Rapidcreekite production method and precipitate

By synthesizing rapidocreekite through mixing calcium carbonate with dilute sulfuric acid and optimizing conditions, the method addresses the lack of artificial synthesis, enabling improved fire resistance and strength in gypsum-based materials.

JP2024151414APending Publication Date: 2024-10-25NIHON UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023064688
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

There is a lack of artificial synthesis methods for rapidocreekite, a double-salt compound that could potentially enhance fire resistance and strength in gypsum-based materials, limiting its application in infrastructure and reinforcing materials.

Method used

A method involving the mixing of calcium carbonate with dilute sulfuric acid, allowing the mixture to stand, and separating the precipitate to synthesize rapidocreekite, optimizing the molar ratio and conditions for high purity.

Benefits of technology

The method enables the production of rapidocreekite, a double-salt compound with improved properties, suitable for replacing dihydrate gypsum in infrastructure materials and reinforcing calcium carbonate applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151414000001
    Figure 2024151414000001
  • Figure 2024151414000002
    Figure 2024151414000002
  • Figure 2024151414000003
    Figure 2024151414000003
Patent Text Reader

Abstract

To provide a novel rapidcreekite production method and a precipitate obtained by the production method.SOLUTION: A rapidcreekite production method includes: a mixing step of mixing calcium carbonate into dilute sulfuric acid to obtain a liquid mixture; and an isolating step of producing a precipitate from the liquid mixture by precipitation and isolating the precipitate. The isolating step preferably includes allowing the liquid mixture to stand. The liquid mixture is preferably a transparent solution. The mixing molar ratio of the calcium carbonate and sulfuric acid in the dilute sulfuric acid is preferably 0.96:1.00 to 1.04:1.00.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing rapidokrikite and a precipitate obtained by the method. [Background technology]

[0002] Rapidcreekite (Ca2(SO4)(CO3)·4H2O), a double salt compound of gypsum, is rarely found in nature (Non-patent Documents 1-4). The currently used gypsum board (ceiling, wall material) is a monosalt structure material made of gypsum dihydrate. On the other hand, the crystal structure (atomic arrangement) of rapidokrit is roughly Ca in the dihydrate structure. 2+ Ionic radicals and SO4 2- Among the structures in which ionic groups are arranged alternately, SO4 2- Ionic groups in every other layer CO3 2- The structure is exchanged with an ionic group. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] ANDREW C. ROBERTS, H. GARY ANSELL and IAN R. JONASSON, Canadian Mineralogist, 24 (1986) 51-54. [Non-Patent Document 2] Bogdan P. Onac, Herta s. Effenberger, Jonathan G. Wynn, and Ioan Povara, Rapidcreekite in the sulfuric acid weathering environment of Diana Cave, Romania, American Mineralogist, 98 (2013) 1302-1309. [Non-Patent Document 3] Margarita S. AVDONTCEVA, Andrey A. ZOLOTAREV, Sergey V. KRIVOVICHEV, Maria G. KRZHIZHANOVSKAYA, Vladimir N. BOCHAROV, Vladimir V. SHILOVSKIKH, Rapidcreekite of anthropogenic origin - 'korkinoite' from burnt mine dump in the Chelyabinsk basin, South Urals, Russia: CRYSTAL structure refinement, Thermal behavior and spectroscopic characterization, Journal of Geosciences, 66 (2021), 147-156. [Non-Patent Document 4] Yasue, Nin, "Materials design of calcium-based materials," Journal of the Society of Inorganic Materials, Japan, 13 (2006) 309-320. Summary of the Invention [Problem to be solved by the invention]

[0004] If the single-salt structural material gypsum dihydrate could be replaced with rapidokurkite, a double-salt compound that is expected to exhibit high physical and chemical properties, it is believed that rapidokurkite boards with even better fire resistance, strength resistance, and long life could be developed. However, there are no reports of the artificial synthesis of rapidokrit.

[0005] An object of the present invention is to provide a novel method for producing rapidokkurikite and a precipitate obtained by the method. [Means for solving the problem]

[0006] The inventors discovered that when calcium carbonate was mixed with dilute sulfuric acid and then allowed to stand, a precipitate soon formed. When the precipitate was subjected to X-ray crystallography, the main peak matched the main peak obtained by X-ray diffraction (XRD) pattern simulation of rapidokkurikite, and thus it was possible to synthesize rapidokkurikite, which led to the completion of the present invention.

[0007] In order to solve the above problems, the present invention employs the following configuration. [1] A mixing step of mixing calcium carbonate with dilute sulfuric acid to obtain a mixed liquid; A method for producing rapidokrit, comprising: a step of precipitating a precipitate from the mixed liquid and separating the precipitate. [2] The method for producing rapidokkurikite described in [1], wherein the separation step includes allowing the mixture to stand. [3] The method for producing rapidokkurikite according to [1] or [2], wherein the mixture is a transparent solution. [4] The method for producing rapidokkrite according to any one of [1] to [3], wherein a mixing molar ratio of the calcium carbonate to the sulfuric acid in the dilute sulfuric acid is 0.96:1.00 to 1.04:1.00. [5] A precipitate obtained by the method for producing rapidokrikite according to any one of [1] to [4]. Effect of the Invention

[0008] According to the present invention, there is provided a novel method for producing rapidokkurikite and a precipitate obtained by said method. [Brief description of the drawings]

[0009] [Figure 1] 1 shows the results of X-ray diffraction (XRD) measurement of the precipitates obtained in Examples 1 and 2. [Diagram 2] 1 shows the results of X-ray diffraction (XRD) measurement of calcium carbonate powder used in the examples. [Diagram 3] This is the result of X-ray diffraction (XRD) measurement of calcium sulfate powder. [Figure 4]1 shows a thermogravimetric curve and a differential heat curve of the precipitate obtained in Example 1. [Diagram 5] 1 is a field emission scanning electron microscope (FE-SEM) image of the precipitate obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Manufacturing method of Rapidokurikite> A method for producing rapidokrit according to one embodiment of the present invention includes a mixing step of mixing calcium carbonate with dilute sulfuric acid to obtain a mixed liquid, and a separation step of precipitating a precipitate from the mixed liquid and separating the precipitate.

[0011] (Mixing process) In the mixing step, calcium carbonate is mixed with dilute sulfuric acid to obtain a mixed liquid. The calcium carbonate used as a raw material is preferably in powder form. It may be, but is not limited to, aragonite (CaCO3) with a crystal structure similar to rapidocrackite. It may be calcite (CaCO3) or vaterite (CaCO3). Waste shells (calcite, aragonite) may also be used.

[0012] The sulfuric acid concentration of the dilute sulfuric acid may be 0.010 to 0.200 mol / L, may be 0.015 to 0.150 mol / L, or may be 0.020 to 0.100 mol / L.

[0013] The mixing molar ratio of the calcium carbonate to the sulfuric acid in the dilute sulfuric acid is preferably 0.96:1.00 to 1.04:1.00, more preferably 0.98:1.00 to 1.02:1.00, and further preferably 0.99:1.00 to 1.01:1.00. The mixing molar ratio is the ratio of CO3 2- ions and SO4 in the dilute sulfuric acid 2- It is also the molar ratio with ions. By adjusting the mixing molar ratio to be close to 1.00:1.00, the purity of rapidokrit in the precipitate can be increased.

[0014] The mixture obtained by mixing calcium carbonate with dilute sulfuric acid is preferably a transparent solution. The transparent solution can be obtained by adjusting the mixing molar ratio to the above range and stirring well. The transparent solution contains substantially Ca 2+ Ions, CO3 2- Ion, SO4 2- Only ions and H2O are present. This makes it easy to precipitate rapidokkrite (Ca2(SO4)(CO3)·4H2O), and the purity of rapidokkrite in the precipitate can be increased.

[0015] The temperature condition in the mixing step is preferably 10 to 80° C., more preferably 15 to 60° C., and even more preferably room temperature in the range of 20 to 40° C. Here, room temperature refers to a temperature that is neither cooled nor heated.

[0016] (Preparative separation process) The separating step comprises separating a precipitate from the mixture and separating the precipitate.

[0017] The separation step preferably includes leaving the mixture standing still. Here, leaving the mixture standing still means placing the container of the mixture in a stationary state without stirring the mixture. By leaving the mixture standing still, the yield of the precipitate can be increased. The time for leaving the mixture to stand may be 0.2 to 20 minutes, 0.3 to 10 minutes, 0.5 to 5 minutes, or 0.8 to 3 minutes. By adjusting the mixture molar ratio to be within the above range and stirring well, the yield of the precipitate can be increased even if the time for leaving the mixture to stand is shortened.

[0018] The precipitate is filtered, and if necessary, washed and dried to obtain a powder containing rapidcreekite (Ca2(SO4)(CO3)·4H2O), which is a double salt compound.

[0019] Drying may be performed at atmospheric pressure or under reduced pressure. The temperature condition for drying may be 20 to 80°C, 20 to 60°C, or 20 to 40°C.

[0020] <Precipitate> The precipitate according to one embodiment of the present invention is obtained by the rapidokkrite manufacturing method according to the above embodiment. The precipitate according to this embodiment may be put to practical use as an infrastructure material to replace gypsum dihydrate, a simple salt structural material. It may also be put to practical use in the same role as calcium carbonate, which is used as a reinforcing material when mixed. EXAMPLES

[0021] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0022] [Example 1] <Artificial synthesis of rapidocrispykite> 0.500g of calcium carbonate powder (CaCO3, 0.0050mol, Fujifilm Wako Pure Chemical Industries, Ltd.) was mixed with 100mL of dilute sulfuric acid (0.05mol / L, 0.0050mol) and stirred at room temperature for about 1 minute, whereby all of the calcium carbonate dissolved to obtain a transparent solution. The molar ratio of calcium carbonate to sulfuric acid in the dilute sulfuric acid was 1.00:1.00. After standing at room temperature for about 1 minute, a crystalline precipitate formed on the surface of the solution. The precipitate was filtered and further dried at atmospheric pressure at 40°C for 12 hours. The mass of the precipitate was about 1.82g (yield: about 90%).

[0023] X-ray diffraction (XRD) The dried precipitate was filled into a holder for a measurement sample and set in a wide-angle X-ray diffraction (XRD) device (Miniflex II, manufactured by Rigaku Corporation) and measurements were performed under the following conditions: Cu / Kα radiation, 30 kV / 15 mA, scan speed: 2θ=8° / min, scan range: 2θ=5° to 60°. The measurement results are shown in Figure 1.

[0024] FIG. 2 shows the results of X-ray diffraction (XRD) measurement of the calcium carbonate powder used in the examples. FIG. 3 shows the results of X-ray diffraction (XRD) measurement of calcium sulfate powder.

[0025] In the X-ray diffraction (XRD) pattern of the precipitate obtained in Example 1 shown in Figure 1, small peaks of impurities of calcite (▲, CaCO3), aragonite (★, CaCO3), and vaterite (●, CaCO3) are observed, but all four main peaks (2θ = 11.1°, 20.2°, 22.9°, 28.6°) matched the main peaks obtained by the X-ray diffraction (XRD) pattern simulation of rapidokrikite (ICSD♯425547). The X-ray diffraction (XRD) pattern of the precipitate obtained in Example 1 was different from that of calcium carbonate monosalt and calcium sulfate monosalt and mixture, and it was confirmed that rapidokrikite was synthesized.

[0026] Thermogravimetry - Differential Thermal Analysis The precipitate after drying was subjected to thermal analysis using a thermal analyzer (a TG / DTA simultaneous measurement device DTG-60 manufactured by Shimadzu Corporation) to measure the temperature from 20°C to 1000°C at a heating rate of 10°C / min in air using a reference sample of alumina particles of approximately the same amount as the measurement sample, and the thermogravimetric curve and differential heat curve were obtained. The results are shown in Figure 4.

[0027] Electron microscope observation The precipitate after drying was photographed using a field emission scanning electron microscope (FE-SEM). The FE-SEM image is shown in Figure 5. Plate-like crystals similar in shape to gypsum dihydrate were observed, with average particle sizes of approximately 30-100 μm and aspect ratios of approximately 1:3.

[0028] ·Elemental analysis by energy dispersive X-ray spectroscopy (EDS) The precipitate after drying was subjected to energy dispersive X-ray spectroscopy (EDS) analysis. The four elements that make up rapidocrete (Ca2(SO4)(CO3)·4H2O), Ca, C, O, and S, were uniformly detected.

[0029] [Example 2] <Artificial synthesis of rapidocrispykite> As in Example 1, 0.500 g of calcium carbonate powder (CaCO3, 0.0050 mol) was mixed with 100 mL of dilute sulfuric acid (0.05 mol / L, 0.0050 mol) and stirred at room temperature for about 1 minute to obtain a transparent solution. The molar ratio of calcium carbonate to sulfuric acid in the dilute sulfuric acid was 1.00:1.00. After standing at room temperature for about 1 minute, a precipitate was formed. The precipitate was filtered and further vacuum-dried at 51°C for 12 hours (gauge pressure: -90 kPa). The results of X-ray diffraction (XRD) measurement of the precipitate after vacuum drying at 51° C. are shown in FIG. All of the main peaks matched those obtained by the X-ray diffraction (XRD) pattern simulation (ICSD♯425547) of rapidokrikite, and it was confirmed that rapidokrikite had been synthesized. However, the diffraction peak intensity obtained was small, indicating low crystallinity. The 20-30° bulge is thought to be the result of the background peaks of the quartz cell remaining due to the low crystallinity of rapidokrikite.

[0030] [Comparative Example 1] 0.525g of calcium carbonate powder (CaCO3, 0.00525mol) was mixed with 100mL of dilute sulfuric acid (0.05mol / L, 0.0050mol) and stirred at room temperature for about 1 minute to obtain a transparent solution. The molar ratio of calcium carbonate to sulfuric acid in the dilute sulfuric acid was 1.05:1.00. When left to stand at room temperature, no precipitate was formed.

[0031] From the above results, it was confirmed that rapidokrit can be synthesized by going through the steps of mixing calcium carbonate with dilute sulfuric acid to obtain a mixed liquid, leaving the mixed liquid to stand, and separating the precipitate. [Industrial Applicability]

[0032] The rapidokkurikite manufacturing method of the present invention allows for easy and artificial synthesis of large amounts of rapidokkurikite. This allows for the possibility of practical application as an infrastructure material to replace the monosalt structural material gypsum dihydrate. In addition, there is a possibility that rapidokkurikite can be used in the same role as calcium carbonate, which is currently used as a reinforcing material when mixed with other materials.

Claims

1. A mixing step of mixing calcium carbonate with dilute sulfuric acid to obtain a mixed liquid; A method for producing rapidokrit, comprising: a step of precipitating a precipitate from the mixed liquid and separating the precipitate.

2. The method for producing rapidokrit as described in claim 1, wherein the separating step includes allowing the mixed liquid to stand.

3. The method for producing rapidokkurikite according to claim 1 or 2, wherein the mixture is a transparent solution.

4. The method for producing rapidokkurikite according to claim 1 or 2, wherein the mixing molar ratio of the calcium carbonate to the sulfuric acid in the dilute sulfuric acid is 0.96:1.00 to 1.04:1.

00.

5. A precipitate obtained by the method for producing rapidokkurikite according to claim 1 or 2.