% total MgO (magnesium oxide), Al2O3 (alumina), and SiO2 (silica) as best illustrated in region 342 of FIG. 3 (where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3). As shown and described, these relative weight ratios (MgO:Al2O3:SiO2) add up to 100%.

[0055] In another embodiment, the ceramic body 100 includes 2% to 6% titania by weight, and 94% to 98% by weight MgO, Al2O3, and SiO2 (wherein the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 14.3:34.9:50.8; 13.3:34.9:51.8; 14.3:32.3:53.4; and 15.3:32.3:52.4).

[0056] Thus, in terms of oxide concentration, ceramic body 100 can include 1% to 11% titania by weight in embodiments having an MgO:Al2O3:SiO2 oxide ratio within the edge boundary of region 340, and 2.5% to 11% titania in embodiments having an MgO:Al2O3:SiO2 oxide ratio within the edge boundary of region 342.

[0057] The ceramic body 100 can further have an oxide concentration of titania (TiO2) of 1 wt% to 6 wt% based on 100 wt% total inorganic oxides present in the ceramic body 100, in some embodiments. In other embodiments, the ceramic body 100 can further have an oxide concentration of titania (TiO2) of 2 wt% to 6 wt%. Further, in terms of weight percent of oxides, the ceramic body 100 can have an oxide concentration of magnesia (MgO) of 12 wt% to 17 wt%, or even 12.5 wt% to 14 wt%, in some embodiments, based on 100 wt% total inorganic oxides present in the ceramic body 100.

[0058] It should be appreciated that the presence of titania along with the cordierite and indialite phases provides a relatively high porosity (%P) and narrow pore size distribution as well as a low CTE. Without being bound by theory, it is believed that the function of titania is to generate a stable liquid during reactive sintering that migrates in response to capillary forces to fill undesirable fine pores. This allows for a narrower pore size distribution than nominally stoichiometric cordierite. Thus, particulate filters utilizing the ceramic body 100 embodied as a plugged honeycomb body 100P can have excellent permeability, washcoat compatibility, and filtration efficiency.

[0059] Exemplary embodiments of the ceramic body 100 of the present disclosure may have an E of 4.5 GPa or less, where E is the Young's modulus of the ceramic body 100 at room temperature (RT) in GPa. In other exemplary embodiments, the ceramic body 100 can have an E of 2.0 GPa or less, or even 1.5 GPa or less. In some embodiments, E can be between 1.33 GPa and 4.5 GPa, or even between 1.33 GPa and 1.5 GPa, or even between 1.33 GPa and 2.0 GPa.

[0060] According to exemplary embodiments of the present disclosure, the ceramic body 100 exhibits a favorable crystallographic texture of the cordierite phase, which can be quantified by an i-ratio calculated from the (110) and (200) surface x-ray diffraction (XRD) peak intensities. For the axial i-ratio, the XRD peak intensities were measured perpendicular to the wall 102 of the ceramic body 100. For the lateral i-ratio, the XRD peak intensities were measured on the wall surface or on a slightly polished honeycomb wall surface. Rietveld deconvolution can be used to extract the cordierite peak intensities from the overlapping peak contributions of other phases present. In exemplary embodiments of the present disclosure, the cordierite phase of the ceramic body exhibits an axial i-ratio of 0.43 to 0.59 and a lateral i-ratio of 0.80 to 0.88. In some embodiments, the axial i-ratio can be less than 0.55 or even less than 0.5.

[0061] Extrusion Molding Method Exemplary embodiments of the present disclosure also provide a method for producing a cordierite-indialite-pseudobrookite composite ceramic body from inorganic powder raw materials, organic powder materials, a liquid vehicle (e.g., water), and processing aids. The method comprises the steps of: 50 and dB) and weight percentages (wt %) of magnesia, alumina, silica, and titania. The inorganic batch composition mixture can then be mixed and / or kneaded with the organic powdered materials, such as organic binders, pore formers, the liquid vehicle, and one or more processing aids selected from the group consisting of plasticizers and lubricants, to form a plasticized batch composition mixture 210. The plasticized ceramic precursor batch composition mixture 210 can be molded or otherwise shaped into a green body 100G (see FIG. 2), such as a honeycomb green body. The green body 100G can then be dried and then fired under conditions effective to convert the green body 100G into a ceramic body 100 having the cordierite-indialite-pseudobrookite composite crystalline composition described above.

[0062] For example, the plasticized batch composition can be formed into a green body 100G by an extrusion process. For example, FIG. 2 shows a side cross-sectional view of an exemplary embodiment of an extruder 200 (e.g., a continuous twin screw extruder). The extruder 200 includes a barrel 212, which includes a chamber 214 formed therein. The barrel 212 can be monolithic or can be formed of multiple barrel segments connected in series in a longitudinal direction 215 (e.g., in the direction indicated by the arrow). The chamber 214 extends longitudinally 215 through the barrel 212 between an upstream side 215U and a downstream side 215D. The upstream side 215U of the barrel 212 can include a material feed port 216, which can include a hopper or other material feed structure, for feeding the batch composition mixture 210 to the extruder 200. A cartridge assembly 217 including a honeycomb extrusion die 218 is provided downstream 215D for extruding the batch mixture 210 into a desired shape, such as a green honeycomb body 100G. Other structures, such as a generally open cavity, a screen 220, a homogenizer 222, etc., may be present prior to the honeycomb extrusion die 218 to facilitate the formation of a stable plug-type flow front before the plasticized batch composition mixture 210 reaches the honeycomb extrusion die 218.

[0063] As further shown in FIG. 2, a pair of extrusion screws 224 may be rotatably mounted within the barrel 212. The screws 224 may be disposed generally parallel to one another as shown, but may optionally be disposed at various angles to one another. The screws 224 may also be coupled to a drive mechanism 220 located outside the barrel 212 for rotation of the screws 224 in the same or different directions. It should be understood that both screws 224 may be coupled to a single drive mechanism 220 as shown, or to independent drive mechanisms (not shown). The screws 224 operate to move the batch composition mixture 210 in a longitudinal direction 215 through the chamber 214 by pumping and further mixing action. Additional support structures may be provided to support the screws 224 at their ends and / or along their length. Such support structures may include perforations or holes therein through which the batch composition mixture 210 may flow.

[0064] 2 further illustrates an extruder 200 with a green body 100G being extruded therefrom. The extruder cartridge 217 may include extrusion hardware such as a honeycomb extrusion die 218 and a skin forming mask 226. The green body 100G is extruded from the extruder 200, and in some embodiments, a skin 106 is also formed along and surrounding the multiple walls 102 during extrusion. The honeycomb body 100G is then cut to length by a cutting element 228 and provided on a tray 230. The tray 230 may be as described, for example, in U.S. Pat. Nos. 9,440,373; 9,085,089; and 8,407,915.

[0065] Cutting can be accomplished by wire cutting, saw cutting with a band saw or reciprocating saw, or other cutting methods. The tray 232 can be fed into a dryer, such as those described in U.S. Pat. Nos. 9,038,284, 9,335,093, 7,596,885, and 6,259,078. Any suitable drying method can be used, such as RF drying, microwave drying, oven drying, or combinations thereof. In some embodiments, the green honeycomb body 100G can be cut, such as after drying, from a log from which a plurality of honeycomb bodies are provided.

[0066] After drying, the green body 100G can be fired under conditions effective to convert the green honeycomb body to a ceramic body 100 comprising cordierite, indialite, and pseudobrookite, as well as other crystalline phases.

[0067] Batch Composition The batch composition mixture may include: inorganic components including a magnesia source, an alumina source, a silica source, and a titania source; a pore-forming agent (e.g., starch and / or graphite), which may further have the particle size and particle size distribution, and width (dBp), as set forth in Table 1 below.

[0068] [Table 1]

[0069] To this end, when referred to herein, all particle sizes are measured by laser diffraction techniques and a Microtrac particle size analyzer, with the exception of dispersible alumina (AlOH), the properties of which were defined by the supplier.

[0070] Magnesia Source For example, the magnesia source can be any suitable compound capable of providing an oxide of magnesium useful in forming the cordierite-indialite-pseudobrookite structured crystalline phase composition, by way of example and not limitation. For example, the magnesia source can be selected as a talc source, or magnesium hydroxide, or a combination thereof. For example, the talc source can be calcined or uncalcined talc. Optionally, the magnesia source can be one or more of MgO, Mg(OH)2, MgCO3, MgAl2O4, Mg2SiO4, MgSiO3, MgTiO3, Mg2TiO4, MgTi2O5. Alternatively, the magnesia source can be one or more of forsterite, olivine, chlorite, and serpentine. When the magnesia source is talc, it has a particle median diameter (d p50 ) and dB p ≦2.2, where dB p is the width factor, (d p90 -d p10 ) / d p50 The magnesia source may comprise 25% to 40% by weight based on 100% of the total weight of the minerals present in the batch composition mixture 210.

[0071] Alumina Source The alumina source can be any suitable compound capable of providing an oxide of aluminum useful in forming the cordierite-indialite-pseudobrookite structured crystalline phase composition, for example and not by way of limitation. The alumina source can be selected from alumina-forming sources such as corundum, aluminum hydroxide (or alumina hydroxide) such as Al(OH), dispersible aluminas such as boehmite capable of forming colloidal suspensions, diaspore, or transition aluminas such as gamma alumina or p-alumina. Alternatively, the alumina source can be a compound of aluminum and another metal oxide, such as MgAl2O4, Al2TiO5, mullite, kaolin, calcined kaolin, pyrophyllite, kyanite, chlorite, and the like. In some embodiments, the median particle size (d p50The alumina source may comprise 25% to 40% by weight based on 100% of the total weight of the inorganics present in the batch composition mixture 210.

[0072] Silica Source The silica source can be any suitable compound capable of providing an oxide of silica useful in forming the cordierite-indialite-pseudobrookite structured crystalline phase composition, for example and not by way of limitation. The silica source can be selected from silica sources such as SiO2 powders, such as quartz, cryptocrystalline quartz, fused silica, diatomaceous silica, low alkali zeolites, colloidal silica, or combinations thereof. Additionally, the silica source can be provided as a compound with magnesium and / or aluminum, including, for example, talc, cordierite, chlorite, kaolin, kyanite, and the like. In an embodiment, the median particle size (d 50 The silica source may comprise 15% to 30% by weight based on 100% of the total weight of the minerals present in the batch composition mixture 210.

[0073] Titania Source The titania source can be provided as TiO2 powder. The median particle size (d p50 ) and / or particle size distribution. For example, the titania source may have a median particle size of 0.25 μm to 0.45 μm. Further, the titania source may have a width factor dB p ≦2.0 and even dB p ≦1.5 (where dB p =(d p90 -d p10 ) / d p50 The particle size distribution may be

[0074] Porosifier To achieve a relatively high average bulk porosity (%P≧50%), the batch composition mixture 210 can contain a pore former to help tailor the average bulk porosity and possibly the pore size distribution of the ceramic body 100. The pore former is a fugitive material that is used to control the desired coarse pore median diameter (d 50 ) is evaporated or vaporized during drying and / or heating of the green body 100G to obtain the desired high bulk porosity. Suitable pore formers include, but are not limited to: carbon; graphite; starch; wood, husk, or nut powders; polymers such as polyethylene beads, and the like; and combinations thereof. Starches include corn starch, rice starch, pea starch, sago starch, potato starch, and the like. Other suitable pore formers may also be used. When using certain pore formers, such as potato starch, the relatively coarse (e.g., d p50 Utilizing a talc, alumina, and / or silica source (which has a higher df) can reduce df.

[0075] Relatively high porosity and relatively large d 50 Exemplary embodiments that help provide a useful combination with can include a combination of starch and graphite. For example, the pore-forming agent can include pea starch, alone or in combination with graphite, or corn starch, alone or in combination with graphite. The pore-forming agent can be present in an amount of about 25% by weight add-on (SA) based on 100% by weight of the minerals present in the batch composition mixture 210. pf ) ~ approx. 57% SA by weight pf 20% SA by weight based on 100% by weight of inorganics present in the batch composition mixture 210. pf ~Approx. 47%SA by weight pf of starch and 20% SA by weight pf ~Approx. 47%SA by weight pf The embodiments including the combination of graphite and SiO2 have high average bulk porosity and median pore size (d 50The amount of the pore former is w i ×Weight%SA pf / 100, where w i is the total weight of inorganic raw materials.

[0076] Starch has a particle median diameter (d) of about 5 μm to 50 μm, and in other embodiments, about 8 μm to 30 μm. p50 The graphite may have a median particle diameter (d) of about 5 μm to 50 μm in some embodiments. p50 ).

[0077] Organic Binder The batch composition mixture 210 may include an organic binder. The organic binder may be, for example, a cellulose ether binder, such as a hydrophobically modified cellulose ether binder. In some embodiments, the hydrophobically modified cellulose ether binder may be, but is not limited to, methylcellulose, ethyl hydroxyethyl cellulose, hydroxybutyl methylcellulose, hydroxymethylcellulose, hydroxypropyl methylcellulose, hydroxyethyl methylcellulose, hydroxybutyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, sodium carboxymethylcellulose, combinations thereof, and the like. Methylcellulose and / or methylcellulose derivatives are particularly suitable as organic binders for use in the batch composition mixture 210, with methylcellulose and hydroxypropyl methylcellulose being excellent choices. The source of the cellulose ether is METHOCEL™ cellulose products available from DOW Chemical Co.

[0078] Some embodiments of the batch compositions, such as those disclosed in Tables 2A-2E below, may include methylcellulose (methylcellulose 1) and hydroxypropyl methylcellulose (methylcellulose 2). Other combinations of cellulose ether binders may include cellulose ethers with different molecular weights. Alternatively, the combinations of cellulose ethers may include cellulose ethers with different hydrophobic groups or different concentrations of the same hydrophobic group, or combinations of other cellulose ethers. The different hydrophobic groups may be, as non-limiting examples, hydroxyethyl or hydroxypropyl. In some embodiments, the organic binder may be a combination of hydroxyethyl methylcellulose binder and hydroxypropyl methylcellulose binder. Other suitable combinations of organic binders may be used.

[0079] The organic binder may be provided in the batch composition in an amount between about 2.0 wt. % SAP and 8.0 wt. % SAP, and even between about 3.0 wt. % SAP and about 5.0 wt. % SAP, where SAP is based on an add-on to 100% total weight of the inorganics and pore-forming agents present in the batch composition mixture 210.

[0080] Liquid Vehicle In one or more embodiments, the batch composition mixture 210 includes a liquid vehicle, which can be provided at a liquid vehicle percentage, LV%, as an addition to 100% by weight of the inorganic matter and pore-forming agent present in the batch. The LV% in the batch composition mixture 210 can be added to the batch composition mixture in an amount of about 15% by weight≦LV%≦50% by weight, by addition to 100% by weight of the total inorganic matter and pore-forming agent present in the batch composition mixture 210.

[0081] In use, the liquid vehicle provides a medium for dissolving the organic binder, thus providing plasticity to the batch composition mixture 210, and providing wetting of the inorganic particles therein. The liquid vehicle can be a water-based liquid, such as water or a water-miscible solvent. In one implementation, the liquid vehicle is water, such as deionized water, although other solvents, such as alcohols (e.g., methanol or ethanol), may also be used alone or in combination with water.

[0082] Processing Aids Additionally, the batch composition mixture 210 may include other processing aids, such as plasticizers, surfactants, and / or oil-based lubricants. Non-limiting examples of surfactants that may be used as processing aids include C8-C 22 Further surfactant compositions that may be used with these fatty acids include C8-C 22 Aliphatic esters, C8-C 22 and fatty alcohols, and combinations thereof. Exemplary surfactants are: stearic acid, lauric acid, myristic acid, oleic acid, linoleic acid, and palmitic acid and derivatives thereof; tall oil; stearic acid in combination with ammonium lauryl sulfate; and combinations of all of the above. In an exemplary embodiment, the surfactant is lauric acid, stearic acid, oleic acid, tall oil, or combinations thereof. In some embodiments, the amount of surfactant can be from about 0.25% SA by weight to about 2% SA by weight, and in the illustrated embodiment, from about 0.5% SA by weight to 1.5% SA by weight.

[0083] Non-limiting examples of oil-based lubricants that can be used as processing aids include light mineral oil, corn oil, high molecular weight polybutene, polyol esters, blends of light mineral oil with wax emulsions, blends of paraffin wax in corn oil, or combinations of these with olefins. In some embodiments, the amount of oil-based lubricant can be from about 0 wt% SA to about 10 wt% SA. In some exemplary embodiments, the oil-based lubricant can be present up to about 2 wt% SA. In some embodiments, no lubricant is used.

[0084] The inorganic batch powder ingredients, organic binders, and pore formers can be thoroughly blended with a liquid vehicle and one or more processing aids to provide the plasticized batch composition mixture with plastic formability and green strength when formed into a green body 100G. When forming is performed by extrusion, most typically, cellulose ether binders such as methyl cellulose, hydroxypropyl methyl cellulose, and / or combinations thereof function as temporary organic binders. Tall oil can function as a suitable processing aid. The inorganic batch ingredients, organic binders, and pore formers are typically mixed in dry form and then mixed with a liquid vehicle (e.g., water) and one or more processing aids. The amount of liquid vehicle (e.g., water) can vary from batch composition mixture to batch composition mixture, and is determined by pre-testing a particular batch composition mixture for extrudability and adjusting the LV% of the liquid vehicle, if necessary, to achieve the appropriate plasticity for extrusion and optimal handling properties.

[0085] In addition to forming and shaping the green body 100G from the plasticized batch composition mixture by extrusion, other suitable forming methods may be used. For example, uniaxial or isostatic pressing, casting, and injection molding may be used to form the green body 100G. For example, extrusion may be used when the ceramic body 100 is embodied as a honeycomb body, such as a pass-through substrate (e.g., catalyst substrate) for a catalytic converter, or a plugged honeycomb body for use in particulate wall-flow filter applications. The resulting green body 100G may be dried and then fired in a furnace, such as a gas kiln or electric kiln, under conditions effective to convert the green body 100G into the ceramic body 100. After firing, the ceramic body 100 may be plugged as described herein to form a plugged ceramic body 100P.

[0086] Firing In one or more embodiments, firing conditions effective to convert the green body 100G to the ceramic body 100 can include heating the green body 100G to a maximum soak temperature of 1,350°C to 1,410°C, followed by holding the maximum soak temperature for a soak time sufficient to produce a cordierite-indialite-pseudobrookite crystalline phase composite structure. In some embodiments, the maximum soak temperature can be 1,360°C to 1,400°C or 1,380 to 1,395°C. The maximum soak temperature is maintained for a soak time sufficient to convert the green body 100G to a ceramic body 100 having a cordierite-indialite-pseudobrookite crystalline phase composite structure. The soak time can be, for example, about 6 hours to about 24 hours. The soak time is followed by cooling at a rate slow enough to avoid thermal shock to the ceramic body 100.

[0087] Plugging To obtain a plugged honeycomb body 100P for use in wall-flow particulate filter applications, a portion of the cells of the ceramic honeycomb body 100 at the inlet end and / or face can be plugged as known in the art. This plugging can be done at the ends of the channels 104 and can be about 3 mm to 20 mm deep, although this depth can vary. In some embodiments, a portion of the channel 104 is plugged at the outlet end 105 but not at the inlet end 103 (e.g., the inlet channel), and another portion of the channel 104 is plugged at the inlet end 103 but not at the outlet end 105 (e.g., the outlet channel). Thus, each channel 104 is plugged only at one end of a fully plugged embodiment. In some embodiments, a plugging configuration can be provided such that every other channel 104 on a given face is plugged in a checkerboard pattern. However, other plugging patterns are possible and not all channels 104 may include plugging. Some channels 104 may not include plugging, i.e., they may be unplugged through channels. Suitable, non-limiting plugging materials and plugging processes are described, for example, in U.S. Patent Nos. 4,329,162; 4,557,773; 6,673,300; 7,744,669; and 7,922,951. Other suitable plugging methods, patterns, and types of plugging may also be used.

[0088] Exemplary Batch Composition Mixtures Exemplary embodiments of the present disclosure will now be further described with respect to certain batch composition mixtures, which are merely illustrative and not intended to be limiting. Tables 2A-2E below provide several examples (E1-E27) of batch composition mixtures 210 useful in forming a ceramic body 100 comprising a cordierite-indialite-pseudobrookite structured composite ceramic. In particular, exemplary batch mixtures 210 according to embodiments described herein can include inorganic components including a magnesia source, an alumina source, a silica source, and a titania source, which can be powdered particulate source materials, and the like. The magnesia source may be provided in the batch composition mixture in an amount of 20% to 42% by weight; the alumina source may be provided in an amount of 25% to 40% by weight; the silica source may be provided in an amount of 15% to 30% by weight; and the titania source may be provided in an amount of 1% to 10% by weight, where the weight percentages of each of the magnesia source, alumina source, silica source, and titania source are all based on 100% of the total weight of the inorganics present in the batch composition mixture 210, i.e., each inorganic component is added to 100%.

[0089] When the magnesia source is a talc source provided to the batch composition mixture as a powdered particulate talc material, it can be provided, for example, according to one of the talc particle size distributions and materials shown in Table 1. The alumina source can be any suitable source of alumina and / or aluminum hydroxide, such as calcined alumina, hydrated alumina, or even derived from clays such as kaolin clay. Other types of clays such as halloysite or attapulgite may also be used. In some embodiments, the alumina source can include: 11% to 33% by weight of calcined alumina particulate material; and 0% to 16% by weight of hydrated alumina, each based on 100% of the total weight of the minerals in the batch composition mixture 210.

[0090] The silica source can be derived from particulate silica, clay such as kaolin clay, or talc, or a combination thereof. The titania source can be any source of particulate titania (TiO2) as described above.

[0091] The batch composition mixture further comprises 26 wt.% SA pf ~56wt%SA pf , and further 35% by weight SA pf ~56wt%SA pf where wt% SA is the weight percent of the addition based on 100% total weight of the inorganics in the batch composition mixture 210. In some embodiments, the pore-forming agent is 44 wt% SA pf ~56wt%SA pf In a further embodiment, the pore-forming agent is 44 wt.% SA pf ~51wt%SA pf Exemplary pea starches may include pea starches having a median particle size (d 50 ) and particle size distribution.

[0092] In some embodiments, the pore-forming agent comprises starch alone or a combination of starch and graphite. For example, the pore-forming agent comprises 44 wt.% SA pf ~46wt%SA pf of pea starch, and 9% by weight SA pf ~11wt%SA pf of graphite, where wt.% SA pf is the weight percent of the addition based on 100% total weight of the inorganics in the batch composition mixture 210.

[0093] [Table 2A]

[0094] [Table 2B]

[0095] [Table 2C]

[0096] [Table 2D]

[0097] [Table 2E]

[0098] Tables 3A-3G below provide the nominal oxide chemistry, processing details, microstructural geometry and properties, and various phase compositions as phase fractions in weight percent (wt%) of exemplary fired ceramic bodies E1A-E28 produced from batch composition mixture 210 utilizing the raw materials in Table 1 and the batch composition mixtures defined in Tables 2A-2E.

[0099] Examples E1A-E28 in Tables 3A-3G, which correspond to E1-E28 in Tables 2A-2E, respectively have axial lengths of about 200 mm to 305 mm, nominal diameters of 54 mm in transverse cross section, and cell densities of 46.6 cells / cm 2 The honeycomb bodies 100G were obtained by extruding the honeycomb bodies 100G having a wall thickness of 0.20 mm to 0.23 mm. The honeycomb bodies 100G were made from various batch materials listed in Tables 2A to 2E and then fired in an electric furnace at the firing conditions listed. The maximum soaking temperature (°C) and soaking time in hours (hr) are shown.

[0100] Figure 1 shows the calculated oxide weight percentages for various sources. Figure 2 shows the phase fractions of various phases present in the cordierite-indialite-pseudobrookite (CID) composite ceramics. For example, E2 contains cordierite, indialite, spinel, enstatite, armalcolite as pseudobrookite structure, rutile, and amorphous phase. Phase fractions of all examples E1A-E28 were determined by Rietveld method and X-ray diffraction.

[0101] [Table 3A]

[0102] [Table 3B]

[0103] [Table 3C]

[0104] [Table 3D]

[0105] [Table 3E]

[0106] [Table 3F]

[0107] [Table 3G]

[0108] The pore size distribution of the ceramic body 100 was investigated by mercury intrusion porosimetry using an Autopore® IV 9520 porosimeter. In this measurement system, pressure is increased such that mercury invades the relatively narrow pore channels and fills the increased pore volume until a critical pressure is reached at which mercury spreads throughout the specimen.

[0109] Thermal expansion was measured on bar specimens with dimensions of approximately 0.25 in. x 0.25 in. x 2 in. (0.64 x 0.64 x 5.1 cm) after heating from room temperature to 1,000°C at a rate of 4°C / min and then cooling to room temperature (RT). For the reported data, the thermal expansion was provided in the axial direction of the honeycomb body 100 by orienting the long axis of the test bars in the direction of the honeycomb channels 104. The average coefficient of thermal expansion from room temperature (RT) to 800°C is defined as L(800°C)-L(25°C) / 775°C.

[0110] The elastic modulus (E) was measured by bending resonance frequency using bar-shaped specimens with dimensions 5 in. x 1 in. x 0.5 in. (12.7 x 2.54 x 1.27 cm) and long axis oriented in the direction of the honeycomb channels 104. The specimens were heated to 1200°C and cooled again to room temperature. For each temperature, the elastic modulus was derived directly from the resonance frequency by reference to ASTM C 1198-01 and normalized for specimen geometry and weight.

[0111] 4A-4C show scanning electron microscope (SEM) photographs of polished fired products of Examples E9, E7C, and E18, showing a close-up view of the phase distribution, with the cordierite and indialite phases in dark grey, the pores in black, and the pseudobrookite structure phase in light grey. The phases present in the ceramic body 100 were identified by X-ray diffraction (XRD). A Phillips X'Pert diffraction system equipped with an X'Celerator high speed detector was utilized. High resolution spectra were typically acquired from 15° to 100° (2θ). The Rietveld method was used to quantitate the percentage of phases.

[0112] 5 illustrates a method of making the ceramic body 100. The method 500 includes, at 502, providing inorganic components including 20% ​​to 42% by weight of a magnesia source, 25% to 40% by weight of an alumina source, 15% to 30% by weight of a silica source, and 1% to 10% by weight of a titania source, where the weight percentages of each of the magnesia source, alumina source, silica source, and titania source are based on 100% total weight of the minerals present.

[0113] The method 500 further comprises, at 504, mixing the inorganic components with an organic binder, 26 wt. % SA pf ~56wt%SA pf and a liquid vehicle to form a batch composition mixture, wherein wt. % SA pf is the weight percent of the addition based on 100% total weight of the inorganic material.

[0114] The manufacturing method 500 further includes, at 506, forming the batch composition mixture into a green body (e.g., green body 100G), and, at 508, drying the green body 100G as described herein. Forming the batch composition mixture 210 into a green body 100G may include extruding the batch composition mixture 210 through an extrusion die 218 to form a green honeycomb body. Optionally, the forming may be by any other suitable method.

[0115] The method 500 further includes, at 510, firing the green body under conditions effective to convert the green body to a ceramic body (e.g., ceramic body 100) comprising a crystalline phase containing cordierite and indialite with a combined weight percentage of at least 85% by weight and a crystalline pseudobrookite-structured phase of up to 10% by weight. The crystalline phase comprising the pseudobrookite-structured phase can include armalcolite in some embodiments. However, other pseudobrookite-structured phases can be provided. In some embodiments, the firing conditions effective to convert the green body (e.g., green body 100G) to ceramic body 100 include heating green body 100G to a soak temperature of between 1350° C. and 1410° C. and maintaining the soak temperature for a soak time sufficient to convert green body 100G to ceramic body 100.

[0116] It will be apparent to those skilled in the art that various modifications and variations can be made to the various embodiments disclosed herein without departing from the scope of the present disclosure, and therefore, the present disclosure is intended to cover the modifications and variations of the disclosed embodiments, provided they come within the scope of the appended claims and their equivalents.

[0117] Preferred embodiments of the present invention will be described below in detail.

[0118] EMBODIMENT 1 %P≧50% (where %P is the average bulk volume porosity); df≦0.36 (where df is (d 50 -d 10 ) / d 50 ) is; comprising a crystalline phase containing cordierite and indialite with a combined weight percentage of at least 85% by weight; 1. A ceramic body comprising up to 10 wt. % of a crystalline phase comprising a pseudobrookite structure, The ceramic body comprises, expressed as weight percent on an oxide basis: 1 wt% to 11 wt% titania, and 89 wt% to 99 wt% MgO, Al2O3, and SiO2 (wherein the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4); or 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al2O3, and SiO2 (where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3). A ceramic body comprising:

[0119] EMBODIMENT 2 Microcrack index Nb3 Nb 3 ≧0.10.

[0120] EMBODIMENT 3 2. The ceramic body of embodiment 1, wherein %P≧55%.

[0121] EMBODIMENT 4 2. The ceramic body of embodiment 1, wherein %P≧60%.

[0122] EMBODIMENT 5 2. The ceramic body of embodiment 1, wherein %P≧65%.

[0123] EMBODIMENT 6 2. The ceramic body of embodiment 1, wherein 50%≦%P≦72%.

[0124] EMBODIMENT 7 2. The ceramic body of embodiment 1, wherein 60%≦%P≦72%.

[0125] EMBODIMENT 8 2. The ceramic body of embodiment 1, wherein 65%≦%P≦72%.

[0126] EMBODIMENT 9 2. The ceramic body of embodiment 1, wherein df≦0.32.

[0127] EMBODIMENT 10 2. The ceramic body of embodiment 1, wherein df≦0.25.

[0128] EMBODIMENT 11 2. The ceramic body of embodiment 1, wherein df≦0.22.

[0129] EMBODIMENT 12 2. The ceramic body of embodiment 1, wherein df≦0.20.

[0130] EMBODIMENT 13 2. The ceramic body of embodiment 1, wherein df≦0.18.

[0131] EMBODIMENT 14 2. The ceramic body of embodiment 1, wherein df≦0.17.

[0132] EMBODIMENT 15 2. The ceramic body of embodiment 1, wherein 0.16≦df≦0.30.

[0133] EMBODIMENT 16 2. The ceramic body of embodiment 1, wherein 0.16≦df≦0.25.

[0134] EMBODIMENT 17 2. The ceramic body of embodiment 1, wherein 0.16≦df≦0.22.

[0135] EMBODIMENT 18 2. The ceramic body of embodiment 1, wherein 0.16≦df≦0.20.

[0136] EMBODIMENT 19 2. The ceramic body of embodiment 1, wherein the .DELTA..times ...

[0137] EMBODIMENT 20 2. The ceramic body of embodiment 1, wherein the .DELTA..times ...

[0138] EMBODIMENT 21 2. The ceramic body of embodiment 1, wherein the .DELTA..times ...

[0139] EMBODIMENT 22 7μm≦d 50 ≦20μm (where d 50 is the median pore size of the ceramic body.

[0140] EMBODIMENT 23 10μm≦d 50 ≦20μm (where d 50 is the median pore size of the ceramic body.

[0141] EMBODIMENT 24 12μm≦d 50 ≦20μm (where d 50 is the median pore size of the ceramic body.

[0142] EMBODIMENT 25 When measured at 25℃~800℃, CTE≦14×10 -7 13. The ceramic body of embodiment 1, wherein CTE is the coefficient of thermal expansion.

[0143] EMBODIMENT 26 CTE≦13×10 -7 26. The ceramic body of embodiment 25, wherein the temperature is 100 / °C.

[0144] EMBODIMENT 27 CTE≦12×10 -7 26. The ceramic body of embodiment 25, wherein the temperature is 100 / °C.

[0145] EMBODIMENT 28 CTE≦10×10 -7 26. The ceramic body of embodiment 25, wherein the temperature is 100 / °C.

[0146] EMBODIMENT 29 CTE≦9×10 -7 26. The ceramic body of embodiment 25, wherein the temperature is 100 / °C.

[0147] EMBODIMENT 30 3×10 -7 / ℃≦CTE≦14×10 -7 26. The ceramic body of embodiment 25, wherein the temperature is 100 / °C.

[0148] EMBODIMENT 31 3×10 -7 / ℃≦CTE≦12×10 -7 26. The ceramic body of embodiment 25, wherein the temperature is 100 / °C.

[0149] EMBODIMENT 32 50%≦%P≦72%; 7μm≦d50 ≦20μm (where d 50 is the median pore size; 0.16≦df≦0.36; 3×10 -7 / K≦CTE≦14×10 -7 2. The ceramic body of embodiment 1, wherein N is 0.1-0.25N / K.

[0150] EMBODIMENT 33 60%≦%P≦72%; 10μm≦d 50 ≦20μm (where d 50 is the median pore size; 0.16≦df≦0.25; 3×10 -7 / ℃≦CTE≦13×10 -7 2. The ceramic body of embodiment 1, wherein CTE is the coefficient of thermal expansion of the ceramic body measured from 25° C. to 800° C.

[0151] EMBODIMENT 34 60%≦%P≦72%; 12μm≦d 50 ≦20μm (where d 50 is the median pore size of the ceramic body; 0.16≦df≦0.20; 3×10 -7 / K≦CTE≦12×10 -7 2. The ceramic body of embodiment 1, wherein CTE is the coefficient of thermal expansion of the ceramic body as measured from 25° C. to 800° C.

[0152] EMBODIMENT 35 60%≦%P≦72%; 13μm≦d 50 ≦20μm (where d 50 is the median pore size of the ceramic body; 0.16≦df≦0.18; 3×10 -7 / K≦CTE≦12×10 -72. The ceramic body of embodiment 1, wherein CTE is the coefficient of thermal expansion of the ceramic body as measured from 25° C. to 800° C.

[0153] EMBODIMENT 36 2. The ceramic body of embodiment 1, wherein the crystalline phases of cordierite and indialite are 85% to 92% by weight.

[0154] EMBODIMENT 37 2. The ceramic body of embodiment 1, wherein the crystalline phase of cordierite is 53% to 78% by weight.

[0155] EMBODIMENT 38 2. The ceramic body of embodiment 1, wherein the crystalline phase of Indialite is 15% to 35% by weight.

[0156] EMBODIMENT 39 2. The ceramic body of embodiment 1, wherein the pseudobrookite structure comprises a crystalline phase of armalcolite.

[0157] EMBODIMENT 40 40. The ceramic body of embodiment 39, wherein the crystalline phase of armalcolite is 2% to 8% by weight.

[0158] EMBODIMENT 41 2. The ceramic body of embodiment 1 comprising 1.5 wt.% to 3 wt.% of a mullite crystalline phase.

[0159] EMBODIMENT 42 2. The ceramic body of embodiment 1 comprising less than 1.0 wt. % of a rutile crystalline phase.

[0160] EMBODIMENT 43 2. The ceramic body of embodiment 1 comprising less than 7 wt. % of an amorphous phase.

[0161] EMBODIMENT 44 2. The ceramic body of embodiment 1, wherein the titania oxide concentration is 1% to 6% by weight.

[0162] EMBODIMENT 45 45. The ceramic body of embodiment 44, wherein the titania oxide concentration is 2% to 6% by weight.

[0163] EMBODIMENT 46 2. The ceramic body of embodiment 1, wherein the oxide of magnesia has a concentration of 12% to 17% by weight.

[0164] EMBODIMENT 47 2. The ceramic body of embodiment 1, comprising 2 wt.% to 6 wt.% titania, and 94 wt.% to 98 wt.% MgO, Al2O3, and SiO2, wherein the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 14.3:34.9:50.8; 13.3:34.9:51.8; 14.3:32.3:53.4; and 15.3:32.3:52.4.

[0165] EMBODIMENT 48 2. The ceramic body of embodiment 1 comprising a honeycomb body.

[0166] EMBODIMENT 49 49. The ceramic body of embodiment 48, wherein the honeycomb body comprises a matrix of interconnected porous walls.

[0167] EMBODIMENT 50 50. The ceramic body of embodiment 49, wherein the matrix of interconnected porous walls has a lateral wall thickness of 0.05 mm to 0.41 mm.

[0168] EMBODIMENT 51 The matrix of the interconnected porous walls is 15.5 cells / cm 2 ~62 cells / cm 2 50. The ceramic body of embodiment 49, having a cell density of

[0169] EMBODIMENT 52 1. A ceramic body comprising a crystalline phase comprising cordierite and indialite with a combined weight percentage of 85% to 92% by weight and a second crystalline phase of pseudobrookite structure comprising armalcolite with a maximum weight percentage of 10% by weight, the ceramic body contains, expressed in weight percent on an oxide basis, 1 wt.% to 11 wt.% titania, and 89 wt.% to 99 wt.% MgO, Al2O3, and SiO2, where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4; 55% ≤ %P ≤ 72%; 8μm≦d 50 ≦20μm (where d 50 is the median pore size; 0.16≦df≦0.32 (where df is (d 50 -d 10 ) / d 50 ) is; 3×10 at 25℃~800℃ -7 / ℃≦CTE≦14×10 -7 / ℃, ceramic body.

[0170] EMBODIMENT 53 1. A ceramic body comprising a crystalline phase comprising cordierite and indialite with a combined weight percentage of 85% to 92% by weight and a second crystalline phase of pseudobrookite structure comprising armalcolite with a maximum weight percentage of 10% by weight, the ceramic body contains, expressed in weight percent on an oxide basis, 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al2O3, and SiO2, wherein the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3; 55% ≤ %P ≤ 72%; 8μm≦d 50 ≦20μm (where d50 is the median pore size; 0.16≦df≦0.32 (where df is (d 50 -d 10 ) / d 50 ) is; 3×10 at 25℃~800℃ -7 / ℃≦CTE≦14×10 -7 / ℃, ceramic body.

[0171] EMBODIMENT 54 Expressed as weight percent on an oxide basis: 1 wt.% to 11 wt.% titania, and 89 wt.% to 99 wt.% MgO, Al2O3, and SiO2, where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4; or 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al2O3, and SiO2 (where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3). a batch composition mixture comprising a magnesia source, an alumina source, a silica source, and a titania source.

[0172] EMBODIMENT 55 20% to 42% by weight of said magnesia source; 25% to 40% by weight of the alumina source; 15% to 30% by weight of the silica source; and 1% to 10% by weight of a titania source Including, 55. The batch composition mixture of embodiment 54, wherein the weight percentages of each of the magnesia source, the alumina source, the silica source, and the titania source are all based on 100% total weight of minerals present in the batch composition mixture.

[0173] EMBODIMENT 56 The alumina sources each comprise, based on the total weight of the minerals in the batch composition mixture: 20% to 35% by weight of alumina; and 0% to 16% by weight of hydrated alumina 55. The batch composition mixture of embodiment 54, comprising:

[0174] EMBODIMENT 57 Contains 26% by weight SA to 56% by weight SA of a pore-forming agent, 55. The batch composition mixture of embodiment 54, wherein wt. % SA is the weight percent of the add-on based on the total weight of the minerals in the batch composition mixture.

[0175] EMBODIMENT 58 58. The batch composition mixture of embodiment 57, wherein the pore-forming agent is provided in the range of 35 wt.% SA to 56 wt.% SA.

[0176] EMBODIMENT 59 58. The batch composition mixture of embodiment 57, wherein the pore-forming agent comprises pea starch provided in the range of 35 wt.% SA to 51 wt.% SA.

[0177] EMBODIMENT 60 58. The batch composition mixture of embodiment 57, wherein the pore-forming agent comprises 36 wt.% SA to 46 wt.% SA of pea starch and 9 wt.% SA to 11 wt.% SA of graphite.

[0178] EMBODIMENT 61 58. The batch composition mixture of embodiment 57, wherein the pore-forming agent comprises starch alone or a combination of starch and graphite.

[0179] EMBODIMENT 62 1. A method for making a ceramic body, comprising: The above method: 20% to 42% by weight of a magnesia source; 25% to 40% by weight of an alumina source; 15% to 30% by weight of a silica source, and 1 wt. % to 10 wt. % of a titania source; wherein all of said weight percentages of each of said magnesia source, said alumina source, said silica source, and said titania source are based on 100% total weight of minerals present; The inorganic components are mixed at 26% by weight SA pf ~56wt%SA pf and a liquid vehicle to form a batch composition mixture, pf is the weight percent of the addition based on 100% total weight of the inorganic material; forming the batch composition mixture into a green body; and firing the green body under conditions effective to convert the green body into a ceramic body having a combined weight percentage of at least 85% by weight of a crystalline phase containing cordierite and indialite, and up to 10% by weight of a crystalline phase containing a pseudobrookite structure. A method comprising:

[0180] EMBODIMENT 63 63. The method of embodiment 62, wherein the firing conditions effective to convert the green body to a ceramic body include heating the green body to a soak temperature of 1350°C to 1410°C and maintaining the soak temperature for a soak time sufficient to convert the green body to the ceramic body.

[0181] EMBODIMENT 64 63. The method of embodiment 62, wherein the pseudobrookite structure comprises an armalcolite crystalline phase.

[0182] EMBODIMENT 65 63. The method of embodiment 62, wherein the step of shaping the batch composition mixture into the green body comprises extruding the batch composition mixture through an extrusion die to form a green honeycomb body.

[0183] EMBODIMENT 66 %P≧50% (where %P is the average bulk volume porosity); df≦0.36 (where df is (d 50 -d 10 ) / d 50 ) is; comprising a crystalline phase containing cordierite and indialite with a combined weight percentage of at least 85% by weight; 1. A ceramic body comprising up to 10 wt. % of a crystalline phase comprising a pseudobrookite structure, The ceramic body comprises, expressed as weight percent on an oxide basis: 1 wt% to 11 wt% titania, and 89 wt% to 99 wt% MgO, Al2O3, and SiO2 (wherein the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4); or 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al2O3, and SiO2 (where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.3). A ceramic body comprising:

[0184] EMBODIMENT 67 7μm≦d 50 ≦20μm (where d 50 is the median pore size of the ceramic body.

[0185] EMBODIMENT 68 50%≦%P≦72%; 7μm≦d 50 ≦20μm (where d 50 is the median pore size; 0.16≦df≦0.36; 3×10 -7 / K≦CTE≦14×10 -7 67. The ceramic body of embodiment 66, wherein N is 0.1-0.25 Mg / K.

[0186] EMBODIMENT 69 60%≦%P≦72%; 10μm≦d 50 ≦20μm (where d 50 is the median pore size; 0.16≦df≦0.25; 3×10 -7 / ℃≦CTE≦13×10 -7 67. The ceramic body of embodiment 66, wherein CTE is the coefficient of thermal expansion of the ceramic body measured from 25° C. to 800° C.

[0187] EMBODIMENT 70 67. The ceramic body of embodiment 66, comprising 2 wt.% to 6 wt.% titania and 94 wt.% to 98 wt.% MgO, Al2O3, and SiO2, where the relative weight ratios of MgO:Al2O3:SiO2 are within the fields defined by 14.3:34.9:50.8; 13.3:34.9:51.8; 14.3:32.3:53.4; and 15.3:32.3:52.4.

[0188] EMBODIMENT 71 1. A method for making a ceramic body, comprising: The method includes: 20% to 42% by weight of a magnesia source; 25% to 40% by weight of an alumina source; 15% to 30% by weight of a silica source, and 1 wt. % to 10 wt. % of a titania source; wherein all of said weight percentages of each of said magnesia source, said alumina source, said silica source, and said titania source are based on 100% total weight of minerals present; The inorganic component is 26% by weight SA pf ~56wt%SA pfand a liquid vehicle to form a batch composition mixture, pf is the weight percent of the addition based on 100% total weight of the inorganic material; shaping the batch composition mixture into a green body; and firing the green body under conditions effective to convert the green body into a ceramic body having a combined weight percentage of at least 85% by weight of a crystalline phase containing cordierite and indialite, and up to 10% by weight of a crystalline phase containing a pseudobrookite structure. A method comprising: [Explanation of symbols]

[0189] 100 Ceramic body 100G Base, Base Honeycomb Body 100P Plugged ceramic honeycomb body 102 Porous wall 103 First end, inlet end 104, 104L, 104S Channels 105 second end, outlet end 106 Epidermis 200 Extrusion Machine 210 Plasticized batch composition mixture 212 barrels 214 Chamber 215 Longitudinal 215D downstream 215U upstream side 216 Material supply port 217 Cartridge Assembly, Extruder Cartridge 218 Honeycomb Extrusion Die 220 screens 222 Homogenizer 224 Extrusion screw 226 Epidermal Formation Mask 228 Cutting Element 230 Tray

Claims

1. %P≧50%, where %P is the average bulk volume porosity; df≦0.36 (where df is (d 50 -d 10 ) / d 50 ) is; comprising a crystalline phase containing cordierite and indialite with a combined weight percentage of at least 85% by weight; 1. A ceramic body comprising up to 10 wt. % of a crystalline phase comprising a pseudobrookite structure, The ceramic body comprises, expressed as weight percent on an oxide basis: 1% to 11% by weight of titania, and 89% to 99% by weight of MgO, Al 2 O 3 , and SiO 2 (where MgO:Al 2 O 3 : SiO 2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 13.9:30.7:55.4, and 16.9:30.7:52.4; or 2.5% to 11% titania, and 89% to 97.5% by weight MgO, Al 2 O 3 , and SiO 2 (where MgO:Al 2 O 3 : SiO 2 are within the fields defined by 15.6:34.0:50.4, 12.6:34.0:53.4, 12.0:35.7:52.3, and 15.0:35.7:49.

3. A ceramic body comprising:

2. 7 μm≦d 50 ≦20 μm (where d 50 is the median pore size of the ceramic body.

3. 50%≦%P≦72%; 7 μm≦d 50 ≦20 μm (where d 50 is the median pore size; 0.16≦df≦0.36; 3×10 -7 / K≦CTE≦14×10 -7 2. The ceramic body of claim 1 , wherein:

4. 60%≦%P≦72%; 10 μm≦d 50 ≦20 μm (where d 50 is the median pore size; 0.16≦df≦0.25; 3×10 -7 / °C≦CTE≦13×10 -7 10. The ceramic body of claim 1, wherein CTE is the coefficient of thermal expansion of the ceramic body as measured from 25°C to 800°C.

5. 2% to 6% by weight of titania, and 94% to 98% by weight of MgO, Al 2 O 3 , and SiO 2 (where MgO:Al 2 O 3 : SiO 2 13.3:34.9:51.8; 14.3:32.3:53.4; and 15.3:32.3:52.

4.

6. 1. A method for making a ceramic body, comprising: The method comprises: 20% to 42% by weight of a magnesia source; 25% to 40% by weight of an alumina source; 15% to 30% by weight of a silica source, and 1 wt. % to 10 wt. % of a titania source; wherein all of said weight percentages of each of said magnesia source, said alumina source, said silica source, and said titania source are based on 100% total weight of minerals present; The inorganic component is 26% by weight SA pf ~56%SA by weight pf and a liquid vehicle to form a batch composition mixture, pf is the weight percent of the addition based on 100% total weight of the inorganic material; shaping the batch composition mixture into a green body; and firing the green body under conditions effective to convert the green body into a ceramic body comprising a combined weight percentage of at least 85% by weight of a crystalline phase comprising cordierite and indialite, and up to 10% by weight of a crystalline phase comprising a pseudobrookite structure. A method comprising:

Citation Information

Patent Citations

  • High-porosity ceramic honeycomb articles containing rare earth oxides and methods for manufacturing the same

    JP2011510890A

  • Cordierite enhanced with dispersions for filters and substrates

    JP2011514875A