Method for producing nonwoven fabric sheet, device for producing nonwoven fabric sheet, and nonwoven fabric sheet
By adjusting the viscosity of the liquid material and using coating and impregnation techniques, the neck-in issue is resolved, enabling stable production of nonwoven fabric sheets with enhanced strength and versatility.
Patent Information
- Application Number
- JP2023064249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
The neck-in phenomenon occurs when extruding molten resin with low viscosity, making it difficult to maintain the desired shape of the resulting sheet.
A method and apparatus that adjust the viscosity of the liquid material to 100,000 mPa·s or less, apply it onto a nonwoven fabric using a coating machine, impregnate and solidify it to form a nonwoven fabric sheet, and wind it up, utilizing devices like die coaters and gravure coaters.
Stable production of nonwoven fabric sheets with desired shapes is achieved, even with low-viscosity materials, enhancing strength and handling ease while expanding application possibilities.
Smart Images

Figure 2024151109000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a nonwoven fabric sheet, an apparatus for producing a nonwoven fabric sheet, and a nonwoven fabric sheet. [Background technology]
[0002] A widely known method for producing sheets involves melting raw materials in an extruder and extruding the resulting molten resin into a sheet shape through an extrusion die (T-die) (see, for example, Patent Document 1 (JP 2020-146853 A)). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-146853 A Summary of the Invention [Problem to be solved by the invention]
[0004] By the way, since a certain distance (air gap) is provided between the extrusion die (T-die) and the cooling roll for the extruded molten resin, a phenomenon called neck-in occurs in the air gap, where the weight, tension, speed, etc. of the molten resin cause the obtained film width to be narrower than the die width.
[0005] At this time, if the viscosity of the molten resin is low, the amount of neck-in tends to be large, which may make it difficult to produce a sheet in the desired shape.
[0006] Therefore, an object of the present invention is to provide a nonwoven fabric sheet manufacturing method and a nonwoven fabric sheet manufacturing apparatus that can obtain a sheet of a desired shape when manufacturing a sheet made of a resin material, even if the viscosity of the liquid material containing the raw material is low. Other objects and novel features will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]
[0007] A method for producing a nonwoven fabric sheet in one embodiment includes the steps of: (a) preparing a liquid material containing raw materials and having a viscosity of 100,000 mPa s or less; (b) applying the liquid material in the form of a sheet onto a nonwoven fabric using a coating machine; (c) impregnating the nonwoven fabric with the liquid material; (d) solidifying the liquid material impregnated into the nonwoven fabric to obtain a nonwoven fabric sheet; and (e) winding up the nonwoven fabric sheet.
[0008] One embodiment of a nonwoven fabric sheet manufacturing apparatus includes a raw material container that adjusts and stores a liquid material of a predetermined viscosity containing raw materials, a nonwoven fabric discharge section that sends out the nonwoven fabric, a coater that applies the liquid material to the nonwoven fabric, an impregnation area that impregnates the nonwoven fabric with the liquid material, a solidification area that solidifies the liquid material to form a nonwoven fabric sheet, and a sheet winding section that winds up the nonwoven fabric sheet.
[0009] In the above-mentioned method and apparatus for producing a nonwoven fabric sheet, the liquid material is adjusted so that its viscosity is 100,000 mPa·s or less. Effect of the Invention
[0010] According to one embodiment, in the production of a nonwoven fabric sheet, even when a liquid material with a viscosity that causes a large neck-in amount is used when an extrusion molding die (T-die) is used, the nonwoven fabric sheet can be stably produced. [Brief description of the drawings]
[0011] [Figure 1] 1 is a diagram showing a schematic configuration of a manufacturing apparatus for a nonwoven fabric sheet according to a first embodiment. [Diagram 2] FIG. 2 is a diagram for explaining a case where a gravure roll is used as a coater in FIG. [Diagram 3] FIG. 13 is a diagram showing a schematic configuration of a nonwoven fabric sheet manufacturing apparatus according to a second embodiment. [Figure 4] FIG. 1 is a diagram showing the chemical structure of glucomannan. [Diagram 5] FIG. 1 is a diagram showing the chemical structural formula of cellulose. [Figure 6] FIG. 1 is a diagram showing a schematic configuration of a moisture recovery device using a nonwoven fabric sheet. [Figure 7] FIG. 1 is a diagram showing a schematic configuration of a moisture recovery device using a nonwoven fabric sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the present embodiment will be described in detail with reference to the drawings. In all the drawings for explaining the embodiment, the same reference numerals are used to designate members having the same functions, and the repeated description thereof will be omitted.
[0013] (Embodiment 1) <Nonwoven fabric sheet manufacturing equipment> FIG. 1 is a diagram showing a schematic configuration of a manufacturing apparatus for a nonwoven fabric sheet according to the present embodiment.
[0014] The nonwoven fabric sheet manufacturing apparatus 10 shown in Figure 1 comprises a raw material container 11 that prepares and stores liquid material LM containing raw materials and having a viscosity of 100,000 mPa·s or less, a nonwoven fabric discharge section 12 that feeds out the nonwoven fabric NW, a coater 13 that applies the liquid material LM onto the nonwoven fabric NW fed out from the nonwoven fabric discharge section 12, an impregnation region 14 that impregnates the nonwoven fabric NW with the sheet-like liquid material SLM applied onto the nonwoven fabric NW, a solidification region 15 that solidifies the liquid material SLM impregnated into the nonwoven fabric NW to form a nonwoven fabric sheet 50, and a sheet winding section 16 that winds up the nonwoven fabric sheet 50 following the solidification region 15.
[0015] The raw material container 11 is a container for preparing and storing a liquid material containing the raw material and having a viscosity of 100,000 mPa s or less. The liquid material stored in the raw material container 11 can also be called a coating liquid to be coated on the nonwoven fabric NW by a coating machine 13 described later.
[0016] This raw material container 11 contains raw material, and adjusts the viscosity of the raw material to be a liquid material of 100,000 mPa·s or less. For example, when the above viscosity is satisfied by heating and melting the raw material, only the raw material can be stored in the raw material container 11. In this case, the viscosity can be adjusted by providing a heating unit that heats the raw material to the above viscosity. An example of this heating unit is a heating source such as a heater, and the raw material is heated by this heating source and the temperature is maintained in the raw material container 11.
[0017] The raw material can also be mixed with a solvent to adjust the viscosity to 100,000 mPa·s or less in liquid form. For example, when the raw material must be heated to an extremely high temperature to be heated and melted as described above, or when it is difficult to adjust the viscosity to 100,000 mPa·s even after heating and melting, a solvent can be used to dissolve the raw material and adjust the viscosity to 100,000 mPa·s or less. Even if the raw material has a viscosity of 100,000 mPa·s or less when heated and melted, the viscosity can be adjusted to 100,000 mPa·s or less by using a solvent.
[0018] In this way, when the raw material and the solvent are mixed to prepare a raw material solution, for example, a solvent supply section that supplies the solvent to the raw material container 11 is provided, and the amount of the solvent supplied is adjusted so that the raw material solution (liquid material) has a viscosity within the above range.
[0019] The viscosity of the liquid material herein refers to the viscosity of the coating liquid to be applied by the coater 13, and is preferably 10 to 80,000 mPa·s, and more preferably 100 to 10,000 mPa·s.
[0020] The nonwoven fabric discharge section 12 is a component that feeds out the nonwoven fabric NW. Here, the nonwoven fabric NW is a substrate for coating with the liquid material. In this nonwoven fabric discharge section, the nonwoven fabric NW is wound in a roll shape, and the nonwoven fabric NW can be continuously fed to the coater 13 so that the liquid material can be coated on the surface of the nonwoven fabric NW.
[0021] The coater 13 is a device that coats the nonwoven fabric NW with the liquid material sent from the raw material container 11 by a pump or the like. This coater 13 can be a known coater used in sheet forming, and examples of such coaters include coaters that perform contact coating processing, such as a die coater, a gravure coater, a bar coater, and a blade coater. The coater 13 can coat the nonwoven fabric NW with the liquid material in a uniform width. These coaters can be selected, for example, depending on the viscosity of the liquid material.
[0022] 1 shows an example in which a die coater is used as the coater 13. In this case, a slot die type die coater is preferred in which the liquid material is extruded from a die head and coated onto the nonwoven fabric NW. In this case, a back roll 17 is provided at a position opposite to the slit of the coater 13 for discharging the liquid material across the substrate.
[0023] 2 shows an example in which a gravure coater is used as the coater 13. Fig. 2 is a diagram illustrating a configuration in which a gravure coater is used to coat a liquid material LM onto a substrate BM in a sheet manufacturing apparatus 10. Here, the cross-sectional structure of the gravure coater is shown so that the internal structure can be seen.
[0024] 2 is a vertical coater with a chamber (tank) 13a arranged vertically (parallel to the direction of gravity). This coater has a chamber (tank) 13a for storing the liquid material LM, a coating roll (gravure roll) CR partially immersed in the chamber (tank) 13a, a blade 13b for preventing the liquid material LM from scattering and for adjusting the amount of liquid on the roll surface, and a second blade 13c for preventing the coating liquid from leaking from the gap between the liquid material in the chamber (tank) and the coating roll (gravure roll) CR.
[0025] The first blade 13b is disposed on the rotation direction side of the coating roll CR so that the angle and pressing pressure of the first blade 13b can be adjusted to adjust the amount of liquid material LM adhering to the surface of the coating roll CR. Then, the liquid material LM adhering to the surface of the coating roll CR is transferred to the surface of the substrate BM to form a sheet-like liquid material SLM.
[0026] The chamber (tank) 13a of the gravure coater may be of either a vertical or horizontal type. In the case of a horizontal type, the second blade 13c for preventing leakage of the coating liquid is not required, and the chamber (tank) 13a can be configured to have only the first blade 13b for preventing splashing of the liquid material LM and adjusting the amount of liquid on the roll surface.
[0027] The impregnation area 14 is an area where the sheet-shaped liquid material SLM applied by the coater 13 is impregnated into the nonwoven fabric NW. In this impregnation area 14, the sheet-shaped liquid material SLM is permeated into gaps between fibers of the nonwoven fabric NW. For example, impregnation rolls 14a may be provided to sandwich the nonwoven fabric NW coated with the sheet-shaped liquid material SLM from above and below, thereby impregnating the nonwoven fabric NW with the sheet-shaped liquid material SLM. In this case, although an example in which two sets of impregnation rolls 14a are provided is shown in FIG. 1, one set or three or more sets may be provided. In addition, the impregnation rolls 14a may be configured to apply pressure to the nonwoven fabric NW coated with the sheet-shaped liquid material SLM to promote impregnation.
[0028] Depending on the relationship between the viscosity of the liquid material LM used and the basis weight of the nonwoven fabric NW, the liquid material LM may be applied from the coater 13 onto the nonwoven fabric NW while the nonwoven fabric NW is being impregnated with the liquid material LM. If sufficient impregnation can be achieved in this manner, it is not necessary to provide an impregnation member such as the impregnation roll 14a.
[0029] The solidification region 15 is a region where the nonwoven fabric NW impregnated with the sheet-like liquid material SLM in the impregnation region 14 is solidified to form a nonwoven fabric sheet 50, and it is the raw material that is solidified at this time. In this solidification region 15, when the liquid material consists of only the raw material, the temperature of the liquid material (raw material) impregnated into the nonwoven fabric NW is lowered to solidify it. At this time, for example, without providing a specific cooling means, the temperature of the raw material impregnated into the nonwoven fabric NW can be naturally lowered at room temperature of about 25°C to solidify it. Alternatively, a cooling means may be provided to actively lower the temperature of the raw material impregnated into the nonwoven fabric NW to solidify it.
[0030] Furthermore, when the liquid material is a raw material solution in which the raw material and the solvent are mixed, the liquid material impregnated into the nonwoven fabric NW is solidified by volatilizing the solvent by heating or the like. At this time, the solvent can be naturally volatilized at room temperature or the like without providing a special heating means. Alternatively, a heating means such as a heater may be provided to actively heat the temperature of the liquid material impregnated into the nonwoven fabric NW, promoting the volatilization of the solvent and solidifying it.
[0031] As described above, by solidifying the liquid material impregnated into the nonwoven fabric NW, a nonwoven fabric sheet 50 in which the nonwoven fabric NW and the raw material are integrated is obtained.
[0032] The sheet winding section 16 is a member capable of winding up the obtained nonwoven fabric sheet 50 and storing it as a rolled nonwoven fabric sheet. The nonwoven fabric sheet 50 wound up here can be made into a rolled nonwoven fabric sheet product. If necessary, this nonwoven fabric sheet can also be further processed to make a sheet product.
[0033] Furthermore, it is preferable to provide a feed roll 18 between the nonwoven fabric discharge section 12 and the sheet winding section 16 so as to stably feed the nonwoven fabric NW. The feed roll 18 functions to sandwich the nonwoven fabric NW (the nonwoven fabric NW or the nonwoven fabric sheet 50 impregnated with the liquid material after the liquid material has been applied) and feed it to the subsequent stage.
[0034] <Sheet manufacturing method> Next, a method for manufacturing the sheet in embodiment 1 will be described. The method for manufacturing the sheet includes a step (step (a)) of preparing a liquid material containing raw materials and having a viscosity of 100,000 mPa s or less, a step (step (b)) of applying the liquid material to a nonwoven fabric in a sheet form using a coater after step (a), a step (step (c)) of impregnating the nonwoven fabric with the liquid material after step (b), a step (step (d)) of solidifying the liquid material impregnated into the nonwoven fabric to obtain a nonwoven fabric sheet after step (c), and a step (step (e)) of winding up the nonwoven fabric sheet after step (d).
[0035] Hereinafter, a sheet manufacturing method using the sheet manufacturing apparatus 10 explained in FIG. 1 will be explained as a specific apparatus configuration.
[0036] First, a step of preparing a liquid material containing raw materials and having a viscosity of 100,000 mPa·s or less is carried out (step (a)).
[0037] In this viscosity adjustment step, as described above, a liquid material containing raw materials and having a viscosity of 100,000 mPa s or less is prepared in raw material container 11. For example, when the above viscosity is satisfied by heating and melting the raw material, only the raw material is stored in raw material container 11, and the raw material is heated to the above viscosity to adjust the viscosity.
[0038] In addition, when mixing the raw material with a solvent and adjusting the viscosity to 100,000 mPa s or less, the supply amount of the solvent is adjusted so that the raw material solution (liquid material) obtained by mixing the raw material with the solvent has a viscosity in the above range. In this case, temperature adjustment such as heating may be combined as necessary.
[0039] The viscosity of the liquid material in step (a) is the viscosity of the coating liquid for coating by the coater 13 as described above, and is preferably 10 to 50,000 mPa·s, and more preferably 100 to 10,000 mPa·s.
[0040] Next, after step (a), a step of applying the liquid material in the form of a sheet onto the nonwoven fabric using a coater is carried out (step (b)).
[0041] In this embodiment, a nonwoven fabric discharge section 12 is provided, and a liquid material LM is applied in sheet form onto the nonwoven fabric NW sent out from this nonwoven fabric discharge section 12 by a coating machine 13, thereby obtaining a sheet-shaped liquid material SLM (coated body).
[0042] The nonwoven fabric NW used here is not particularly limited, and any known nonwoven fabric can be used without restriction. Examples of the nonwoven fabric NW include inorganic fibers such as carbon fiber, glass fiber, and metal fiber, and chemical fibers such as nylon (polyamide), tetron, rayon, cupra, acetate, vinylon, acrylic, polyethylene terephthalate (polyester), polypropylene, aramid, polyester, polyimide, and polyacrylic. Natural fibers such as cellulose fiber, cotton, linter, kapok, flax, hemp, ramie, silk, and wool can also be used. Carbon fiber, glass fiber, and chemical fibers are preferable because they have relatively high rigidity and can increase the rigidity of the nonwoven fabric sheet 50 and improve the strength of the sheet itself.
[0043] The average fiber diameter of the fibers constituting the nonwoven fabric is preferably 0.1 μm to 0.5 mm, more preferably 0.4 μm to 200 μm. The average fiber length of the fibers is preferably 1 mm to 200 mm. The thickness of the nonwoven fabric is preferably 10 μm to 5 mm, more preferably 20 μm to 3 mm.
[0044] The weight of the nonwoven fabric NW is 0.1 to 10,000 g / m 2 is preferably 0.2 to 5000 g / m 2 is more preferable. By setting the fiber basis weight in this range, not only can a sufficient amount of liquid material be impregnated into the voids of the nonwoven fabric NW, but also the strength of the nonwoven fabric sheet 50 can be maintained. It is preferable to select the basis weight of the nonwoven fabric NW appropriately after comprehensively considering the design strength, such as the tensile strength, bending strength, and fatigue strength, and the heat resistance, of the nonwoven fabric sheet 50 impregnated with the liquid material.
[0045] In this case, the coating amount of the liquid material is adjusted according to the amount of raw material to be impregnated into the nonwoven fabric NW, and the thickness of the sheet-shaped liquid material SLM is determined. That is, when the liquid material is composed of only raw materials, the impregnated liquid material LM is entirely solidified to become the nonwoven fabric sheet 50, so the coating amount is applied so as to be the impregnated amount. When a raw material solution obtained by mixing raw materials and a solvent is used as the liquid material, the solvent in the impregnated liquid material LM volatilizes, and the remaining raw material components are solidified to become the nonwoven fabric sheet 50. Therefore, the coating amount of the liquid material LM is determined and applied in consideration of the amount of the raw material components.
[0046] In coating the liquid material LM, the thickness of the sheet-like liquid material SLM to be coated varies depending on various factors such as the conveying speed of the nonwoven fabric NW, the viscosity of the liquid material LM used, and the amount of liquid material LM discharged in the coater 13, so these coating conditions can be adjusted to achieve the desired thickness.
[0047] The viscosity of the liquid material LM is set to 100000 mPa·s or less as described above. The conveying speed of the nonwoven fabric NW is, for example, preferably 1 to 500 m / min, and more preferably 5 to 300 m / min.
[0048] It is preferable to select the coater 13 according to the viscosity of the liquid material LM. For example, when the viscosity of the liquid material LM is 1000 mPa·s or more, it is preferable to use a die coater as the coater 13, and when the viscosity of the liquid material LM is less than 1000 mPa·s, it is preferable to use a gravure coater as the coater 13. Furthermore, when the viscosity of the liquid material LM is 10000 mPa·s or more, it is preferable to use a device having a screw shape, such as a single-screw extruder or a twin-screw extruder, instead of a pump.
[0049] Next, after step (b), a step of impregnating the nonwoven fabric NW with the liquid material LM is carried out (step (c)).
[0050] In this embodiment, the sheet-like liquid material SLM formed by coating on the nonwoven fabric NW is allowed to permeate into gaps between the fibers of the nonwoven fabric NW in the impregnation region 14. This impregnation operation can be performed, for example, by providing impregnation rolls 14a and sandwiching the nonwoven fabric NW coated with the sheet-like liquid material SLM from above and below, thereby impregnating the nonwoven fabric NW with the sheet-like liquid material SLM.
[0051] As described above, the impregnation roll 14a may be configured to apply pressure to the nonwoven fabric NW coated with the sheet-like liquid material SLM to promote the impregnation. In this case, the pressure applied by the impregnation roll 14a is preferably 0.01 to 100 MPa, and more preferably 0.1 to 50 MPa.
[0052] As described above, depending on the relationship between the viscosity of the liquid material LM used and the basis weight of the nonwoven fabric NW, the liquid material LM may be applied from the coater 13 onto the nonwoven fabric NW while the nonwoven fabric NW is being impregnated with the liquid material LM. If sufficient impregnation can be achieved in this manner, it is not necessary to provide an impregnation member such as the impregnation roll 14a.
[0053] Furthermore, after the step (c), a step (d) is performed in which the liquid material impregnated into the nonwoven fabric NW is solidified to obtain a nonwoven fabric sheet 50.
[0054] In this embodiment, the liquid material impregnated into the nonwoven fabric NW is solidified to obtain a nonwoven fabric sheet 50 in which the nonwoven fabric NW and the liquid material (raw material) are integrated together. Here, the solidification of the liquid material (raw material) is performed in a solidification region 15.
[0055] When the liquid material is composed of only the raw material, the temperature of the liquid material impregnated into the nonwoven fabric NW is lowered to solidify it. At this time, for example, the temperature of the raw material can be naturally lowered at room temperature or the like without providing a cooling means to solidify it. Alternatively, a cooling means may be provided to actively lower the temperature of the raw material to solidify it.
[0056] The solidification temperature is specific to the raw material used, and may be set to a temperature lower than the melting point or glass transition point of the raw material. By setting the temperature at such a temperature, the liquid raw material solidifies to obtain a sheet.
[0057] In addition, when the liquid material is a raw material solution in which a raw material and a solvent are mixed, the solvent is evaporated from the liquid material impregnated in the nonwoven fabric NW by heating or the like, and the liquid material is solidified. At this time, the solvent may be evaporated naturally at room temperature or the like, but in order to improve manufacturing efficiency, it is preferable to provide a heating means such as a heater to heat the nonwoven fabric NW impregnated with the liquid material, promote the evaporation of the solvent, and solidify the liquid material. In this manner, the nonwoven fabric sheet 50 can be formed.
[0058] After this solidification, the nonwoven fabric sheet 50 is wound up (step (e)). Here, the nonwoven fabric sheet 50 is wound up into a roll by the sheet winding unit 16. In this manner, the nonwoven fabric sheet can be continuously obtained as a product.
[0059] By adopting the configuration of the above embodiment, even when a low-viscosity liquid material is used as the raw material, it is possible to prevent the sheet from becoming significantly different from the desired shape, such as necking-in, and the limitations on the raw materials that can be used are significantly relaxed, making it possible to provide a manufacturing technology for nonwoven fabric sheets with a wide range of applications. Furthermore, the nonwoven fabric sheet obtained in this manner is stronger than a sheet made only from the raw material, and is easier to handle, which is preferable.
[0060] (Embodiment 2) <Nonwoven fabric sheet manufacturing equipment> FIG. 3 is a diagram showing a schematic configuration of a nonwoven fabric sheet manufacturing apparatus according to another embodiment.
[0061] Similar to the above-described sheet manufacturing apparatus 10, the sheet manufacturing apparatus 20 shown in FIG. 3 comprises a raw material container 11 for preparing and storing a liquid material containing raw materials and having a viscosity of 100,000 mPa·s or less, a nonwoven fabric discharge section 12 for feeding out the nonwoven fabric NW, a coater 13 for applying the liquid material to the nonwoven fabric NW fed out from the nonwoven fabric discharge section 12, an impregnation region 14 for impregnating the nonwoven fabric NW with the liquid material applied onto the nonwoven fabric NW, a solidification region 15 for solidifying the liquid material impregnated into the nonwoven fabric NW to form a nonwoven fabric sheet 50, and a sheet winding section 16 for winding up the nonwoven fabric sheet 50 following the solidification region 15.
[0062] This sheet manufacturing apparatus 20 differs from the sheet manufacturing apparatus 10 in that it further includes a drying processing section 21. In the following, a description of the same configuration will be omitted, and different configurations will be described in detail.
[0063] As described above, the sheet manufacturing apparatus 20 includes the components of the sheet manufacturing apparatus 10, and further includes a drying processing unit 21. The drying processing unit 21 is disposed in the solidification area 15, and is a member that dries the solvent contained in the liquid material impregnated into the nonwoven fabric NW. That is, the second embodiment is an embodiment in which a raw material solution (liquid material) obtained by mixing a raw material and a solvent is used as the liquid material.
[0064] The drying processing section 21 is provided to efficiently volatilize the solvent contained in the liquid material impregnated into the nonwoven fabric NW in the step (d). Usually, a heated atmosphere is created inside the drying processing section 21 to promote the volatilization of the solvent. To create a heated atmosphere, for example, a gas (air, etc.) heated to a set temperature by a heat source such as a heater may be introduced into the drying processing section 21. At this time, it is preferable to continue the operation of introducing the heated gas so that the temperature inside the drying processing section 21 can be maintained near the set temperature.
[0065] The heating temperature can be set to an optimum temperature depending on the solvent used. For example, when water or a lower alcohol is used as the solvent, the heating temperature is preferably 50 to 90°C. However, the upper limit is set to a temperature below the boiling point of the solvent. By setting the temperature in this range, the volatilization efficiency of the solvent can be significantly improved, and it is possible to prevent the occurrence of bubbles in the sheet due to the boiling of the solvent. In addition, in order to promote volatilization and drying, a configuration may be provided in which a blower is provided that can blow air against the sheet-shaped liquid material SLM.
[0066] Furthermore, when the drying processing section 21 is provided, a solvent recovery mechanism may be provided to cool, liquefy, and recover the volatilized solvent generated in the drying processing section 21. By providing this solvent recovery mechanism, the solvent can be reused. Furthermore, the recovered solvent can be reused by circulating it as a solvent for dissolving the raw material again. By reusing it in this manner, the costs of the manufacturing operation of the nonwoven fabric sheet of this embodiment can be reduced, and the nonwoven fabric sheet can be manufactured efficiently.
[0067] <Method of manufacturing nonwoven fabric sheet> In the present embodiment, the nonwoven fabric sheet manufacturing apparatus 20 used differs from the nonwoven fabric sheet manufacturing apparatus 10 described above in that it has a drying processing section 21 or not. Therefore, the basic operations in the nonwoven fabric sheet manufacturing method are the same as those in the first embodiment.
[0068] In this embodiment 2, in addition to the operations in embodiment 1, the liquid material impregnated into the nonwoven fabric NW is heated by a drying unit 21 to volatilize the solvent contained in the liquid material and dry it, efficiently forming a nonwoven fabric sheet 50 in which the nonwoven fabric and the raw material are integrated. This drying process is performed in a solidification area 15.
[0069] In this drying process, it is preferable to heat the sheet to a temperature at which the volatilization of the solvent used is promoted as described above, and the optimum temperature is set according to the solvent used. For example, when water or a lower alcohol is used as the solvent, the heating temperature is preferably 50 to 90°C. However, the upper limit is set to a temperature below the boiling point of the solvent. By setting the temperature in this range, the volatilization efficiency of the solvent can be significantly improved, and it is possible to prevent the occurrence of bubbles in the sheet due to the boiling of the solvent. In addition, in order to promote the volatilization and drying, a configuration may be provided in which a blower capable of blowing air against the sheet-shaped liquid material SLM is provided.
[0070] In addition, by providing a solvent recovery mechanism as described above, the solvent evaporated in the drying processing unit 21 can be cooled and liquefied, and the solvent can be recovered. The solvent recovered in this manner can be circulated and reused as a solvent for the raw material.
[0071] <Raw materials> Next, the raw material used in the first and second embodiments will be described. The raw material is not particularly limited, and as described above, it is sufficient that the liquid material has a viscosity of 100,000 mPa s or less as a liquid material for coating by the coater 13. This liquid material may be prepared by melting the raw material, or by mixing and dissolving it in a solvent.
[0072] An example of this raw material is a resin such as a so-called injection grade or spinning grade low-viscosity liquid resin that is injected from a die in the molding of resin or the like.
[0073] In addition, biodegradable materials can also be used as raw materials. As the biodegradable material in the present invention, a water-soluble material is suitable, and since it is easy to dissolve the material in water as a solvent to obtain a low-viscosity liquid material, it is excellent not only in moldability but also in terms of low environmental impact.
[0074] Examples of raw materials that can be used in this embodiment include polysaccharides and gelatin. Examples of polysaccharides include glucomannan, cellulose-based materials, pectin, starch, isomaltodextrin, agar, etc. These may be used alone or in combination of two or more. In particular, it is preferable to contain at least one selected from glucomannan, cellulose-based materials, gelatin, and agar.
[0075] Glucomannan is a water-soluble polysaccharide that is contained in about 10% of the tubers of konjac root, and can be extracted by purifying konjac flour with alcohol. Glucomannan has the chemical structure shown in Figure 4, and is a polysaccharide in which D-glucose and D-mannose are bonded by β-1,4 bonds in a ratio of 1:1.6 (n indicates the number of repeating unit structures). It has one branch for every 50 to 60 sugars, and has a large molecular weight, with some exceeding 1 million.
[0076] The glucomannan used here preferably has a molecular weight in the range of 20 to 2,000,000. Glucomannan having such a molecular weight has a viscosity of 1,000 to 20,000 mPa·s when added to water at 1% by mass and melted.
[0077] In addition, glucomannan has many hydroxyl groups and can be dissolved in an alcohol solvent to easily reduce the viscosity.
[0078] Cellulosic materials are materials that contain cellulose or cellulose in part. Cellulose is a naturally occurring polymer in which many β-glucose molecules are polymerized in a linear chain through glycosidic bonds. It has the chemical structure shown in Figure 6 and the molecular formula (C6H 10 O5) n The cellulose-based material is a carbohydrate (polysaccharide) represented by the formula: Examples of the cellulose-based material include carboxymethyl cellulose and cellulose nanofiber.
[0079] The cellulosic material used here preferably has a molecular weight in the range of 1000 to 500000. A cellulosic material having such a molecular weight has a viscosity of 50 to 50000 mPa·s when melted by heating to 20 to 60° C.
[0080] Furthermore, cellulosic materials have many hydroxyl groups, and can be dissolved in alcohols as a solvent, allowing the viscosity to be easily reduced.
[0081] Gelatin is a fibrous protein called collagen, and agar is obtained by freezing and drying solidified mucus from red algae. It is insoluble in water as is, but can be melted and made low-viscosity by heating.
[0082] Furthermore, the liquid material may contain a filler. Examples of the filler include inorganic substances such as alumina, silica, aluminum hydroxide, and boehmite, as well as cellulose (including cellulose nanofibers), carbon fibers, carbon nanotubes, carbon nanofibers, graphene, fullerene, and aramid fibers. Cellulose in which the hydrophilic group of cellulose is replaced with a hydrophobic group may be used as the cellulose.
[0083] (Embodiment 3) <Nonwoven fabric sheet> The nonwoven fabric sheet of this embodiment is a sheet-like material formed by impregnating and solidifying the above-mentioned low-viscosity liquid material into the nonwoven fabric NW. As described above, this low-viscosity liquid material is obtained by melting the raw material or dissolving the raw material in a solvent, and the raw material preferably contains at least one material selected from, for example, glucomannan, cellulose-based material, gelatin, and agar.
[0084] This nonwoven fabric sheet 50 is made of a nonwoven fabric NW and an impregnating material containing a low-viscosity liquid material that is impregnated and solidified in this nonwoven fabric NW. This nonwoven fabric sheet 50 may have various treatments performed on its surface. The nonwoven fabric sheet can have any thickness, and is preferably, for example, 10 μm to 5 mm, and more preferably 20 μm to 3 mm.
[0085] The ratio of the nonwoven fabric to the solidified material (raw material) in this nonwoven fabric sheet 50 can be any ratio. For example, it is preferable that the ratio of the solidified raw material to the entire nonwoven fabric sheet is 5 volume % or more and 90 volume % or less. In this way, by increasing the ratio of the raw material relative to the nonwoven fabric, it is possible to effectively exhibit the characteristics derived from the solidified portion made of the raw material. In this case, the ratio of this raw material can be calculated by the following formula (1). Percentage of raw material [%] = (volume of solidified raw material) / (volume of nonwoven sheet) (1)
[0086] In this case, by increasing the proportion of nonwoven fabric, it is possible to improve the strength of the nonwoven fabric sheet 50. The composition ratio can be determined according to the purpose of the nonwoven fabric sheet 50, and can be adjusted by appropriately selecting the nonwoven fabric and liquid material to be used.
[0087] This nonwoven fabric sheet can be a multi-layered sheet having other layers on its surface, in which case all layers may be the nonwoven fabric sheet of this embodiment, or some layers may be the nonwoven fabric sheet of this embodiment and the remaining layers may be sheets other than those of this embodiment (which may be sheets made of nonwoven fabric or nonwoven fabric sheets not made of nonwoven fabric). In other words, it is sufficient to have one or more layers of the nonwoven fabric sheet used in this embodiment.
[0088] The following is a specific example of a nonwoven fabric sheet made from glucomannan. When glucomannan is added at 0.5% by mass to water used as a solvent, it becomes a liquid material with a viscosity of 10,000 mPa·s.
[0089] The liquid material obtained by adding the liquid material to the solvent in this manner can be used, for example, to manufacture a nonwoven fabric sheet using the nonwoven fabric sheet manufacturing apparatus 10 shown in Figure 1. In this case, for example, the nonwoven fabric NW has a width of 50 cm, a thickness of 2 mm, and a basis weight of 500 g / cm. 2A nonwoven fabric made of polyethylene (PE) with a porosity of 50% is used, and the liquid material LM is applied onto the nonwoven fabric NW at a conveying speed of 0.1 m / sec and a discharge rate of 3000 mL / min from a coater 13 (die coater) with a slit width of 1 mm for discharging the liquid material LM.
[0090] In the impregnation region 14, the nonwoven fabric NW on which the sheet-like liquid material SLM was formed was sandwiched from above and below by impregnation rolls 14a with a pressure of 1 MPa applied, so that the liquid material LM was impregnated into the nonwoven fabric NW. The nonwoven fabric NW was then conveyed by the feed roll 19 while being solidified by natural cooling at room temperature, to form a nonwoven fabric sheet 50. The nonwoven fabric sheet 50 having a thickness of 2 mm was wound up by the sheet winding section 16, to obtain a roll-like nonwoven fabric sheet 50.
[0091] The nonwoven sheet made of glucomannan thus obtained can be used as a water-absorbent sheet by utilizing the hygroscopicity of the raw material.
[0092] The glucomannan sheet obtained in this way can be used as a water-absorbent sheet by utilizing the hygroscopicity of the raw material. An example of its use as a water-absorbent sheet will be explained using Figures 6 and 7. In these figures, the arrows indicate the transfer of thermal energy.
[0093] 6 and 7 show an example of the application of a glucomannan nonwoven fabric sheet 50 as a water-absorbing sheet that utilizes sunlight. The moisture recovery device 100 shown here is composed of a heat collector 101, a heat storage tank 102, an inclined plate 103, and a moisture recovery container 104.
[0094] The heat collector 101 is, for example, a device that can extract thermal energy from sunlight and transfer it to the heat storage tank 102. The heat storage tank 102 is a portion that stores the heat collected by the heat collector 101, and the stored heat can be used to heat the nonwoven fabric sheet 50 at a desired timing. The inclined plate 103 is a plate-like body that is arranged at an incline above the nonwoven fabric sheet 50. This inclined plate 103 cools and liquefies the water vapor released from the nonwoven fabric sheet 50, and guides it to the moisture collection container 104. The moisture collection container 104 is a container that stores the liquefied water guided to the inclined plate 103.
[0095] For example, this moisture recovery device 100 is used as follows. First, as shown in Fig. 6, during the day, thermal energy of sunlight is collected by a heat collector 101, and the collected thermal energy is stored in a heat storage tank 102. Here, the nonwoven fabric sheet 50 is exposed to the outside atmosphere, and absorbs moisture (water vapor) contained in the air. As described above, the nonwoven fabric sheet 50 made of glucomannan has excellent moisture absorption properties and can retain a large amount of moisture.
[0096] Next, at night after the sun has set, the nonwoven fabric sheet 50 is heated using the thermal energy stored in the heat storage tank 102, as shown in FIG. 7. This heating is performed to a temperature at which the nonwoven fabric sheet 50 releases (discharges) the moisture absorbed by the nonwoven fabric sheet 50, and a temperature of, for example, 80 to 100° C. is preferable. The moisture released from the nonwoven fabric sheet 50 diffuses upward and comes into contact with the inclined plate 103, and is liquefied on the surface of the inclined plate 103. The liquefied moisture flows in the lower direction of the inclined plate 103 along the inclination of the inclined plate 103, is guided to the moisture recovery container 104, and is finally stored in the moisture recovery container 104.
[0097] The present invention has been specifically described above using embodiments and examples. However, the present invention should not be construed as being limited to these embodiments and examples, and it goes without saying that the present invention can be modified in various ways without departing from the spirit of the present invention. [Explanation of symbols]
[0098] 10,20 Sheet manufacturing equipment 11 Raw material container 12 Nonwoven fabric unloading section 13 Coating machine 14 Impregnation area 15 Solidification area 16 Sheet winding section 17 Back Roll 18 Feed roll 21 Drying processing section 50 Nonwoven Sheet LM Liquid Material NW Non-woven fabric SLM Sheet-shaped liquid material
Claims
1. A method for producing a nonwoven sheet, comprising: (a) preparing a liquid material containing raw materials and having a viscosity of 100,000 mPa·s or less; (b) after the step (a), applying the liquid material onto a nonwoven fabric in a sheet form using a coating machine; (c) after the step (b), a step of impregnating the nonwoven fabric with the liquid material; (d) after the step (c), solidifying the liquid material impregnated into the nonwoven fabric to obtain a nonwoven fabric sheet; and (e) after the step (d), a step of winding up the nonwoven fabric sheet.
2. The method for producing a nonwoven fabric sheet according to claim 1, The method for producing a sheet, wherein the nonwoven fabric is made of a material containing at least one selected from polyester, polypropylene, polyethylene, rayon, nylon, polyethylene terephthalate, aramid glass fiber, and carbon fiber.
3. The method for producing a nonwoven fabric sheet according to claim 1, The nonwoven fabric has a basis weight of 0.1 g / m 2 ~10000g / m 2 A method for producing a nonwoven fabric sheet, the range being:
4. The method for producing a nonwoven fabric sheet according to claim 1, In the step (c), the nonwoven fabric is impregnated with the liquid material by impregnation rolls disposed above and below the nonwoven fabric.
5. The method for producing a nonwoven fabric sheet according to claim 4, In the step (c), the nonwoven fabric is pressed by the impregnated roll.
6. The method for producing a nonwoven fabric sheet according to claim 5, The method for producing a nonwoven fabric sheet, wherein the pressure applied by the impregnated roll is 0.01 to 100 MPa.
7. The method for producing a nonwoven fabric sheet according to claim 1, A method for producing a nonwoven fabric sheet, comprising using, as the raw material, a powdery filler containing at least one selected from glucomannan, a cellulose-based material, gelatin, and agar.
8. The method for producing a nonwoven fabric sheet according to claim 1, The liquid material contains the raw material and a solvent, The method for producing a nonwoven fabric sheet, further comprising a drying treatment step of volatilizing the solvent by heating in the step (d).
9. The method for producing a nonwoven fabric sheet according to claim 8, The method for producing a nonwoven sheet, wherein the solvent is water or alcohol.
10. A nonwoven sheet manufacturing apparatus, including: a raw material container for preparing and storing a liquid material containing the raw material and having a viscosity of 100,000 mPa·s or less; a nonwoven fabric discharge section for delivering the nonwoven fabric; a coater that applies the liquid material in a sheet form onto the nonwoven fabric delivered from the nonwoven fabric discharge section; an impregnation region for impregnating the nonwoven fabric with the applied liquid material; A solidification region in which the liquid material impregnated in the nonwoven fabric is solidified to form a sheet; and a sheet winding section for winding up the nonwoven fabric sheet obtained by solidifying the liquid material;
11. The nonwoven fabric sheet manufacturing apparatus according to claim 10, The nonwoven fabric sheet manufacturing apparatus has a drying treatment section in the solidification area, which volatilizes the solvent in the sheet by heating.
12. The nonwoven fabric sheet manufacturing apparatus according to claim 11, The liquid material contains the raw material and a solvent, The nonwoven fabric sheet manufacturing apparatus further comprises a recovery section in the solidification area that recovers the evaporated solvent.
13. A nonwoven sheet, comprising: Nonwoven fabrics; and The nonwoven fabric is impregnated and solidified with an impregnated material containing at least one material selected from glucomannan, a cellulose-based material, gelatin, and agar.
14. The nonwoven fabric sheet according to claim 13, The nonwoven fabric sheet has a multi-layer structure in which two or more layers are laminated, and has one or more layers of the nonwoven fabric sheet.
Citation Information
Patent Citations
Method for preparing wear-resistant water-absorption-type non-woven fabric
CN108018716A
Hydrolytic clarifying article, and its manufacture
JP2000300464A
Wound covering material
JP2004248949A
Method for preparing a cosmetic pack sheet and pack sheet prepared by the same
KR1020170044435A
Die for extrusion molding and extrusion molding apparatus
JP2020146853A