Photosensitive coloring composition, color filter, liquid crystal display device, and solid imaging element

The photosensitive coloring composition with a specific compound and oxime ester photoinitiator addresses development residues and solvent resistance issues, enhancing the quality of color filters in liquid crystal displays and solid-state image sensors.

JP2024150911AActive Publication Date: 2024-10-24TOYO INK MFG CO LTD

Patent Information

Application Number
JP2023063954
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

Conventional photosensitive coloring compositions used in liquid crystal displays and solid-state image sensors face issues with development residues and lack of solvent resistance, particularly as pixel sizes shrink and color filters become thinner.

Method used

A photosensitive coloring composition containing a colorant, resin, polymerizable compound, and photoinitiator, with a specific compound represented by general formula (1) and a photopolymerization initiator having an oxime ester skeleton, where the colorant content is 45 to 85% by mass, and the polymerizable compound content is 1 to 30% by mass, enhancing solvent resistance and reducing development residues.

Benefits of technology

The composition achieves improved solvent resistance and reduces development residues, enabling the formation of high-quality color filters with suppressed residues, suitable for liquid crystal displays and solid-state image sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150911000001_ABST
    Figure 2024150911000001_ABST
Patent Text Reader

Abstract

To provide a photosensitive coloring composition that has good solvent resistance and allows pattern formation reduced in the development residue.SOLUTION: A photosensitive coloring composition contains a colorant (A), a resin (B), a polymerizable compound (C), and a photoinitiator (D). The content of the colorant (A) is 45 to 85 mass% based on 100 mass% of nonvolatile contents of the photosensitive coloring composition. The polymerizable compound (C) includes a compound (C1) represented by the general formula (1).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive coloring composition for use in the production of color filters for use in liquid crystal displays, solid-state image pickup devices, and the like. [Background technology]

[0002] Color filters that constitute liquid crystal displays (LCDs), solid-state imaging devices, and the like are formed by coating a photosensitive coloring composition on a substrate, and forming a pattern using a photolithography method.

[0003] Generally, color filters used in solid-state imaging devices have smaller pixel sizes and are thinner than LCDs. In addition, solid-state imaging devices themselves are becoming smaller. While color filters are becoming thinner, the chromaticity of the pixels must be maintained, so the colorant concentration in the coating cannot be reduced. Therefore, the content of the colorant in the photosensitive coloring composition must be increased, while the amount of other components (resins, polymerizable compounds, photopolymerization initiators, etc.) must be relatively reduced. As a result, there has been a problem of residues occurring between patterns after the development process (hereinafter referred to as development residues). In response to the above problem, Patent Document 1 discloses a photosensitive coloring composition comprising a fluorine atom-containing surfactant obtained by reacting a copolymer having a hydroxyl group obtained by copolymerizing a radically polymerizable monomer having a poly(perfluoroalkylene ether) chain with a radically polymerizable monomer having a polyalkylene glycol chain, and a compound having an isocyanate group and a radically polymerizable group. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-250256 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, while conventional photosensitive coloring compositions have been able to improve water spots to some extent, there is still room for improvement in terms of development residues, and there is also a problem of insufficient solvent resistance of the cured film.

[0006] An object of the present invention is to provide a photosensitive coloring composition which has good solvent resistance and is capable of forming a pattern with reduced development residue. [Means for solving the problem]

[0007] [1] The photosensitive coloring composition of the present invention comprises a colorant (A), a resin (B), a polymerizable compound (C), and a photopolymerization initiator (D), and the content of the colorant (A) is 45 to 85 mass% in 100 mass% of the nonvolatile content of the photosensitive coloring composition, and the polymerizable compound (C) is a compound (C1) represented by the following general formula (1). General formula (1) [ka]

[0008] (In the general formula (1), X is a partial structure represented by the following general formula (2), general formula (3), or general formula (4).) [ka]

[0009] In the general formula (2), n represents an integer of 2 to 4, and R 3 represents a hydrogen atom or a methyl group. In general formula (3), n represents an integer of 1 to 4. In general formula (4), n represents an integer of 1 to 4. When X in general formula (1) represents general formula (2) or general formula (4), R 1 , R 2 represents a hydrogen atom or a methyl group, and when X in general formula (1) is general formula (3) and n=2, R 1 , R 2 indicates a hydrogen atom, and when n=1, 3, or 4, R 1 , R 2 represents a hydrogen atom or a methyl group.

[0010] [2] The present invention also relates to the photosensitive coloring composition according to claim 1, wherein the content of the polymerizable compound (C) is 1 to 30 mass% in 100 mass% of the nonvolatile content of the photosensitive coloring composition, and the content of the compound (C1) represented by general formula (1) is 50 to 100 mass% in 100 mass% of the polymerizable compound (C).

[0011] [3] The present invention also relates to the photosensitive resin composition [1] or [2] above, wherein the photopolymerization initiator (D) comprises a photopolymerization initiator (D1) having an oxime ester skeleton.

[0012] [4] The present invention also relates to a photosensitive resin composition according to any one of the above [1] to [3], which contains the compound (C1) represented by the general formula (1) in an amount of 5 to 30 mass % based on 100 mass % of the nonvolatile content of the photosensitive coloring composition.

[0013] [5] The present invention further relates to the photosensitive resin composition according to any one of the above [1] to [3], wherein the colorant (A) contains a blue pigment (A1).

[0014] [6] The present invention also relates to a color filter having filter segments formed from the photosensitive coloring composition according to any one of the above [1] to [5].

[0015] [7] The present invention also relates to a solid-state imaging device comprising the color filter according to [6] above.

[0016] [8] The present invention also relates to a liquid crystal display device comprising the color filter according to [6] above. Effect of the Invention

[0017] According to the present invention, it is possible to provide a photosensitive coloring composition having good solvent resistance and capable of forming a pattern with suppressed development residue. Further, the present invention can provide a color filter, a solid-state imaging device, a liquid crystal display device, etc. [Brief description of the drawings]

[0018] [Figure 1]FIG. 1 is a schematic cross-sectional view of a liquid crystal display device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The terms used in the present invention are defined below. When written as "(meth)acryloyl", "(meth)acryl", "(meth)acrylic acid", "(meth)acrylate", or "(meth)acrylamide", unless otherwise specified, it means "acryloyl and / or methacryl", "acrylic and / or methacrylic", "acrylic acid and / or methacrylic acid", "acrylate and / or methacrylate", or "acrylamide and / or methacrylamide", respectively. The polymerizable unsaturated group is a vinyl group, a (meth)acryloyl group, a (meth)allyl group, or the like. In addition, "CI" as used herein means Color Index (CI).

[0020] The photosensitive coloring composition of the present invention comprises a colorant (A), a resin (B), a polymerizable compound (C), and a photopolymerization initiator (D), the content of the colorant (A) being 45 parts by mass or more and 85 parts by mass or less in 100 parts by mass of the total non-volatile content of the photosensitive coloring composition, and the polymerizable compound (C) comprises a compound (C1) represented by the following general formula (1). The photosensitive coloring composition of the present invention is preferably used for, for example, color filter applications. General formula (1) [ka]

[0021] (In the general formula (1), X is a partial structure represented by the following general formula (2), general formula (3), or general formula (4).) [ka]

[0022] In the general formula (2), n represents an integer of 2 to 4, and R 3represents a hydrogen atom or a methyl group. In general formula (3), n represents an integer of 1 to 4. In general formula (4), n represents an integer of 1 to 4. When X in general formula (1) represents general formula (2) or general formula (4), R 1 , R 2 represents a hydrogen atom or a methyl group, and when X in general formula (1) is general formula (3) and n=2, R 1 , R 2 indicates a hydrogen atom, and when n=1, 3, or 4, R 1 , R 2 represents a hydrogen atom or a methyl group.

[0023] The coating film formed from the photosensitive coloring composition of the present invention has a hydrophilic portion, namely, a hydroxyl group and an ether bond derived from the compound (C1) represented by the general formula (1), and therefore has a high affinity to the developer, and the developed portion is easily dissolved during development. This makes it possible to suppress development residues. In addition, the presence of a highly polar hydrophilic portion makes it difficult for non-polar oxygen molecules to coexist in the coating film. This makes it difficult for oxygen inhibition to occur during exposure, and allows the formation of a higher molecular weight crosslinked structure, as well as improving the solvent resistance of the coating film pattern.

[0024] <Colorant (A)> The colorant (A) may be a dye or a pigment. The pigment may be an inorganic pigment or an organic pigment, with the organic pigment being preferred. The colorant (A) is contained in an amount of 45 parts by mass or more and 85 parts by mass or less in 100 parts by mass of the total non-volatile content of the photosensitive coloring composition. This allows the pattern to have a thin film and good chromaticity. The content is preferably 49 parts by mass or more and 65 parts by mass or less.

[0025] Examples of the colorant (A) are given below. Red pigments include, for example, CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 14, 17, 22, 23, 31, 38, 41, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 57:1, 81, 81:1, 81:2, 81:3, 81:4, 83, 88, 90, 105, 112, 119, 122, 123, 144, 146, 149, 150, 155, 166, 168, 169, 170, 171, 172, 175, 176, 177, 178, 179, 184, 185, 187, 188, 19 0, 200, 202, 206, 207, 208, 209, 210, 216, 220, 221, 224, 226, 242, 246, 254, 255, 264, 270, 272, 273, 274, 276, 277, 278, 279, 280, 281, 282, 283, 284, 285, 286, 287, 291, 296. Azo pigments described in JP-A-2014-112527, azo pigments described in JP-A-2013-161026, or diketopyrrolopyrrole pigments described in JP-T-2011-523433, etc. are mentioned. Among these, CI Pigment Red 254 and CI Pigment Red 177 are preferred in terms of high transmittance.

[0026] Examples of orange pigments include CI Pigment Orange 36, 38, 43, 51, 55, 59, 61, 71, and 73. Among these, CI Pigment Orange 71 is preferred in terms of reproducing the color gamut of a color filter. Yellow pigments include, for example, CI Pigment Yellow 1, 1:1, 2, 3, 4, 5, 6, 9, 10, 12, 13, 14, 16, 17, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 41, 42, 43, 48, 53, 55, 61, 62, 62:1, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 109, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 124, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 5, 73, 74, 75, 81, 83, 87, 93, 94, 95, 97, 100, 101, 104, 105, 108, 109, 110, 111, 116, 117, 119, 120, 126, 127, 127:1, 128, 129, 133, 134, 136, 138, 139, 142, 147, 148, 150, 151, 153, 154, 155, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 172, 173, 174, 175, 176, 180, 181, 182, 183, 184, 185, 188, 189, 190, 191, 191:1, 192, 193, 194, 195, 196, 197, 198, 199, 200, 202, 203, 204, 205, 206, 207, 208, 231,233, and quinophthalone compounds described in JP-A-2012-226110. Among these, CI Pigment Yellow 138, 139, 150, and 185, and the quinophthalone compounds described in JP-A-2012-226110 are preferred in terms of reproducing the color gamut of a color filter.

[0027] Examples of green pigments include CI Pigment Green 1, 2, 4, 7, 8, 10, 13, 14, 15, 17, 18, 19, 26, 36, 45, 48, 50, 51, 54, 55, 58, 59, 62, and 63. Among these, from the viewpoint of brightness and coloring power, CI Pigment Green 7, 36, 58, 59, 62, and 63 are preferred. In addition, zinc phthalocyanine pigments described in JP-A-2008-19383, JP-A-2007-320986, and JP-A-2004-70342, and aluminum phthalocyanine pigments described in JP-A-2004-333817 and JP-A-2012-247588 are preferred. Examples of blue pigments include CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 60, 64, and 80. Examples of purple pigments include CI Pigment Violet 1, 19, 23, 27, 29, 30, 32, 37, 40, 42, and 50. Examples of black pigments include carbon black, aniline black, anthraquinone-based black pigments, perylene-based black pigments, etc. Specific examples include CI Pigment Black 1, 6, 7, 12, 20, 31, etc. Also included are metal lake pigments of rhodamine dyes such as CI Pigment Red 81, 81:1, 81:2, 81:3, 81:4, and 81:5.

[0028] Other inorganic pigments include silicon oxide, zirconia oxide, barium sulfate, zinc oxide, lead sulfate, yellow lead, zinc yellow, red iron oxide (red iron (III)), cadmium red, ultramarine, Prussian blue, chromium oxide green, cobalt green, amber, titanium black, synthetic iron black, titanium oxide, iron tetroxide and other metal oxide powders, metal sulfide powders, and metal powders.

[0029] Examples of the dye include acid dyes, direct dyes, basic dyes, salt-forming dyes, oil-soluble dyes, disperse dyes, reactive dyes, mordant dyes, vat dyes, sulfur dyes, etc. Furthermore, the dye may be a derivative of these dyes or a lake pigment obtained by converting a dye into a lake.

[0030] The acid dye preferably has an acid group such as sulfonic acid or carboxylic acid. The direct dye preferably forms an inorganic salt of the acid dye, or a salt-forming compound between the acid dye and a nitrogen-containing compound such as a quaternary ammonium salt compound, a tertiary amine compound, a secondary amine compound, or a primary amine compound. Also preferred are salt-forming compounds that are salts between a resin component having these functional groups and an acid dye. The salt-forming compound is also sulfonamidated to modify it into a sulfonic acid amide compound, which makes it easy to obtain a photosensitive coloring composition with excellent resistance (light resistance, solvent resistance). In addition, a salt-forming compound of an acid dye and a compound having an onium salt group is also preferable because it has excellent resistance (light resistance, solvent resistance). The compound having an onium salt group is preferably a resin having a cationic group.

[0031] Although the basic dye can be used as it is, a salt-forming compound that forms a salt with an organic acid, perchloric acid or a metal salt thereof is preferred. The salt-forming compound of the basic dye is preferred because it has excellent resistance (light resistance, solvent resistance) and affinity with pigments. In addition, the anion component that acts as a counter ion in the salt-forming compound of the basic dye is preferably an organic sulfonic acid, an organic sulfuric acid, a fluorine group-containing phosphorus anion compound, a fluorine group-containing boron anion compound, a cyano group-containing nitrogen anion compound, an anion compound having a conjugate base of an organic acid having a halogenated hydrocarbon group, or a salt-forming compound formed with an acid dye. The resistance of the salt-forming compound is further improved when the salt-forming compound contains a polymerizable unsaturated group in the molecule.

[0032] The chemical structure of the dye may be, for example, an azo dye, a disazo dye, an azomethine dye (such as indoaniline dye, indophenol dye), a dipyrromethene dye, a quinone dye (such as benzoquinone dye, naphthoquinone dye, anthraquinone dye, anthrapyridone dye), a carbonium dye (such as diphenylmethane dye, triphenylmethane dye, xanthene dye, acridine dye), a quinoneimine dye (such as oxazine dye, thiazine ... dyes, etc.), azine dyes, polymethine dyes (oxonol dyes, merocyanine dyes, arylidene dyes, styryl dyes, cyanine dyes, squarylium dyes, croconium dyes, etc.), quinophthalone dyes, phthalocyanine dyes, subphthalocyanine dyes, perinone dyes, indigo dyes, thioindigo dyes, quinoline dyes, nitro dyes, nitroso dyes, rhodamine dyes, and metal complex dyes thereof.

[0033] Among these, from the viewpoint of color properties such as hue, color separation, and color unevenness, azo dyes, xanthene dyes, cyanine dyes, triphenylmethane dyes, anthraquinone dyes, dipyrromethene dyes, squarylium dyes, quinophthalone dyes, phthalocyanine dyes, and subphthalocyanine dyes are preferred, and xanthene dyes, cyanine dyes, triphenylmethane dyes, anthraquinone dyes, dipyrromethene dyes, and phthalocyanine dyes are more preferred.

[0034] The colorant (A) can be used alone or in combination of two or more kinds.

[0035] The colorant (A) preferably contains a blue pigment (A1). Blue pigments are highly hydrophobic and therefore more likely to produce development residues than other colorants when used in large quantities. However, the use of compound (C1) represented by general formula (1) can suppress the generation of residues.

[0036] <Minification of pigments> It is preferable that the organic pigment is micronized before use. The micronization method can be, for example, any of wet grinding, dry grinding, and dissolution precipitation. As exemplified in the present invention, the pigment can be micronized by salt milling using a kneader method, which is a type of wet grinding. The average primary particle size of the pigment determined by TEM (transmission electron microscope) is preferably in the range of 10 to 80 nm. If it is smaller than 10 nm, it becomes difficult to disperse it in an organic solvent, and if it is larger than 80 nm, a sufficient contrast ratio may not be obtained. For these reasons, the average primary particle size is more preferably in the range of 15 to 70 nm.

[0037] The salt milling process is a process in which a mixture of a pigment, a water-soluble inorganic salt, and a water-soluble organic solvent is mechanically kneaded while being heated using a batch or continuous kneader such as a kneader, a two-roll mill, a three-roll mill, a ball mill, an attritor, a sand mill, or a planetary mixer, and then the water-soluble inorganic salt and the water-soluble organic solvent are removed by washing with water. The water-soluble inorganic salt acts as a crushing aid, and the pigment is crushed during salt milling by utilizing the high hardness of the inorganic salt. By optimizing the conditions for salt milling the pigment, it is possible to obtain a pigment with a very fine primary particle size, a narrow distribution width, and a sharp particle size distribution.

[0038] As the water-soluble inorganic salt, sodium chloride, barium chloride, potassium chloride, sodium sulfate, etc. can be used, but sodium chloride (table salt) is preferred from the viewpoint of cost. From the viewpoints of both treatment efficiency and production efficiency, the water-soluble inorganic salt is preferably used in an amount of 50 to 2000 parts by mass, and most preferably 300 to 1000 parts by mass, per 100 parts by mass of the pigment.

[0039] The water-soluble organic solvent is not particularly limited as long as it functions to wet the pigment and the water-soluble inorganic salt, dissolves (mixes) in water, and does not substantially dissolve the inorganic salt used. However, since the temperature rises during salt milling and the solvent becomes easily evaporated, a high boiling point solvent with a boiling point of 120°C or more is preferable from the viewpoint of safety. For example, 2-methoxyethanol, 2-butoxyethanol, 2-(isopentyloxy)ethanol, 2-(hexyloxy)ethanol, diethylene glycol, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, liquid polyethylene glycol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, liquid polypropylene glycol, etc. are used. The water-soluble organic solvent is preferably used in an amount of 5 to 1000 parts by mass, and most preferably 50 to 500 parts by mass, relative to 100 parts by mass of the pigment.

[0040] When the pigment is subjected to salt milling, a resin may be added as necessary. The type of resin used is not particularly limited, and natural resins, modified natural resins, synthetic resins, synthetic resins modified with natural resins, etc. can be used. The resin used is preferably solid at room temperature and insoluble in water, and more preferably partially soluble in the above organic solvents. The amount of the resin used is preferably in the range of 5 to 200 parts by mass relative to 100 parts by mass of the pigment.

[0041] <Metal Removal> If the coloring composition contains a large amount of specific metal elements as impurities other than the pigment components, it may hinder the dispersion stability over time, and may cause a decrease in heat resistance or a decrease in sensitivity. In addition, a color filter made using this may have foreign matter, which may result in a decrease in brightness. The total content of Li, Na, K, Mg, Ca, Fe, Al, and Cr (hereinafter also referred to as specific metal elements) contained in the photosensitive coloring composition is preferably 500 mass ppm or less.

[0042] The total amount of specific metal elements contained in the photosensitive coloring composition is more preferably 300 mass ppm or less, particularly preferably 200 mass ppm or less.The lower limit of the total amount of specific metal elements is not particularly limited, but is preferably 1 mass ppm or more, more preferably 5 mass ppm or more.Within the above range, it is possible to obtain a photosensitive coloring composition that can form a color filter that can suppress costs, has excellent storage stability, and has little generation of foreign matter and little decrease in brightness.

[0043] The amount of each specific metal element contained in the photosensitive coloring composition is preferably 100 ppm by mass or less, and more preferably 50 ppm by mass or less.

[0044] In addition, it is also preferable that the amount of impurities that do not function effectively, such as metals such as Ni, Zn, Cu, Al, Fe, Fe, Co, and Co that constitute the pigment, is small, and these can be removed in the same manner as the specific metal elements by the following method. Furthermore, it is also preferable that Mn, Cs, Ti, Co, Si, Pd, etc., that are mixed in by materials (such as catalysts) used in the manufacturing process of various raw materials for the photosensitive coloring composition, are low in concentration.

[0045] Methods for removing the colorant (A) or metals that have become mixed in from equipment during the manufacturing process include methods using water washing as described in JP-A-2010-83997, JP-A-2018-36521, JP-A-7-198928, JP-A-8-333521, JP-A-2009-7432, etc., and methods for removing magnetic foreign matter using a magnet as described in JP-A-2011-48736, and the like. One or more of these methods can be used as appropriate.

[0046] The content of specific metal elements can be measured by inductively coupled plasma emission spectrometry (ICP).

[0047] <Resin (B)> The resin (B) includes a dispersion resin (B1) and an alkali-soluble resin (B2).

[0048] <Dispersion resin (B1)> The dispersing resin (B1) has an adsorption site that adsorbs to the colorant and a steric repulsion site that disperses the colorant. The dispersing resin (B1) is not particularly limited, and a known resin can be used. Examples of the dispersing resin (B1) include urethane resins, polycarboxylates such as polyacrylates, unsaturated polyamides, polycarboxylic acids, polycarboxylate (partial) amine salts, polycarboxylate ammonium salts, polycarboxylate alkylamine salts, polysiloxanes, long-chain polyaminoamide phosphates, hydroxyl-containing polycarboxylates, and modified products thereof, amides formed by the reaction of poly(lower alkylene imines) with polyesters having free carboxyl groups, salts thereof, water-soluble resins and water-soluble polymer compounds such as (meth)acrylic acid-styrene copolymers, (meth)acrylic acid-(meth)acrylic acid ester copolymers, styrene-maleic acid copolymers, polyvinyl alcohols, and polyvinylpyrrolidone, polyesters, modified polyacrylates, ethylene oxide / propylene oxide adducts, and phosphates. Examples of polymer dispersants having a basic functional group include nitrogen atom-containing graft copolymers, and nitrogen atom-containing acrylic block copolymers and urethane polymer dispersants having functional groups including tertiary amino groups, quaternary ammonium bases, nitrogen-containing heterocycles, etc. in the side chains.

[0049] Commercially available dispersion resins include Disperbyk-101, 103, 107, 108, 110, 111, 116, 130, 140, 154, 161, 162, 163, 164, 165, 166, 167, 168, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 2000, 2001, 2009, 2010, 2020, 2025, 2050, 2070, 2095, 2150, 2155, and 2200, manufactured by BYK Chemical Japan Co., Ltd. 2163, 2164 or Anti-Terra-U, 203, 204 or BYK-P104, P104S, 220S, LPN6919, LPN21116, LPN21324 or Lactimon, Lactimon-WS or Bykumen, SOLSPERSE-3000, 9000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000 manufactured by Nippon Lubrizol Co., Ltd. , 24000, 26000, 27000, 28000, 31845, 32000, 32500, 32550, 33500, 32600, 34750, 35100, 36600, 38500, 41000, 41090, 53095, 55000, 56000, 76500, etc., EFKA-46, 47, 48, 452, 4008, 4009, 4010, 4015, 4020, 4047, 4050, 4055, 4060, 4080, 4400, 4401, 4402, 4403, 4406, 4408, 4300, 4310, 4320, 4330, 4340, 450, 451, 453, 4540, 4550, 4560, 4800, 5010, 5065, 5066, 5070, 7500, 7554, 1101, 120, 150, 1501, 1502, 1503, etc., and Ajispa-PA111, PB711, PB821, PB822, PB824, etc. manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0050] The content of the dispersing resin (B1) is preferably from 1 to 30% by mass, and more preferably from 5 to 20% by mass, based on 100% by mass of the nonvolatile content of the photosensitive coloring composition.

[0051] <Alkali-soluble resin (B2)> The alkali-soluble resin (B2) is, for example, a resin having an acidic group such as a carboxyl group, a sulfonic group, etc. This can impart photolithographic properties to a coating film formed from the photosensitive coloring composition.

[0052] Examples of the resin species of the alkali-soluble resin (B2) include acrylic resins, α-olefin / maleic anhydride copolymers, styrene / styrene sulfonic acid copolymers, ethylene / (meth)acrylic acid copolymers, and isobutylene / maleic anhydride copolymers. Among these, acrylic resins and styrene / styrene sulfonic acid copolymers are preferred.

[0053] The alkali-soluble resin (B2) can be classified into an alkali-soluble resin (B2-1) having no polymerizable unsaturated group, and an alkali-soluble resin (B2-2) having a polymerizable unsaturated group.

[0054] The weight average molecular weight (Mw) of the alkali-soluble resin is preferably 2,000 to 40,000, more preferably 3,000 to 30,000, and even more preferably 4,000 to 20,000, in order to impart solubility in alkali development. The Mw / Mn value is preferably 10 or less. By having a suitable weight average molecular weight (Mw), it is easy to achieve both improved adhesion and suppression of development residues. The acid value of the alkali-soluble resin is preferably from 50 to 200 mgKOH / g, more preferably from 70 to 180 mgKOH / g, and even more preferably from 90 to 170 mgKOH / g. When the resin has a suitable acid value, it is easy to simultaneously improve adhesion and suppress development residues.

[0055] <Alkali-soluble resin having no polymerizable unsaturated group (B2-1)> The alkali-soluble resin (B2-1) having no polymerizable unsaturated group can be appropriately selected from resins such as the acrylic resins already exemplified, and resins obtained by removing the polymerizable unsaturated group from the alkali-soluble resin (B2-2) having a polymerizable unsaturated group described below.

[0056] <Alkali-soluble resin having polymerizable unsaturated group (B2-2)> The alkali-soluble resin (B2-2) having a polymerizable unsaturated group may be, for example, a resin obtained by adding a polymerizable unsaturated group to the resin such as the acrylic resin already exemplified. In this specification, for example, the resin synthesized by the following method (i) or (ii) is preferred. This allows the coating formed from the photosensitive coloring composition to have a higher crosslink density due to light irradiation.

[0057] [Method (i)] In the method (i), for example, a polymer of an epoxy group-containing monomer and other monomers is first synthesized, and then a carboxyl group-containing monomer is added to the epoxy group of the polymer, and the resulting hydroxyl group is reacted with a polybasic acid anhydride to obtain an alkali-soluble resin (C2).

[0058] Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 2-glycidoxyethyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, and 3,4-epoxycyclohexyl (meth)acrylate. Among these, glycidyl (meth)acrylate is preferred from the viewpoint of reactivity.

[0059] Examples of the monocarboxyl group-containing monomer include monocarboxylic acids such as (meth)acrylic acid, crotonic acid, o-, m-, and p-vinylbenzoic acid, and (meth)acrylic acid substituted with haloalkyl, alkoxyl, halogen, nitro, or cyano at the α-position.

[0060] Examples of polybasic acid anhydrides include tetrahydrophthalic anhydride, phthalic anhydride, hexahydrophthalic anhydride, succinic anhydride, and maleic anhydride.

[0061] The monomers and polybasic acid anhydrides can each be used alone or in combination of two or more kinds.

[0062] As a method similar to the method (i), for example, a carboxyl group-containing monomer and other monomers are synthesized to prepare a polymer, and then an epoxy group-containing monomer is added to a part of the carboxyl groups of the polymer to obtain an alkali-soluble resin (C2).

[0063] [Method (ii)] In the method (ii), for example, a hydroxyl group-containing monomer, a carboxyl group-containing monomer, and other monomers are synthesized to prepare a polymer, and then the hydroxyl group of the polymer is reacted with an isocyanate group of an isocyanate group-containing monomer.

[0064] The hydroxyl group-containing monomer may be any of the monomers already exemplified. Among them, 2-hydroxyethyl methacrylate and glycerol mono(meth)acrylate are preferred in terms of preventing foreign matter from being generated in the coating. Glycerol mono(meth)acrylate is also preferred in terms of photosensitivity.

[0065] Examples of the monomer having an isocyanate group include 2-(meth)acryloylethyl isocyanate, 2-(meth)acryloyloxyethyl isocyanate, and 1,1-bis[methacryloyloxy]ethyl isocyanate.

[0066] Other monomers that can be used in the synthesis of alkali-soluble resins include (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, or ethoxypolyethylene glycol (meth)acrylate; Alternatively, examples of the monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, diacetone(meth)acrylamide, and acryloylmorpholine; styrenes such as styrene and α-methylstyrene; vinyl ethers such as ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, and isobutyl vinyl ether; and fatty acid vinyls such as vinyl acetate and vinyl propionate.

[0067] Cyclohexylmaleimide, phenylmaleimide, methylmaleimide, ethylmaleimide, 1,2-bismaleimidoethane 1,6-bismaleimidohexane, 3-maleimidopropionic acid, 6,7-methylenedioxy-4-methyl-3-maleimidocoumarin, 4,4'-bismaleimidodiphenylmethane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, N,N'-1,3-phenylenedimaleimide, N,N'-1,4-phenylenedimaleimide, N-(1-pyrenyl)maleimide, N-(2,4,6-trichloro N-substituted maleimides such as N-(4-aminophenyl)maleimide, N-(4-nitrophenyl)maleimide, N-benzylmaleimide, N-bromomethyl-2,3-dichloromaleimide, N-succinimidyl-3-maleimide benzoate, N-succinimidyl-3-maleimide propionate, N-succinimidyl-4-maleimide butyrate, N-succinimidyl-6-maleimide hexanoate, N-[4-(2-benzimidazolyl)phenyl]maleimide, and 9-maleimide acridine; Also included are monomers represented by the following general formula (4). Examples of the monomers represented by general formula (4) include EO-modified cresol acrylate, n-nonylphenoxy polyethylene glycol acrylate, phenoxyethyl acrylate, ethoxylated phenyl acrylate, ethylene oxide (EO)-modified (meth)acrylate of phenol, EO- or propylene oxide (PO)-modified (meth)acrylate of paracumylphenol, EO-modified (meth)acrylate of nonylphenol, and PO-modified (meth)acrylate of nonylphenol. Here, EO means ethyleneoxy, and PO means propyleneoxy.

[0068] General formula (4) [ka]

[0069] (In general formula (4), R6 is a hydrogen atom or a methyl group, R7 is an alkylene group having 2 or 3 carbon atoms, R8 is an alkyl group having 1 to 20 carbon atoms which may have a benzene ring, and n is an integer of 1 to 15.)

[0070] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2- or 3-hydroxypropyl (meth)acrylate, 2-, 3- or 4-hydroxybutyl (meth)acrylate, and cyclohexanedimethanol mono(meth)acrylate. Examples of the hydroxyalkyl (meth)acrylate include polyether mono(meth)acrylates obtained by addition polymerization of ethylene oxide, propylene oxide, and / or butylene oxide to the above hydroxyalkyl (meth)acrylates, and (poly)ester mono(meth)acrylates obtained by addition of (poly)γ-valerolactone, (poly)ε-caprolactone, and / or (poly)12-hydroxystearic acid.

[0071] The content of the binder resin (B2) is preferably from 3 to 20 mass %, more preferably from 4 to 17 mass %, based on 100 mass % of the nonvolatile content of the photosensitive coloring composition.

[0072] The resin (B) can be used alone or in combination of two or more kinds.

[0073] <Dye derivative (b)> The photosensitive coloring composition of the present invention can use a dye derivative (b). The dye derivative (b) is a compound having an acidic group, a basic group, a neutral group, or the like in an organic dye residue. Examples of the dye derivative include compounds having an acidic substituent such as a sulfo group, a carboxy group, or a phosphate group, and their amine salts, compounds having a basic substituent such as a sulfonamide group or a tertiary amino group at the end, and compounds having a neutral substituent such as a phenyl group or a phthalimidoalkyl group. Since the resin-type dispersant used in combination has an acidic group, a dye derivative having a basic group is preferred. Examples of the organic dye of the organic dye residue include diketopyrrolopyrrole pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, perinone pigments, perylene pigments, thiazineindigo pigments, triazine pigments, benzimidazolone pigments, indole pigments such as benzoisoindole, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, naphthol pigments, threne pigments, metal complex pigments, azo pigments such as azo, disazo, and polyazo, and the like. These dye derivatives can be used alone or in combination of two or more kinds.

[0074] The amount of the dye derivative used is preferably from 1 to 30 parts by mass, more preferably from 3 to 25 parts by mass, and even more preferably from 5 to 20 parts by mass, relative to 100 parts by mass of the colorant (A).

[0075] By adding a dye derivative to a pigment and carrying out a micronization treatment such as acid pasting, acid slurry, dry milling, salt milling, or solvent salt milling, the dye derivative is adsorbed onto the pigment surface, and the primary particles of the pigment can be made finer than when the dye derivative is not added.

[0076] <Polymerizable compound (C)> The polymerizable compound (C) may be a monomer or oligomer having a polymerizable unsaturated group. The polymerizable compound (C) may be, for example, a compound (C1) represented by general formula (1), a polymerizable compound having an acid group, a polymerizable compound having a urethane bond, or other polymerizable compounds. In this specification, the compound (C1) represented by general formula (1) is included.

[0077] (Polymerizable compound (C1)) A coating containing the compound (C1) represented by general formula (1) has highly hydrophilic ether bonds and hydroxyl groups in the developed portion after photocuring, which increases solubility in an alkaline developer and reduces development residues. On the other hand, the non-developed portion has highly polar hydrophilic sites, which makes it less susceptible to oxygen inhibition, and is less soluble in an alkaline developer because a higher molecular weight crosslinked body can be formed by photocuring. In addition, high solvent resistance can be obtained by forming a high molecular weight crosslinked structure. General formula (1) [ka]

[0078] (In the general formula (1), X is a partial structure represented by the following general formula (2), general formula (3), or general formula (4).) [ka]

[0079] In the general formula (2), n represents an integer of 2 to 4, and R 3 represents a hydrogen atom or a methyl group. In general formula (3), n represents an integer of 1 to 4. In general formula (4), n represents an integer of 1 to 4. When X in general formula (1) represents general formula (2) or general formula (4), R 1 , R 2 represents a hydrogen atom or a methyl group, and when X in general formula (1) is general formula (3) and n=2, R 1 , R 2 indicates a hydrogen atom, and when n=1, 3, or 4, R 1 , R 2 represents a hydrogen atom or a methyl group.

[0080] Examples of the compound (C1) represented by the general formula (1) include diethylene glycol diglycidyl ether di(meth)acrylate, triethylene glycol diglycidyl ether di(meth)acrylate, tetraethylene glycol diglycidyl ether di(meth)acrylate, dipropylene glycol diglycidyl ether di(meth)acrylate, tripropylene glycol diglycidyl ether di(meth)acrylate, tetrapropylene glycol diglycidyl ether di(meth)acrylate, methylene glycol diglycidyl ether di(meth)acrylate, diglycidyl ether di(meth)acrylate, ethylene glycol diglycidyl ether diacrylate, 1,3-propanediol diglycidyl ether di(meth)acrylate, 1,4-butanediol diglycidyl ether di(meth)acrylate, glycerin diglycidyl ether di(meth)acrylate, diglycerin diglycidyl ether di(meth)acrylate, triglycerin diglycidyl ether di(meth)acrylate, tetraglycerin diglycidyl ether di(meth)acrylate, and the like.

[0081] In the general formula (2), n is preferably 3 or 4, and in the general formula (3), n is preferably 3 or 4. In the general formula (4), n is preferably 1.

[0082] The content of the compound (C1) represented by the general formula (1) is preferably from 5 to 30 mass %, and more preferably from 5 to 20 mass %, in 100 mass % of the nonvolatile content of the photosensitive coloring composition.

[0083] (Polymerizable compound having an acid group) Examples of the acid group of the polymerizable compound having an acid group include a sulfonic acid group, a carboxyl group, and a phosphoric acid group.

[0084] Examples of the polymerizable compound having an acid group include esters of free hydroxyl group-containing poly(meth)acrylates of polyhydric alcohols and (meth)acrylic acid with dicarboxylic acids; esters of polycarboxylic acids with monohydroxyalkyl (meth)acrylates; and the like. Specific examples include free carboxyl group-containing monoesters of monohydroxy oligoacrylates or monohydroxy oligomethacrylates, such as trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol pentamethacrylate, with dicarboxylic acids, such as malonic acid, succinic acid, glutaric acid, and phthalic acid; and free carboxyl group-containing oligoesters of tricarboxylic acids, such as propane-1,2,3-tricarboxylic acid (tricarballylic acid), butane-1,2,4-tricarboxylic acid, benzene-1,2,3-tricarboxylic acid, benzene-1,3,4-tricarboxylic acid, and benzene-1,3,5-tricarboxylic acid, with monohydroxy monoacrylates or monohydroxy monomethacrylates, such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, and 2-hydroxypropyl methacrylate.

[0085] Commercially available products include Viscoat #2500P manufactured by Osaka Organic Chemical Industry Co., Ltd., and Aronix M-5300, M-5400, M-5700, M-510, and M-520 manufactured by Toagosei Co., Ltd.

[0086] (Polymerizable compound having a urethane bond) Examples of the polymerizable compound having a urethane bond include a polyfunctional urethane acrylate obtained by reacting a (meth)acrylate having a hydroxyl group with a polyfunctional isocyanate, and a polyfunctional urethane acrylate obtained by reacting an alcohol with a polyfunctional isocyanate and further reacting the alcohol with a (meth)acrylate having a hydroxyl group.

[0087] Examples of the (meth)acrylate having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol ethylene oxide modified penta(meth)acrylate, dipentaerythritol propylene oxide modified penta(meth)acrylate, dipentaerythritol caprolactone modified penta(meth)acrylate, glycerol acrylate methacrylate, glycerol dimethacrylate, 2-hydroxy-3-acryloylpropyl methacrylate, a reaction product of an epoxy group-containing compound and a carboxy(meth)acrylate, and a hydroxyl group-containing polyol polyacrylate.

[0088] Examples of the polyfunctional isocyanate include tolylene diisocyanate, hexamethylene diisocyanate, diphenylmethylene diisocyanate, isophorone diisocyanate, and polyisocyanate.

[0089] Commercially available products include AH-600, AT-600, UA-306H, UA-306T, UA-306I, UA-510H, UF-8001G, and DAUA-167 manufactured by Kyoeisha Chemical Co., Ltd., UA-160TM manufactured by Shin-Nakamura Chemical Co., Ltd., and UV-4108F and UV-4117F manufactured by Osaka Organic Chemical Industry Co., Ltd.

[0090] Other polymerizable compounds include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, cyclohexyl (meth)acrylate, β-carboxyethyl (meth)acrylate, polyethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, phenoxytetraethylene glycol (meth)acrylate, phenoxyhexaethylene glycol (meth)acrylate, trimethylolpropane PO-modified tri(meth)acrylate, trimethylolpropane EO-modified tri(meth)acrylate, isocyanuric acid EO-modified di(meth)acrylate, isocyanuric acid EO-modified tri(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate. , pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, 1,6-hexanediol diglycidyl ether di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol diglycidyl ether di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, tricyclodecanyl (meth)acrylate, (meth)acrylic acid ester of methylolated melamine, epoxy (meth)acrylate, urethane acrylate, and other various acrylic acid esters and methacrylic acid esters, (meth)acrylic acid, styrene, vinyl acetate, hydroxyethyl vinyl ether, ethylene glycol divinyl ether, pentaerythritol trivinyl ether, (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-vinyl formamide, and acrylonitrile.

[0091] Commercially available products include KAYARAD R-128H, R526, PEG400DA, MAND, NPGDA, R-167, HX-220, R-551, R712, R-604, R-684, GPO-303, TMPTA, DPHA, DPEA-12, DPHA-2C, D-310, D-330, DPCA-20, DPCA-30, DPCA-60, and DPCA-120 manufactured by Nippon Kayaku Co., Ltd., and Aronix M-303, M-305, M-306, M-309, M-310, and M-320 manufactured by Toagosei Co., Ltd. Examples of such acrylic resins include 321, M-325, M-350, M-360, M-313, M-315, M-400, M-402, M-403, M-404, M-405, M-406, M-450, M-452, M-408, M-211B, and M-101A, Viscoat #310HP, #335HP, #700, #295, #330, #360, #GPT, #400, and #405 manufactured by Osaka Organic Chemical Industry Co., Ltd., and NK Ester A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd.

[0092] The polymerizable compound (C) can be used alone or in combination of two or more kinds.

[0093] The content of the polymerizable compound (C) is preferably 1 to 30 mass%, more preferably 2 to 25 mass%, based on 100 mass% of the nonvolatile content of the photosensitive coloring composition. The content of the compound (C1) represented by the general formula (1) is preferably 50 to 100 mass%, more preferably 70 to 100 mass%, based on 100 mass% of the polymerizable compound (C).

[0094] <Photopolymerization initiator (D)> The photopolymerization initiator (D) preferably contains an oxime ester-based polymerization initiator (D1).

[0095] (Oxime ester photoinitiator (D1)) In the oxime ester photopolymerization initiator (D1), the NO bond of the oxime is cleaved by absorbing ultraviolet light, generating iminyl radicals and alkyloxy radicals. These radicals further decompose to generate highly active radicals, so patterns can be formed with less exposure compared to when other photopolymerization initiators are used, improving photocuring properties.

[0096] The oxime ester photopolymerization initiator (D1) can be classified according to the skeleton in the molecule, and includes a carbazole skeleton, a fluorene skeleton, a diphenyl skeleton, and a dioxime skeleton having two oxime ester groups. The specific structure in the molecule is preferably a hydroxyl group, a nitro group, a carbonyl group, a fluorocarbon group, or a benzofuran.

[0097] (Oxime ester photoinitiator with diphenyl skeleton) [ka]

[0098] (Oxime ester photopolymerization initiator having a carbazole skeleton) [ka] JPEG2024150911000011.jpg103148

[0099] (Fluorene skeleton-containing oxime ester photoinitiator) [ka]

[0100] (Oxime ester photoinitiator with two oxime ester groups) As shown below, examples of the photopolymerization initiator include an oxime ester type photopolymerization initiator having two oxime ester groups on both sides of a carbazole skeleton or a phenothiazine skeleton. [ka]

[0101] Among these, oxime ester photopolymerization initiators having a carbazole structure, oxime ester photopolymerization initiators having a diphenyl skeleton, and oxime ester photopolymerization initiators having two oxime ester groups (including those having a carbazole skeleton) are preferred, and oxime ester photopolymerization initiators having a carbazole structure are the most preferred. In addition, for oxime ester photopolymerization initiators having a diphenyl skeleton, if the molecular weight of the radical compound generated upon exposure is high, the mobility in the coating film decreases and the radical reactivity with the polymerizable compound decreases, so it is preferable that the terminal of the ester moiety in the oxime ester moiety does not become a phenyl ester.

[0102] Other examples of the oxime ester photopolymerization initiator include 3-benzoyloxyiminobutan-2-one, 3-acetoxyiminobutan-2-one, 3-propionyloxyiminobutan-2-one, 2-acetoxyiminopentan-3-one, 2-acetoxyimino-1-phenylpropan-1-one, 2-benzoyloxyimino-1-phenylpropan-1-one, 3-(4-toluenesulfonyloxy)iminobutan-2-one, and 2-ethoxycarbonyloxyimino-1-phenylpropan-1-one.

[0103] Examples of the oxime ester-based photopolymerization initiator include compounds described in JP-A-2001-233842, compounds described in JP-A-2000-80068, compounds described in JP-A-2006-342166, compounds described in J.C.S. Perkin II (1979, pp. 1653-1660), compounds described in J.C.S. Perkin II (1979, pp. 156-162), compounds described in Journal of Photopolymer Science and Compounds described in JP-A-2000-66385, compounds described in JP-A-2000-80068, compounds described in JP-T-2004-534797, compounds described in JP-A-2006-342166, compounds described in JP-A-2017-19766, compounds described in JP-A-6065596, compounds described in WO 2017 Examples of the compound include those described in WO2015 / 152153, WO2017 / 051680, JP2007-210991A, JP2009-179619A, JP2010-037223A, JP2010-215575A, and JP2011-020998A.

[0104] As the photopolymerization initiator (D), other photopolymerization initiators can be used in combination with the oxime ester photopolymerization initiator (D1). Other photopolymerization initiators include, for example, 4-phenoxydichloroacetophenone, 4-t-butyl-dichloroacetophenone, diethoxyacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-1-[4-(4-morpholino)phenyl]-2-(phenylmethyl)-1-butanone, or 2-(dimethylamino)-2-[(4- acetophenone compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, or benzil dimethyl ketal; benzophenone, benzoylbenzoic acid, benzoylbenzoic acid methyl, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, or 3,3',4,4'-tetra(t- butylperoxycarbonyl)benzophenone and other benzophenone compounds; thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, 2,4-diethylthioxanthone and other thioxanthone compounds; 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis( triazine-based compounds such as 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, or 2,4-trichloromethyl-(4'-methoxystyryl)-6-triazine;Examples of the compounds include phosphine-based compounds such as bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and diphenyl-2,4,6-trimethylbenzoylphosphine oxide; quinone-based compounds such as 9,10-phenanthrenequinone, camphorquinone, and ethylanthraquinone; borate-based compounds; carbazole-based compounds; imidazole-based compounds; and titanocene-based compounds.

[0105] The content of the photopolymerization initiator (D) is preferably 0.1 to 20 parts by mass, and more preferably 0.2 to 10 parts by mass, in 100 parts by mass of the nonvolatile content of the photosensitive composition. When an appropriate amount is added, the photocurability is improved and development residues can be further suppressed.

[0106] <Organic solvent (S)> The organic solvent (S) is not particularly limited, and known compounds can be used. For example, 1,2,3-trichloropropane, 1-methoxy-2-propanol, ethyl lactate, 1,3-butanediol, 1,3-butylene glycol, 1,3-butylene glycol diacetate, 1,4-dioxane, 2-heptanone, 2-methyl-1,3-propanediol, 3,5,5-trimethyl-2-cyclohexen-1-one, 3,3,5-trimethylcyclohexanone, 3-ethoxyethyl propionate, 3-methyl-1,3-butanediol, 3-methoxy-3-methyl-1-butanol, 3-methoxy-3-methyl butyl acetate, 3-methoxybutanol, 3-methoxybutyl acetate, 4-heptanone, m-xylene, m-diethylbenzene, m-dichlorobenzene, N,N-dimethylacetamide, N,N-dimethylformamide, n-butyl alcohol, n-butylbenzene, n-propyl acetate, N-methylpyrrolidone, o-xylene, toluene, o-chlorotoluene, benzene, o-diethylbenzene, o-dichlorobenzene, p-chlorotoluene, p-diethylbenzene, sec-butylbenzene, tert-butyl Benzene, γ-butyrolactone, isobutyl alcohol, isophorone, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monotertiary butyl ether, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, ethylene glycol monopropyl ether, ethylene glycol monohexyl ether, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, diisobutyl ketone, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether, cyclohexanol, cyclohexanol acetate, cyclohexanone,Dipropylene glycol dimethyl ether, dipropylene glycol methyl ether acetate, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monomethyl ether, diacetone alcohol, triacetin, tripropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, propylene glycol diacetate, propylene glycol phenyl ether, propylene glycol monoethyl ether, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether propionate, benzyl alcohol, methyl isobutyl ketone, methylcyclohexanol, n-amyl acetate, n-butyl acetate, isoamyl acetate, isobutyl acetate, propyl acetate, dibasic acid esters, etc.,

[0107] <Thermosetting compound (E)> In this specification, the composition may further contain a thermosetting compound (E), which reacts in a post-bake step after pattern formation by photolithography to increase the crosslink density and improve heat resistance.

[0108] Examples of the thermosetting compound (E) include epoxy compounds, oxetane compounds, benzoguanamine compounds, rosin-modified maleic acid compounds, rosin-modified fumaric acid compounds, melamine compounds, urea compounds, and phenol compounds. Among these, epoxy compounds and oxetane compounds are preferred.

[0109] (Epoxy compounds) Examples of epoxy compounds include polycondensates of bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.), phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), polycondensates of phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene ... Examples of the epoxy resins include polymers of phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.), polycondensates of phenols and aromatic dimethanols (benzene dimethanol, α,α,α',α'-benzene dimethanol, biphenyl dimethanol, α,α,α',α'-biphenyl dimethanol, etc.), polycondensates of phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethylbiphenyl, etc.), polycondensates of bisphenols and various aldehydes, glycidyl ether epoxy resins obtained by glycidylating alcohols, alicyclic epoxy resins, heterocyclic epoxy resins, aliphatic epoxy resins, glycidyl amine epoxy resins, and glycidyl ester epoxy resins.

[0110] Commercially available products include, for example, Epicoat 807, Epicoat 815, Epicoat 825, Epicoat 827, Epicoat 828, Epicoat 190P, Epicoat 191P (all trade names; manufactured by Yuka Shell Epoxy Co., Ltd.), Epicoat 1004, Epicoat 1256 (all trade names; manufactured by Japan Epoxy Resins Co., Ltd.), TECHMORE VG3101L (trade name; manufactured by Mitsui Chemicals, Inc.), EPPN-501H, 502H (trade names; manufactured by Nippon Kayaku Co., Ltd.), JER 1032H60 (trade name; manufactured by Japan Epoxy Resins Co., Ltd.), JER 157S65, 157S70 (product name; manufactured by Japan Epoxy Resin Co., Ltd.), EPPN-201 (product name; manufactured by Nippon Kayaku Co., Ltd.), JER152, JER154 (all of the above are product names; manufactured by Japan Epoxy Resin Co., Ltd.), EOCN-102S, EOCN-103S, EOCN-104S, EOCN-1020 (all of the above are product names; manufactured by Nippon Kayaku Co., Ltd.), Celloxide 2021, EHPE- 3150 (all trade names; manufactured by Daicel Chemical Industries, Ltd.), Denacol EX-211, 212, 252, 313, 314, 321, 411, 421, 512, 521, 611, 612, 614, 614B, 622, 711, 721 (all trade names; manufactured by Nagase ChemteX Corporation), TEPIC-L, TEPIC-H, TEPIC-S (manufactured by Nissan Chemical Industries, Ltd.), and the like.

[0111] The content of the epoxy compound is preferably from 0.5 to 50 mass %, and more preferably from 1 to 40 mass %, in 100 mass % of the nonvolatile content of the photosensitive coloring composition.

[0112] (Oxetane Compounds) The oxetane compound is a known compound having an oxetane group. Examples of the oxetane compound include monofunctional oxetane compounds, bifunctional oxetane compounds, and trifunctional or higher oxetane compounds.

[0113] Examples of monofunctional oxetane compounds include (3-ethyloxetan-3-yl)methyl acrylate, (3-ethyloxetan-3-yl)methyl methacrylate, 3-ethyl-3-hydroxymethyloxetane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-(phenoxymethyl)oxetane, 3-ethyl-3-(2-methacryloxymethyl)oxetane, and 3-ethyl-3-{[3-(triethoxysilyl)propoxy]methyl}oxetane.

[0114] Examples of the bifunctional oxetane compound include 4,4'-bis[(3-ethyl-3-oxetanyl)methoxymethyl]biphenyl), 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, di[1-ethyl(3-oxetanyl)]methyl ether, di[1-ethyl(3-oxetanyl)]methyl ether 3-ethyl-3-hydroxymethyl oxetane, 3- Ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-(2-phenoxymethyl)oxetane, 3,7-bis(3-oxetanyl)-5-oxa-nonane, 1,2-bis[(3-ethyl-3-oxetanylmethoxy)methyl]ethane, 1,3-bis[(3-ethyl-3-oxetanylmethoxy)methyl]propane, ethyleneglycol bis(3-ethyl-3-oxetanylmethyl)ether, dicyclopentenyl bis(3-ethyl- 3-oxetanylmethyl) ether, triethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, tetraethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, 1,4-bis(3-ethyl-3-oxetanylmethoxy)butane, 1,6-bis(3-ethyl-3-oxetanylmethoxy)hexane, polyethylene glycol bis(3-ethyl-3-oxetanylmethyl) ether, ethylene oxide (EO)-modified bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, propylene oxide (PO)-modified bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, EO-modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, PO-modified hydrogenated bisphenol A bis(3-ethyl-3-oxetanylmethyl) ether, EO-modified bisphenol F(3-ethyl-3-oxetanylmethyl) ether, and the like.

[0115] Examples of the trifunctional or higher oxetane compounds include pentaerythritol tris(3-ethyl-3-oxetanylmethyl) ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol hexa(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl) ether, dipentaerythritol hexa(3-ethyl-3-oxetanylmethyl) ether, caprolactone-modified dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl) ether, caprolactone-modified dipentaerythritol pentakis(3-ethyl-3-oxetanylmethyl) ether, ditrimethylolpropane tetrakis(3-ethyl-3-oxetanylmethyl) ether, and resins containing an oxetane group (for example, the oxetane-modified phenol novolak resin described in Japanese Patent No. 3783462).

[0116] Examples of commercially available oxetane compounds include OXBP and OXTP manufactured by Ube Industries, OXE-10 and 30 manufactured by Osaka Organic Chemical Industry Co., Ltd., and OXT-101 and 212 manufactured by Toagosei Co., Ltd.

[0117] The content of the oxetane compound is preferably from 0.5 to 50 mass %, and more preferably from 1 to 40 mass %, in 100 mass % of the nonvolatile content of the photosensitive coloring composition.

[0118] (Melamine compounds) The melamine compound is a compound having a melamine ring structure. The melamine compound is preferably a methylol type or ether type compound, and more preferably a melamine compound having an average of 5.0 or more methylol groups and / or ether groups per melamine ring. If the melamine compound has an appropriate number of methylol groups or ether groups, it is easy to obtain the right heat resistance.

[0119] Examples of commercially available melamine compounds include Nikalac MW-30HM, MW-390, MW-100LM, MX-750LM, MW-30M, MW-30, MW-22, MS-21, MS-11, MW-24X, MS-001, MX-002, MX-730, MX-750, MX-708, MX-706, MX-042, MX-45, MX-500, MX-520, MX-43, MX-417, and MX-410 manufactured by Sanwa Chemical Co., Ltd., and Cymel 232, 235, 236, 238, 285, 300, 301, 303, 350, and 370 manufactured by Nippon Cytec Industries Co., Ltd.

[0120] The melamine compounds can be used alone or in combination of two or more kinds.

[0121] The content of the melamine compound is preferably from 0.01 to 10 mass %, and more preferably from 0.1 to 5 mass %, based on 100 mass % of the nonvolatile content of the photosensitive coloring composition.

[0122] The thermosetting compound (E) can be used alone or in combination of two or more kinds.

[0123] (hardening agent) The photosensitive coloring composition of the present invention may contain a curing agent (curing accelerator) to assist the curing of the thermosetting compound.

[0124] Examples of the curing agent include amine compounds, acid anhydrides, active esters, carboxylic acid compounds, sulfonic acid compounds, etc. Examples of the curing agent include amine compounds (e.g., dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, 4-methyl-N,N-dimethylbenzylamine, etc.), quaternary ammonium salt compounds (e.g., triethylbenzylammonium chloride, etc.), blocked isocyanate compounds (e.g., dimethylamine, etc.), imidazole derivative bicyclic amidine compounds and their salts (e.g., imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole, etc.), phosphorus compounds (e.g., triphenylphosphine, etc.), S-triazine derivatives (e.g., 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct, etc.).

[0125] The curing agents can be used alone or in combination of two or more kinds.

[0126] The content of the curing agent is preferably 0.01 to 15 parts by mass based on 100 parts by mass of the thermosetting compound (I).

[0127] <Sensitizer (F)> The photosensitive coloring composition of the present invention may further contain a sensitizer. Examples of sensitizers include chalcone derivatives, unsaturated ketones such as dibenzalacetone, 1,2-diketone derivatives such as benzil and camphorquinone, benzoin derivatives, fluorene derivatives, naphthoquinone derivatives, anthraquinone derivatives, xanthene derivatives, thioxanthene derivatives, xanthone derivatives, thioxanthone derivatives, coumarin derivatives, ketocoumarin derivatives, cyanine derivatives, merocyanine derivatives, and oxonol derivatives, and other polymethine dyes, acridine derivatives, azine derivatives, thiazine derivatives, oxazine derivatives, indoline derivatives, azulene derivatives, azulenium derivatives, squarylium derivatives, porphyrin derivatives, tetraphenylporphyrin derivatives, triarylmethane derivatives, tetrabenzoporphyrin derivatives, and tetrapyrazinoporphyrazine derivatives. , phthalocyanine derivatives, tetraazaporphyrazine derivatives, tetraquinoxalyloporphyrazine derivatives, naphthalocyanine derivatives, subphthalocyanine derivatives, pyrylium derivatives, thiopyrylium derivatives, tetraphylline derivatives, annulene derivatives, spiropyran derivatives, spirooxazine derivatives, thiospiropyran derivatives, metal arene complexes, organic ruthenium complexes, or Michler's ketone derivatives, α-acyloxy esters, acylphosphine oxides, methylphenyl glyoxylates, benzyl, 9,10-phenanthrenequinone, camphorquinone, ethyl anthraquinone, 4,4'-diethylisophthalophenone, 3,3' or 4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 4,4'-bis(diethylamino)benzophenone, and the like.

[0128] Commercially available products include "KAYACURE DETX-S" (2,4-diethylthioxanthone, manufactured by Nippon Kayaku Co., Ltd.) and "CHEMARK DEABP" (4,4'-bis(diethylamino)benzophenone, manufactured by Chemark Chemical Co., Ltd.).

[0129] The sensitizers can be used alone or in combination of two or more.

[0130] The content of the sensitizer is preferably 3 to 60 parts by mass, more preferably 5 to 50 parts by mass, based on 100 parts by mass of the photopolymerization initiator (D). When an appropriate amount is contained, the photocurability is improved and development residues can be further suppressed.

[0131] <Thiol-based chain transfer agent (G)> The photosensitive coloring composition of the present invention can contain a thiol chain transfer agent (G). When the thiol chain transfer agent (G) is used in combination with a photopolymerization initiator, it generates a thiyl radical that is not easily inhibited by oxygen during radical polymerization after irradiation with light, and the sensitivity of the photosensitive coloring composition is improved.

[0132] The thiol chain transfer agent is preferably a polyfunctional thiol having two or more thiol groups (SH groups). It is more preferable that the thiol chain transfer agent has four or more SH groups. As the number of functional groups increases, the coating becomes easier to photocure from the surface to the deepest part.

[0133] Examples of polyfunctional thiols include hexanedithiol, decanedithiol, 1,4-butanediol bisthiopropionate, 1,4-butanediol bisthioglycolate, ethylene glycol bisthioglycolate, ethylene glycol bisthiopropionate, trimethylolpropane tristhioglycolate, trimethylolpropane tristhiopropionate, trimethylolpropane tris(3-mercaptobutyrate), pentaerythritol tetrakisthioglycolate, pentaerythritol tetrakisthioglycolate, and ethylene glycol bisthiopropionate. Examples of the thiopropionate include erythritol tetrakisthiopropionate, trimercaptopropionic acid tris(2-hydroxyethyl)isocyanurate, 1,4-dimethylmercaptobenzene, 2,4,6-trimercapto-s-triazine, 2-(N,N-dibutylamino)-4,6-dimercapto-s-triazine, and preferably, ethylene glycol bisthiopropionate, trimethylolpropane tristhiopropionate, and pentaerythritol tetrakisthiopropionate.

[0134] The thiol chain transfer agents can be used alone or in combination of two or more.

[0135] The content of the thiol chain transfer agent is preferably 0.1 to 10 mass%, more preferably 0.1 to 3 mass%, based on 100 mass% of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the photosensitivity and taper shape are improved, and wrinkles are less likely to occur on the coating surface.

[0136] <Polymerization inhibitor (H)> The photosensitive coloring composition may contain a polymerization inhibitor, which can suppress photosensitivity due to diffracted light from a mask during exposure in a photolithography method, making it easier to obtain a pattern of a desired shape.

[0137] Examples of the polymerization inhibitor include alkyl catechol compounds such as catechol, resorcinol, 1,4-hydroquinone, 2-methyl catechol, 3-methyl catechol, 4-methyl catechol, 2-ethyl catechol, 3-ethyl catechol, 4-ethyl catechol, 2-propyl catechol, 3-propyl catechol, 4-propyl catechol, 2-n-butyl catechol, 3-n-butyl catechol, 4-n-butyl catechol, 2-tert-butyl catechol, 3-tert-butyl catechol, 4-tert-butyl catechol, and 3,5-di-tert-butyl catechol; 2-methyl resorcinol, 4-methyl resorcinol, 2-ethyl resorcinol, 4-ethyl resorcinol, 2-propyl resorcinol, 4-propyl resorcinol, and 2-n-butyl catechol. Examples of the alkyl resorcinol include alkyl resorcinol compounds such as ethylresorcinol, 4-n-butylresorcinol, 2-tert-butylresorcinol, and 4-tert-butylresorcinol; alkylhydroquinone compounds such as methylhydroquinone, ethylhydroquinone, propylhydroquinone, tert-butylhydroquinone, and 2,5-di-tert-butylhydroquinone; phosphine compounds such as tributylphosphine, trioctylphosphine, tricyclohexylphosphine, triphenylphosphine, and tribenzylphosphine; phosphine oxide compounds such as trioctylphosphine oxide and triphenylphosphine oxide; phosphite compounds such as triphenylphosphite and trisnonylphenylphosphite; pyrogallol; and phloroglucinone.

[0138] The content of the polymerization inhibitor is preferably 0.01 to 0.4 parts by mass in the non-volatile content of the photosensitive coloring composition. When an appropriate amount is contained, a good pattern shape is easily obtained.

[0139] <Ultraviolet absorber (I)> The photosensitive coloring composition may contain an ultraviolet absorbing agent. Examples of the ultraviolet absorbing agent include benzotriazole-based compounds, triazine-based compounds, benzophenone-based compounds, salicylic acid ester-based compounds, cyanoacrylate-based compounds, and salicylate-based compounds.

[0140] The content of the ultraviolet absorber is preferably 5 to 70% by mass relative to 100% by mass of the total of the photopolymerization initiator and the ultraviolet absorber. When an appropriate amount is contained, the resolution after development is further improved.

[0141] The total content of the photopolymerization initiator and the ultraviolet absorber is preferably 1 to 20% by mass based on 100% by mass of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the adhesion between the substrate and the coating is further improved, and good resolution can be obtained.

[0142] Benzotriazole organic compounds include 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-(2-hydroxy-5-t-butylphenyl)-2H-benzotriazole, 2-[2-hydroxy-3,5-bis(α, α-Dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 5% 2-methoxy-1-methylethyl acetate and 95% benzenepropanoic acid, 3-(2H-benzotriazol-2-yl)-(1,1-dimethylethyl)-4-hydroxy, C7-9 side and linear alkyl ester mixture, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, methyl 3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300 reaction products, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol], 2-(2H-benzotriazol-2-yl)-p-cresol, 2-(5-chloro-2H-benzotriazol-2-yl)-6-t- Butyl-4-methylphenol, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole, octyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, and 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate.

[0143] Commercially available products include TINUVIN P, PS, 234, 326, 329, 384-2, 900, 928, 99-2, and 1130 manufactured by BASF Japan Ltd., ADK STAB LA-29, LA-31RG, LA-32, and LA-36 manufactured by ADEKA Corporation, KEMISORB71, 73, 74, 79, and 279 manufactured by Chemipro Chemical Co., Ltd., and RUVA-93 manufactured by Otsuka Chemical Co., Ltd.

[0144] As triazine-based organic compounds, 2,4-bis(2,4-dimethylphenyl)-6-(2-hydroxy-4-n-octyloxyphenyl)-1,3,5-triazine, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol, and the reaction of 2-(2,4-dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine with (2-ethylhexyl)-glycidic acid ester are The product may include 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)phenol, 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]phenol, and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine.

[0145] Commercially available products include KEMISORB 102 manufactured by Chemipro Chemicals, TINUVIN 400, 405, 460, 477, 479, and 1577ED manufactured by BASF Japan, Adeka STAB LA-46 and LA-F70 manufactured by ADEKA, and CYASORB UV-1164 manufactured by Sun Chemical.

[0146] Benzophenone-based organic compounds include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid-3H2O, 2-hydroxy-4-n-octoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2,2'dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.

[0147] Commercially available products include KEMISORB 10, 11, 11S, 12, and 111 manufactured by Chemipro Chemicals, SEESORB 101 and 107 manufactured by Shipro Chemicals, Adeka STAB 1413 manufactured by ADEKA, and UV-12 manufactured by Sun Chemical. Examples of the salicylate organic compounds include phenyl salicylate, p-octylphenyl salicylate, and p-tert-butylphenyl salicylate.

[0148] <Antioxidants (J)> The photosensitive coloring composition can contain an antioxidant. The antioxidant can prevent the coating film formed from the photosensitive coloring composition from yellowing due to oxidation during the thermal process of heat curing or ITO annealing, and suppress the decrease in the transmittance of the coating film. In particular, when the colorant concentration of the photosensitive coloring composition is high, the content of the photopolymerizable compound (D) is relatively reduced, so that the coating film is likely to yellow when the amount of the photopolymerization initiator is increased or a thermosetting compound is blended. Therefore, by including an antioxidant, yellowing due to oxidation during the heating process can be prevented, and the decrease in the transmittance of the coating film can be suppressed.

[0149] The antioxidant is a compound having a radical scavenging function or a peroxide decomposition function. Examples of the antioxidant include hindered phenol compounds, hindered amine compounds, phosphorus compounds, sulfur compounds, and hydroxylamine compounds. The antioxidant is preferably a compound that does not contain a halogen atom.

[0150] Hindered phenol antioxidants include 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,1,3-tris-(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-butane, 4,4'-butylidene-bis-(2-t-butyl-5-methylphenol), 3-(3,5-di-t-butyl-4-hydroxyphenyl)stearyl propionate, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 3,9-bis[2-[3-(3-t-butyl-4-hydroxy-5 -methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]Undecane, 1,3,5-tris(3,5-di-t-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene, 1,3,5-tris(3-hydroxy-4-t-butyl-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,2'-methylenebis(6-t-butyl-4-ethylphenol), 2,2'-thiodiethylbis-(3,5-di- t-Butyl-4-hydroxyphenyl)-propionate, N,N-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), i-octyl 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,6-bis(dodecylthiomethyl)-o-cresol, calcium salt of 3,5-di-t-butyl-4-hydroxybenzylphosphonic acid monoethyl ester, 4, 6-bis(octylthiomethyl)-o-cresol, bis[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propionic acid]ethylene bisoxybisethylene, 1,6-hexanediol bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, Examples of such phenols include 2,2'-thio-bis-(6-t-butyl-4-methylphenol), 2,5-di-t-amyl-hydroquinone, 2,6-di-t-butyl-4-nonylphenol, 2,2'-isobutylidene-bis-(4,6-dimethyl-phenol), 2,2'-methylene-bis-(6-(1-methyl-cyclohexyl)-p-cresol), and 2,4-dimethyl-6-(1-methyl-cyclohexyl)-phenol.

[0151] Commercially available products include ADK STAB AO-20, AO-30, AO-40, AO-50, AO-60, AO-80, and AO-330 manufactured by ADEKA CORPORATION; KEMINOX 101, 179, 76, and 9425 manufactured by Chemipro Corporation; IRGANOX 1010, 1035, 1076, 1098, 1135, 1330, 1726, 1425WL, 1520L, 245, 259, 3114, 5057, and 565 manufactured by BASF Japan; and Cyanox CY-1790 and CY-2777 manufactured by Sun Chemical Company.

[0152] Examples of hindered amine antioxidants include tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)1,2,3,4-butane tetracarboxylate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)1,2,3,4-butane tetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, and 1,2,2,6,6-pentamethyl-4-piperidyl. Methyl-4-piperidyl methacrylate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, polycondensate of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine, poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-s-triazine-2,4-diyl]-[(2,2,6,6-tetramethyl-4-piperidyl)imino]-hexamethylene-[(2,2,6,6-tetramethyl-4-piperidyl)imino]], 4-hydroxy-2,2,6,6-tetramethyl-1-pi Ester of peridineethanol with 3,5,5-trimethylhexanoic acid, N,N'-4,7-tetrakis[4,6-bis{N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino}-1,3,5-triazin-2-yl]-4,7-diazadecane-1,10-diamine, decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl)ester, reaction products of 1,1-dimethylethyl hydroperoxide with octane, bis(1,2,2,6,6-pentamethyl-4-pyridyl)[[3,5-bi 1,2,2,6,6-pentamethyl-4-pyridyl sebacate, poly[[6-morpholino-s-triazine-2,4-diyl]-[(2,2,6,6-tetramethyl-4-piperidyl)imino]-hexamethylene-[(2,2,6,6-tetramethyl-4-piperidyl)imino]], 2,2,6,6-tetramethyl-4-piperidyl-C12-21 and C18 unsaturated fatty acid esters, N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)-1,6-Hexamethylenediamine, 2-methyl-2-(2,2,6,6-tetramethyl-4-piperidyl)amino-N-(2,2,6,6-tetramethyl-4-piperidyl)propionamide, etc.

[0153] Commercially available products include ADKA STAB LA-52, LA-57, LA-63P, LA-68, LA-72, LA-77Y, LA-77G, LA-81, LA-82, LA-87, LA-402F, and LA-502XP manufactured by ADEKA CORPORATION; KAMISTAB 29, 62, 77, and 94 manufactured by Chemipro Chemicals; Tinuvin 249, TINUVIN 111FDL, 123, 144, 292, and 5100 manufactured by BASF Japan; and Cyasorb UV-3346, UV-3529, and UV-3853 manufactured by Sun Chemical Co., Ltd.

[0154] Phosphorus-based antioxidants include di(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, 2,2'-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, tris(nonylphenyl)phosphite, tetra(C12-C15 alkyl)-4,4'-isopropylidenediphenyl diphosphite, diphenyl mono(2 -ethylhexyl)phosphite, diphenyl isodecyl phosphite, tris(isodecyl)phosphite, triphenyl phosphite, tetrakis(2,4-di-t-butylphenyl)-4,4-biphenyl diphosphonate, tris(tridecyl)phosphite, phenyl isooctyl phosphite, phenyl isodecyl phosphite, phenyl di(tridecyl)phosphite, diphenyl isooctyl phosphite, diphenyl tridecyl phosphite, 4,4'-isopropylide diphenol alkyl phosphite, trisnonylphenyl phosphite, trisdinonylphenyl phosphite, tris(biphenyl) phosphite, di(2,4-di-t-butylphenyl)pentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, tetratridecyl 4,4'-butylidenebis(3-methyl-6-t-butylphenol) diphosphite, hexatridecyl Examples of such phosphite include 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane triphosphite, 3,5-di-t-butyl-4-hydroxybenzyl phosphite diethyl ester, sodium bis(4-t-butylphenyl)phosphite, sodium-2,2-methylene-bis(4,6-di-t-butylphenyl)-phosphite, 1,3-bis(diphenoxyphosphonyloxy)-benzene, and ethyl bis(2,4-ditert-butyl-6-methylphenyl)phosphite.

[0155] Commercially available products include ADK STAB PEP-36, PEP-8, HP-10, 2112, 1178, 1500, C, 135A, 3010, and TPP manufactured by ADEKA Corporation, IRGAFOS168 manufactured by BASF Japan, and HostanoxP-EPQ manufactured by Clariant Chemicals.

[0156] Examples of sulfur-based antioxidants include 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diylbis[3-(dodecylthio)propionate], ditridecyl 3,3'-thiobispropionate, 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,4-bis[(octylthio)methyl]-o-cresol, and 2,4-bis[(laurylthio)methyl]-o-cresol.

[0157] Commercially available products include Adeka STAB AO-412S and AO-503 manufactured by ADEKA Corporation, and KEMINOXPLS manufactured by Chemipro Chemicals.

[0158] The antioxidants may be used alone or in combination of two or more.

[0159] The content of the antioxidant is preferably 0.5 to 5.0% by mass based on 100% by mass of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the transmittance, spectral characteristics, and sensitivity are improved.

[0160] <Leveling agent (K)> The photosensitive coloring composition can contain a leveling agent. This improves the wettability of the transparent substrate during film formation and the drying property of the film. Examples of the leveling agent include silicone surfactants, fluorine surfactants, nonionic surfactants, cationic surfactants, and anionic surfactants.

[0161] Examples of silicone surfactants include linear polymers formed from siloxane bonds and modified siloxane polymers in which organic groups have been introduced into the side chains or ends.

[0162] Commercially available products include BYK-300, 306, 310, 313, 315N, 320, 322, 323, 330, 331, 333, 342, 345 / 346, 347, 348, 349, 370, 377, 378, 3455, UV3510, 3570 manufactured by BYK-Chemie, and FZ-7002, 2110, 2111 manufactured by Dow Corning Toray. 122, 2123, 2191, 5609, and Shin-Etsu Chemical Co., Ltd.'s X-22-4952, X-22-4272, X-22-6266, KF-351A, KF-354L, KF-355A, KF-945, KF-640, KF-642, KF-643, X-22-4515, KF-6004, and KP-341.

[0163] The fluorosurfactant may be a surfactant or a leveling agent having a fluorocarbon chain.

[0164] Commercially available products include Surflon S-242, S-243, S-420, S-611, S-651, and S-386 manufactured by AGC Seimi Chemical Co., Ltd., Megafac F-253, F-477, F-551, F-552, F-555, F-558, F-560, F-570, F-575, F-576, R-40-LM, R-41, RS-72-K, and DS-21 manufactured by DIC Corporation, FC-4430 and FC-4432 manufactured by Sumitomo 3M Limited, EF-PP31N09, EF-PP33G1, and EF-PP32C1 manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd., and Futergent 602A manufactured by Neos Corporation.

[0165] Examples of nonionic surfactants include polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene alkyl ether, polyoxyethylene myristyl ether, polyoxyethylene octyldodecyl ether, polyoxyalkylene alkyl ether, polyoxyphenylenedistyrenated phenyl ether, polyoxyethylene tribenzyl phenyl ether, polyoxyethylene polyoxypropylene glycol, polyoxyalkylene alkenyl ether, polyoxyethylene nonyl phenyl ether, polyoxyethylene alkyl ether phosphate ester, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan distearate, and sorbitan tristearate. , sorbitan monooleate, sorbitan trioleate, sorbitan sesquioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan triisostearate, polyoxyethylene sorbitan tetraoleate, glycerol monostearate, glycerol monooleate, polyethylene glycol monolaurate, polyethylene glycol monostearate, polyethylene glycol distearate, polyethylene glycol monooleate, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkylamines, alkyl alkanolamides, alkyl imidazolines, and the like.

[0166] Commercially available products include Kao's Emulgen 103, 104P, 106, 108, 109P, 120, 123P, 130K, 147, 150, 210P, 220, 306P, 320P, 350, 404, 408, 409PV, 420, 430, 705, 707, 709, 1108, 1118S-70, 1135S-70, 1150S-60, 2020G-HA, 2025G, LS-106, and LS-1. 10, LS-114, MS-110, A-60, A-90, B-66, PP-290, Latemul PD-420, PD-430, PD-430S, PD450, Leodor SP-L10, SP-P10, SP-S10V, SP-S20, SP-S30V, SP-O10V, SP-O30V, Super SP-L10, AS-10V, AO-10V, AO-15V, TW-L120, TW-L1 06, TW-P120, TW-S120V, TW-S320V, TW-O120V, TW-O106V, TW-IS399C, Super TW-L120, 430V, 440V, 460V, MS-50, MS-60, MO-60, MS-165V, Emanone 1112, 3199V, 3299V, 3299RV, 4110, CH-25, CH-40, CH-60(K), Amiit 102, Examples of such copolymers include 105, 105A, 302, 320, Aminone PK-02S, L-02, Homogenol L-95, ADEKA Pluronic (registered trademark) L-23, 31, 44, 61, 62, 64, 71, 72, 101, 121, TR-701, 702, 704, 913R manufactured by ADEKA Corporation, and (meth)acrylic acid-based (co)polymer Polyflow No. 75, No. 90, No. 95 manufactured by Kyoeisha Chemical Co., Ltd.

[0167] Examples of the cationic surfactant include alkylamine salts, alkyl quaternary ammonium salts such as lauryltrimethylammonium chloride, stearyltrimethylammonium chloride, and cetyltrimethylammonium chloride, and ethylene oxide adducts thereof.

[0168] Commercially available products include Kao Corporation's Acetamine 24, Cortamine 24P, 60W, and 86P Concentrate.

[0169] Examples of the anionic surfactant include polyoxyethylene alkyl ether sulfate, sodium dodecylbenzene sulfonate, alkali salts of styrene-acrylic acid copolymers, sodium alkyl naphthalene sulfonate, sodium alkyl diphenyl ether disulfonate, monoethanolamine lauryl sulfate, triethanolamine lauryl sulfate, ammonium lauryl sulfate, monoethanolamine stearate, sodium stearate, sodium lauryl sulfate, monoethanolamine styrene-acrylic acid copolymers, and polyoxyethylene alkyl ether phosphates.

[0170] Commercially available products include Futergent 100 and 150 manufactured by Neos Corporation, and Adeka Hope YES-25, Adeka Col TS-230E, PS-440E, and EC-8600 manufactured by ADEKA Corporation.

[0171] Examples of the amphoteric surfactant include alkyl betaines such as lauric acid amidopropyl betaine, lauryl betaine, cocamidopropyl betaine, stearyl betaine, and alkyl dimethylamino acetate betaine; and alkyl amine oxides such as lauryl dimethylamine oxide.

[0172] Commercially available products include Anhithol 20AB, 20BS, 24B, 55AB, 86B, 20Y-B, ​​and 20N manufactured by Kao Corporation.

[0173] The leveling agents (K) can be used alone or in combination of two or more kinds.

[0174] The content of the leveling agent (K) is preferably 0.001 to 2.0 mass%, more preferably 0.005 to 1.0 mass%, based on 100 mass% of the nonvolatile content of the photosensitive coloring composition. When an appropriate amount is contained, the balance between the coatability and adhesion of the photosensitive coloring composition is further improved.

[0175] <Storage stabilizer (L)> The photosensitive coloring composition can contain a storage stabilizer. This improves the viscosity stability of the composition over time. Examples of the storage stabilizer include quaternary ammonium chlorides such as benzyl trimethyl chloride and diethylhydroxyamine, organic acids such as lactic acid and oxalic acid and their methyl ethers, organic phosphines such as t-butylpyrocatechol, tetraethylphosphine and tetraphenylphosphine, and phosphites.

[0176] The content of the storage stabilizer is preferably 0.1 to 10 parts by mass based on 100 parts by mass of the colorant (A).

[0177] <Adhesion improver (M)> The photosensitive coloring composition can contain an adhesion improver. This improves the adhesion between the coating and the substrate. In addition, it becomes easier to form a narrow pattern by photolithography. Examples of the adhesion improver include a silane coupling agent.

[0178] Examples of the silane coupling agent include vinyl silanes such as vinyl trimethoxy silane and vinyl triethoxy silane, (meth)acrylic silanes such as 3-methacryloxypropyl methyl dimethoxy silane, 3-methacryloxypropyl trimethoxy silane, 3-methacryloxypropyl methyl diethoxy silane, 3-methacryloxypropyl triethoxy silane and 3-acryloxypropyl trimethoxy silane, epoxy silanes such as 2-(3,4-epoxycyclohexyl) ethyl trimethoxy silane, 3-glycidoxypropyl methyl dimethoxy silane, 3-glycidoxypropyl trimethoxy silane, 3-glycidoxypropyl methyl diethoxy silane and 3-glycidoxypropyl triethoxy silane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxy silane, N-2-( aminosilanes such as N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride; mercaptos such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; styryls such as p-styryltrimethoxysilane; ureidos such as 3-ureidopropyltriethoxysilane; sulfides such as bis(triethoxysilylpropyl)tetrasulfide; and isocyanates such as 3-isocyanatepropyltriethoxysilane.

[0179] The content of the adhesion improver is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the colorant (A). When an appropriate amount is contained, the photosensitivity of the photosensitive coloring composition is improved, the adhesion of the coating is further improved, and the resolution of the pattern is further improved.

[0180] <Method for producing photosensitive coloring composition> The photosensitive coloring composition is prepared, for example, by dispersing a colorant (A), a resin (B), etc. to prepare a colorant dispersion. Then, the colorant dispersion, the resin (B), a polymerizable compound (C), a photopolymerization initiator (D), etc. are blended and mixed to produce the photosensitive coloring composition. The materials to be blended and the timing of blending are optional. The dispersion process can also be carried out multiple times.

[0181] The dispersion treatment can be carried out using a dispersion device such as a kneader, a two-roll mill, a three-roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, or an attritor.

[0182] <Removal of large particles> The photosensitive coloring composition of the present invention is preferably subjected to removal of coarse particles of 5 μm or more, preferably coarse particles of 1 μm or more, more preferably coarse particles of 0.5 μm or more, and mixed dust by means of centrifugation, filtration with a sintered filter or membrane filter, etc. In this way, it is preferable that the coloring composition does not substantially contain particles of 0.5 μm or more. More preferably, the particles are 0.3 μm or less.

[0183] <Water content in photosensitive coloring composition> The photosensitive coloring composition of the present invention preferably has a water content of 2% by mass or less. When the photosensitive coloring composition has a water content within the above range, it has excellent dispersion stability and sensitivity even after storage over time.

[0184] The water content in the photosensitive coloring composition is preferably 1.8% by mass or less, and more preferably 1.6% by mass or less. If the water content is sufficiently low within this range, problems with dispersion stability and sensitivity are unlikely to occur even after storage over time.

[0185] The method for controlling the water content is not particularly limited, and a known method can be used. For example, a method for producing a photosensitive coloring composition while blowing in a dry inert gas, or a method for dehydrating the composition by adding molecular sieves after production, etc. can be mentioned. Among them, the method for producing the composition while blowing in a dry inert gas is preferred.

[0186] The water content can be measured by a known method such as the Karl Fischer method.

[0187] <Amount of toluene in the photosensitive coloring composition> The photosensitive coloring composition of the present invention may contain toluene, and when it does contain toluene, the content of toluene is preferably 0.1 to 10 mass ppm. The upper limit of the toluene content is preferably 9 mass ppm or less, more preferably 8 mass ppm or less, and even more preferably 7 mass ppm or less. The lower limit is preferably 0.2 mass ppm or more, more preferably 0.3 mass ppm or more, and even more preferably 0.4 mass ppm or more.

[0188] <Color filters> The color filter of the present invention preferably has a filter segment formed from a photosensitive coloring composition. The color filter preferably has a red filter segment, a green filter segment, and a blue filter segment by appropriately selecting the type of colorant (A) used. In addition, the color filter can have a magenta filter segment, a cyan filter segment, and a yellow filter segment of complementary colors instead of these color filter segments. In addition, a reflective substrate can be used instead of the transparent substrate. For example, a transparent substrate can be a glass substrate. For example, a reflective substrate can be a substrate using an aluminum electrode or a metal thin film as a reflective surface. In addition, each color filter can form a color filter segment with high color separation because the color mixing with other colors can be suppressed by reducing the transmission of wavelengths other than the wavelength range of the target color. In the case of a blue color filter, it is preferable to reduce the transmittance of wavelengths in the visible range other than around 380 to 490 nm. In addition, in the case of a green color filter, it is preferable to reduce the transmittance of wavelengths in the visible range other than around 490 to 590 nm. For example, in the case of a red color filter, it is preferable to lower the transmittance at wavelengths in the visible range other than those in the vicinity of 590 to 780 nm. In order to improve color separation between the colors of the color filters, the minimum transmittance of each color filter in the range of 380 to 780 nm is preferably less than 2.5%, and most preferably less than 1.0%.

[0189] <Manufacturing method for color filters> It is preferable to form a color filter by first forming a black matrix on a substrate and then forming filter segments. It is also possible to form a thin film transistor (TFT) on the substrate before forming the black matrix. Examples of the black matrix include a multilayer film of chromium or chromium / chromium oxide, an inorganic film such as titanium nitride, and a resin film with a light-shielding agent dispersed therein.

[0190] The filter segments can be formed by, for example, a printing method, an electrodeposition method, a transfer method, an inkjet method, a photolithography method, etc. In this specification, the most preferred method is the photolithography method.

[0191] In the photolithography method, for example, a photosensitive coloring composition containing a colorant of a certain color tone is applied onto a transparent substrate so that the dry film thickness is about 0.2 to 5 μm to form a coating. The obtained coating (hereinafter referred to as the first coating) is exposed (irradiated with light) through a mask having a predetermined pattern. Then, the coating is developed by immersing in a solvent or an alkaline developer or spraying the developer with a spray or the like, and the uncured parts are removed to obtain a desired pattern. This process can be similarly carried out using a photosensitive coloring composition containing a colorant of another color tone to produce a color filter having filter segments of each color. In addition, a second coating (oxygen barrier film) can be formed on the first coating before exposure using polyvinyl alcohol or a water-soluble acrylic resin. This prevents the first coating from coming into contact with oxygen, thereby further improving the exposure sensitivity. In addition, the color filter can be heated to cure the uncured photopolymerizable compound in the filter segment.

[0192] Examples of the coating device include a spray coater, a spin coater, a slit coater, and a roll coater. A drying step can be carried out during coating. Examples of the drying device include a hot air oven and an infrared heater.

[0193] The developer may be an alkaline developer, for example, an inorganic alkali such as sodium carbonate or sodium hydroxide, or an organic alkali such as dimethylbenzylamine or triethanolamine. A defoaming agent or a surfactant may be added to the developer.

[0194] The color filter of the present invention is laminated to an opposing substrate using a sealant, liquid crystal is injected through an injection port provided in the sealing part, the injection port is sealed, and a polarizing film or a retardation film is laminated to the outside of the substrate as necessary, to produce a color liquid crystal display device. This color liquid crystal display device can be used in liquid crystal display modes that use color filters such as twisted nematic (TN), super twisted nematic (STN), in-plane switching (IPS), vertically aligned (VA), and optically convencive bend (OCB).

[0195] The color filter in this specification can be used for applications such as solid-state imaging devices, organic EL displays, quantum dot displays, electronic paper, and head-mounted displays, in addition to liquid crystal displays.

[0196] <Solid-state imaging element> The solid-state imaging element of the present invention includes a color filter. For example, the solid-state imaging element may include a substrate having a plurality of photodiodes constituting a light receiving area of ​​the solid-state imaging element (such as a CCD image sensor, a CMOS image sensor, or an organic CMOS image sensor) and a light receiving element made of polysilicon or the like, and the color filter of the present invention is provided on the side of the light receiving element forming surface or the opposite side of the forming surface.

[0197] <Liquid crystal display device> The image display device of this specification includes a color filter. The image display device preferably further includes a light source. A liquid crystal display device will be described as an example of the image display device. The liquid crystal display device includes a color filter and a light source. Examples of the light source include a cold cathode fluorescent lamp (CCFL) and a white LED, but in the present invention, it is preferable to use a white LED because it widens the red reproduction range. Fig. 1 is a schematic cross-sectional view of a liquid crystal display device 10 including a color filter of the present invention. The device 10 shown in Fig. 1 includes a pair of transparent substrates 11 and 21 arranged to face each other with a space therebetween, and a liquid crystal LC is sealed between them.

[0198] The liquid crystal LC is aligned according to a driving mode such as TN (Twisted Nematic), STN (Super Twisted Nematic), IPS (In-Plane switching), VA (Vertical Alignment), OCB (Optically Compensated Birefringence), etc. A TFT (Thin Film Transistor) array 12 is formed on the inner surface of the first transparent substrate 11, and a transparent electrode layer 13 made of, for example, ITO is formed thereon. An alignment layer 14 is provided on the transparent electrode layer 13. In addition, a polarizing plate 15 is formed on the outer surface of the transparent substrate 11.

[0199] On the other hand, a color filter 22 of the present invention is formed on the inner surface of the second transparent substrate 21. Red, green and blue filter segments constituting the color filter 22 are separated by a black matrix (not shown).

[0200] A transparent protective film (not shown) is formed as necessary to cover the color filter 22, and a transparent electrode layer 23 made of, for example, ITO is formed on top of the transparent protective film. An alignment layer 24 is provided to cover the transparent electrode layer 23.

[0201] In addition, a polarizing plate 25 is formed on the outer surface of the transparent substrate 21. Below the polarizing plate 25, a backlight unit 30 is provided.

[0202] The white LED light source may be one in which a fluorescent filter is formed on the surface of a blue LED, or one in which a fluorescent material is contained in the resin package of a blue LED, and has a wavelength (λ3) in the range of 430 nm to 485 nm at which the emission intensity is maximized, a wavelength (λ4) in the range of 530 nm to 580 nm at which the emission intensity is maximized, and a wavelength (λ5) in the range of 600 nm to 650 nm at which the emission intensity is maximized, and the ratio (I4 / I3) of the emission intensity I3 at wavelength λ3 to the emission intensity I4 at wavelength λ4 is 0.2 or more and 0.4 or less. In particular, a white LED light source (LED1) having spectral characteristics in which the ratio (I5 / I3) of the emission intensity I3 at wavelength λ3 to the emission intensity I5 at wavelength λ5 is 0.1 or more and 1.3 or less, or a white LED light source (LED2) having a wavelength (λ1) at which the emission intensity is maximum within the range of 430 nm to 485 nm, a peak wavelength (λ2) of the second emission intensity within the range of 530 nm to 580 nm, and a ratio (I2 / I1) of the emission intensity I1 at wavelength λ1 to the emission intensity I2 at wavelength λ2 is 0.2 or more and 0.7 or less is preferred.

[0203] Specific examples of the LED 1 include NSSW306D-HG-V1 (manufactured by Nichia Chemical Industries, Ltd.) and NSSW304D-HG-V1 (manufactured by Nichia Chemical Industries, Ltd.).

[0204] Specific examples of the LED 2 include NSSW440 (manufactured by Nichia Chemical Industries, Ltd.) and NSSW304D (manufactured by Nichia Chemical Industries, Ltd.). EXAMPLES

[0205] The present invention will be described below with reference to examples. However, the present invention is not limited to the examples. In the examples, "parts" means "parts by mass" and "%" means "% by mass".

[0206] The weight average molecular weight (Mw), number average molecular weight (Mn), acid value (mgKOH / g), amine value (mgKOH / g), and ammonium salt value (mgKOH / g) of the resin are as follows.

[0207] <Non-volatile content, non-volatile content concentration> In the present invention, the non-volatile content refers to the mass remaining after standing in an oven at 200° C. for 30 minutes.

[0208] <Weight average molecular weight (Mw), number average molecular weight (Mn)> The number average molecular weight (Mn) and weight average molecular weight (Mw) of the resin were measured by gel permeation chromatography (GPC) equipped with an RI detector. The instrument used was an HLC-8220GPC (manufactured by Tosoh Corporation), with two separation columns connected in series, and both packings were "TSK-GEL SUPER HZM-N" connected in series. The oven temperature was 40°C, THF solution was used as the eluent, and the flow rate was 0.35 ml / min. The sample was dissolved in a solvent consisting of 1% by mass of the above eluent, and 20 microliters were injected. All molecular weights are polystyrene equivalent values.

[0209] <Acid value (mgKOH / g)> 80 ml of acetone and 10 ml of water were added to 0.5 to 1 g of resin solution, and the solution was stirred to dissolve uniformly. The solution was titrated using an automatic titrator ("COM-555" manufactured by Hiranuma Sangyo Co., Ltd.) with a 0.1 mol / L KOH aqueous solution as the titrant, and the acid value (mgKOH / g) of the resin solution was measured. The acid value per unit of non-volatile content of the resin was calculated from the acid value of the resin solution and the concentration of non-volatile content of the resin solution.

[0210] <Ammonium salt value (mgKOH / g)> The ammonium salt value is determined by titrating with 0.1N silver nitrate aqueous solution using 5% potassium chromate aqueous solution as an indicator, and then converted to the potassium hydroxide equivalent, and indicates the ammonium salt value of the non-volatile content.

[0211] <Fine particle size of colorant (A)> (Colorant (A-1)) 100 parts of CI Pigment Red 254 (BASF Japan "Irgaphor Red B-CF"), 10 parts of dye derivative (b-1), 1000 parts of ground salt, and 120 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (Inoue Seisakusho Co., Ltd.) and kneaded for 8 hours at 70° C. This mixture was added to 2000 parts of warm water, heated to about 80° C. and stirred with a high-speed mixer for about 1 hour to form a slurry, filtered and washed repeatedly with water to remove salt and solvent, and then dried at 80° C. for 24 hours to obtain colorant (A-1).

[0212] (Colorant (A-2)) 500 parts of CI Pigment Red 177 ("Chromophthal Red A2B" manufactured by BASF Japan Co., Ltd.), 500 parts of sodium chloride, and 250 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 8 hours at 120° C. Next, this kneaded mixture was poured into 5 liters of warm water, heated to 70° C. and stirred for 1 hour to form a slurry, which was then repeatedly filtered and washed with water to remove the sodium chloride and diethylene glycol, and then dried at 80° C. for one day to obtain colorant (A-2).

[0213] (Colorant (A-3)) 100 parts of CI Pigment Red 272 (BASF Japan "Irgazin (r) Flame Red K 3800"), 1600 parts of sodium chloride, and 190 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (Inoue Seisakusho Co., Ltd.) and kneaded for 10 hours at 60 ° C. Next, this mixture was poured into 3 liters of warm water, heated to about 80 ° C. and stirred with a high-speed mixer for about 1 hour to make a slurry, filtered and washed with water repeatedly to remove sodium chloride and the solvent, and then dried at 80 ° C. for one day and night to obtain colorant (A-3).

[0214] (Colorant (A-4)) 100 parts of CI Pigment Red 269 ("Toner Magenta F8B" manufactured by Clariant), 800 parts of sodium chloride, and 180 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 5 hours at 70° C. This mixture was poured into 4,000 parts of warm water, and stirred with a high-speed mixer for about 1 hour while heating to about 80° C. to form a slurry, which was filtered and washed repeatedly with water to remove the salt and solvent, and then dried at 80° C. for 24 hours to obtain colorant (A-4).

[0215] (Colorant (A-5)) 100 parts of CI Pigment Green 58 (DIC "FASTGEN GREEN A110"), 1200 parts of sodium chloride, and 120 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (Inoue Seisakusho) and kneaded for 6 hours at 70° C. This kneaded mixture was poured into 3000 parts of warm water, heated to 70° C. and stirred for 1 hour to form a slurry, filtered and washed repeatedly to remove the sodium chloride and diethylene glycol, and then dried at 80° C. for a day and night to obtain 97 parts of colorant (A-5).

[0216] (Colorant (A-6)) 500 parts of CI Pigment Green 36 ("Leonol Green 6YK" manufactured by Toyo Color Co., Ltd.), 500 parts of sodium chloride, and 250 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 4 hours at 120° C. Next, this kneaded mixture was poured into 5 liters of warm water, heated to 70° C. and stirred for 1 hour to form a slurry, which was then filtered and repeatedly washed with water to remove the sodium chloride and diethylene glycol, and then dried at 80° C. for one day to obtain 490 parts of colorant (A-6).

[0217] (Colorant (A-7)) 500 parts of CI Pigment Green 63 ("OPTLION GREEN 8885" manufactured by Toyo Color Co., Ltd.), 500 parts of sodium chloride, and 250 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 120°C for 4 hours. Next, this kneaded mixture was poured into 5 liters of warm water, heated to 70°C and stirred for 1 hour to form a slurry, which was then filtered and repeatedly washed with water to remove the sodium chloride and diethylene glycol, and then dried at 80°C for a day and night to obtain 490 parts of colorant (A-7).

[0218] (Colorant (A-8)) 100 parts of CI Pigment Yellow 138 (BASF Japan "Paliotol Yellow K0961HD"), 800 parts of ground salt, and 180 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (Inoue Seisakusho) and kneaded for 4 hours at 70° C. This mixture was poured into 3000 parts of warm water, heated to about 80° C. and stirred with a high-speed mixer for about 1 hour to form a slurry, which was filtered and washed repeatedly with water to remove the salt and solvent, and then dried at 80° C. for 24 hours to obtain colorant (A-8).

[0219] (Colorant (A-9)) 100 parts of CI Pigment Yellow 139 (BASF Japan "Irgaphor Yellow 2R-CF"), 1600 parts of sodium chloride, and 190 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (Inoue Seisakusho Co., Ltd.) and kneaded for 10 hours at 60° C. Next, this mixture was poured into 3 liters of warm water, heated to about 80° C. and stirred with a high-speed mixer for about 1 hour to form a slurry, which was filtered and washed repeatedly with water to remove the sodium chloride and solvent, and then dried at 80° C. for one day and night to obtain colorant (A-9).

[0220] (Colorant (A-10)) 100 parts of CI Pigment Yellow 150 (Yellow Pigment E4GN manufactured by Lanxess), 1600 parts of sodium chloride, and 190 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 10 hours at 60° C. Next, this mixture was poured into 3 liters of warm water, and stirred with a high-speed mixer for about 1 hour while heating to about 80° C. to form a slurry, which was filtered and washed repeatedly with water to remove the sodium chloride and solvent, and then dried at 80° C. for one day and night to obtain colorant (A-10).

[0221] (Colorant (A-11)) 500 parts of CI Pigment Yellow 185 (BASF Japan "Paliotol Yellow D1155"), 500 parts of sodium chloride, and 250 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (Inoue Seisakusho Co., Ltd.) and kneaded for 8 hours at 120° C. Next, this kneaded mixture was poured into 5 liters of warm water, heated to 70° C. and stirred for 1 hour to form a slurry, which was then filtered and washed repeatedly to remove the sodium chloride and diethylene glycol, and then dried at 80° C. overnight to obtain colorant (A-11).

[0222] (Colorant (A-12)) 300 parts of a dioxazine-based purple pigment, Pigment Violet 23 ("Lionogen Violet RL" manufactured by Toyo Color Co., Ltd.) was added to 3000 parts of 96% sulfuric acid, stirred for 1 hour, and then poured into water at 5°C. After stirring for 1 hour, the mixture was filtered, washed with warm water until the washing liquid became neutral, and dried at 70°C. 120 parts of the obtained acid pasting-treated pigment, 5 parts of the dye derivative (b-2), 1500 parts of ground salt, and 100 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 70°C for 20 hours. This mixture was added to 5000 parts of warm water, stirred with a high-speed mixer for about 1 hour while heating to about 70°C to form a slurry, filtered, washed with water repeatedly to remove salt and solvent, and then dried at 80°C for 24 hours to obtain pigment (A-12).

[0223] (Colorant (A1)) 100 parts of CI Pigment Blue 15:6 ("Lionol Blue ES" manufactured by Toyo Color Co., Ltd.), 1000 parts of ground salt, and 100 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 12 hours at 50° C. This mixture was poured into 3000 parts of warm water, heated to about 70° C. and stirred with a high-speed mixer for about 1 hour to form a slurry, which was filtered and washed repeatedly with water to remove the salt and solvent, and then dried at 80° C. for 24 hours to obtain colorant (A1).

[0224] (Dye solution (a-1~a-3)) (Resin 1 having cationic groups on the side chains) A four-necked separable flask equipped with a thermometer, stirrer, distillation tube, and condenser was charged with 67.3 parts of methyl ethyl ketone and heated to 75°C under a nitrogen stream. Separately, 34.0 parts of methyl methacrylate, 28.0 parts of n-butyl methacrylate, 28.0 parts of 2-ethylhexyl methacrylate, 10.0 parts of dimethylaminoethyl methacrylate, 6.5 parts of 2,2'-azobis(2,4-dimethylvaleronitrile), and 25.1 parts of methyl ethyl ketone were homogenized, then charged into a dropping funnel, attached to a four-necked separable flask, and dropped over 2 hours. Two hours after the end of the dropwise addition, it was confirmed from the non-volatile content that the polymerization yield was 98% or more and the weight average molecular weight (Mw) was 6830, and the mixture was cooled to 50°C. To this, 3.2 parts of methyl chloride and 22.0 parts of ethanol were added, and the mixture was reacted at 50°C for 2 hours, then heated to 80°C over 1 hour, and further reacted for 2 hours. In this way, resin 1 having cationic groups on the side chains having ammonium groups and a resin component of 47% by mass was obtained. The ammonium salt value of the obtained resin was 34 mgKOH / g.

[0225] (dye 1) 30 parts of resin 1 having a cationic group in the side chain in terms of non-volatile content was added to 2000 parts of water, thoroughly stirred and mixed, and then heated to 60°C. Meanwhile, an aqueous solution was prepared by dissolving 10 parts of CI Acid Red 52 in 90 parts of water, and the solution was gradually dropped into the resin solution. After the dropwise addition, the solution was stirred at 60°C for 120 minutes to thoroughly react. To confirm the end point of the reaction, the reaction solution was dropped onto a filter paper, and the end point was determined to be when no bleeding occurred, and the salt-forming compound was obtained. After cooling to room temperature while stirring, suction filtration was performed, and the salt-forming compound remaining on the filter paper was dried by removing moisture in a dryer to obtain a colorant (dye 1) which is a salt-forming compound of CI Acid Red 52 and resin 1 having a cationic group in the side chain. At this time, the content of the active colorant component derived from CI Acid Red 52 in the colorant (dye 1) was 25% by mass.

[0226] (dye 2) A colorant (dye 2), which is a salt-forming compound of CI Acid Red 289 and resin 1 having a cationic group on its side chain, was obtained in the same manner as in the production of colorant (dye 1), except that CI Acid Red 52 was changed to CI Acid Red 289. At this time, the content of the active colorant component derived from CI Acid Red 289 in the colorant (dye 2) was 27% by mass.

[0227] (dye 3) In a 1L stainless steel reaction vessel equipped with a reflux condenser, 5.0 parts of CI Basic Violet 10 (BV10: Taoka Chemical Co., Ltd.: Rodamine B) and 1.6 parts of hydroxyethyl methacrylate (HEMA) were dissolved in 40 ml of dichloromethane under a nitrogen atmosphere, and 2.2 parts of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.25 parts of dimethylaminopyridine were added and stirred at room temperature for 24 hours. The resulting dichloromethane solution was washed with water and dried under reduced pressure, and then purified with a silica gel column to obtain a colorant (dye 3).

[0228] (Preparation of dye solution (a-1)) The following mixture was stirred and mixed to be homogeneous, and then filtered through a filter having a pore size of 5.0 μm to prepare a colored composition (dye solution (a-1)). Colorant (dye 1) 12.5 parts Propylene glycol monomethyl ether acetate (hereinafter referred to as PGMAc) 87.5 parts

[0229] (Preparation of dye solutions (a-2) and (a-3)) In the same manner as for the dye solution (a-1), dye solutions (a-2) and (a-3) were prepared using colorants (dye 2 and dye 3), respectively.

[0230] (Dye derivative (b)) The structures of the dye derivatives (b-1 to b-5) used are shown below. [ka] JPEG2024150911000015.jpg4375JPEG2024150911000016.jpg65110JPEG2024150911000017.jpg50119

[0231] (Preparation of Resin (B1-1) Solution) A reaction vessel equipped with a gas inlet tube, temperature control, condenser, and stirrer was charged with 10 parts of methacrylic acid, 100 parts of methyl methacrylate, 70 parts of iso-butyl methacrylate, 20 parts of benzyl methacrylate, and 50 parts of PGMAc, and the atmosphere was replaced with nitrogen gas. The inside of the reaction vessel was heated to 50°C with stirring, and 12 parts of 3-mercapto-1,2-propanediol was added. The temperature was raised to 90°C, and a solution of 0.1 parts of 2,2'-azobisisobutyronitrile in 90 parts of PGMAc was added and reacted for 7 hours. Measurement of the non-volatile content confirmed that 95% had reacted. 19 parts of pyromellitic anhydride, 50 parts of PGMAc, 50 parts of cyclohexanone, and 0.4 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added and reacted at 100 ° C for 7 hours. The reaction was terminated when it was confirmed that 98% or more of the acid anhydride had been half-esterified by measuring the acid value. PGMAc was added to adjust the non-volatile content to 40%, and a resin-type dispersant (B1-1) solution with an acid value of 70 mg KOH / g and a weight average molecular weight of 8500 was obtained.

[0232] (Preparation of Resin (B1-2) Solution) In a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, 80 parts of n-butyl acrylate, 60 parts of methyl methacrylate, 20 parts of methacrylic acid, 20 parts of Karenz MOI-BM (Showa Denko K.K.), 20 parts of ETERNACOLL OXMA (methacrylate (3-ethyloxetan-3-yl) methyl, Ube Industries K.K.), and 100 parts of PGMAc were charged and replaced with nitrogen gas. The inside of the reaction vessel was heated to 80°C, and a solution in which 0.1 parts of 2,2'-azobisisobutyronitrile was dissolved in 14 parts of 2-mercapto-2-methyl-1,3-propanediol was added and reacted for 10 hours. It was confirmed that 95% had reacted by measuring the non-volatile content. Next, BPAF: 39 parts of 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (manufactured by JFE Chemical Co., Ltd.), C-1015N (bifunctional polycarbonate polyol, trade name Kuraray Polyol C-1015N (hydroxyl value 112 mgKOH / g, manufactured by Kuraray Co., Ltd.)) 106 parts, 33 parts of trimellitic anhydride, 392 parts of cyclohexanone, and 0.40 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added and reacted at 100 ° C. for 7 hours. The reaction was terminated when it was confirmed that 98% or more of the acid anhydride was half-esterified by measuring the acid value. PGMAc was added to adjust the non-volatile content to 40%, and a resin-type dispersant (B1-2) solution with an acid value of 94 mgKOH / g and a weight average molecular weight of 25,000 was obtained.

[0233] (Preparation of Resin (B1-3) Solution) In a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, 108 parts of 3-mercapto-1,2-propanediol, 174 parts of pyromellitic dianhydride, 650 parts of PGMAc, and 0.2 parts of monobutyltin oxide as a catalyst were charged, and after replacing with nitrogen gas, the reaction was carried out at 120°C for 5 hours (first step). It was confirmed by measuring the acid value that 95% or more of the acid anhydride groups were half-esterified. Next, 160 parts of the compound obtained in the first step, calculated as non-volatile content, 200 parts of 2-hydroxypropyl methacrylate, 200 parts of ethyl acrylate, 150 parts of t-butyl acrylate, 200 parts of 2-methoxyethyl acrylate, 200 parts of methyl methacrylate, 50 parts of methacrylic acid, and 663 parts of PGMAc were charged, and the inside of the reaction vessel was heated to 80°C, and 1.2 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) were added, and the reaction was carried out for 12 hours (second step). It was confirmed that 95% had reacted by measuring the non-volatile content. Finally, 500 parts of a 50% PGMAc solution of the compound obtained in the second step, 27.0 parts of 2-methacryloyloxyethyl isocyanate (MOI), and 0.1 parts of hydroquinone were charged, and IR was used to measure the 2270 cm based on the isocyanate group. -1 The reaction was continued until the disappearance of the peak was confirmed (third step). After the disappearance of the peak was confirmed, the reaction solution was cooled to terminate the reaction. PGMAc was added to obtain a resin-type dispersant (B1-3) solution with a non-volatile content of 40%. The acid value of the obtained dispersant was 68 mg KOH / g, the unsaturated double bond equivalent was 1593, and the weight average molecular weight was 13000.

[0234] (Preparation of Resin (B1-4) Solution) In a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, 50.0 parts of t-butyl acrylate, 45.0 parts of methyl methacrylate, and 5.0 parts of methacrylic acid were charged and replaced with nitrogen gas. The reaction vessel was heated to 80°C, and a solution of 0.1 parts of 2,2'-azobisisobutyronitrile dissolved in 70.7 parts of PGMAc was added to 6.0 parts of 3-mercapto-1,2-propanediol, and reacted for 10 hours. It was confirmed that 95% had reacted by measuring the non-volatile content. Next, 14.5 parts of pyromellitic dianhydride (manufactured by Daicel Chemical Industries, Ltd.), 38.0 parts of PGMAc, and 0.2 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added, and the mixture was reacted at 120 ° C. for 5 hours. Then, 12.1 g of 3-methoxybutanol was added, and the mixture was reacted at 120 ° C. for 3 hours. The reaction was terminated after confirming that 98% or more of the acid anhydride had been half-esterified by measuring the acid value. After the reaction was completed, PGMAc was added so that the non-volatile content was 40% by mass, and a solution of dispersant (B1-4) with an acid value of 110 mg KOH / g and a weight average molecular weight of 9000 was obtained.

[0235] (Preparation of Resin (B1-5) Solution) In a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, 20.0 parts of t-butyl acrylate, 45.0 parts of methyl methacrylate, 30.0 parts of ethyl acrylate, and 5.0 parts of methacrylic acid were charged and replaced with nitrogen gas. The reaction vessel was heated to 80°C, and a solution of 0.1 parts of 2,2'-azobisisobutyronitrile dissolved in 70.7 parts of PGMAc was added to 6.0 parts of 3-mercapto-1,2-propanediol, and reacted for 10 hours. It was confirmed that 95% had reacted by measuring the non-volatile content. Next, 14.5 parts of pyromellitic dianhydride (manufactured by Daicel Chemical Industries, Ltd.), 38.0 parts of PGMAc, and 0.2 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added, and the mixture was reacted at 120 ° C. for 5 hours. Then, 12.1 g of 3-methoxybutanol was added, and the mixture was reacted at 120 ° C. for 3 hours. The reaction was terminated after confirming that 98% or more of the acid anhydride had been half-esterified by measuring the acid value. After the reaction was completed, PGMAc was added so that the non-volatile content was 40% by mass, and a solution of dispersant (B1-5) with an acid value of 105 mg KOH / g and a weight average molecular weight of 9400 was obtained.

[0236] <Preparation of Colored Composition> (Production of Coloring Composition) [Production Example 1] The mixture below was stirred and mixed to make it uniform, and then dispersed for 3 hours in an Eiger mill (Eiger Japan's "Mini Model M-250 MKII") using zirconia beads with a diameter of 0.5 mm. The mixture was then filtered through a filter with a pore size of 5.0 μm to produce a colored composition (X-1) with a non-volatile content of 20% by mass. Pigment (A-1) 15.0 parts Pigment derivative (b-1) 1.0 part Dispersant (B1-1: 40% non-volatile liquid) 10.0 parts Solvent (SM) 74.0 parts The solvent (SM) is a mixture of the following (S-1) to (S-6) in the parts by mass shown below. (S-1) PGMAc (boiling point 146℃) 20 parts (S-2) Cyclohexanone (boiling point 155°C) 20 parts (S-3) Ethyl 3-ethoxypropionate (boiling point 169°C) 20 parts (S-4) Propylene glycol monomethyl ether (boiling point 121°C) 20 parts (S-5) Cyclohexanol acetate (boiling point 172°C) 10 parts (S-6) Dipropylene glycol methyl ether acetate (boiling point 188°C) 10 parts

[0237] [Manufacturing Examples 2 to 23] (Production of Colored Compositions (X-2 to 23)) Colored compositions (X-2 to 23) were prepared in the same manner as for colored composition (X-1), except that the composition was changed as shown in Table 1.

[0238] [Table 1]

[0239] [Example 1] (Photosensitive coloring composition (Y-1)) The following raw materials were mixed and stirred, and filtered through a filter having a pore size of 1.0 μm to obtain a photosensitive coloring composition (Y-1) having a nonvolatile content of 18.78%. Coloring composition (X-1: non-volatile content 20.0%): 58.0 parts Resin solution (B2-1-M: non-volatile content 40%): 7.0 parts Polymerizable compound (C-1): 2.0 parts Photopolymerization initiator (D1-1-1): 0.4 parts Thermosetting compound (E-1): 0.5 part Thermosetting compound (E-2): 0.5 part Sensitizer (F): 0.1 parts Thiol chain transfer agent (G): 0.4 parts Polymerization inhibitor (H): 0.05 parts Ultraviolet absorber (I): 0.1 part Antioxidant (J): 0.1 part Leveling agent (K: non-volatile content 3%): 1.0 part Storage stabilizer (L): 0.1 part Adhesion improver (M): 0.1 part Solvent (SM): 29.65 parts

[0240] [Examples 2 to 49, Comparative Examples 1 to 3] (Photosensitive Coloring Compositions (Y-2 to Y-52) Except for changing the materials and blending amounts shown in Tables 2 and 3, the same procedure as for the photosensitive coloring composition (Y-1) was carried out to obtain photosensitive coloring compositions (Y-2 to Y-52).

[0241] [Table 2]

[0242] [Table 3]

[0243] In the table, details of each component are as follows.

[0244] <Production of resin (B2-1-M: non-photosensitive resin)> (Preparation of resin (B2-1-1) solution) A separable 4-neck flask was equipped with a thermometer, a cooling tube, a nitrogen gas inlet tube, a dropping tube and a stirrer. 196 parts of PGMAc was charged into the reaction vessel, which was then heated to 80°C. The atmosphere in the reaction vessel was replaced with nitrogen, and then a mixture of 37.2 parts of n-butyl methacrylate, 12.9 parts of 2-hydroxyethyl methacrylate, 12.0 parts of methacrylic acid, 20.7 parts of paracumylphenol ethylene oxide modified acrylate ("Aronix M110" manufactured by Toagosei Co., Ltd.), and 1.1 parts of 2,2'-azobisisobutyronitrile was dropped into the reaction vessel over a period of 2 hours. After the dropping was completed, the reaction was continued for another 3 hours and then cooled to room temperature. PGMAc was then added to adjust the non-volatile content to 40%, to obtain a binder resin (B2-1-1) solution. The mass average molecular weight (Mw) was 26,000.

[0245] (Preparation of resin (B2-1-2) solution) A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was filled with nitrogen, and 210 parts of PGMAc was added and heated to 100°C while stirring. Next, 106 parts of benzyl methacrylate, 22 parts of acrylic acid and 22 parts of dicyclopentanyl methacrylate (FA-513M manufactured by Hitachi Chemical Co., Ltd.) were dissolved in 215 parts of PGMAc, and 3.6 parts of 2,2'-azobisisobutyronitrile were dissolved to prepare a solution, which was then dropped into the flask and reacted at 100°C for 5 hours, after which it was cooled to room temperature. Next, PGMAc was added to adjust the non-volatile content to 40%, to obtain a binder resin (B2-1-2) solution. The mass average molecular weight (Mw) was 10,000.

[0246] (Preparation of resin (B2-1-M) mixed solution) Equal amounts of resin (B2-1-1) liquid and resin (B2-1-2) liquid were mixed and stirred to prepare a resin (B2-1-M) mixed solution.

[0247] <Production of resin (B2-2-M: photosensitive resin) mixed solution> (Preparation of resin (B2-2-1) solution) A separable 4-neck flask was fitted with a thermometer, a cooling tube, a nitrogen gas inlet tube, a dropping tube and a stirrer. 207 parts of PGMAc was charged into the reaction vessel, which was then heated to 80°C and substituted with nitrogen in the reaction vessel. From the dropping tube, a mixture of 20 parts of methacrylic acid, 20 parts of paracumylphenol ethylene oxide modified acrylate (Aronix M110 manufactured by Toagosei Co., Ltd.), 45 parts of methyl methacrylate, 8.5 parts of 2-hydroxyethyl methacrylate and 1.33 parts of 2,2'-azobisisobutyronitrile was added dropwise over 2 hours. After the dropping was completed, the reaction was continued for another 3 hours to obtain a copolymer resin solution. Next, the nitrogen gas was stopped and the whole amount of the obtained copolymer solution was stirred while injecting dry air for 1 hour, and then cooled to room temperature. Then, a mixture of 6.5 parts of 2-methacryloyloxyethyl isocyanate (Karens MOI manufactured by Showa Denko K.K.), 0.08 parts of dibutyltin laurate, and 26 parts of PGMAc was added dropwise at 70°C for 3 hours. After the dropwise addition, the reaction was continued for another hour and then cooled to room temperature. Next, PGMAc was added to adjust the non-volatile content to 40%, and a binder resin (B2-2-1) solution was obtained. The mass average molecular weight (Mw) was 18,000 and the acid value was 130 mgKOH / g.

[0248] (Preparation of resin (B2-2-2) solution) A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was introduced with 333 parts of PGMAc, and the atmosphere in the flask was changed from air to nitrogen, and then the temperature was raised to 100 ° C., and a solution of 70.5 parts of benzyl methacrylate, 71.1 parts of glycidyl methacrylate, 22.0 parts of tricyclodecane-skeleton monomethacrylate (Hitachi Chemical Co., Ltd. FA-513M), and 3.6 parts of azobisisobutyronitrile was added to a mixture consisting of 164 parts of PGMAc, was dropped into the flask from the dropping funnel over 2 hours, and further stirring was continued for 5 hours at 100 ° C. Next, the atmosphere in the flask was changed from nitrogen to air, and 43.0 parts of methacrylic acid, 0.9 parts of trisdimethylaminomethylphenol and 0.145 parts of hydroquinone were added to the flask, and the reaction was continued for 6 hours at 110 ° C., and the reaction was terminated when the non-volatile acid value became 1 mgKOH / g. Next, 60.9 parts of tetrahydrophthalic anhydride and 0.8 parts of triethylamine were added, and the mixture was reacted at 120°C for 3.5 hours, after which it was cooled to room temperature. PGMAc was then added to adjust the non-volatile content to 40%, to obtain a binder resin (B2-2-2) solution. The mass average molecular weight (Mw) was 12,000, and the acid value was 80 mgKOH / g.

[0249] (Preparation of binder resin (B2-2-3) solution) A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was introduced with 182 parts of PGMAc, and the atmosphere in the flask was changed from air to nitrogen, and then the temperature was raised to 100 ° C., and a solution of 70.5 parts of benzyl methacrylate, 43.0 parts of methacrylic acid, 22.0 parts of tricyclodecane-skeleton monomethacrylate (Hitachi Chemical Co., Ltd. FA-513M) and 3.6 parts of azobisisobutyronitrile was added to a mixture consisting of 136 parts of PGMAc from the dropping funnel over 2 hours, and the mixture was stirred for 5 hours at 100 ° C. Next, the atmosphere in the flask was changed from nitrogen to air, and 35.5 parts of glycidyl methacrylate, 0.9 parts of trisdimethylaminomethylphenol and 0.145 parts of hydroquinone were added to the flask, and the mixture was reacted at 110 ° C. for 6 hours, and then cooled to room temperature. Next, PGMAc was added to adjust the non-volatile content to 40%, to obtain a binder resin (B2-2-3) solution, which had a mass average molecular weight (Mw) of 13,000 and an acid value of 79 mgKOH / g.

[0250] (Preparation of resin (B2-2-4) solution) A separable flask with a cooling tube was prepared as a reaction vessel, and a mixture of 40 parts of dimethyl-2,2'-[oxybis(methylene)]bis-2-propenoate, 40 parts of methacrylic acid, 120 parts of methyl methacrylate, 4 parts of t-butylperoxy-2-ethylhexanoate ("Perbutyl O" manufactured by Nippon Oil & Fats), and 40 parts of PGMAc was prepared as a monomer dropping vessel, and a mixture of 8 parts of n-dodecanethiol and 32 parts of PGMAc was prepared as a chain transfer agent dropping vessel. 395 parts of PGMAc was charged into the reaction vessel, and after nitrogen replacement, the temperature of the reaction vessel was heated in an oil bath while stirring to raise the temperature to 90°C. After the temperature of the reaction vessel was stabilized at 90°C, dropping was started from the monomer dropping vessel and the chain transfer agent dropping vessel. Dropping was carried out over 135 minutes, respectively, while maintaining the temperature at 90°C. 60 minutes after the end of the dripping, the temperature was raised to 110°C. After maintaining 110°C for 3 hours, a gas inlet tube was attached to the separable flask, and bubbling of oxygen / nitrogen = 5 / 95 (volume ratio) mixed gas was started. Next, 70 parts of glycidyl methacrylate, 0.4 parts of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts of triethylamine were charged into the reaction vessel, and the reaction was carried out at 110°C for 12 hours, and then cooled to room temperature. Next, PGMAc was added to adjust the non-volatile content to 40%, and a binder resin (B2-2-4) solution was obtained. The mass average molecular weight (Mw) was 18,000, and the acid value was 2 mgKOH / g.

[0251] (Preparation of resin (B2-2-M) mixed solution) Equal amounts of the four types of resin solutions (B2-2-1) to (B2-2-4) were mixed and stirred to prepare a resin (B2-2-M) mixed solution.

[0252] <Polymerizable compound (C)> [ka]

[0253] (C-2) Mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate [Aronix M-402 (manufactured by Toagosei)] (C-3) Propylene glycol diglycidyl ether diacrylate

[0254] [ka]

[0255] <Photopolymerization initiator (D)> (D-1) 2-Methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one [Omnirad 907 (IGM Resins)] (D-2) 2-(Dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone [Omnirad 379EG (IGM Resins)] (D-3) 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide [Omnirad TPO (manufactured by IGM Resins)] (D-4) 2,2'-bis(o-chlorophenyl)-4,5,4',5'-tetraphenyl-1,2'-biimidazole [Biimidazole (Kurokane Chemicals)] (D-5) p-Dimethylaminoacetophenone [DMA (manufactured by Daikifine)] (D-6) Ethan-1-one, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl], 1-(O-acetyloxime) [Omnirad 2959 (IGM Resins)] (D-7) Bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide [Omnirad 819 (IGM Resins)] The above (D-1) to (D-7) were mixed in equal amounts to prepare a photopolymerization initiator (DM). (D1-1-1) An oxime ester-based photopolymerization initiator having a carbazole skeleton represented by the following formula (2). Formula (2) [ka]

[0256] (D1-1-2) A mixture of equal amounts of the following four types of oxime ester photopolymerization initiators having a carbazole skeleton: [ka]

[0257] (D1-1-3) A mixture of equal amounts of three types of oxime ester photopolymerization initiators having a carbazole skeleton, as shown in the following formula (4). Formula (4) [ka]

[0258] (D1-2-1) An oxime ester-based photopolymerization initiator having a diphenyl skeleton represented by the following formula (5). Formula (5) [ka]

[0259] (D1-2-2) An oxime ester-based photopolymerization initiator having a diphenyl skeleton represented by the following formula (6). Formula (6) [ka] (D1-2-3) An oxime ester-based photopolymerization initiator having a diphenyl skeleton represented by the following formula (6). Formula (6) [ka]

[0260] (D1-3) An oxime ester-based photopolymerization initiator having a fluorene skeleton represented by the following formula (7). Formula (7) [ka]

[0261] (D1-4) An oxime ester photopolymerization initiator having two oxime ester groups represented by the following formula (8). Formula (8) [ka]

[0262] <Thermosetting compound (E)> ·Thermosetting compound (E-1) (E-1-1) 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2'-bis(hydroxymethyl)-1-butanol [EHPE-3150 (manufactured by Daicel)], (E-1-2) Glycidyl etherified epoxy compounds of sorbitol [Denacol EX611 (Nagase ChemteX)] (E-1-3) Triglycidyl isocyanurate Equal amounts of (E-1-1) to (E-1-3) were mixed together to prepare a thermosetting compound (E-1). ·Thermosetting compound (E-2): 3-Ethyl-3-[(3-ethyloxetan-3-yl)methoxymethyl]oxetane [Aron Oxetane OXT-221 (manufactured by Toagosei)]

[0263] <Sensitizer (F)> (F-1) 2,4-Diethylthioxanthone [Kayacure DETX-S (manufactured by Nippon Kayaku)] (F-2) 4,4'-Bis(diethylamino)benzophenone [CHEMARK DEABP (manufactured by Chemark Chemical)] The above (F-1) and (F-2) were mixed in equal amounts to prepare sensitizer (F).

[0264] <Thiol-based chain transfer agent (G)> (G-1) Trimethylolethane tris(3-mercaptobutyrate) [TEMB (Showa Denko)] (G-2) Trimethylolpropane tris(3-mercaptobutyrate) [TPMB (Showa Denko)] (G-3) Pentaerythritol tetrakis(3-mercaptopropionate) [PEMP (manufactured by Sakai Chemical Industry Co., Ltd.)] (G-4) Trimethylolpropane tris(3-mercaptopropionate) [TMMP (manufactured by Sakai Chemical Industry Co., Ltd.)] (G-5) Tris[(3-mercaptopropionyloxy)-ethyl]-isocyanurate [TEMPIC (manufactured by Sakai Chemical Industry Co., Ltd.)] The above (G-1) to (G-5) were mixed in equal amounts to prepare a thiol-based chain transfer agent (G).

[0265] <Polymerization inhibitor (H)> (H-1) 3-Methylcatechol (H-2) Methylhydroquinone (H-3) tert-Butylhydroquinone The above (H-1) to (H-3) were mixed in equal amounts to prepare a polymerization inhibitor (H).

[0266] <Ultraviolet absorber (I)> (I-1) 2-[4-[(2-hydroxy-3-(dodecyl and tridecyl)oxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine [TINUVIN400 (BASF Japan)] (I-2) 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol [TINUVIN900 (BASF Japan)] The above (I-1) and (I-2) were mixed in equal amounts to prepare an ultraviolet absorber (I).

[0267] <Antioxidants (J)> (J-1) Pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (J-2) Dioctadecyl 3,3'-thiodipropanoate (J-3) Tris[2,4-di-(t)-butylphenyl]phosphine (J-4) Bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate (J-5) p-Octylphenyl Salicylate The above (J-1) to (J-5) were mixed in equal amounts to prepare antioxidant (J).

[0268] <Leveling agent (K)> 1 copy of "BYK-330" manufactured by BYK Chemical Co., Ltd. One copy of DIC's "Megafac F-551" and A mixed solution of 1 part of Kao Corporation's "Emulgen 103" dissolved in 97 parts of PGMAc.

[0269] <Storage stabilizer (L)> (L-1) 2,6-bis(1,1-dimethylethyl)-4-methylphenol ("BHT" manufactured by Honshu Chemical Industry Co., Ltd.) (L-2) Triphenylphosphine ("TPP" manufactured by Hokko Chemical Industry Co., Ltd.) The above (L-1) and (L-2) were mixed in equal amounts to prepare a storage stabilizer (L).

[0270] <Adhesion improver (M)> (M-1) "KBM-5103 (Shin-Etsu Chemical Co., Ltd.)" (M-2) 3-Glycidoxypropyltriethoxysilane [Shin-Etsu Silicone Silane Coupling Agent KBM-403 (Shin-Etsu Chemical Co., Ltd.)] (M-3) 3-Methacryloxypropyltriethoxysilane [Shin-Etsu Silicone Silane Coupling Agent KBE-503 (Shin-Etsu Chemical Co., Ltd.)] (M-4) N-2-(aminoethyl)-3-aminopropyltrimethoxysilane [Shin-Etsu Silicone Silane Coupling Agent KBM-603 (Shin-Etsu Chemical Co., Ltd.)] (M-5) 3-Mercaptopropyltrimethoxysilane [Shin-Etsu Silicone Silane Coupling Agent KBM-803 (Shin-Etsu Chemical Co., Ltd.)] The above (M-1) to (M-5) were mixed in equal amounts to prepare an adhesion improver (M).

[0271] <Solvent (S)> The solvent (SM) is a mixture of the following (S-1) to (S-6) in the parts by mass shown below. (S-1) PGMAc (boiling point 146℃) 20 parts (S-2) Cyclohexanone (boiling point 155°C) 20 parts (S-3) Ethyl 3-ethoxypropionate (boiling point 169°C) 20 parts (S-4) Propylene glycol monomethyl ether (boiling point 121°C) 20 parts (S-5) Cyclohexanol acetate (boiling point 172°C) 10 parts (S-6) Dipropylene glycol methyl ether acetate (boiling point 188°C) 10 parts

[0272] <Evaluation of Photosensitive Coloring Composition> The obtained photosensitive coloring compositions (Y-1 to Y-47) were evaluated by the following methods. The results are shown in Table 4. Each test was carried out by the following method. The test results are shown in Table 4. The meanings of the evaluation ranks are as follows: ◎: Very good 〇: Good △: Practical ×: Not practical

[0273] <Formation of filter segments> A black matrix was patterned on a 100 mm x 100 mm, 0.7 mm thick glass substrate, the obtained photosensitive coloring composition was applied onto the substrate using a spin coater, and the obtained composition was dried at 90°C for 90 seconds to remove the solvent, to obtain a coating film having a thickness of 1 μm. Next, the coating film was irradiated with 100 mJ / cm using an ultra-high pressure mercury lamp through a photomask having a predetermined pattern. 2 The coating was irradiated with ultraviolet light of 1000 nm, and then spray-developed with an alkaline developer consisting of a 0.2% by mass aqueous solution of sodium carbonate to remove the uncured parts and form the desired pattern. The resulting coating was heat-treated in an oven at 230°C for 20 minutes to form a filter segment. The coating thickness was measured using Dektak3030 (manufactured by Japan Vacuum Engineering Co., Ltd.).

[0274] <Evaluation of development residue> The obtained filter segments were checked for the presence or absence of development residues using a microscope (Olympus Optical Co., Ltd. "BX-51") The remaining area of ​​residues in a square pixel with a 50 μm × 50 μm hollow was calculated and evaluated as follows. ◎: No residue ○: 100μm 2 less than △: 100μm 2 More than 500μm 2 less than ×:500μm 2 End

[0275] <Evaluation of Solvent Resistance> The photosensitive coloring composition for color filters was applied onto a glass substrate using a slit die coater, and then prebaked on a hot plate at 90°C for 2 minutes to form a coating film with a thickness of 1 μm. Next, the substrate on which the coating film was formed was cooled to room temperature, and then the coating film was irradiated with radiation having wavelengths of 365 nm, 405 nm, and 436 nm at 1,000 J / m using a high-pressure mercury lamp through a striped photomask. 2The substrate was exposed to light at an exposure dose of 1000 nm. After alkaline development, the substrate was washed with ultrapure water and post-baked at 230°C for 20 minutes to form stripe-shaped pixels on the substrate. The chromaticity ([L*(1), a*(1), b*(1)]) of the stripe-shaped pixels under Illuminant C was measured using a microspectrophotometer (Olympus Optical Co., Ltd., OSP-SP100). The substrate was then immersed in N-methyl-2-pyrrolidone (NMP) or methanol (MeOH) for 15 minutes, and the chromaticity ([L*(2), a*(2), b*(2)]) under Illuminant C after immersion was measured. The color difference ΔEab* was calculated using the above formula and evaluated using the same criteria as for heat resistance. ΔEab* = √((L*(2)- L*(1))2+ (a*(2)- a*(1)) 2+( b*(2)- b*(1)) 2) ◎: ΔEab* is less than 1.0 (very good) ◯: ΔEab* is 1.0 or more and less than 2.5 (good) △: ΔEab* is 2.5 or more and less than 5.0 (practical) ×: ΔEab* is 5.0 or more (not practical)

[0276] <Transmittance evaluation> The photosensitive coloring composition for color filters was applied onto a glass substrate using a slit die coater, and then prebaked for 2 minutes on a hot plate at 90°C. Next, the substrate on which the coating film was formed was cooled to room temperature, and then the coating film was irradiated with radiation having wavelengths of 365 nm, 405 nm, and 436 nm at 1,000 J / m2 using a high-pressure mercury lamp through a striped photomask. 2 After alkaline development, the substrate was washed with ultrapure water and post-baked at 230°C for 20 minutes to form stripe-shaped pixels with a film thickness of 0.5 μm on the substrate. The spectral transmittance of the stripe-shaped pixels at 380 to 780 nm under C light source was then measured and evaluated using a microspectrophotometer (Olympus Optical Co., Ltd., "OSP-SP100"). ◎: Minimum transmittance in the range of 380 to 780 nm is less than 1.0% (very good) 〇: Minimum transmittance in the range of 380 to 780 nm is 1.0% or more and less than 2.5% (good) △: Minimum transmittance in the range of 380 to 780 nm is 2.5% or more and less than 5.0% (practical) ×: Minimum transmittance in the range of 380 to 780 nm is 5.0% or more (not practical)

[0277] [Table 4]

[0278] From the results in Table 4, the photosensitive coloring compositions of Examples 1 to 49 suppressed the development residue and had good solvent resistance. Furthermore, even if the composition was thinner than conventional ones (thickness 0.5 μm), the minimum transmittance was in the practical range, so that a color filter that maintained good pixel chromaticity could be produced. [Explanation of symbols]

[0279] 10 LCD display device 11 Transparent substrate 12 TFT array 13 Transparent electrode layer 14 Alignment layer 15 Polarizing plate 21 Transparent substrate 22 Color Filter 23 Transparent electrode layer 24 Alignment layer 25 Polarizing Plate 30 Backlight unit 31 White LED light source LC Liquid Crystal

Claims

1. A photosensitive coloring composition comprising a colorant (A), a resin (B), a polymerizable compound (C), and a photopolymerization initiator (D), The content of the colorant (A) is 45 to 85% by mass based on 100% by mass of the nonvolatile content of the photosensitive coloring composition, The photosensitive coloring composition, wherein the polymerizable compound (C) contains a compound (C1) represented by the following general formula (1): General formula (1) 【Chemistry 1】 (In the general formula (1), X is a partial structure represented by the following general formula (2), general formula (3), or general formula (4).) 【Chemistry 2】 (In the general formula (2), n represents an integer of 2 to 4, and R 3 represents a hydrogen atom or a methyl group. In general formula (3), n represents an integer of 1 to 4. In general formula (4), n represents an integer of 1 to 4. When X in general formula (1) represents general formula (2) or general formula (4), R 1 , R 2 represents a hydrogen atom or a methyl group, and when X in general formula (1) is general formula (3) and n=2, R 1 , R 2 represents a hydrogen atom, and similarly, when n=1, 3, or 4, R 1 , R 2 represents a hydrogen atom or a methyl group.

2. The content of the polymerizable compound (C) is 1 to 30 mass% in 100 mass% of the nonvolatile content of the photosensitive coloring composition, and the content of the compound (C1) represented by the general formula (1) is 50 to 100 mass% in 100 mass% of the polymerizable compound (C), the photosensitive coloring composition according to claim 1.

3. The photosensitive resin composition according to claim 1 , wherein the photopolymerization initiator (D) includes a photopolymerization initiator (D1) having an oxime ester skeleton.

4. The photosensitive resin composition according to claim 1, wherein the compound (C1) represented by the general formula (1) is contained in an amount of 5 to 30% by mass based on 100% by mass of the nonvolatile content of the photosensitive coloring composition.

5. The photosensitive coloring composition according to claim 1 , wherein the colorant (A) comprises a blue pigment (A1).

6. A color filter having filter segments formed from the photosensitive coloring composition according to any one of claims 1 to 5.

7. A solid-state imaging device comprising the color filter according to claim 6.

8. A liquid crystal display device comprising the color filter according to claim 7.

Citation Information

Patent Citations

  • Color resist composition, color filter, and liquid crystal display device

    JP2010250256A

Cited By

  • Photosensitive coloring composition, color filter, solid-state imaging device, and liquid crystal display device

    JP2026098942A