Polyamide acid, polyamide acid composition, polyimide, laminate thereof, flexible device and method for producing laminate
A polyamic acid composition with a xanthene and fluorene structure addresses the issues of thermal instability and corrosive gas generation in polyimides, providing transparent and stress-free polyimides for flexible electronic devices.
Patent Information
- Application Number
- JP2023063812
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Existing polyimides used in flexible electronic devices suffer from issues such as low thermal decomposition temperatures, generation of corrosive gases like hydrogen fluoride, and high internal stress, leading to peeling and misalignment during high-temperature processes, which compromise transparency and process compatibility.
A polyamic acid composition with a xanthene structure in the main chain and fluorene structure in the side chain, combined with specific aromatic diamines, is used to create a polyimide that maintains high transparency and heat resistance, minimizing internal stress and corrosive gas generation during high-temperature processes.
The resulting polyimide exhibits excellent transparency, high thermal stability, and low internal stress, preventing peeling and corrosion at the interface with barrier films, suitable for flexible electronic devices requiring high heat resistance and transparency.
Smart Images

Figure 2024150826000001 
Figure 2024150826000002 
Figure 2024150826000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamic acid, a polyamic acid composition, a polyimide, a laminate thereof, a flexible device, and a method for producing the laminate. The present invention further relates to an electronic device material, a TFT substrate, a flexible display substrate, a color filter, a printed matter, an optical material, a liquid crystal display device, an image display device such as an organic electroluminescence (EL) display and an electronic paper, a 3-D display, a solar cell, a touch panel, a transparent conductive film substrate, and a substitute material for a portion where glass is currently used, using the polyimide. [Background technology]
[0002] With the rapid progress of electronics such as displays (LCD, OLED, electronic paper, etc.), solar cells, touch panels, etc., devices are becoming thinner, lighter, and more flexible. In these devices, polyimide is used as the substrate instead of glass.
[0003] In these devices, various electronic elements, such as thin-film transistors and transparent electrodes, are formed on the substrate, and high-temperature processes are required to form these electronic elements. General aromatic polyimides have sufficient heat resistance to be applicable to high-temperature processes, and their coefficient of linear thermal expansion (CTE) is close to that of glass substrates and electronic elements, making them less susceptible to internal stress, making them suitable for use as substrate materials for flexible displays and the like.
[0004] Aromatic polyimides are generally colored yellowish brown due to intramolecular conjugation and the formation of charge transfer (CT) complexes, but in top-emission organic electroluminescence (EL) displays, the light is extracted from the opposite side of the substrate, so the substrate does not require transparency, and general aromatic polyimides have been used. However, in cases where the light emitted from the display element is emitted through the substrate, such as transparent displays, bottom-emission organic electroluminescence (EL) displays, and liquid crystal displays, or when smartphones are made into full-screen displays (notchless), or when sensors or camera modules are placed on the back of the substrate, the substrate is now required to have high optical properties. Against this background, there is a demand for materials that have the same heat resistance as general aromatic polyimides and also have excellent transparency.
[0005] In general, in order to reduce the coloration of polyimide, the formation of CT complexes can be suppressed by using an aliphatic monomer (Patent Documents 1 and 2), or the transparency can be increased by using a monomer having a fluorine atom (Patent Document 3). The polyimides described in Patent Documents 1 and 2 are highly transparent and have a low CTE, but have a low thermal decomposition temperature due to their aliphatic structure, and are not suitable for high-temperature processes for forming electronic devices. The polyimide described in Patent Document 3 has high transparency and high heat resistance due to the introduction of a fluorene structure, but has a high coefficient of thermal expansion (CTE), which causes misalignment during the formation of electronic devices, and when laminated, the internal stress increases due to the mismatch in CTE, causing the substrate to warp, making it unsuitable for manufacturing processes. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2016-29177 A (Published March 3, 2016) [Patent Document 2] JP 2012-41530 A (Published March 1, 2012) [Patent Document 3] TW201713726A (released April 16, 2017) [Patent Document 4] WO2019 / 195148A1 (published on April 1, 2019) Summary of the Invention [Problem to be solved by the invention]
[0007] The authors' investigation revealed that although the polyimide described in Patent Document 4 is highly transparent, it generates corrosive gases such as hydrogen fluoride due to decomposition gases at around 350° C. As a result, it became clear that outgassing such as hydrogen fluoride occurs during high-temperature processes such as the production of displays and the like, for example, TFT elements, corroding barrier films laminated on the polyimide, causing peeling, floating, and aggregation at the interface of the laminate, and not only lacking in process compatibility, but also discoloring the polyimide film itself, making it unsuitable for applications requiring high transparency.
[0008] The present invention has been made in view of the above circumstances, and aims to provide a polyimide having excellent transparency and high heat resistance, not generating fluorine-containing corrosive gases even in high-temperature processes exceeding 400°C, not floating or corroding at the interface between the polyimide and a barrier film (e.g., a silicon oxide film or a silicon nitride film) laminated thereon or a substrate, and showing little color change, and a polyamic acid composition as its precursor. Another aim is to provide a product or member that requires high heat resistance and transparency by using the polyimide and polyamic acid. In particular, an aim is to provide a product and member that uses the polyimide and polyamic acid of the present invention for application in forming the polyimide and polyamic acid on the surface of an inorganic material such as glass, metal, metal oxide, and single crystal silicon. [Means for solving the problem]
[0009] As a result of intensive research, the authors have found that by using a polyamic acid consisting of an acid dianhydride having a highly linear xanthene structure in the main chain and a fluorene structure in its side chain, s-BPDA and a-BPDA, and an aromatic diamine, when made into a polyimide film, the polyimide has excellent transparency without impairing the inherent thermal properties of the polyimide, does not float on the glass substrate or barrier film, and can withstand high-temperature processes, thereby completing the present invention. That is, the present invention has the following configuration.
[0010] 1) A polyamic acid having a structure represented by the following general formula (1), (2), or (3). (In the formula, X contains at least one of the general formula (4), and R 1 are each independently a hydrogen atom or a monovalent aliphatic or aromatic group; R 2 is an organic group selected from the group (5).
[0011] [ka]
[0012] [ka]
[0013] [ka]
[0014] [ka]
[0015] [ka] 2) The polyamic acid according to 1), wherein the proportion of fluorine atoms contained in the polyamic acid is less than 1% by weight.
[0016] 3) A polyamic acid composition comprising the polyamic acid composition according to 1) or 2) and an organic solvent.
[0017] 4) The polyamic acid composition according to 3), characterized in that it contains an imidization accelerator in an amount of 10 parts by weight or less based on the polyamic acid.
[0018] 5) A polyimide which is an imidized product of the polyamic acid composition according to 3) or 4).
[0019] 6) A polyimide characterized in that when the polyamic acid composition (solution) according to 3) or 4) is cast onto a glass substrate and imidized, the internal stress generated between the polyimide film and the glass substrate is 20 MPa or less.
[0020] 7) The polyimide according to 5) or 6), which has a yellow index (YI) of 15 or less when the film thickness is 10 μm.
[0021] 8) The polyimide according to any one of 5) to 7), having a 1% weight loss temperature of 500° C. or higher.
[0022] 9) A laminate of the polyimide according to any one of 5) to 8) and a support.
[0023] 10) A method for producing a laminate of a polyimide and a support, which comprises casting the polyamic acid composition (solution) according to 3) or 4) on a support and heating it to effect imidization.
[0024] 11). A flexible device comprising the polyimide according to any one of 5) to 8) and an electronic element formed on the polyimide. Effect of the Invention
[0025] The polyimide produced by using the polyamic acid according to the present invention is excellent in transparency and heat resistance, does not generate corrosive gases such as hydrogen fluoride even in a high-temperature process, and does not cause floating at the interface with a glass substrate or a barrier film when formed into a laminate. Therefore, the polyimide according to the present invention and the polyamic acid according to the present invention are suitable as films or substrates for members requiring heat resistance and transparency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present invention will be described in detail below, but the present invention is not limited thereto. The polyamic acid produced in the present invention is characterized by having a structure represented by the following general formula (1), (2), or (3): In the formula, X contains at least one of the groups represented by general formula (4), and R 1 are each independently a hydrogen atom or a monovalent aliphatic or aromatic group; R 2 is preferably an organic group selected from the group (5).
[0027] [ka]
[0028] [ka]
[0029] [ka]
[0030] [ka]
[0031] [ka]
[0032] In the polyamic acid according to the present invention, it is preferable that the general formula (1) contains a structure composed of an acid dianhydride derived from spiro[11H-difluoro[3,4-b:3',4'-i]xanthene-11,9'-[9H]fluorene]1,3,7,9-tetrahydrofuran (SFDA) and an aromatic diamine.
[0033] SFDA has a rigid structure derived from the xanthene structure, and is effective not only in providing high Tg, low CTE, and low internal stress, but also in providing transparency and low retardation due to the fluorene structure of the side chain. In addition, by combining SFDA with s-BPDA and a-BPDA in order to balance transparency, heat resistance, and internal stress, a high balance between transparency, heat resistance, and internal stress can be achieved. When the total acid dianhydride constituting the polyamic acid is taken as 100 mol%, it is desirable that each of the general formulas (1) to (3) is contained in an amount of 1 mol% or more, and in particular, it is more preferable that the total mol% of the general formulas (1) and (3) is equal to or less than the mol% of the general formula (2).
[0034] As the aromatic diamine, from the viewpoint of low CTE and high Tg, 1,4-phenylenediamine (PDA), 4-aminophenyl-4-aminobenzoate (4-BAAB), 4,4-diaminobenzanilide (DABA) and structures similar thereto are preferred.
[0035] The polyamic acid according to the present embodiment may contain a diamine other than X, provided that the performance is not impaired. Specific examples include 1,4-diaminocyclohexane, 1,3-phenylenediamine, 9,9-bis(4-aminophenyl)fluorene, 4,4'-oxydianiline, 3,4'-oxydianiline, 4,4'-diaminodiphenylsulfone, m-tolidine, o-tolidine, 4,4'-bis(aminophenoxy)biphenyl, 2-(4-aminophenyl)-6-aminobenzoxazole, 3,5-diaminobenzoic acid, 4,4'-diamino-3,3'dihydroxybiphenyl, 4,4'-methylenebis(cyclohexaneamine), 1,3-bis(3-aminopropyl)tetramethyldisiloxane (PAM-E), and similar compounds thereof, and these may be used alone or in combination of two or more. From the viewpoint of improving transparency, heat resistance, Tg and low internal stress, when the total diamines constituting the polyamic acid are taken as 100 mol%, it is preferable that PDA, 4-BAAB, or DABA is contained at 50 mol% or more, more preferably 70 mol%, even more preferably 80 mol% or more, and it may be 100 mol%. Furthermore, when the total diamines are taken as 100 mol%, it is possible to impart appropriate adhesion to inorganic films and substrates by containing 0.01 mol% or more and 1 mol% or less of PAM-E, without deteriorating heat resistance or Tg.
[0036] The polyamic acid according to the present embodiment may contain components other than SFDA, s-BPDA, and a-BPDA within a range that does not impair its performance. Specifically, pyromellitic dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 4,4-oxydiphthalic dianhydride, 1,4-phenylenebis(trimellitate dianhydride), 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 4,4' ...1,4-phenylenebis(trimellitate dianhydride), 1,4-phenylenebis(trimellitate dianhydride), 1,4-phenylenebis(trimellitate dianhydride), 1,4-phenylenebis(trimellitate dianhydr Examples thereof include phthalic dianhydride, dicyclohexyl-3,3',4,4'-tetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, cyclobutanetetracarboxylic dianhydride, 2'-oxodispiro[bicyclo[2.2.1]heptane-2,1''-cycloheptane-3,2''-bicyclo[2.2.1]heptane]-5,5'-6,6'-tetracarboxylic dianhydride, and analogs thereof, and these may be used alone or in combination of two or more.
[0037] From the viewpoints of transparency, heat resistance, Tg, and low internal stress, when the total acid dianhydride constituting the polyamic acid is taken as 100 mol%, the components other than SFDA, s-BPDA, and a-BPDA are preferably 1 mol% or more and 50 mol% or less, more preferably 20 mol% or less, and even more preferably 10 mol% or less. By setting the content within the above range, when the polyimide is made, it is possible to exhibit low YI, excellent internal stress, excellent glass transition temperature, and excellent heat resistance. From the viewpoint of suppressing the generation of fluorine-containing corrosive gas even in a high-temperature process exceeding 400°C, the proportion of fluorine atoms contained in the polyamic acid is preferably less than 1 wt%, more preferably less than 0.5 wt%, and even more preferably less than 0.1 wt%.
[0038] Next, the imidization accelerator in the present invention will be described. In this specification, the imidization accelerator refers to imidazoles containing a 1,3-diazole ring structure. The imidazoles added to the polyamic acid of the present invention are not particularly limited, but examples thereof include 1H-imidazole, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-phenylimidazole. 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-phenylimidazole are preferred, and 1,2-dimethylimidazole and 1-benzyl-2-methylimidazole are preferred. is more preferred.
[0039] The content of imidazoles is preferably 0.005 mol or more and 0.1 mol or less, more preferably 0.01 mol or more and 0.08 mol or less, and more preferably 0.015 mol or more and 0.050 mol or less, per mol of amide group of polyamic acid. By containing 0.005 mol or more, it is effective in improving the film strength and transparency of polyimide, and by making it 0.1 mol or less, the storage stability of polyamic acid can be maintained and Tg and heat resistance can be improved. Regarding the improvement of transparency, it is known that polymerization solvents such as NMP form complexes by hydrogen bonding with carboxylic acid of polyamic acid, and when the imidization rate is slow, NMP etc. may remain in the film and cause coloring by oxidation or decomposition. When imidazoles are added, they coordinate with carboxylic acid of polyamic acid and promote imidization, so that NMP etc. are less likely to remain in the film and at the same time, the decomposition of polyamic acid during the thermal imidization process is suppressed, which is thought to improve transparency. In this specification, the term "amide group of polyamic acid" refers to an amide group formed by a polyaddition reaction of diamine and tetracarboxylic dianhydride. The method of adding imidazole to polyamic acid is not particularly limited. From the viewpoint of controlling the molecular weight of polyamic acid, a method of mixing with polyamic acid is preferable. At this time, the imidazole may be added directly to polyamic acid, or the imidazole may be dissolved in a solvent in advance and the solution may be added, and the method is not particularly limited.
[0040] The imidization of polyamic acid is accelerated by adding imidazoles, and in-plane orientation is induced from rigid units that are imidized in the early stage of thermal imidization. The polyamic acid of the present invention can be synthesized by a known general method, and can be obtained by reacting a diamine with a tetracarboxylic dianhydride in an organic solvent. Specifically, for example, in an inert atmosphere such as argon or nitrogen, a diamine is dissolved in an organic solvent or dispersed in a slurry state to obtain a diamine solution. Meanwhile, the tetracarboxylic dianhydride may be added to the diamine solution after being dissolved in an organic solvent or dispersed in a slurry state, or in a solid state.
[0041] When synthesizing polyamic acid using diamine and tetracarboxylic dianhydride, the total molar amount of single or multiple diamine components and the total molar amount of single or multiple tetracarboxylic dianhydride components can be adjusted to obtain any polyamic acid copolymer. In addition, polyamic acid containing multiple tetracarboxylic dianhydrides and diamines can be obtained by blending two kinds of polyamic acid. The temperature condition of the reaction between the diamine and tetracarboxylic dianhydride, i.e., the synthesis reaction of polyamic acid, is not particularly limited, but may be in the range of 25°C to 150°C as necessary, and the reaction time may be set arbitrarily in the range of 10 minutes to 30 hours.
[0042] The organic solvent used in the polymerization of polyamic acid is preferably one capable of dissolving the tetracarboxylic dianhydride and diamines used, and is also preferably one capable of dissolving the polyamic acid produced. Examples of the organic solvent used in the synthesis reaction of the polyamic acid include urea-based solvents such as tetramethylurea and N,N-dimethylethylurea, sulfoxide or sulfone-based solvents such as dimethylsulfoxide, diphenylsulfone, and tetramethylsulfone, N,N-dimethylacetamide (DMAC), N,N-dimethylformamide (DMF), N,N'-diethylacetamide, N-methyl-2-pyrrolidone (NMP), N-butyl-2-pyrrolidone (NBP), 3-methoxy-N,N-dimethylpropanamide (MPA), hexamethyl Examples of suitable solvents include amide solvents such as phosphoric acid triamide, ester solvents such as γ-butyrolactone, halogenated alkyl solvents such as chloroform and methylene chloride, aromatic hydrocarbon solvents such as benzene and toluene, phenol solvents such as phenol and cresol, ketone solvents such as cyclopentanone, and ether solvents such as tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, dimethyl ether, diethyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, and p-cresol methyl ether. Usually, these solvents are used alone, but two or more of them may be used in combination as necessary. In order to increase the solubility and reactivity of polyamic acid, the organic solvent used in the synthesis reaction of the polyamic acid is preferably selected from amide solvents, ketone solvents, ester solvents, and ether solvents, and particularly preferably amide solvents such as DMF, DMAC, NMP, NBP, and MPA. In addition, it is preferable that the reaction is carried out in an inert atmosphere such as argon or nitrogen.
[0043] The weight-average molecular weight of the polyamic acid according to the present invention is preferably in the range of 10,000 to 1,000,000, more preferably in the range of 20,000 to 500,000, and even more preferably in the range of 30,000 to 200,000. In addition, when a polyamic acid solution is applied to a substrate by a slit coater or the like to form a film, it is important from the viewpoint of productivity that the viscosity and solid content concentration of the polyamic acid solution are in the optimum range, and by setting them in the above range, a polyamic acid solution or polyimide solution with the optimum viscosity and solid content concentration can be obtained. If the weight-average molecular weight is 10,000 or more, it is possible to form a coating film or film from the polyamic acid and polyimide. On the other hand, if the weight-average molecular weight is 1,000,000 or less, the polyamic acid and polyimide show sufficient solubility in the solvent, so that a coating film or film with a smooth surface and a uniform thickness can be obtained from the polyamic acid solution and polyimide solution described later. The molecular weight used here refers to a value calculated as polyethylene glycol by gel permeation chromatography (GPC).
[0044] In addition, as a method for controlling the molecular weight, the molecular weight may be adjusted by using an excess of either the acid dianhydride or the diamine, or by reacting with a monofunctional acid anhydride or amine such as phthalic anhydride or aniline to quench the reaction. When polymerizing with an excess of either the acid dianhydride or the diamine, a polyimide film with sufficient strength can be obtained as long as the molar ratio of the acid dianhydride divided by the molar ratio of the diamine is between 0.95 and 1.05. In addition, in general, when the acid dianhydride is used in excess to form a polyimide film with an acid dianhydride terminal, it is advantageous in terms of transparency, but at high temperatures there is a possibility that decarboxylation due to decomposition of carboxylic acid may occur. Therefore, by making the terminal amine, it is easier to suppress decomposition, but there is also an influence of coloring due to the oxidation of the amine, so the terminal structure can be controlled according to the desired characteristics. In addition, coloring can be suppressed or crosslinking can be performed by blocking the terminals with phthalic anhydride, maleic anhydride, aniline, etc.
[0045] The polyimide of the present invention can be obtained by a known method, and the manufacturing method is not particularly limited. In view of the availability of monomers and the ease of polymerization, the polyimide of the present invention is preferably obtained from its precursor, polyamic acid. A method of imidizing the polyamic acid to obtain a polyimide using the polyamic acid will be described. The imidization is performed by dehydrating and ring-closing the polyamic acid. This dehydrating and ring-closing can be performed by an azeotropic method using an azeotropic solvent, a thermal method, or a chemical method. In addition, the imidization of the polyamic acid to the polyimide can take any ratio of 1 to 100%. In other words, a polyamic acid that is partially imidized may be synthesized. In particular, when imidization is performed by heating and increasing the temperature, the ring-closing reaction from the polyamic acid to the polyimide and the hydrolysis of the polyamic acid proceed simultaneously, When polyimide is produced, its molecular weight may be lower than that of polyamic acid, and coloring may occur due to oxidation of terminal diamines produced by hydrolysis. For this reason, it is preferable to use a polyamic acid solution in which a portion of the polyamic acid has been imidized in advance from the viewpoints of transparency and mechanical properties.
[0046] In this specification, the solution containing polyamic acid and an organic solvent is referred to as a polyamic acid solution. Here, the organic solvent contained in the polyamic acid solution can be the same organic solvent as that used in the synthesis reaction of the polyamic acid, and among them, an organic solvent selected from amide solvents, ketone solvents, ester solvents and ether solvents can be more preferably used, and amide solvents such as DMF, DMAC, NMP, NBP, and MPA can be particularly preferably used. When polyamic acid is obtained by the above-mentioned method, the synthesis reaction solution itself can be expressed as a polyamic acid solution.
[0047] The dehydration ring closure may be performed by heating the polyamic acid. The method of heating the polyamic acid is not particularly limited, but for example, the polyamic acid solution may be cast or applied onto a support such as a glass plate, a metal plate, or PET (polyethylene terephthalate), and then heat-treated within the range of 80°C to 500°C. Alternatively, the polyamic acid solution may be directly placed in a container that has been subjected to a release treatment such as coating with a fluorine-based resin, and the polyamic acid solution may be heated and dried under reduced pressure to perform the dehydration ring closure of the polyamic acid. Polyimide can be obtained by the dehydration ring closure of the polyamic acid using this method. The heating time of each of the above treatments varies depending on the amount of the polyamic acid solution to be dehydrated and the heating temperature, but it is generally preferable to perform the treatment within a range of 1 minute to 5 hours after the treatment temperature reaches the maximum temperature. In order to shorten the heating time and to express characteristics, an imidizing agent and / or a dehydration catalyst may be added to the polyamic acid solution, and the polyamic acid solution to which the imidizing agent and / or the dehydration catalyst have been added may be heated by the above method to perform imidization.
[0048] The imidizing agent is not particularly limited, but a tertiary amine can be used. As the tertiary amine, a heterocyclic tertiary amine is more preferable. Specific examples of the heterocyclic tertiary amine include pyridine, picoline, quinoline, isoquinoline, and 1,2-dimethylimidazole. Specific examples of the dehydration catalyst include acetic anhydride, propionic anhydride, n-butyric anhydride, benzoic anhydride, and trifluoroacetic anhydride.
[0049] The amount of the imidizing agent and the dehydration catalyst added is preferably 0.5 to 5.0 times the molar equivalent of the imidizing agent relative to the amide group of the polyamic acid, more preferably 0.7 to 2.5 times the molar equivalent, and particularly preferably 0.8 to 2.0 times the molar equivalent. The amount of the dehydration catalyst is preferably 0.5 to 10.0 times the molar equivalent of the imidizing agent relative to the amide group of the polyamic acid, more preferably 0.7 to 5.0 times the molar equivalent, and particularly preferably 0.8 to 3.0 times the molar equivalent. When the imidizing agent and / or the dehydration catalyst are added to the polyamic acid solution, they may be added directly without being dissolved in an organic solvent, or may be added after being dissolved in an organic solvent. In the method of adding directly without being dissolved in an organic solvent, the reaction may proceed rapidly before the imidizing agent and / or the dehydration catalyst are diffused, and a gel may be formed. It is more preferable to mix the solution obtained by dissolving the imidizing agent and / or the dehydration catalyst in an organic solvent with the polyamic acid solution.
[0050] In order to impart processing properties and various functionalities to the polyamic acid and polyimide according to the present invention, various organic or inorganic low-molecular or high-molecular compounds may be blended. For example, plasticizers, antioxidants, dyes, surfactants, leveling agents, silicones, fine particles, sensitizers, etc. can be used. The fine particles include organic fine particles such as polystyrene and polytetrafluoroethylene, and inorganic fine particles such as colloidal silica, carbon, and layered silicate, and may have a porous or hollow structure. In addition, the function or form of the fine particles includes pigments, fillers, fibers, etc.
[0051] The plasticizer of the present invention is preferably dissolved in a solvent used in the polymerization of polyamic acid and exists in a liquid state during imidization. It is also necessary that the plasticizer does not volatilize at low temperatures in order to impart sufficient mobility during imidization. Therefore, the boiling point of the plasticizer of the present invention is preferably 50°C or higher, more preferably 100°C or higher, and even more preferably 150°C or higher, and it is preferable that the plasticizer does not have a decomposition temperature below the boiling point.
[0052] The amount of plasticizer added varies depending on the compatibility between the plasticizer and the polyamic acid and the targeted physical properties. From the standpoint of imparting molecular mobility and avoiding the effects of decomposition of the plasticizer itself, the amount of plasticizer added is preferably from 0.001 to 20 parts by weight, more preferably from 0.01 to 15 parts by weight, and even more preferably from 0.1 to 10 parts by weight, per 100 parts by weight of polyamic acid.
[0053] The plasticizer of the present invention can improve the molecular motion when polyamic acid undergoes dehydration ring closure to form polyimide, and can also impart functions such as adjusting the glass transition temperature, flame retardancy, and oxidation prevention, and can be any known plasticizer. Examples of the plasticizer include phthalates, adipic esters, trimellitic esters, polyesters, phosphorus-based plasticizers, citric esters, epoxy-based plasticizers, polyethylene glycol, and polypropylene glycol, and low molecular weight organic compounds and thermoplastic resins may also be used.
[0054] Among them, phosphorus-based compounds, polyethylene glycol, and polypropylene glycol are preferable from the viewpoint of availability and plasticizing effect. The phosphorus-based compounds used in the present invention are not particularly limited, but it is preferable to use phosphoric acids, phosphorous acids, phosphonic acids, phosphinic acids, phosphines, phosphine oxides, phosphoranes, phosphazenes, etc. These phosphorus-based compounds may be esters or condensates thereof, may contain a cyclic structure, or may form salts with amines, etc. In addition, some of these phosphorus-based compounds have a tautomeric relationship, such as phosphorous acids and phosphonic acids, and they may exist in either state.
[0055] Specific examples of phosphorus-based phosphates include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tri(2-ethylhexyl) phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, tris(isopropylphenyl) phosphate, tris(phenylphenyl) phosphate, trinaphthyl phosphate, cresyl diphenyl phosphate, xylenyl diphenyl phosphate, diphenyl(2-ethylhexyl) phosphate, di(isopropylphenyl) phosphate, phenyl)phenyl phosphate, monoisodecyl phosphate, 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, diphenyl-2-acryloyloxyethyl phosphate, diphenyl-2-methacryloyloxyethyl phosphate, melamine phosphate, dimelamine phosphate, melamine pyrophosphate, triphenylphosphine oxide, tricresylphosphine oxide, diphenyl methanephosphonate, diethyl phenylphosphonate, resylcinol bis(diphenyl bisphenol A bis(diphenyl phosphate), phosphaphenanthrene, tris(β-chloropropyl)phosphate, triphenyl phosphite, trisnonylphenyl phosphite, tricresyl phosphite, triethyl phosphite, triisobutyl phosphite, tris(2-ethylhexyl)phosphite, tridecyl phosphite, trilauryl phosphite, tris(tridecyl)phosphite, diphenyl phosphite, diethyl phosphite, dibutyl phosphite, dimethyl phosphite, Diphenyl mono(2-ethylhexyl)phosphite, diphenyl modecyl phosphite, diphenyl mono(tridecyl)phosphite, trilauryl trithiophosphite, diethyl hydrogen phosphite, bis(2-ethylhexyl) hydrogen phosphite, dilauryl hydrogen phosphite, dioleyl hydrogen phosphite, diphenyl hydrogen phosphite, tetraphenyl dipropylene glycol diphosphite, tetra(C12-C15 alkyl)-4,4-isopropylidene diphenyl diphosphite, 4,Examples of such phosphite include 4-butylidenebis(3-methyl-6-t-butylphenyl ditridecyl phosphite), bis(decyl)pentaerythritol diphosphite, bis(tridecyl)pentaerythritol diphosphite, tristearyl phosphite, distearyl pentaerythritol diphosphite, and tris(2,4-di-tert-butylphenyl)phosphite.
[0056] Examples of the condensates include trialkyl polyphosphate, resorcinol polyphenyl phosphate, resorcinol poly(di-2,6-xylyl) phosphate (manufactured by Daihachi Chemical Industry Co., Ltd., trade name PX-200), hydroquinone poly(2,6-xylyl) phosphate, resorcinol polyphenyl phosphate (trade name CR-733S), bisphenol A polycresyl phosphate (trade name CR-741), aromatic condensed phosphate ester (trade name CR747), resorcinol polyphenyl phosphate, bisphenol A polycresyl phosphate (trade names FP-600, FP-700), etc. These phosphorus-based compounds can be used alone or in combination.
[0057] Examples of phosphazenes include phenoxycyclophosphazene (trade name: FP-110, manufactured by Fushimi Pharmaceutical Co., Ltd.) and cyclic cyanophenoxyphosphazene (trade name: FP-300, manufactured by Fushimi Pharmaceutical Co., Ltd.).
[0058] Specific examples of the aliphatic dibasic acid ester include dibutyl adipate, diisobutyl adipate, bis(2-ethylhexyl) adipate, diisonyl adipate, diisodecyl adipate, bis[2-(2-butoxyethoxy)ethyl]adipate, bis(2-ethylhexyl)azelate, dibutyl sebacate, bis(2-ethylhexyl) sebacate, and diethyl succinate.
[0059] In addition, low molecular weight organic compounds and thermoplastic resins may be used as long as they exhibit a plasticizing effect. The low molecular weight organic compounds in the present invention generally have a molecular weight of about 1000 or less, and examples thereof include phthalimides such as phthalimide, N-phenylphthalimide, N-glycidylphthalimide, N-hydroxyphthalimide, and cyclohexylthiophthalimide, and maleimides such as N,Np-phenylenebismaleimide and 2,2-(ethylenedioxy)bis(ethylmaleimide). Examples of thermoplastic resins include polyimides and polyamides having an asymmetric structure. These plasticizers may be dissolved in a solvent before polymerization of polyamic acid, or may be added to the polyamic acid solution later.
[0060] Next, the phenolic compound in the present invention will be described. The phenolic compound of the present invention has a function as an antioxidant and also has an effect of suppressing coloration of the polymer, so it is suitable for applications requiring transparency. It is preferable that the phenolic compound in the present invention dissolves in the solvent used for polymerization of the polyamic acid and exists in liquid form during imidization. In order to suppress coloration of the film, it is preferable that the phenolic compound remains during imidization, so that the boiling point of the phenolic compound is preferably 50°C or higher, more preferably 100°C or higher, and even more preferably 150°C or higher, and it is preferable that the decomposition temperature is not lower than the boiling point.
[0061] Phenol compounds include hindered, semi-hindered, and less hindered types. Specific examples include dibutylhydroxytoluene, ethylene bis(oxyethylene) bis-(3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate (trade name: Irganox245), 1,3.5-tris(3,5-ditert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)trione (trade name: AO-20), 4,4,4-(1-methylpropanyl-3-ylidene) ) Tris(6-tert-butyl-m-cresol) (trade name: AO-30), 6,6-di-tert-butyl-4,4-butylidenedi-m-cresol (trade name: AO-40), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (trade name: AO-50), pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) (trade name: AO-60), 3,9-bis(2-(3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy) -1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5,5)undecane (trade name: GA-80), 1,3,5-tris(3,5-ditert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene (trade name: AO-330), 1-hydroxy(2,2-ethylidenebis(4,6-bis(1,1-dimethylpropyl)benzene))-1-yl acrylate (trade name: Sumilizer GS), 2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl acrylate) Examples include phenyl (trade name: Sumilizer GM), 2-tert-butyl-6-methyl-4-(3-((2,4,8,10-tetra-tert-butyldibenzo(d,f)(1,3,2)dioxaphosphepin-6-yl)oxy)propyl)phenol (trade name: Sumilizer GP), and among these, since polyamic acid and amide-based solvents may generate nitrided oxides as decomposition products, GA-80, Sumilizer GS, Sumilizer GP, Sumilizer GM, etc. are preferred from the viewpoint of resistance to these gases and suppression of discoloration of the phenol-based compound itself.
[0062] Phenolic compounds mainly function as primary antioxidants that capture peroxy radicals, convert them to hydroperoxides, and inhibit the autoxidation of polymers, so they are effective in suppressing discoloration caused by the oxidation of polymers. Furthermore, by combining them with phosphites, which function as secondary antioxidants that convert hydroperoxides into stable alcohol compounds, further synergistic effects can be obtained. For example, by using an equivalent to 10 equivalents of phosphites relative to phenolic compounds, the generation of radicals can be efficiently suppressed, and discoloration of polymers can be suppressed.
[0063] In order to obtain a sufficient plasticizing effect and an antioxidant effect, the amount of the phenolic compound is preferably 0.001 to 10 parts by weight, more preferably 0.01 to 5 parts by weight, and even more preferably 0.02 to 1 part by weight, based on 100 parts by weight of the polyamic acid. The phenolic compound may be dissolved in a solvent before polymerization of the polyamic acid, or may be added to the polyamic acid solution afterwards.
[0064] The method of preparing nanosilica-containing polyamic acid by compounding polyamic acid with nanosilica can be a known method, and is not particularly limited.As an example, a method using organosilica sol in which nanosilica is dispersed in an organic solvent will be described.As a method of compounding polyamic acid with organosilica sol, polyamic acid may be synthesized, and then the synthesized polyamic acid and organosilica sol are mixed, but it is preferable to synthesize polyamic acid in organosilica sol, because nanosilica can be more highly dispersed in polyamic acid.
[0065] The organosilica sol can also be surface-treated to enhance the interaction with the polyamic acid. As the surface treatment agent, a known agent such as a silane coupling agent can be used. As the silane coupling agent, an alkoxysilane compound having an amino group or a glycidyl group as a functional group is widely known, and can be appropriately selected. From the viewpoint of providing the interaction, an amino group-containing alkoxysilane is preferable, and examples thereof include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, 2-aminophenyltrimethoxysilane, and 3-aminophenyltrimethoxysilane, but from the viewpoint of the stability of the raw material, it is preferable to use 3-aminopropyltriethoxysilane. As a method of surface treatment, a silane coupling agent is added to the dispersion (organosilica sol) and stirred at 20 to 80° C. for about 1 to 10 hours to cause a reaction. At this time, a catalyst or the like that promotes the reaction may be added.
[0066] The nanosilica content of the nanosilica-containing polyamic acid is preferably 1 wt% to 30 wt%, more preferably 1 wt% to 20 wt%, based on 100 parts by weight of polyamic acid. When the content is 1 wt% or more, the heat resistance of the nanosilica-containing polyimide can be improved and the internal stress and retardation can be sufficiently reduced, and when the content is 30 wt% or less, the mechanical properties and transparency of the nanosilica-containing polyimide are not adversely affected.
[0067] The polyamic acid according to the present invention may contain a silane coupling agent in order to develop appropriate adhesion to the support. Any known silane coupling agent may be used without particular limitation, but a compound containing an amino group is particularly preferred in terms of reactivity with the polyamic acid.
[0068] The blending ratio of these silane coupling agents to 100 parts by weight of polyamic acid is preferably 0.01 to 0.50 parts by weight, more preferably 0.01 to 0.10 parts by weight, and even more preferably 0.01 to 0.05 parts by weight. By making the blending ratio of the silane coupling agent 0.01 parts by weight or more, the peeling suppression effect on the support is sufficiently exhibited, and by making it 0.50 parts by weight or less, the molecular weight of the polyamic acid is sufficiently maintained, so that problems such as embrittlement do not occur.
[0069] As described above, the polyimide film produced from the polyamic acid according to the present embodiment is colorless, transparent, and has low yellowness, and has Tg and heat resistance sufficient to withstand the TFT fabrication process, and is therefore suitable for use in transparent substrates of flexible displays.
[0070] When manufacturing a flexible display, a flexible substrate is formed on an inorganic film such as glass as a support, and electronic elements such as TFTs are then formed on top of that (flexible device). The process of forming TFTs is generally carried out over a wide temperature range of 150℃ to 650℃, but in order to actually achieve the desired performance, oxide semiconductors and a-Si are formed at 300℃ or higher, and in some cases a-Si is further crystallized using a laser or the like to form LTPS (Low Temperature Polysilicone).
[0071] In this case, if the thermal decomposition temperature of the polyimide film is low, outgassing occurs during element formation and adheres to the inside of the oven as sublimate, which may cause contamination inside the oven or cause the inorganic film or element formed on the polyimide film to peel off. Therefore, it is preferable that the 1% weight loss temperature of the polyimide film is 500°C or higher, and the higher the better.
[0072] More specifically, SiOx or SiNx is formed on the polyimide film as a barrier film before TFT formation. If the heat resistance of the polyimide is low, if imidization has not progressed completely, or if there is a large amount of residual solvent, peeling or lifting occurs at the interface between the polyimide and the inorganic film due to volatile components such as polyimide decomposition gas in high-temperature processes after lamination of the inorganic film, such as the dehydrogenation process of LTPS. Therefore, depending on the device fabrication process, in addition to the 1% weight loss temperature being 500°C or higher, there is a need for low outgassing when isothermally held at 400°C to 500°C. Specifically, after forming an inorganic film such as SiOx on the polyimide film, it is desirable that there is no peeling between the polyimide film and the inorganic film when held at 400°C for 1 hour. Since the performance of TFT improves with higher processing temperatures, it is more desirable that there is no peeling at 430°C, and even more desirable that there is no peeling at 470°C.
[0073] Even if the thermal decomposition temperature exceeds 500°C, if the polyimide film contains fluorine atoms, hydrogen fluoride and other substances are generated as decomposition products, corroding the inorganic film laminated on the polyimide film. Specifically, hydrogen fluoride reacts with SiOx to generate silicon tetrafluoride (SiF4) and other substances, which cause further reactions and hydrolysis to decompose and yellow not only the inorganic film but also the polyimide film itself, resulting in poor quality of the display. For this reason, it is desirable for the polyimide film not to contain fluorine atoms.
[0074] In addition, if the Tg is significantly lower than the process temperature, there is a possibility that misalignment may occur during element formation, so the Tg of the polyimide film used as the flexible substrate is preferably higher than the process temperature, and is preferably 420°C or higher, more preferably 430°C or higher, and more preferably 450°C or higher. Furthermore, if the internal stress generated in the glass substrate used as the support, the electronic element, and the polyimide film is high, problems such as warping or breakage of the glass substrate and peeling of the flexible substrate from the glass substrate will occur when the polyimide film expands during the high-temperature TFT process and then shrinks during cooling at room temperature. In general, the thermal expansion coefficient of the glass substrate is smaller than that of the resin, so that an internal stress occurs between the polyimide film and the glass substrate. Therefore, the internal stress generated between the polyimide film and the glass substrate is preferably 40 MPa or less, more preferably 30 MPa or less, and most preferably 20 MPa or less.
[0075] The polyimide of the present invention can be suitably used as a display substrate material such as a TFT substrate or a touch panel substrate. When used for the above purposes, a laminate of a support and polyimide is produced, and electronic elements are often formed thereon. In addition, non-alkali glass is suitably used as the support. Hereinafter, a method for producing a laminate of polyimide and a support and a method for producing polyimide via the laminate will be specifically described. These are examples of the method for producing polyimide, and are not limited to the following.
[0076] First, it is preferable to cast the polyamic acid solution on the support, and heat the laminate of the support and the polyamic acid at a temperature of 40 to 200°C for 3 to 120 minutes. It is also possible to dry the laminate at two temperatures, for example, at 50°C for 30 minutes and then at 100°C for 30 minutes. Next, in order to advance the imidization, the laminate of the support and the polyamic acid is heated at a temperature of 200 to 470°C for 3 to 300 minutes to obtain a laminate of the support and the polyimide. At this time, it is preferable to gradually increase the temperature from a low temperature to a maximum temperature. The rate of temperature increase is preferably 2°C / min to 10°C / min, more preferably 4°C / min to 10°C / min. It is also preferable that the maximum temperature is in the range of 250 to 470°C. If the maximum temperature is 250°C or higher, the imidization proceeds sufficiently, and if the maximum temperature is 470°C or lower, the polyimide is not easily formed. The heat deterioration and coloring of the polyamic acid can be suppressed. In addition, the polyamic acid may be held at any temperature for any time until the maximum temperature is reached. The heating atmosphere can be air, reduced pressure, or an inert gas such as nitrogen, but in order to achieve higher transparency, it is preferable to perform the heating under reduced pressure or in an inert gas such as nitrogen. In addition, known devices such as hot air ovens, infrared ovens, vacuum ovens, inert ovens, and hot plates can be used as heating devices. In order to shorten the heating time and to achieve characteristic development, an imidizing agent or a dehydration catalyst may be added to the polyamic acid solution, and the solution may be heated and imidized by the above-mentioned method. In other words, a laminate with a support in which a part or all of the polyamic acid is imidized can also be obtained by the same method. The polyimide layer can be peeled off from the obtained laminate of the support and polyimide by a known method. For example, it may be peeled off by hand, or by using a mechanical device such as a driving roll or a robot. Furthermore, it is also possible to use a method in which a peeling layer is provided between the substrate and the polyimide layer, or a method in which a silicon oxide film is formed on a substrate having a large number of grooves and an etching solution is infiltrated therein to peel off the film. It is also possible to use a method in which the film is separated by irradiation with laser light.
[0077] At this time, if there is any lift at the interface between the polyimide and the supporting substrate (e.g. glass), the laminate will peel off during the process, and the lift at the interface between the support substrate and the polyimide during peeling is influenced by the components released during imidization and residual solvents. In particular, highly oriented polyimides such as BPDA / PDA and BPDA / 4-BAAB have densely packed molecular chains, which make them less gas-releasing and prone to lifting. As a result of our investigations, we found that lifting can be prevented by introducing a bulky or soft structure into the molecular chain or at the end, and in particular, despite having a rigid SFDA structure, it is possible to achieve both good gas-releasing properties and a high glass transition temperature due to the bulky structure of the side chain.
[0078] The transparency of polyimide can be evaluated by the total light transmittance (TT) and haze according to JIS K7361 and JIS K7163. When a polyimide film is used in the application of the present invention, the total light transmittance of the polyimide is preferably 75% or more, more preferably 80% or more. The haze is preferably 1.5% or less, more preferably 1.2% or less, and even more preferably less than 1.0%. In the application of the present invention, polyimide is required to have high transmittance in the entire wavelength range, but polyimide tends to absorb light on the short wavelength side, and the film itself is often colored yellow. For use in the application of the present invention, the yellow index (YI), which is an index indicating yellowness, is preferably 25 or less, more preferably 20 or less, and even more preferably 15 or less. YI can be measured according to JIS K 7373. By imparting transparency in this way, the polyimide film can be used as a transparent substrate for glass replacement applications, and even if a sensor or camera module is installed on the back of the substrate, the effect on the resolution and color reproducibility of the sensor or camera module can be suppressed.
[0079] In addition, there are two types of light extraction methods for flexible displays: the top emission method, in which light is extracted from the TFT element side, and the bottom emission method, in which light is extracted from the back side of the TFT element. The top emission method is characterized by the fact that the aperture ratio is easily increased because light is not blocked by the TFT element, and high-definition image quality can be obtained, while the bottom emission method is characterized by easy alignment and ease of manufacture. If the TFT element is transparent, it is possible to improve the aperture ratio even in the bottom emission method, so there is a tendency for the bottom emission method, which is easy to manufacture, to be adopted for large displays. YI and materials with excellent heat resistance as in the present invention can be used for both of the above applications.
[0080] In addition, in a batch-type device manufacturing process in which a polyamic acid solution is applied onto a support such as glass, heated to imidize, electronic elements, etc. are formed to form a substrate, and then peeled off, it is more preferable that the adhesion between the support and the polyimide is good. The adhesion here means adhesion strength. In the manufacturing process in which electronic elements, etc. are formed on a polyimide film on a support to form a substrate, and then the polyimide substrate on which the electronic elements, etc. are formed is peeled off from the support, excellent adhesion to the support means that electronic elements, etc. can be formed or mounted more accurately. In terms of the manufacturing process in which electronic elements, etc. are laminated on a support, the higher the peel strength, the better. Specifically, 0.05 N / cm or more is preferable, and 0.1 N / cm or more is even more preferable.
[0081] In the above-mentioned manufacturing process, when the polyimide layer is peeled off from the laminate of the support and the polyimide, it is often peeled off from the support by laser irradiation. From the viewpoint of the workability of this peeling, it is necessary to make the polyimide absorb the light of the laser wavelength. An excimer laser is often used for laser peeling, and since it is necessary to absorb the light of the wavelength of the laser, the cut-off wavelength is preferably 312 nm or more, more preferably 330 nm or more. Furthermore, if the cut-off wavelength is 400 nm or less, sufficient transparency can be expressed, so the cut-off wavelength is preferably 320 nm or more and 400 nm or less, more preferably 330 nm or more and 390 nm or less. In this specification, the cut-off wavelength means a wavelength at which the transmittance is 0.1% or less as measured by an ultraviolet-visible spectrophotometer.
[0082] The polyamic acid and polyimide according to the present invention may be directly subjected to a coating or molding process for producing a product or member, but may also be used as a laminate for further coating a molded product formed into a film shape. In order to subject the polyamic acid and polyimide to a coating or molding process, the polyamic acid and polyimide may be dissolved or dispersed in an organic solvent as necessary, and further blended with a photo- or thermosetting component, a non-polymerizable binder resin other than the polyamic acid and polyimide according to the present invention, and other components to prepare a polyamic acid and polyimide resin composition.
[0083] The polyimide film according to the present invention may have various inorganic thin films formed on its surface, such as metal oxides, transparent electrodes, etc. The method for forming these inorganic thin films is not particularly limited, and examples thereof include CVD, sputtering, vacuum deposition, ion plating, and other PVD methods.
[0084] The polyimide according to the present invention has heat resistance, low thermal expansion, transparency, and also has small internal stress with a glass substrate. Therefore, it is preferably used in fields and products in which these properties are effective, such as printed matter, color filters, flexible displays, optical films, liquid crystal displays, image display devices such as organic electroluminescence (EL) and electronic paper, 3-D displays, touch panels, transparent conductive film substrates, or solar cells, and further preferably as a replacement material for portions in which glass is currently used.
[0085] The polyamic acid, polyimide and polyamic acid solution according to the present invention can be suitably used in a batch-type device fabrication process in which a polyamic acid solution is applied onto a support, heated to be imidized, electronic elements and the like are formed on the support to form a substrate, and then the substrate is peeled off. Thus, the present invention also includes a method for fabricating an electronic device, which includes a substrate formation step in which a polyamic acid solution is applied onto a support, heated to be imidized, and electronic elements and the like are formed on the polyimide film formed on the support. The method for fabricating an electronic device may further include a step of peeling off the polyimide substrate on which the electronic elements and the like are formed from the support after the substrate formation step.
[0086] The present invention will be described in detail below with reference to examples. However, these are described for the purpose of illustration only, and the scope of the present invention is not limited to the following examples. EXAMPLES
[0087] (Evaluation method) The material property values and the like described in this specification were obtained by the following evaluation methods. (1) Calculation of YI of polyimide film The light transmittance of the polyimide film in the range of 200-800 nm was measured using a JASCO UV-Vis-NIR spectrophotometer (V-650), and the yellow index (YI) was calculated as an index representing yellowness according to the formula described in JIS K 7373.
[0088] (2) Measurement of internal stress The polyamic acid solutions prepared in the Examples and Comparative Examples were applied by a spin coater onto Corning alkali-free glass (thickness 0.7 mm, 100 mm x 100 mm) whose warpage had been measured in advance, and baked in air at 120°C for 30 minutes and in a nitrogen atmosphere at 430°C for 30 minutes to obtain a glass substrate and polyimide laminate with a thickness of 10 μm. The warpage of this glass substrate and polyimide laminate was measured using a Tencor thin film stress measuring device FLX-2320-S to evaluate the internal stress generated between the glass substrate and polyimide film at 25°C in a nitrogen atmosphere. In order to prevent the polyimide film from absorbing water, the glass substrate and polyimide laminate was measured immediately after baking or after drying at 120°C for 10 minutes.
[0089] (3) 1% weight loss temperature (TD1) Using a Hitachi High-Tech Science TGDTA7200, the film was heated from 25°C to 650°C at a rate of 20°C / min in a N2 atmosphere. Taking into account the effect of moisture, the temperature at which the weight decreased by 1% from the weight at 150°C was defined as the TD1 of the polyimide film.
[0090] The abbreviations of the reagents used are as follows: NMP: 1-methyl-2-pyrrolidone SFDA: spiro[11H-difluoro[3,4-b:3',4'-i]xanthene-11,9'-[9H]fluorene] 1,3,7,9 tetrone s-BPDA: 3,3'-4,4'-biphenyltetracarboxylic dianhydride a-BPDA: 2,3-3',4'-biphenyltetracarboxylic dianhydride BPAF: 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride 6FDA: 4,4-(Hexafluoroisopropylidene)diphthalic acid PDA: 1,4-phenylenediamine TFMB: 2,2-bis(trifluoromethyl)benzidine 4-BAAB: 4-aminophenyl-4-aminobenzoate DMI: 1,2-dimethylimidazole PHI: 2-phenylimidazole
[0091] Example 1 A 300mL glass separable flask equipped with a stainless steel stirrer and a nitrogen inlet tube was charged with 50.0g of NMP as an organic solvent for polymerization and stirred. 4.954g of 4-BAAB was added and dissolved. 3.076g of SFDA, 3.831g of s-BPDA, and 0.639g of a-BPDA were added to this solution and stirred at room temperature for 24 hours to obtain a uniform and transparent polyamic acid solution. This polyamic acid solution was applied to a glass plate with a spin coater and baked in air at 80°C for 30 minutes and in a nitrogen atmosphere at 430°C for 30 minutes to obtain a polyimide film with a thickness of 10μm. The properties of the obtained polyimide film are shown in Table 1.
[0092] Example 2 A polyimide film was obtained in the same manner as in Example 1, except that DMI was added at a ratio of 1 phr to the polyamic acid synthesized in Example 1. The properties of the obtained polyimide film are shown in Table 1.
[0093] Example 3 A polyimide film was obtained in the same manner as in Example 1, except that PHI was added at a ratio of 3 phr to the polyamic acid synthesized in Example 1. The properties of the obtained polyimide film are shown in Table 1.
[0094] (Examples 4 to 8) A polyimide film was obtained in the same manner as in Example 3, except that polyamic acid was synthesized so as to have the composition ratio of monomers shown in Table 1. The properties of the obtained polyimide film are shown in Table 1.
[0095] Comparative Example 1 A 300 mL glass separable flask equipped with a stainless steel stirrer and a nitrogen inlet tube was charged with 88.0 g of NMP as an organic solvent for polymerization and stirred. 4.848 g of TFMB was added and dissolved. 7.152 g of SFDA was added to this solution and stirred at room temperature for 24 hours to obtain a uniform and transparent polyamic acid solution. This polyamic acid solution was applied to a glass plate with a spin coater and baked in air at 80°C for 30 minutes and in a nitrogen atmosphere at 430°C for 30 minutes to obtain a polyimide film with a thickness of 10 μm. The properties of the obtained polyimide film are shown in Table 1.
[0096] (Comparative Examples 2 to 8) A polyimide film was obtained in the same manner as in Comparative Example 1, except that the monomers used were changed to those shown in Table 1.
[0097] As described above, in this example, a polyamic acid composition having the general formula (1) was used. (1) YI is less than 10 (2) Thermal decomposition temperature is 500°C or higher (3) Internal stress is 20 MPa or less (4) Does not contain fluorine, which generates corrosive gases.
[0098] Comparative Examples 1 and 2 have low YI and high TD1, but have high internal stress and contain fluorine, which may generate hydrogen fluoride. Comparative Examples 3 to 5 use SFDA alone or in combination with s-BPDA, and either YI or internal stress is insufficient. In Comparative Examples 6 to 8, BPAF, which has a structure similar to SFDA, was used, and although the YI was excellent, the internal stress was insufficient due to the low rigidity of the skeleton. In Examples 1 to 8, which combined SFDA, s-BPDA, and a-BPDA, the internal stress, YI, and TD1 were highly balanced.
[0099] From these results, it was confirmed that the polyimide obtained from the fluorine-free polyamic acid consisting of SFDA having a xanthene structure in the main chain and a fluorene structure in the side chain according to the present invention, s-BPDA, and a-BPDA, is colorless and transparent, has a high thermal decomposition temperature, has a small internal stress with the inorganic substrate, and has process heat resistance at high temperatures. Note that the present invention is not limited to the above-mentioned embodiment, and can be practiced with various modifications.
[0100] [Table 1]
Claims
1. A polyamic acid having a structure represented by the following general formula (1), (2), or (3): (wherein X contains at least one of the general formula (4), and R 1 are each independently a hydrogen atom or a monovalent aliphatic or aromatic group; R 2 is an organic group selected from the group (5). 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】
2. 2. The polyamic acid according to claim 1, wherein the proportion of fluorine atoms contained in the polyamic acid is less than 1% by weight.
3. A polyamic acid composition comprising the polyamic acid composition according to claim 1 and an organic solvent.
4. 4. The polyamic acid composition according to claim 3, further comprising 10 parts by weight or less of an imidization accelerator based on the polyamic acid.
5. A polyimide which is an imidized product of the polyamic acid composition according to claim 3.
6. 4. A polyimide comprising the polyamic acid composition according to claim 3, which is cast onto a glass substrate and imidized, and which generates an internal stress of 20 MPa or less between the polyimide film and the glass substrate.
7. 6. The polyimide according to claim 5, which has a yellow index (YI) of less than 10 when the film thickness is 10 μm.
8. 6. The polyimide according to claim 5, wherein the 1% weight loss temperature is 500° C. or higher.
9. A laminate comprising the polyimide according to claim 5 and a support.
10. A method for producing a laminate of a polyimide and a support, comprising casting the polyamic acid composition according to claim 3 on a support and heating the composition to effect imidization.
11. A flexible device comprising the polyimide according to claim 5 and an electronic element formed on the polyimide.
Citation Information
Patent Citations
Copolyimide precursor and copolyimide
JP2012041530A
Polyimide precursor and polyimide
JP2016029177A
Polyimide film
TW201713726A
Polymers for use in electronic devices
WO2019195148A1