Powder for powder bed melt bonding molding, method for producing the same and molded product
The composite resin powder with thermoplastic resin, carbon nanotubes, and cellulose dispersant addresses electrical charging issues in powder bed fusion bonding, ensuring high fluidity, moldability, and antistatic properties, enhancing safety and product quality.
Patent Information
- Application Number
- JP2023064686
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing resin powders for powder bed fusion bonding face issues with electrical charging, leading to potential fires or explosions, and adding carbon materials for conductivity compromises fluidity and moldability.
A composite resin powder containing thermoplastic resin, carbon nanotubes, and a cellulose-based dispersant, with controlled amounts of carbon nanotubes and dispersant, ensuring excellent fluidity, moldability, and antistatic properties.
The composite resin powder achieves high fluidity and moldability while providing effective antistatic properties, reducing the risk of electrostatic discharge and maintaining product integrity.
Smart Images

Figure 2024151413000001 
Figure 2024151413000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder for powder bed fusion shaping, a method for producing the same, and a shaped article. [Background technology]
[0002] There is a type of additive manufacturing technology known as additive manufacturing technology. One example of additive manufacturing technology is the Powder Bed Fusion (PFB) method, which uses powder materials such as resin powder and metal powder. Powder Bed Fusion can manufacture highly detailed and durable objects with high accuracy in a short time. Therefore, objects manufactured using the PFB method are expected to be used for components of equipment used in cutting-edge technology fields such as semiconductors, the aircraft industry, and medicine.
[0003] As the resin powder for powder bed fusion molding, a thermoplastic resin powder is used because it has the property of softening when heated and solidifying when cooled. However, because resin materials are generally insulators, objects made using resin powders are prone to becoming charged through contact or friction with each other or with other materials. If a charged object comes into contact with a flammable or highly inflammable liquid, static electricity will be discharged, which may ignite the liquid and cause a fire or explosion.
[0004] As a technique for preventing electrostatic buildup in resin materials, a technique for imparting electrical conductivity by compounding a carbon material such as carbon black with a resin material is known. When compounding a carbon material with a resin material for the purpose of imparting electrical conductivity, a large amount of carbon material is generally added, for example, carbon black is added in an amount of about 40 to 50 mass% relative to the resin. However, carbon materials are generally harder than resin materials, and increasing the amount of carbon added causes the resin powder to lose its inherent fluidity. In addition, the presence of a large amount of carbon material between resin particles impairs the adhesion between the resin particles, reducing the moldability and the inherent flexibility of the resin.
[0005] Patent Document 1 proposes a conductive polyamide resin composition containing a polyamide resin and, as a conductive material, 5 to 9 mass % of carbon black and 1 to 5 mass % of carbon middle fiber. However, Patent Document 1 does not disclose the use of the conductive polyamide resin composition in powder bed fusion molding. In addition, the conductive polyamide resin composition described in Patent Document 1 must contain 6% by mass or more of carbon black and carbon fiber, which are carbon materials, in total in order to impart conductivity. Therefore, the powder of the conductive polyamide resin composition is considered to be inferior in flowability, moldability, and flexibility compared to the powder of polyamide resin. Since the powder for powder bed fusion molding is required to have high flowability and fluidity, it is considered that the powder of the conductive polyamide resin composition described in Patent Document 1 is not suitable for powder bed fusion molding.
[0006] Patent Document 2 proposes a powder material for powder bed fusion molding, which has a resin powder for molding that has a first polarity due to friction and a charged powder that has been charged in advance to a second polarity opposite to the first polarity. Patent Document 2 claims that the charged powder can suppress static electricity generated in the powder material, thereby preventing defects in the production of the molded object. Charged silica powder is used as the charged powder. However, suppressing the static electricity of the molded object is not considered in Patent Document 2. Also, although there is a description that when carbon black is added as an antistatic agent to a resin powder to form a powder material, static electricity generated in the resin powder can be removed via the carbon black, the obtained molded object does not necessarily have sufficient conductivity to suppress static electricity when carbon black is simply added to the resin powder. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2019-52201 A [Patent Document 2] JP 2019-130854 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and has as its objective the provision of a powder for powder bed fusion manufacturing which has excellent fluidity, shapeability, and antistatic properties for the resulting molded objects, a method for manufacturing the same, and objects made using the powder for powder bed fusion manufacturing. [Means for solving the problem]
[0009] The present invention has the following aspects. [1] Composite resin particles containing a thermoplastic resin, carbon nanotubes, and a cellulose-based dispersant, The carbon nanotubes have an average length of 15 μm or more, The powder for powder bed fusion manufacturing, wherein the content of the carbon nanotubes is 0.01 to 0.2% by mass relative to the mass of the thermoplastic resin. [2] The powder for powder bed fusion manufacturing according to [1], wherein the cellulose-based dispersant is ethyl cellulose. [3] A mixing step of mixing resin particles containing a thermoplastic resin, carbon nanotubes, a cellulose-based dispersant, and a dispersion medium capable of swelling the resin particles; A drying step of drying the mixture obtained in the mixing step, The carbon nanotubes have an average length of 150 to 600 μm; A method for producing a powder for powder bed fusion manufacturing, wherein the content of the carbon nanotubes is 0.01 to 0.2% by mass based on the mass of the thermoplastic resin. [4] A molded object molded by powder bed fusion molding using the powder for powder bed fusion molding described in [1] or [2] by powder bed fusion molding. [5] Volume resistivity is 10 1 ~10 12 The object according to [4], wherein the resistivity is Ω·cm. Effect of the Invention
[0010] According to the present invention, it is possible to provide a powder for powder bed fusion shaping which has excellent flowability, shaping properties, and antistatic properties of the resulting shaped object, a method for producing the same, and a shaped object made using the powder for powder bed fusion shaping. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In this specification, "carbon nanotube" is also referred to as "CNT." A numerical range expressed by "to" means that the numerical values before and after the "to" are the lower and upper limits of the numerical range.
[0012] A powder for powder bed fusion shaping according to one embodiment of the present invention (hereinafter, also simply referred to as "shaping powder") contains composite resin particles. The composite resin particles contain a thermoplastic resin, CNTs, and a cellulose-based dispersant. Each component will be described in detail later.
[0013] In the composite resin particles, the CNT content is 0.01 to 0.2% by mass, preferably 0.05 to 0.20% by mass, based on the mass of the thermoplastic resin. When the CNT content is equal to or greater than the lower limit, the flowability of the powder for molding and the antistatic properties of the molded product are excellent. When the CNT content is equal to or less than the upper limit, the moldability of the powder for molding is excellent. In addition, the risk of contamination due to CNT falling off the composite resin particles and the increase in costs due to the increased amount of CNT can be suppressed.
[0014] The content of the cellulose-based dispersant is preferably 0.01 to 0.20% by mass, more preferably 0.05 to 0.20% by mass, based on the mass of the thermoplastic resin. When the content of the cellulose-based dispersant is equal to or greater than the lower limit, the CNTs are well dispersed, improving the flowability of the shaping powder and the antistatic properties of the shaped product. When the content of the cellulose-based dispersant is equal to or less than the upper limit, sintering inhibition due to gasification of the dispersant during sintering is unlikely to occur, improving moldability.
[0015] The composite resin particles typically have at least the surface and its vicinity composed of a mixture containing a thermoplastic resin, CNTs, and a cellulose-based dispersant. The composite resin particles are preferably particles having a core containing a thermoplastic resin and a surface layer covering the core, the surface layer being a layer of the mixture. Such particles can be obtained, for example, by mixing resin particles containing a thermoplastic resin, CNTs, a cellulose-based dispersant, and a dispersion medium capable of swelling the resin particles, and drying the resulting mixture, as described below. In this method, at least a portion of the CNTs is embedded or fixed in a dispersed state on the surface of the resin particles swollen with the dispersion medium, and is stably fixed.
[0016] The thickness of the mixed layer is preferably 10 μm or less. When the thickness of the mixed layer is 10 μm or less, the amount of CNT can be reduced, and costs can be suppressed. In addition, when the thickness of the mixed layer is thin, resin particles with a small average particle size can be used as the raw material, and the average particle size of the composite resin particles can be reduced. When the average particle size of the composite resin particles is reduced, it becomes easier to obtain a molded product in which the CNTs are uniformly dispersed. The lower limit of the thickness of the mixed layer is not particularly limited, but is, for example, 1.0 μm. The thickness of the mixed layer can be adjusted by the size of the resin particles of the raw material and the mixing conditions.
[0017] The average particle size of the composite resin particles is preferably 10 to 100 μm, more preferably 20 to 60 μm. When the average particle size of the composite resin particles is equal to or greater than the lower limit, the ratio of the surface area of the composite resin particles is small, making aggregation less likely to occur and easier to handle. When the average particle size of the composite resin particles is equal to or less than the upper limit, a shaped product in which CNTs are uniformly dispersed is easily obtained. The average particle size is the median diameter (D 50 ).
[0018] <Thermoplastic resin> A thermoplastic resin is a resin that has the property of softening when heated and solidifying when cooled. However, the thermoplastic resin in the present invention is different from a cellulose-based dispersant. The thermoplastic resin may be any of those known to be used in resin powders for PBF molding. The thermoplastic resin preferably has a melting point. The melting point of the crystalline thermoplastic resin is preferably 150 to 350° C. The melting point is measured by differential scanning calorimetry (DSC).
[0019] The thermoplastic resin is preferably a crystalline thermoplastic resin, which has a melting point and a crystallization temperature and is therefore suitable for PBF molding. Examples of crystalline thermoplastic resins include polyamide (PA), polypropylene (PP), polyethylene (PE), polyacetal (POM), polyether ether ketone (PEEK), and polyether ketone ketone (PEKK). Examples of PA include polyamide 12 (PA12). These thermoplastic resins may be used alone or in combination of two or more. Among the above, PA and PEEK are preferable as thermoplastic resins, and PA is particularly preferable. PA and PEEK have excellent mechanical strength, toughness, abrasion resistance, and chemical resistance, so objects made from these resins are expected to be used in parts for semiconductor and electronic component manufacturing equipment, automobile parts, etc.
[0020] <cnt> The CNTs contained in the composite resin particles may be single-walled CNTs, multi-walled CNTs, or both. The average length of the CNTs in the composite resin particles is preferably 15 μm or more. When the average length is equal to or more than the lower limit, the antistatic properties of the molded product are excellent. The longer the average length of the CNTs in the composite resin particles, the better the antistatic properties of the molded product are, so the upper limit of the average length is not limited, but when the average length is 600 μm or less, the manufacturing cost of the CNTs can be suppressed. In order to manufacture CNTs with an average length exceeding 600 μm, various additional processes are required, which significantly increases the manufacturing cost. The average diameter of the CNTs in the composite resin particles is, for example, 5 to 20 nm.
[0021] The "average length" and "average diameter" of the CNTs in the composite resin particles are measured by observation with a transmission electron microscope (TEM). Specifically, the cross section of the composite resin particle is observed with a TEM, 10 CNTs are randomly selected from the TEM image, their lengths and diameters are measured, and the average of the lengths is calculated to be the average length, and the average of the diameters is calculated to be the average diameter.
[0022] The CNTs used in producing the composite resin particles (hereinafter also referred to as "raw CNTs") may be those produced by a known method or may be commercially available products. The average length of the raw CNTs is preferably 150 to 600 μm. If the average length of the raw CNTs is 150 μm or more, the average length of the CNTs in the obtained composite resin particles tends to be 15 μm or more. In order to produce CNTs whose average length exceeds 600 μm, various additional processes are required, which significantly increases the production cost. Raw CNTs having an average length of 150 to 600 μm can be produced, for example, by the method described in Japanese Patent No. 4512750. An example of a commercially available CNT having an average length of 150 to 600 μm is long CNT manufactured by Taiyo Nippon Sanso (EL grade: multi-walled CNT with a diameter of 5 to 20 nm and a length of 50 to 800 μm).
[0023] <Cellulose-based dispersant> Cellulose-based dispersants increase the dispersibility of CNTs, which allows them to be distributed uniformly on the surface of composite resin particles, improving the flowability of the modeling powder, modeling properties, and antistatic properties of the modeled object. Examples of the cellulose-based dispersant include various cellulose derivatives such as ethyl cellulose, hydroxyethyl cellulose, methyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, etc. These cellulose-based dispersants may be used alone or in combination of two or more.
[0024] The composite resin particles may further contain other components in addition to the thermoplastic resin, the CNTs, and the cellulose-based dispersant. Examples of other components include carbon materials other than CNTs, dispersants other than cellulose-based dispersants, and the like.
[0025] <Method of Manufacturing Composite Resin Particles> The composite resin particles can be produced by a production method including, for example, a step of mixing resin particles containing a thermoplastic resin, CNTs, a cellulose-based dispersant, and a dispersion medium capable of swelling the resin particles (mixing step), and a step of drying the mixture obtained in the mixing step (drying step). The resin particles may further include other components in addition to the thermoplastic resin, CNTs, and the cellulose-based dispersant. This method makes it possible to compound a very small amount of CNTs with resin powder, resulting in a molding powder that can impart excellent antistatic properties to the molded object without impairing the excellent fluidity and moldability that are inherent to resin powder.
[0026] The CNTs used in the mixing step, ie, the raw material CNTs, may be single-walled CNTs or multi-walled CNTs, or a combination of both. The average length of the raw material CNTs is 150 to 600 μm. When the average length is equal to or greater than the lower limit, the shaped object has excellent antistatic properties. When the average length is equal to or less than the upper limit, the production cost of the raw material CNTs can be suppressed. To produce raw material CNTs with an average length exceeding 600 μm, various additional steps are required, which significantly increases the production cost. The average diameter of the raw material CNTs is, for example, 5 to 20 nm. The "average length" and "average diameter" of the raw CNTs are measured by scanning electron microscope (SEM) observation. Specifically, the raw CNT powder is observed with an SEM, 10 raw CNTs are randomly selected from the SEM image, and their lengths and diameters are measured. The average of the lengths is calculated to obtain the average length, and the average of the diameters is calculated to obtain the average diameter.
[0027] The average particle size of the resin particles is set depending on the average particle size of the composite resin particles to be produced. The average particle size of the resin particles is preferably 10 to 100 μm, more preferably 20 to 60 μm. When the average particle size of the resin particles is within the above range, the average particle size of the obtained composite resin particles tends to be within the above-mentioned preferred range.
[0028] The dispersion medium swells the resin particles, allowing the CNTs to be fixed onto the surfaces of the resin particles. The dispersion medium may be any medium capable of swelling the resin particles, but in terms of compatibility with the resin, dispersant, and CNT, ketone-based solvents and alcohol-based solvents are preferred. Examples of ketone-based solvents include methyl ethyl ketone, acetone, diethyl ketone, methyl propyl ketone, and cyclohexanone. Examples of alcohol-based solvents include ethanol, methanol, and isopropanol. These dispersion media may be used alone or in combination of two or more.
[0029] In the mixing step, the method of mixing the resin particles, raw CNTs, cellulose-based dispersant, and dispersion medium is not particularly limited, but a method of mixing a resin particle dispersion containing resin particles and a dispersion medium with a CNT dispersion containing raw CNTs, a cellulose-based dispersant, and a dispersion medium is preferred. The dispersion medium of the resin particle dispersion and the dispersion medium of the CNT dispersion may be the same or different.
[0030] For example, the resin particle dispersion and the CNT dispersion are placed in a container and stirred with a stirring means to obtain the desired mixed liquid. As the stirring method, various known mixing and dispersion methods such as a bead mill method, an ultrasonic method, a wet atomization method, a turbulent flow stirring method, etc. can be used. Among these, the wet atomization method is more preferable. The raw CNTs may be cut during stirring, and the average length of the CNTs in the mixture may become shorter than the average length of the raw CNTs, but by using the wet atomization method, it is possible to prevent the average length from becoming shorter.
[0031] In the drying step, the mixed liquid may be dried by any method capable of removing the dispersion medium, such as air drying, heating, etc. The drying temperature is, for example, 30 to 90° C. The drying time varies depending on the drying temperature, but is, for example, 1 to 10 hours.
[0032] The powder for molding in this embodiment may consist only of the above-mentioned composite resin particles, or may be a mixture of the above-mentioned composite resin particles with other particles. The content of the composite resin particles is preferably 50% by mass or more, more preferably 80% by mass or more, and may be 100% by mass, based on the mass of the powder for shaping.
[0033] The powder for molding in this embodiment is molded into a molded object by powder bed fusion molding. In powder bed fusion molding, for example, the powder for molding is arranged in an arbitrary shape, sintered by a laser (laser sintering method) or discharge (discharge sintering method) to mold layers, and the next layer is sequentially stacked on the molded layer to obtain a three-dimensional molded object. One example of powder bed fusion molding is selective laser sintering (SLS) method. Fabrication using the powder bed fusion molding method can be carried out using a known powder bed fusion molding type 3D printer.
[0034] The volume resistivity of the molded object is 10 1 ~10 12 Ω cm is preferred, 10 1 ~10 8 Ω cm is more preferable, 10 1 ~10 4 When the volume resistivity is equal to or less than the above upper limit, the molded object has excellent antistatic properties. "Volume resistivity" is measured in accordance with the JIS standard for evaluating the electrical properties of conductive plastics (JIS K 7194 (measurement method for low volume resistivity) or JIS K 6911 (measurement method for high volume resistivity)).
[0035] <Action and effect> The molding powder described above has excellent fluidity and molding properties. In addition, the resulting molded object can be made conductive and antistatic. The range of conductivity can be adjusted by changing the amount of CNT added. 1 ~10 12 It can be controlled in the Ω·cm range.
[0036] It is believed that the fact that the CNTs to be composited are long CNTs with an average length of 15 μm or more and that the amount of CNTs is appropriate contributes to improving the fluidity and conductivity of the molding powder. When short CNTs are used, there is a risk that sufficient conductivity may not be obtained. If the CNT content is more than 0.2% by mass, the moldability may be reduced. For example, the powder particles stacked during molding may not be densely packed, and the resulting molded object may be weak and prone to cracking. Because the powder sintering additive manufacturing method does not apply pressure to the powder, unless the powder has the properties of being highly fluid and densely packed, it is not possible to create a structure with high strength and it will not be able to exhibit conductivity.
[0037] The fact that the dispersant is cellulose-based is believed to contribute to firmly compounding the CNTs and thermoplastic resin, and to improving the fluidity and electrical conductivity of the powder for granulation. Even when long CNTs are used, if the dispersant is acrylic (Comparative Example 4 described later), there is a risk that the fluidity will be impaired and electrical conductivity will not be obtained. This is thought to be because, in the case of an acrylic dispersant, the thermoplastic resin and CNTs are not firmly compounded, and the excess CNTs that are not compounded in the powder for molding aggregate and are mixed into the resin. These CNT aggregates hinder the flow of the resin, and the powders stacked during molding are not densely packed together, so the strength of the resulting molded object is weak and it is likely to break easily. In addition, since the thermoplastic resin and CNTs are not compounded, electrical conductivity will be insufficient. In addition to dispersing the CNTs, the cellulose-based dispersant also acts as a binder, adhering the CNTs to the thermoplastic resin and making them difficult to remove. This is thought to make it possible to produce shaped objects without significantly impairing the fluidity of the granulation powder, and to achieve high electrical conductivity. EXAMPLES
[0038] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these.
[0039] [Materials used] Resin powder: Polyamide (nylon) powder for powder sintering additive manufacturing manufactured by Microtec (average particle size (D 50 )60μm, gray, melting point 180℃). CNT-1: Long carbon nanotubes (DL grade) manufactured by Taiyo Nippon Sanso (multi-walled carbon nanotubes with a diameter of 5 to 20 nm and a length of 50 to 800 μm). CNT-2: Long carbon nanotubes (DL grade) manufactured by Taiyo Nippon Sanso (multi-walled carbon nanotubes with a diameter of 5 to 20 nm and a length of 50 to 150 μm). CNT-3: Carbon nanotubes made of Nanocyl (average diameter 9.5 nm, average length 1.5 μm). MEK: Methyl ethyl ketone (99.5% purity). Ethyl cellulose: Manufactured by Fujifilm Wako Pure Chemical Industries. Acrylic resin: Made by BYK.
[0040] [Example 1] A composite resin powder (powder for molding) was produced by the following procedure. First, a resin powder dispersion was obtained by mixing resin powder and MEK at a mass ratio of resin powder:MEK = 1:5. Also, CNT-1, MEK, and ethyl cellulose (dispersant) were mixed to obtain a CNT dispersion with a CNT concentration of 0.2 mass% and an ethyl cellulose concentration of 0.2 mass%. Next, the resin powder dispersion and the CNT dispersion were poured into the beaker. The amount of the CNT dispersion was set so that the ratio (addition amount) of CNT to the mass of the resin powder in the resin powder dispersion was 0.05 mass%. The resulting mixture was stirred for 60 minutes at room temperature using a magnetic stirrer. The dispersed CNT adhered to the resin particle surfaces during the stirring process, and when the stirring was finally stopped, the supernatant of the mixture became transparent and the resin powder coagulated and precipitated. Next, the supernatant of the mixture was separated and collected using a dropper, and the remaining mixture was transferred to a stainless steel tray and dried overnight (12 hours) in a vacuum dryer (Yamato Scientific) to obtain the desired composite resin powder. When the cross section of the obtained composite resin powder was observed with a transmission electron microscope (TEM), it was found that a CNT mixed layer with a thickness of 10 μm or less was formed on the surface of the resin particles, in which the CNTs were embedded in a dispersed state.
[0041] <Evaluation> The obtained powder for molding was evaluated as follows, and the results are shown in Table 1.
[0042] (1) Average length of raw CNTs The CNT powder before obtaining the CNT dispersion was observed by scanning electron microscopy (SEM), and 10 CNTs were randomly selected from the SEM image, their lengths were measured, and the average was calculated.
[0043] (2) Average length of CNTs attached to composite resin powder The cross section of the composite resin powder was observed with a transmission electron microscope (TEM), and 10 CNTs were randomly selected from the TEM image, their lengths were measured, and the average was calculated.
[0044] (3) Flow rate The flow rate (FR) of the powder for molding was measured using the POWDERFLOW powder flow measurement kit from LPW Technology. PA / CNT The amount of powder used for the flow rate evaluation was 20.0 g ± 0.1 g. The measurement was performed three times, and the average value was used as the evaluation result.
[0045] (4)Angle of repose The angle of repose of the molding powder was evaluated using the POWDERFLOW powder flow measurement kit from LPW Technology. The amount of powder used to evaluate the angle of repose was 20.0g ± 0.1g. The evaluation was performed three times, and the average value was used as the evaluation result.
[0046] (5) Bulk density The bulk density (D) of the powder for molding was measured using the POWDERFLOW powder flow measurement kit from LPW Technology. PA / CNT The bulk density was evaluated using an evaluation device with a volume of 20 mL. The evaluation was performed three times, and the average value was used as the evaluation result.
[0047] (6) Tap density The tap density (DT) of the powder for molding was measured using the POWDERFLOW powder flow measurement kit from LPW Technology. PA / CNT The tap density was evaluated using an evaluation device with a volume of 20 mL. The evaluation was performed three times, and the average value was used as the evaluation result.
[0048] (7) Formability The powder for modeling was modeled using a 3D printer (Sintratec's "Sintratec Kit") that uses an SLS method, which is a powder bed fusion modeling method using a laser. The model to be produced was a plate-shaped object measuring 30 mm x 30 mm x 5 mm thick. The printing speed was laser speed: 70 mm / sec, the temperature inside the printer: 150°C, and the laser used was a diode laser (output: 2300 mW, laser wavelength: 445 nm). The moldability and surface shape of the molded product were evaluated. Specifically, if the molded product could be molded into a plate shape, it was deemed moldable, and if the molded product was not plate-shaped or the lamination was loose and peeled off in layers, it was deemed unprintable. Specifically, the surface shape of the molded product was observed visually, and if there were 5 or more protrusions or dents of 1 mm or more on the front or back of the plate-shaped molded product, it was deemed x, if there were 1 to 4 protrusions or dents, it was deemed △, and if there were 0 protrusions or dents, it was deemed ◯.
[0049] (8) Electrical conductivity The volume resistivity of the molded objects (shape: 30mm x 30mm x thickness 5mm) created in the above moldability evaluation was measured in accordance with the JIS standard evaluation method for the electrical properties of conductive plastics (JIS K 7194 (measurement method for low volume resistivity) or JIS K 6911 (measurement method for high volume resistivity)). The measuring device used was a resistivity meter (Mitsubishi Chemical Analytech's "Loresta GP" and "Hi-Resta UX"). The thickness used to calculate the volume resistivity was measured with a digital caliper.
[0050] [Examples 2 and 3] The powders for molding were produced and evaluated in the same manner as in Example 1, except that the amount of CNT added relative to the mass of the resin powder was 0.01% by mass and 0.2% by mass, respectively. The evaluation results are shown in Table 1.
[0051] [Example 4] Except for using CNT-2 instead of CNT-1, the powder for molding was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.
[0052] [Comparative Example 1] The raw resin powder was used as it was as the powder for molding, and the same evaluation was carried out as in Example 1. The evaluation results are shown in Table 2.
[0053] [Comparative Example 2] Except for using CNT-3 instead of CNT-1, the powder for molding was produced and evaluated in the same manner as in Example 3. The evaluation results are shown in Table 2.
[0054] [Comparative Example 3] Except for changing the amount of CNT added to the resin powder to 0.25% by mass, the powder for molding was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 2.
[0055] [Comparative Example 4] Except for changing the amount of CNT added to the resin powder to 0.005% by mass, the powder for molding was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 2.
[0056] [Comparative Example 5] Except for using an acrylic resin instead of ethyl cellulose as a dispersant, the powder for molding was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 2.
[0057] [Table 1]
[0058] [Table 2]
[0059] The molding powders of Examples 1 to 4 had fluidity equal to or greater than that of the raw resin powder (Comparative Example 1). In addition, molded objects could be produced by powder bed fusion molding, and the obtained molded objects exhibited excellent electrical conductivity. Furthermore, a comparison of Examples 1 to 4 showed that by adjusting the amount of long CNTs added, it was possible to increase the volume resistivity of the molded object by 10 1 ~10 12 It was also confirmed that the resistance could be controlled within the range of Ω·cm. In Comparative Example 2, in which the average length of the CNTs attached to the composite resin particles was 0.1 μm, the CNT addition amount was 0.2 mass%, which was equivalent to that of Example 3, but the volume resistivity was equivalent to that of Comparative Example 1 and the conductivity was poor. Comparative Example 3, in which the amount of CNT added was 0.25% by mass, was inferior in moldability. In addition, the volume resistivity of the molded object was the same as in Example 3, and no effect commensurate with the amount added was obtained. In Comparative Example 4, in which the CNT addition amount was 0.005 mass %, the volume resistivity of the shaped article was equivalent to that of Comparative Example 1, and the electrical conductivity was poor. Comparative Example 5, which used an acrylic dispersant, was inferior in fluidity and moldability compared to the raw resin powder. In addition, the volume resistivity of the molded object was the same as that of Comparative Example 1, and the electrical conductivity was inferior. [Industrial Applicability]
[0060] The powder for molding of the present invention is excellent in flowability, moldability, and antistatic properties of the resulting molded objects. The shaped object of the present invention has excellent antistatic properties, and therefore can reduce the risk of static electricity generation. Therefore, the shaped object of the present invention can eliminate the risk of electrostatic breakdown, which is a concern in parts of equipment in the semiconductor / electronic parts industry, chemicals industry, semiconductor industry, and other industries. In addition, since the carbon nanotube content is low, there is a low risk of carbon nanotubes falling off due to contact with liquid or wear, and the cleanliness is excellent. Therefore, the shaped object of the present invention is useful for various applications. For example, it is useful for components of fluid control devices, films, sheets, joints, tables, tubes, rods, rollers, bearings, etc.< / cnt>
Claims
1. Composite resin particles including a thermoplastic resin, carbon nanotubes, and a cellulose-based dispersant, The average length of the carbon nanotubes is 15 μm or more, The powder for powder bed fusion shaping, wherein the carbon nanotube content is 0.01 to 0.2% by mass relative to the mass of the thermoplastic resin.
2. 2. The powder for powder bed fusion manufacturing of claim 1, wherein the cellulosic dispersant is ethyl cellulose.
3. A mixing step of mixing resin particles including a thermoplastic resin, carbon nanotubes, a cellulose-based dispersant, and a dispersion medium capable of swelling the resin particles; A drying step of drying the mixture obtained in the mixing step, The carbon nanotubes have an average length of 150 to 600 μm; A method for producing a powder for powder bed fusion shaping, wherein the carbon nanotubes are present in an amount of 0.01 to 0.2% by mass relative to the mass of the thermoplastic resin.
4. 3. A shaped object produced by powder bed fusion shaping using the powder for powder bed fusion shaping according to claim 1 or 2 by powder bed fusion shaping.
5. Volume resistivity is 10 1 ~10 12 The shaped object according to claim 4, wherein the resistivity is Ω·cm.
Citation Information
Patent Citations
Electroconductive polyamide resin composition and molded product using the same
JP2019052201A
Powder material for powder bed fusion bonded molding and forming method thereof, and powder bed fusion bonded molding