Separation film and method for manufacturing the same

A separation membrane with an isocyanuric acid skeleton and siloxane bond, combined with metal ions, addresses the limitations of existing membranes by enhancing CO2 permeability and selectivity, enabling effective CO2 separation and storage.

JP2024151464APending Publication Date: 2024-10-25HIROSHIMA UNIVERSITY +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023064810
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing separation membranes face challenges in achieving high carbon dioxide permeability and gas selectivity, particularly for large molecules like CO2, due to small pore sizes and non-uniform pore formation, which limits their effectiveness in carbon dioxide collection and storage processes.

Method used

A separation membrane comprising a polymer with an isocyanuric acid skeleton and siloxane bond, combined with metal ions, forms an amorphous structure that enhances CO2 permeability and selectivity through a network of coordinated bonds and siloxane networks, allowing for efficient CO2/N2 separation.

Benefits of technology

The membrane exhibits excellent carbon dioxide permeability and selectivity, facilitating efficient separation, recovery, and storage of CO2 from mixed gases and solvents, with improved mechanical strength and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151464000012
    Figure 2024151464000012
  • Figure 2024151464000013
    Figure 2024151464000013
  • Figure 2024151464000014
    Figure 2024151464000014
Patent Text Reader

Abstract

To provide a separation film that can achieve high carbon dioxide permeability and high gas selectivity.SOLUTION: A separation film comprises a separation layer which includes a polymer (A) having an isocyanuric acid skeleton and a siloxane bond and a metal ion (B) and has an amorphous structure. It is preferable that the polymer (A) is a polymer made by polymerizing a precursor including tris [3-(trimethoxysilyl)propyl] isocyanurate, and it is preferable that metal in the metal ion (B) is one or more metal selected from nickel, copper, silver, cobalt and zinc.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separation membrane and a method for producing the same. [Background technology]

[0002] The separation method using a porous separation membrane is inexpensive and has a high separation ability compared to separation methods such as filtration, evaporation, crystallization, solvent extraction, distillation, etc. The porous separation membrane separates the target substance by molecular sieving.

[0003] Silicon-based materials have excellent mechanical strength, heat resistance, and chemical stability, and are used as materials for porous inorganic separation membranes. However, when silicon-based materials are used as materials for separation membranes, pores become denser under high-temperature steam, and the permeability of the separation membrane decreases. In order to reduce this densification, a separation membrane has been developed that includes a separation layer in which metal ions are doped into the silicon-based material (Patent Document 1).

[0004] In addition, with regard to carbon dioxide (CO2) capture and storage technologies using silicon-based materials, separation membranes having a separation layer using a polymer obtained by polymerizing a precursor containing a compound having a urea group and an alkoxysilyl group, and separation membranes having a separation layer using a polymer obtained by polymerizing a precursor containing a compound having an amino group and an alkoxysilyl group are known (Patent Documents 2 and 3). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-151708 A [Patent Document 2] JP 2021-186712 A [Patent Document 3] Patent Publication No. 2022-21175 Summary of the Invention [Problem to be solved by the invention]

[0006] In Patent Document 1, pores are formed in the separation layer by doping with metal ions. However, the size of the formed pores is small, and the permeability of carbon dioxide, which is a relatively large molecule, is low. Furthermore, it is difficult to form uniform pores in the separation layer and improve gas selectivity. Furthermore, as in Patent Documents 2 and 3, with conventional separation membranes using organosilicon compounds having amino groups or urea groups, it has been difficult to achieve sufficient carbon dioxide permeability and CO2 / N2 selectivity.

[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a separation membrane that can achieve high carbon dioxide permeability and gas selectivity. [Means for solving the problem]

[0008] As a result of extensive research to achieve the above-mentioned object, the inventors discovered that a separation membrane having a separation layer containing a polymer having an isocyanuric acid skeleton and a siloxane bond and a metal ion exhibits high carbon dioxide permeability and CO2 / N2 selectivity, and thus completed the present invention.

[0009] That is, the present invention provides 1. A separation membrane comprising (A) a polymer having an isocyanuric acid skeleton and a siloxane bond and (B) a metal ion, and having a separation layer having an amorphous structure; 2. The separation membrane according to 1, wherein the component (A) is a polymer obtained by polymerizing a precursor containing a compound represented by the following general formula (1): [ka] (In the formula, each X is independently a group represented by the following formula (2) or a monovalent hydrocarbon group having 1 to 8 carbon atoms, and at least one of X is a group represented by the following formula (2).) [ka] (In the formula, R 1 is an alkylene group having 1 to 8 carbon atoms, R 2are each independently a monovalent hydrocarbon group having 1 to 8 carbon atoms; R 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 1 to 3. A wavy line represents a bond. 3. The separation membrane according to 2, wherein the component (A) is a polymer obtained by polymerizing a precursor containing tris[3-(trimethoxysilyl)propyl]isocyanurate. 4. The separation membrane according to any one of 1 to 3, wherein the metal in the component (B) is one or more selected from nickel, copper, silver, cobalt, and zinc. 5. (I) a metal-doped polymer sol preparation step of preparing a metal-doped polymer sol containing (A) a polymer having an isocyanuric acid skeleton and a siloxane bond and (B) a metal ion; (II) a coating step of coating the metal-doped polymer sol directly or via an intermediate layer onto a porous support; (III) a firing step of firing the metal-doped polymer sol applied in the coating step to form a separation layer having an amorphous structure; A method for producing a separation membrane comprising the steps of: 6. The method for producing a separation membrane according to 5, wherein the metal-doped polymer sol preparation step is carried out by mixing the (A) polymer sol with the (B) metal salt serving as a source of metal ions. 7. The method for producing a separation membrane according to 5, wherein the component (A) is a polymer obtained by polymerizing a precursor containing a compound represented by the following general formula (1): [ka] (In the formula, each X is independently a group represented by the following formula (2) or a monovalent hydrocarbon group having 1 to 8 carbon atoms, and at least one of X is a group represented by the following formula (2).) [ka] (In the formula, R 1 is an alkylene group having 1 to 8 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 8 carbon atoms; R 3is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 1 to 3. 8. The method for producing a separation membrane according to 7, wherein the component (A) is a polymer obtained by polymerizing a precursor containing tris[3-(trimethoxysilyl)propyl]isocyanurate. 9. The method for producing a separation membrane according to any one of 5 to 8, wherein the metal in the component (B) is at least one selected from nickel, copper, silver, cobalt, and zinc. to provide. Effect of the Invention

[0010] INDUSTRIAL APPLICABILITY The separation membrane of the present invention has excellent carbon dioxide permeability and gas selectivity, and is therefore useful in processes for separating, capturing and storing carbon dioxide from mixed gases and mixed organic solvents. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a separation membrane according to the present invention. [Diagram 2] FIG. 1 shows the characteristics of nickel-doped TTPI and TTPI, where (a) is the measurement result of ultraviolet-visible spectroscopy, (b) is the measurement result of Fourier transform infrared spectroscopy (wave number 500 to 2000 cm-1), and (c) and (d) are the measurement results of X-ray photoelectron spectroscopy. [Diagram 3] FIG. 1 shows the characteristics of nickel-doped TTPI powder and TTPI powder, where (a) is the result of X-ray diffraction measurement of the powder sintered at 250° C., and (b) is an image taken by a transmission electron microscope. [Figure 4] 13 shows N2 adsorption and desorption isotherms of nickel-doped TTPI powder and TTPI powder. [Diagram 5] FIG. 1 is a schematic diagram showing the mechanism of Ni-TTPI network formation at Ni / N molar ratios of 0, 0.25, and 0.50. [Figure 6] 1 is a graph showing CO2 adsorption / desorption isotherms of nickel-doped TTPI powder and TTPI powder. [Figure 7]FIG. 2 is a graph showing the relationship between gas molecule size and gas permeability, illustrating the permeability of a separation membrane. [Figure 8] FIG. 1 shows the permeability of the separation membrane, where (a) is a graph showing the temperature dependence of the CO2, N2 permeability and the CO2 / N2 permeability ratio of the separation membrane obtained in Comparative Example 1, (b) is a graph showing the temperature dependence of the CO2, N2 permeability and the CO2 / N2 permeability ratio of the separation membrane obtained in Example 1, (c) is a graph showing the temperature dependence of the CO2, N2 permeability and the CO2 / N2 permeability ratio of the separation membrane obtained in Example 2, and (d) is a graph showing the temperature dependence of the CO2, N2 permeability and the CO2 / N2 permeability ratio of the separation membrane obtained in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be specifically described below. (1) Separation membrane The separation membrane of the present invention includes (A) a polymer having an isocyanuric acid skeleton and a siloxane bond, and (B) a metal ion, and has a separation layer having an amorphous structure. In the present invention, the amorphous structure refers to a state in which a network structure in which the polymer is bound in a mesh shape by siloxane bonds and a network structure in which nitrogen atoms in the isocyanuric acid skeleton are coordinately bonded to metal ions are formed, as described below, resulting in the formation of a large number of pores consisting of gaps in the network in the separation layer.

[0013] The structure of the separation membrane of the present invention is not particularly limited as long as it has the above-mentioned separation layer, but an example thereof is shown in Fig. 1. Fig. 1 is a schematic cross-sectional view of a separation membrane 10 according to one embodiment of the present invention, and separation membrane 10 is configured to include a support 11, an intermediate layer 12 formed on this support 11, and a separation layer 13 formed on this intermediate layer 12.

[0014] (Support) The separation membrane 10 preferably includes a support 11 in order to increase the mechanical strength and shape stability of the separation membrane 10. The support 11 preferably has both a support function for the separation layer 13 and liquid permeability. A specific example of such a support is a porous support. The material of the support is not particularly limited, but examples thereof include ceramics such as α-alumina (Al2O3), silica (SiO2), and zirconia (ZrO2). The shape of the support is not particularly limited, and examples thereof include a tubular, cylindrical, and plate-like shape.

[0015] The average pore size of the porous support is not particularly limited, but is preferably 1 μm or less, more preferably 100 nm or less. The average pore size of the porous support is preferably 0.1 nm or more, more preferably more than 2 nm, even more preferably more than 3 nm, and particularly preferably more than 5 nm. A porous support having such an average pore size has a good support function and liquid permeability of the separation layer, and does not affect the CO2 permeability and gas selectivity of the separation layer. In the present invention, the average pore size is a value measured by a nanoperm porometer.

[0016] The thickness of the support is not particularly limited, but is preferably 0.5 to 5 mm, and more preferably 1 to 3 mm.

[0017] (Middle class) The separation membrane 10 preferably includes an intermediate layer 12 between the separation layer 13 and the support 11. The material of the intermediate layer is not particularly limited, but examples thereof include fine particles of metal oxides such as alumina, silica, zirconia, and mixtures thereof. The average particle size of the metal oxide fine particles is not particularly limited, and can be selected from a conventionally known range so as to form a desired average pore size.

[0018] The intermediate layer 12 can be formed by appropriately applying a colloidal sol containing these fine particles to the surface of the support 11 and baking it. By providing such an intermediate layer, the surface of the support can be made homogenous, and the difference in thermal expansion coefficient between the support and the separation layer can be mitigated, thereby improving the shape stability of the separation membrane.

[0019] The average pore diameter of the intermediate layer 12 is not particularly limited, but is preferably smaller than the average pore diameter of the support 11 and larger than the average pore diameter of the separation layer 13, and is, for example, preferably 0.5 to 5 nm, more preferably 0.5 to 3 nm, and even more preferably 1 to 2 nm. The thickness of the intermediate layer is not particularly limited, but is preferably 1 to 1000 nm.

[0020] In this embodiment, the intermediate layer is a single layer, but it may be two or more layers. When two or more intermediate layers are formed, the same material may be used for each layer, or different materials may be used for each layer. It is also possible not to provide an intermediate layer.

[0021] (separation layer) The separation layer 13 is formed on the support 11 directly or via the intermediate layer 12, and separates the target substance by pores that allow the target substance to pass through. The separation layer contains (A) a polymer having an isocyanuric acid skeleton and a siloxane bond, and (B) metal ions, and has an amorphous structure. The metal ions contained in the separation layer and the nitrogen atoms derived from the isocyanuric acid skeleton in the polymer form coordinate bonds with the metal ions acting as electron acceptors and the nitrogen atoms acting as electron donors, respectively. When a carbon atom, which has a lower electronegativity than the nitrogen atom, is bonded to the nitrogen atom, which serves as an electron donor in the polymer having a siloxane bond, a charge imbalance occurs between the nitrogen atom and the carbon atom, promoting the formation of coordinate bonds.

[0022] The separation layer 13 preferably has a network structure formed by siloxane bonds in a mesh shape (hereinafter also referred to as a "siloxane network") and a network structure formed by coordination bonds between nitrogen atoms in an isocyanuric acid skeleton and metal ions (hereinafter also referred to as a "coordination network"). By using a separation layer formed with such a siloxane network and a coordination network, a large number of pores that can selectively permeate CO2 are formed, so that a separation membrane excellent in CO2 permeability and CO2 / N2 selectivity can be obtained.

[0023] [Component (A)] The component (A) is a polymer having an isocyanuric acid skeleton and a siloxane bond (hereinafter, also referred to as "polymer (A)"). The component (A) is not particularly limited as long as it has the above structure. For example, a polymer obtained by polymerizing a precursor containing a compound represented by the following general formula (1) (hereinafter also referred to as "compound (1)") is preferable.

[0024] [ka] (In the formula, each X is independently a group represented by the following formula (2) or a monovalent hydrocarbon group having 1 to 8 carbon atoms, and at least one of X is a group represented by the following formula (2).) [ka] (In the formula, R 1 is an alkylene group having 1 to 8 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 8 carbon atoms; R 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 1 to 3. A wavy line represents a bond.

[0025] In formula (1), X is a monovalent hydrocarbon group having 1 to 8 carbon atoms and may be linear, branched, or cyclic. Specific examples thereof include linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, i-butyl, tert-butyl, neopentyl, n-hexyl, n-heptyl, and n-octyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl, allyl, 3-butenyl, 5-hexenyl, and 7-octenyl; and aryl groups such as phenyl. Of these, x is preferably a group having 1 to 3 carbon atoms, more preferably a vinyl group or an allyl group, and even more preferably an allyl group. However, it is preferable that at least one of X is a group represented by the above formula (2), and that all of X are groups represented by the above formula (2).

[0026] In formula (2), R 1 Specific examples of the alkylene group having 1 to 8 carbon atoms include methylene, ethylene, trimethylene, propylene, tetramethylene, hexamethylene, and octamethylene groups. Among these, R 1 is preferably an alkylene group having 2 or 3 carbon atoms, more preferably an alkylene group having 3 carbon atoms, and further preferably a trimethylene group.

[0027] R 2 Examples of the monovalent hydrocarbon group having 1 to 8 carbon atoms include the same groups as those exemplified for X. Among these, R 2 is preferably a group having 1 to 6 carbon atoms, more preferably a methyl group, a vinyl group, or a phenyl group.

[0028] R 3 Specific examples of the alkyl group having 1 to 4 carbon atoms may be linear or branched, and specific examples thereof include linear or branched alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, i-butyl, and tert-butyl groups. Among these, R 3 is preferably a methyl group or an ethyl group, more preferably a methyl group.

[0029] n is an integer of 1 to 3, with 3 being preferred.

[0030] Specific examples of compound (1) include tris[3-(trimethoxysilyl)propyl]isocyanurate (TTPI), allyl bis[3-(trimethoxysilyl)propyl]isocyanurate, diallyl[(3-trimethoxysilyl)propyl]isocyanurate, and the like. Among these, tris[3-(trimethoxysilyl)propyl]isocyanurate is preferred.

[0031] The compound (1) may be used alone or in combination of two or more kinds.

[0032] The polymer of component (A) can be obtained by hydrolysis and condensation of a precursor containing compound (1). The precursor may contain a compound capable of co-hydrolysis and condensation other than compound (1) within a range that does not impair the effects of the present invention. Examples of such compounds include silane compounds having a hydrolyzable group.

[0033] The silane compound having a hydrolyzable group is not particularly limited as long as it contains 1 to 4 hydrolyzable groups, that is, chloro groups or alkoxy groups, on the silicon atom. Specific examples thereof include tetrachlorosilane, tetramethoxysilane, tetraethoxysilane, tetraisopropoxysilane, tetrabutoxysilane, methyltrichlorosilane, methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, methyltributoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldiisopropoxysilane, trimethylchlorosilane, trimethylmethoxysilane, trimethylethoxysilane, trimethylisopropoxysilane, ethyltrichlorosilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrichlorosilane, propyltrimethoxysilane, propyltriethoxysilane, butyltrichlorosilane, butyltrimethoxysilane, butyltriethoxysilane, hexyltrichlorosilane, hexyltrimethoxysilane, hexyltriethoxysilane, phenyl Examples of suitable silanes include trichlorosilane, phenyltrimethoxysilane, phenyltriethoxysilane, cyclohexyltrichlorosilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, propylmethyldichlorosilane, propylmethyldimethoxysilane, propylmethyldiethoxysilane, hexylmethyldichlorosilane, hexylmethyldimethoxysilane, hexylmethyldiethoxysilane, phenylmethyldichlorosilane, phenylmethyldimethoxysilane, phenylmethyldiethoxysilane, diphenyldichlorosilane, diphenyldimethoxysilane, diphenyldiethoxysilane, dimethylphenylchlorosilane, dimethylphenylmethoxysilane, dimethylphenylethoxysilane, and partial hydrolysates thereof. From the viewpoints of operability, ease of distilling off by-products, and ease of availability of raw materials, methoxysilane and ethoxysilane are preferred. The above silane compounds may be used alone or in combination of two or more.

[0034] The proportion of compound (1) in the precursor is preferably 90 mol % or more, more preferably 95 mol % or more, and even more preferably 100 mol %, based on the total number of moles of the precursor.

[0035] [(B) Component] The component (B) is a metal ion, and examples of the metal include nickel, copper, silver, cobalt, and zinc (examples of the metal ion include Ni 2+ , Cu 2+ , Ag + , Co 2+ , Zn 2+ These may be used alone or in combination of two or more, with nickel being preferred.

[0036] The molar ratio (metal ion / nitrogen atom) of the (B) metal ion to the nitrogen atom derived from the isocyanuric acid skeleton in the polymer (A) in the separation layer is preferably 0.01 to 0.75, more preferably 0.10 to 0.60, and even more preferably 0.125 to 0.50, from the viewpoint of CO2 / N2 selectivity of the separation membrane. In addition, from the viewpoint of simultaneously achieving CO2 permeability of the separation membrane, it is most preferably 0.125 to 0.25.

[0037] The average pore size of the separation layer is not particularly limited, but is preferably smaller than the average pore size of the intermediate layer, for example, preferably less than 1 nm, more preferably less than 0.5 nm. The lower limit is not particularly limited, but is preferably 0.1 nm or more.

[0038] The thickness of the separation layer is preferably 100 nm or more and 1000 nm or less. If the separation layer is 1000 nm or less, a long time or high pressure is not required for CO2 separation, and separation efficiency is excellent. Also, if the separation layer is 100 nm or more, the permeation of gases other than CO2 can be suppressed, and CO2 selectivity is further improved.

[0039] (2) Method for producing separation membrane The method for producing the separation membrane according to the present invention is not particularly limited as long as it can produce a separation membrane having the above-mentioned separation layer, and examples thereof include a method including the following steps. (I) A metal-doped polymer sol preparation step for preparing a metal-doped polymer sol containing (A) a polymer having an isocyanuric acid skeleton and a siloxane bond and (B) a metal ion. (II) a coating step of coating the metal-doped polymer sol onto a porous support directly or via an intermediate layer. (III) A firing step of firing the metal-doped polymer sol applied in the coating step to form a separation layer having an amorphous structure.

[0040] Step (I): Preparation of metal-doped polymer sol This step is a step of preparing a metal-doped polymer sol containing (A) a polymer having an isocyanuric acid skeleton and a siloxane bond, and (B) metal ions. The metal-doped polymer sol can be obtained by mixing (A) a sol of a polymer having an isocyanuric acid skeleton and a siloxane bond and (B) a metal salt that serves as a source of metal ions.

[0041] The sol of polymer (A) can be obtained by hydrolysis and condensation of a precursor containing compound (1). In this case, the sol of polymer (A) may be prepared by synthesizing polymer (A) by hydrolysis and condensation in advance, and then dispersing the obtained polymer (A) in a solvent, or the sol containing polymer (A) after the hydrolysis and condensation reaction may be used as it is. In the present invention, however, it is preferable to use the sol containing polymer (A) after the hydrolysis and condensation reaction as it is.

[0042] When carrying out the hydrolysis condensation, a hydrolysis catalyst may be used. As the hydrolysis catalyst, a conventionally known catalyst can be used, and a catalyst (acid catalyst) whose aqueous solution shows an acidity of pH 2 to 7 is preferable, and particularly, an acidic hydrogen halide, a sulfonic acid, a carboxylic acid, an acidic or weakly acidic inorganic salt, a solid acid such as an ion exchange resin, etc. are preferable. Specific examples of acidic catalysts include hydrogen fluoride, hydrochloric acid, nitric acid, sulfuric acid, methanesulfonic acid, p-toluenesulfonic acid, formic acid, acetic acid, maleic acid, benzoic acid, lactic acid, phosphoric acid, and cation exchange resins having sulfonic acid or carboxylic acid groups on the surface.

[0043] The amount of the hydrolysis catalyst used is not particularly limited, but in order to ensure that the reaction proceeds quickly and to facilitate easy removal of the catalyst after the reaction, it is preferably 0.0002 to 0.5 mol per 1 mol of silicon atoms in the precursor.

[0044] The amount of water required for the hydrolysis condensation reaction is not particularly limited, but in order to prevent the deactivation of the catalyst and to allow the reaction to proceed sufficiently, a ratio of 0.1 to 200 moles of water per mole of silicon atoms in the precursor is preferred. The reaction temperature during hydrolysis and condensation is not particularly limited, but in consideration of improving the reaction rate and preventing decomposition of the organic functional group, it is preferably −10 to 150° C. The reaction time is not particularly limited, but is preferably 0.5 to 24 hours.

[0045] In addition, an organic solvent may be used during the hydrolysis and condensation. Specific examples of the organic solvent that can be used include methanol, ethanol, propanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, toluene, and xylene.

[0046] Subsequently, a metal salt is added to the obtained sol of polymer (A) and stirred to prepare a metal-doped polymer sol. The metal salt used is one that serves as a source of metal ions for component (B). Specific examples include Ni(NO3)2·6H2O, AgNO3, Cu(NO3)2·3H2O, Co(NO3)2·6H2O, Zn(NO3)2·6H2O, etc., with Ni(NO3)2·6H2O being preferred. The amount of metal salt added is such that the molar ratio of the (B) metal ion to the nitrogen atom derived from the isocyanuric acid skeleton in the polymer (A) (metal ion / nitrogen atom) falls within the above-mentioned range.

[0047] The concentration of the metal-doped polymer in the metal-doped polymer sol is preferably 0.1 to 0.5% by mass from the viewpoint of efficiently producing a uniform separation layer.

[0048] Process (II): Coating process This step is a step of applying the metal-doped polymer sol obtained in the above step (I) onto a porous support directly or via an intermediate layer. The coating method and coating amount are not particularly limited and can be appropriately selected from known methods such as dipping and brush coating, and it is preferable to coat to a desired thickness.

[0049] In addition, when an intermediate layer is provided in the separation membrane of the present invention, the intermediate layer forming step may be performed after the metal-doped polymer sol preparing step or before the metal-doped polymer sol preparing step. Also, the metal-doped polymer sol preparing step and the intermediate layer forming step may be performed in parallel.

[0050] An example of the intermediate layer formation process is a method in which the surface of the support 11 is coated with a SiO2-ZrO2 sol mixed with α-alumina particles and fired to form a first intermediate layer, and then a SiO2-ZrO2 sol is applied onto the first intermediate layer and fired to form a second intermediate layer, thereby forming intermediate layer 12 on the support 11. The firing conditions in the intermediate layer formation step are preferably a firing temperature of 400 to 500° C. in air and a firing time of 10 to 30 minutes.

[0051] Step (III): Firing step This step is a step of baking the metal-doped polymer sol applied in the application step to form a separation layer. The calcination conditions are preferably, for example, a calcination temperature of 200 to 400°C and a calcination time of 30 to 60 minutes in an inert gas atmosphere such as nitrogen or argon. Within such ranges, the CO2 permeability and CO2 / N2 selectivity of the separation membrane can be further improved. EXAMPLES

[0052] The present invention will be explained in more detail below with reference to Synthesis Examples, Comparative Synthesis Examples, Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0053] [Synthesis Examples 1 to 3, Comparative Synthesis Example 1] Process (I): Water and nitric acid were added to TTPI (KBM-9659: Shin-Etsu Chemical Co., Ltd.) dissolved in ethanol, and TTPI was hydrolyzed and condensed. The molar ratio was TTPI / H2O / HNO3=1 / 300 / 1. The mixture was stirred at 25°C for 12 hours to prepare a sol of the hydrolysis condensation product of TTPI (TTPI sol). The concentration of the TTPI sol was adjusted to 5% by mass using ethanol.

[0054] Next, the metal salt Ni(NO3)2·6H2O (Sigma-Aldrich) was added to the TTPI sol obtained above and stirred to prepare nickel-doped TTPI sol (Ni-TTPI). The concentration of Ni-TTPI was adjusted to 0.1% by mass using ion-exchanged water. At this time, nickel-doped TTPI sols were prepared in which the molar ratio of nickel to nitrogen atoms in TPPI (Ni / N) was 0.125 (Ni-TPPI 0.125: Synthesis Example 1), 0.25 (Ni-TPPI 0.25: Synthesis Example 2), and 0.50 (Ni-TPPI 0.50: Synthesis Example 3). In addition, as a TPPI sol to which no metal salt was added, the TPPI sol obtained in the above step (I) was diluted with ion-exchanged water to 0.1 mass % (TTPI: Comparative Synthesis Example 1) was prepared.

[0055] (Characteristics of nickel-doped TTPI sol) 2(a) shows the results of measurement by ultraviolet-visible spectroscopy (UV-Vis) of the nickel-doped TTPI sols obtained in Synthesis Examples 1 to 3, the TTPI sol obtained in Comparative Synthesis Example 1, and Ni(NO3)2·6H2O. The UV-Vis measurements were performed using a UV-3600plus ultraviolet-visible-near-infrared spectrophotometer (Shimadzu Corporation). In the nickel-doped TTPI sol and TTPI sol, peaks were detected at 200 to 212 nm, which indicates the intraligand transition (n → σ*) of electrons in the amino group. In the nickel-doped TTPI sol, two peaks were detected at 400 nm and 600 nm. In addition, as the nickel ratio increased, the two peaks at 400 nm and 600 nm shifted to the higher wavelength side due to changes in the state of the free electrons in the amino group.

[0056] Figure 2(b) shows the Fourier transform infrared spectroscopy (FT-IR) (wavenumber 500-2000 cm -1 The nickel-doped TTPI sols obtained in Synthesis Examples 1 to 3 and the TTPI sol obtained in Comparative Synthesis Example 1 were each coated onto a KBr plate, baked at 250° C. in a N2 atmosphere, and then measured using a Fourier transform infrared spectrophotometer FT / IR-4100 (manufactured by JASCO Corporation). The isocyanuric acid skeleton has a wave number of 1550 to 1650 cm -1 As the amount of nickel doped increases, the peak increases from 1610 to 1620 cm -1 The peaks became broader and stronger at 100°C, which is believed to be due to the promotion of coordination bonds between amino groups and metal ions by the hydrolysis and condensation reaction of TTPI.

[0057] 2(c) and (d) show the results of X-ray photoelectron spectroscopy (XPS). The nickel-doped TTPI sols obtained in Synthesis Examples 1 to 3 and the TTPI sol obtained in Comparative Synthesis Example 1 were each coated onto a silicon wafer and baked at 250°C, after which measurements were performed using an X-ray photoelectron spectrometer (ESCA 3400-HSE, manufactured by Shimadzu Corporation). As shown in Figure 2(c), the N(1s) binding energy peak shifted upon nickel doping, and the increase in binding energy is believed to be due to nitrogen, which is an electron donor that forms a coordinate bond. In addition, in the Ni(2p) binding energy shown in Figure 2(d), the two peaks at 874 eV and 857 eV observed in nickel-doped TPPI (Ni-TPPI 0.25), which contains nitrogen atoms that form coordinate bonds with nickel, are thought to be due to the presence of Ni-OH.

[0058] The results of measurements by UV-Vis, FT-IR, and XPS show that coordinate bonds are formed between the isocyanuric acid skeleton and nickel ions in nickel-doped TTPI sols with any nickel ratio.

[0059] (Characteristics of Nickel-doped TTPI Powder) The nickel-doped TTPI sols obtained in the above Synthesis Examples 1 to 3 and the TTPI sol obtained in Comparative Synthesis Example 1 were dried at 180°C, crushed into powder, and sintered for 30 minutes at 250°C in a N2 atmosphere. The resulting powders were characterized by X-ray diffraction (XRD) and transmission electron microscope (TEM) images. The XRD analysis was performed using an XRD D2 PHASER (manufactured by Bruker), and the transmission electron microscope used was a TEM JEOL2010 (manufactured by JEOL Ltd.).

[0060] Figure 3(a) shows the XRD measurement results of the calcined nickel-doped TTPI powder and the TTPI powder. The characteristic broad peaks at 8° and 20° in 2θ angles originating from the siloxane network (Si-O-Si) were observed, and in the nickel-doped TTPI powder, a peak of Ni(OH)2 was observed at 15°. As the Ni / N molar ratio increases, the first peak at 8° shifts lower and the second peak at 20° becomes broader, indicating that a more amorphous structure is formed.

[0061] Figure 3(b) shows TEM images of the calcined nickel-doped TTPI powder and TTPI powder. The upper row shows low-resolution TEM images, and the lower row shows high-resolution TEM images. When the nickel ratio was 0.25 or higher, nickel was distributed unevenly, and many dark spots were confirmed, which indicate non-coordinated nickel that did not form coordinate bonds with amino groups.

[0062] Figure 4 shows the N2 adsorption isotherms (-196°C) of the calcined nickel-doped TTPI powder and the TTPI powder. The measurements were performed using a BELMAX (BELJAPAN). Table 1 shows the BET (Brunauer-Emmett-Teller) specific surface area and total pore volume calculated from the N2 adsorption / desorption isotherms.

[0063] [Table 1]

[0064] As shown in Table 1, the nickel-doped TTPI powder has a larger BET specific surface area and total pore volume than the TTPI powder. In these metal-doped TTPI powders, pores are formed by coordinate bonds between the amino groups in the TTPI molecule, which are electron donors, and the metal ions, which are electron acceptors.

[0065] In addition, the BET specific surface area and total pore volume were the largest for the Ni-TTPI 0.25 powder, while both the surface area and pore volume decreased when the Ni / N ratio was further increased to 0.5. This is thought to be due to the aggregation of excess nickel that has not formed coordinate bonds with TTPI to form nanoparticles, blocking the pore structure. Figure 5 shows a schematic diagram of the mechanism of Ni-TTPI network formation at Ni / N molar ratios of 0, 0.25, and 0.50.

[0066] The CO2 adsorption and desorption isotherms of the calcined nickel-doped TTPI and TTPI powders are shown in Figure 6. The Ni-TTPI0.25 sample showed higher CO2 adsorption than TPPI or low-concentration nickel-doped powders. Meanwhile, under similar conditions, Ni-TTPI0.50 showed lower CO2 adsorption capacity due to the pores being blocked by uncoordinated nickel particles.

[0067] [Example 1] (Intermediate layer formation process) An α-alumina tube (manufactured by Nikkato Corporation, length 100 mm, inner diameter 8 mm, outer diameter 10 mm) was used as the porous support. A dispersion liquid obtained by mixing α-alumina particles with a number average particle size of 0.2 μm and α-alumina particles with a number average particle size of 2 μm with SiO2-ZrO2 sol (number average particle size: approximately 10 nm, 2.0 mass%) and diluting it with ion-exchanged water to 10 mass% was coated on the outer surface of the porous support, allowed to dry naturally, and then sintered at 550° C. for 15 minutes in air. The first intermediate layer was formed by repeating the application and sintering of the above dispersion liquid three times.

[0068] Next, the first intermediate layer was coated with SiO2-ZrO2 sol (number-average particle size: about 10 nm, 0.5 mass%) and baked in air at 550°C for 10 minutes. The second intermediate layer was formed by repeating the application and baking of SiO2-ZrO2 sol until the average pore size measured by a nanoperm porometer was 1 nm or more and 2 nm or less, and the first and second intermediate layers were formed sequentially on the outer surface of the support.

[0069] Process (II): Next, in the coating step, the 0.1 mass % nickel-doped TTPI sol (Ni-TPPI 0.125) obtained in Synthesis Example 1 above was coated onto the second intermediate layer.

[0070] Process (III): Next, in the calcination process, the nickel-doped TTPI sol was applied onto the second intermediate layer formed on the support obtained in the above step (II), and calcined at 250°C for 30 minutes in a N2 atmosphere to form a separation layer and produce a separation membrane.

[0071] [Example 2] A separation membrane was produced in the same manner as in Example 1, except that in step (II), the 0.1 mass% nickel-doped TTPI sol obtained in Synthesis Example 1 was changed to the 0.1 mass% nickel-doped TTPI sol (Ni-TPPI 0.25) obtained in Synthesis Example 2.

[0072] [Example 3] A separation membrane was produced in the same manner as in Example 1, except that in step (II), the 0.1 mass% nickel-doped TTPI sol obtained in Synthesis Example 1 was changed to the 0.1 mass% nickel-doped TTPI sol (Ni-TPPI 0.50) obtained in Synthesis Example 3.

[0073] [Comparative Example 1] A separation membrane was produced in the same manner as in Example 1, except that in step (II), the 0.1 mass% nickel-doped TTPI sol obtained in Synthesis Example 1 above was changed to the 0.1 mass% TTPI sol (TPPI) obtained in Comparative Synthesis Example 1 above.

[0074] The permeability of the separation membranes obtained in Examples 1 to 3 and Comparative Example 1 was evaluated for helium, hydrogen, carbon dioxide, nitrogen, methane, carbon tetrafluoride, and sulfur hexafluoride. The gas to be permeated was supplied from the separation layer side of the separation membrane (separation layer 13 side in FIG. 1) at a pressure of 200 to 400 kPa, and the permeability was evaluated at 200° C. The permeation flow rate was measured using a film flow meter (manufactured by Horiba, Ltd.).

[0075] The relationship between gas molecular size and gas permeability is shown in Figure 7. As the molecular size of the gas to be permeated increases, the permeability decreases. Therefore, it is believed that the gas separation by the separation membranes obtained in Examples 1 to 3 is due to molecular sieving. The separation membrane using Ni-TTPI0.25 (Example 2) was more porous than the separation membrane using TPPI (Comparative Example 1) or the separation membrane using Ni-TTPI (Example 1), and therefore had improved gas permeability. On the other hand, when Ni-TTPI0.50 was used (Example 3), the gas permeability was low, indicating that the membrane structure became dense due to the blocking of pores by nickel particles, which was consistent with the above-mentioned results of CO2 adsorption of Ni-TTPI particles.

[0076] Figure 8 shows the temperature dependence of the CO2 and N2 gas permeabilities and the CO2 / N2 permeability ratio for the separation membranes obtained in Examples 1 to 3 and Comparative Example 1. (a) to (d) are the results using the separation membranes obtained in Comparative Example 1 and Examples 1 to 3, respectively. For all separation membranes, the higher the measurement temperature T, i.e., the lower the reciprocal of the measurement temperature T (1 / T), the higher the N2 permeability. This is presumably because (1) the siloxane network of the separation membrane vibrates due to heat, increasing the size of the pores in the separation membrane, and (2) the increased kinetic energy of the N2 molecules promotes the diffusion of the N2 molecules. This gas permeation mechanism, in which the permeability increases as the measurement temperature T increases, is called "activated diffusion."

[0077] On the other hand, for CO2, the higher the Ni / NH molar ratio in the Ni-TTPI separation layer, the higher the CO2 permeability at low temperatures, which is presumably due to the dominance of the gas permeation mechanism known as “surface diffusion.” In surface diffusion, CO2 molecules are adsorbed onto the surface of the CO2 separation membrane, creating a gradient of CO2 concentration from the upstream side to the downstream side of the separation membrane, and the molecules move two-dimensionally along this concentration gradient. The lower the measurement temperature T, the lower the energy of the CO2 molecules, making it easier for them to be adsorbed onto the surface of the separation membrane, and the diffusion movement that occurs according to the concentration gradient is promoted. Therefore, in surface diffusion, the higher the measurement temperature T, the lower the transmittance.

[0078] The CO2 / N2 permeation selectivity of the separation membranes obtained in Examples 1 to 3 improved significantly as the temperature decreased from high to low. This is presumably because the N2 gas permeation mechanism is activated diffusion, and the permeability decreases as the temperature decreases, whereas the CO2 gas permeation mechanism in the Ni-TTPI separation layer is such that the reversible physical adsorption of amine-CO2 occurs more easily due to an increase in nickel coordination to the amine in the isocyanuric acid skeleton, and as a result, the contribution of surface diffusion, which increases the permeability as the temperature decreases, becomes greater.

[0079] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. [Explanation of symbols]

[0080] 10 Separation membrane 11 Support 12 Middle Class 13 Separation layer

Claims

1. A separation membrane comprising (A) a polymer having an isocyanuric acid skeleton and a siloxane bond, and (B) a metal ion, and comprising a separation layer having an amorphous structure.

2. 2. The separation membrane according to claim 1, wherein the component (A) is a polymer obtained by polymerizing a precursor containing a compound represented by the following general formula (1): 【Chemistry 1】 (In the formula, each X is independently a group represented by the following formula (2) or a monovalent hydrocarbon group having 1 to 8 carbon atoms, and at least one of the Xs is a group represented by the following formula (2).) 【Chemistry 2】 (In the formula, R 1 is an alkylene group having 1 to 8 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 8 carbon atoms; R 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer from 1 to 3. A wavy line represents a bond.

3. 3. The separation membrane according to claim 2, wherein the component (A) is a polymer obtained by polymerizing a precursor containing tris[3-(trimethoxysilyl)propyl]isocyanurate.

4. 4. The separation membrane according to claim 1, wherein the metal in the component (B) is at least one selected from the group consisting of nickel, copper, silver, cobalt and zinc.

5. (I) a metal-doped polymer sol preparation step of preparing a metal-doped polymer sol containing (A) a polymer having an isocyanuric acid skeleton and a siloxane bond and (B) a metal ion; (II) a coating step of coating the metal-doped polymer sol directly or via an intermediate layer onto a porous support; (III) a baking step for baking the metal-doped polymer sol applied in the coating step to form a separation layer having an amorphous structure; A method for producing a separation membrane comprising the steps of:

6. 6. The method for producing a separation membrane according to claim 5, wherein the metal-doped polymer sol preparation step is carried out by mixing the polymer sol (A) with the metal salt (B) which serves as a source of metal ions.

7. The method for producing a separation membrane according to claim 5, wherein the component (A) is a polymer obtained by polymerizing a precursor containing a compound represented by the following general formula (1): 【Chemistry 3】 (In the formula, each X is independently a group represented by the following formula (2) or a monovalent hydrocarbon group having 1 to 8 carbon atoms, and at least one of the Xs is a group represented by the following formula (2).) 【Chemistry 4】 (In the formula, R 1 is an alkylene group having 1 to 8 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 8 carbon atoms; R 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and n is an integer of 1 to 3.

8. The method for producing a separation membrane according to claim 7, wherein the component (A) is a polymer obtained by polymerizing a precursor containing tris[3-(trimethoxysilyl)propyl]isocyanurate.

9. The method for producing a separation membrane according to any one of claims 5 to 8, wherein the metal in the component (B) is at least one selected from the group consisting of nickel, copper, silver, cobalt and zinc.

Citation Information

Patent Citations

  • Gas dehumidification device and gas dehumidification method

    JP2020151708A

  • Co2 separation film and method for producing co2 separation film

    JP2021186712A

  • Co2 separation membrane

    JP2022021175A