Highly stretchable adhesive silicone compositions and uses thereof as sealing / bonding agents
A two-part addition-curing silicone adhesive composition addresses the inadequacies of existing airbag seam adhesives by providing high elongation and peel strength, ensuring effective airbag sealing and safety without solvent evaporation hazards.
Patent Information
- Application Number
- JP2024120376
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-02-06
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024150698000001 
Figure 2024150698000002 
Figure 2024150698000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is an international application under the Patent Cooperation Treaty claiming priority to U.S. Provisional Application No. 62 / 971,049, filed February 6, 2020, the contents of which are incorporated herein by reference in their entirety.
[0002] The present invention relates to novel addition-curable silicone compositions which, when applied to textile fabrics and cured, have excellent self-adhesive properties and very high elongation at break properties.
[0003] These silicone compositions provide excellent adhesive properties such as peel strength and cohesive failure when used to seal the joint / seam between two pieces of textile fabric.
[0004] Airbag fabrics using such novel addition curable adhesive silicone compositions are also encompassed by this invention. [Background technology]
[0005] Many automobiles today are equipped with acceleration sensors that measure the vehicle's deceleration. When a reference deceleration value is exceeded, explosive pellets cause the combustion of an additional charge, which in turn causes the combustion of a combustible solid. This solid is converted to a gas (such as nitrogen), which inflates the cushion. An airbag (or inflatable cushion) is an air-filled bag made of pleated and tight-stitched fabric. For more information regarding these personal protection bags, or "airbags", see especially U.S. Pat. No. 5,193,847.
[0006] Traditionally, airbags are made of fabric made of synthetic fibers, e.g. polyamide, and are manufactured as a single piece or from two pieces assembled, e.g. by adhesive bonding or sewing with polyamide thread. The outer surface of airbags manufactured in a single piece is generally coated with a crosslinked silicone elastomer film that forms a protective and mechanically reinforcing coating. On the other hand, in the case of airbags made from two pieces sewn together, the silicone elastomer film is provided on the inner surface of the airbag. Assembly by sewing results in some disadvantages, since needle punctures in the silicone elastomer film and the fabric can form holes in the area of the seam, compromising the leak-proof properties and resistance to chemical, thermal and climatic attacks.
[0007] Although fabrics coated with conventional silicone compositions may be satisfactory for standard airbag applications, the airbag industry now needs to meet the requirement that pressurized air be retained in the fabric envelope for a relatively long period of time. This requirement exists, for example, when applying such coatings to side curtain airbags for the automotive industry. Curtain airbags are currently designed to inflate as quickly as driver and passenger side bags, but their deflation must be very slow to protect the occupants in the event of a rollover or side impact. The side curtain deploys to form a cushion curtain between the occupant and a portion of the side of the vehicle body, such as a window. Since the intention is not just to cushion the impact itself, as is the case with conventional driver and passenger airbags, but to protect the passengers when, for example, the car is rolling, it is important that the side curtain airbag is adequately pressurized during such a rolling process. Whereas conventional driver and passenger airbags only need to maintain pressure for a fraction of a second, side curtain airbags need to maintain the proper pressure for at least several seconds.
[0008] One solution to this problem of leak-proofing the seam areas of airbags consists of applying an adhesive joint to the seam area. According to this known method, the airbag parts are cut at the top and bottom, a bead of adhesive is placed around one of the parts, and then the two parts are compressed to create a joint. The bag with the adhesive then proceeds to the "sewing" part of the manufacturing process.
[0009] The adhesive used in this method is generally a tacky silicone composition. Such adhesive compositions are described, for example, in EP 0 131 854 and are capable of permanently bonding two surfaces. This composition is obtained by mixing: (i) Essentially RSiO 1 / 2 Units and SiO 4 / 2 units, containing hydroxyl groups, and 9 to 70 weight percent of a solid resinous copolymer soluble in benzene, where R is a monovalent hydrocarbon group containing less than 5 carbon atoms, and at least 95 percent of the R groups in (i) are methyl groups; (ii) 30 to 91% by weight of the formula HO(RSiO) a Polydiorganosiloxanes of H, where R is as defined above and the average value of a is such that the viscosity of (ii) is greater than 10,000 Pa·s at 25°C; (iii) is compatible with mixtures of (i) and (ii), based on 100 parts by weight of (i) and (ii), and has the formula R b H c SiO (4-b-c) / 2 wherein R is as defined above, b is between 1.00 and less than 2, c is between 0.3 and 1.00, the sum of b+c is between 1.30 and less than 3.00, there are an average of more than 2 silicon-bonded hydrogen atoms per molecule of (iii) and no silicon atoms have one or more silicon-bonded hydrogen atoms, the molar ratio of SiH units in (iii) to SiOH units in (i) and (ii) is between 0.2 / 1 and 1 / 1, and the weight of hydrogen atoms present on silicon is less than 0.05 g per 100 g of (i) and (ii); (iv) 0.5 to 2 parts by weight per 100 parts by weight of (i) and (ii) of a tin-based soluble catalyst; and (v) A sufficient amount of non-reactive solvent to mix (i), (ii), (iii), and (iv) to obtain a flowable adhesive having a viscosity and solids tack capable of achieving an adhesive thickness of at least 0.1 mm in a single application of the adhesive. Summary of the Invention [Problem to be solved by the invention]
[0010] The method described for applying this composition specifies a step for evaporating the solvent which increases part manufacturing time, reduces yields, and creates safety and health hazards.
[0011] Furthermore, the performance of this adhesive is limited and insufficient for this adhesive to be used in all cases in the field of airbag assembly.
[0012] Now, in the special case of airbags, it is necessary to use adhesives with sufficient adhesive strength (e.g. peel strength, cohesive failure) and high elongation at break. Indeed, when the airbag opens, the fabric expands very quickly, leading to very large deformations of the fabric in the stitching area. This is especially seen in side airbags, which, unlike front and passenger airbags, owing to the complex shape of the bag, the fabric in the stitching area is folded outwards instead of inwards.
[0013] Flexible properties are easy to achieve. Stretchability, on the other hand, represents a more challenging type of mechanical, where the system must accommodate large strain deformations, typically of any form, including not only bending, but also twisting, stretching, compression, etc.
[0014] Elongation at break is the percentage increase in length a material achieves before breaking. This number is expressed as a percentage and is usually measured using standard test method ASTM D412. A higher percentage usually indicates a higher quality material when combined with good tensile strength.
[0015] Other formulations have been developed to improve the mechanical properties of adhesives. In particular, U.S. Patent No. 6,811,650 discloses an adhesive composition comprising: A. 100 parts by weight of an organopolysiloxane having an average of two or more alkenyl groups per molecule; B. an organopolysiloxane having an average of two or more silicon-bonded hydrogen atoms in each molecule (in an amount such that the molar ratio of silicon-bonded hydrogen atoms in component B to alkenyl groups in component A is 0.01 to 20); C. 5 to 200 parts by weight of a precipitated calcium carbonate powder selected from the group consisting of: (i) calcium carbonate treated with an organic acid, and (ii) calcium carbonate treated with an ester of an organic acid, said calcium carbonate powder being 5 to 50 parts by weight. 2 / g BET specific surface area; and D. A platinum-based catalyst in an amount sufficient to effect cure of the composition.
[0016] This composition gives an adhesive with a tensile strength of 3.5 MPa (JISK6251 test) and an elongation at break of 1500%. However, it is indicated that this composition should be cured for 7 days at 25° C. to obtain an adhesive with the desired properties in elongation and tensile strength. It is clear that in industrial production it is not possible to take into account such crosslinking times.
[0017] A method for adhesively bonding at least two substrates using a crosslinkable adhesive silicone composition is described in U.S. Pat. No. 8,431,647, which comprises: (A) at least one polyorganosiloxane POS(A) having at least two alkenyl groups per molecule; (B) at least one polyorganosiloxane crosslinker having at least two silicon-bonded hydrogen atoms per molecule; (C) a catalytically effective amount of at least one catalyst based on at least one metal compound, and (D) Reinforcing filler Including, It is also characterized in that it contains at least one polyorganosiloxane gum POS (A') different from POS (A), has a content of alkenyl group or groups between 0.001 and 0.2% by weight, and has a consistency between 300 and 1200 at 25°C.
[0018] The mechanical properties of the composition in terms of adhesive strength (peel strength of 34 N / cm) and elongation at break (1180%) are acceptable for producing adhesive joints in the seam areas of airbags. However, there is a need for adhesive silicone compositions with improved mechanical properties, e.g., greater adhesive strength combined with greater elongation at break for use as joint sealers in airbags, especially side airbags, where a leak-proof seal must be maintained for several seconds. [Means for solving the problem]
[0019] After extensive research, the inventors have found that the above problems can be solved by using an addition-curable silicone adhesive composition X. Upon curing, composition X becomes a highly extensible silicone elastomer additive Z having an elongation at break value of at least 1200%, preferably at least 1500%, as measured according to ASTM D-412, and a peel strength of at least 40 N / cm.
[0020] The addition-curing silicone adhesive composition X can be used to bond two substrates that constitute an inflatable bag for protecting vehicle occupants, for example, two substrates that are assembled by sewing.
[0021] Also provided is a method of adhesively bonding at least two substrates, the method comprising applying an addition curable silicone adhesive composition X to at least one surface of one or more of the at least two substrates to form at least one adhesively coated surface, and assembling the substrates such that the at least one adhesively coated surface contacts the at least two substrates, thereby forming an adhesive bond between the at least two substrates.
[0022] Airbag fabrics using addition curable silicone adhesive composition X are also provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Before the present disclosure is further described, it should be understood that the present disclosure is not limited to the specific embodiments of the present disclosure described below. Variations of the specific embodiments may be made and still fall within the scope of the appended claims. It should also be understood that the terms used are for the purpose of describing the specific embodiments and are not intended to be limiting. Instead, the scope of the present disclosure is established by the appended claims.
[0024] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs.
[0025] As used herein, the term "silicone rubber" includes the crosslinked product of any crosslinkable silicone composition. The terms "silicone rubber" and "silicone elastomer" can be used interchangeably.
[0026] As used herein, the terms "crosslinked" and "cured" may be used interchangeably and refer to the reaction that occurs when the components of the curable silicone composition are combined and reacted to result in a cured silicone elastomer.
[0027] The term "alkenyl" as used herein is understood to mean a substituted or unsubstituted, unsaturated, linear or branched hydrocarbon chain having at least one olefinic double bond, more preferably a single double bond. Preferably, the "alkenyl" group has 2 to 10 carbon atoms, more preferably 2 to 6 carbon atoms. This hydrocarbon chain optionally contains at least one heteroatom, such as O, N, S. Preferred examples of "alkenyl" groups are vinyl, allyl and homoallyl groups, with vinyl being particularly preferred.
[0028] As used herein, "alkyl" refers to a saturated, straight or branched, optionally substituted (e.g., with one or more alkyl) hydrocarbon chain, preferably having 1 to 10 carbon atoms, such as 1 to 8 carbon atoms, more preferably 1 to 4 carbon atoms. Examples of alkyl groups are methyl, ethyl, isopropyl, n-propyl, tert-butyl, isobutyl, n-butyl, n-pentyl, isoamyl, and 1,1-dimethylpropyl, among others.
[0029] In order to achieve the objective of obtaining a highly elastic silicone adhesive (i.e., a silicone adhesive having an elongation at break value of at least 1200%) and a peel strength of at least 40 N / cm, the applicant has demonstrated that the problems not solved by the prior art can be overcome by the combination of: (A) an alkenyl-containing organopolysiloxane A having at least two silicon-bonded alkenyl groups per molecule, (B) at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender CE, (C) at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker containing at least three silicon-bonded alkenyl groups per molecule. Alk-XL, and optionally (D) at least one organosilicon crosslinker H-XL containing at least three hydrogen atoms per molecule in amounts such that: 1) the molar ratio of hydrogen atoms to alkenyl groups in the silicone adhesive (RHalk) is 1.05-1.40, 2) the percentage of the number of moles of hydrogen atoms directly bonded to silicon atoms of CE out of the number of moles of hydrogen atoms directly bonded to silicon atoms of both CE and H-XL combined (RHCE) is 90%-100%, and 3) the percentage of the number of moles of alkenyl groups directly bonded to silicon atoms of A out of the total number of moles of alkenyl groups directly bonded to silicon atoms in the composition (RAlkA) is 80%-95%.
[0030] In particular, addition-curing silicone adhesive X has the following properties: (A) At least two silicon bonds C2 to C per molecule 20 At least one alkenyl-containing organopolysiloxane A having an alkenyl group; (B) at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender CE; (C) at least three silicon-bonded C2-C per molecule having a total alkenyl content of 0.02-0.10 wt.% 20 at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL containing alkenyl groups; (D) optionally, at least one organosilicon crosslinker H-XL containing at least three silicon-bonded hydrogen atoms per molecule; (E) at least one addition reaction catalyst C; (F) at least one reinforcing mineral filler F1, (G) optionally, at least one complementary filler F2; (H) optionally, at least one cure rate modifier G; (I) optionally at least one rheology modifier H; (J) optionally at least one adhesion promoter I, and (K) optionally, at least one functional additive to impart a particular property J Includes.
[0031] As mentioned above, the amounts of A, CE, Alk-XL, and optional H-XL in the curable silicone adhesive composition X are preferably selected so that: 1) the molar ratio of hydrogen atoms to alkenyl groups in the silicone elastomer (RHalk) is from 1.05 to 1.40; 2) the percentage of hydrogen atoms directly bonded to silicon atoms of CE out of the number of moles of hydrogen atoms directly bonded to silicon atoms in both the combination of CE and H-XL (RHCE) is from 90 to 100%; and 3) the percentage of the number of moles of alkenyl groups directly bonded to silicon atoms of A out of the total number of moles of alkenyl groups directly bonded to silicon atoms in the entire composition (RAlkA) is from 80% to 95%.
[0032] The curable silicone adhesive composition X can be prepared by simply mixing the components in the desired ratio. However, for reasons of storage stability and bath life, it is preferred to store the composition X in two parts A and B by separating the curing catalyst (C) from the diorganopolysiloxane with hydrogen substituents (CE) or the optional organosilicon crosslinker (H-XL) before or during application of the composition to a substrate. The other components of the composition X are often dispersed in both parts in a ratio that allows the two parts to be easily mixed immediately before application. Such an easy mixing ratio can be, for example, a ratio of 1 / 10 or 1 / 1.
[0033] Preferably, the two-part curable liquid silicone adhesive composition of the present invention comprises a first liquid composition comprising components A, Alk-XL, and C, but not including CE and H-XL, and a second liquid composition comprising components A, Alk-XL, CE, and optionally H-XL, but not including C.
[0034] Once mixed together, parts A and B form a ready-to-use silicone adhesive composition which can be applied to a substrate by any suitable means to obtain an adhesive having a thickness of at least 0.3 mm.
[0035] Curable silicone adhesive composition X, upon curing, provides a silicone adhesive elastomer Z having an elongation at break value of at least 1200% as measured according to ASTM D-412. In some embodiments, curable silicone adhesive composition X, upon curing, provides a silicone adhesive elastomer Z having an elongation at break value of at least 1300%, at least 1400%, at least 1500%, at least 1600%, at least 1700%, at least 1800%, at least 1900%, or at least 2000% as measured according to ASTM D-412.
[0036] ASTM D412 measures the elasticity of a material while under tensile strain as well as how the material behaves after the test when it is unstressed. ASTM D412 measures a variety of properties, the most common of which are: Tensile Strength: The maximum tensile stress that can be applied to a test specimen when it is stretched to break. Tensile Stress at Given Elongation: The stress required to stretch a uniform cross-section of a test specimen to a given elongation. Ultimate Elongation: The elongation at which failure occurs upon application of continued tensile stress. Permanent Elongation: The elongation remaining in a specimen after it has been stretched and then retracted in a specified manner, expressed as a percentage of the original length.
[0037] The curable silicone adhesive composition X of the present invention comprises at least one alkenyl-containing organopolysiloxane A having at least two silicon-bonded alkenyl groups per molecule. In some embodiments, the curable silicone adhesive composition X of the present invention comprises two or more alkenyl-containing organopolysiloxanes A having at least two silicon-bonded alkenyl groups per molecule. For example, the curable silicone adhesive composition X of the present invention may comprise two alkenyl-containing organopolysiloxanes A (A1 and A2), each having at least two silicon-bonded alkenyl groups per molecule.
[0038] In some embodiments, the at least one alkenyl-containing organopolysiloxane A comprises: Two siloxy units of the formula (A-1): [ka] In the formula, the symbol "Alk" represents a C2-C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl group, preferably a vinyl group. 20 Represents an alkenyl group, where R is a C1-C alkyl group such as methyl, ethyl, or propyl. 20 C6-C alkyl groups such as xylyl, tolyl, and phenyl groups 12 represents an aryl group, preferably a methyl group, in which "Alk" and "R" in each instance may be the same or different; Other siloxy units of formula (A-2): [ka] In the formula, the symbol L is a C1-C aryl such as methyl, ethyl, or propyl. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 It represents an aryl group, preferably a methyl group, the symbol g is equal to 0, 1, 2, or 3, and L in each instance can be the same or different.
[0039] In some preferred embodiments, the at least one alkenyl-containing organopolysiloxane A has the following formula (1): [ka] where: n is an integer of 1 to 1000, preferably 50 to 1000; R is independently C1-C such as methyl, ethyl, propyl, etc. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 An aryl group, preferably a methyl group, or a C2-C alkyl group such as a vinyl, allyl, hexenyl, decenyl, or tetradecenyl group. 20 alkenyl groups, preferably vinyl groups, R' is independently a C2-C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl group. 20 alkenyl groups, preferably vinyl groups, R" is independently C1-C such as methyl, ethyl, propyl, etc. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 aryl groups, preferably methyl groups;
[0040] In a preferred embodiment, the at least one alkenyl-containing organopolysiloxane A is one or more α,ω-vinylpolydimethylsiloxanes, more preferably one or more linear α,ω-vinylpolydimethylsiloxanes.
[0041] In some embodiments, the viscosity of the at least one alkenyl-containing organopolysiloxane A is about 50 to about 100,000 mPa·s, preferably about 500 to about 50,000 mPa·s, and more preferably about 1,000 to about 25,500 mPa·s. In some embodiments, the curable silicone adhesive composition X of the present invention comprises at least one alkenyl-containing organopolysiloxane A1 having a viscosity of about 5,000 to about 100,000 mPa·s and at least one alkenyl-containing organopolysiloxane A2 having a viscosity of about 500 to about 10,000 mPa·s. In a preferred embodiment, the viscosity of the at least one alkenyl-containing organopolysiloxane A1 is about 7,500 to about 50,000 mPa·s, and more preferably about 10,000 to about 25,000 mPa·s. In a preferred embodiment, the viscosity of the at least one alkenyl-group-containing organopolysiloxane A2 is from about 500 to about 7,500 mPa·s, more preferably from about 1,000 to about 5,000 mPa·s.
[0042] All viscosities considered herein correspond to the magnitude of dynamic viscosity measured in a manner known per se using a Brookfield viscometer, model RV or RVT, at 25° C. For fluid products, the viscosity considered herein is the dynamic viscosity at 25° C. known as the “Newtonian” viscosity, i.e. the dynamic viscosity measured in a manner known per se.
[0043] In some embodiments, the molecular weight of the at least one alkenyl-containing organopolysiloxane A is about 1,000 g / mol to about 80,000 g / mol, preferably about 5,000 g / mol to about 70,000 g / mol, and more preferably about 10,000 g / mol to about 60,000 g / mol. In some embodiments, the curable silicone adhesive composition X of the present invention comprises at least one alkenyl-containing organopolysiloxane A1 having a molecular weight of about 5,000 to about 80,000 g / mol and at least one alkenyl-containing organopolysiloxane A2 having a viscosity of about 1,000 to about 50,000 g / mol. In a preferred embodiment, the molecular weight of at least one alkenyl-containing organopolysiloxane A1 is about 15,000 to about 75,000 g / mol, more preferably about 30,000 to about 60,000 g / mol. In a preferred embodiment, the molecular weight of at least one alkenyl-containing organopolysiloxane A2 is about 5,000 to about 40,000 g / mol, more preferably about 10,000 to about 30,000 g / mol.
[0044] At least one alkenyl-containing organopolysiloxane A is preferably linear.
[0045] The curable silicone adhesive composition X of the present invention further comprises at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender CE. The at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender CE can be included in the curable silicone adhesive composition X in an amount by weight of the total composition of from about 0.1% to about 20%, preferably from about 0.5% to about 15%, preferably from about 0.5% to about 10%.
[0046] In some embodiments, the diorganohydrogensiloxy-terminated diorganopolysiloxane CE has the following formula (2): [ka] where: R is independent, C1~C 20or C6-C alkyl groups such as xylyl, tolyl, or phenyl groups. 12 R is independently selected from the group consisting of methyl, ethyl, propyl, and aryl, and most preferably, R is methyl; n is an integer ranging from 1 to 500, preferably from 2 to 100, and more preferably from 3 to 50.
[0047] In some embodiments, the viscosity of the at least one diorganohydrogensiloxy-terminated diorganopolysiloxane CE is from about 1 to about 500 mPa·s, preferably from about 2 to about 100 mPa·s, and more preferably from about 4 to about 50 mPa·s or from about 5 to about 20 mPa·s.
[0048] In some embodiments, the molecular weight of the at least one diorganohydrogensiloxy-terminated diorganopolysiloxane CE is from about 100 to about 5,000 g / mole, preferably from about 250 to about 2,500 g / mole, and more preferably from about 500 to about 1,000 g / mole.
[0049] The curable silicone adhesive composition X of the present invention further comprises at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL, which is different from the at least one alkenyl-containing organopolysiloxane A and contains at least three silicon-bonded alkenyl groups per molecule. In particular, the at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL, which contains at least three silicon-bonded alkenyl groups per molecule, has a total alkenyl content of 0.02 to 0.10% by weight. In some embodiments, the at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL, which contains at least three silicon-bonded alkenyl groups per molecule, has a total alkenyl content of 0.02 to 0.065% by weight. In some embodiments, at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL, containing at least three silicon-bonded alkenyl groups per molecule, has a total alkenyl content of 0.04 to 0.06 weight percent.
[0050] In general, the at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL can be defined in the same way as the at least one alkenyl-group-containing organopolysiloxane A, and advantageously contains at least three siloxy units of formula (A-3) and other siloxy units of formula (A-2): [ka] In the formula, the symbol "Alk" represents a C2-C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl. 20 It represents an alkenyl group, preferably a vinyl group, and the symbol R is a C1-C alkyl group such as methyl, ethyl, or propyl. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 represents an aryl group, preferably a methyl group, where "Alk" and R in each case may be the same or different, and "h" is equal to 1 or 2; [ka] In the formula, the symbol L is a C1-C aryl such as methyl, ethyl, or propyl. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 It represents an aryl group, preferably a methyl group, the symbol g is equal to 2, and L in each instance may be the same or different.
[0051] In some preferred embodiments, at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL is of formula (1): [ka] where: -n is an integer ranging from 1000 to 10000, preferably from 2000 to 5000, -R is independently C1-C such as methyl, ethyl, propyl, etc. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 An aryl group, preferably a methyl group, or a C2-C alkyl group such as a vinyl, allyl, hexenyl, decenyl, or tetradecenyl group. 20 alkenyl groups, preferably vinyl groups, -R' is independently a C2-C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl group. 20 alkenyl groups, preferably vinyl groups, -R" is independently a C1-C alkyl group such as methyl, ethyl, or propyl. 20 C6-C alkyl groups, such as xylyl, tolyl, or phenyl groups 12 It is selected from aryl groups, preferably methyl groups.
[0052] Preferably, the organopolysiloxane chain of gum Alk-XL is blocked at each end by a vinyl group.
[0053] In some embodiments, the alkenyl groups of gum Alk-XL are randomly distributed on the organopolysiloxane chain of said gum, except for the terminal ones.
[0054] In a preferred embodiment, the at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL is a dimethylvinylsiloxy-terminated copolymer of methylvinylsiloxane and dimethylsiloxane.
[0055] It is evident that these various types of gum Alk-XL may be combined.
[0056] In some embodiments, at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL is a homopolymer or copolymer having at least three alkenyl groups per molecule and a viscosity of greater than 500,000 mPa·s at 25° C. In some embodiments, the viscosity of at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL is greater than 1 million mPa·s at 25° C. In some embodiments, the viscosity of at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL is greater than 10 million mPa·s at 25° C.
[0057] In some embodiments, the at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL has a consistency of 300-1200 at 25°C, preferably 500-1000 at 25°C, and more preferably 600-900 at 25°C.
[0058] The consistency or permeability of the gum is measured under standardized conditions at 25° C. using a PNR12 type penetrometer or an equivalent model which allows applying a cylindrical head to the sample.
[0059] Gum permeability is expressed in tenths of a millimeter as the depth to which a calibrated cylinder penetrates the sample in one minute.
[0060] For this, the gum sample is placed in an aluminium bucket with a diameter of 40 mm and a height of 60 mm. The bronze or brass cylindrical head is 6.35 mm in diameter and 4.76 mm in height and is supported by a metal rod with a length of 51 mm and a diameter of 3 mm, which is suitable for a penetrometer. This rod is ballasted with an overload of 100 g. The total weight of the assembly is 151.8 g, including the cylindrical part and its support rod weighing 4.3 g. The bucket with the gum sample is placed in a thermostatic bath at 25 °C ± 0.5 °C for a minimum of 30 minutes. The measurements are carried out according to the manufacturer's instructions. The instrument indicates the value of the depth (V) (in tenths of a millimetre) and the time (t) (in seconds) to reach this depth. The penetration is equal to 60 V / t, expressed in tenths of a millimetre per minute.
[0061] At least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL may be included in the curable silicone adhesive composition X in an amount by weight of from about 10% to about 40%, preferably from about 10% to about 30%, from about 15% to 30%, or from about 20% to about 30% of the total composition.
[0062] The curable silicone adhesive composition X of the present invention optionally comprises at least one organosilicon crosslinker H-XL containing at least three silicon-bonded hydrogen atoms per molecule. In some embodiments, the organosilicon crosslinker H-XL containing at least three silicon-bonded hydrogen atoms per molecule is an organohydrogenopolysiloxane containing from 10 to 500 silicon atoms in each molecule, preferably from 10 to 250 silicon atoms in each molecule.
[0063] The optional organosilicon crosslinker H-XL may be included in curable silicone adhesive composition X in an amount by weight of the total composition of from about 0.01% to about 5%, preferably from about 0.05% to about 2%, preferably from about 0.1% to about 1%. According to one embodiment, curable silicone adhesive composition X does not include organosilicon crosslinker H-XL.
[0064] In some embodiments, the organosilicon crosslinker H-XL is selected such that the ratio α (d / (ΣSi)) is in the range of 0.01<α<0.957, where d=the number of H atoms directly bonded to Si atoms per molecule and ΣSi is the total number of silicon atoms per molecule. In preferred embodiments, the ratio α is in the range of 0.10<α<0.75. In other preferred embodiments, the ratio a is in the range of 0.15<α<0.30.
[0065] The organosilicon crosslinker H-XL preferably contains 0.45 to 40% by weight SiH, more preferably 0.5 to 35% by weight SiH, more preferably 0.5 to 15% by weight SiH, or 3 to 13% by weight SiH.
[0066] In some embodiments, the organosilicon crosslinker H-XL comprises: (i) at least three siloxy units of the formula (XL-1), which may be the same or different: [ka] During the ceremony, H represents a hydrogen atom, Z represents an alkyl group containing 1 to 8 carbon atoms; e is equal to 0, 1, or 2; and / or (ii) at least one, preferably 1 to 550, siloxy units of formula (XL-2): [ka] During the ceremony, Z is an alkyl group having 1 to 8 carbon atoms, or a C6 to C6 alkyl group such as xylyl, tolyl, or phenyl group. 12 represents an aryl group, preferably an alkyl group, g is equal to 0, 1, 2, or 3.
[0067] In some embodiments, Z in XL-1 and / or XL-2 is selected from methyl, ethyl, and propyl groups, cycloalkyl groups such as cyclohexyl, cycloheptyl, or cyclooctyl groups, and aryl groups such as xylyl, tolyl, and phenyl groups. Preferably, Z is a methyl group. However, Z in XL-1 and XL-2 may be the same or different.
[0068] In a preferred embodiment, e in XL-1 is 1 or 2.
[0069] In a preferred embodiment, g in XL-2 is 2.
[0070] In a preferred embodiment, the organosilicon crosslinker H-XL contains from 3 to 60 siloxy units of formula (XL-1) and from 1 to 250 siloxy units of formula (XL-2).
[0071] The amounts of alkenyl-containing organopolysiloxane A, diorganohydrogensiloxy-terminated diorganopolysiloxane CE, diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL, and optional organosilicon crosslinker H-XL contained in curable silicone adhesive composition X of the present invention are determined so that: 1) the molar ratio of hydrogen atoms to alkenyl groups in the silicone elastomer (RHalk) is 1.05 to 1.40, 2) the percentage of the number of moles of hydrogen atoms bonded directly to silicon atoms of CE out of the number of moles of hydrogen atoms bonded directly to silicon atoms of both CE and H-XL combined (RHCE) is 90% to 100%, and 3) the percentage of the number of moles of alkenyl groups bonded directly to silicon atoms of A out of the total number of moles of alkenyl groups bonded directly to silicon atoms in composition X (RAlkA) is 80% to 95%.
[0072] The molar ratio of hydrogen atoms to alkenyl groups (RHalk) can be determined using the following formula: RHalk=nH / tAlk During the ceremony, nH is the number of moles of hydrogen atoms directly bonded to silicon atoms in the curable silicone adhesive composition X, tAlk is the number of moles of alkenyl groups directly bonded to silicon atoms in the curable silicone adhesive composition X.
[0073] In the curable silicone adhesive composition X of the present invention, the value of RHalk is preferably 1.05 to 1.40. When the value of RHalk is less than 1.05, it has been confirmed that the resulting cured composition Z has a gel-like structure. Similarly, when the value of RHalk is 1.40 or more, the network of the resulting cured composition Z has too strong crosslinking, resulting in non-uniform cohesive failure and elongation of the resulting cured composition. Preferably, in the curable silicone adhesive composition X of the present invention, the value of RHalk is 1.05 < RHalk < 1.40. Alternatively, in the curable silicone adhesive composition X of the present invention, the value of RHalk is 1.05 < RHalk ≤ 1.30. In another alternative, in the curable silicone adhesive composition X of the present invention, the value of RHalk is 1.05 < RHalk ≤ 1.30. In another alternative, in the curable silicone adhesive composition X, the value of RHalk is 1.15 ≤ RHalk ≤ 1.25.
[0074] In addition to the RHalk value, the mole percentage of hydrogen atoms directly bonded to silicon atoms of the diorganohydrosiloxy-terminated diorganopolysiloxane CE with respect to the hydrogen atoms directly bonded to silicon atoms of both CE and the organosilicon crosslinking agent H-XL (i.e., the RHCE value) is another important feature of the curable silicone adhesive composition X of the present invention.
[0075] The mole percentage RHCE can be determined using the following formula: RHCE = nHCE / (nHCE + nHXL) × 100 In the formula, nHCE is the number of moles of hydrogen atoms directly bonded to silicon atoms of the diorganohydrosiloxy-terminated diorganopolysiloxane CE, nHXL is the number of moles of hydrogen atoms directly bonded to silicon atoms of the organosilicon crosslinking agent H-XL.
[0076] According to an embodiment, the value of RHCE is advantageously within the range 85%≦RHCE≦100%, preferably 90%≦RHCE≦100%, more preferably 90%≦RHCE≦99.5%.
[0077] In addition to the values of RHalk and RHCE, the mole percentage of alkenyl groups bonded directly to silicon atoms in the alkenyl-containing organopolysiloxane A relative to the alkenyl groups bonded directly to silicon atoms in the total composition X (i.e., the RAlkA value) is another important feature of the curable silicone adhesive composition X of the present invention.
[0078] The mole percentage of RAlkA can be determined using the following formula: RAlkA = (nAlkA / tAlk) × 100 During the ceremony, nAlkA is the number of moles of alkenyl groups directly bonded to silicon atoms in the alkenyl-containing organopolysiloxane A, tAlk is the number of moles of alkenyl groups bonded directly to silicon atoms in the curable silicone composition X.
[0079] The value of RAlkA is advantageously within the range 80%≦RAlkA<95%, 85%≦RAlkA<95%, 86%≦RAlkA≦93%, 87%≦RAlkA≦92%, or 87%≦RAlkA≦91%.
[0080] The curable silicone adhesive composition X of the present invention further comprises at least one addition reaction catalyst C. The addition reaction catalyst C can be contained in any amount that allows the composition to be cured. For example, the addition reaction catalyst C can be contained in an amount such that the amount of platinum group metal in the catalyst C is 0.01 to 500 parts by weight per 1 million parts by weight of the alkenyl group-containing organopolysiloxane A and the diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL.
[0081] Catalyst C can be selected from platinum and rhodium compounds in particular.In particular, it is possible to use platinum complexes and organic products (described in US Pat. No. 3,159,601, US Pat. No. 3,159,602, US Pat. No. 3,220,972, and European patents EP-A-0057459, EP-A-0118978, EP-A-0190530), platinum and vinylorganosiloxane complexes (described in US Pat. No. 3,419,593, US Pat. No. 3,715,334, US Pat. No. 3,377,432, and US Pat. No. 3,814,730).In a preferred embodiment, addition reaction catalyst C is a platinum group metal-containing catalyst.
[0082] The curable silicone adhesive composition X further comprises at least one reinforcing inorganic filler F1. In a preferred embodiment, the at least one reinforcing mineral filler F1 is ground quartz, preferably natural ground silicon dioxide having a particle size of about 5 μm.
[0083] In some embodiments, the at least one reinforcing mineral filler F1 is selected from silica and / or alumina, preferably from silica.
[0084] For usable silicas, the filler is assumed to be characterized by a fine particle size, often below 0.1 μm, and a high ratio of specific surface area to weight, generally within the range of about 50 square meters per gram to more than 300 square meters per gram. This type of silica is a commercially available product and is well known in the field of manufacturing adhesive silicone compositions. These silicas can be colloidal silicas, pyrogenically prepared silicas (silicas called combustion or fumed silicas), or silicas prepared by wet process (precipitated silicas) of mixtures of these silicas.
[0085] Of course, various cuts of silica are also available.
[0086] These silica powders generally have an average particle size of 0.1 μm or less and a BET specific surface area of 50 m2 / g, preferably 50 to 400m 2 / g, especially 150~350m 2 / g.
[0087] These silicas are optional: It is pretreated with the aid of at least one compatibilizer selected from a group of molecules that meet at least two criteria: Has high interaction with silica in the area of hydrogen bonding with itself and with the surrounding silicone oil; As such, or their decomposition products, they are easily removed from the final mixture by heating under vacuum in a gas stream; low molecular weight compounds are preferred; and / or In a specific manner with the aid of at least one silica, and / or in a complementary manner by using at least one compatibilizer of similar nature to those defined above, which can be used in the pretreatment, It is processed on site.
[0088] In situ treatment of the silica filler is understood to mean placing the filler and the compatibilizer in the presence of at least a portion of the predominant silicone polymer A mentioned above.
[0089] The compatibilizer is selected according to the treatment method (pre-treatment or in situ) and may be selected, for example, from the group comprising: Chlorosilanes, Polyorganocyclosiloxanes such as octamethylcyclosiloxane (D4); Silazane, preferably disilazane, or mixtures thereof, hexamethyldisilazane (HMDZ) is a preferred silazane, which can be combined with divinyltetramethyldisilazane. an organopolysiloxane having one or more silicon-bonded hydroxyl groups per molecule; an amine such as ammonia or a low molecular weight alkylamine such as diethylamine; low molecular weight organic acids such as formic acid and acetic acid, and mixtures thereof.
[0090] In some embodiments, the treated fumed silica contains 0-0.7% reactive alkenyl groups, such as vinyl groups, derived from a compatibilizer.
[0091] In a preferred embodiment, the compatibilizer does not contain reactive alkenyl groups, such as vinyl groups.
[0092] For in situ treatments, the compatibilizer is preferably used in the presence of water.
[0093] For more information on this matter, reference may be made, for example, to patent FR-B-2764894.
[0094] As a variant, it is possible to use prior art compatibilization methods which provide for early treatment with silazanes (eg FR-A-2320324) or delayed treatment (eg EP-A-462032).
[0095] As reinforcing aluminas that can be used as filler E, highly dispersible aluminas are advantageously used, which may or may not be doped in a known manner. Of course, it is also possible to use different cuts of alumina. As non-limiting examples of such aluminas, reference may be made to aluminas A125, CR125, D65CR from the Baikowski Company.
[0096] Preferably, the at least one reinforcing mineral filler F1 is ground quartz and / or treated fumed silica. If treated fumed silica is included, it is preferred that the treated fumed silica does not contain reactive vinyl groups.
[0097] In terms of weight, it is preferred to use a reinforcing mineral filler F1 in an amount of 5-50%, preferably 10-40%, more preferably 12-30%, by weight, based on the total components of composition X. In some embodiments, the reinforcing mineral filler F1 is a combination of ground quartz in an amount of 3-20% by weight, preferably 4-12% by weight (based on the total components of composition X), and treated fumed silica in an amount of 10-20% by weight (based on the total components of composition X).
[0098] According to the invention, the use of complementary fillers F2, such as thermally conductive fillers and / or electrically conductive fillers, can be envisaged.
[0099] The curable silicone adhesive composition X of the present invention may also contain at least one cure rate modifier G. The cure rate modifier G may for example be a crosslinking inhibitor G1 and / or a crosslinking retarder G2.
[0100] Crosslinking inhibitors are also well known. Examples of crosslinking inhibitors G1 that can be used as cure rate regulators G include: polyorganosiloxanes, advantageously cyclic and substituted with at least one alkenyl group, tetramethylvinyltetrasiloxane being particularly preferred; Pyridine, Phosphines and organic phosphites, Unsaturated amides, Alkylated maleates, Acetylenic alcohol.
[0101] These acetylenic alcohols (see FR-B-1528464 and FR-A-2372874) form part of the preferred thermal blockers for the hydrosilylation reaction and have the formula: [ka] During the ceremony: R is a linear or branched alkyl radical, or a phenyl radical; R' is H or a linear or branched alkyl radical, or a phenyl radical; The radicals R, R' and the carbon atom alpha to the triple bond may form a ring; The total number of carbon atoms contained in R and R' is at least 5, and preferably 9-20.
[0102] The alcohols are preferably chosen with a boiling point of about 250° C. By way of example, mention may be made of: 1-ethynyl-1-cyclohexanol (ECH); Methyl-3 dodecyn-1ol-3; Trimethyl-3,7,11-dodecyn-1-ol-3; Diphenyl-1,1-propyn-2-ol-1 Ethyl-3 ethyl-6 nonynoyl-3; Methyl-3-pentadecyn-1-ol-3. These α-acetylenic alcohols are commercially available.
[0103] Such modifiers are present in an amount up to 2,000 ppm, preferably 20 to 50 ppm, based on the total weight of organopolysiloxanes A, CE, Alk-XL, and H-XL.
[0104] Examples of crosslinking retarders G2 that can be used as curing rate regulator G include so-called inhibitors for controlling the crosslinking reaction and extending the pot life of the silicone composition. Examples of advantageous crosslinking retarders G2 that can be used as curing rate regulator G include, for example, vinyl siloxane, 1,3-divinyltetramethyldisiloxane, or tetravinyl-tetramethyl-tetracyclosiloxane. It is also possible to use other known inhibitors, such as ethynylcyclohexanol, 3-methylbutynol, or dimethyl maleate.
[0105] The curable silicone adhesive composition X of the present invention may also comprise one or more of the following optional ingredients, optionally at least one rheology modifier H, at least one adhesion promoter I, and / or at least one functional additive J to impart specific properties.
[0106] Examples of rheology modifiers H that can be used include, for example, epoxy functional silanes, poly(aryl)siloxanes, polyalkylene glycols, polyester polyols, polyhydric alcohols, dicarboxylic acids, polyester diols, and silicone polyethers such as silicone polyether block copolymers, free polyethers, and mixtures thereof, such as, for example, BLUESIL SP-3300 (siloxane and silicone, di-Me, 3-hydroxypropyl Me, ethoxylated propoxylated; Elkem Silicones).
[0107] Examples of adhesion promoters I include, for example, epoxy-functional organotitanates or amino-functional organosilicons. In a preferred embodiment, the adhesion promoter (I) compound is a mixture of: - (1.1) at least one alkoxyorganosilane containing at least one C2-C6 alkenyl group per molecule, (I.2) at least one organosilicon compound containing at least one epoxy group, and - (1.3) at least one metal chelate M and / or metal alkoxide of the general formula: M(OJ)n During the ceremony, -M is selected from the group formed by Ti, Zr, Ge, Li, Mn, Fe, Al, and Mg; -n=valence of M, J=linear or branched Ci-Ce alkyl.
[0108] According to the invention, advantageous combinations of adhesion promoters are: vinyltrimethoxysilane (VTMO) of formula (I.1), 3-glycidoxypropyltrimethoxysilane (GLYMO) of formula (I.2), and - butyl titanate of the formula (I.3):
[0109] Examples of additives J that can be used include organic dyes or pigments, stabilizers introduced into silicone rubber to improve thermal stability, resistance to hot air, reversion, depolymerization under attack by traces of acid or water at high temperatures, plasticizers, release oils, or hydrophobizing oils without reactive alkenyl or SiH groups, such as polydimethylsiloxane oils, release agents such as fatty acid derivatives, fatty alcohol derivatives, fluoroalkyls, and compatibilizers such as hydroxylated silicone oils.
[0110] Curable silicone adhesive composition X may be cured by any suitable method at any suitable temperature. For example, curable silicone adhesive composition X may be cured at room temperature (about 20-25°C) or higher. In some embodiments, curable silicone adhesive composition X may be cured at 50°C or higher, 80°C or higher, 100°C or higher, 120°C or higher, or 150°C or higher. In some embodiments, curable silicone adhesive composition X cures at room temperature upon mixing.
[0111] The curing reaction may proceed for any length necessary to obtain a suitable cured silicone adhesive elastomer Z according to the present invention. One skilled in the art will readily appreciate that the length of the reaction may vary depending on the reaction temperature, among other variables. In some embodiments, the curable silicone adhesive composition X is cured at room temperature for about 1 day. In other embodiments, the curable silicone adhesive composition X is cured at ≧100° C. for about 5 minutes. In some embodiments, the curable silicone adhesive composition X is cured at about 80° C. for about 2 minutes.
[0112] The cured silicone adhesive elastomers Z of the present invention exhibit elongation at break values of at least 1200%, as measured by any standard test known in the art, such as ASTM D-412. Alternatively, the cured silicone adhesive elastomers Z of the present invention exhibit elongation at break values of at least 1300%, at least 1400%, at least 1500%, at least 1600%, at least 1700%, at least 1800%, at least 1900%, or at least 2000%.
[0113] In some embodiments, the cured silicone adhesive elastomers Z of the present invention exhibit elongation at break values of up to 5000%. Alternatively, the cured silicone elastomers Z of the present invention exhibit elongation at break values of up to 4000%, up to 3000%, up to 2500%, or up to 2000%.
[0114] In some embodiments, the cured silicone adhesive elastomers Z of the present invention exhibit elongation at break values of 1200% to 5000%. In other embodiments, the cured silicone elastomers Z of the present invention exhibit elongation at break values of 1200% to 1400%, 1200% to 1500%, 1200% to 1600%, 1200% to 1700%, 1200% to 1800%, 1200% to 2000%, 1200% to 2500%, 1200% to 3000%, 1200% to 4000%, or 1200% to 5000%. In other embodiments, the cured silicone elastomer Z of the present invention exhibits an elongation at break value of 1300% to 1400%, 1300% to 1500%, 1300% to 1600%, 1300% to 1700%, 1300% to 1800%, 1300% to 2000%, 1300% to 2500%, 1300% to 3000%, 1300% to 4000%, or 1300% to 5000%. In other embodiments, the cured silicone elastomers Z of the present invention exhibit elongation values at break of 1400% to 1500%, 1400% to 1600%, 1400% to 1700%, 1400% to 1800%, 1400% to 2000%, 1400% to 2500%, 1400% to 3000%, 1400% to 4000%, or 1400% to 5000%. In other embodiments, the cured silicone elastomers Z of the present invention exhibit elongation values at break of 1500% to 2000%, 1500% to 2500%, 1500% to 3000%, 1500% to 4000%, or 1500% to 5000%. In other embodiments, the cured silicone elastomers Z of the present invention exhibit elongation values at break of 1700% to 2000%, 1700% to 2500%, 1700% to 3000%, 1700% to 4000%, or 1700% to 5000%. In other embodiments, the cured silicone elastomers Z of the present invention exhibit elongation values at break of 1800% to 2000%, 1800% to 2500%, 1800% to 3000%, 1800% to 4000%, or 1800% to 5000%. In other embodiments, the cured silicone elastomers Z of the present invention exhibit elongation values at break of 2000% to 2500%, 2000% to 3000%, 2000% to 4000%, or 2000% to 5000%. In other embodiments, the cured silicone elastomers Z of the present invention exhibit elongation at break values of from 2500% to 3000%, from 2500% to 4000%, or from 2500% to 5000%.
[0115] In some embodiments, the cured silicone adhesive elastomer Z of the present invention exhibits a tensile strength of at least about 150 psi (1.03 MPa), at least about 200 psi (1.37 MPa), at least about 250 psi (1.72 MPa), at least about 300 psi (2.06 MPa), or at least about 350 psi (2.41 MPa).
[0116] For example, the cured silicone adhesive elastomer Z of the present invention may have a viscosity of about 150 psi (1.03 MPa) to about 1300 psi (8.96 MPa), about 150 (1.03 MPa) to about 1200 psi (8.27 MPa), about 150 (1.03 MPa) to about 1100 psi (7.58 MPa), about 150 (1.03 MPa) to about 1000 psi (6.89 MPa), about 150 (1.03 MPa) to about 900 psi (6.21 MPa), about 150 (1.03 MPa) to about 1000 psi (6.89 MPa), about 150 (1.03 MPa) to about 1000 psi (6.21 ... 3MPa) to about 800psi (5.52MPa), about 150 (1.03MPa) to about 700psi (4.83MPa), about 150 (1.03MPa) to about 600psi (4.13MPa), about 200 (1.37MPa) to about 1300psi (8.96MPa), about 200 (1.37MPa) to about 1200psi (8.27MPa), about 200 (1.37MPa) to about 1100psi (7.58MPa), about 200 (1.37MPa) to about 1000psi (6.89MPa), about 200 (1.37MPa) to about 900psi (6.21MPa), about 200 (1.37MPa) to about 800psi (5.52MPa), about 200 (1.37MPa) to about 700psi (4.83MPa), about 200 (1.37MPa) to about 600psi (4.13MPa), about 250psi (1.72MPa) to about 600psi (4.13MPa), about 300psi (2.06MPa) to about 600 The tensile strength may be about 350 psi (2.41 MPa) to about 600 psi (4.13 MPa), about 400 psi (2.75 MPa) to about 600 psi (4.13 MPa), about 450 psi (3.10 MPa) to about 600 psi (4.13 MPa), about 500 psi (3.44 MPa) to about 600 psi (4.13 MPa), or about 550 psi (3.79 MPa) to about 600 psi (4.13 MPa).In other embodiments, the cured silicone adhesive elastomer Z of the present invention has a viscosity of from about 150 psi (1.03 MPa) to about 200 psi (1.37 MPa), from about 200 psi (1.37 MPa) to about 250 psi (1.72 MPa), from about 250 psi (1.72 MPa) to about 300 psi (2.06 MPa), from about 300 psi (2.06 MPa) to about 350 psi (2.41 MPa), or from about 350 psi (2.41 MPa). (2.41 MPa) to about 400 psi (2.75 MPa), about 400 psi (2.75 MPa) to about 450 psi (3.10 MPa), about 450 psi (3.10 MPa) to about 500 psi (3.44 MPa), about 500 psi (3.44 MPa) to about 550 psi (3.79 MPa), or about 550 psi (3.79 MPa) to about 600 psi (4.13 MPa).
[0117] In some embodiments, the cured silicone adhesive elastomers Z of the present invention exhibit a peel strength of at least 40 N / cm, measured according to the peel test method of standard JIS K 6854. For example, the cured silicone adhesive elastomers Z of the present invention can exhibit a peel strength of about 40 N / cm to about 85 N / cm, measured according to the peel test method of standard JIS K 6854.
[0118] In some embodiments, the cured silicone adhesive elastomer Z exhibits at least partial cohesive failure. In some embodiments, the cured silicone adhesive elastomer Z of the present invention exhibits at least 50%, at least 60%, at least 70%, at least 80%, at least 85%, at least 90%, at least 95%, at least 96%, at least 97%, at least 98%, or at least 99% cohesive failure. In some embodiments, the cured silicone adhesive elastomer Z of the present invention exhibits 100% cohesive failure.
[0119] The invention also relates to a method for adhesively bonding at least two substrates S1 and S2, the method comprising the steps of: Preparing a curable silicone composition X as described above; applying a curable silicone composition X to at least one of the surfaces of S1 and / or S2 to form at least one adhesively coated surface; Assembling substrates S1 and S2 such that at least one adhesive coated surface forms a bond between the at least two substrates S1 and S2; Optionally, applying pressure to the at least one adhesive coated surface; and Optionally, heating the assembled substrates S1 and S2. Includes.
[0120] The heating temperature is preferably less than 190° C. and the heating time is less than 30 minutes. In some embodiments, the heating temperature is about 100° C. and the heating time is less than 30 minutes, preferably about 20 minutes, more preferably about 10 minutes, 5 minutes, 2 minutes or less. In some embodiments, the heating temperature is about 85° C. and the heating time is less than 30 minutes, preferably about 20 minutes, more preferably about 15 minutes, 10 minutes, 5 minutes, 2 minutes or less.
[0121] The substrates S1 and S2 to be assembled are preferably flexible and may be selected from the group comprising textiles, non-woven fibrous substrates, polymeric films, in particular polyesters, polyamides, polyolefins, polyurethanes and silicone polyvinyl chlorides. The substrates S1 and S2 may be made of glass.
[0122] According to a variant, at least one of the surfaces S1 and / or S2 comprises a silicone, preferably an elastomeric silicone, which advantageously forms a coating on said substrate. A curable silicone adhesive composition X is then applied to the silicone. Such elastomeric silicone compositions are well known to those skilled in the art and do not require a detailed description.
[0123] Curable silicone adhesive composition X according to the present invention is applied to obtain an adhesive having a thickness of at least 0.1 mm, preferably from about 0.3 mm to about 1.5 mm, and more preferably from about 0.5 mm to about 1.0 mm.
[0124] The field of application of the recommended use of the present invention is that of the assembly of inflatable bags for protecting vehicle occupants, advantageously assembled by gluing and sewing, the substrates S1 and S2 being the two parts constituting the bag, and the curable silicone adhesive composition X according to the invention being applied to at least one of the surfaces of S1 and / or S2 in the area of the stitching.
[0125] When the curable silicone adhesive composition X of the present invention is crosslinked by heating, the step of heating said composition X is preferably carried out before sewing the substrates S1 and S2 together.
[0126] The present invention also relates to the use of the above curable silicone adhesive composition X as an adhesive and / or leak-proof joint for the stitching of two substrates S1 and S2 assembled by sewing. There is also provided the use of the above curable silicone adhesive composition X as, for example, a joint sealant in the manufacture of inflatable bags, such as airbags.
[0127] The present invention also relates to an inflatable bag for protecting vehicle occupants, which is made of two parts that are sewn together, adhesively bonded and / or leak-proofed in the area of the seam with the curable silicone adhesive composition described above.
[0128] Other advantages provided by the present invention will become apparent from the following illustrative examples. EXAMPLES
[0129] Materials and Methods Preparation of Silicone Composition In the examples below, the following ingredients were used: A1: Linear α,ω-vinylpolydimethylsiloxane (average viscosity 20000 mPa s; Mn = 49,000 g / mol) A2: Linear α,ω-vinylpolydimethylsiloxane (average viscosity 3500 mPa s; Mn = 27,000 g / mol) A3: Linear α,ω-vinylpolydimethylsiloxane (average viscosity 1000 mPa s; Mn = 18,000 g / mol) CE: α,ω-hydridopolydimethylsiloxane (H-PDMS-H) (viscosity 7-10 mPa s; Mn = 750 g / mol) Alk-XL1: Vinyldimethyl terminated (vinylmethylsiloxane)-dimethylsiloxane copolymer gum (total vinyl content 0.04-0.06 wt%, viscosity >500,000 mPa·s, Mn=220,000 g / mol) Alk-XL2: Trimethyl-terminated (vinylmethylsiloxane)-dimethylsiloxane copolymer gum (total vinyl content 0.0675-0.0825 wt%; viscosity >500,000 mPa·s; Mn=220,000 g / mol) Alk-XL3: Vinyldimethyl terminated polydimethylsiloxane gum (total vinyl content 0.009-0.017 wt%, viscosity >500,000 mPa·s, Mn=220,000 g / mol) H-XL: Trimethyl-terminated (methylhydrogensiloxane)-dimethylsiloxane copolymer (viscosity 6-12 mPa·s; 9.5-11.0 wt% SiH) C: Platinum catalyst solution: Platinum metal diluted in short linear α,ω-vinyl polydimethylsiloxane oil (wt% in platinum=10) F1a: Ground Quartz (MIN-U-SIL(R)5) F1b: In-situ treated hydrophilic fumed silica (AEROSIL® 300 treated with hexamethyldisilazane) F1c: In-situ treated hydrophilic fumed silica (AEROSIL® 300 treated with hexamethyldisilazane and divinyltetramethyldisilazane) G: ECH (1-ethynyl-1-cyclohexanol) H: Non-hydrolyzable silicone polyether copolymer (BLUESILSP-3300) J1: Blue pigment J2: Red pigment
[0130] Adhesive properties a) Mechanical properties Cured slabs of silicone rubber were prepared by curing the silicone adhesive compositions under pressure at 25°C for 24 hours before testing. The following mechanical properties were evaluated: durometer Shore A / Shore OO, tensile strength, elongation at break, tear strength, and modulus (according to the method described in standard ASTM D412). Some cured silicone rubber compositions did not break at the maximum elongation achievable by the testing equipment. In these cases, it was not possible to calculate the actual elongation at break and tensile strength values, so the elongation at break and tensile strength values were calculated at the maximum elongation achieved and are reported in the tables below with a greater than sign (>).
[0131] b) Adhesive strength The silicone adhesive composition is applied at a rate of 25 to 35 g / m 2 The silicone rubber coated nylon tape was applied in the form of a 50 mm wide strip onto a nylon substrate coated with silicone rubber of 1000 g. The silicone rubber coated nylon substrate was then overlaid on top of the nylon substrate to which the silicone rubber composition had been applied, such that the silicone adhesive composition formed a layer of 0.5-1 mm thickness between the silicone rubber coated nylon substrates. The coated substrate was cured for 24 hours at 25°C. The resulting silicone rubber coated nylon tape was then subjected to a T-shaped peel test at a peel rate of 4 in / min according to the peel test method of standard JIS K6854 to measure the adhesion to the silicone rubber. The load (peel force or peel strength) was also measured. The type of break obtained was also recorded as the percentage of adhesion or cohesive A / C.
[0132] Example 1 - Exemplary Compositions of the Invention Three compositions according to the invention, as described in Table 1, were prepared by mixing parts A and B in a 1:1 weight ratio and curing at room temperature for one day. The resulting cured silicone adhesive elastomers Z were tested using standard ASTM D-412 and standard JIS K6854 as described above.
[0133] [Table 1]
[0134] Example 2 - Effect of Varying Organopolysiloxane Gum Crosslinker To test the effect of varying the vinyl content and / or the position of the vinyl groups in the organopolysiloxane gum crosslinker Alk-XL on the properties of the silicone adhesive, five comparative compositions, listed in Table 2, were prepared by mixing parts A and B in a 1:1 weight ratio and curing at room temperature for one day. The resulting cured silicone adhesive elastomers Z were tested using standard ASTM D-412 and standard JIS K6854 as described above.
[0135] [Table 2]
[0136] As shown in Table 2, replacement of an organopolysiloxane gum crosslinker containing terminal and internal vinyl groups (Alk-XL1) with other organopolysiloxane gums with a total vinyl content of 0.04-0.06 wt% degraded the performance of the resulting silicone adhesives. Specifically, both peel strength and cohesive failure were adversely affected by the use of a methyl-terminated gum containing internal vinyl groups (Alk-XL2) with a total vinyl content of 0.0675-0.0825 wt%.
[0137] The use of vinyl-terminated gums without internal vinyl groups (total vinyl content 0.009–0.017 wt %; Alk-XL3) or gums without vinyl groups (e.g., polydimethylsiloxane gum (viscosity >500,000 mPa·s; Mn = 220,000 g / mol); data not shown) resulted in silicone adhesives that failed to cure.
[0138] Similarly, removal of Alk-XL (Comparative 5), such that the RAlkA value increased to 100%, resulted in a composition that failed to cure.
[0139] Example 3 – Effect of various quartz fillers To test the effect of varying the amount of ground quartz filler (F1a), three additional exemplary compositions, listed in Table 3, were prepared by mixing parts A and B in a 1:1 weight ratio and curing at room temperature for one day. The resulting breathable silicone adhesive elastomers Z were tested using standard ASTM D-412 and standard JIS K6854 as described above.
[0140] [Table 3]
[0141] The addition of ground quartz (F1a) significantly improved the mechanical properties of the cured silicone adhesive elastomer, as shown in Table 3. Optimal conditions could be reached.
[0142] Additionally, the compositions containing crushed quartz exhibited superior peel strength compared to compositions in which the crushed quartz (F1a) was replaced with calcium carbonate (precipitated calcium carbonate (ALBACAR® 5970)).
[0143] Example 4 - Effect of Variations in Treated Fumed Silica To test the effect of varying the treatment of the fumed silica, two comparative compositions, listed in Table 4, were prepared by mixing parts A and B in a 1:1 weight ratio and curing at room temperature for one day. The resulting cured silicone adhesive elastomer Z was tested using standard ASTM D-412 and standard JIS K6854 as described above.
[0144] [Table 4]
[0145] As shown in Table 4, the use of fumed silica treated with both hexamethyldisilazane and divinyltetramethyldisilazane (F1c) resulted in an RAlkA <80% and adversely affected the mechanical properties of the resulting silicone adhesive. Thus, the presence of vinyl groups on the fumed silica appears to adversely affect the adhesive properties of the resulting composition.
[0146] Example 5 - Effect of changing RHalk value To test the effect of varying the RHalk value, three comparative compositions and three additional exemplary compositions, as set forth in Table 5, were prepared by mixing parts A and B in a 1:1 weight ratio and curing at room temperature for one day. The resulting cured silicone adhesive elastomers Z were tested using standard ASTM D-412 and standard JIS K6854 as described above.
[0147] [Table 5]
[0148] As shown in Table 5, increasing the molar ratio of hydrogen atoms to alkenyl groups in the silicone composition (RHalk) to 1.40 adversely affected the mechanical properties of the resulting silicone adhesive. Similarly, decreasing the molar ratio of hydrogen atoms to alkenyl groups in the silicone composition (RHalk) to 1.05 or less adversely affected the mechanical properties of the resulting silicone adhesive.
[0149] Example 6 - Effect of cure temperature / time Two exemplary silicone adhesive compositions of the present invention were prepared using a 25-35 g / m 2 The composition was applied in the form of a 50 mm wide strip onto a nylon substrate coated with silicone rubber of 1000 g. The silicone rubber coated nylon fabric was then overlaid on top of the nylon fabric to which the silicone rubber composition had been applied, as described in the above examples, such that the silicone adhesive composition formed a layer 0.5-1 mm thick between the silicone rubber coated nylon fabrics. However, instead of curing the composition at 25°C for 24 hours, the composition was cured at 85°C for 20 minutes. The adhesive strength to the silicone rubber was then measured as described above.
[0150] Both of the exemplary silicone adhesive elastomers tested cured at 85° C. for 20 minutes exhibited 100% cohesive failure and peel strengths of over 40 N / cm, demonstrating that the silicone adhesive compositions of the present invention can be rapidly cured by relatively moderate increases in temperature without compromising the adhesive properties of the resulting composition.
[0151] All references cited herein are incorporated by reference as if each reference was specifically and individually indicated to be incorporated by reference. The citation of a reference is for its disclosure prior to the filing date and should not be construed as an admission that the present disclosure is not entitled to antedate such reference by virtue of prior invention.
[0152] It is understood that each of the above elements, or a collection of two or more, may also find useful application in other types of methods different from the types described above. Without further analysis, the foregoing fully reveals the gist of the present disclosure so that others can easily adapt it to various applications by applying their current knowledge without omitting features that, in the light of the prior art, fairly constitute essential features of the general or specific aspects of the present disclosure as set forth in the appended claims. The above-described embodiments are presented only as examples. The scope of the present disclosure should be limited only by the following claims.
Claims
1. A curable silicone composition X, (A) at least two silicon bonds C per molecule 2 ~C 20 At least one alkenyl-containing organopolysiloxane A having an alkenyl group; (B) at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender CE; (C) at least three silicon bonds C per molecule 2 ~C 20 at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL, which contains alkenyl groups; (D) optionally, at least one organosilicon crosslinker, H-XL, containing at least three silicon-bonded hydrogen atoms per molecule; (e) at least one addition reaction catalyst C; (F) at least one reinforcing mineral filler F1, (G) optionally, at least one complementary filler F2; (H) optionally at least one cure rate modifier G; (I) optionally at least one rheology modifier H; (J) optionally at least one adhesion promoter I; and (K) Optionally, at least one functional additive to impart a particular property J. Including, At least 3 silicon bonds per molecule 2 ~C 20 said at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL containing alkenyl groups has a total alkenyl content of 0.02 to 0.10 weight percent; The amounts of the alkenyl group-containing organopolysiloxane A, the diorganohydrogensiloxy-terminated diorganopolysiloxane CE, the diorganohydrogensiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL, and optionally the organosilicon crosslinker H-XL are determined to result in a curable silicone composition X: 1) the value of the ratio RHalk is 1.05<RHalk<1.40, where RHalk=nH / tAlk, and a) nH is the number of moles of hydrogen atoms directly bonded to silicon atoms in the curable silicone composition X, b) tAlk is the number of moles of alkenyl groups bonded directly to silicon atoms in the curable silicone composition X; 2) the percent molar ratio RHCE is in the range of 90%≦RHCE≦100%, where RHCE=nHCE / (nHCE+nHXL)×100; and a) nHCE is the number of moles of hydrogen atoms directly bonded to silicon atoms of the diorganohydrogensiloxy-terminated diorganopolysiloxane CE; b) nHXL is the number of moles of hydrogen atoms directly bonded to silicon atoms of the organosilicon crosslinker H-XL; 3) the percent molar ratio RAlkA is in the range 80%<RAlkA<95%, where RAlkA=(nAlkA / tAlk)×100; and a) nAlkA is the number of moles of alkenyl groups bonded directly to silicon atoms of organopolysiloxane A; b) tAlk is the number of moles of alkenyl groups bonded directly to silicon atoms in the curable silicone composition X.
2. At least two silicon bonds C per molecule 2 ~C 20 The at least one alkenyl-containing organopolysiloxane A having an alkenyl group is represented by the following formula (1): [Formula 1] where: -n is an integer from 1 to 1000, -R is independently C such as methyl, ethyl, propyl, etc. 1 ~C 20 C alkyl groups, or xylyl, tolyl, or phenyl groups, etc. 6 ~C 12 C such as an aryl group, or a vinyl, allyl, hexenyl, decenyl, or tetradecenyl group 2 ~C 20 alkenyl groups, -R' is independently a C alkyl group such as a vinyl, allyl, hexenyl, decenyl, or tetradecenyl group. 2 ~C 20 alkenyl groups, -R" is independently a C alkyl group such as methyl, ethyl, or propyl. 1 ~C 20 C alkyl groups, or xylyl, tolyl, or phenyl groups 6 ~C 12 aryl groups, The curable silicone composition according to claim 1.
3. At least two silicon bonds C per molecule 2 ~C 20 The at least one alkenyl-containing organopolysiloxane A having an alkenyl group is represented by the following formula (1): [Case 2] where: -n is an integer from 1 to 1000, -R is a methyl group; -R' is a vinyl group, -R" is a methyl group; The curable silicone composition X according to claim 1 or 2.
4. The at least one diorganohydrogensiloxy-terminated diorganopolysiloxane chain extender CE has the following formula (2): [C3] where: -R is independently C 1 ~C 20or a C alkyl group such as xylyl, tolyl, or phenyl. 6 ~C 12 and wherein the aryl group is selected from the group consisting of - n is an integer from 1 to 500; The curable silicone composition X according to any one of claims 1 to 3.
5. At least 3 silicon bonds per molecule 2 ~C 20 The curable silicone composition X according to any one of claims 1 to 4, wherein the at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL containing alkenyl groups comprises at least three siloxy units of formula (A-3) and other siloxy units of formula (A-2): [C4] In the formula, the symbol "Alk" represents a C alkyl group such as vinyl, allyl, hexenyl, decenyl, or tetradecenyl group. 2 ~C 20 It represents an alkenyl group, and the symbol R is C, such as methyl, ethyl, or propyl. 1 ~C 20 C alkyl groups, or xylyl, tolyl, or phenyl groups 6 ~C 12 represents an aryl group, and "Alk" and R in each occurrence may be the same or different; h=1 or 2; [C5] In the formula, the symbol L is a C alkyl group such as methyl, ethyl, or propyl. 1 ~C 20 C alkyl groups, or xylyl, tolyl, or phenyl groups 6 ~C 12 represents an aryl group, the symbol g is equal to 2, and each occurrence of L may be the same or different.
6. At least 3 silicon bonds per molecule 2 ~C 20The curable silicone composition X according to any one of claims 1 to 5, wherein the at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL containing alkenyl groups contains at least three siloxy units of formula (A-3) and other siloxy units of formula (A-2): [C6] In the formula, the symbol "Alk" represents a vinyl group, and the symbol R represents a methyl group. h=1 or 2; [C7] In this formula, the symbol L represents a methyl group and the symbol g is equal to 2.
7. At least 3 silicon bonds per molecule 2 ~C 20 7. The curable silicone composition X of any one of claims 1 to 6, wherein the at least one diorganoalkenylsiloxy-terminated diorganopolysiloxane gum crosslinker Alk-XL containing alkenyl groups is a vinyl-terminated (vinylmethylsiloxane)-dimethylsiloxane copolymer gum having a total vinyl content of 0.020 to 0.065 wt%.
8. The curable silicone composition of any one of claims 1 to 7, wherein the at least one organosilicon crosslinker H-XL containing at least three silicon-bonded hydrogen atoms per molecule comprises: (i) at least three siloxy units of the formula (XL-1), which may be the same or different: [C8] During the ceremony, The symbol H represents a hydrogen atom, the symbol Z represents an alkyl group containing 1 to 8 carbon atoms, the symbol e is equal to 0, 1 or 2; and (ii) at least one, preferably from 1 to 550, siloxy units of formula (XL-2): [C9] During the ceremony, The symbol Z is an alkyl group having 1 to 8 carbon atoms, such as xylyl, tolyl, or phenyl groups. 6 ~C 12 represents an aryl group, the symbol g is equal to 0, 1, 2 or 3; However, Z in XL-1 and XL-2 may be the same or different.
9. 9. The curable silicone composition X of claim 8, wherein the at least one organosilicon crosslinker H-XL contains from 3 to 60 siloxy units of formula (XL-1) and from 1 to 250 siloxy units of formula (XL-2).
10. The curable silicone composition X according to any one of claims 1 to 9, wherein the catalyst C is a platinum group metal-containing catalyst.
11. A curable silicone composition X according to any one of the preceding claims, wherein the at least one reinforcing mineral filler F1 is selected from the group consisting of ground quartz, fumed silica, and mixtures thereof.
12. 12. Curable silicone composition X according to any one of claims 1 to 11, wherein the at least one reinforcing mineral filler F1 is a fumed silica which has been treated with at least one compatibilizer in the presence of at least a portion of the at least one alkenyl-containing organopolysiloxane A.
13. 13. The curable silicone composition of claim 12, wherein the at least one compatibilizer is free of reactive alkenyl groups.
14. 14. The curable silicone composition X according to claim 12 or 13, wherein the at least one reinforcing mineral filler F1 further comprises ground quartz.
15. 15. The curable silicone composition X according to claim 1, wherein the value of the ratio RHalk is 1.15≦RHalk≦1.
30.
16. The curable silicone composition X according to any one of claims 1 to 15, wherein the % molar ratio RAlkA is within the range of 86% ≦ RAlkA ≦ 93%.
17. 17. The curable silicone composition X according to any one of claims 1 to 16, wherein the curable silicone composition X cures to give a silicone elastomer Z having an elongation at break value of at least 1200%, measured according to ASTM D-412.
18. The curable silicone composition X according to any one of claims 1 to 17, wherein, upon curing of the curable silicone composition X, a silicone elastomer Z having a peel strength of at least 40 N / cm as measured in accordance with JIS K6854 is obtained.
19. 19. An inflatable bag for protecting vehicle occupants, consisting of two parts sewn together, adhesively bonded and / or leak-proofed in the area of the seams with a curable silicone composition X according to any one of claims 1 to 18.
20. A method for bonding at least two substrates S1 and S2, comprising the steps of: Preparing a curable silicone composition X according to any one of claims 1 to 18; applying said curable silicone composition X to at least one of the surfaces of S1 and / or S2 to form at least one adhesively coated surface; Assembling said substrates S1 and S2 such that said at least one adhesive coated surface forms a bond between said at least two substrates S1 and S2; Optionally, applying pressure to the at least one adhesive coated surface; and Optionally, heating the assembled substrates S1 and S2. The method includes:
21. Use of a curable silicone composition X according to any one of claims 1 to 18 in the manufacture of an airbag.
22. 22. The use according to claim 21, wherein the curable silicone composition X is used as a joint sealant.